The optical laminate configuration with controlled adhesive force and evaluation methods addresses the challenge of measuring optical properties in VR goggles, enhancing visibility by ensuring accurate lamination and evaluation of optical members.

WO2024247837A1PCT designated stage expired Publication Date: 2024-12-05NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018787
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Measuring the optical properties of optical laminates used in VR goggles is challenging due to the complexity of stacked optical members, which affects visibility improvements in these devices.

Method used

An optical laminate configuration is developed, comprising a first optical member, a polarizing member, and a second optical member, laminated with an adhesive force of 25N/25mm or less, potentially including a protective member with an antireflection function, and a method for manufacturing and evaluating these laminates to ensure satisfactory optical property measurement.

Benefits of technology

The solution allows for effective measurement and improvement of optical properties in VR goggles, enhancing visibility by ensuring accurate lamination and evaluation of optical members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018787_05122024_PF_FP_ABST
    Figure JP2024018787_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an optical laminate for which optical characteristics can be favorably measured. The optical laminate comprises, in the following order: a first optical member having an optical axis; a polarizing member; and a second optical member having an optical axis. The first optical member is laminated through an adhesive layer to the polarizing member side with an adhesive force of 25 N / 25 mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Optical laminate, method for manufacturing optical laminate, and method for evaluating optical laminate

[0001] The present invention relates to an optical laminate, a method for producing an optical laminate, and a method for evaluating an optical laminate.

[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices), are rapidly becoming popular. In image display devices, optical components such as polarizing components and phase difference components are generally used to realize image display and improve image display performance (see, for example, Patent Document 1).

[0003] In recent years, new applications of image display devices have been developed. For example, goggles with displays (VR goggles) for realizing virtual reality (VR) have begun to be commercialized. Applications of VR goggles in various situations are being considered, and improved visibility is desired.

[0004] Japanese Patent Application Laid-Open No. 2021-103286

[0005] In VR goggles, for example, a large number of optical elements may be used to improve visibility. These optical elements may be pre-stacked (as an optical laminate) and installed inside the VR goggles. However, it may be difficult to measure the optical properties of the optical laminate.

[0006] In view of the above, one object of the present invention is to provide an optical laminate that allows for good measurement of optical properties.

[0007] 1. An optical laminate according to an embodiment of the present invention includes a first optical member having an optical axis, a polarizing member, and a second optical member having an optical axis, in this order, and the first optical member is laminated to the polarizing member side via an adhesive layer with an adhesive strength of 25 N / 25 mm or less. 2. The optical laminate described in 1 above may further include a protective member. The protective member may be disposed on the side of the first optical member or the second optical member where the polarizing member is not disposed. The protective member may be a laminate film having a substrate and a surface treatment layer. 3. In the optical laminate described in 2 above, the surface treatment layer of the laminate film may have an anti-reflection function. 4. In the optical laminate described in any one of 1 to 3 above, the adhesive layer may be formed from a pressure-sensitive adhesive composition containing a (meth)acrylic polymer. 5. In the optical laminate described in any one of 1 to 4 above, the first optical member or the second optical member may be disposed adjacent to a display element main body.

[0008] 6. A method for manufacturing an optical laminate according to an embodiment of the present invention includes preparing a first laminate including a first optical member having an optical axis and a polarizing member, performing a first measurement on the first laminate to obtain a first evaluation result, laminating a second optical member having an optical axis on the polarizing member side to obtain a second laminate, and performing a second measurement on the second laminate to obtain a second evaluation result. 7. In the manufacturing method described in item 6 above, the second measurement may be performed on the second laminate cut to a desired shape. 8. In the manufacturing method described in item 6 or 7 above, the second measurement may be performed in a state in which the first optical member has been peeled from the second laminate. 9. In the manufacturing method described in item 8 above, the peel force when peeling the first optical member from the second laminate may be 25 N / 25 mm or less. 10. The manufacturing method described in any one of items 6 to 9 above may further include obtaining a third evaluation result from the first evaluation result and the second evaluation result.

[0009] 11. An evaluation method according to an embodiment of the present invention is a method for evaluating an optical laminate comprising, in this order, a first optical member having an optical axis, a polarizing member, and a second optical member having an optical axis, the method comprising: performing a first measurement on a first laminate comprising the first optical member and the polarizing member to obtain a first evaluation result; and performing a second measurement on a second laminate comprising the polarizing member and the second optical member to obtain a second evaluation result. 12. The evaluation method described in 11 above may further comprise obtaining a third evaluation result from the first evaluation result and the second evaluation result.

[0010] According to the optical laminate according to the embodiment of the present invention, the optical properties can be measured satisfactorily.

[0011] 3A is a schematic diagram showing a general configuration of a display system of VR goggles according to one embodiment of the present invention; FIG. 3B is a schematic cross-sectional diagram showing a general configuration of an optical laminate according to one embodiment of the present invention; FIG. 3C is a diagram showing a manufacturing process of an optical laminate according to one embodiment; FIG. 3D is a diagram continuing from FIG. 3A; FIG. 3B is a diagram continuing from FIG. 3C; and FIG. 3D is a diagram seen from above of a second laminate according to one embodiment; FIG. 3C is a diagram showing a modified example of a first measurement; and FIG. 3D is a diagram showing a modified example of a second measurement.

[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In order to clarify the description, the drawings may schematically show the width, thickness, shape, etc. of each part compared to the embodiments, but these are merely examples and do not limit the interpretation of the present invention. Furthermore, in the drawings, the same or equivalent elements are given the same reference numerals, and redundant explanations may be omitted.

[0013] (Definition of Terms and Symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive Index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the in-plane direction perpendicular to the slow axis (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-Plane Retardation (Re) "Re(λ)" is the in-plane retardation measured with light having a wavelength of λ nm at 23°C. For example, "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C. Re(λ) is calculated by the formula: Re(λ) = (nx - ny) × d, where d (nm) is the thickness of the layer (film). (3) Thickness Direction Retardation (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light having a wavelength of λ nm at 23°C. For example, "Rth(550)" is the retardation in the thickness direction measured with light having a wavelength of 550 nm at 23°C. Rth(λ) is calculated by the formula: Rth(λ) = (nx - nz) x d, where d (nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz = Rth / Re. (5) Angle When an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise angles relative to the reference direction. Therefore, for example, "45°" means ±45°.

[0014] A. Display System FIG. 1 is a schematic diagram showing the overall configuration of a display system for VR goggles according to one embodiment of the present invention. FIG. 1 schematically illustrates the arrangement and shape of each component of a display system 2. The display system 2 includes a display element 12, a reflective polarizing element 14, a first lens unit 16, a half mirror 18, a first phase difference element 20, a lens unit phase difference element 22, and a second lens unit 24. The reflective polarizing element 14 is disposed in front of the display surface 12a of the display element 12 and can reflect light emitted from the display element 12. The first lens unit 16 is disposed on the optical path between the display element 12 and the reflective polarizing element 14, and the half mirror 18 is disposed between the display element 12 and the first lens unit 16. The first phase difference element 20 is disposed on the optical path between the display element 12 and the half mirror 18, and the lens unit phase difference element 22 is disposed on the optical path between the half mirror 18 and the reflective polarizing element 14.

[0015] The half mirror or the components arranged in front of the first lens unit (in the illustrated example, the half mirror 18, the first lens unit 16, the lens unit phase difference member 22, the reflective polarizing member 14, and the second lens unit 24) may be collectively referred to as the lens unit (lens unit 4).

[0016] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12 a for displaying an image. The light emitted from the display surface 12 a passes through, for example, a polarizing member (typically, a polarizing film) that may be included in the display element 12, and is converted into first linearly polarized light.

[0017] The first phase difference member 20 includes a first λ / 4 member that can convert first linearly polarized light incident on the first phase difference member 20 into first circularly polarized light. When the first phase difference member does not include any member other than the first λ / 4 member, the first phase difference member may correspond to the first λ / 4 member. The first phase difference member 20 may be provided integrally with the display element 12.

[0018] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflective polarizing member 14 back toward the reflective polarizing member 14. The half mirror 18 is provided integrally with the first lens portion 16.

[0019] The lens portion phase difference member 22 includes a second λ / 4 member that can transmit light reflected by the reflective polarizing member 14 and the half mirror 18 through the reflective polarizing member 14. When the lens portion phase difference member does not include any member other than the second λ / 4 member, the lens portion phase difference member can correspond to the second λ / 4 member. The lens portion phase difference member 22 may be provided integrally with the first lens portion 16.

[0020] The first circularly polarized light emitted from the first λ / 4 element included in the first phase difference element 20 passes through the half mirror 18 and the first lens portion 16, and is converted into the second linearly polarized light by the second λ / 4 element included in the lens portion phase difference element 22. The second linearly polarized light emitted from the second λ / 4 element is reflected toward the half mirror 18 without passing through the reflective polarizing element 14. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarizing element 14 is the same as the reflection axis of the reflective polarizing element 14. Therefore, the second linearly polarized light incident on the reflective polarizing element 14 is reflected by the reflective polarizing element 14.

[0021] The second linearly polarized light reflected by the reflective polarizing element 14 is converted into second circularly polarized light by the second λ / 4 element included in the lens portion phase difference element 22, and the second circularly polarized light output from the second λ / 4 element passes through the first lens portion 16 and is reflected by the half mirror 18. The second circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16 and is converted into third linearly polarized light by the second λ / 4 element included in the lens portion phase difference element 22. The third linearly polarized light is transmitted through the reflective polarizing element 14. At this time, the polarization direction of the third linearly polarized light incident on the reflective polarizing element 14 is the same as the transmission axis of the reflective polarizing element 14. Therefore, the third linearly polarized light incident on the reflective polarizing element 14 is transmitted through the reflective polarizing element 14.

[0022] The light transmitted through the reflective polarizing member 14 passes through the second lens portion 24 and enters the user's eye 26 .

[0023] For example, the absorption axis of the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member 14 may be disposed approximately parallel to each other or approximately perpendicular to each other. The angle formed between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the first λ / 4 member included in the first retardation member 20 is, for example, 40° to 50°, may be 42° to 48°, or may be approximately 45°. The angle formed between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the second λ / 4 member included in the lens portion retardation member 22 is, for example, 40° to 50°, may be 42° to 48°, or may be approximately 45°.

[0024] The in-plane retardation Re(550) of the first λ / 4 component is, for example, 100 nm to 190 nm, or may be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The first λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The first λ / 4 component preferably satisfies the relationship Re(450)<Re(550)<Re(650). The Re(450) / Re(550) of the first λ / 4 component may be, for example, 0.75 or more and less than 1, or 0.8 or more and 0.95 or less.

[0025] The in-plane retardation Re(550) of the second λ / 4 component is, for example, 100 nm to 190 nm, or may be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The second λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The second λ / 4 component preferably satisfies the relationship Re(450)<Re(550)<Re(650). The Re(450) / Re(550) of the second λ / 4 component may be, for example, 0.75 or more and less than 1, or 0.8 or more and 0.95 or less.

[0026] Although not shown, the display system 2 may also include an absorptive polarizer disposed in front of the reflective polarizer 14. The reflection axis of the reflective polarizer and the absorption axis of the absorptive polarizer may be disposed approximately parallel to each other.

[0027] B. Optical Stack The optical stack according to the embodiment of the present invention may include, for example, the optical elements included in the display system. Specifically, the optical stack may include a polarizing element (e.g., a reflective polarizing element, an absorptive polarizing element), a retardation element such as a λ / 4 element, an optical element such as a protective element, and an adhesive layer for integrating adjacent elements.

[0028] FIG. 2 is a schematic cross-sectional view showing the overall configuration of an optical laminate according to an embodiment of the present invention. The optical laminate 100 includes a polarizing member 12b, a first phase difference member 20 disposed on one side of the polarizing member 12b, and a second phase difference member 30 disposed on the other side of the polarizing member 12b. The polarizing member 12b may correspond to a polarizing member that may be included in the display element (display element 12). The second phase difference member 30 may correspond to a phase difference member that may be included in the display element 12. For example, the second phase difference member 30 includes a λ / 4 member. The angle between the absorption axis of the polarizing member 12b and the slow axis of the λ / 4 member included in the second phase difference member 30 is, for example, 40° to 50°, or may be 42° to 48°, or may be approximately 45°. When the display element 12 is an organic EL display, providing a λ / 4 member together with the polarizing member 12b can solve problems such as external light reflection and background glare caused by metal layers that may be included in the organic EL display. In addition, it is possible to solve the problem of reflection due to light leakage from the display element 12 in the display system 2. When the second phase difference member 30 does not include any member other than the λ / 4 member, the second phase difference member 30 can correspond to the λ / 4 member.

[0029] The polarizing member 12b and the first phase difference member 20 are laminated via an adhesive layer 41. The polarizing member 12b and the second phase difference member 30 are laminated via an adhesive layer 42. An adhesive layer (e.g., a pressure-sensitive adhesive layer) 40 is provided on the side of the second phase difference member 30 on which the polarizing member 12b is not arranged. The adhesive layer 40 enables the optical laminate 100 to be attached to the main body of the display element 12 (e.g., an organic EL panel). A protective member 50 is provided on the side of the first phase difference member 20 on which the polarizing member 12b is not arranged. The first phase difference member 20 and the protective member 50 are laminated via an adhesive layer 43.

[0030] The first λ / 4 member included in the first phase difference member 20 preferably has a refractive index characteristic that satisfies the relationship nx>ny≧nz. Here, "ny=nz" does not only include the case where ny and nz are completely equal, but also includes the case where they are substantially equal. Therefore, there may be cases where ny<nz. The Nz coefficient of the first λ / 4 member is preferably 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3. The first phase difference member 20 may have an optical axis. Specifically, the first phase difference member 20 may have a slow axis and a fast axis.

[0031] The first λ / 4 member may be made of any suitable material that satisfies the above-mentioned characteristics, and may be, for example, a stretched resin film or an oriented and solidified layer of a liquid crystal compound.

[0032] Examples of resins contained in the resin film include polycarbonate-based resins, polyester carbonate-based resins, polyester-based resins, polyvinyl acetal-based resins, polyarylate-based resins, cyclic olefin-based resins, cellulose-based resins, polyvinyl alcohol-based resins, polyamide-based resins, polyimide-based resins, polyether-based resins, polystyrene-based resins, and acrylic-based resins. These resins may be used alone or in combination. Examples of methods for combining include blending and copolymerization. When the first λ / 4 member exhibits reverse dispersion wavelength characteristics, a resin film containing a polycarbonate-based resin or a polyester carbonate-based resin (hereinafter sometimes simply referred to as a polycarbonate-based resin) can be suitably used.

[0033] Any suitable polycarbonate resin can be used as the polycarbonate resin. For example, the polycarbonate resin contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanols, di-, tri-, or polyethylene glycols, and alkylene glycols or spiroglycols. Preferably, the polycarbonate resin contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, structural units derived from an alicyclic dimethanol and / or structural units derived from di-, tri-, or polyethylene glycol; more preferably, it contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, and structural units derived from di-, tri-, or polyethylene glycol. The polycarbonate resin may contain structural units derived from other dihydroxy compounds as needed. Details of polycarbonate-based resins that can be suitably used for the first λ / 4 member and methods for forming the first λ / 4 member are described, for example, in JP 2014-10291 A, JP 2014-26266 A, JP 2015-212816 A, JP 2015-212817 A, and JP 2015-212818 A, and the descriptions in these publications are incorporated herein by reference.

[0034] The thickness of the first λ / 4 member made of a stretched resin film is, for example, 10 μm to 100 μm, may be 10 μm to 70 μm, or may be 20 μm to 60 μm.

[0035] The above-mentioned liquid crystal compound alignment solidified layer is a layer in which the liquid crystal compound is aligned in a predetermined direction within the layer and the alignment state is fixed. The term "alignment solidified layer" encompasses an alignment solidified layer obtained by curing a liquid crystal monomer, as described below. In the first λ / 4 member, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the first λ / 4 member (homogeneous alignment). Examples of rod-shaped liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The liquid crystal compound is preferably polymerizable. If the liquid crystal compound is polymerizable, the alignment state of the liquid crystal compound can be fixed by aligning the liquid crystal compound and then polymerizing it.

[0036] The alignment and solidification layer of the liquid crystal compound (liquid crystal alignment and solidification layer) can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. Any appropriate alignment treatment can be used as the alignment treatment. Specific examples include mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique vapor deposition and photoalignment treatment. Any appropriate treatment conditions can be used for the various alignment treatments depending on the purpose.

[0037] The alignment of liquid crystal compounds is achieved by treating them at a temperature at which they exhibit a liquid crystal phase depending on the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compounds assume a liquid crystal state and are aligned in accordance with the alignment treatment direction of the substrate surface.

[0038] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.

[0039] Any suitable liquid crystal polymer and / or liquid crystal monomer can be used as the liquid crystal compound. The liquid crystal polymer and the liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for producing a liquid crystal alignment solidified layer are described in, for example, JP 2006-163343 A, JP 2006-178389 A, and WO 2018 / 123551 A. The descriptions in these publications are incorporated herein by reference.

[0040] The thickness of the first λ / 4 member constituted by the liquid crystal alignment solidified layer is, for example, 1 μm to 10 μm, or may be 1 μm to 8 μm, 1 μm to 6 μm, or 1 μm to 4 μm.

[0041] The polarizing member 12b may include, for example, a resin film containing a dichroic material (sometimes referred to as an absorptive polarizing film). The polarizing member 12b typically includes at least an absorptive polarizing film, and may be configured by laminating a protective layer on one or both sides of the absorptive polarizing film via an adhesive layer. The thickness of the absorptive polarizing film is, for example, from 1 μm to 20 μm, and may be from 2 μm to 15 μm, 12 μm or less, 10 μm or less, 8 μm or less, or 5 μm or less.

[0042] The absorptive polarizing film may be made from a single layer of resin film or may be made from a laminate of two or more layers.

[0043] When the absorptive polarizing film is produced from a single-layer resin film, for example, an absorptive polarizing film can be obtained by subjecting a hydrophilic polymer film such as a polyvinyl alcohol (PVA)-based film, a partially formalized PVA-based film, or a partially saponified ethylene-vinyl acetate copolymer-based film to a dyeing treatment with iodine or a dichroic substance such as a dichroic dye, a stretching treatment, etc. Among these, an absorptive polarizing film obtained by dyeing a PVA-based film with iodine and uniaxially stretching it is preferred.

[0044] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment or while dyeing. Alternatively, the PVA-based film may be dyed after stretching. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like.

[0045] Examples of laminates produced using the two or more layer laminate include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, and a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. An absorptive polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced, for example, by applying a PVA-based resin solution to the resin substrate and drying the solution to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer, and then stretching and dyeing the laminate to convert the PVA-based resin layer into an absorptive polarizing film. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically involves immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may optionally include in-air stretching of the laminate at a high temperature (e.g., 95°C or higher) before stretching in the boric acid aqueous solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an auxiliary in-air stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment, in this order. By introducing auxiliary stretching, it is possible to increase the crystallinity of the PVA, even when the PVA is coated on a thermoplastic resin substrate, thereby achieving high optical properties. Furthermore, by simultaneously increasing the orientation of the PVA in advance, problems such as a decrease in orientation or dissolution of the PVA when immersed in water in the subsequent dyeing or stretching steps can be prevented, thereby achieving high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disordering of the polyvinyl alcohol molecules and the decrease in orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the absorptive polarizing film obtained through treatment steps in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment.Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage treatment.The obtained resin substrate / absorptive polarizing film laminate may be used as is (i.e., the resin substrate may be used as a protective layer for the absorptive polarizing film), or any suitable protective layer may be laminated depending on the purpose on the surface obtained by peeling the resin substrate from the resin substrate / absorptive polarizing film laminate or on the surface opposite to the peeled surface. Details of such methods for producing an absorptive polarizing film are described in, for example, JP-A-2012-73580 and Japanese Patent No. 6,470,455. The entire disclosures of these publications are incorporated herein by reference.

[0046] The in-plane retardation Re(550) of the λ / 4 member (sometimes referred to as the third λ / 4 member) included in the second retardation member 30 is, for example, 100 nm to 190 nm, but may also be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The third λ / 4 member preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases depending on the wavelength of the measurement light. The Re(450) / Re(550) of the third λ / 4 member may be, for example, 0.75 or greater but less than 1, or 0.8 or greater but 0.95 or less. The third λ / 4 member preferably exhibits a refractive index characteristic of nx > ny ≧ nz. The Nz coefficient of the third λ / 4 member is preferably 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3. The second phase difference member 30 may have an optical axis. Specifically, the second phase difference member 30 may have a slow axis and a fast axis.

[0047] The third λ / 4 member is formed of any appropriate material that can satisfy the above characteristics. The third λ / 4 member may be, for example, a stretched resin film or an oriented and solidified layer of a liquid crystal compound. The same explanation as for the first λ / 4 member can be applied to a third λ / 4 member formed of a stretched resin film or an oriented and solidified layer of a liquid crystal compound. The first λ / 4 member and the third λ / 4 member may be members having the same configuration (e.g., forming material, thickness, optical properties, etc.) or may be members having different configurations.

[0048] The protective member 50 typically includes a substrate. The substrate may be composed of any appropriate film. Examples of materials that form the main component of the film constituting the substrate include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based, polyvinyl alcohol-based, polycarbonate-based, polyamide-based, polyimide-based, polyethersulfone-based, polysulfone-based, polystyrene-based, cycloolefin-based resins such as polynorbornene, polyolefin-based, (meth)acrylic, and acetate-based resins. The thickness of the substrate is preferably 5 μm to 80 μm, more preferably 10 μm to 50 μm, and even more preferably 15 μm to 40 μm.

[0049] The protective member 50 is preferably a laminated film having a substrate and a surface treatment layer. A protective member having a surface treatment layer can be disposed so that the substrate is located on the first retardation member 20 side. The thickness of the surface treatment layer is, for example, 0.5 μm to 10 μm, or may be 1 μm to 7 μm, or may be 2 μm to 5 μm. The surface treatment layer can have any appropriate function. For example, the surface treatment layer preferably has an anti-reflection function. In this case, the reflectance of the protective member 50 is preferably 5% or less, and more preferably 3% or less. The reflectance can be measured using a spectrophotometer (for example, the "U-4100" manufactured by Hitachi High-Technologies Corporation).

[0050] Although not shown, the optical stack 100 may include another phase difference member having any appropriate refractive index characteristics. For example, the optical stack 100 may include another phase difference member disposed between the polarizing member 12b and the first phase difference member 20. Furthermore, for example, the first phase difference member 20 and / or the second phase difference member 30 may include another phase difference member having any appropriate refractive index characteristics. Specifically, the first phase difference member 20 and / or the second phase difference member 30 may include another phase difference member that satisfies the relationship nz > nx ≧ ny.

[0051] Adjacent members can be laminated together via an adhesive layer. The adhesive layer may be formed of an adhesive or a pressure-sensitive adhesive. Specifically, the adhesive layer may be an adhesive layer or a pressure-sensitive adhesive layer. The thickness of the adhesive layer is, for example, 0.05 μm to 30 μm. In this specification, "adjacent" includes not only being directly adjacent to each other, but also being adjacent to each other via an adhesive layer.

[0052] The optical laminate 100 can be obtained by laminating the constituent members in any appropriate order. In one embodiment, the first phase difference member 20 and the polarizing member 12b are laminated together, and then the second phase difference member 30 is laminated on the polarizing member 12b to obtain the optical laminate 100.

[0053] 3A to 3E are diagrams showing manufacturing steps of an optical laminate according to one embodiment. Fig. 3A shows a state in which a first phase difference member 20 is prepared, on which a protective member 50 is pre-laminated using an adhesive layer 43. Next, the first phase difference member 20 is laminated on a polarizing member 12b via an adhesive layer (e.g., a pressure-sensitive adhesive layer) 41, to obtain a first laminate 101 as shown in Fig. 3B. Here, lamination of the polarizing member 12b and the first phase difference member 20 may be performed in a state in which an adhesive layer 42 has been formed on the polarizing member 12b in advance.

[0054] Next, as shown in FIG. 3C , a first measurement of the optical properties of the first laminate 101 is performed to obtain a first evaluation result. The shape of the first laminate 101 during the first measurement is not particularly limited. Specifically, the shape of the first laminate 101 during the first measurement may be either elongated or sheet-like. For example, a sheet-like test piece obtained by cutting out a portion of the elongated first laminate 101 may be used for the first measurement. The test piece may be, for example, approximately rectangular.

[0055] Examples of measuring devices for the first measurement include a KOBRA manufactured by Oji Scientific Instruments Co., Ltd. and an AxoScan manufactured by Axometrics. The first measurement provides a first evaluation result. The first measurement can evaluate the retardation value (e.g., in-plane retardation) of the first retardation member 20. The first measurement can also evaluate the angle between the absorption axis of the polarizing member 12b and the optical axis (e.g., slow axis, fast axis) of the first retardation member 20. For example, it can be confirmed whether the absorption axis of the polarizing member 12b and the optical axis of the first retardation member 20 form a predetermined angle.

[0056] Next, the second phase difference member 30 is laminated on the polarizing member 12b (first laminate 101) via the adhesive layer 42, thereby obtaining a second laminate 102 (optical laminate 100) as shown in Fig. 3D. Here, the second phase difference member 30 and the polarizing member 12b may be laminated in a state in which the adhesive layer 40 has been formed on the second phase difference member 30 in advance.

[0057] Next, as shown in FIG. 3E , a second measurement of the optical properties of the second laminate 102 is performed to obtain a second evaluation result. During the second measurement, the second laminate 102 is cut into a desired shape (e.g., chipped). A typical example of the desired shape is the shape (sometimes referred to as the final shape) that the second laminate 102 will have when mounted in a final product such as VR goggles. FIG. 4 is a top view of the second laminate 102 according to one embodiment. In the illustrated example, the second laminate 102 has a substantially rectangular shape, with the corners of the rectangle cut out. The second measurement is performed, for example, by aligning the second laminate 102 with a reference portion of a measuring device using the linear portion 102b on the periphery of the second laminate 102. The shape of the second laminate 102 is not limited to this.

[0058] The second measurement may be performed in a state where a part of the first phase difference member 20 is peeled off from the second laminate 102, or may be performed in a state where the entire first phase difference member 20 is peeled off from the second laminate 102. Specifically, the second measurement is performed by aligning a reference part of the measuring device with a laminate portion 102a that includes the polarizing member 12b and the second phase difference member 30 and does not include the first phase difference member 20.

[0059] Examples of measuring devices for the second measurement include a KOBRA manufactured by Oji Scientific Instruments Co., Ltd. and an AxoScan manufactured by Axometrics. The second measurement provides a second evaluation result. The second measurement can evaluate the retardation value (e.g., in-plane retardation) of the second phase difference member 30. The second measurement can also evaluate the angle between the absorption axis of the polarizing member 12b and the optical axis (e.g., slow axis, fast axis) of the second phase difference member 30. For example, it can be confirmed whether the absorption axis of the polarizing member 12b and the optical axis of the second phase difference member 30 form a predetermined angle. Furthermore, the second measurement can evaluate the position and angle of the absorption axis of the polarizing member 12b in the final shape.

[0060] A third evaluation result may be obtained by calculation or the like from the first evaluation result and the second evaluation result. For example, the position and angle of the optical axes of the first phase difference member 20 and the second phase difference member 30 in the final shape can be evaluated from the first evaluation result and the second evaluation result. Specifically, the position and angle of the optical axes of the first phase difference member 20 and the second phase difference member 30 in the final shape can be evaluated from the evaluation results of the angle between the absorption axis of the polarizing member 12b and the optical axis of the first phase difference member 20, the angle between the absorption axis of the polarizing member 12b and the optical axis of the second phase difference member 30, and the position and angle of the absorption axis of the polarizing member 12b in the final shape. Note that the above evaluation result 1, the second evaluation result, and the third evaluation result cannot be obtained by measuring the optical properties (e.g., phase difference value, optical axis) of the finally obtained optical laminate 100 using a measuring device such as KOBRA manufactured by Oji Scientific Instruments Co., Ltd. or AxoScan manufactured by Axometrics.

[0061] The peel force when peeling the first phase difference member 20 from the second laminate 102 is preferably 25 N / 25 mm or less, more preferably 15 N / 25 mm or less. Such a peel force allows for smooth peeling of the first phase difference member 20 and the second measurement. Such a peel force can be achieved, for example, by adjusting the adhesive strength of the adhesive layer disposed between the polarizing member 12 b and the first phase difference member 20. In this case, the adhesive strength of the adhesive layer disposed between the polarizing member 12 b and the first phase difference member 20 to the adjacent member is preferably 25 N / 25 mm or less, more preferably 15 N / 25 mm or less. In the illustrated example, the first phase difference member 20 is peeled from the second laminate 102 at the boundary of the surface of the adhesive layer 41 disposed adjacent to the first phase difference member 20. Specifically, the first phase difference member 20 is preferably laminated to the polarizing member 12 b side (the laminate portion including the polarizing member 12 b) via the adhesive layer 41 with an adhesive strength of 25 N / 25 mm or less.

[0062] The peel force when peeling the first retardation member 20 from the second laminate 102 is preferably 2 N / 25 mm or more. For example, the adhesive strength of the adhesive layer disposed between the polarizing member 12b and the first retardation member 20 to the adjacent member is preferably 2 N / 25 mm or more. The peel force (adhesive strength) can be determined, for example, by measuring the peel force (N / 25 mm) when a sample cut to a size of 25 mm wide and 150 mm long is peeled in the lengthwise direction using a universal tensile tester at a peel rate of 300 mm / min and a peel angle of 90° under an environment of 23±5°C and 50±10% RH.

[0063] A pressure-sensitive adhesive layer can be used as an adhesive layer that can satisfy the above peel strength (adhesion strength). In one embodiment, the adhesive layer that can satisfy the above peel strength (adhesion strength) can be a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing a (meth)acrylic polymer as a base polymer. Here, (meth)acrylic refers to acrylic and / or methacrylic.

[0064] The monomer component constituting the (meth)acrylic polymer is typically a monomer represented by the general formula CH 2 = C(R 1 ) COOR 2 (However, R1 is hydrogen or a methyl group, and R 2 is an alkyl group having 2 to 14 carbon atoms, preferably 3 to 12 carbon atoms, and more preferably 4 to 9 carbon atoms, as a main component.

[0065] General formula CH 2 = C(R 1 ) COOR 2 Examples of the (meth)acrylic monomer represented by the formula (I) include ethyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, Examples of suitable acrylates include acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, isomyristyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and phenoxyethyl (meth)acrylate. Of these, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and the like are preferably used. 2 = C(R 1 ) COOR 2 The (meth)acrylic monomers represented by the formula (I) may be used alone or in combination of two or more.

[0066] In the monomer components constituting the (meth)acrylic polymer, 2 = C(R 1 ) COOR 2 The content of the (meth)acrylic monomer represented by the formula (I) is, for example, 50 to 98% by weight, preferably 60 to 90% by weight, and more preferably 70 to 80% by weight.

[0067] The monomer components constituting the (meth)acrylic polymer preferably further contain a nitrogen-containing monomer. The content of the nitrogen-containing monomer in the monomer components is, for example, 0.1 wt % to 35 wt %, preferably 3 wt % to 30 wt %, and more preferably 5 wt % to 25 wt %. When the content of the nitrogen-containing monomer is within the above range, a pressure-sensitive adhesive layer having excellent durability in a heated environment and / or a high-humidity environment can be obtained.

[0068] The nitrogen-containing monomer is a polymerizable monomer containing one or more nitrogen atoms in the monomer structure, and preferred examples thereof include imide group-containing monomers and amide group-containing monomers. Among these, amide group-containing monomers are more preferred. The content of the amide group-containing monomer in the above-mentioned monomer components is, for example, 3% by weight to 15% by weight, preferably 5% by weight to 10% by weight. The nitrogen-containing monomer may be used alone or in a mixture of two or more types.

[0069] Examples of imide group-containing monomers include N-cyclohexylmaleimide, N-phenylmaleimide, N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-butylmaleimide, and itaconimide.

[0070] Examples of the amide group-containing monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-diethylmethacrylamide, N-isopropyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, dimethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate, diacetone(meth)acrylamide, N-vinylacetamide, N,N'-methylenebis(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and N-vinylcaprolactam.

[0071] Other nitrogen-containing monomers include amino group-containing monomers, (meth)acrylonitrile, N-(meth)acryloylmorpholine, and N-vinyl-2-pyrrolidone.

[0072] The monomer component may contain other polymerizable monomers. Examples of other polymerizable monomers include carboxyl group-containing monomers, sulfonic acid group-containing monomers, phosphate group-containing monomers, vinyl ester monomers, and aromatic vinyl monomers, which can contribute to improving cohesive strength, heat resistance, and the like. Examples of other polymerizable monomers include acid anhydride group-containing monomers, hydroxyl group-containing monomers, epoxy group-containing monomers, and vinyl ether monomers, which can contribute to improving adhesive strength and have functional groups that function as crosslinking base points. These polymerizable monomers may be used alone or in combination of two or more.

[0073] Examples of the carboxyl group-containing monomer include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc. Among these, acrylic acid and methacrylic acid are preferably used.

[0074] Examples of sulfonic acid group-containing monomers include styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid.

[0075] Examples of the phosphate group-containing monomer include 2-hydroxyethyl acryloyl phosphate.

[0076] Examples of vinyl ester monomers include vinyl acetate, vinyl propionate, vinyl laurate, and vinylpyrrolidone.

[0077] Examples of aromatic vinyl monomers include styrene, chlorostyrene, chloromethylstyrene, and α-methylstyrene.

[0078] Examples of the acid anhydride group-containing monomer include maleic anhydride and itaconic anhydride.

[0079] Examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, (4-hydroxymethylcyclohexyl)methyl acrylate, N-methylol (meth)acrylamide, N-hydroxy (meth)acrylamide, vinyl alcohol, allyl alcohol, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether.

[0080] Examples of epoxy group-containing monomers include glycidyl (meth)acrylate and allyl glycidyl ether.

[0081] Examples of vinyl ether monomers include methyl vinyl ether, ethyl vinyl ether, and isobutyl vinyl ether.

[0082] In the above monomer component, the content of the other polymerizable monomers is, for example, 0.1 to 10% by weight, preferably 0.2 to 7% by weight, and more preferably 0.5 to 5% by weight.

[0083] The weight-average molecular weight of the (meth)acrylic polymer is, for example, 600,000 or more, preferably 1.5 million or more, more preferably 1.6 million or more, and even more preferably 1.8 million or more. The weight-average molecular weight of the (meth)acrylic polymer is, for example, 3 million or less, preferably 2.5 million or less. The weight-average molecular weight is measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.

[0084] The pressure-sensitive adhesive composition contains a (meth)acrylic polymer as a base polymer, and preferably further contains a peroxide and an isocyanate crosslinking agent.

[0085] The amount of peroxide to be blended is, for example, 0.02 to 2 parts by weight, preferably 0.04 to 1.5 parts by weight, and more preferably 0.05 to 1 part by weight, relative to 100 parts by weight of the (meth)acrylic polymer. When the amount of peroxide to be blended is within the above range, a PSA layer having excellent durability and adhesiveness can be obtained.

[0086] The amount of the isocyanate crosslinking agent added is, for example, 0.02 to 2 parts by weight, preferably 0.04 to 1.5 parts by weight, and more preferably 0.05 to 1 part by weight, relative to 100 parts by weight of the (meth)acrylic polymer. When the amount of the isocyanate crosslinking agent added is within the above range, a pressure-sensitive adhesive layer having excellent cohesive strength and adhesiveness can be obtained.

[0087] A silane coupling agent may be blended into the pressure-sensitive adhesive composition for the purpose of increasing adhesive strength and durability. The blending amount of the silane coupling agent is, for example, 0.01 to 1 part by weight, preferably 0.02 to 0.6 parts by weight, and more preferably 0.05 to 0.3 parts by weight, per 100 parts by weight of the (meth)acrylic polymer.

[0088] The adhesive strength of the adhesive layer disposed between the polarizing member 12b and the second phase difference member 30 to the member adjacent to the second phase difference member 30 side is, for example, 2 N / 25 mm to 30 N / 25 mm, and preferably 2 N / 25 mm to 25 N / 25 mm. In one embodiment, the adhesive strength of the adhesive layer disposed between the polarizing member 12b and the second phase difference member 30 to the member adjacent to the second phase difference member 30 side may be 15 N / 25 mm or more, or may be 25 N / 25 mm or more. With such a peel force, for example, the first phase difference member 20 can be selectively peeled off during the second measurement.

[0089] In the example shown in FIG. 3 , the first phase difference member 20 and the polarizing member 12b are laminated to obtain the first laminate 101, and then the second phase difference member 30 is laminated on the polarizing member 12b to obtain the second laminate 102. However, this order may be reversed. Specifically, the polarizing member 12b and the second phase difference member 30 may be laminated to obtain the first laminate 101, and then the first phase difference member 20 may be laminated on the polarizing member 12b to obtain the second laminate. In this case, as shown in FIG. 5A , the first measurement may be performed on the first laminate 101 including the polarizing member 12b and the second phase difference member 30. The first measurement may evaluate the retardation value of the second phase difference member 30. The first measurement may also evaluate the angle between the absorption axis of the polarizing member 12b and the optical axis of the second phase difference member 30. 5B , the second measurement can be performed in a state in which the second phase difference member 30 is peeled from the second laminate 102, and the description of the peel force (adhesion force) when peeling the first phase difference member from the second laminate can be applied to the case of peeling the second phase difference member from the second laminate. The second measurement can evaluate the phase difference value of the first phase difference member 20. The second measurement can also evaluate the angle between the absorption axis of the polarizing member 12b and the optical axis of the first phase difference member 20. This modified example is preferable in that, for example, the first phase difference member 20, which may require more strict control of optical properties, is not peeled.

[0090] The present invention will be described in detail below using examples, but the present invention is not limited to these examples. The thickness, retardation value, and peel strength (adhesion strength) were measured using the following measurement methods. Unless otherwise specified, "parts" and "%" are based on weight. <Thickness> Thicknesses of 10 μm or less were measured using a scanning electron microscope (manufactured by JEOL Ltd., product name "JSM-7100F"). Thicknesses exceeding 10 μm were measured using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C"). <Retardation Value> Retardation values ​​at each wavelength at 23°C were measured using a retardation measurement device (KOBRA manufactured by Oji Scientific Instruments Co., Ltd.). <Peel Force> A sample cut into a size of 25 mm wide and 150 mm long was peeled in the longitudinal direction at a peel speed of 300 mm / min and a peel angle of 90° using a universal tensile tester (manufactured by Minebea Co., Ltd., product name: TGI-1kNB), and the peel force (N / 25 mm) was measured under an environment of 23±5°C and 50±10% RH.

[0091] [Example 1] (Preparation of λ / 4 Member) Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and reflux condensers controlled at 100° C. 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19×10 calcium acetate monohydrate as a catalyst. -2 Parts by mass (6.78×10 -5mol) was charged. After purging the reactor with nitrogen under reduced pressure, heating was performed with a heat medium, and stirring was initiated when the internal temperature reached 100°C. 40 minutes after the start of the temperature increase, the internal temperature reached 220°C, and while controlling to maintain this temperature, pressure reduction was initiated. 90 minutes after reaching 220°C, the pressure was reduced to 13.3 kPa. Phenol vapor by-produced during the polymerization reaction was introduced into a reflux condenser at 100°C, and a small amount of monomer components contained in the phenol vapor were returned to the reactor, while uncondensed phenol vapor was introduced into a condenser at 45°C and recovered. Nitrogen was introduced into the first reactor, and the pressure was temporarily restored to atmospheric pressure. The oligomerized reaction liquid in the first reactor was then transferred to the second reactor. Next, heating and pressure reduction in the second reactor were initiated, and the internal temperature reached 240°C and the pressure reached 0.2 kPa in 50 minutes. Polymerization was then allowed to proceed until the predetermined stirring power was achieved. When the predetermined power was reached, nitrogen was introduced into the reactor to restore pressure, and the polyester carbonate resin produced was extruded into water, and the strands were cut to obtain pellets.

[0092] The obtained polyester carbonate resin (pellets) was vacuum dried at 80 ° C for 5 hours, and then a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder set temperature: 250 ° C), a T-die (width 200 mm, set temperature: 250 ° C), a chill roll (set temperature: 120-130 ° C), and a winder was used to produce a long resin film with a thickness of 135 μm. The obtained long resin film was stretched in the width direction at a stretching temperature of 143 ° C and a stretch ratio of 2.8 times to obtain a stretched film with a thickness of 48 μm. The Re (550) of the obtained stretched film was 143 nm, Re (450) / Re (550) was 0.86, and the Nz coefficient was 1.12.

[0093] (Preparation of Protective Member) An antireflection layer-forming material shown below was applied to an acrylic film having a lactone ring structure and heated at 80°C for 1 minute. After heating, the coating layer was irradiated with an integrated light amount of 300 mJ / cm using a high-pressure mercury lamp. 2 The coating layer was cured by irradiation with ultraviolet light of 1000 kJ / cm, to obtain an acrylic film (thickness: 44 μm) on which an antireflection layer having a thickness of 0.1 μm was formed.

[0094] (Antireflection Layer-Forming Material) 100 parts by weight of a polyfunctional acrylate containing pentaerythritol triacrylate as a main component (manufactured by Osaka Organic Chemical Industry Ltd., trade name "Viscoat #300", solid content 100% by weight), 100 parts by weight of hollow nanosilica particles (manufactured by JGC Catalysts and Chemicals Industries, Ltd., trade name "Surulia 5320", solid content 20% by weight, weight average particle diameter 75 nm), 100 parts by weight of solid nanosilica particles (manufactured by Nissan Chemical Industries, Ltd., trade name "MEK-2140Z-AC", solid content 30% by weight, weight average particle diameter 10 nm), 12 parts by weight of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907", solid content 100% by weight) were mixed. To this mixture was added a mixed solvent of tertiary butyl alcohol, methyl isobutyl ketone, and propylene glycol monomethyl ether acetate in a weight ratio of 60:25:15, and the mixture was stirred to give a total solids content of 4% by weight, thereby preparing an anti-reflection layer-forming material.

[0095] (Preparation of Polarizing Member) A long PVA-based resin film having an average degree of polymerization of 2400, a degree of saponification of 99.9 mol%, and a thickness of 30 μm was immersed in warm water at 30°C and uniaxially stretched while swelling to 2.0 times its original length. The film was then immersed in a 0.3 wt% iodine solution (weight ratio: iodine / potassium iodide = 0.5 / 8) at 30°C and dyed while uniaxially stretching to 3.0 times its original length. The PVA-based resin film was then stretched in an aqueous solution of 4 wt% boric acid and 5 wt% potassium iodide to 6 times its original length. The film was then impregnated with iodine ions in an aqueous solution of 3 wt% potassium iodide (iodine impregnation bath) and dried in an oven at 60°C for 4 minutes to obtain a polarizing member having a thickness of 12 μm.

[0096] (Other Retardation Member 1) A positive B plate having a refractive index characteristic of nz>nx>ny was prepared as follows. 48 parts by weight of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "Metolose 60SH-50"), 15,601 parts by weight of distilled water, 8,161 parts by weight of diisopropyl fumarate, 240 parts by weight of 3-ethyl-3-oxetanylmethyl acrylate, and 45 parts by weight of the polymerization initiator t-butyl peroxypivalate were placed in an autoclave equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer. After nitrogen bubbling for 1 hour, the mixture was stirred at 49 ° C. for 24 hours, whereby radical suspension polymerization was carried out. The mixture was then cooled to room temperature, and the suspension containing the resulting polymer particles was centrifuged. The resulting polymer was washed twice with distilled water and twice with methanol, and then dried under reduced pressure to obtain a fumarate ester-based resin. The obtained fumarate ester resin was dissolved in a toluene-methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone 50% by weight / 50% by weight) to obtain a solution with a solids concentration of 20% by weight. Furthermore, 5 parts by weight of tributyl trimellitate as a plasticizer was added to 100 parts by weight of the fumarate ester resin to obtain a dope. A biaxially stretched polyester (polyethylene terephthalate / isophthalate copolymer) film with a thickness of 75 μm and a width of 1350 mm was used as the support film. The rolled support film was set in the unwinding section of a film-forming device, and while the support film was unwound and conveyed downstream, the obtained dope was coated onto the support film to a film thickness of 20 μm after drying and dried at 140°C to obtain a laminate. The obtained laminate was set in the unwinding section of a stretching device, and while the laminate was unwound and conveyed downstream, it was subjected to free-end uniaxial stretching in a stretching furnace at a temperature of 140°C. The support film was peeled off from the stretched laminate to obtain a positive B plate (thickness 5 μm, Re(550): 35 nm, Rth(550): −85 nm).

[0097] (Another Retardation Member 2) A negative B plate having refractive index characteristics of nx>ny>nz was prepared. As the negative B plate, a stretched film of a cycloolefin-based resin film (manufactured by Zeon Corporation, product name: ZT12, thickness: 18 μm, Re(550): 116 nm, Rth(550): 139 nm) was prepared.

[0098] (Preparation of Pressure-Sensitive Adhesive Layer A) A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with a monomer mixture containing 91.5 parts of butyl acrylate, 3 parts of acrylic acid, 0.5 parts of 4-hydroxybutyl acrylate, and 5 parts of acryloylmorpholine. Furthermore, 100 parts of this monomer mixture was charged with 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator along with 100 parts of ethyl acetate. Nitrogen gas was introduced into the flask with gentle stirring to replace the atmosphere with nitrogen, and the liquid temperature in the flask was maintained at around 55°C, allowing the polymerization reaction to proceed for 8 hours. Ethyl acetate was then added to the resulting reaction solution to adjust the solids concentration to 12 wt%, thereby preparing a solution of an acrylic polymer having a weight-average molecular weight (Mw) of 2,500,000. A pressure-sensitive adhesive composition was prepared by blending 0.3 parts of a peroxide-based crosslinking agent, benzoyl peroxide (trade name: Niper BMT, manufactured by NOF Corporation), 0.2 parts of a trimethylolpropane / tolylene diisocyanate adduct (trade name: Coronate L, manufactured by Tosoh Corporation), and 0.2 parts of a silane coupling agent (trade name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.), per 100 parts of the solids content of the obtained acrylic polymer solution. The obtained pressure-sensitive adhesive composition was applied to the release surface of a 38 μm-thick PET film (Mitsubishi Chemical Polyester Film Corporation, MRF38), which was a release liner whose release surface had been silicone-treated, and then dried to form a 5 μm-thick pressure-sensitive adhesive layer A.

[0099] (Preparation of Optical Laminate) The protective member was laminated on one side of the λ / 4 member using an adhesive, and the positive B plate was laminated on the other side via the adhesive layer A. The negative B plate was then laminated on the surface of the positive B plate using an adhesive, and the polarizing member on which an adhesive layer B with a thickness of 5 μm had been formed using an adhesive was then laminated to obtain a first laminate. The λ / 4 member on which an adhesive layer with a thickness of 15 μm had been formed was laminated on the polarizing member side (adhesive layer B) of the obtained first laminate to obtain an optical laminate.

[0100] In the obtained optical laminate, the adhesive strength of the adhesive layer A to the positive B plate was 5 N / 25 mm, and when evaluating the optical properties of the obtained optical laminate, peeling could be easily performed at the surface of the adhesive layer A.

[0101] The present invention is not limited to the above-described embodiment, and various modifications are possible. For example, the configurations shown in the above-described embodiment can be replaced with configurations that are substantially the same as those shown in the above-described embodiment, that have the same effects, or that can achieve the same purpose.

[0102] The coating method according to the embodiment of the present invention is used to produce an optical laminate that can be suitably employed in image display devices such as VR goggles, for example.

[0103] 2 Display system, 4 Lens portion, 12 Display element, 14 Reflective polarizing member, 16 First lens portion, 18 Half mirror, 20 First phase difference member, 22 Lens portion phase difference member, 24 Second lens portion, 28 Absorptive polarizing member, 30 Second phase difference member, 40 Adhesive layer (pressure-sensitive adhesive layer), 41 Adhesive layer, 42 Adhesive layer, 43 Adhesive layer, 50 Protective member, 100 Optical laminate, 101 First laminate, 102 Second laminate.

Claims

1. An optical laminate comprising, in this order, a first optical member having an optical axis, a polarizing member, and a second optical member having an optical axis, the first optical member being laminated to the polarizing member side via an adhesive layer with an adhesive strength of 25 N / 25 mm or less.

2. The optical laminate according to claim 1, further comprising a protective member, the protective member being arranged on the side of the first optical member or the second optical member on which the polarizing member is not arranged, the protective member being a laminated film having a base material and a surface treatment layer.

3. The optical laminate according to claim 2, wherein the surface treatment layer of the laminate film has an anti-reflection function.

4. The optical laminate according to claim 1, wherein the adhesive layer is formed from a pressure-sensitive adhesive composition containing a (meth)acrylic polymer.

5. The optical laminate according to claim 1, wherein the first optical member or the second optical member is disposed adjacent to a display element body.

6. A method for manufacturing an optical laminate, comprising: preparing a first laminate having a first optical element having an optical axis and a polarizing element; performing a first measurement on the first laminate to obtain a first evaluation result; laminating a second optical element having an optical axis on the polarizing element side to obtain a second laminate; and performing a second measurement on the second laminate to obtain a second evaluation result.

7. The method of claim 6, wherein the second measurement is performed on the second laminate that has been cut to a desired shape.

8. The manufacturing method according to claim 6, wherein the second measurement is performed in a state where the first optical member is peeled off from the second laminate.

9. The manufacturing method according to claim 8, wherein a peeling force when peeling the first optical member from the second laminate is 25 N / 25 mm or less.

10. The manufacturing method according to claim 6, further comprising obtaining a third evaluation result from the first evaluation result and the second evaluation result.

11. A method for evaluating an optical laminate comprising, in this order, a first optical member having an optical axis, a polarizing member, and a second optical member having an optical axis, the method comprising: performing a first measurement on a first laminate comprising the first optical member and the polarizing member to obtain a first evaluation result; and performing a second measurement on a second laminate comprising the polarizing member and the second optical member to obtain a second evaluation result.

12. The evaluation method according to claim 11, further comprising obtaining a third evaluation result from the first evaluation result and the second evaluation result.

Citation Information

Patent Citations

  • Polarizing plate integrated with optical compensating layer and liquid crystal display device

    JP1996240716A

  • Polarizing plate with optical compensating layer and image display device using same

    JP2004078171A

  • Retardation film, polarization and retardation plate and display device

    JP2013235207A

  • Antireflection layer-equipped circular polarizing plate and image display device using antireflection layer-equipped circular polarizing plate