Single-crystal lithium niobate, method for producing single-crystal lithium niobate, and ar glasses

By controlling the platinum concentration in lithium niobate single crystals to 1.0 ppm or less during crystal growth, the issue of high light absorption in visible wavelengths is addressed, improving the display quality of augmented reality glasses by reducing color distortion and maintaining accurate image colors.

WO2024247857A1PCT designated stage expired Publication Date: 2024-12-05SUMITOMO METAL MINING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018912
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Lithium niobate single crystals used in waveguides for augmented reality glasses exhibit high light absorption in the visible light range, leading to color distortion of displayed images due to insufficient reduction of light absorption coefficients at specific wavelengths.

Method used

The lithium niobate single crystal is produced with a platinum concentration of 1.0 ppm or less, and the method involves using a platinum-containing crucible for crystal growth, adjusting the platinum content to minimize light absorption coefficients, particularly at 470 nm, thereby reducing the difference between absorption coefficients at 470 nm and 600 nm.

Benefits of technology

This approach results in a lithium niobate single crystal that absorbs little light in the visible wavelength range, effectively reducing color distortion and enhancing the display quality of augmented reality glasses by minimizing the difference in light absorption coefficients, ensuring accurate color representation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018912_05122024_PF_FP_ABST
    Figure JP2024018912_05122024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide single-crystal lithium niobate which absorbs little light having wavelengths in the visible light region. [Solution] This single-crystal lithium niobate has a platinum concentration of 1.0 ppm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium niobate single crystal, method for manufacturing lithium niobate single crystal, and AR glass

[0001] The present invention relates to a lithium niobate single crystal, a method for producing the lithium niobate single crystal, and AR glass.

[0002] The qualities required for waveguide materials used in AR glasses (augmented reality glasses) are (1) a high refractive index, (2) low light absorption in the visible light range, (3) high flatness when processed into wafer form, and (4) low specific gravity.

[0003] The high refractive index of the waveguide material in AR glass allows for a wider field of view (FOV) of the image displayed on the AR glass, enabling a more immersive and realistic image display. Until now, high-refractive-index glass has generally been used as the material for the waveguide in AR glass, but the refractive index of high-refractive-index glass is thought to be limited to around 2.1. Therefore, the possibility of using lithium niobate single crystal, which has a refractive index of 2.2, higher than that of glass, is being investigated.

[0004] Lithium niobate (LiNbO 3 LN single crystals (sometimes abbreviated as LN) are artificial ferroelectric crystals with a melting point of approximately 1250°C and a Curie temperature of approximately 1140°C. LN single crystal substrates, which are cut from LN single crystals and polished, are used primarily as materials for surface acoustic wave elements (SAW filters) installed in mobile communication devices.

[0005] If a waveguide for AR glass absorbs light at wavelengths in the visible light range, the light is attenuated significantly when the image passes through the waveguide through total reflection, resulting in the color of the image displayed on the AR glass differing from the intended image.

[0006] Patent Document 1 discloses a method for producing lithium niobate single crystals that are not used for AR glass but are used for optical elements, and discloses that the oxygen concentration during growth is kept to 5% by volume or less to suppress light absorption at wavelengths around 420 nm.

[0007] Japanese Unexamined Patent Publication No. 1-96095

[0008] It was found that the lithium niobate single crystal produced by the production method described in Patent Document 1 absorbs wavelengths in the visible light region, and the reduction in absorption of wavelengths in the visible light region is still insufficient.

[0009] Therefore, an object of the present invention is to provide a lithium niobate single crystal that absorbs little light with wavelengths in the visible light region.

[0010] As a result of extensive research, the inventors have found that the optical absorption coefficient of lithium niobate single crystal in the vicinity of a wavelength of 470 nm is affected by platinum impurities in the crystal. The present invention was completed based on this finding.

[0011] The lithium niobate single crystal according to an embodiment of the present invention has a platinum concentration of 1.0 ppm or less in the single crystal. Preferably, the lithium niobate single crystal has a platinum concentration of 0.5 ppm or less in the single crystal.

[0012] In addition, the lithium niobate single crystal according to the present invention has a difference in the optical absorption coefficient between a wavelength of 470 nm and a wavelength of 600 nm of 0.01 cm -1 The following is the result.

[0013] Furthermore, the lithium niobate single crystal according to the present invention has a light absorption coefficient of 0.01 cm at a wavelength of 470 nm. -1 It is preferable that:

[0014] Furthermore, the AR glass according to the present invention uses the lithium niobate single crystal according to the above-described embodiment as a waveguide.

[0015] A method for producing a lithium niobate single crystal according to an embodiment of the present invention is a method for producing a lithium niobate single crystal, which includes using a crucible made of a platinum-containing material for growing the single crystal, and adjusting the platinum content of the crucible so that the platinum concentration in the grown single crystal is 1.0 ppm or less.

[0016] According to an aspect of the present invention, it is possible to provide a lithium niobate single crystal that has little absorption of light with wavelengths in the visible light region. Furthermore, according to a method for producing a lithium niobate single crystal of an aspect of the present invention, it is possible to produce the lithium niobate single crystal of an aspect of the present invention. The AR glass of an aspect of the present invention has little absorption of light with wavelengths in the visible light region in a waveguide.

[0017] 1 is a cross-sectional view showing an example of the general configuration of a single crystal growth apparatus using the Czochralski method, and FIG. 2 is a schematic diagram showing measurement of reflectance and transmittance using a spectrophotometer to calculate an absorption coefficient.

[0018] Specific embodiments of the present invention will be described in detail below. Note that the present invention is not limited to the following embodiments and can be modified as appropriate without departing from the spirit of the present invention. In each drawing, some or all of the components are depicted schematically and at different scales as appropriate. To facilitate understanding of the description, the same components in each drawing are denoted by the same reference numerals as much as possible, and redundant description will be omitted. In addition, in the following description, the expression "A to B" means "greater than or equal to A and less than or equal to B."

[0019] [Outline of Single Crystal Growth Apparatus and Single Crystal Growth Method] First, an outline of a single crystal growth apparatus and a single crystal growth method for lithium niobate single crystal will be described. Typical methods for growing lithium niobate single crystals include the Cz method (Czochralski method) and the VB method (Vertical Bridgman method).

[0020] Hereinafter, with reference to FIG. 1, an example of the configuration of a single crystal growth apparatus 10 using the Czochralski method (Cz method) and an overview of the single crystal growth method will be described.

[0021] FIG. 1 is a cross-sectional view showing a schematic configuration of an example of a high-frequency induction heating single crystal growth apparatus. While the example shown in FIG. 1 is a high-frequency induction heating single crystal growth apparatus, resistance heating single crystal growth apparatuses are also used to grow LN single crystals. The difference between a high-frequency induction heating single crystal growth apparatus and a resistance heating single crystal growth apparatus is that in the case of the high-frequency induction heating type, a high-frequency magnetic field generated by a work coil 15 generates eddy currents in the sidewall of a metal crucible 12 placed within the work coil 15. These eddy currents cause the crucible 12 itself to become a heating element, melting the raw materials in the crucible 12 and creating the temperature environment required for crystal growth. In the case of the resistance heating type, heat generated by a resistance heater placed around the crucible melts the raw materials and creates the temperature environment required for crystal growth. Regardless of which heating method is used, the essence of the Cz method remains the same. Therefore, an example of a single crystal growth method using a high-frequency induction heating single crystal growth apparatus will be described below.

[0022] As shown in FIG. 1 , in a high-frequency induction heating single crystal growth apparatus 10, a crucible 12 is placed in a chamber 11. The crucible 12 has a diameter of, for example, 150 mm to 300 mm and a depth of, for example, 150 mm to 300 mm, and is placed on a crucible stand 13 as shown in FIG. 1 . A refractory material 14 is placed in the chamber 11 so as to surround the crucible 12. A work coil 15 is placed so as to surround the crucible 12, and the high-frequency magnetic field generated by the work coil 15 causes eddy currents to flow in the wall of the crucible 12, causing the crucible 12 itself to become a heating element. A pulling shaft (seed rod) 16 is provided at the top of the chamber 11 so as to be rotatable and movable in the vertical direction. A seed holder 17 for holding a seed crystal 1 is attached to the tip of the lower end of the pulling shaft (seed rod) 16.

[0023] In the Cz method, a single crystal piece to become the seed crystal 1 is brought into contact with the surface of the melt of the single crystal raw material 18 in the crucible 12, and this seed crystal 1 is pulled upward while being rotated by a pulling shaft (seed rod) 16, thereby growing a cylindrical single crystal in the same direction as the crystal orientation of the seed crystal 1.

[0024] In the Cz method, the rotation speed and pulling speed of the seed crystal 1 depend on the type of crystal to be grown and the temperature environment during growth, and must be appropriately selected depending on these conditions. Furthermore, during crystal growth, the latent heat of solidification generated by the crystallization of the melt at the growth interface must be released upward through the seed crystal, so the crystal must be grown under a temperature gradient in which the temperature decreases upward from the growth interface. Additionally, to prevent the shape of the grown crystal from bending or twisting, the raw material melt must also be grown under a temperature gradient in which the temperature increases horizontally from the growth interface toward the crucible wall and vertically from the growth interface toward the crucible bottom.

[0025] When growing an LN single crystal, a crucible 12 made of chemically stable platinum (Pt) with a melting point of approximately 1760°C is used because the melting point of LN crystal is 1250°C. The pulling rate during growth is generally several mm / hour, and the rotation speed is several to several tens of rpm (e.g., 3 rpm to 10 rpm). The furnace atmosphere during growth is typically air or a nitrogen-oxygen mixed gas atmosphere with an oxygen concentration of approximately 20%. After growing a crystal to a desired size under these conditions, the grown crystal is separated from the melt by changing the pulling rate or gradually increasing the melt temperature. The power of the growth furnace is then reduced at a predetermined rate to allow for slow cooling. Once the furnace temperature reaches approximately room temperature, the crystal is removed from the growth furnace.

[0026] Crystals grown in this way and removed from the furnace are subjected to an annealing process to remove residual strain caused by temperature differences within the crystal, and a poling process to align the direction of spontaneous polarization within the crystal, before being delivered to the substrate processing process, where they are sliced, polished, etc.

[0027] The method for manufacturing LN single crystals described above is a method for manufacturing LN single crystals used as materials for surface acoustic wave elements (SAW filters). When LN single crystals manufactured by this manufacturing method are used as waveguide materials for AR glass, it has been found that the LN single crystals manufactured as described above have a light absorption peak at a specific wavelength in the visible light range, and when an image passes through the waveguide via total reflection, light attenuation at that specific wavelength increases, resulting in a problem in which the color of the image displayed on the AR glass differs from the intended image. When using LN single crystals as waveguide materials for AR glass, it is particularly important to reduce the difference between the light absorption coefficient at wavelengths of 470 nm and 600 nm in the visible light range.

[0028] While conducting research to solve the above problems, the inventors investigated the difference in the optical absorption coefficient of LN single crystal between wavelengths of 470 nm and 600 nm and the influence of impurities in the crystal, and found that there is a correlation with platinum (Pt). The inventors also discovered that the optical absorption coefficient of LN single crystal near wavelength 470 nm is influenced by platinum (Pt) impurities in the crystal. The LN single crystal and its manufacturing method according to this embodiment were completed through further research based on these findings.

[0029] The LN single crystal according to this embodiment is described below. The LN single crystal according to this embodiment is characterized in that the platinum (Pt) concentration (content) in the single crystal is 1.0 ppm or less. Furthermore, the LN single crystal according to this embodiment has a difference in the optical absorption coefficient between the wavelength of 470 nm and the wavelength of 600 nm of 0.01 cm. -1 The LN single crystal according to one aspect of this embodiment is characterized in that it has a light absorption coefficient of 0.01 cm at a wavelength of 470 nm. -1 The present invention is characterized by the following:

[0030] As shown in Table 1, which will be described later, the LN single crystal according to this embodiment can significantly reduce the difference between the optical absorption coefficient at wavelengths of 470 nm and 600 nm by suppressing the platinum (Pt) concentration, thereby significantly reducing the optical absorption coefficient at a wavelength of 470 nm.

[0031] In the LN single crystal of this embodiment, the upper limit of the platinum (Pt) concentration is preferably 1.0 ppm or less, more preferably 0.9 ppm or less, more preferably 0.8 ppm or less, more preferably 0.5 ppm or less, more preferably 0.4 ppm or less, and more preferably 0.3 ppm or less. In the LN single crystal, the upper limit of the difference between the optical absorption coefficient at a wavelength of 470 nm and the optical absorption coefficient at a wavelength of 600 nm is 0.01 cm. -1 Preferably less than 0.008 cm -1 More preferably, 0.005 cm or less -1 More preferably, it is 0.004 cm or less. -1 The following is more preferable: By setting the platinum (Pt) concentration of the LN single crystal to 1.0 ppm or less, the difference in the optical absorption coefficient between the wavelength of 470 nm and the wavelength of 600 nm (sometimes referred to as the difference in the optical absorption coefficient between the wavelengths of 470 nm and 600 nm) can be reduced, for example, to 0.01 cm -1 The LN single crystal preferably has a platinum (Pt) concentration of 0.5 ppm or less, which can further reduce the difference in the optical absorption coefficient between wavelengths of 470 nm and 600 nm, for example, to 0.005 cm -1 In the LN single crystal, the lower limit of the platinum (Pt) concentration is 0 ppm or more, and may be 0.1 ppm or more. In the LN single crystal, the lower limit of the difference between the optical absorption coefficient at a wavelength of 470 nm and the optical absorption coefficient at a wavelength of 600 nm is not particularly limited, but may be 0 cm -1 or more, and -1or more. In the LN single crystal, the platinum (Pt) concentration is, for example, within a range between any one of the upper and lower limits described above, or within a range between any two of the upper limits described above. In the LN single crystal, the difference between the optical absorption coefficient at a wavelength of 470 nm and the optical absorption coefficient at a wavelength of 600 nm is, for example, within a range between any one of the upper and lower limits described above, or within a range between any two of the upper limits described above. In the LN single crystal, when the platinum (Pt) concentration exceeds 1.0 ppm, the difference between the optical absorption coefficient at a wavelength of 470 nm and the optical absorption coefficient at a wavelength of 600 nm becomes large. In the LN single crystal, when the platinum (Pt) concentration exceeds 1.0 ppm, the optical absorption coefficient at a wavelength of 470 nm becomes large, and the difference between the optical absorption coefficient at a wavelength of 470 nm and the optical absorption coefficient at a wavelength of 600 nm becomes large.

[0032] In addition, in an LN single crystal, if a transition metal other than platinum is present as an impurity in the crystal, it will affect the difference in the optical absorption coefficient at wavelengths of 470 nm and 600 nm in the visible light region, so as in Examples 1 and 2 and Comparative Example 1, the concentration (content) of elements other than platinum was also analyzed by ICP mass spectrometry (ICP-MS), but in this example, no elements were found that showed a correlation with the difference in the optical absorption coefficient at wavelengths of 470 nm and 600 nm. Table 2, which will be explained later, shows the analysis results for representative transition metal elements.

[0033] The concentration of impurities other than platinum in the LN single crystal will now be described. The upper limit of the Fe concentration in the LN single crystal is preferably 2 ppm or less, more preferably 1.5 ppm or less. The lower limit of the Fe concentration is 0 ppm or more, and may be 0.5 ppm or more, or 1.0 ppm or more. In the LN single crystal, the Fe concentration is, for example, within a range between any of the above-mentioned lower limit values ​​and any of the above-mentioned upper limit values. When the Fe concentration is within the above-mentioned range, it does not significantly affect the light absorption coefficient at wavelengths of 470 nm and 600 nm in the visible light region.

[0034] The upper limit of the Ni concentration in the LN single crystal is preferably 0.2 ppm or less, more preferably 0.1 ppm or less. The lower limit of the Ni concentration is 0 ppm or more, and may be 0.05 ppm or more. In the LN single crystal, the Ni concentration is, for example, within a range between any of the above-mentioned lower limit values ​​and any of the above-mentioned upper limit values. When the Ni concentration is within the above range, it does not significantly affect the light absorption coefficient at wavelengths of 470 nm and 600 nm in the visible light region.

[0035] The upper limit of the Cr concentration in the LN single crystal is preferably 0.4 ppm or less, more preferably 0.3 ppm or less. The lower limit of the Cr concentration is 0 ppm or more, and may be 0.1 ppm or more. In the LN single crystal, the Cr concentration is, for example, within a range between any of the above-mentioned lower limit values ​​and any of the above-mentioned upper limit values. When the Cr concentration is within the above-mentioned range, it does not significantly affect the light absorption coefficient at wavelengths of 470 nm and 600 nm in the visible light region.

[0036] The upper limit of the Cu concentration in the LN single crystal is preferably 0.2 ppm or less, more preferably 0.1 ppm or less. The lower limit of the Cu concentration is 0 ppm or more, and may be 0.05 ppm or more. In the LN single crystal, the Cu concentration is, for example, within a range between any of the above-mentioned lower limit values ​​and any of the above-mentioned upper limit values. When the Cu concentration is within the above-mentioned range, it does not significantly affect the light absorption coefficient at wavelengths of 470 nm and 600 nm in the visible light region. Note that the LN single crystal may also contain elements other than those described above within a range that does not deviate from the spirit of the present invention.

[0037] It is also important to suppress the peak of the optical absorption coefficient at a wavelength of 470 nm in the LN single crystal. -1 can be less than or equal to 0.005 cm, and preferably -1 For example, by reducing the platinum (Pt) concentration in the single crystal, the light absorption coefficient at a wavelength of 470 nm can be reduced to 0.01 cm -1For example, by making the platinum (Pt) concentration in the single crystal 1.0 ppm or less, the light absorption coefficient at a wavelength of 470 nm can be reduced to 0.01 cm -1 Preferably, the platinum (Pt) concentration is 0.5 ppm or less, so that the light absorption coefficient at a wavelength of 470 nm is 0.005 cm -1 In the LN single crystal, the lower limit of the light absorption coefficient at a wavelength of 470 nm is not particularly limited, but is preferably 0 cm -1 or more, and -1 In the LN single crystal, the optical absorption coefficient at a wavelength of 470 nm is, for example, within a range between any of the lower and upper limits described above. Furthermore, in the LN single crystal, the upper limit of the optical absorption coefficient at a wavelength of 600 nm is not particularly limited as long as it falls within the scope of the present invention, but may be, for example, 0.0006 cm -1 It may be less than 0.0004 cm -1 In the LN single crystal, the lower limit of the light absorption coefficient at a wavelength of 600 nm is not particularly limited as long as it is within the scope of the present invention, but it is not particularly limited to 0 cm -1 It can be more than 0.001 cm -1 In the LN single crystal, the optical absorption coefficient at a wavelength of 600 nm is, for example, within a range between any of the above-mentioned lower limits and any of the above-mentioned upper limits.

[0038] In this specification, the concentration (content) of elements such as platinum (Pt) in the LN single crystal is determined by inductively coupled plasma mass spectrometry (ICP-MS). ICP mass spectrometry can be performed by the method described in the Examples. In this specification, the optical absorption coefficient is a value determined by the method described in the Examples.

[0039] The LN single crystal may be in the form of an ingot, a wafer, or a thin plate. The size of the LN single crystal is not particularly limited, but the diameter may be, for example, 1 inch or more, 6 inches, or 8 inches. The thickness of the crystal is not particularly limited, but may be 100 μm or more, for example, 100 μm to 1000 μm. For example, in the case of a wafer, the thickness may be 250 μm to 1000 μm, and a thickness of 350 μm to 500 μm is often used. In the case of an ingot, the thickness may be 10 mm to 150 mm.

[0040] As described above, the LN single crystal according to one aspect of this embodiment is characterized in that the platinum (Pt) concentration (content) in the single crystal is 1.0 ppm or less. Furthermore, the LN single crystal according to one aspect of this embodiment has a difference in the optical absorption coefficient between the wavelength of 470 nm and the wavelength of 600 nm of 0.01 cm. -1 The LN single crystal according to one aspect of this embodiment is characterized in that it has a light absorption coefficient of 0.01 cm at a wavelength of 470 nm. -1 The LN single crystal according to the present embodiment has the following characteristics: It has low absorption of light with wavelengths in the visible light region.

[0041] The LN single crystal according to this embodiment has the above-described properties and can therefore be suitably used for the waveguide of an AR display device (an augmented reality display device) such as AR glasses (augmented reality glasses). For example, the AR display device or AR glasses may be configured to use the LN single crystal according to this embodiment as a waveguide. For example, such an AR display device or AR glasses may use the LN single crystal according to this embodiment for at least a portion of the waveguide, and the remainder may have any configuration, and this any configuration may be, for example, a known configuration. The LN single crystal has the above-described properties and can therefore be suitably used for optical elements that can be used for visible light.

[0042] Next, a method for producing the LN single crystal according to the present embodiment will be described. The LN single crystal according to the present embodiment can be produced by, for example, reducing the concentration (content) of platinum (Pt) in the crystal.

[0043] There are several methods for reducing the platinum impurity concentration in lithium niobate single crystals. For example, by using a platinum-iridium alloy for the crucible used for crystal growth and reducing the platinum ratio, lithium niobate single crystals with a low platinum impurity concentration can be obtained.

[0044] Next, a method for reducing the platinum impurity concentration in lithium niobate single crystals will be described. First, platinum impurities in LN single crystals may be impurities contained in the raw materials. It is also important to improve the purity of the raw materials. It is preferable to use raw materials with a purity of 99.99 or higher. However, since platinum is not usually used in the raw material manufacturing stage for LN single crystals, the possibility is considered small.

[0045] Next, the crucible material used during growth is also important. Methods for growing lithium niobate single crystals include the Cz method (Czochralski method) and the VB method (vertical Bridgman method), as mentioned above. The crucible used to melt the raw materials is used. In the Cz method, crucibles generally used are made of materials with high melting points and chemical stability, such as platinum, iridium, or alloys thereof. For growing LN single crystals, relatively inexpensive platinum crucibles are typically used. Platinum crucibles are chemically stable and are not easily dissolved into solutions. However, as shown in Table 1 (described later), trace amounts of platinum (Pt) from the crucible are dissolved into the melt (raw material melt), and during growth, platinum (Pt) from the crucible is incorporated into the crystal, affecting the optical absorption coefficient.

[0046] Therefore, in this embodiment, tests were conducted using crucibles made of platinum or platinum-iridium alloy, and it was found that the lower the platinum content of the platinum-iridium alloy, the less elution there was into the LN single crystal. Therefore, the method for producing an LN single crystal according to this embodiment may be configured such that the crucible used for growing the single crystal is made of platinum and the platinum content of the crucible is adjusted so that the platinum concentration in the grown single crystal is 1.0 ppm or less. This can be achieved, for example, by the method described in the Examples. For example, when adjusting the platinum content of the crucible so that the platinum concentration in the single crystal is 1.0 ppm or less, the platinum content of the platinum-iridium alloy crucible is 50% or less, preferably 20% or less. The elution of iridium into the LN single crystal was not so great as to affect the light absorption coefficient of the LN single crystal in the visible light region.

[0047] The oxygen concentration in the furnace during growth is generally atmospheric air or a nitrogen-oxygen mixed gas atmosphere with an oxygen concentration of about 20%. However, when iridium is contained in a platinum-iridium alloy or the like, it is preferable to set the oxygen concentration low because iridium easily combines with oxygen and sublimes. Furthermore, in consideration of the stability of the crystal, the oxygen concentration in the furnace during growth is preferably more than 5%, atmospheric air, or about 20%.

[0048] In this embodiment, the platinum impurity concentration in the lithium niobate single crystal is reduced by reducing the platinum concentration in the alloy in the crucible, but the present invention is not limited to this example. For example, a method for producing a crystal that does not use platinum, such as the cold crucible method, may also be used.

[0049] As described above, the method for producing an LN single crystal according to this embodiment is a method for producing an LN single crystal, and includes using a crucible containing platinum as the material for growing the single crystal and adjusting the platinum content of the crucible so that the platinum concentration in the grown single crystal is 1.0 ppm or less. Note that, in the method for producing an LN single crystal according to this embodiment, other configurations than those described above can be appropriately achieved by, for example, known methods. According to the method for producing a lithium niobate single crystal according to this embodiment, a lithium niobate single crystal according to this embodiment can be produced.

[0050] The present invention will be specifically described below using examples, but the present invention is not limited to these examples in any way.

[0051] [Example 1] Using the high-frequency induction heating single crystal growth apparatus shown in Figure 1, the flow rates of nitrogen gas and oxygen gas were adjusted so that the oxygen concentration in the growth furnace was 20%, and an LN crystal was grown by the Cz method along the Z-axis. Note that Z-axis growth refers to the crystal growth orientation (the crystal orientation of the seed crystal).

[0052] In order to reduce the platinum concentration in the LN crystal to be produced, LN powder with a purity of 99.99 or higher was charged as raw material 18 into crucible 12 containing a platinum-iridium alloy with a platinum ratio of 20%, and after melting raw material 18, the tip of seed crystal 1 was immersed in the raw material melt in crucible 12 and pulled up while rotating, thereby growing an LN single crystal ingot with a diameter of 6 inches (=152 mm) and a straight body length of 70 mm. The grown LN single crystal ingot was separated from the raw material melt, and the crystal was cooled to near room temperature and then removed.

[0053] The extracted single crystal ingot was annealed and poled, then the outer periphery was ground into a cylindrical shape and cut into 500 μm-thick wafers using a multi-wire saw. One wafer each from the upper and lower sides of the cut crystal was sampled, crushed in an agate ball mill, sieved through a 150 μm mesh, mixed with a reagent mixture of hydrofluoric acid and nitric acid, and then dissolved using a microwave pretreatment device. The platinum concentration of the dissolved sample was analyzed by ICP-MS, and found to be 0.3 ppm in each wafer. To measure the absorption coefficient, both sides of the remaining wafers were chemically mechanically polished with colloidal silica. The absorption coefficient of the polished wafers was measured using a spectrophotometer (Agilent, Cary 7000). In this example, the elemental analysis accuracy by ICP-MS was 0.1 ppm.

[0054] To determine the absorption coefficient, first, the angle of incidence θ of light onto the sample was fixed at 6°, and the reflectance R and transmittance T were measured. The detector angle when measuring reflectance R was set to 2θ = 12°, and the detector angle when measuring transmittance was set to 180°. Furthermore, to reduce noise in the measurement values, the incident light was passed through a depolarizing plate during measurement. Based on the principle that the sum of reflectance R, transmittance T, and absorbance A is 100%, the absorbance A was calculated from the measured reflectance R and transmittance T using the following formula (1). Figure 2 shows a schematic diagram of the measurement of reflectance and transmittance using a spectrophotometer to calculate the absorption coefficient.

[0055]

[0056] The absorption coefficient is defined as the following equation (2) according to the Beer-Lambert law, using α in the natural logarithm format and β in the common logarithm format. In this specification, the absorption coefficient will be expressed using β in the common logarithm format. In the formula, x is the length of the sample through which the light passes, I 0 is the light intensity just before the light passes through the sample a distance x, and I is the light intensity after the light passes through the sample a distance x. Therefore, the absorptance A is I 0 Using I, it can be expressed by the following equation (3).

[0057]

[0058] From equations (1) and (3), the absorption coefficient β is given by the following equation (4).

[0059] By measuring the reflectance R and transmittance T of a sample with a thickness x (cm) using equation (4), the absorption coefficient β (cm -1 ) was calculated.

[0060] The absorption coefficient can also be calculated using the following formula (5), which takes multiple reflections within the sample into consideration, but please note that this will result in a slight difference from the value calculated using formula (4). All absorption coefficients in this embodiment are calculated using the definition of formula (4).

[0061]

[0062] In Example 1, the absorption coefficient calculated using the formula (4) as described above was as follows: (1) 0.0039 cm at a wavelength of 470 nm -1 , (2) 0.0006 cm at a wavelength of 600 nm -1 , (1)-(2) is 0.0033 cm -1 It was.

[0063] [Example 2] Next, the material of the crucible was changed to a platinum-iridium alloy with a platinum ratio of 50%, and crystal growth was carried out under the same conditions as in Example 1, and the platinum concentration and absorption coefficient were measured. As a result, the platinum concentration was 0.8 ppm. The absorption coefficient was (1) 0.0079 cm at a wavelength of 470 nm. -1 , (2) 0.0004 cm at a wavelength of 600 nm -1 , (1)-(2) is 0.0075 cm -1 It was.

[0064] [Comparative Example 1] Next, the material of the crucible was changed to pure platinum, and crystal growth was carried out under the same conditions as in Example 1, and the platinum concentration and absorption coefficient were measured. As a result, the platinum concentration was 1.2 ppm. The absorption coefficient was (1) 0.0110 cm at a wavelength of 470 nm. -1 , (2) 0.0007 cm at a wavelength of 600 nm -1 , (1)-(2) is 0.0103 cm -1 It was.

[0065] The results of Examples 1 and 2 and Comparative Example 1 are summarized in Table 1.

[0066]

[0067] Furthermore, if transition metals other than platinum are present as impurities in the LN crystal, an absorption peak around 470 nm may occur, so elements other than platinum in Examples 1 and 2 and Comparative Examples 1 and 2 were also analyzed by ICP-MS, but no elements were found that showed a correlation with the absorption coefficient at 470 nm. Table 2 shows the analysis results of representative transition metal elements by ICP-MS.

[0068]

[0069] The above results show that the absorption peak around 470 nm can be suppressed by reducing the platinum impurity concentration during crystal growth. Furthermore, by keeping the platinum impurity concentration during crystal growth at 0.1 ppm or less, the difference in the optical absorption coefficient between the wavelength of 470 nm and the wavelength of 600 nm can be reduced to 0.01 cm. -1 It has been confirmed that the LN single crystal according to this embodiment has the property of having little absorption of light with wavelengths in the visible light region.

[0070] The technical scope of the present invention is not limited to the aspects described in the above-mentioned embodiments, etc. One or more of the requirements described in the above-mentioned embodiments, etc. may be omitted. Furthermore, the requirements described in the above-mentioned embodiments, etc. may be combined as appropriate. For example, the single crystal of this embodiment may be appropriately combined with the features described in the manufacturing method and examples of this embodiment, and the manufacturing method of this embodiment may be appropriately combined with the features described in the single crystal and examples of this embodiment. Furthermore, to the extent permitted by law, the disclosures of Japanese Patent Application No. 2023-090005 and all documents cited in the above-mentioned embodiments, etc. are incorporated herein by reference. It is clear that the lithium niobate single crystal and manufacturing method described in this embodiment can also be applied to lithium niobate having a stoichiometric composition and a congruent composition, as well as various lithium niobate single crystals to which a substance has been added, such as doped, within the scope of the present invention.

Claims

1. A lithium niobate single crystal having a platinum concentration of 1.0 ppm or less in the single crystal.

2. The lithium niobate single crystal according to claim 1, wherein the concentration of platinum in the single crystal is 0.5 ppm or less.

3. The difference between the light absorption coefficient of 470 nm and that of 600 nm is 0.01 cm -1 The following is a lithium niobate single crystal.

4. The light absorption coefficient of 470 nm is 0.01 cm -1 The lithium niobate single crystal according to claim 3, wherein:

5. AR glass using the lithium niobate single crystal according to any one of claims 1 to 4 as a waveguide.

6. A method for producing a lithium niobate single crystal, comprising: using a crucible made of a platinum-containing material for growing the single crystal; and adjusting the platinum content of the crucible so that the platinum concentration in the grown single crystal is 1.0 ppm or less.

Citation Information

Patent Citations

  • Production of lithium niobate single crystal

    JP1989096095A

  • Method for suppressing fatigue crack progression of bent part of metal plate and automobile component

    JP2023090005A

  • Production of lithium niobate single crystal and optical element therefrom

    JP1993097591A

  • METHOD FOR GROWING LiNbO3 SINGLE CRYSTAL

    JP2018100202A