Zirconia sintered body and method for producing same
The described method for manufacturing zirconia sintered bodies using microwave heating and rapid cooling achieves both excellent translucency and hydrothermal resistance, addressing the limitations of partially stabilized zirconia bodies with low yttria content.
Patent Information
- Application Number
- PCT/JP2024/018979
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Partially stabilized zirconia sintered bodies with low yttria content face challenges in achieving both excellent translucency and hydrothermal deterioration resistance, as they tend to have poor mechanical properties and stability.
A zirconia sintered body is manufactured using a method involving a molded body with zirconia and yttria/yttobia, heated in a microwave oven to 1600°C or more and then rapidly cooled to 1300°C, with a c/a axis length ratio of the unit cell within 1.0055 to 1.010, and processed in an oxidizing atmosphere to suppress plasma generation and darkening.
The method results in a zirconia sintered body with enhanced light transmittance and hydrothermal deterioration resistance, suitable for dental materials like dentures and orthodontic brackets.
Smart Images

Figure JP2024018979_05122024_PF_FP_ABST
Abstract
Description
Zirconia sintered body and its manufacturing method
[0001] The present disclosure relates to a zirconia sintered body and a method for producing the same. This application claims priority to Japanese Patent Application No. 2023-091593, filed on June 2, 2023, the entire contents of which are incorporated herein by reference.
[0002] Yttria (Y) is used as a stabilizer. 2 O 3 Zirconia sintered bodies in which a small amount of rare earth elements such as ZnO, Ni, NiAl, NiFe, NiAl, NiO, NiAl ...
[0003] For example, Patent Document 1 discloses a translucent zirconia sintered body containing more than 4.0 mol % and not more than 6.5 mol % yttria as a stabilizer. Furthermore, Patent Documents 2 and 3 disclose that a zirconia sintered body having excellent resistance to hydrothermal degradation can be realized by setting the sintering temperature of the zirconia sintered body to at least 1,350° C. or less.
[0004] Japanese Patent Application Publication No. 2015-143178 Japanese Patent Application Publication No. 2014-12627 Japanese Patent Application Publication No. 2014-218421
[0005] By adjusting the content of the stabilizer contained in the partially stabilized zirconia sintered body, the mechanical properties of the zirconia sintered body can be adjusted. For example, lowering the content of the stabilizer tends to improve mechanical properties such as bending strength and fracture toughness. However, such partially stabilized zirconia sintered bodies tend to have lower hydrothermal degradation resistance and translucency.
[0006] A main object of the present disclosure is to provide a technology for realizing a zirconia sintered body having excellent translucency and resistance to hydrothermal degradation.
[0007] In order to achieve the above object, the present inventors have conducted research and found that a predetermined ratio of yttria and / or ytterbia (Yb 2 O 3 They found that a zirconia sintered body excellent in translucency and resistance to hydrothermal degradation can be realized by sintering a molded body of partially stabilized zirconia having the above-mentioned structure by microwave heating and then rapidly cooling it to 1300°C. Analysis of the crystalline phase of such a zirconia sintered body revealed that the zirconia sintered body has a crystalline phase in which the c / a axial length ratio of the unit lattice is in the range of 1.0055 or more and less than 1.010.
[0008] The present disclosure provides a method for producing a zirconia sintered body. The method for producing a zirconia sintered body includes a molded body preparation step of preparing a molded body containing zirconia and yttria and / or ytterbia, where the total proportion of yttria and ytterbia is 3 mol% or more and less than 4 mol% when the total of zirconia, yttria, and ytterbia is 100 mol%, a first heating step of heating the molded body at 800°C or more and 1200°C or less, a second heating step of heating the molded body that has undergone the first heating step at 1600°C or more and 2000°C or less by microwave heating, and a cooling step of cooling the molded body that has undergone the second heating step to 1300°C at a rate of 50°C / min or more. This production method allows for the production of a zirconia sintered body with excellent translucency and resistance to hydrothermal degradation.
[0009] In some preferred embodiments, the microwave heating is performed in a multi-mode. This allows heating while suppressing plasma generation. As a result, the occurrence of cracks in the zirconia sintered body is suppressed, and a zirconia sintered body with excellent translucency and hydrothermal degradation resistance can be produced.
[0010] In some preferred embodiments, the microwave heating in the second heating step is carried out in an oxidizing atmosphere, which prevents the zirconia sintered body from darkening and allows the production of a zirconia sintered body that is excellent in translucency, resistance to hydrothermal degradation, and aesthetics.
[0011] In some preferred embodiments, in the second heating step, the microwave heating is performed in an atmosphere having an oxygen concentration of 30 vol % or more and 100 vol % or less. This effectively prevents the zirconia sintered body from darkening, thereby enabling the production of a zirconia sintered body that is more aesthetically pleasing and has excellent translucency and resistance to hydrothermal degradation.
[0012] In some preferred embodiments, in the second heating step, SiC susceptors are disposed to sandwich the green body from both sides in a predetermined direction, thereby allowing sintering of the inside of the green body to proceed more suitably, thereby producing a zirconia sintered body having excellent translucency and resistance to hydrothermal degradation.
[0013] In some preferred embodiments, the green body is prepared by molding a material containing zirconia-containing granules in the green body preparation step, which can improve the shape stability of the green body and improve handling and workability.
[0014] The present disclosure also provides a zirconia sintered body. The zirconia sintered body contains zirconia and yttria and / or ytterbia, and when the total of the zirconia, yttria, and ytterbia is taken as 100 mol%, the total proportion of yttria and ytterbia is 3 mol% or more and less than 4 mol%, and when the entire crystalline phase is taken as 100 mass%, the proportion of the crystalline phase having a c / a axial length ratio of the unit lattice in the range of 1.0055 or more and less than 1.010 is 10 mass% or more. The zirconia sintered body having such a configuration achieves excellent translucency and hydrothermal degradation resistance.
[0015] In this specification, the c / a axial length ratio and the proportion thereof of the unit lattice of the zirconia sintered body can be obtained by Rietveld analysis of the profile of the X-ray diffraction pattern of the zirconia sintered body using RIETAN-FP as an analysis program.
[0016] In some preferred embodiments, when the entire crystalline phase is taken as 100% by mass, the proportion of crystalline phases having a unit lattice c / a axial length ratio in the range of 1.007 or more and less than 1.010 is 10% by mass or more, thereby further improving hydrothermal degradation resistance.
[0017] In some embodiments, the proportion of monoclinic crystals is 10% or less after immersion for 6 hours in hot water at 134° C. The zirconia sintered body disclosed herein can have such excellent resistance to hydrothermal degradation.
[0018] In some embodiments, when the entire crystalline phase is taken as 100 mass %, the proportion of the crystalline phase having a c / a axial length ratio of the unit lattice in the range of 1 to less than 1.0055 is 20 mass % or less. With this configuration, the crystalline phase becomes more homogeneous, and therefore, better light transmittance and hydrothermal degradation resistance can be achieved.
[0019] In some embodiments, the total light transmittance in the thickness direction of a 1 mm thick test piece to a D65 light source is 44% or more.
[0020] The present disclosure also provides a dental material containing the zirconia sintered body disclosed herein. Such a dental material can be used, for example, as a denture, a denture mill blank, or an orthodontic bracket. The zirconia sintered body disclosed herein is suitable for use as a dental material because of its excellent translucency and resistance to hydrothermal degradation.
[0021] 1 is a flowchart showing an outline of a method for producing a zirconia sintered body in one embodiment. FIG. 2 is a schematic diagram showing an example of a method for microwave heating a compact (preliminary sintered body).
[0022] Hereinafter, several embodiments of the technology disclosed herein will be described. It should be noted that matters necessary for carrying out the present technology other than those specifically mentioned in this specification (e.g., the microwave heating temperature) can be understood based on the technical content taught by this specification and the general technical common sense of a person skilled in the art. The technology disclosed herein can be carried out based on the content disclosed in this specification and the general technical common sense of a person skilled in the art. In this specification, when a numerical range is described as "A to B (where A and B are arbitrary numerical values)," this means "A or more and B or less," and also encompasses the meanings of "greater than A and less than B," "greater than A and B or less," and "greater than A and less than B."
[0023] The zirconia sintered body disclosed herein contains at least zirconia (ZrO 2 The zirconia sintered body disclosed herein also contains yttria (Y 2 O 3 ) and ytterbia (Yb 2 O 3 ) contains at least one of the above. That is, the zirconia sintered body disclosed herein may be an embodiment containing both yttria and ytterbia, an embodiment containing yttria but not ytterbia, or an embodiment containing ytterbia but not yttria. The zirconia sintered body disclosed herein contains zirconia as a main component. Here, "containing zirconia as a main component" means that zirconia accounts for the largest proportion of the compounds constituting the zirconia sintered body. When the entire zirconia sintered body is taken as 100 mass%, the proportion of zirconia is, for example, 70 mass% or more, preferably 80 mass% or more, and more preferably 90 mass% or more. A high proportion of zirconia can improve the strength, toughness, hydrothermal degradation resistance, etc. of the zirconia sintered body.
[0024] The yttria and / or ytterbia contained in the zirconia sintered body can be contained, for example, as part of partially stabilized zirconia partially dissolved in zirconia (so-called stabilizer). Partially stabilized zirconia can improve mechanical properties such as strength and toughness because the proportion of monoclinic crystals is suppressed at room temperature. Furthermore, suppressing the proportion of monoclinic crystals suppresses variation in the crystalline phases constituting the zirconia sintered body, thereby improving translucency.
[0025] Generally, when the proportion of stabilizer in partially stabilized zirconia is reduced, mechanical properties improve, but the stability of the crystalline phase tends to decrease. When the stability of the crystalline phase is low, a phase transition from tetragonal to monoclinic crystals is likely to occur, resulting in a decrease in translucency. Furthermore, an increase in the proportion of monoclinic crystals tends to decrease hydrothermal degradation resistance. Therefore, it is desirable to improve the translucency and hydrothermal degradation resistance of partially stabilized zirconia with a low proportion of stabilizer.
[0026] The zirconia sintered body disclosed herein has a relatively low proportion of yttria and / or ytterbia contained as a stabilizer, but has excellent translucency and hydrothermal degradation resistance. When the total of zirconia, yttria, and ytterbia contained in the zirconia sintered body is taken as 100 mol%, the total proportion of yttria and ytterbia can be, for example, 4.2 mol% or less, 4 mol% or less, less than 4 mol%, or 3.9 mol% or less. Thus, despite the low total proportion of yttria and / or ytterbia, excellent translucency and hydrothermal degradation resistance are achieved. Furthermore, the lower limit of the total proportion of yttria and ytterbia can be, for example, 3 mol% or more, 3.1 mol% or more, 3.3 mol% or more, or 3.5 mol% or more. This stabilizes the crystalline phase. The "total proportion of yttria and ytterbia" also includes the case where the proportion of yttria or ytterbia is 0 mol% (i.e., the case where the zirconia sintered body does not contain yttria or ytterbia). That is, in an embodiment where yttria is contained but not ytterbia, the proportion of yttria is the same as the range of the total proportion described above. Also, in an embodiment where ytterbia is contained but not yttria, the proportion of ytterbia is the same as the range of the total proportion described above.
[0027] When the zirconia sintered body contains both yttria and ytterbia, the proportion of yttria may be greater than or less than that of ytterbia. Note that all of the yttria and / or ytterbia may be solid-dissolved in zirconia, or may contain yttria and / or ytterbia that is not solid-dissolved in zirconia.
[0028] In some embodiments, the zirconia sintered body further comprises alumina (Al 2 O 3). In a zirconia sintered body containing alumina, abnormal grain growth is suppressed, which can improve the strength and translucency of the zirconia sintered body. Furthermore, low-temperature degradation resistance can be improved, which can enable the strength and translucency of the zirconia sintered body to be maintained for a long period of time. On the other hand, since alumina remains as an impurity inside the sintered body and acts as a light scattering factor, it is preferable that the alumina content is not too high. Therefore, when the entire zirconia sintered body is taken as 100% by mass, the alumina content may be, for example, 0.15% by mass or less, and may be 0.125% by mass or less, 0.1% by mass or less, or 0.05% by mass or less.
[0029] The zirconia sintered body may also contain a conventionally known colorant, provided that the effects of the technology disclosed herein are not significantly impaired. Examples of colorants include transition metal elements and lanthanoid rare earth elements. Examples of such elements include iron, nickel, cobalt, manganese, niobium, praseodymium, neodymium, europium, gadolinium, and erbium. The colorant content may be, for example, 2% by mass or less, 1% by mass or less, or 0.5% by mass or less, based on the total mass of the zirconia sintered body.
[0030] The zirconia sintered body may contain elements that may be unavoidably mixed in. Examples include hafnium, magnesium, silicon, titanium, etc. The total content of these elements is preferably 2.5 mass% or less, more preferably 2 mass% or less, for example 1.8 mass% or less, calculated as oxides, based on the entire zirconia sintered body.
[0031] 1 is a flowchart showing a method for producing a zirconia sintered body in one embodiment. In some embodiments, the method for producing a zirconia sintered body may include a molded body preparation step S10 for preparing a molded body (work) containing zirconia and yttria and / or ytterbia, a first heating step S20 for heating the molded body, a second heating step S30 for heating the molded body (hereinafter also referred to as a "pre-sintered body") that has undergone the first heating step S20 by microwave heating, and a cooling step S40 for lowering the temperature of the molded body that has undergone the second heating step.
[0032] <Molded body preparation step S10> The molded body preparation step S10 may include preparing a material that constitutes the molded body (hereinafter also referred to as a "molded body material") (hereinafter also referred to as a "molded body material preparation step") and molding the molded body material (hereinafter also referred to as a "molding step").
[0033] In the compact material preparation step, first, a zirconia raw material is prepared. The zirconia raw material is not particularly limited, but for example, a zirconium salt or a hydrate thereof can be used. Examples of zirconium salts include zirconium oxychloride, zirconium chloride, zirconium sulfate, and zirconium nitrate. These may be used alone or in combination of two or more.
[0034] Next, an aqueous solution of zirconia raw material is prepared, and a hydrolysis reaction is carried out to prepare a zirconia sol. The hydrolysis reaction can be carried out by adding an alkali metal hydroxide, an alkaline earth metal hydroxide, an aqueous ammonia solution, or the like to the aqueous solution. Examples of alkali metal hydroxides that can be used include lithium hydroxide, sodium hydroxide, and potassium hydroxide, and examples of alkaline earth metal hydroxides that can be used include magnesium hydroxide and calcium hydroxide.
[0035] Next, the zirconia sol (ZrO 2 ・nH 2 0) is mixed with yttria and / or ytterbia, or a raw material thereof. The raw material for yttria is an yttrium-containing compound that can become yttria by firing. Examples of the yttrium-containing compound include yttrium chloride and yttrium nitrate. The raw material for ytterbia may be an ytterbium-containing compound that can become ytterbia by firing. Examples of the ytterbium-containing compound include ytterbium chloride and ytterbium nitrate.
[0036] When yttria and / or ytterbia are mixed with the zirconia sol, the proportion of the yttria and / or ytterbia to be mixed may be the same as the total proportion of yttria and ytterbia in the zirconia sintered body described above. When the total of zirconia, yttria, and ytterbia is taken as 100 mol%, the proportion may be, for example, 3 mol% or more, 3.1 mol% or more, 3.3 mol% or more, or 3.5 mol% or more. Furthermore, the total proportion of yttria and ytterbia may be, for example, 4.2 mol% or less, 4 mol% or less, less than 4 mol%, or 3.9 mol% or less.
[0037] In addition, when the zirconia sol is mixed with an yttria raw material and / or an ytterbia raw material, the amount of yttria and / or ytterbia obtained by firing these raw materials should be set to fall within the above-mentioned range of the ratio of yttria and / or ytterbia. For example, yttrium chloride (YCl) is used as the yttria raw material. 3 ) X mol (X is a positive number) is used, 2 O 3 ) can be obtained, so yttrium chloride should be mixed in such a way that the amount of substance is twice as much as when yttria itself is mixed.
[0038] Next, the zirconia sol to which yttria and / or ytterbia or raw materials thereof have been added is dried to obtain a dry powder in which the raw materials are uniformly dispersed. The drying method is not particularly limited, and can be appropriately selected from, for example, natural drying, air drying, hot air drying, drying by heating using a heating furnace or the like, vacuum drying, suction drying, freeze drying, etc.
[0039] The dried powder is calcined to obtain a calcined powder containing yttria and / or ytterbia partially stabilized zirconia. The calcination temperature is not particularly limited, but can be, for example, 800°C to 1200°C, preferably 1000°C to 1200°C. By such calcination, the yttria raw material can be oxidized to yttria, and the ytterbia raw material can be oxidized to ytterbia. A conventionally known heating device can be used as the heating device for calcination, and examples of the heating device include an electric furnace, a muffle furnace, a tunnel heating furnace, and a microwave furnace.
[0040] The calcined powder contains particles of various shapes and particle sizes, and is therefore preferably pulverized. The pulverization method is not particularly limited, and the powder can be pulverized, for example, using a known pulverizer (such as a ball mill). For example, it is preferable to use zirconia balls with a diameter of approximately 0.1 mm to 5 mm in the ball mill. Furthermore, it is preferable to sort the pulverized powder into particles of the desired particle size. For example, zirconia powder of the desired particle size can be obtained using a mesh sieve, and the size of the mesh openings can be appropriately selected according to the desired particle size.
[0041] The average particle size of the zirconia powder used as the compact material is preferably, for example, 100 nm to 300 nm, and more preferably 150 nm to 200 nm. An average particle size within this range can provide high sinterability, improved strength, and improved light transmittance. In this specification, the term "average particle size" refers to the particle size (D) corresponding to the cumulative 50% from the fine particle side in the volume-based particle size distribution measured by a laser diffraction / light scattering method. 50 For such measurement, for example, a particle size distribution measuring device LA950V2 (manufactured by Horiba Ltd.) can be used.
[0042] The zirconia powder produced as described above mainly contains yttria and / or ytterbia partially stabilized zirconia particles. The proportion of yttria and / or ytterbia partially stabilized zirconia particles in such zirconia powder is 50% by number or more, preferably 60% by number or more, and may be 70% by number or more, 80% by number or more, 90% by number or more, or 95% by number or more. The zirconia powder may also contain fully stabilized zirconia. The zirconia powder may also contain zirconia particles in which yttria and / or ytterbia are not solid-dissolved. Furthermore, the zirconia powder may also contain yttria particles and / or ytterbia particles.
[0043] In this manner, zirconia powder can be obtained as a compact material, but the compact material is not limited to such zirconia powder.
[0044] In some embodiments, an aluminum compound may be mixed with the zirconia powder. The aluminum compound may be oxidized to alumina by heating in the first heating step S20 and / or the second heating step S30. Therefore, the amount of aluminum compound mixed may be determined so as to achieve the alumina content in the zirconia sintered body described above, assuming that all of the aluminum contained in the aluminum compound is oxidized to alumina. Examples of aluminum compounds that can be used include alumina powder, alumina sol, hydrated alumina, aluminum hydroxide, aluminum chloride, aluminum nitrate, and aluminum sulfate. The zirconia powder and the aluminum compound may be dispersed in a solvent such as water to form a slurry. When the slurry is prepared, the zirconia powder in which the aluminum compound is suitably dispersed can be obtained by drying the slurry.
[0045] The average particle size of the aluminum compound is preferably similar to or smaller than that of the zirconia powder. Although not particularly limited, the average particle size of the aluminum compound is preferably, for example, 300 nm or less, more preferably 200 nm or less, and may be 150 nm or less, or 100 nm or less (e.g., 20 nm to 50 nm). This allows the aluminum compound to be suitably dispersed in the zirconia powder. Therefore, alumina can be more uniformly distributed in the zirconia sintered body, and abnormal grain growth of the zirconia sintered body can be suitably suppressed.
[0046] In some embodiments, the compact material contains granules. The average particle size of the granular compact material is, for example, 10 μm to 100 μm, and may be 20 μm to 90 μm, or 40 μm to 80 μm. When the compact material contains granules, shape stability is improved, and handling and workability can be improved. In addition, residual stress during molding is alleviated, which can suppress the occurrence of hot spots due to differences in powder density during microwave heating. Furthermore, in the manufacturing method disclosed herein, zirconia is sintered by microwave heating, so even granules with an average particle size larger than that of the powder can be suitably heated to their interior.
[0047] The method for producing the granular compact material is not particularly limited, but it can be produced, for example, by spray-drying zirconia powder. The zirconia powder may contain an aluminum compound and may further contain a binder. In the spray-drying method, the zirconia powder is mixed with a dispersion medium (e.g., water) to prepare a slurry, which is then sprayed onto droplets and dried to obtain the granular compact material.
[0048] The binder is preferably a component that burns out at the heating temperature of the first or second heating step described below. Examples of binders include acrylic resins, epoxy resins, phenolic resins, amine resins, alkyd resins, and cellulose-based polymers. Among these, an acrylic resin is preferred. The inclusion of an acrylic resin enhances adhesion between zirconia powder particles, allowing for the efficient production of zirconia granules. Furthermore, the shape stability of the molded body is enhanced, allowing the molded body to be stably maintained. Examples of acrylic resins include polymers containing alkyl (meth)acrylate as the main monomer (a component accounting for 50% or more by mass of the total monomers) and copolymers containing such a main monomer and a secondary monomer copolymerizable with the main monomer. In this specification, the term "(meth)acrylate" refers to acrylate and methacrylate.
[0049] If the amount of binder is too large, voids may easily form in the zirconia sintered body after the binder burns through. If voids form in the zirconia sintered body, hydrothermal degradation resistance may decrease. Furthermore, the voids may easily refract light, reducing translucency. Therefore, the binder content may be, for example, 10% by mass or less, preferably 5% by mass or less, when the total powder used in spray drying is taken as 100% by mass. Furthermore, if the amount of binder is too small, the effect of the binder may be insufficient. Therefore, the binder content may be, for example, 0.5% by mass or more, and may be 1% by mass or more.
[0050] Next, the molding process will be described. The method for molding the molded body material is not particularly limited, and for example, pressure molding, injection molding, extrusion molding, cast molding, etc. can be used. As the pressure molding, for example, cold isostatic pressing (CIP), hot isostatic pressing (HIP), etc. are preferably used. By using CIP or HIP, a molded body (molded body) with high homogeneity and high density can be produced.
[0051] <First Heating Step S20> In the first heating step S20, the molded body is heated to pre-sinter it, obtaining a pre-sintered body. This heating can remove components such as moisture, binders, and impurities that may be present in the molded body. Pre-sintering can also reduce voids that may exist in the molded body, thereby effectively preventing cracks that may occur during sintering at high temperatures and high speeds. Pre-sintering can be carried out at a heating temperature of, for example, 800°C to 1200°C, preferably 1000°C to 1100°C. The pre-sintering time can vary depending on the shape, size, composition, etc. of the molded body, and can be adjusted as appropriate. For example, it can be 1.5 to 5 hours, or 2 to 4 hours. Heating of the molded body can be carried out by known methods, and heating devices such as a muffle furnace, electric furnace, or microwave oven can be used.
[0052] The shape of the molded body is not particularly limited, and may be, for example, a plate, a disk, a rectangular parallelepiped, a cube, a column, or the like.
[0053] The temperature increase rate in the first heating step S20 is not particularly limited, but can be, for example, 100°C / h to 250°C / h until the temperature reaches 800°C, and 50°C / h to 150°C / h until the predetermined temperature (for example, 1000°C to 1200°C) is reached. This prevents rapid sintering and suppresses the occurrence of cracks.
[0054] <Second Heating Step S30> In the second heating step S30, the molded body (preliminary sintered body) that has undergone the first heating step S20 is sintered by microwave heating to obtain a sintered product. By performing microwave heating, the interior of the preliminarily sintered body can be heated quickly, thereby reducing the difference in sintering progress between the surface side and the interior side of the preliminarily sintered body, and further reducing voids inside the zirconia sintered body. Below, one embodiment of the second heating step S30 will be described with reference to the drawings. Note that the microwave heating method is not limited to the following example.
[0055] Figure 2 is a schematic diagram showing an example of a method for microwave heating a pre-sintered body. Note that the dimensional relationships (length, width, thickness, etc.) in Figure 2 do not reflect actual dimensional relationships. The directions of up, down, left, and right are represented by arrows U, D, L, and R, respectively, in the figure. Here, the directions of up, down, left, and right are defined merely for the convenience of explanation and do not limit the installation form.
[0056] As shown in Fig. 2, the microwave heating device 10 has a partition wall 12 and a heating space 14. An insulated container 20 is installed in the heating space 14, and a susceptor 40 and a pre-sintered body 50 are accommodated in an accommodation space 22 of the insulated container 20. A gas supplier 30 is connected to the accommodation space 22 of the insulated container 20. A radiation thermometer 60 is installed at a position remote from the outside of the microwave heating device 10.
[0057] The microwave heating device 10 has a heating space 14 surrounded by a partition wall 12. The heating space 14 is a space that contains an object to be microwave-heated. Although not shown, the side walls, ceiling, and / or bottom wall of the heating space 14 have microwave irradiation units that can irradiate and heat the object contained in the heating space 14 with microwaves. The microwaves may have a frequency that is conventionally used for microwave heating; for example, microwaves with a frequency of 0.3 GHz to 3 GHz (e.g., 2.45 GHz) can be used.
[0058] The partition wall 12 insulates the heating space 14 of the microwave heating device 10 from the outside, and a commercially available microwave device can be used. In order to improve the thermal insulation, the heating space 14 side of the partition wall 12 may be lined with an insulating material.
[0059] The partition wall 12 is provided with a through-hole 16 for measuring the temperature of an object in the heating space 14. The through-hole 16 penetrates so as to connect the heating space 14 to the outside of the microwave heating device 10. As the microwave heating device 10 having such a configuration, for example, μ-Reactor EX or μ-Reactor Mx manufactured by Shikoku Keisoku Kogyo Co., Ltd. can be used.
[0060] The insulated container 20 has an internal storage space 22 capable of accommodating the susceptor 40 and the pre-sintered body 50. As shown in FIG. 2 , the insulated container 20 has a gas inlet 24 connecting the storage space 22 to the gas supplier 30, a gas outlet 26 connecting the storage space 22 to the heating space 14, and a through-hole 28 for measuring the temperature of the object to be heated in the storage space 22. In this embodiment, the insulated container 20 is a rectangular box-shaped container, but its shape is not particularly limited and may be, for example, cylindrical or prismatic. Although not shown, the insulated container 20 is designed to be separable into a lid portion and a case portion, allowing the object to be easily placed in and removed from the storage space 22. The insulated container 20 may be made of ceramic fiber, such as alumina-silica fiber, or other suitable material.
[0061] The gas introduction hole 24 is a through-hole that connects the accommodation space 22 and the heating space 14, and is designed to allow a pump 32 connected to a gas supplier 30 to be inserted therethrough. This allows a desired gas to be supplied to the accommodation space 22, and the atmosphere within the accommodation space 22 to be controlled.
[0062] The gas exhaust hole 26 is a through-hole that connects the accommodation space 22 and the heating space 14 and is designed so that the accommodation space 22 is not sealed. This prevents oxygen in the accommodation space 22 from being consumed as the firing of the pre-sintered body 50 progresses, and prevents the accommodation space 22 from becoming a reducing atmosphere. The gas exhaust hole 26 also prevents the gas supplied from the gas inlet hole 24 from stagnating in the accommodation space 22. Note that while one gas exhaust hole 26 is provided in FIG. 2 , multiple (two or more) gas exhaust holes may be provided. In this embodiment, the gas exhaust hole 26 is provided in the wall opposite the wall in which the gas inlet hole 24 is provided, but the position of the gas exhaust hole 26 is not particularly limited. The diameter of the gas exhaust hole 26 is not particularly limited, but may be, for example, approximately 5 mm to 50 mm, or approximately 5 mm to 20 mm.
[0063] As shown in FIG. 2 , in this embodiment, a through-hole 28 that communicates the storage space 22 and the heating space 14 is provided on the upper side of the insulated container 20. The through-hole 28 and the through-hole 16 of the microwave heating device 10 are aligned in a straight line. This allows the temperature of the object to be heated placed in the storage space 22 to be measured by a radiation thermometer 60 installed outside the microwave heating device 10. The through-hole 28 is not particularly limited as long as it is sized to allow the radiation thermometer 60 to measure the temperature of the object to be heated. For example, the diameter of the through-hole 28 may be approximately 5 mm to 10 mm. In this embodiment, both the gas exhaust hole 26 and the through-hole 28 are provided. However, since a single through-hole can fulfill the functions of both the gas exhaust hole 26 and the through-hole 28, a configuration in which only one of them is provided may also be used.
[0064] The gas supplier 30 supplies a desired gas to the storage space 22 of the insulated container 20 via a pump 32, thereby adjusting the atmosphere in the storage space 22. The gas supplier 30 can be appropriately changed according to the desired gas, and any commercially available gas supplier (e.g., an oxygen supplier) can be used without particular restrictions. Note that when adjusting the storage space 22 to an atmospheric atmosphere, a blower or the like may be used as the gas supplier 30.
[0065] If the oxygen concentration around the pre-sintered body 50 decreases during firing, the zirconia contained in the pre-sintered body 50 may be reduced. This can cause the zirconia sintered body to darken and lose its aesthetic appeal. Therefore, microwave heating is preferably performed in an oxidizing atmosphere. Examples of oxidizing atmospheres include air and atmospheres with a higher oxygen concentration than air. In particular, an oxygen concentration of 30 vol% or more is preferable, and it can be, for example, 50 vol% or more, or 70 vol% or more. Such an oxidizing atmosphere can further suppress darkening of the zirconia sintered body. Note that there is no particular upper limit to the oxygen concentration in the atmosphere, and the oxygen concentration can be 100 vol% or less. However, if the oxygen concentration is too high, abnormal heating by oxygen plasma may occur. Therefore, the oxygen concentration is preferably 95 vol% or less, and more preferably 90 vol% or less. Note that such control of the oxidizing atmosphere need only be performed at least in the storage space 22 of the insulated container 20 in which the pre-sintered body 50 is placed.
[0066] Furthermore, during firing of the pre-sintered body 50, it is preferable to continuously supply air or a gas containing the above oxygen concentration to the accommodation space 22 (specifically, the pre-sintered body 50) in order to maintain the above-mentioned oxidizing atmosphere. This makes it possible to suppress fluctuations in the atmosphere of the accommodation space 22 (e.g., a decrease in oxygen concentration) that accompany firing. Furthermore, as shown by the arrows in FIG. 2 , the gas supplied from the gas supply device 30 flows into the accommodation space 22 and is then discharged from the gas exhaust hole 26 and / or the through-hole 28. By creating such an oxygen flow environment around the pre-sintered body 50, it is possible to suppress abnormal heating due to oxygen plasma.
[0067] The susceptor 40 is a heating auxiliary member that can improve the efficiency of microwave heating by efficiently converting microwave energy into thermal energy. Specifically, the susceptor 40 absorbs microwaves and reaches a higher temperature more quickly than the pre-sintered body 50, thereby assisting in the temperature increase of the pre-sintered body 50 through thermal conduction. When the pre-sintered body 50 reaches a high temperature, it becomes easier for the pre-sintered body 50 itself to absorb microwaves and can act as a microwave absorber. When the pre-sintered body 50 becomes easier to absorb microwaves, the internal heating mechanism of the pre-sintered body 50 is more easily promoted by microwave heating. This promotes sintering within the pre-sintered body 50, making it less likely for voids to remain inside, and making it possible to produce a zirconia sintered body with excellent strength and translucency.
[0068] From the viewpoint of raising the temperature of the pre-sintered body 50 in a shorter time, it is preferable to arrange the susceptors 40 in positions sandwiching the pre-sintered body 50 from both sides in a predetermined direction before microwave heating. For example, the susceptors 40 may be arranged on both sides (i.e., the upper and lower sides) of the pre-sintered body 50 in the vertical direction (up and down direction), or on both sides in at least one horizontal direction of the pre-sintered body 50. This allows the surfaces of both sides in the predetermined direction of the pre-sintered body 50 to be heated by the susceptors 40, thereby improving the microwave absorption efficiency of the pre-sintered body 50 in a shorter time. As a result, internal heating of the pre-sintered body 50 by microwave heating can be achieved in a shorter time, thereby further reducing voids within the zirconia sintered body. The susceptor 40 is typically arranged so as to contact the surface of the pre-sintered body 50, but a gap may be present between the susceptor 40 and the surface of the pre-sintered body 50. The gap is not particularly limited, but is preferably 3 mm or less, more preferably 2 mm or less, and even more preferably 1 mm or less.
[0069] Furthermore, it is preferable that the pre-sintered body 50 is not sealed by the susceptor 40. This allows microwaves to be easily absorbed directly into the pre-sintered body 50 without being obstructed by the susceptor 40. Therefore, internal heating of the pre-sintered body can be induced at a lower temperature range than when the susceptor completely encases the pre-sintered body (for example, when the pre-sintered body is placed inside a closed box-shaped susceptor). As a result, the number of pores remaining inside the zirconia sintered body can be reduced compared to sintering caused by heat conduction from the surface. Furthermore, since the pre-sintered body 50 is not sealed by the susceptor 40, it is possible to prevent the oxygen around the pre-sintered body 50 from being consumed and creating a reducing atmosphere.
[0070] Furthermore, it is preferable that the pre-sintered body 50 has no susceptor 40 installed (is open) on both sides of at least one direction different from the predetermined direction in which the susceptor 40 is arranged. This makes it easier for microwaves to be directly absorbed by the pre-sintered body 50, and internal heating can be induced more uniformly from a lower temperature range. Furthermore, by providing one direction in which the susceptor 40 is not installed, the pre-sintered body 50 can be placed in the flow of gas supplied from the gas supplier 30, so that the atmosphere around the pre-sintered body 50 can be more suitably controlled.
[0071] 2, in this embodiment, the pre-sintered body 50 is sandwiched between two plate-shaped susceptors 40 from above and below, and the horizontal side of the pre-sintered body 50 is not covered by the susceptors 40. In this configuration, since no susceptors 40 are arranged on either side of the pre-sintered body 50 in the horizontal direction, microwaves are particularly easily absorbed by the pre-sintered body 50, making it easier to manufacture a zirconia sintered body with reduced internal voids.
[0072] A SiC susceptor primarily composed of silicon carbide (SiC) is preferably used as the susceptor 40. Here, "primarily composed of SiC" refers to a material in which SiC accounts for 50% by mass or more of the compounds constituting the susceptor 40. Examples of SiC susceptors include single-crystal SiC, recrystallized SiC, reaction-sintered SiC, nitride-bonded SiC, oxide-bonded SiC, and silicon carbide fiber. Furthermore, from the viewpoint of enhancing microwave absorption efficiency, recrystallized SiC and silicon carbide fiber, which have relatively high porosity, are preferably used. Among these, recrystallized SiC is particularly preferred due to its excellent heat resistance. Furthermore, even in the case of recrystallized SiC, dense recrystallized SiC may have a reduced microwave absorption efficiency. Therefore, the porosity of recrystallized SiC is preferably, for example, 10% to 90%, and more preferably 10% to 30%. The porosity can be measured by a conventional method, such as mercury intrusion porosimetry.
[0073] When the susceptor 40 is plate-shaped, the thickness of each sheet is preferably, for example, 1 mm to 4 mm, and more preferably 2 mm to 3 mm. If the susceptor 40 is too thin, the strength of the susceptor may decrease. If the susceptor 40 is too thick, the susceptor 40 may be difficult to heat, and the temperature rise rate may be slow. Therefore, within the above thickness range, a good balance is achieved between the strength of the susceptor 40 and the temperature rise rate of the susceptor 40. This makes it possible to more effectively reduce voids inside the zirconia sintered body.
[0074] 2, one plate-shaped susceptor 40 is disposed above and one below the pre-sintered body 50, but the number of plate-shaped susceptors 40 is not particularly limited as long as there are multiple (two or more) of them. For example, two or more susceptors 40 may be stacked on each of the upper and lower sides of the pre-sintered body 50. Also, different numbers of susceptors 40 may be used on the upper and lower sides of the pre-sintered body 50.
[0075] In this embodiment, the susceptor 40 is plate-shaped, but the susceptor 40 is not particularly limited as long as it is disposed on both sides of the pre-sintered body 50 in a predetermined direction. For example, a box-shaped (e.g., hexahedral) susceptor having through-holes on a pair of opposing surfaces, a columnar susceptor (e.g., cylindrical or prismatic), etc. may be used.
[0076] The radiation thermometer 60 can measure the temperature of an object without contact. As shown in FIG. 2 , in this embodiment, the radiation thermometer 60 is installed at a position separate from the microwave heating device 10 and measures the surface temperature of the susceptor 40 above the pre-sintered body 50. In this specification, the heating temperature in the second heating step S30 and the temperature used to calculate the temperature drop rate in the cooling step S40 (described later) refer to the temperatures measured by the radiation thermometer 60. To more accurately measure the temperature change due to microwave heating, it is preferable to fix the radiation thermometer 60 in a predetermined position using a clamp or the like. For example, an OPTCTRF1MHSFVFC3 sensor (pseudo emissivity setting 1.0) manufactured by Optris can be used as the radiation thermometer 60.
[0077] The microwave heating temperature is preferably 1600°C or higher (e.g., above 1600°C), preferably 1630°C or higher, more preferably 1650°C or higher, even more preferably 1700°C or higher (e.g., above 1700°C), and particularly preferably 1720°C or higher. Although the mechanism is not particularly limited, by setting the microwave heating temperature to a high temperature of 1600°C or higher, a dense sintered body is produced in which voids that may occur inside the zirconia sintered body are suppressed. Furthermore, in the crystalline phase of the zirconia sintered body, variation in the crystalline phase can be reduced, and discontinuities at the grain boundaries can be reduced. This is thought to improve the light transmittance because light passing through the zirconia sintered body is less likely to be reflected or refracted at the crystal interfaces. Furthermore, although not particularly limited, from the viewpoint of the heat resistance of the heating device, it is appropriate that the microwave heating temperature be, for example, 2000°C or less, and it can be 1900°C or less, 1800°C or less, 1750°C or less, or 1730°C or less. The microwave heating holding time varies appropriately depending on the shape, size, composition, etc. of the pre-sintered body 50, but can be, for example, about 1 to 20 minutes, or about 1 to 10 minutes. Note that the holding time here does not include the time it takes for the temperature to rise to the microwave heating temperature.
[0078] The microwave heating method is not particularly limited, and either single mode or multimode can be used, but multimode is preferably used. In single mode, depending on the position and size of the pre-sintered body 50, plasma may be generated in the pre-sintered body 50, which may cause cracks in the zirconia sintered body. On the other hand, in multimode, concentration of the electromagnetic field in the heating space 14 is suppressed, making it difficult for plasma to be generated. This can suppress the occurrence of cracks in the zirconia sintered body.
[0079] The heating rate of microwave heating is not particularly limited, as it can be appropriately changed depending on the shape, size, composition, etc. of the pre-sintered body. For example, the heating rate until reaching 1000°C to 1100°C can be set to 500°C / min to 900°C / min, preferably 500°C / min to 700°C / min. This allows the zirconia sintered body to be produced in a shorter time. Thereafter, until reaching 1100°C to 1200°C, the heating rate can be set to, for example, 10°C / min to 50°C / min, preferably 15°C / min to 25°C / min. This can reduce the occurrence of cracks due to rapid sintering of zirconia. Thereafter, until reaching approximately 1600°C to 2000°C, the heating rate can be set to, for example, 40°C / min to 100°C / min, preferably 40°C / min to 60°C / min. This allows the progress of sintering of the pre-sintered body to be appropriately controlled, making it possible to produce a zirconia sintered body with better translucency and resistance to hydrothermal degradation.
[0080] The shape of the pre-sintered body 50 is not particularly limited, but from the viewpoint of more uniform sintering by microwaves, it is preferably, for example, disk-shaped. The thickness of the pre-sintered body 50 is preferably, for example, 0.5 mm to 10 mm, and more preferably 0.5 mm to 2 mm. Within this range, microwave sintering can be carried out efficiently while maintaining the strength of the pre-sintered body 50. Furthermore, the maximum diameter of the pre-sintered body 50 is preferably, for example, 10 mm to 60 mm, and more preferably 10 mm to 20 mm. Within this range, microwave sintering can be carried out more uniformly.
[0081] <Cooling Step S40> In the cooling step S40, the molded body that has been subjected to the second heating step S30 is rapidly cooled to 1300°C. The cooling step S40 is performed after the microwave-heated molded body in the second heating step S30 has been heated to and maintained at a predetermined temperature (e.g., 1600°C to 2000°C), and is typically performed consecutively from the microwave heating. Such rapid cooling allows the zirconia sintered body disclosed herein to be obtained.
[0082] The temperature drop rate when cooling the molded body to 1300°C is, for example, 50°C / min or more, preferably 100°C / min or more, and more preferably 200°C / min or more. The faster the cooling rate, the more improved the hydrothermal degradation resistance. The upper limit of the temperature drop rate is not particularly limited, but may be, for example, 1000°C / min or less, or 500°C / min or less. The cooling method is not particularly limited as long as it can achieve a temperature drop rate within the above range, but examples include microwave irradiation control, natural cooling, and air blowing. In the cooling step S40, if an oxygen-containing gas was supplied from the gas supplier 30 in the second heating step S30, the supply of the gas may be continued or stopped. According to the inventor's investigations, stopping the supply of the gas during temperature drop can facilitate more stable production of zirconia sintered bodies. In this specification, the "temperature decreasing rate" in the cooling step S40 refers to the average temperature decreasing rate from the start of the temperature decrease until the temperature reaches 1300°C.
[0083] As described above, the manufacturing method disclosed herein sinters the molded body by microwave heating, making it possible to obtain a dense zirconia sintered body with few internal voids. Furthermore, by performing microwave heating, the temperature of the heating space itself of the microwave heating device does not become as high as that of the molded body and the susceptor, making it possible to rapidly cool the zirconia sintered body at the temperature drop rate described above, and increasing the proportion of crystalline phases in which the c / a axial length ratio of the unit lattice of the zirconia sintered body is in the range of 1.0055 or more and less than 1.010. As a result, a zirconia sintered body with excellent translucency and resistance to hydrothermal degradation is realized.
[0084] The reason for the excellent translucency and resistance to hydrothermal degradation is not particularly limited, but is presumed to be as follows. In a molded body sintered in a conventional heating furnace where the heating space itself is heated to a high temperature, the cooling rate after sintering is slow, resulting in a mixture of a crystalline phase (e.g., tetragonal) in which the c / a axial length ratio of the unit lattice is greater than 1.012 and less than 1.017, and a crystalline phase (e.g., cubic) in which the c / a axial length ratio of the unit lattice is greater than 1 and less than 1.0055, which tends to result in localized segregation of yttrium concentration. It is generally believed that this segregation induces hydrothermal degradation of zirconia sintered bodies. On the other hand, in this technology, rapid cooling after microwave sintering is presumed to suppress yttrium segregation. As a result, a phase that previously precipitated as a crystalline phase (e.g., cubic) in which the c / a axial length ratio of the unit lattice is in the range of 1 or more and less than 1.0055 is now precipitated as a crystalline phase (e.g., metastable tetragonal) in which the c / a axial length ratio of the unit lattice is in the range of 1.0055 or more and less than 1.010, or a crystalline phase (e.g., tetragonal) in which the c / a axial length ratio of the unit lattice is in the range of more than 1.012 and less than 1.017, which is believed to result in a more homogeneous crystalline structure than conventional ones. A homogeneous crystalline structure is less likely to induce hydrothermal degradation, suppressing the reflection and refraction of light at the crystal interface. Furthermore, microwave heating produces a highly dense zirconia sintered body with few voids, making it difficult for water to penetrate into the zirconia sintered body. From the above, it is presumed that the zirconia sintered body disclosed herein has excellent translucency and resistance to hydrothermal degradation.
[0085] In the zirconia sintered body disclosed herein, when the entire crystalline phase is taken as 100% by mass, the proportion of the crystalline phase having a unit lattice c / a axial length ratio in the range of 1.0055 or more and less than 1.010 is, for example, 10% by mass or more, preferably 15% by mass or more, and more preferably 20% by mass or more. The upper limit of this proportion is not particularly limited, but may be, for example, 50% by mass or less, 40% by mass or less, 30% by mass or less, or 25% by mass or less. If the proportion of such a crystalline phase is 10% by mass or more, the translucency and resistance to hydrothermal degradation tend to be improved.
[0086] In some embodiments, when the entire crystalline phase is taken as 100% by mass, the proportion of crystalline phases having a unit lattice c / a axial length ratio in the range of 1.007 or more and less than 1.010 is, for example, 10% by mass or more, preferably 15% by mass or more, and more preferably 20% by mass or more. The upper limit of this proportion is not particularly limited, but may be, for example, 50% by mass or less, 40% by mass or less, 30% by mass or less, or 25% by mass or less. By having a c / a axial length ratio in this range, hydrothermal degradation resistance can be further improved.
[0087] In the zirconia sintered body disclosed herein, when the entire crystalline phase is taken as 100% by mass, the total proportion of the crystalline phase having a unit lattice c / a axial length ratio in the range of 1.0055 or more and less than 1.010 and the crystalline phase having a unit lattice c / a axial length ratio in the range of more than 1.012 and less than 1.017 is, for example, 75% by mass or more, preferably 85% by mass or more, more preferably 95% by mass or more, particularly preferably 98% by mass or more, or even 100% by mass. The higher this proportion, the more homogeneity of the crystalline structure can be improved, thereby achieving better translucency and hydrothermal degradation resistance.
[0088] In the zirconia sintered body disclosed herein, when the entire crystalline phase is taken as 100% by mass, the proportion of the crystalline phase having a unit lattice c / a axial length ratio in the range of 1 or more and less than 1.0055 may be, for example, 25% by mass or less, more preferably 15% by mass or less, even more preferably 5% by mass or less, particularly preferably 2% by mass or less, or even 0% by mass (not included or below the detection limit). The lower this proportion, the more the segregation of yttrium and / or ytterbium is suppressed, and better translucency and hydrothermal degradation resistance can be achieved.
[0089] In the zirconia sintered body disclosed herein, the proportion of monoclinic crystals after a hydrothermal degradation test in which the body is immersed in hot water at 134°C for 6 hours is, for example, 5% or less, preferably 2% or less, more preferably 1% or less, and particularly preferably 0.5% or less. The hydrothermal degradation test can be performed by immersing a zirconia sintered body with a mirror-polished surface in hot water at 134°C for 6 hours using a high-pressure microreactor (MMS-500, manufactured by OM Labotec Co., Ltd.). The proportion of monoclinic crystals can be measured by obtaining an X-ray diffraction pattern of the polished surface of the zirconia sintered body after the hydrothermal degradation test.
[0090] The translucency of the zirconia sintered body disclosed herein is, for example, a total light transmittance of 44% or more, preferably 44.5% or more, more preferably 45% or more, and even more preferably 46% or more. Furthermore, although not particularly limited, the total light transmittance may be, for example, 60% or less. In this specification, "total light transmittance" refers to the total light transmittance for a D65 light source in the thickness direction of a 1 mm thick disk-shaped test piece.
[0091] As described above, the zirconia sintered body disclosed herein has both excellent translucency and excellent resistance to hydrothermal degradation, and therefore can be suitably used, for example, as a dental material, such as dentures for anterior teeth, dentures for posterior teeth, denture mill blanks, orthodontic brackets, dental prostheses, and bridges.
[0092] As described above, specific aspects of the technology disclosed herein include those described in the following items. Item 1: A method for producing a zirconia sintered body, comprising the following steps: a molded body preparation step of preparing a molded body containing zirconia and yttria and / or ytterbia, wherein the total proportion of yttria and ytterbia is 3 mol% or more and less than 4 mol%, when the total of zirconia, yttria, and ytterbia is 100 mol%; a first heating step of heating the molded body at 800°C or more and 1200°C or less; a second heating step of heating the molded body that has undergone the first heating step at 1600°C or more and 2000°C or less by microwave heating; and a cooling step of cooling the molded body that has undergone the second heating step to 1300°C at a rate of 50°C / min or more. Item 2: The method for producing a zirconia sintered body according to Item 1, wherein the microwave heating is performed in a multi-mode manner. Item 3: The manufacturing method according to Item 1 or 2, wherein the microwave heating in the second heating step is performed in an oxidizing atmosphere. Item 4: The manufacturing method according to Item 3, wherein the microwave heating in the second heating step is performed in an atmosphere having an oxygen concentration of 30 vol% or more and 100 vol% or less. Item 5: The manufacturing method according to any one of Items 1 to 4, wherein, in the second heating step, SiC susceptors are arranged to sandwich the molded body from both sides in a predetermined direction. Item 6: The manufacturing method according to any one of Items 1 to 5, wherein, in the molded body preparing step, the molded body is prepared by molding a material containing granules having zirconia. Item 7: A zirconia sintered body containing zirconia and yttria and / or ytterbia, wherein when the total of the zirconia, yttria, and ytterbia is taken as 100 mol%, the total proportion of yttria and ytterbia is 3 mol% or more and less than 4 mol%, and when the entire crystalline phase is taken as 100 mass%, the proportion of the crystalline phase having a c / a axial length ratio of the unit lattice in the range of 1.0055 or more and less than 1.010 is 10 mass% or more. Item 8: The zirconia sintered body according to Item 7, wherein when the entire crystalline phase is taken as 100 mass%, the proportion of the crystalline phase having a c / a axial length ratio of the unit lattice in the range of 1.007 or more and less than 1.010 is 10 mass% or more.Item 9: The zirconia sintered body according to Item 7 or 8, wherein the proportion of monoclinic crystals after immersion in hot water at 134°C for 6 hours is 10% or less. Item 10: The zirconia sintered body according to any one of Items 7 to 9, wherein, when the entire crystalline phase is taken as 100% by mass, the proportion of crystalline phases having a c / a axial length ratio of the unit lattice in the range of 1 or more and less than 1.0055 is 20% by mass or less. Item 11: The zirconia sintered body according to any one of Items 7 to 10, wherein a 1 mm thick test piece has a total light transmittance of 44% or more in the thickness direction using a D65 light source. Item 12: A dental material comprising the zirconia sintered body according to any one of Items 7 to 11. Item 13: The dental material according to Item 12, which is a denture, a denture mill blank, or an orthodontic bracket.
[0093] Examples of the technology disclosed herein will be described below, but these examples are not intended to limit the technology disclosed herein.
[0094] Example 1: Yttrium chloride was mixed with zirconia sol produced by hydrolysis of a zirconium oxychloride solution. When the yttrium chloride was converted to yttria, the total of zirconia and yttria was 100 mol %, and yttrium chloride was mixed so that the yttria content was 3.3 mol %. This mixture was dried and then calcined at 1120°C for 4 hours to obtain a partially stabilized zirconia powder. This zirconia powder was pulverized in a ball mill using 1 mm diameter zirconia balls and then screened through a mesh sieve to obtain a zirconia powder with an average particle size of 150 nm to 200 nm as a compact material. This zirconia powder was filled into a disc-shaped mold, and a pressure of 0.78 MPa was applied. The compact was then removed from the mold and subjected to CIP molding at 196 MPa. The resulting compact was then heated at 1100°C for 2 hours to obtain a pre-sintered compact. The temperature was increased at a rate of 120°C / h up to 800°C and 100°C / h up to 1100°C.
[0095] The pre-sintered body was placed on a 2 mm thick plate-shaped SiC susceptor, and the 2 mm thick plate-shaped SiC susceptor was placed on the pre-sintered body and then housed in an insulated container. The insulated container had the same configuration as the insulated container 20 shown in FIG. 2. The insulated container was then placed in a microwave heating device. Recrystallized SiC was used as the SiC susceptor. A μ-Reactor EX manufactured by Shikoku Keisoku Kogyo Co., Ltd. was used as the microwave heating device.
[0096] Next, using an MO2 Silent gas supply (manufactured by Kobe Medicare Co., Ltd.), gas with an oxygen concentration of 90 vol% was supplied into the insulated container. Then, while supplying the gas, microwave heating was started, and the temperature was increased to 1000°C at 600°C / min, 1100°C at 20°C / min, and 1730°C at 50°C / min, and maintained at 1730°C for 1 minute. The temperature was then decreased to 1300°C at a rate of 10°C / min, and the microwave heating device was turned off when the temperature reached 1300°C. The gas supply was stopped during the temperature decrease. In this way, the zirconia sintered body of Example 1 was produced. The microwave heating method was multimode. For temperature measurement, an OPTCTRF1MHSFVFC3 sensor manufactured by Optris was used to measure the temperature of the SiC susceptor above the pre-sintered body.
[0097] Example 2 A zirconia sintered body of Example 2 was produced in the same manner as in Example 1, except that the rate of temperature decrease to 1,300° C. after microwave heating was changed to 50° C. / min.
[0098] Example 3 A zirconia sintered body of Example 3 was produced in the same manner as in Example 1, except that the rate of temperature decrease to 1,300° C. after microwave heating was changed to 100° C. / min.
[0099] Example 4 A zirconia sintered body of Example 4 was produced in the same manner as in Example 1, except that the rate of temperature decrease to 1,300° C. after microwave heating was changed to 200° C. / min.
[0100] (Example 5) In the manufacturing method of Example 1, the microwave heating was changed to heating in an electric furnace. Specifically, the temperature of the pre-sintered body was raised to 1500°C at a rate of 120°C / h, held for 120 minutes, and then lowered at a rate of 5°C / min. The remaining operations were the same as in Example 1, and the zirconia sintered body of Example 5 was manufactured.
[0101] (Example 6) The manufacturing method of Example 4 was modified by mixing yttrium chloride so that the yttria content in the zirconia powder was 3.9 mol%, resulting in a zirconia powder with an average particle size of 150 nm to 200 nm. A polyacrylic binder was mixed with the zirconia powder as a binder at 3 mass% of the total. This mixture was granulated by minute drying to obtain zirconia granules with an average particle size of 70 μm. Using these zirconia granules as a compact material, a zirconia sintered body of Example 6 was manufactured in the same manner as in Example 4. However, the sintering temperature by microwave heating was changed from 1730°C to 1630°C.
[0102] (Example 7) In the manufacturing method of Example 6, the microwave heating was changed to heating in an electric furnace. Specifically, the temperature of the pre-sintered body was raised to 1500°C at a rate of 120°C / h, held for 120 minutes, and then lowered at a rate of 5°C / min. The zirconia sintered body of Example 7 was manufactured by the same procedures as in Example 6 except for these.
[0103] Example 8: Yttrium chloride and ytterbium chloride were mixed with zirconia sol produced by hydrolysis of a zirconia oxychloride solution. The yttrium chloride and ytterbium chloride were mixed so that the yttria was 1.7 mol% and the ytterbia was 1.8 mol%, assuming that the total of zirconia, yttria, and ytterbia was 100 mol%. The mixture was dried and then calcined at 1120°C for 4 hours to obtain a partially stabilized zirconia powder. The zirconia powder was pulverized in a ball mill using 1 mm diameter zirconia balls and then screened through a mesh sieve to obtain a zirconia powder with an average particle size of 150 nm to 200 nm as a compact material. Zirconia granules were then produced in the same manner as in Example 6. The zirconia granules were filled into a disk-shaped mold, and a pressure of 0.78 MPa was applied. The molded body was then removed from the mold and subjected to CIP molding at 196 MPa. The resulting molded body was then heated at 1100°C for 2 hours to obtain a pre-sintered body. The heating rate was 120°C / h up to 800°C and 100°C / h up to 1100°C. Microwave heating was then performed in the same manner as in Example 1, followed by a temperature decrease rate of 200°C / min down to 1300°C, yielding the zirconia sintered body of Example 8. However, the maximum sintering temperature of microwave heating was changed to 1640°C. The microwave heating conditions were also changed: 600°C / min up to 1000°C, 20°C / min up to 1100°C, and 50°C / min up to 1730°C, followed by a 1-minute hold at 1730°C.
[0104] Example 9: In the manufacturing method of Example 8, the microwave heating was changed to heating in an electric furnace. Specifically, the temperature of the pre-sintered body was increased to 1500°C at a rate of 120°C / h, held for 120 minutes, and then decreased at a rate of 5°C / min. The remaining operations were the same as in Example 8, and the zirconia sintered body of Example 9 was manufactured.
[0105] <Crystalline Phase Analysis> An X-ray diffraction pattern profile of the zirconia sintered body produced in each example was obtained using an X'Pert Pro Alpha-1 (manufactured by Malvern Paralytical) as an X-ray diffractometer. The measurement conditions were as follows: Radiation source: CuKα1 (45 kV 40 mA) Measurement range: 10°≦2θ≦90° Scan rate: 1.5° / min Step size: 0.0131°
[0106] The obtained XRD profile was subjected to Rietveld analysis using analysis software: RIETAN-FP, and the c / a axis length ratio of the unit cell and the proportion (mass%) of the crystalline phase were analyzed. The analysis was performed on a mixed phase of tetragonal, metastable tetragonal, and cubic, and the temperature parameters for each element were the same. Note that the metastable tetragonal phase referred to here is a crystalline phase in which only the a-axis length and c-axis length of the tetragonal phase differ. The results are shown in Table 1.
[0107] <Evaluation of Translucency> The zirconia sintered body produced in each example was processed into a disk-shaped test piece with a thickness of 1 mm, and both sides of the test piece were mirror-polished using diamond slurry (average particle size 0.5 μm) as an abrasive, and then the total light transmittance of a D65 light source in the thickness direction was measured. For this measurement, a haze meter NDH4000 manufactured by Nippon Denshoku Industries Co., Ltd. was used. The results are shown in Table 1.
[0108] <Hydrothermal Degradation Test> The zirconia sintered body produced in each example was measured for monoclinic fraction (%) after hydrothermal treatment according to the method shown below. Specifically, first, the surface of the zirconia sintered body was mirror-polished with diamond slurry (average particle size 0.5 μm). Next, the polished sintered body was subjected to hydrothermal degradation treatment at 140 ° C for 100 hours using a device named: High-Pressure Microreactor (manufactured by OM Labotec Co., Ltd.). Thereafter, the X-ray diffraction pattern of the polished surface was measured using an X-ray diffractometer (device named: Ultima IV, manufactured by Rigaku Corporation). Then, using the measurement results, the monoclinic fraction (%) was calculated using the following formula. As can be understood from the following formula, the monoclinic fraction is determined by the X-ray diffraction peak intensity [I m (111)], and the X-ray diffraction peak intensity corresponding to the monoclinic phase (11-1) plane [I m(11-1)], and the sum of the X-ray diffraction peak intensities corresponding to the (111) plane of a crystal phase other than the monoclinic phase [I o (111)]. The results are shown in Table 1. [Monoclinic crystal ratio (%)] = {I m (111) + I m (11-1)} / {I m (111) + I m (11-1) + I o (111)} × 100 The conditions for the X-ray diffraction device were as follows: Radiation source: CuKα (40 kV 40 mA) Measurement range: 26°≦2θ≦38° Scan rate: 2.0° / min Step size: 0.02°
[0109]
[0110] As shown in Table 1, in Examples 1 to 5, the rate of temperature decrease from the maximum sintering temperature to 1300°C was set to 50°C / min or more, which resulted in a decrease in the monoclinic fraction after hydrothermal degradation and improved resistance to hydrothermal degradation of the zirconia sintered body. This is thought to be due to the fact that when the rate of temperature decrease from the maximum sintering temperature to 1300°C was set to 50°C / min or more, the zirconia sintered body had a crystalline phase in which the c / a axial length ratio of the unit lattice was in the range of 1.0055 or more and less than 1.010.
[0111] Furthermore, as shown in Examples 2 to 4, when the temperature drop rate to 1300 ° C. was increased, the crystalline phase with a c / a axial length ratio of 1.0066 in Example 2 shifted to a crystalline phase with a c / a axial length ratio of 1.0070 in Example 3, and to a crystalline phase with a c / a axial length ratio of 1.0074 in Example 4. Furthermore, among Examples 2 to 4, the monoclinic fraction after hydrothermal degradation was lower in Examples 3 and 4 than in Example 2. From this, it can be seen that in the range of the c / a axial length ratio of the unit lattice being 1.0055 or more but less than 1.010, a zirconia sintered body having a crystalline phase with a relatively high c / a axial length ratio (for example, a c / a axial length ratio of 1.0070 or more) has improved resistance to hydrothermal degradation.
[0112] Examples 6 and 7 are test examples of zirconia sintered bodies in which the proportion of yttria is higher than in Examples 1 to 5. In this case as well, as shown in Example 6, it is clear that a zirconia sintered body having excellent permeability and resistance to hydrothermal degradation can be realized.
[0113] Examples 8 and 9 are test examples of zirconia sintered bodies containing ytterbia. In these cases, too, as shown in Example 8, it is clear that a zirconia sintered body having excellent permeability and resistance to hydrothermal degradation can be realized.
[0114] While specific examples of the technology disclosed herein have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above.
[0115] REFERENCE SIGNS LIST 10 Microwave heating device 12 Partition wall 14 Heating space 16 Through-hole 20 Heat-insulating container 22 Storage space 24 Gas inlet hole 26 Gas outlet hole 28 Through-hole 30 Gas supplier 32 Pump 40 Susceptor 50 Pre-sintered body 60 Radiation thermometer
Claims
1. A method for producing a zirconia sintered body, comprising the following steps: a molded body preparation step of preparing a molded body containing zirconia and yttria and / or ytterbia, in which the total ratio of yttria and ytterbia is 3 mol% or more and less than 4 mol% when the total of zirconia, yttria, and ytterbia is 100 mol%; a first heating step of heating the molded body at 800°C or more and 1200°C or less; a second heating step of heating the molded body that has undergone the first heating step at 1600°C or more and 2000°C or less by microwave heating; and a cooling step of lowering the temperature of the molded body that has undergone the second heating step to 1300°C at a rate of 50°C / min or more.
2. The method according to claim 1, wherein the microwave heating is performed in a multi-mode manner.
3. The manufacturing method according to claim 1 or 2, wherein in the second heating step, the microwave heating is carried out in an oxidizing atmosphere.
4. The manufacturing method according to claim 3, wherein in the second heating step, the microwave heating is carried out in an atmosphere having an oxygen concentration of 30 vol.% or more and 100 vol.% or less.
5. A manufacturing method according to claim 1 or 2, wherein in the second heating step, SiC susceptors are positioned to sandwich the molded body from both sides in a predetermined direction.
6. The manufacturing method according to claim 1 or 2, wherein in the compact preparation step, the compact is prepared by molding a material containing granules having zirconia.
7. A zirconia sintered body containing zirconia and yttria and / or ytterbia, wherein when the total of zirconia, yttria, and ytterbia is 100 mol%, the total ratio of yttria and ytterbia is 3 mol% or more and less than 4 mol%, and when the entire crystal phase is 100 mass%, the ratio of the crystal phase having a c / a axial length ratio of the unit lattice in the range of 1.0055 or more and less than 1.010 is 10 mass% or more.
8. The zirconia sintered body according to claim 7, wherein the proportion of the crystalline phase having a c / a axial length ratio of the unit lattice in the range of 1.007 or more and less than 1.010 is 10 mass % or more when the entire crystalline phase is taken as 100 mass %.
9. The zirconia sintered body according to claim 7, having a monoclinic ratio of 10% or less after immersion in hot water at 134°C for 6 hours.
10. A zirconia sintered body as described in claim 7, in which the proportion of the crystalline phase having a c / a axial length ratio of the unit lattice in the range of 1 or more and less than 1.0055 is 20 mass% or less, when the entire crystalline phase is taken as 100 mass%.
11. The zirconia sintered body according to claim 7, having a total light transmittance of 44% or more in the thickness direction of a test piece having a thickness of 1 mm for a D65 light source.
12. A dental material comprising the zirconia sintered body according to any one of claims 7 to 11.
13. The dental material of claim 12 which is a denture, a denture mill blank, or an orthodontic bracket.
Citation Information
Patent Citations
Densification of ceramic materials using ultra-high frequency electromagnetic waves and container for performing the method
JP2006513963A
Method and device for densifying ceramics
JP2010025452A
Zirconia sintered compact, sintering composition for the same and calcined object
JP2011178610A
Translucent zirconia sintered body and manufacturing method thereof and application thereof
JP2017105689A
Zirconia sintered body and manufacturing method therefor
JP2018052806A