Multilayer optical film and method for producing multilayer optical film

The laminated optical film with a curable adhesive layer containing metal oxide particles and specific monomers addresses refractive index and adhesive strength issues, enhancing durability and transmittance stability.

WO2024247659A1PCT designated stage expired Publication Date: 2024-12-05NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017403
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-10
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing laminated optical films face challenges with refractive index stability, adhesive strength, and curing shrinkage in their adhesive layers, particularly when incorporating metal oxide particles, which are not adequately addressed by current techniques.

Method used

A laminated optical film design featuring an adhesive layer composed of a curable component and metal oxide particles, with specific formulations including phenoxybenzyl (meth)acrylate and hydroxyl group-containing (meth)acrylates, along with isocyanurate and polysiloxane compounds, to enhance refractive index and adhesive strength while minimizing curing shrinkage.

Benefits of technology

The proposed solution achieves a high refractive index and excellent adhesive strength in the adhesive layer, reducing curing shrinkage and improving the durability and transmittance stability of the laminated optical film, especially under heat exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017403_05122024_PF_FP_ABST
    Figure JP2024017403_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a multilayer optical film, in which at least a first optical film and a second optical film are stacked with an adhesive layer being interposed therebetween, wherein the adhesive layer is a cured product layer of an adhesive composition for multilayer optical films, the adhesive composition containing a curable component and metal oxide particles. It is preferable that the content of the metal oxide particles is 10% by mass to 50% by mass if the total amount of the adhesive composition for multilayer optical films is taken as 100% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

LAMINATED OPTICAL FILM AND METHOD FOR PRODUCING LAMINATED OPTICAL FILM

[0001] The present invention relates to a laminated optical film and a method for producing the laminated optical film, which can be used to form image displays such as liquid crystal displays (LCDs), organic EL displays, CRTs, and PDPs.

[0002] 2. Description of the Related Art Image display devices are known in which a circular polarizer is disposed on the viewing side of a display panel in order to improve poor visibility caused by reflection of external light or glare of the background on the display screen of the image display device.

[0003] For example, Patent Document 1 listed below describes a polarizing plate composite comprising, in this order, a linear polarizing plate, a half-wave layer, a first adhesive layer formed by curing an active energy ray-curable adhesive, and a quarter-wave layer, in which the angle between the fast axis of the half-wave layer and the transmission axis of the linear polarizing plate is 10° or more and 20° or less, and the absolute value of the difference between the refractive index of the first adhesive layer at a wavelength of 589 nm and the refractive index of the half-wave layer in the fast axis direction at a wavelength of 589 nm is less than 0.05.

[0004] Furthermore, Patent Document 2 listed below describes a retardation layer-attached polarizing plate that includes a polarizer, a first retardation layer, and a second retardation layer in this order, the polarizer and the first retardation layer being bonded together via a first adhesive layer, the first retardation layer and the second retardation layer being bonded together via a second adhesive layer, the thicknesses of the first retardation layer and the second retardation layer being 5 μm or less, the average refractive index of the second adhesive layer being 1.55 or more, and the difference between the average refractive index of the second adhesive layer and that of the first retardation layer and that of the second retardation layer being less than 0.08.

[0005] Incidentally, Patent Document 3 listed below describes an active energy ray-curable resin composition characterized by containing metal oxide nanoparticles (A), phenoxybenzyl (meth)acrylates (B), and a bifunctional (meth)acrylate having a (poly)alkylene glycol structure (C), with the aim of providing an active energy ray-curable resin composition and a cured product thereof that have a balance of various properties required for optical sheets and the like used in optical applications.

[0006] JP 2020-52365 A JP 2018-17996 A JP 2017-128688 A

[0007] As a result of intensive research by the present inventors, it has been found that the techniques described in Patent Documents 1 and 2 above leave room for further improvement when it comes to stably improving the refractive index of interlayer adhesives for laminated films. The technique described in Patent Document 3 above relates to an active energy ray-curable resin composition for producing a lens sheet, and is not intended for use in bonding at least two optical films. In addition, adhesive compositions for laminated optical films are applied to optical films at fairly thin film thicknesses, and therefore, when metal oxide particles are contained, the compositions are required to have excellent liquid stability. However, the technique described in Patent Document 3 above does not address this issue, let alone describe or suggest a means for solving this issue.

[0008] The present invention was developed in consideration of the above-mentioned circumstances, and aims to provide a laminated optical film having an adhesive layer that has a high refractive index, excellent adhesive strength, and a reduced cure shrinkage rate.

[0009] The above-mentioned problems can be solved by the following configuration: That is, the present invention relates to a laminated optical film (1) in which at least a first optical film and a second optical film are laminated via an adhesive layer, wherein the adhesive layer is a cured layer of an adhesive composition for laminated optical films that contains a curable component and metal oxide particles.

[0010] In the laminated optical film (1), the adhesive composition for laminated optical films is preferably a laminated optical film (2) in which the content of the metal oxide particles is 10 to 50 mass % when the total amount of the composition is 100 mass %.

[0011] In the laminated optical film (1) or (2), a laminated optical film (3) is preferred in which the adhesive composition for a laminated optical film further contains a (meth)acrylate containing an aromatic ring skeleton.

[0012] In the laminated optical film (3), the adhesive composition for laminated optical films is preferably a laminated optical film (4) in which the content of the (meth)acrylate containing an aromatic ring skeleton is 30 to 70 mass % when the total amount of the composition is 100 mass %.

[0013] In the laminated optical film (3), a laminated optical film (5) is preferred in which the (meth)acrylate containing an aromatic ring skeleton contains at least one selected from the group consisting of (meth)acrylates having a polycyclic aromatic ring skeleton and (meth)acrylates having two or more aromatic rings.

[0014] In the laminated optical film (3), the (meth)acrylate containing an aromatic ring skeleton is preferably phenoxybenzyl (meth)acrylate.

[0015] In any one of the laminated optical films (1) to (6), the adhesive composition for a laminated optical film further contains a compound represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent), is preferred.

[0016] In the laminated optical film (7), the adhesive composition for laminated optical films is preferably a laminated optical film (8) in which the content of the compound represented by the general formula (1) is 0.1 to 10 mass % when the total amount of the composition is 100 mass %.

[0017] In any one of the laminated optical films (1) to (8), a laminated optical film (9) is preferred in which the adhesive composition for a laminated optical film further contains a hydroxyl group-containing (meth)acrylate.

[0018] In the laminated optical film (9), the adhesive composition for laminated optical films is preferably a laminated optical film (10) in which the content of the hydroxyl group-containing (meth)acrylate is 1 to 30 mass % when the total amount of the composition is 100 mass %.

[0019] In any one of the laminated optical films (1) to (10), the adhesive composition for laminated optical films preferably further contains a leveling agent containing at least one selected from the group consisting of an isocyanurate compound and a polysiloxane compound.

[0020] In the laminated optical film (11), the adhesive composition for laminated optical films is preferably a laminated optical film (12) in which the content of the isocyanurate compound is 0.05 to 10 mass % when the total amount of the composition is 100 mass %.

[0021] In the laminated optical film (11), the adhesive composition for laminated optical films is preferably a laminated optical film (13) in which the content of the polysiloxane compound is 0.05 to 2.0 mass% when the total amount of the composition is 100 mass%.

[0022] In any one of the laminated optical films (1) to (13), a laminated optical film (14) is preferred in which the viscosity of the adhesive composition for a laminated optical film at 25° C. is 100 mPa·s or less.

[0023] Of the laminated optical films (1) to (14), a laminated optical film (15) is preferred which includes at least a polarizer as the optical film.

[0024] The present invention also relates to a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, the method comprising: a coating step of applying an adhesive composition for laminated optical films to one or both of a bonding surface of the first optical film and a bonding surface of the second optical film; a laminating step of laminating the first optical film and the second optical film; and an adhering step of adhering the first optical film and the second optical film via the adhesive layer formed by irradiating active energy rays from the first optical film surface side or the second optical film surface side to cure at least the adhesive composition for laminated optical films, wherein the adhesive composition for laminated optical films contains a curable component and metal oxide particles.

[0025] The laminated optical film according to the present invention has an adhesive layer formed from a cured product layer of an adhesive composition for laminated optical films containing a curable component and metal oxide particles, and therefore has a high refractive index, excellent adhesive strength, and a reduced cure shrinkage. In particular, when the adhesive composition for laminated optical films contains a compound represented by general formula (1) together with metal oxide particles, this is preferable because it can further improve the refractive index of the adhesive layer and the adhesive strength. Furthermore, when the adhesive composition for laminated optical films contains phenoxybenzyl (meth)acrylate together with metal oxide particles, this is preferable because it can further improve the refractive index of the adhesive layer.

[0026] It is preferable that the laminated optical film according to the present invention is a polarizing film having at least a polarizer as an optical film, or a laminated optical film having one or more optical films laminated in addition to a polarizing film having a polarizer, because this suppresses changes in transmittance after a heat durability test. The reason for this effect is unclear, but can be assumed as follows. Metal oxide particles expand less and deform less when heated than resin components used in conventional adhesives, so that an adhesive layer containing metal oxide particles is suppressed from expanding or deforming when heated. As a result, a laminated optical film having an adhesive layer containing metal oxide suppresses the expansion and contraction of the various optical films that make up the laminated optical film when heated, so it is assumed that deterioration of the optical film's properties (including a decrease in transmittance) can be suppressed. The above-mentioned effects attributable to metal oxide particles can be achieved not only when an adhesive layer formed from a cured product layer of an adhesive composition for a laminated optical film containing metal oxide particles is in direct contact with a polarizer, but also when the adhesive layer is not in direct contact with a polarizer.

[0027] An example of the laminated optical film according to the present invention

[0028] FIG. 1 shows an example of a laminated optical film according to the present invention. The laminated optical film 10 shown in FIG. 1 includes a first optical film 1 and a second optical film 2 laminated together via an adhesive layer 3, which is a cured layer of an adhesive composition for laminated optical films. The adhesive composition for laminated optical films used in the present invention to form the adhesive layer 3 has a high refractive index due to the stable dispersion of metal oxide particles. Therefore, when, for example, a retardation film, preferably a liquid crystal retardation film, is used as the first optical film 1 and the second optical film 2, the refractive index difference between the first optical film 1 and the adhesive layer 3 can be reduced. Similarly, the refractive index difference between the second optical film 2 and the adhesive layer 3 can be reduced. This reduces interference unevenness in the laminated optical film and improves visibility.

[0029] The laminated optical film according to the present invention may be a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer that is a cured layer of an adhesive composition for a laminated optical film, and may further include any optical film. The laminated optical film 10 shown in FIG. 1 includes a polarizer 5 on the first optical film 1 (on the viewing side) and a transparent protective film 4. Adhesive layers are typically provided between the first optical film 1 and the polarizer 5 and between the polarizer 5 and the transparent protective film 4 (omitted in FIG. 1 ). These adhesive layers may be the same as the adhesive layer 3 that is a cured layer of the adhesive composition for a laminated optical film used in the present invention, or may be a cured layer of an adhesive composition for a laminated optical film known to those skilled in the art. The laminated optical film 10 shown in FIG. 1 also includes an organic light-emitting diode layer 7 below the second optical film (on the display device side) via a pressure-sensitive adhesive layer 6.

[0030] The laminated optical film according to the present invention comprises at least a first optical film and a second optical film laminated together via an adhesive layer. The adhesive layer is formed of a cured layer of an adhesive composition for laminated optical films, which contains a curable component and metal oxide particles. The adhesive composition for laminated optical films, which is a raw material for the adhesive layer, will be described below.

[0031] <Metal oxide particles> The adhesive composition for laminated optical film used in the present invention contains metal oxide particles. Examples of metal oxide particles include silicon oxide, zirconium oxide, titanium oxide, zinc oxide, antimony pentoxide, tin oxide, aluminum oxide, indium oxide, indium tin oxide, ferric oxide, cerium oxide, yttrium oxide, manganese oxide, holmium oxide, copper oxide, bismuth oxide, cobalt oxide, tricobalt tetroxide, triiron tetroxide, magnesium oxide, lanthanum oxide, praseodymium oxide, neodymium oxide, samarium oxide, eurobium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, erbium oxide, thulium oxide, ytterbium oxide, lutetium oxide, scandium oxide, tantalum pentoxide, niobium pentoxide, iridium oxide, rhodium oxide, ruthenium oxide, and composite oxides formed by combining these. Among these, zirconium oxide and titanium oxide are preferred, and zirconium oxide is particularly preferred. The metal oxide particles used in the present invention may be composed solely of the metal oxides listed above, or may contain other components, but it is preferable that the metal oxide accounts for the largest proportion by weight of the components in the particles. The shape of the metal oxide particles may be any shape, such as spherical, ellipsoidal, cubic, rectangular, or pyramidal. In the present invention, the metal oxide particles may be surface-treated by a method known to those skilled in the art.

[0032] From the viewpoint of improving the stability of the metal oxide particles in the adhesive composition and improving the refractive index of the adhesive layer, the average particle size of the metal oxide particles used is preferably 1 to 150 nm, and more preferably 1 to 50 nm. In the present invention, the average particle size of the metal oxide particles can be calculated by performing magnified observation using a transmission electron microscope (TEM), a field emission transmission electron microscope (FE-TEM), a field emission scanning electron microscope (FE-SEM), or the like, randomly selecting, for example, 1,000 particles, measuring their maximum lengths, and determining the arithmetic mean.

[0033] The average particle size of the metal oxide particles blended in the adhesive composition can also be calculated by dynamic light scattering or laser diffraction. When calculated by dynamic light scattering or laser diffraction, the average particle size means the particle size at 50% of the integrated value in the particle size distribution determined by the laser diffraction / scattering method.

[0034] From the standpoint of improving the stability of the metal oxide particles in the adhesive composition and improving the refractive index of the adhesive layer, the amount of metal oxide particles used is preferably 10 to 50% by mass, and more preferably 15 to 40% by mass, when the total amount of the composition is 100% by mass.

[0035] <Curable Component> The adhesive composition for laminated optical films used in the present invention contains a curable component. In the present invention, the curable component is preferably an active energy ray-curable component. Active energy ray-curable components can be classified into radical polymerization-curable components and cationic polymerization-curable components. In the present invention, active energy rays in the wavelength range of 10 nm to less than 380 nm are referred to as ultraviolet rays, and active energy rays in the wavelength range of 380 nm to 800 nm are referred to as visible light.

[0036] The adhesive composition for laminated optical films used in the present invention may contain a monofunctional radical polymerizable compound as a curable component. Examples of the monofunctional radical polymerizable compound include various (meth)acrylic acid derivatives having a (meth)acryloyloxy group. Specific examples include (meth)acrylic acid (C1-20) alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and n-octadecyl (meth)acrylate.

[0037] Examples of the (meth)acrylic acid derivatives include cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate and cyclopentyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxy Examples of suitable (meth)acrylates include polycyclic (meth)acrylates such as ethyl (meth)acrylate and dicyclopentanyl (meth)acrylate; and alkoxy or phenoxy group-containing (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, and alkylphenoxy polyethylene glycol (meth)acrylate. Among these, dicyclopentenyloxyethyl acrylate and phenoxyethyl acrylate are preferred because of their excellent adhesion to various protective films.

[0038] In addition, examples of the (meth)acrylic acid derivatives include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate. hydroxyl group-containing (meth)acrylates such as [4-(hydroxymethyl)cyclohexyl]methyl acrylate, cyclohexanedimethanol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate; epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether; 2,2,2-trifluoroethyl (meth)acrylate, 2,2,2-trifluoroethylethyl (meth)acrylate; Halogen-containing (meth)acrylates such as acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; alkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate; 3-oxetanylmethyl (meth)acrylate, 3-methyl-oxetanylmethyl (meth)acrylate; oxetane group-containing (meth)acrylates such as acrylate, 3-ethyl-oxetanylmethyl (meth)acrylate, 3-butyl-oxetanylmethyl (meth)acrylate, and 3-hexyl-oxetanylmethyl (meth)acrylate; (meth)acrylates having a heterocycle such as tetrahydrofurfuryl (meth)acrylate and butyrolactone (meth)acrylate; hydroxypivalic acid neopentyl glycol (meth)acrylic acid adduct; and p-phenylphenol (meth)acrylate. Among these, 2-hydroxy-3-phenoxypropyl acrylate is preferred because of its excellent adhesion to various protective films.

[0039] The adhesive composition for laminated optical films used in the present invention preferably contains a hydroxyl group-containing (meth)acrylate in addition to the metal oxide particles and the compound represented by general formula (1), since this further improves the adhesive strength of the adhesive layer. From the viewpoint of improving the adhesive strength of the adhesive layer, the blending amount of the hydroxyl group-containing (meth)acrylate is preferably 1 to 30% by mass, and more preferably 3 to 20% by mass, when the total amount of the composition is taken as 100% by mass.

[0040] Furthermore, examples of the monofunctional radically polymerizable compound include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.

[0041] Examples of the monofunctional radically polymerizable compound include lactam vinyl monomers such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, and methylvinylpyrrolidone; and vinyl monomers having a nitrogen-containing heterocycle such as vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, and vinylmorpholine.

[0042] Furthermore, as the monofunctional radical polymerizable compound, a radical polymerizable compound having an active methylene group can be used. The radical polymerizable compound having an active methylene group is a compound having an active double bond group such as a (meth)acrylic group at the end or in the molecule, and also having an active methylene group. Examples of the active methylene group include an acetoacetyl group, an alkoxymalonyl group, and a cyanoacetyl group. It is preferable that the active methylene group is an acetoacetyl group. Specific examples of radically polymerizable compounds having an active methylene group include acetoacetoxyalkyl (meth)acrylates such as 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxypropyl (meth)acrylate, and 2-acetoacetoxy-1-methylethyl (meth)acrylate; 2-ethoxymalonyloxyethyl (meth)acrylate, 2-cyanoacetoxyethyl (meth)acrylate, N-(2-cyanoacetoxyethyl)acrylamide, N-(2-propionylacetoxybutyl)acrylamide, N-(4-acetoacetoxymethylbenzyl)acrylamide, and N-(2-acetoacetylaminoethyl)acrylamide. The radically polymerizable compound having an active methylene group is preferably an acetoacetoxyalkyl (meth)acrylate.

[0043] The adhesive composition for laminated optical films used in the present invention may contain a bifunctional or higher polyfunctional radically polymerizable compound as a curable component. Examples of the polyfunctional radically polymerizable compound include polyfunctional (meth)acrylamide derivatives such as N,N'-methylenebis(meth)acrylamide, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol diacrylate, 2-ethyl-2-butylpropanediol di(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, and bisphenol A diglycidyl ether di(meth)acrylate. esters of (meth)acrylic acid with polyhydric alcohols such as acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, cyclic trimethylolpropane formal(meth)acrylate, dioxane glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and EO-modified diglycerin tetra(meth)acrylate; and 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene. Specific examples include Aronix M-220 (manufactured by Toagosei Co., Ltd.), Light Acrylate 1,9ND-A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DGE-4A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DCP-A (manufactured by Kyoeisha Chemical Co., Ltd.), SR-531 (manufactured by Sartomer Co., Ltd.), and CD-536 (manufactured by Sartomer Co., Ltd.), etc. Furthermore, various epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, and various (meth)acrylate monomers may be used as needed.It is preferable to include a polyfunctional (meth)acrylamide derivative in the adhesive composition because it has a high polymerization rate, is excellent in productivity, and has excellent crosslinking properties when the adhesive composition is cured.

[0044] For example, when a polarizer and a transparent protective film are used as the optical film, it is preferable to use a monofunctional radically polymerizable compound and a polyfunctional radically polymerizable compound in combination as the radically polymerizable compound, from the viewpoint of achieving both adhesion to the polarizer and various transparent protective films and optical durability under harsh environments. The amount of the monofunctional radically polymerizable compound in the adhesive composition is preferably 10 to 95% by mass, and more preferably 30 to 80% by mass, when the total amount of the composition is taken as 100% by mass. The amount of the polyfunctional radically polymerizable compound in the adhesive composition is preferably 0.5 to 60% by mass, and more preferably 1 to 40% by mass, when the total amount of the composition is taken as 100% by mass.

[0045] <(Meth)acrylate containing an aromatic ring skeleton> When the adhesive composition for a laminated optical film used in the present invention contains a (meth)acrylate containing an aromatic ring skeleton together with metal oxide particles, the refractive index of the adhesive layer is improved, which is preferable. From the viewpoint of more stably increasing the refractive index of the adhesive layer, in the present invention, it is preferable to use, as the (meth)acrylate containing an aromatic ring skeleton, one containing at least one selected from the group consisting of (meth)acrylates having a polycyclic aromatic ring skeleton and (meth)acrylates having two or more aromatic rings. Examples of (meth)acrylates containing an aromatic ring skeleton include benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 1-naphthalenemethyl (meth)acrylate, phenoxybenzyl (meth)acrylate, ethylene oxide-modified orthophenylphenol (meth)acrylate, and a reaction product of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and (meth)acrylic acid. Among these, it is more preferable to use phenoxybenzyl (meth)acrylate and phenoxyethyl (meth)acrylate, and it is particularly preferable to use phenoxybenzyl (meth)acrylate. Phenoxybenzyl (meth)acrylate is represented by the following formula (A): In the above formula (A), X is a single bond forming part of an adjacent bonding group, or a structure having 1 to 5 repeating ethylene oxide, propylene oxide, butylene oxide, or styrene oxide structures. R represents a hydrogen atom or a methyl group. The adhesive composition for laminated optical films used in the present invention is a compound having the following formula (A-1): It is preferable that the phenoxybenzyl (meth)acrylate contains an o- or m-substituted product represented by the following formula:

[0046] From the viewpoint of improving the refractive index of the adhesive layer, the blending amount of the (meth)acrylate containing an aromatic ring skeleton used, particularly phenoxybenzyl (meth)acrylate, is preferably 30 to 70% by mass when the total amount in the composition is taken as 100% by mass.

[0047] <Compound Represented by General Formula (1)> The adhesive composition for laminated optical films used in the present invention contains a compound represented by the following general formula (1) together with metal oxide particles: (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2 each independently represents a hydrogen atom, an optionally substituted aliphatic hydrocarbon group, an aryl group, or a heterocyclic group), the adhesive strength of the adhesive layer is further improved, which is preferable. In addition, when the adhesive composition for a laminated optical film used in the present invention contains a compound represented by the above general formula (1) together with metal oxide particles, the cure shrinkage of the adhesive layer is reduced. Therefore, when a laminated optical film is formed, the stress applied to each optical film can be reduced, which is preferable because the durability of the laminated optical film can be expected to be improved.

[0048] Examples of the aliphatic hydrocarbon group include a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, a cyclic alkyl group having 3 to 20 carbon atoms which may have a substituent, and an alkenyl group having 2 to 20 carbon atoms. Examples of the aryl group include a phenyl group having 6 to 20 carbon atoms which may have a substituent, and a naphthyl group having 10 to 20 carbon atoms which may have a substituent. Examples of the heterocyclic group include a 5- or 6-membered ring group which contains at least one hetero atom and may have a substituent. These may be linked to each other to form a ring. In general formula (1), R 1 and R 2 is preferably a hydrogen atom or a linear or branched alkyl group having 1 to 3 carbon atoms, and most preferably a hydrogen atom.

[0049] X in the compound represented by general formula (1) is a reactive group, which is a functional group that can react with a curable component that constitutes the cured product layer, particularly the adhesive layer, and examples thereof include a hydroxyl group, an amino group, an aldehyde group, a carboxyl group, a vinyl group, a (meth)acrylic group, a styryl group, a (meth)acrylamide group, a vinyl ether group, an epoxy group, an oxetane group, an α,β-unsaturated carbonyl group, a mercapto group, and a halogen group. When the curable resin composition constituting the cured product layer, particularly the adhesive layer, is active energy ray-curable, the reactive group X is preferably at least one reactive group selected from the group consisting of vinyl groups, (meth)acrylic groups, styryl groups, (meth)acrylamide groups, vinyl ether groups, epoxy groups, oxetane groups, and mercapto groups. When the curable resin composition constituting the cured product layer, particularly the adhesive layer, is radically polymerizable, the reactive group X is preferably at least one reactive group selected from the group consisting of (meth)acrylic groups, styryl groups, and (meth)acrylamide groups. When the compound represented by general formula (1) has a (meth)acrylamide group, this is more preferred because it has high reactivity and increases the copolymerization rate with the curable component in the cured product layer, particularly the adhesive layer. Furthermore, this is also preferred because the (meth)acrylamide group has high polarity and excellent adhesiveness, allowing the effects of the present invention to be efficiently obtained. When the curable resin composition constituting the cured product layer, particularly the adhesive layer, is cationic polymerizable, the reactive group X preferably has at least one functional group selected from a hydroxyl group, an amino group, an aldehyde, a carboxyl group, a vinyl ether group, an epoxy group, an oxetane group, and a mercapto group. In particular, when the reactive group X has an epoxy group, this is preferred because the resulting cured product layer, particularly the adhesive layer, has excellent adhesion to the adherend, and when the reactive group X has a vinyl ether group, this is preferred because the curability of the curable resin composition is excellent.

[0050] Preferred specific examples of the compound represented by general formula (1) include the following compounds (1a) to (1d). 3 is a hydrogen atom or a methyl group.

[0051] In addition to the compounds exemplified above, examples of the compound represented by general formula (1) include esters of (meth)acrylates and boric acid, such as esters of hydroxyethyl acrylamide and boric acid, esters of methylolacrylamide and boric acid, esters of hydroxyethyl acrylate and boric acid, and esters of hydroxybutyl acrylate and boric acid.

[0052] From the viewpoint of improving the adhesive strength of the adhesive layer, the amount of the compound represented by general formula (1) used is preferably 0.1 to 10 mass %, and more preferably 0.3 to 5 mass %, when the total amount in the composition is 100 mass %.

[0053] The adhesive composition for laminated optical films used in the present invention contains at least one compound selected from the group consisting of an isocyanurate compound and a polysiloxane compound, thereby stably dispersing metal oxide particles. Therefore, despite the inclusion of metal oxide particles, the viscosity can be kept low. From the viewpoint of thinning the adhesive layer and the laminated optical film by thinly coating the adhesive composition for laminated optical films on an optical film, the viscosity of the composition at 25°C is preferably 100 mPa·s or less, and more preferably 60 mPa·s or less.

[0054] <Leveling Agent> The adhesive composition for laminated optical films used in the present invention preferably contains at least one leveling agent selected from the group consisting of an isocyanurate compound and a polysiloxane compound. By including at least one leveling agent selected from the group consisting of an isocyanurate compound and a polysiloxane compound in the composition, the metal oxide particles are stably dispersed, resulting in excellent liquid stability of the adhesive composition for laminated optical films. Furthermore, by including metal oxide particles and at least one leveling agent selected from the group consisting of an isocyanurate compound and a polysiloxane compound in the composition, the occurrence of cissing and bubbles during application to the optical film can be suppressed. From the perspective of further enhancing the above-mentioned effects, the adhesive composition for laminated optical films used in the present invention preferably contains both an isocyanurate compound and a polysiloxane compound. When the adhesive composition for laminated optical films contains both an isocyanurate compound and a polysiloxane compound, the blending amounts thereof are preferably 0.1 to 4 mass%, and more preferably 0.1 to 2 mass%, based on the total amount of the composition as 100 mass%. As described below, when an isocyanurate compound is also blended as a crosslinking agent, and when the adhesive composition for a laminated optical film contains both an isocyanurate compound and a polysiloxane compound, the blending amount thereof is preferably 0.1 to 14 mass%, and more preferably 0.1 to 7 mass%, when the total amount of the composition is 100 mass%.

[0055] <Isocyanurate Compound> The isocyanurate compound is a compound containing an isocyanurate ring structure formed by the trimerization reaction of isocyanate. In the present invention, it is particularly preferable to use a modified isocyanurate compound having a reactive group. Examples of the reactive group of the modified isocyanurate compound include polymerizable functional groups, such as radically polymerizable functional groups having an ethylenic double bond, such as (meth)acryloyl groups, vinyl groups, and allyl groups; cationically polymerizable functional groups, such as epoxy groups, such as glycidyl groups; oxetane groups, vinyl ether groups, cyclic ether groups, cyclic thioether groups, and lactone groups. From the viewpoint of reactivity in the adhesive composition for laminated optical films, modified isocyanurate compounds having a double bond as the reactive group are preferred, and modified isocyanurate compounds having a (meth)acryloyl group are more preferred. The amount of the isocyanurate compound in the adhesive composition for laminated optical films is preferably 0.05 to 2% by mass, and more preferably 0.05 to 1% by mass, based on the total amount of the composition as 100% by mass.

[0056] The isocyanurate compound not only contributes to stabilizing the dispersion of metal oxide particles in the composition, but also has the effect of reducing the cure shrinkage rate when, for example, an adhesive layer is formed. Therefore, when an isocyanurate compound is blended as a crosslinking agent in the adhesive composition for a laminated optical film used in the present invention, the blending amount of the isocyanurate compound is preferably as large as possible, specifically, preferably 0.05 to 10% by mass, and more preferably 0.05 to 5% by mass, when the total amount in the composition is 100% by mass.

[0057] <Polysiloxane Compound> The polysiloxane compound is a compound having a polysiloxane skeleton such as polydimethylsiloxane. In the present invention, it is particularly preferable to use a modified polysiloxane compound having a reactive group. Examples of the reactive group possessed by the modified polysiloxane compound include polymerizable functional groups, specifically, radically polymerizable functional groups having an ethylenic double bond such as a (meth)acryloyl group, a vinyl group, or an allyl group; epoxy groups such as a glycidyl group; and cationically polymerizable functional groups such as an oxetane group, a vinyl ether group, a cyclic ether group, a cyclic thioether group, or a lactone group. From the viewpoint of reactivity in the adhesive composition for laminated optical films, modified polysiloxane compounds having a double bond as the reactive group are preferred, and modified polysiloxane compounds having a (meth)acryloyl group are more preferred. The amount of the polysiloxane compound in the adhesive composition for laminated optical films is preferably 0.05 to 2% by mass, and more preferably 0.05 to 1% by mass, when the total amount of the composition is taken as 100% by mass.

[0058] The adhesive composition for laminated optical films used in the present invention can be used as an active energy ray-curable adhesive composition when the curable component is an active energy ray-curable component. When electron beams or the like are used as the active energy rays, the active energy ray-curable adhesive composition does not need to contain a photopolymerization initiator, but when ultraviolet rays or visible light are used as the active energy rays, it is preferable for the active energy ray-curable adhesive composition to contain a photopolymerization initiator.

[0059] The photopolymerization initiator is appropriately selected depending on the active energy ray. When curing is performed with ultraviolet light or visible light, a photopolymerization initiator that is cleaved by ultraviolet light or visible light is used. Examples of the photopolymerization initiator include benzophenone-based compounds such as benzil, benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; aromatic ketone compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and α-hydroxycyclohexylphenyl ketone; acetophenone-based compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin methyl ether. aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates.

[0060] The amount of the photopolymerization initiator blended is preferably 0.5 to 5% by mass, and more preferably 1 to 4% by mass, when the total amount in the composition is taken as 100% by mass.

[0061] When the active energy ray-curable adhesive composition is used as a visible light-curable type, it is preferable to use a photopolymerization initiator that is particularly sensitive to light of 380 nm or more. Photopolymerization initiators that are highly sensitive to light of 380 nm or more will be described later.

[0062] The photopolymerization initiator may be a compound represented by the following general formula (3): (In the formula, R 7 and R 8 -H, -CH 2 CH 3 , -iPr or Cl, R 7 and R 8 It is preferable to use a compound represented by general formula (3) alone, or to use a compound represented by general formula (3) in combination with a photopolymerization initiator highly sensitive to light of 380 nm or longer, which will be described later. When a compound represented by general formula (3) is used, the adhesiveness is superior to when a photopolymerization initiator highly sensitive to light of 380 nm or longer is used alone. Among the compounds represented by general formula (3), R 7 and R 8 Ga-CH 2 CH 3 The amount of the compound represented by general formula (3) in the active energy ray-curable adhesive composition is preferably 0.1 to 5 mass %, and more preferably 0.3 to 3 mass %, when the total amount of the composition is 100 mass %.

[0063] It is also preferable to add a polymerization initiation aid as needed. Examples of the polymerization initiation aid include triethylamine, diethylamine, N-methyldiethanolamine, ethanolamine, 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, and isoamyl 4-dimethylaminobenzoate, with ethyl 4-dimethylaminobenzoate being particularly preferred. When a polymerization initiation aid is used, the amount added is preferably 0.1 to 2% by mass, and more preferably 0.3 to 1% by mass, when the total amount of the composition is taken as 100% by mass.

[0064] In addition, a known photopolymerization initiator can be used in combination as needed. Since the optical functional layer and the base film having UV absorption ability do not transmit light of 380 nm or less, it is preferable to use a photopolymerization initiator that is highly sensitive to light of 380 nm or more. Specific examples include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, and the like.

[0065] In the present invention, the adhesive composition for laminated optical films preferably contains an acrylic oligomer obtained by polymerizing a (meth)acrylic monomer. By containing an acrylic oligomer in the adhesive composition for laminated optical films, it is possible to reduce cure shrinkage when the composition is irradiated with active energy rays and cured, and to reduce the interfacial stress between the adhesive layer and the optical film. As a result, it is possible to suppress a decrease in adhesion between the adhesive layer and the optical film.

[0066] Considering workability and uniformity during application, the adhesive composition for laminated optical films preferably has a low viscosity, and therefore the acrylic oligomer obtained by polymerizing a (meth)acrylic monomer also preferably has a low viscosity. The acrylic oligomer, which has a low viscosity and can prevent the adhesive layer from shrinking upon curing, preferably has a weight-average molecular weight (Mw) of 15,000 or less, more preferably 10,000 or less, and particularly preferably 5,000 or less. On the other hand, in order to sufficiently suppress the shrinkage of the cured product layer (adhesive layer) upon curing, the weight-average molecular weight (Mw) of the acrylic oligomer is preferably 500 or more, more preferably 1,000 or more, and particularly preferably 1,500 or more. Specific examples of the (meth)acrylic monomer constituting the acrylic oligomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,(Meth)acrylic acid (C1-20) alkyl esters such as 2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and N-octadecyl (meth)acrylate; further, for example, cycloalkyl (meth)acrylates (for example, cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, etc.), aralkyl (meth)acrylates (for example, benzyl (meth)acrylate, etc.), polycyclic (meth)acrylates (for example, 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and 4-methyl-2-propylpentyl (meth)acrylate; (meth)acrylate, etc.), hydroxyl group-containing (meth)acrylic acid esters (for example, hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,3-dihydroxypropylmethyl-butyl (meth)methacrylate, etc.), alkoxy group- or phenoxy group-containing (meth)acrylic acid esters (2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, etc.), epoxy group-containing (meth)acrylic acid esters (for example, glycidyl (meth)acrylate, etc.), halogen-containing (meth)acrylic acid esters (for example, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,Examples of the acrylic oligomer (E) include 2-trifluoroethylethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, etc., and alkylaminoalkyl (meth)acrylates (for example, dimethylaminoethyl (meth)acrylate, etc.). These (meth)acrylates can be used alone or in combination of two or more. Specific examples of the acrylic oligomer (E) include "ARUFON" manufactured by Toagosei Co., Ltd., "Actflow" manufactured by Soken Chemical & Engineering Co., Ltd., and "JONCRYL" manufactured by BASF Japan Ltd.

[0067] The blending amount of the acrylic oligomer in the adhesive composition for laminated optical films is preferably 3 to 40% by mass, and more preferably 5 to 20% by mass.

[0068] The adhesive composition for laminated optical films used in the present invention may contain a silane coupling agent. Specific examples of the silane coupling agent include active energy ray-curable compounds such as vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane.

[0069] Preferred are 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.

[0070] Specific examples of non-active energy ray-curable silane coupling agents other than those mentioned above include 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, and imidazole silane.

[0071] The adhesive composition for a laminated optical film used in the present invention may be a cationic polymerization-curable adhesive composition. The curable component (cationically polymerizable compound) used in the cationic polymerization-curable adhesive composition is classified into monofunctional cationic polymerizable compounds having one cationic polymerizable functional group in the molecule and polyfunctional cationic polymerizable compounds having two or more cationic polymerizable functional groups in the molecule. Monofunctional cationic polymerizable compounds have relatively low liquid viscosity, and their inclusion in the cationic polymerization-curable adhesive composition can reduce the liquid viscosity. Furthermore, monofunctional cationic polymerizable compounds often have functional groups that impart various functions. By including them in the cationic polymerization-curable adhesive composition, various functions can be imparted to the cationic polymerization-curable adhesive composition and / or the cured product of the cationic polymerization-curable adhesive composition. Polyfunctional cationic polymerizable compounds are preferably included in the cationic polymerization-curable adhesive composition because they can three-dimensionally crosslink the cured product of the cationic polymerization-curable resin composition. The ratio of the monofunctional cationically polymerizable compound to the polyfunctional cationically polymerizable compound is preferably 10% by mass to 1000% by mass of the polyfunctional cationically polymerizable compound relative to 100% by mass of the monofunctional cationically polymerizable compound. Examples of the cationically polymerizable functional group include an epoxy group, an oxetanyl group, and a vinyl ether group. Examples of compounds having an epoxy group include an aliphatic epoxy compound, an alicyclic epoxy compound, and an aromatic epoxy compound. The cationically polymerizable resin composition of the present invention particularly preferably contains an alicyclic epoxy compound because of its excellent curability and adhesiveness.Examples of the alicyclic epoxy compound include 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, caprolactone-modified 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, trimethylcaprolactone-modified 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and valerolactone-modified 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate. Specific examples include Celloxide 2021, Celloxide 2021A, Celloxide 2021P, Celloxide 2081, Celloxide 2083, and Celloxide 2085 (all manufactured by Daicel Chemical Industries, Ltd.), and Cyracure UVR-61 05, Cyracure UVR-6107, Cyracure 30, R-6110 (all manufactured by Dow Chemical Japan Co., Ltd.). Compounds having an oxetanyl group are preferably contained because they have the effect of improving the curing properties of the cationically polymerizable adhesive composition and reducing the liquid viscosity of the composition. Examples of compounds having an oxetanyl group include 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, di[(3-ethyl-3-oxetanyl)methyl]benzoate ... Examples of suitable vinyl ether compounds include 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, and phenol novolak oxetane. Commercially available compounds include ARON OXT-101, ARON OXT-121, ARON OXT-211, ARON OXT-221, and ARON OXT-212 (all manufactured by Toagosei Co., Ltd.). Compounds having a vinyl ether group are preferably contained in the cationically polymerizable adhesive composition because they have the effect of improving the curing properties of the composition and reducing the liquid viscosity of the composition. Examples of compounds having an ether group include 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, triethylene glycol divinyl ether, cyclohexanedimethanol divinyl ether, cyclohexanedimethanol monovinyl ether, tricyclodecane vinyl ether, cyclohexyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, and pentaerythritol tetravinyl ether.

[0072] The cationic polymerization-curable adhesive composition contains at least one compound selected from the group consisting of the epoxy group-containing compound, the oxetanyl group-containing compound, and the vinyl ether group-containing compound described above as a curable component. Since all of these compounds cure by cationic polymerization, a photocationic polymerization initiator is incorporated into the composition. This photocationic polymerization initiator generates cationic species or Lewis acids upon irradiation with active energy rays such as visible light, ultraviolet light, X-rays, and electron beams, thereby initiating the polymerization reaction of the epoxy group or oxetanyl group. The photoacid generator described below is preferably used as the photocationic polymerization initiator. Furthermore, when the cationic polymerization adhesive composition is used as a visible light-curable adhesive, it is preferable to use a photocationic polymerization initiator that is highly sensitive to light of 380 nm or longer. However, since photocationic polymerization initiators generally exhibit a maximum absorption in the wavelength range around 300 nm or shorter, incorporating a photosensitizer that exhibits a maximum absorption in the longer wavelength range, specifically, light of wavelengths longer than 380 nm, can enhance the generation of cationic species or acids from the photocationic polymerization initiator by reacting to light of this wavelength range. Examples of photosensitizers include anthracene compounds, pyrene compounds, carbonyl compounds, organic sulfur compounds, persulfides, redox compounds, azo and diazo compounds, halogen compounds, and photoreducible dyes, and these may be used in combination of two or more. Anthracene compounds are particularly preferred because of their excellent photosensitizing effect, and specific examples include Anthracure UVS-1331 and Anthracure UVS-1221 (manufactured by Kawasaki Chemical Industries, Ltd.). The content of the photosensitizer is preferably 0.1% by mass to 5% by mass, and more preferably 0.5% by mass to 3% by mass.

[0073] In the present invention, the adhesive composition for a laminated optical film may contain a photoacid generator. When the adhesive composition for a laminated optical film contains a photoacid generator, the water resistance and durability of the adhesive layer can be dramatically improved compared to when the adhesive composition does not contain a photoacid generator. The photoacid generator can be represented by the following general formula (4).

[0074] (However, L +represents any onium cation. - is PF6 6 - , SbF 6 - , AsF 6 - , SbCl 6 - , BiCl 5 - , SnCl 6 - , ClO 4 - , a dithiocarbamate anion, and a counter anion selected from the group consisting of SCN-.

[0075] Next, the counter anion X in the general formula (4) - This article explains:

[0076] Counter anion X in general formula (4) - Although there is no particular limitation in principle, a non-nucleophilic anion is preferred. - When PF is a non-nucleophilic anion, nucleophilic reactions are unlikely to occur with cations coexisting in the molecule or with various materials used in combination, and as a result, it is possible to improve the stability over time of the photoacid generator represented by general formula (4) itself and compositions using it. The non-nucleophilic anion here refers to an anion with a low ability to cause a nucleophilic reaction. Examples of such anions include PF 6 - , SbF 6 - , AsF 6 - , SbCl 6 - , BiCl 5 - , SnCl 6 - , ClO 4 - , B(C 6 H 5 ) 4 - , dithiocarbamate anion, SCN - Examples include:

[0077] Specifically, "Cyracure UVI-6992" and "Cyracure UVI-6974" (both manufactured by Dow Chemical Japan Co., Ltd.), "ADEKAOPTOMER SP150", "ADEKAOPTOMER SP152", "ADEKAOPTOMER SP170", and "ADEKAOPTOMER SP172" (all manufactured by ADEKA Corporation), and "Omnicat250" (IGM Resins B.V.), "CI-5102", "CI-2855" (all manufactured by Nippon Soda Co., Ltd.), "SAN-AID SI-60L", "SAN-AID SI-80L", "SAN-AID SI-100L", "SAN-AID SI-110L", "SAN-AID SI-180L" (all manufactured by Sanshin Chemical Industry Co., Ltd.), "IK-1", "CPI-100P", "CPI-101A", "CPI-110P", "CPI-200K", "CPI-210S", "CPI Specific preferred examples of the photoacid generator of the present invention include "WPI-310B", "CPI-410B", and "CPI-410S" (all manufactured by San-Apro Ltd.), "WPI-069", "WPI-113", "WPI-116", "WPI-041", "WPI-044", "WPI-054", "WPI-055", "WPAG-281", "WPAG-567", and "WPAG-596" (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).

[0078] The laminated optical film according to the present invention is a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, and the adhesive layer is a cured product layer of the adhesive composition for laminated optical films described above.

[0079] The adhesive composition for laminated optical films used in the present invention contains metal oxide particles, and when it further contains at least one compound selected from the group consisting of an isocyanurate compound and a polysiloxane compound, the viscosity of the composition can be kept low due to the stable dispersion of the metal oxide particles, and therefore the adhesive composition for laminated optical films can be applied thinly onto the optical film, thereby making it possible to reduce the thickness of the adhesive layer.

[0080] The thickness of the adhesive layer provided in the laminated optical film according to the present invention is preferably 0.1 to 5 μm, and more preferably 0.3 to 3 μm.

[0081] In the present invention, examples of the first optical film and the second optical film constituting the laminated optical film include a polarizer, a transparent protective film, and a retardation film.

[0082] In the present invention, the polarizer is not particularly limited, and various polarizers can be used. Examples of polarizers include those obtained by uniaxially stretching a hydrophilic polymer film, such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or a partially saponified ethylene-vinyl acetate copolymer film, after iodine has been adsorbed thereon. The thickness of the polarizer can be, for example, 3 to 20 μm.

[0083] However, in the present invention, from the viewpoint of improving heat durability in a harsh environment under high temperatures, it is preferable to use a thin polarizer having a thickness of 3 μm or more and 15 μm or less as the polarizer. A thickness of 12 μm or less is particularly preferable, and a thickness of 10 μm or less, particularly 8 μm or less, is further preferable. Such a thin polarizer has little thickness unevenness, excellent visibility, and is excellent in durability against thermal shock due to little dimensional change.

[0084] A polarizer obtained by dyeing a polyvinyl alcohol-based film with iodine and uniaxially stretching it can be produced, for example, by immersing the polyvinyl alcohol in an iodine aqueous solution to dye it and then stretching it to 3 to 7 times its original length. If necessary, the polyvinyl alcohol-based film may contain boric acid, zinc sulfate, zinc chloride, or the like, or may be immersed in an aqueous solution of potassium iodide or the like. Furthermore, if necessary, the polyvinyl alcohol-based film may be immersed in water and washed before dyeing. Washing the polyvinyl alcohol-based film with water not only removes dirt and antiblocking agents from the polyvinyl alcohol-based film surface, but also swells the polyvinyl alcohol-based film, thereby preventing unevenness such as uneven dyeing. Stretching may be performed after dyeing with iodine, or the film may be stretched while dyeing, or the film may be dyed with iodine after stretching. Stretching may also be performed in an aqueous solution of boric acid, potassium iodide, or the like, or in a water bath.

[0085] The polarizer preferably contains boric acid from the viewpoints of stretching stability and humidification reliability. Furthermore, the content of boric acid in the polarizer is preferably 22% by mass or less, and more preferably 20% by mass or less, of the total amount of the polarizer, from the viewpoint of suppressing the occurrence of through cracks. From the viewpoints of stretching stability and humidification reliability, the content of boric acid in the polarizer is preferably 10% by mass or more, and more preferably 12% by mass or more, of the total amount of the polarizer.

[0086] Representative examples of the thin polarizer include the thin polarizers described in Japanese Patent No. 4751486, Japanese Patent No. 4751481, Japanese Patent No. 4815544, Japanese Patent No. 5048120, WO 2014 / 077599, and WO 2014 / 077636, and the like, as well as thin polarizers obtained by the manufacturing methods described therein.

[0087] Among the thin polarizers obtained by manufacturing methods including a stretching step and a dyeing step in a laminated state, those obtained by a manufacturing method including a stretching step in a boric acid aqueous solution as described in Japanese Patent Nos. 4751486, 4751481, and 4815544 are preferred because they can be stretched at a high magnification and have improved polarization performance. In particular, those obtained by a manufacturing method including a supplementary in-air stretching step before stretching in a boric acid aqueous solution as described in Japanese Patent Nos. 4751481 and 4815544 are preferred. These thin polarizers can be obtained by a manufacturing method including a stretching step and a dyeing step of a polyvinyl alcohol-based resin (hereinafter also referred to as PVA-based resin) layer and a stretching resin substrate in a laminated state. With this manufacturing method, even if the PVA-based resin layer is thin, it can be stretched without problems such as breakage due to stretching because it is supported by the stretching resin substrate.

[0088] The transparent protective film is made of a thermoplastic resin that exhibits excellent transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose-based resin films, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The transparent protective film may contain one or more suitable additives. Examples of additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants. The content of the thermoplastic resin in the transparent protective film is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, even more preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. If the content of the thermoplastic resin in the transparent protective film is 50% by weight or less, the inherent high transparency of the thermoplastic resin may not be fully exhibited.

[0089] The material for forming the transparent protective film is preferably one that is excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc., and in particular, a moisture permeability of 150 g / m 2 / 24h or less is more preferable, and 140g / m 2 / 24h or less is particularly preferred, and 120g / m 2 / 24 hours or less is even more preferable.

[0090] The surface of the transparent protective film to which the polarizer is not bonded can be provided with a functional layer such as a hard coat layer, an antireflection layer, an antisticking layer, a diffusion layer, an antiglare layer, etc. The functional layer such as the hard coat layer, the antireflection layer, the antisticking layer, the diffusion layer, or the antiglare layer can be provided on the transparent protective film itself, or can be provided separately from the transparent protective film.

[0091] The thickness of the transparent protective film can be determined as appropriate, but is generally about 1 to 500 μm, preferably 1 to 300 μm, more preferably 5 to 200 μm, further preferably 10 to 200 μm, and more preferably 20 to 80 μm, from the viewpoints of workability such as strength and handleability, thinness, etc.

[0092] As the transparent protective film, a retardation film having a front retardation of 40 nm or more and / or a thickness direction retardation of 80 nm or more can be used. The front retardation is usually controlled in the range of 40 to 200 nm, and the thickness direction retardation is usually controlled in the range of 80 to 300 nm. When a retardation film is used as the transparent protective film, the retardation film also functions as the transparent protective film, thereby enabling a thinner film to be achieved.

[0093] Examples of the retardation film include a birefringent film obtained by uniaxially or biaxially stretching a polymer material, an oriented film of a liquid crystal polymer, an oriented layer of a liquid crystal polymer supported by a film, etc. The thickness of the retardation film is not particularly limited, but is generally about 1 to 150 μm.

[0094] The retardation film may be a film satisfying the following formulas (1) to (3): 0.70<Re

[450] / Re

[550] <0.97 (1) 1.5×10 -3 < Δn < 6 × 10 -3 ... (2) 1.13<NZ<1.50 ... (3) (wherein Re

[450] and Re

[550] are in-plane retardation values ​​of the retardation film measured at 23°C with light of wavelengths of 450 nm and 550 nm, respectively; Δn is in-plane birefringence, which is nx-ny, where nx and ny are the refractive indices in the slow axis direction and the fast axis direction of the retardation film, respectively; and NZ is the ratio of nx-nz, which is the birefringence in the thickness direction, to nx-ny, which is the in-plane birefringence, where nz is the refractive index in the thickness direction of the retardation film).

[0095] The laminated optical film according to the present invention may be provided with a retardation layer. The retardation layer may be a single layer or multiple layers, and the retardation layer may also serve as a protective layer for the polarizer.

[0096] A liquid crystalline compound is preferably used to form the retardation layer, and a solvent containing the liquid crystalline compound can be applied using, for example, a wire bar, a gap coater, a comma coater, a gravure coater, a slot die, or the like. In this case, the applied liquid crystalline solution may be dried naturally or by heating. It is preferable that the liquid crystalline solution be applied at a concentration lower than the isotropic phase-liquid crystal phase transition concentration, i.e., in an isotropic phase state. In this case, stable alignment can be achieved by methods such as rubbing treatment or photoalignment.

[0097] The laminated optical film according to the present invention can be produced, for example, by the following production method: A method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, the method comprising the steps of: applying an adhesive composition for laminated optical films to one or both of a bonding surface of the first optical film and a bonding surface of the second optical film; laminating the first optical film and the second optical film; and bonding the first optical film and the second optical film via the adhesive layer formed by irradiating the first optical film surface side or the second optical film surface side with active energy rays to cure at least the adhesive composition for laminated optical films, wherein the adhesive composition for laminated optical films contains a curable component and metal oxide particles.

[0098] In the coating step, the method for coating the adhesive composition for laminated optical films onto one or both of the bonding surface of the first optical film and the bonding surface of the second optical film is appropriately selected depending on the viscosity of the composition and the desired thickness, and examples thereof include a reverse coater, a gravure coater (direct, reverse, or offset), a bar reverse coater, a roll coater, a die coater, a bar coater, and a rod coater.

[0099] The first optical film and / or the second optical film may be subjected to a surface modification treatment before the coating step. In particular, when a polarizer is used as the optical film, it is preferable to subject the polarizer to a surface modification treatment. Examples of surface modification treatments include corona treatment, plasma treatment, and Itro treatment, with corona treatment being particularly preferable. Corona treatment generates reactive functional groups such as carbonyl groups and amino groups on the polarizer surface, improving adhesion to the adhesive layer. Furthermore, the ashing effect removes foreign matter from the surface and reduces surface irregularities, allowing the production of a laminated optical film with excellent appearance characteristics.

[0100] The first optical film and the second optical film are bonded together via the adhesive composition for laminated optical films coated as described above using a roll laminator or the like (laminating step).

[0101] After laminating the first optical film and the second optical film, the adhesive composition for laminated optical films is cured by irradiating with active energy rays (electron beams, ultraviolet rays, visible light, etc.) to form an adhesive layer. The irradiation direction of the active energy rays (electron beams, ultraviolet rays, visible light, etc.) can be any appropriate direction.

[0102] When irradiating with electron beams, any suitable irradiation conditions can be used as long as they are sufficient to cure the adhesive composition for laminated optical films. For example, the acceleration voltage for electron beam irradiation is preferably 5 kV to 300 kV, more preferably 10 kV to 250 kV. If the acceleration voltage is less than 5 kV, the electron beams may not reach the adhesive, resulting in insufficient curing. If the acceleration voltage is greater than 300 kV, the penetration force through the sample may be too strong, potentially damaging the first optical film and the second optical film. The irradiation dose is 5 to 100 kGy, more preferably 10 to 75 kGy. If the irradiation dose is less than 5 kGy, the adhesive may not be cured sufficiently. If the irradiation dose is greater than 100 kGy, the first optical film and the second optical film may be damaged, resulting in a decrease in mechanical strength and yellowing, making it impossible to obtain the desired optical properties.

[0103] Electron beam irradiation is usually performed in an inert gas atmosphere, but may be performed in the atmosphere or with a small amount of oxygen introduced if necessary. Depending on the materials of the first and second optical films, by appropriately introducing oxygen, oxygen inhibition is intentionally caused on the surfaces of the first and second optical films that are first hit by the electron beam, thereby preventing damage to the first and second optical films and allowing the electron beam to be efficiently irradiated only on the adhesive.

[0104] When producing the laminated optical film according to the present invention, it is preferable to use active energy rays that include visible light in the wavelength range of 380 nm to 450 nm, and particularly active energy rays that have the highest exposure dose of visible light in the wavelength range of 380 nm to 450 nm. When using ultraviolet and visible light, if a transparent protective film (ultraviolet-opaque transparent protective film) with ultraviolet absorption ability is used as the optical film, light with a wavelength shorter than approximately 380 nm is absorbed, and therefore light with a wavelength shorter than 380 nm does not reach the curable resin composition and does not contribute to its polymerization reaction. Furthermore, light with a wavelength shorter than 380 nm absorbed by the first optical film and the second optical film is converted into heat, causing the first optical film or the second optical film itself to generate heat, resulting in defects such as curling and wrinkling of the laminated optical film. Therefore, when ultraviolet rays and visible light are used in the present invention, it is preferable to use an active energy ray generator that does not emit light with a wavelength shorter than 380 nm. More specifically, the ratio of the integrated illuminance in the wavelength range of 380 to 440 nm to the integrated illuminance in the wavelength range of 250 to 370 nm is preferably 100:0 to 100:50, more preferably 100:0 to 100:40. When producing the laminated optical film according to the present invention, the active energy ray is preferably a gallium-encapsulated metal halide lamp or an LED light source that emits light in the wavelength range of 380 to 440 nm. Alternatively, light sources containing ultraviolet and visible light, such as low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, incandescent lamps, xenon lamps, halogen lamps, carbon arc lamps, metal halide lamps, fluorescent lamps, tungsten lamps, gallium lamps, excimer lasers, or sunlight, can be used. A bandpass filter can also be used to block ultraviolet rays with a wavelength shorter than 380 nm. In order to prevent curling of the laminated optical film while improving the adhesive performance of the adhesive layer between the first optical film and the second optical film, it is preferable to use active energy rays obtained by using a gallium-encapsulated metal halide lamp and passing through a bandpass filter capable of blocking light with wavelengths shorter than 380 nm, or active energy rays with a wavelength of 405 nm obtained by using an LED light source.

[0105] When the laminated optical film according to the present invention is produced on a continuous line, the line speed depends on the curing time of the adhesive composition for laminated optical films, but is preferably 1 to 500 m / min, more preferably 5 to 300 m / min, and even more preferably 10 to 100 m / min. If the line speed is too slow, productivity will be poor or the damage to the first optical film and the second optical film will be too great, making it impossible to produce a laminated optical film that can withstand durability tests and the like. If the line speed is too high, the adhesive composition for laminated optical films will not cure sufficiently, and the desired adhesiveness may not be obtained.

[0106] The laminated optical film according to the present invention may also be provided with an adhesive layer for bonding to other components such as a liquid crystal cell. The adhesive for forming the adhesive layer is not particularly limited, and may be appropriately selected and used, for example, from an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, a rubber-based polymer, or the like. In particular, an acrylic adhesive, which has excellent optical transparency, exhibits adhesive properties such as moderate wettability, cohesion, and adhesiveness, and is excellent in weather resistance, heat resistance, and the like, can be preferably used.

[0107] The adhesive layer can be provided on one or both sides of the laminated optical film according to the present invention as a superimposed layer of layers with different compositions or types. Furthermore, when provided on both sides, the adhesive layers on the front and back of the laminated optical film according to the present invention can have different compositions, types, thicknesses, etc. The thickness of the adhesive layer can be appropriately determined depending on the intended use, adhesive strength, etc., and is generally 1 to 500 μm, preferably 1 to 200 μm, and particularly preferably 1 to 100 μm.

[0108] The exposed surface of the adhesive layer is covered with a temporary separator to prevent contamination until the adhesive layer is put into practical use. This prevents contact with the adhesive layer during normal handling. As the separator, apart from the thickness requirements described above, any suitable conventional separator can be used, such as a suitable thin sheet such as a plastic film, rubber sheet, paper, cloth, nonwoven fabric, net, foam sheet, metal foil, or a laminate thereof, optionally coated with a suitable release agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide-based release agent.

[0109] The laminated optical film according to the present invention can be preferably used to form various devices such as liquid crystal display devices. The formation of a liquid crystal display device can be carried out in a conventional manner. That is, a liquid crystal display device is generally formed by appropriately assembling a liquid crystal cell, a polarizing film or a laminated optical film, and, if necessary, components such as an illumination system, and incorporating a driving circuit. However, in the present invention, there are no particular limitations except for the use of the polarizing film or laminated optical film according to the present invention, and the method can be carried out in a conventional manner. Any type of liquid crystal cell, such as a TN type, STN type, or π type, can be used.

[0110] Appropriate liquid crystal display devices can be formed, such as those in which an optical laminate is disposed on one or both sides of a liquid crystal cell, or those in which a backlight or reflector is used in the illumination system. In such cases, the optical laminate according to the present invention can be disposed on one or both sides of the liquid crystal cell. When optical laminates are disposed on both sides, they may be the same or different. Furthermore, when forming a liquid crystal display device, appropriate components such as a diffuser, anti-glare layer, anti-reflection film, protective plate, prism array, lens array sheet, light diffuser, backlight, etc. can be disposed in one or more layers at appropriate positions.

[0111] Examples of the present invention will be described below, but the embodiments of the present invention are not limited to these.

[0112] (Preparation of adhesive composition for laminated optical films) According to the recipe shown in Table 1, the components shown below were mixed and stirred at 50°C for 1 hour to obtain adhesive compositions for laminated optical films used in Examples 1 to 8 and Comparative Examples 1 and 2. The values ​​in the table indicate weight percentages when the total amount of the composition is taken as 100 mass%.

[0113] The materials constituting the adhesive composition for laminated optical films are shown below. (i) Metal oxide particles Zirconia Dispersion 1: phenoxybenzyl acrylate dispersion of zirconium oxide having an average particle size of 100 nm (particle concentration 50% by weight) Zirconia Dispersion 2: phenoxybenzyl acrylate dispersion of zirconium oxide having an average particle size of 20 nm (particle concentration 50% by weight) Zirconia Dispersion 3: phenoxybenzyl acrylate dispersion of zirconium oxide having an average particle size of 8 nm (particle concentration 50% by weight) Zirconia Dispersion 4: phenoxydiethylene glycol acrylate dispersion of zirconium oxide having an average particle size of 8 nm (particle concentration 50% by weight) Zirconia Dispersion 5: phenoxyethyl acrylate dispersion of zirconium oxide having an average particle size of 8 nm (particle concentration 50% by weight) Titania Dispersion 1: phenoxybenzyl acrylate dispersion of titanium oxide having an average particle size of 20 nm (particle concentration 30% by weight) (ii) (meth)acrylates containing an aromatic ring skeleton Phenoxybenzyl acrylate: trade name "Light Acrylate POB-A", manufactured by Kyoeisha Chemical Co., Ltd. Phenoxyethyl acrylate: trade name "Light Acrylate PO-A", manufactured by Kyoeisha Chemical Co., Ltd. (iii) Curable components Compound represented by general formula (1) (3-methacrylamidophenylboronic acid): trade name "MAPBA", manufactured by Junsei Chemical Co., Ltd. Hydroxyl group-containing (meth)acrylate (4-hydroxybutyl acrylate): trade name "4HBA", manufactured by Mitsubishi Chemical Corporation Acryloylmorpholine: trade name "ACMO", manufactured by KJ Chemicals Co., Ltd. Multifunctional radical polymerizable compound (tripropylene glycol diacrylate): trade name "Aronix M-220", manufactured by Toagosei Co., Ltd. (iv) Leveling agent (a leveling agent containing a modified isocyanurate compound having a (meth)acryloyl group and a modified polysiloxane compound having a (meth)acryloyl group): Trade name "BYK UV-3505", manufactured by BYK Corporation. (v) Acrylic oligomer obtained by polymerizing (meth)acrylic monomers: Trade name "ARUFON UP-1190", manufactured by Toagosei Co., Ltd. (vi) Photopolymerization initiator Photopolymerization initiator 1 (bis(2,4,Photopolymerization initiator 1 (1-hydroxycyclohexylphenyl ketone): trade name "Omnirad 184" manufactured by IGM Resins B.V. Photopolymerization initiator 2 (1-hydroxycyclohexylphenyl ketone): trade name "Omnirad 184" manufactured by IGM Resins B.V. Photopolymerization initiator 3 (diethylthioxanthone): trade name "KAYACURE DETX-S" manufactured by Nippon Kayaku Co., Ltd. The above-mentioned zirconia dispersions 1 to 5 and titania dispersion 1 were produced by the following methods.

[0114] (Synthesis of Dispersant A) 415 g (1 mol) of tristyrenated phenol and 1 g (0.018 mol) of potassium hydroxide were charged into an autoclave and mixed uniformly. 352 g (8 mol) of ethylene oxide (EO) was added dropwise to the reaction system at 130°C. After the dropwise addition of ethylene oxide was completed, the pressure was maintained at 0.1 MPa and the mixture was aged for 1 hour at 130°C, yielding an adduct of 8 mols of EO with tristyrenated phenol.

[0115] 767 g (1 mol) of the above tristyrenated phenol EO 8 mol adduct and 152 g (1.3 mol) of sodium monochloroacetate were placed in a reactor and stirred until uniform. Next, 52 g of sodium hydroxide was added under conditions of a reaction system of 60 ° C, and the temperature was raised to 80 ° C and aged for 3 hours. After aging, the mixture was cooled to 50 ° C, and 117 g (1.2 mol) of 98% sulfuric acid was added dropwise at the same temperature to obtain a white suspension. This white suspension was washed with distilled water, and the solvent was distilled off under reduced pressure to obtain Dispersant A.

[0116] (Preparation of Zirconia Dispersion 1) An aqueous dispersion of zirconium oxide (manufactured by Sigma-Aldrich, average particle size 100 nm, zirconium oxide solids concentration: 10%) was concentrated using an ultrafiltration membrane, and an amount of methanol equal to the amount of the filtrate obtained was added to the resulting concentrated dispersion. The concentration of the dispersion and dilution with methanol were continuously and simultaneously performed in parallel, thereby replacing the dispersion medium from water with methanol while maintaining the zirconium oxide particle concentration in the dispersion at 10 wt %, thereby obtaining a zirconium oxide particle concentration of 10 wt %. To 100 parts of the resulting methanol dispersion of zirconium oxide, 0.5 parts of Dispersant A and 9.5 parts of m-phenoxybenzyl acrylate (manufactured by Kyoeisha Chemical Industry, trade name "Light Acrylate POB-A"; hereinafter referred to as "POB-A") were added and mixed. The solvent was then removed under reduced pressure using a rotary evaporator, yielding Zirconia Dispersion 1, a zirconium oxide monomer dispersion. The zirconia dispersion A contained zirconium oxide / dispersant A / POB-A in a weight ratio of 50 / 2.5 / 47.5.

[0117] (Preparation of Zirconia Dispersion 2) 1.5 parts of Dispersant A and 28.5 parts of m-phenoxybenzyl acrylate (manufactured by Kyoeisha Chemical Industries, Ltd., trade name "Light Acrylate POB-A"; hereinafter referred to as "POB-A") were added to and mixed with 100 parts of a methyl ethyl ketone dispersion of zirconium oxide (manufactured by Nissan Chemical Industries, Ltd., grade name "OZ-S40K-AC," average particle size (D50) measured by dynamic light scattering: 20 nm, zirconium oxide solids concentration: 30%). The solvent was then removed under reduced pressure using a rotary evaporator to obtain Zirconia Dispersion 2, a zirconium oxide monomer dispersion. This Zirconia Dispersion A contained zirconium oxide / Dispersant A / POB-A in a weight ratio of 50 / 2.5 / 47.5.

[0118] (Preparation of Zirconia Dispersion 3) 1.5 parts of Dispersant A and 28.5 parts of m-phenoxybenzyl acrylate (manufactured by Kyoeisha Chemical Industry Co., Ltd., trade name "Light Acrylate POB-A"; hereinafter referred to as "POB-A") were added to and mixed with 100 parts of a methanol dispersion of zirconium oxide (manufactured by Sakai Chemical Industry Co., Ltd., grade name "SZR-CM," average particle size (D50) determined by dynamic light scattering: 8 nm, zirconium oxide solids concentration: 30%). The solvent was then removed under reduced pressure using a rotary evaporator to obtain Zirconia Dispersion A, which is a monomer dispersion of zirconium oxide. This Zirconia Dispersion 3 contained zirconium oxide / Dispersant A / POB-A in a weight ratio of 50 / 2.5 / 47.5.

[0119] (Preparation of Zirconia Dispersion 4) 1.5 parts of Dispersant A and 28.5 parts of phenoxydiethylene glycol acrylate (manufactured by Kyoeisha Chemical Industry Co., Ltd., trade name "Light Acrylate P2H-A"; hereinafter referred to as "P2H-A") were added to 100 parts of a methanol dispersion of zirconium oxide (manufactured by Sakai Chemical Industry Co., Ltd., grade name "SZR-CM", average particle size (D50) based on dynamic light scattering: 8 nm, zirconium oxide solids concentration: 30%) and mixed. Next, the solvent was removed under reduced pressure using a rotary evaporator to obtain Zirconia Dispersion 4, which is a monomer dispersion of zirconium oxide. This Zirconia Dispersion A contained zirconium oxide / Dispersant A / P2H-A in a weight ratio of 50 / 2.5 / 47.5.

[0120] (Preparation of Zirconia Dispersion 5) 1.5 parts of Dispersant A and 28.5 parts of phenoxyethyl acrylate (manufactured by Kyoeisha Chemical Industry Co., Ltd., trade name "Light Acrylate PO-A"; hereinafter referred to as "PO-A") were added to and mixed with 100 parts of a methanol dispersion of zirconium oxide (manufactured by Sakai Chemical Industry Co., Ltd., grade name "SZR-CM," average particle size (D50) determined by dynamic light scattering: 8 nm, zirconium oxide solids concentration: 30%). The solvent was then removed under reduced pressure using a rotary evaporator to obtain Zirconia Dispersion 5, a zirconium oxide monomer dispersion. This Zirconia Dispersion A contained zirconium oxide / Dispersant A / PO-A in a weight ratio of 50 / 2.5 / 47.5.

[0121] (Preparation of Titania Dispersion 1) 1.5 parts of Dispersant A and 68.5 parts of m-phenoxybenzyl acrylate (manufactured by Kyoeisha Chemical Industries, Ltd., trade name "Light Acrylate POB-A"; hereinafter referred to as "POB-A") were added to and mixed with 100 parts of a methanol dispersion of titanium oxide (manufactured by Nissan Chemical Industries, Ltd., grade name "OT-RA305M7-20," average particle size (D50) measured by dynamic light scattering: 20 nm, titanium oxide solids concentration: 30%). The solvent was then removed under reduced pressure using a rotary evaporator to obtain Zirconia Dispersion A, which is a zirconium oxide monomer dispersion. This Zirconia Dispersion A contained zirconium oxide / Dispersant A / POB-A in a weight ratio of 30 / 1.5 / 68.5.

[0122] The materials constituting the laminated optical film are listed below.

[0123] <Production of Polarizer> A laminate having a 9 μm-thick PVA layer formed on an amorphous PET substrate was subjected to auxiliary in-air stretching at a stretching temperature of 130°C to produce a stretched laminate, the stretched laminate was then dyed to produce a dyed laminate, and the dyed laminate was further stretched integrally with the amorphous PET substrate by stretching in boric acid water at a stretching temperature of 65°C to a total stretch ratio of 5.94 to produce an optical film laminate including a 5 μm-thick PVA layer. This two-stage stretching resulted in highly oriented PVA molecules in the PVA layer formed on the amorphous PET substrate, and an optical film laminate including a 5 μm-thick PVA layer was obtained, which constitutes a thin polarizer in which iodine adsorbed by dyeing was highly oriented in one direction as a polyiodine ion complex.

[0124] <Transparent protective film> "TAC": triacetyl cellulose (TAC) film (product name "TJ25UL", thickness 25 μm, manufactured by Fujifilm Corporation)

[0125] <Photopolymerizable Liquid Crystal Composition> A photopolymerizable liquid crystal compound exhibiting a nematic liquid crystal phase (BASF's "Paliocolor LC242") was dissolved in cyclopentanone to prepare a solution with a solids concentration of 30% by weight. A surfactant (BYK-360, BYK-Chemie) and a photopolymerization initiator (IGM Resins' "Omnirad 907") were added to this solution to prepare a liquid crystal composition solution. The amounts of the leveling agent and polymerization initiator added were 0.01 parts by weight and 3 parts by weight, respectively, relative to 100 parts by weight of the photopolymerizable liquid crystal compound.

[0126] <λ / 2 Retardation Film> A biaxially stretched norbornene film (Zeon Corporation's "ZEONORFILM", thickness: 33 μm, front retardation: 135 nm) was used as a substrate. The liquid crystal composition was applied to the substrate using a bar coater so that the phase difference was λ / 2, and the liquid crystal was aligned by heating at 100° C. for 3 minutes. After cooling to room temperature, the film was irradiated with an integrated light intensity of 400 mJ / cm under a nitrogen atmosphere. 2 The laminate was then photocured by irradiating it with ultraviolet light of 1000 kJ / cm 2 , to obtain a laminate provided with a homogeneously aligned liquid crystal layer.

[0127] <λ / 4 Retardation Film> A biaxially stretched norbornene film (Zeon Corporation's "ZEONORFILM", thickness: 33 μm, front retardation: 135 nm) was used as a substrate. The liquid crystal composition was applied to the substrate using a bar coater so that the phase difference was λ / 4, and the liquid crystal was aligned by heating at 100° C. for 3 minutes. After cooling to room temperature, the film was irradiated with an integrated light intensity of 400 mJ / cm under a nitrogen atmosphere. 2 The laminate was then photocured by irradiating it with ultraviolet light of 1000 kJ / cm 2 , to obtain a laminate provided with a homogeneously aligned liquid crystal layer.

[0128] <Polarizing Film (1)> Polarizing film (1) was coated using an MCD coater (manufactured by Fuji Machinery Co., Ltd.) (cell shape: honeycomb, gravure roll line count: 700 / inch, rotation speed: 140% / line speed) and a corona treatment machine at a treatment density of 50 W·min / m 2 The adhesive composition for a laminated optical film according to Comparative Example 2 was applied to the corona-treated surface of the PVA layer of the polarizer, and the adhesive composition was applied at a treatment density of 50 W·min / m using the same corona treatment machine. 2The corona-treated surface of the TAC film was laminated with a roll machine (the lamination line speed was 15 m / min). Thereafter, a visible light irradiation device (Heraeus Light HAMMER10 Mark III, bulb: V bulb, peak irradiance: 1600 mW / cm) was used from the TAC film side. 2 , cumulative irradiation dose 1000 / mJ / cm 2 The illuminance and cumulative exposure dose of the active energy rays were measured using a Power Puck 2 (manufactured by EIT, UVV measurement values)) to irradiate the adhesive composition for laminated optical films with active energy rays, thereby producing a polarized film (1) in which an amorphous PET substrate, a polarizer, and a TAC film were laminated via a cured layer of the adhesive composition for laminated optical films. The thickness of the cured layer of the adhesive composition for laminated optical films was 1 μm.

[0129] <Polarizing Film (2)> Next, the amorphous PET substrate of the polarizing film (1) was peeled off, and the polarizer surface of the peeled surface was treated with a corona treatment machine at a treatment density of 50 W·min / m 2 The adhesive composition for a laminated optical film according to Comparative Example 2 was applied to the polarizer that had been subjected to the corona treatment using an MCD coater (manufactured by Fuji Machinery Co., Ltd.) (cell shape: honeycomb, gravure roll line count: 700 / inch, rotation speed: 140% / line speed), and the same corona treatment machine was used to apply the adhesive composition at a treatment density of 50 W·min / m 2 The homogeneously aligned liquid crystal layer surface of the λ / 2 retardation film subjected to the corona treatment was laminated to the polarizer by a roller so that the slow axis of the λ / 2 retardation film was in a 15° relationship with the transmission axis of the polarizer (the lamination line speed was 15 m / min). Thereafter, a visible light irradiation device (Heraeus Light HAMMER10 Mark III, bulb: V bulb, peak illuminance: 1600 mW / cm) was used from the λ / 2 retardation film side. 2 , cumulative irradiation dose 1000 / mJ / cm 2The illuminance and cumulative exposure dose of the active energy rays were measured using a Power Puck 2 (manufactured by EIT, UVV measurement values)) to cure the adhesive composition for laminated optical films, thereby producing a polarized film (2) in which a λ / 2 retardation film, a polarizer, and a TAC film were laminated via a cured layer of the adhesive composition for laminated optical films. The thickness of the cured layer of the adhesive composition for laminated optical films was 1 μm.

[0130] (Example of Manufacturing a Laminated Optical Film) The biaxially stretched norbornene-based film of the polarizing film (2) was peeled off, and the λ / 2 retardation film surface on the peeled surface was treated with a corona treatment machine at a treatment density of 50 W·min / m 2 Using an MCD coater (manufactured by Fuji Machinery Co., Ltd.) (cell shape: honeycomb, gravure roll line count: 700 / inch, rotation speed 140% / to line speed), the adhesive compositions for laminated optical films according to Examples 1 to 8 and Comparative Examples 1 and 2, which had the formulations shown in Table 1, were applied to the corona-treated λ / 2 retardation film surface, and then the same corona treatment machine was used to apply the adhesive compositions at a treatment density of 50 W·min / m 2 The homogeneously aligned liquid crystal layer surface of the λ / 4 retardation film subjected to the corona treatment was laminated to the λ / 2 retardation film surface using a roller so that the slow axis of the λ / 4 retardation film was in a 75° relationship with the transmission axis of the polarizer (the lamination line speed was 15 m / min). Thereafter, a visible light irradiation device (Heraeus Light HAMMER10 Mark III, bulb: V bulb, peak illuminance: 1600 mW / cm) was used from the λ / 4 retardation film side. 2 , cumulative irradiation dose 1000 / mJ / cm 2 The illuminance and cumulative exposure dose of the active energy rays were measured using a Power Puck 2 (manufactured by EIT, UVV measurement values)) to irradiate the adhesive compositions for laminated optical films according to Examples 1 to 8 and Comparative Examples 1 and 2 with active energy rays, thereby producing laminated optical films in which a λ / 4 retardation film surface, a λ / 2 retardation film, a polarizer, and a TAC film were laminated via a cured layer of the adhesive composition for laminated optical films. The thickness of the cured layer of the adhesive composition for laminated optical films was 1 μm.

[0131] Details of each evaluation method are as follows.

[0132] <Viscosity of adhesive composition for laminated optical film> The viscosity of the adhesive composition for laminated optical film according to Examples 1 to 8 and Comparative Examples 1 and 2 was measured using an E-type viscometer TVE22LT manufactured by Toki Sangyo Co., Ltd.

[0133] <Measurement of refractive index of adhesive layer> A cycloolefin polymer film (COP film) was coated (100 μm thick) with the adhesive composition for laminated optical films according to Examples 1 to 8 and Comparative Examples 1 and 2, and the same COP film was attached to the coated surface. The coated surface was then irradiated with visible light using an active energy ray irradiation device to obtain a cured product layer (single film) of the adhesive composition for laminated optical films according to Examples 1 to 8 and Comparative Examples 1 and 2. The in-plane refractive index and the refractive index in the thickness direction of the obtained cured product layer were measured using a prism coupler SPA-4000 (manufactured by Cylon Technology), and the average value of these was taken as the average refractive index of the adhesive layer. The measurement temperature was 23° C. and the measurement wavelength was 594 nm.

[0134] <Curing shrinkage of adhesive composition for laminated optical film> The curing shrinkage was measured with a laser displacement meter using a resin curing shrinkage measuring device CUSTRON EU201C (manufactured by Acroedge Co., Ltd.), and the curing shrinkage was calculated by the method described in JP-A 2013-104869.

[0135] <Peel Force Between Laminated Optical Films> The biaxially stretched norbornene film of the laminated optical film was peeled off, and a double-sided tape (No. 500, manufactured by Nitto Denko Corporation) was attached to the λ / 4 retardation film surface. Furthermore, a piece measuring 200 mm x 15 mm was cut out, and a cut was made between the λ / 4 retardation film and the λ / 2 retardation film with a cutter knife. The release film of the double-sided tape was then peeled off, and the adhesive surface was attached to a glass plate. Using an angle-flexible adhesive / film peeling analyzer (VPA-2, manufactured by Kyowa Interface Science Co., Ltd.), the λ / 4 retardation film and the λ / 2 retardation film were peeled off in a 90-degree direction at a peel speed of 20,000 mm / min, and the peel strength (N / 15 mm) was measured.

[0136] <Level of Appearance Defect Caused by Irregularities of Laminated Optical Film> The biaxially stretched norbornene-based film of the laminated optical film was peeled off, and a sample measuring 200 mm x 200 mm was cut out and fixed in a flat state. The visibility of streaks caused by the irregularities was evaluated visually under fluorescent lighting by checking the reflected light on the surface of the λ / 4 retardation film. The evaluation was performed according to the following criteria: 0: Streaks caused by the irregularities were not visible. 1: Streaks caused by the irregularities were almost not visible. 2: Streaks caused by the irregularities were faintly visible. 3: Streaks caused by the irregularities were clearly visible.

[0137] <Interference Unevenness (Room Temperature) of Laminated Optical Film Including Polarizing Film> The biaxially stretched norbornene-based film of the laminated optical film obtained in the Examples and Comparative Examples was peeled off, and a conventional acrylic adhesive was placed on the λ / 4 retardation film side. The laminated optical film was then attached to a V3 reflector (manufactured by NEODIS) via the acrylic adhesive to prepare a test sample. The obtained test sample was visually observed under a three-wavelength fluorescent lamp and evaluated according to the following criteria: 1: No interference unevenness was observed even with careful observation. 2: Slight interference unevenness was observed with careful observation. 3: Slight interference unevenness was observed with normal observation, but to a level that was acceptable for practical use. 4: Interference unevenness was observed to a level that was unacceptable for practical use with normal observation. 5: Significant interference unevenness was observed with normal observation.

[0138] <Interference Unevenness of Laminated Optical Film Including Polarizing Film (After Heating Test)> The biaxially stretched norbornene-based film of the laminated optical film obtained in the Examples and Comparative Examples was peeled off, and a conventional acrylic adhesive was placed on the λ / 4 retardation film side. The laminated optical film was then attached to a V3 reflector (manufactured by NEODIS) via the acrylic adhesive to prepare a test sample. The obtained test sample was heated in a hot air oven at 85°C for 500 hours and allowed to stand for 60 minutes in an environment with a temperature of 23±2°C and a relative humidity of 50±10% RH. After that, the sample was visually observed under a three-wavelength fluorescent lamp and evaluated according to the following criteria: 1: No interference unevenness was observed even with careful observation. 2: Slight interference unevenness was observed with careful observation. 3: Slight interference unevenness was observed with normal observation, but at a level acceptable for practical use. 4: Interference unevenness was observed to an extent unacceptable for practical use with normal observation. 5: Significant interference unevenness was observed with normal observation.

[0139] <Transmittance Change ΔY of Laminated Optical Film Including Polarizing Film (After 85 ° C × 500 h Humidity Durability Test)> The biaxially stretched norbornene film of the laminated optical film obtained in the examples and comparative examples was peeled off, and a conventional acrylic adhesive was placed on the λ / 4 retardation film side. The acrylic adhesive was then bonded to alkali-free glass (trade name: EAGLE XG, manufactured by Corning, thickness 0.7 mm) to obtain a test sample. The obtained test sample was left to stand for 500 hours in a hot air oven at a temperature of 85 ° C., and then left to stand for 60 minutes in an environment at a temperature of 23 ± 2 ° C. and a relative humidity of 50 ± 10% RH, and the single transmittance (ΔY) before and after heating was measured. The single transmittance was measured using a spectrophotometer (manufactured by Murakami Color Research Laboratory Co., Ltd., product name "DOT-3") and evaluated according to the following criteria. The single transmittance is a Y value corrected for visibility using a 2-degree visual field (C light source) according to JIS Z 8701-1982. The measurement wavelength was 380 to 700 nm (in 10 nm increments). The results are shown in Table 1. ΔY (%) = Y500 - Y0 Here, Y0 is the single transmittance of the test sample before heating, and Y500 is the single transmittance of the test sample after heating for 500 hours.

[0140]

[0141]

[0142] It can be seen that, compared to the laminated optical films according to Comparative Examples 1 and 2, in which an adhesive layer is formed using a cured product layer of an adhesive composition for laminated optical films that does not contain metal oxide particles, the laminated optical films according to Examples 1 to 8, in which an adhesive layer is formed using a cured product layer of an adhesive composition for laminated optical films that does contain metal oxide particles, have a well-balanced improvement in the refractive index and adhesive strength of the adhesive layer. In addition, it can be seen that the cured product layers of the adhesive compositions for laminated optical films according to Examples 1 to 8 also have a reduced cure shrinkage. It can be seen that the laminated optical films according to Examples 1 to 8 include polarized films that have at least a polarizer as their optical film, and that the excellent cure shrinkage and adhesive strength of the adhesive layer suppress expansion and shrinkage of the polarizer, thereby suppressing changes in transmittance of the laminated optical films (polarized films) after a heat durability test.

Claims

1. A laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, wherein the adhesive layer is a cured layer of an adhesive composition for laminated optical films that contains a curable component and metal oxide particles.

2. The laminated optical film according to claim 1, wherein the adhesive composition for laminated optical films has a content of the metal oxide particles of 10 to 50 mass % when the total amount of the composition is 100 mass %.

3. The laminated optical film according to claim 1 or 2, wherein the adhesive composition for laminated optical films further contains a (meth)acrylate containing an aromatic ring skeleton.

4. The laminated optical film according to claim 3, wherein the adhesive composition for laminated optical films has a content of the (meth)acrylate containing an aromatic ring skeleton of 30 to 70 mass % when the total amount of the composition is 100 mass %.

5. The laminated optical film according to claim 3 or 4, wherein the (meth)acrylate containing an aromatic ring skeleton contains at least one selected from the group consisting of (meth)acrylates having a polycyclic aromatic ring skeleton and (meth)acrylates having two or more aromatic rings.

6. The laminated optical film according to any one of claims 3 to 5, wherein the (meth)acrylate containing an aromatic ring skeleton is phenoxybenzyl (meth)acrylate.

7. The adhesive composition for laminated optical films further comprises a compound represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent; R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group which may have a substituent, an aryl group, or a heterocyclic group.

8. The laminated optical film according to claim 7, wherein the adhesive composition for laminated optical films contains the compound represented by general formula (1) in an amount of 0.1 to 10 mass % when the total amount of the composition is taken as 100 mass %.

9. The laminated optical film according to any one of claims 1 to 8, wherein the adhesive composition for laminated optical films further contains a hydroxyl group-containing (meth)acrylate.

10. The laminated optical film described in claim 9, wherein the adhesive composition for laminated optical films has a content of the hydroxyl group-containing (meth)acrylate of 1 to 30 mass % when the total amount of the composition is 100 mass %.

11. The laminated optical film according to any one of claims 1 to 10, wherein the adhesive composition for laminated optical films further contains a leveling agent containing at least one compound selected from the group consisting of an isocyanurate compound and a polysiloxane compound.

12. The laminated optical film according to claim 11, wherein the adhesive composition for laminated optical films has a content of the isocyanurate compound of 0.05 to 10 mass % when the total amount of the composition is taken as 100 mass %.

13. The laminated optical film according to claim 11 or 12, wherein the adhesive composition for laminated optical films has a polysiloxane compound content of 0.05 to 2.0 mass % when the total amount of the composition is 100 mass %.

14. The laminated optical film according to any one of claims 1 to 13, wherein the adhesive composition for laminated optical films has a viscosity of 100 mPa·s or less at 25°C.

15. The laminated optical film according to any one of claims 1 to 14, comprising at least a polarizer as an optical film.

16. A method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, comprising: a coating step of applying an adhesive composition for laminated optical films to one or both of a bonding surface of the first optical film and a bonding surface of the second optical film; a laminating step of laminating the first optical film and the second optical film; and a bonding step of bonding the first optical film and the second optical film via the adhesive layer formed by irradiating active energy rays from the first optical film side or the second optical film side to cure at least the adhesive composition for laminated optical films, wherein the adhesive composition for laminated optical films contains a curable component and metal oxide particles.

Citation Information

Patent Citations

  • Active energy ray-curable resin composition, cured product thereof, and lens sheet

    JP2017128688A

  • Method for manufacturing polarization film

    JP2020160408A

  • Manufacturing method for polarizing film

    JP2021039269A

  • Optical member, production method, polarizing plate composite, and liquid crystal display device