Display device

The integration of a colored layer and ultraviolet shielding layer, combined with Eu²⁺ activated phosphors, addresses the degradation issues in display devices, maintaining brightness and color accuracy over time by shielding dyes from heat and UV exposure, achieving high color gamut coverage.

WO2024247895A1PCT designated stage expired Publication Date: 2024-12-05TOPPAN HOLDINGS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019079
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Display devices with wavelength conversion layers face challenges in maintaining brightness and achieving high color reproducibility over long-term use due to degradation of specific wavelength-absorbing dyes from heat and external light, particularly ultraviolet rays.

Method used

Incorporating a colored layer with specific wavelength-absorbing dyes between the wavelength conversion layer and the viewer, and an ultraviolet shielding layer to reduce degradation, along with using Eu²⁺ activated phosphors in the wavelength conversion layer, which have wider emission spectra and are less prone to deterioration.

Benefits of technology

The solution effectively suppresses brightness reduction and maintains high color reproducibility by protecting the dyes from heat and UV exposure, ensuring 90% or more coverage of the BT.2020 color gamut even after long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019079_05122024_PF_FP_ABST
    Figure JP2024019079_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a display device in which a decrease in brightness is suppressed and an image can be displayed with high color reproducibility even after a long period of use. This display device (1A) comprises: a light-emitting diode (23); a color filter (33) that includes a red filter part (33R), a green filter part (33G), and a blue filter part (33B); a wavelength conversion layer that includes a first wavelength conversion part (36R) and a second wavelength conversion part (36G), each wavelength conversion unit containing an Eu2+ activated phosphor; a functional layer that faces the light-emitting diode (23) with the color filter (33) and the wavelength conversion layer interposed therebetween and includes an ultraviolet shielding layer (51) having a JIS L1925:2019-compliant ultraviolet shielding rate of 85% or more; and a colored layer (52) that is interposed between the functional layer and the color filter (33) and includes a first color material having a maximum absorption wavelength within the range of 560-620 nm and an absorption spectrum half-value width within the range of 15-55 nm.
Need to check novelty before this filing date? Find Prior Art

Description

display device

[0001] The present invention relates to a display device.

[0002] Phosphors such as quantum dot phosphors emit light at a wavelength different from that of the excitation light when irradiated with the excitation light, and are therefore used, for example, as wavelength conversion materials. For example, in the backlight of a liquid crystal display device, a blue light emitting diode and a quantum dot phosphor are used, and part of the blue light emitted by the blue light emitting diode is converted into red light and green light by the phosphor (Patent Documents 1 to 3).

[0003] Japanese Patent Publication No. 2013-544018 Japanese Patent Publication No. 2017-21349 Japanese Patent Publication No. 2022-60064

[0004] An object of the present invention is to provide a display device that is capable of suppressing a decrease in brightness and displaying images with high color reproducibility even after long-term use.

[0005] According to one aspect of the present invention, there is provided a light emitting device comprising: a substrate; a plurality of light emitting diodes disposed on the substrate and having equal emission spectra; and a plurality of filter sections including a red filter section, a green filter section, and a blue filter section, the plurality of filter sections including color filters facing the plurality of light emitting diodes, a first wavelength conversion section positioned between the red filter section and the light emitting diode facing it, and a second wavelength conversion section positioned between the green filter section and the light emitting diode facing it, each of the first wavelength conversion section and the second wavelength conversion section being made of Eu. 2+ Provided is a display device comprising: a wavelength conversion layer containing an activated phosphor; a functional layer including an ultraviolet blocking layer that faces the plurality of light-emitting diodes with the color filter and the wavelength conversion layer sandwiched therebetween and has an ultraviolet blocking rate of 85% or more in accordance with JIS L1925:2019; and a coloring layer interposed between the functional layer and the color filter, including a first color material that has a maximum absorption wavelength in the range of 560 to 620 nm and a half-width of an absorption spectrum in the range of 15 to 55 nm.

[0006] According to another aspect of the present invention, the plurality of light emitting diodes are near-ultraviolet light emitting diodes, and the wavelength conversion layer further includes a third wavelength conversion portion positioned between the blue filter portion and the light emitting diode facing the blue filter portion, the third wavelength conversion portion being made of Eu. 2+ A display device according to the above aspect is provided which contains an activated phosphor.

[0007] According to yet another aspect of the present invention, there is provided the display device according to any one of the above aspects, wherein the plurality of light emitting diodes are blue light emitting diodes.

[0008] According to yet another aspect of the present invention, CIE 1976 L * u * v * a coverage rate of the BT.2020 color gamut in the CIE 1931 color system and a coverage rate of the BT.2020 color gamut in the CIE 1976 u'v' color system each being 90% or more, and wherein RY is a stimulus value Y in the CIE 1931 color system of light incident on a surface of the red filter portion facing the light emitting diode, RY' is a stimulus value Y in the CIE 1931 color system of light emitted from a surface of the red filter portion opposite to the surface facing the light emitting diode, GY is a stimulus value Y in the CIE 1931 color system of light incident on a surface of the green filter portion facing the light emitting diode, and There is provided a display device according to any of the above aspects, wherein GY' is the stimulus value Y in the CIE 1931 color system of light emitted from the surface opposite to the surface facing the light-emitting diode, BY is the stimulus value Y in the CIE 1931 color system of light incident on the surface of the blue filter part facing the light-emitting diode, and BY' is the stimulus value Y in the CIE 1931 color system of light emitted from the surface of the blue filter part opposite to the surface facing the light-emitting diode, and satisfy the relationship shown in the following inequality (1).

[0009]

[0010] According to yet another aspect of the present invention, the wavelength conversion layer 2+ In the display device according to any one of the above aspects, the activated phosphor has a particle size in the range of 0.1 to 15 μm.

[0011] According to yet another aspect of the present invention, there is provided a display device according to any of the above aspects, wherein the colored layer further includes at least one of a second colorant having a maximum absorption wavelength in the range of 470 to 530 nm and a half-width of an absorption spectrum in the range of 15 to 45 nm, and a third colorant having a wavelength in the wavelength range of 400 to 780 nm with the lowest transmittance in the range of 650 to 780 nm.

[0012] According to yet another aspect of the present invention, there is provided a display device according to any of the above aspects, wherein the colored layer further contains one or more selected from the group consisting of a radical scavenger, a singlet oxygen quencher, and a peroxide decomposer.

[0013] According to yet another aspect of the present invention, there is provided a display device according to any one of the above aspects, wherein the colored layer contains a polymer having a repeating unit represented by the following formula (i):

[0014]

[0015] Here, R 12 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 13 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.

[0016] According to yet another aspect of the present invention, there is provided a display device according to any of the above aspects, wherein the colored layer includes one or more compounds selected from the group consisting of dialkyldithiophosphates, dialkyldithiocarbanates, benzenedithiols, transition metal complexes thereof, and compounds represented by the following formula (ii):

[0017]

[0018] Here, R 1 are each independently an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, or R 9 CO - , R 10 SO 2 - or R 11 NHCO - R represents a group represented by 9 , R 10 , and R 11 R each independently represents an alkyl group, an alkenyl group, an aryl group, or a heterocyclic group. 2 and R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, or an alkenyloxy group; R 4 ~R 8 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an aryl group.

[0019] According to yet another aspect of the present invention, there is provided a display device according to any of the above aspects, wherein the colored layer contains one or more compounds selected from the group consisting of compounds having any of a porphyrin structure, a merocyanine structure, a phthalocyanine structure, an azo structure, a cyanine structure, a squarylium structure, a coumarin structure, a polyene structure, a quinone structure, a tetradiporphyrin structure, a pyrromethene structure, and an indigo structure, and metal complexes thereof.

[0020] According to yet another aspect of the present invention, there is provided a display device according to any one of the above aspects, wherein the functional layer functions as an anti-reflection layer or an anti-glare layer.

[0021] According to yet another aspect of the present invention, there is provided a display device according to any of the above aspects, wherein the functional layer further includes an antistatic layer or an antifouling layer facing the colored layer with the ultraviolet blocking layer sandwiched therebetween.

[0022] According to the present invention, a display device is provided that is capable of suppressing a decrease in brightness and displaying images with high color reproducibility even after long-term use.

[0023] 1 is a cross-sectional view of a display device according to a first embodiment of the present invention. * u * v * 3 is a graph showing the BT.2020 color gamut in the color system. 3 is a cross-sectional view of a display device according to a second embodiment of the present invention.

[0024] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects, either singly or in combination.

[0025] Furthermore, the embodiments shown below are merely examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of ​​the present invention within the technical scope defined by the claims.

[0026] In the drawings, elements having the same or similar functions are denoted by the same reference numerals, and redundant explanations will be omitted. Furthermore, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, and the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual relationship.

[0027] <1> First Embodiment FIG. 1 is a cross-sectional view of a display device according to a first embodiment of the present invention. The display device 1A shown in FIG. 1 is a micro LED display capable of color display using an active matrix driving method, with each sub-pixel including a light-emitting diode (LED). In FIG. 1, the X and Y directions are parallel to the display surface of the display device 1A and intersect with each other. In one example, the X and Y directions are perpendicular to each other. The Z direction is perpendicular to the X and Y directions. That is, the Z direction is the thickness direction of the display device 1A.

[0028] The display device 1A shown in FIG. 1 includes a display panel DPA, a surface protection member 5, and an adhesive layer 6.

[0029] The display panel DPA includes a light control device 2A, a black matrix substrate 3, and an adhesive layer 4.

[0030] The light control device 2A is a device that emits light toward the black matrix substrate 3 and is capable of adjusting at least one of the intensity of the light and the time for emitting the light for each pixel or each subpixel. The light control device 2A includes a substrate 21, a multilayer wiring layer 22, and a light-emitting diode 23.

[0031] The substrate 21 includes, for example, an insulating substrate such as a glass substrate. The substrate 21 may further include an undercoat layer provided on the main surface of the insulating substrate facing the black matrix substrate 3. The undercoat layer is, for example, a laminate of a silicon nitride layer and a silicon oxide layer sequentially stacked on the insulating substrate. The substrate 21 may also be a semiconductor substrate such as a silicon substrate. The substrate 21 may be either rigid or flexible.

[0032] The multilayer wiring layer 22 is provided on the main surface of the substrate 21 facing the black matrix substrate 3. The multilayer wiring layer 22 includes video signal lines, first power supply lines, second power supply lines, scanning signal lines, pixel circuits, and an interlayer insulating film.

[0033] The video signal lines each extend in the Y direction and are arranged in the X direction. The scanning signal lines each extend in the X direction and are arranged in the Y direction. The first and second power supply lines each extend in the Y direction and are arranged in the X direction in correspondence with the video signal lines. The first and second power supply lines may each extend in the X direction and be arranged in the Y direction in correspondence with the scanning signal lines. Alternatively, one of the first and second power supply lines may each extend in the Y direction and be arranged in the X direction in correspondence with the video signal lines, and the other may each extend in the X direction and be arranged in the Y direction in correspondence with the scanning signal lines.

[0034] The pixel circuits are arranged in the X and Y directions on the main surface of the substrate 21. Each pixel circuit includes a drive control element, a switch, and a capacitor. The drive control element is, for example, a p-channel field effect transistor having a source connected to a first power supply line. The switch is, for example, an n-channel field effect transistor having a gate connected to a scanning signal line, a source connected to a video signal line, and a drain connected to the gate of the drive control element. The capacitor is, for example, a thin-film capacitor having one electrode connected to the gate of the drive control element and the other electrode connected to the first power supply line. The pixel circuits may have other configurations.

[0035] The light-emitting diode 23 has a multi-layer structure. Here, the stacking direction of the layers included in the light-emitting diode 23 is the Z direction. This stacking direction may be perpendicular to the Z direction.

[0036] The light emitting diodes 23 have the same emission spectrum. The light emitting diodes 23 emit light of short wavelengths such as blue light and ultraviolet light. Here, as an example, the light emitting diodes 23 are assumed to be blue light emitting diodes that emit blue light.

[0037] The light emitting diodes 23 are arranged corresponding to the pixel circuits on the multi-layer wiring layer 22. The anode of each of the light emitting diodes 23 is connected to the drain of the drive control element, and the cathode is connected to the second power supply line.

[0038] The black matrix substrate 3 faces the light control device 2A. Specifically, the black matrix substrate 3 faces the substrate 21 with the light emitting diodes 23 and the like sandwiched therebetween.

[0039] The black matrix substrate 3 includes a transparent substrate 31, a black matrix 32, a partition layer 34, a color filter 33 including a red filter portion 33R, a green filter portion 33G, and a blue filter portion 33B, and a wavelength conversion layer including a first wavelength conversion portion 36R, a second wavelength conversion portion 36G, and a filling portion 36B.

[0040] The transparent substrate 31 is transparent to visible light. The transparent substrate 31 is, for example, a colorless substrate. The transparent substrate 31 may have a single-layer structure or a multi-layer structure. The transparent substrate 31 is made of, for example, glass, a transparent resin, or a combination thereof. The transparent substrate 31 may be rigid or flexible. The transparent substrate 31 has a first main surface facing the light control device 2A and a second main surface that is the back surface of the first main surface.

[0041] The black matrix 32 is provided on the first main surface of the transparent substrate 31. The black matrix 32 is a black layer that blocks visible light. The black matrix 32 is made of, for example, a mixture containing a binder resin and a colorant. The colorant is, for example, a black pigment or a mixture of pigments that exhibit black through subtractive color mixing, for example, a mixture containing a blue pigment, a green pigment, and a red pigment.

[0042] The black matrix 32 has first through holes at the positions of the light emitting diodes 23. The opening of each first through hole on the transparent substrate 31 side has a larger dimension in the direction perpendicular to the Z direction than the light emitting diodes 23.

[0043] The red filter portion 33R, the green filter portion 33G, and the blue filter portion 33B form a stripe arrangement on the transparent substrate 31 provided with the black matrix 32. These form a plurality of pixels, each consisting of the red filter portion 33R, the green filter portion 33G, and the blue filter portion 33B, and these pixels are arranged in the X direction and the Y direction.

[0044] Here, the red filter portion 33R and the green filter portion 33G are red colored layers and green colored layers, respectively. The blue filter portion 33B is a colorless light-transmitting layer or a blue colored layer. Each of the red filter portions 33R fills one of the first through holes. Each of the green filter portions 33G fills another of the first through holes. Each of the blue filter portions 33B fills yet another of the first through holes.

[0045] The partition wall layer 34 is provided on a color filter 33 including a red filter portion 33R, a green filter portion 33G, and a blue filter portion 33B. According to one example, the partition wall layer 34 is transparent. In this case, the partition wall layer 34 may be colored or colorless. The partition wall layer 34 may have light scattering properties.

[0046] The partition layer 34 has second through holes at the positions of the first through holes, respectively. Here, the second through holes are provided such that the outline of the orthogonal projection of the opening on the transparent substrate 31 side onto the first main surface (hereinafter referred to as the second outline) surrounds the outline of the orthogonal projection of the first through hole onto the first main surface (hereinafter referred to as the first outline). The second outline does not have to surround the first outline. In a structure in which the second outline surrounds the first outline, the effect of stray light on display is smaller than in a structure in which the second outline does not surround the first outline.

[0047] The portion of the partition layer 34 that is sandwiched between adjacent second through holes has a rectangular cross-sectional shape. This portion may have a forward tapered cross-sectional shape, a reverse tapered cross-sectional shape, or another cross-sectional shape.

[0048] The partition wall layer 34 may have a multi-layer structure. For example, the partition wall layer 34 may include a resin layer and a reflective layer that covers at least a part of the surface of the resin layer.

[0049] The reflective layer may have a single-layer structure or a multi-layer structure. The layers included in the reflective layer are, for example, metals, alloys, or transparent dielectrics. The reflective layer made of a metal or alloy is, for example, made of aluminum or an aluminum alloy.

[0050] The first wavelength-converting portion 36R is provided on the red filter portion 33R. The first wavelength-converting portion 36R is made of Eu, which is an inorganic phosphor. 2+ The first wavelength-converting portion 36R is a layer containing an activated phosphor and a transparent resin. Here, the first wavelength-converting portion 36R converts the blue light emitted by the light-emitting diode 23 into red light.

[0051] Eu contained in the first wavelength conversion portion 36R 2+ The activated phosphor is, for example, SrCaAlSiN 3 :Eu, (Ba, Sr, Ca) 3 SiO 5 :Eu, (Ba, Sr, Ca) 2 (Si, Al) 5 N 8 :Eu or (Ca,Sr)AlSi(O,N) 3 The transparent resin contained in the first wavelength-converting portion 36R is, for example, a hardened product of a silicone resin or an acrylic resin having a siloxane bond (Si—O—Si bond) as the main chain.

[0052] The second wavelength-converting portion 36G is provided on the green filter portion 33G. The second wavelength-converting portion 36G is made of Eu, an inorganic phosphor. 2+ The second wavelength converter 36G is a layer containing an activated phosphor and a transparent resin. Here, the second wavelength converter 36G converts the blue light emitted by the light emitting diode 23 into green light.

[0053] Eu contained in the second wavelength conversion portion 36G 2+ The activated phosphor is, for example, (Ba,Sr)Ga 2 S 4 :Eu, (Ba, Sr, Ca, Mg) 2 SiO 4 :Eu, SiAlON:Eu (β-sialon), or (Ca, Sr) 8 Mg(SiO 4 ) 4 Cl 2 The transparent resin contained in the second wavelength-converter 36G is, for example, the same as the transparent resin contained in the first wavelength-converter 36R.

[0054] The filling portion 36B is provided on the blue filter portion 33B. As described above, the filling portion 36B is a colorless and transparent layer. In this case, the filling portion 36B is made of, for example, a transparent resin. The transparent resin contained in the filling portion 36B is, for example, the same as the transparent resin contained in the first wavelength-converting portion 36R.

[0055] As described above, the light emitting diode 23 is a blue light emitting diode that emits blue light. When the light emitting diode 23 is an ultraviolet light emitting diode that emits ultraviolet light, for example, a near-ultraviolet light emitting diode, the Eu contained in the first wavelength conversion unit 36R is 2+ Eu contained in the activated phosphor and the second wavelength conversion portion 36G 2+ The activated phosphor converts the ultraviolet light emitted by the light-emitting diode 23 into red light and green light, respectively. In this case, the filler 36B is a third wavelength conversion layer that converts the ultraviolet light emitted by the light-emitting diode 23 into blue light.

[0056] The filling portion 36B as the third wavelength conversion layer contains, in addition to a transparent resin, an inorganic phosphor, Eu 2+ The third wavelength conversion layer may further include an activated phosphor. 2+ The activated phosphor is, for example, (Sr, Ba, Ca, Mg) 10 (P.O. 4 ) 6 Cl 2 :Eu, BaMgAl 10 O 17 : Eu, Sr 10 (P.O. 4 ) 6 Cl 2 : Eu or Ba 2 P.O. 4 Cl:Eu.

[0057] Each wavelength conversion layer contains Eu 2+ The particle size of the activated phosphor is preferably in the range of 0.1 to 15 μm, more preferably in the range of 1 to 10 μm. 2+ The particle diameter of the activated phosphor is defined as the particle diameter at 50% of the cumulative value in the particle size distribution obtained by photon correlation spectroscopy. Simply put, the particle diameter is the arithmetic mean value of the diameters of the phosphor particles observed by observing a predetermined area of ​​the cross section of the wavelength conversion layer with a scanning microscope.

[0058] Each wavelength conversion layer is made of a transparent resin and Eu 2+ Eu in the total amount of activated phosphor 2+ The proportion of the activated phosphor is preferably in the range of 5 to 70% by mass, and more preferably in the range of 30 to 50% by mass.

[0059] The adhesive layer 4 is interposed between the light control device 2A and the black matrix substrate 3, and bonds them together. The adhesive layer 4 transmits light emitted by the light-emitting diodes 23. The adhesive layer 4 is, for example, a colorless and transparent layer. The adhesive layer 4 is made of an adhesive or a pressure-sensitive adhesive.

[0060] The surface protection member 5 is provided on the front surface of the display panel DPA. The surface protection member 5 is transparent to visible light and covers the front surface of the display panel DPA. The surface protection member 5 is, for example, a film, a sheet, or a plate.

[0061] The surface protective member 5 includes an ultraviolet blocking layer 51, a colored layer 52, a first surface layer 53, and a second surface layer 54. The colored layer 52, the ultraviolet blocking layer 51, the first surface layer 53, and the second surface layer 54 are laminated in this order. The surface protective member 5 is disposed such that the ultraviolet blocking layer 51 faces the black matrix substrate 3 with the colored layer 52 sandwiched therebetween.

[0062] The ultraviolet ray blocking layer 51 is transparent to visible light and transmits visible light from the display panel DPA that has passed through the colored layer 52. The ultraviolet ray blocking rate of the ultraviolet ray blocking layer 51 is 85% or more, preferably 90% or more, more preferably 95% or more, and may be 100%. The ultraviolet ray blocking layer 51 prevents ultraviolet rays from outside the display device 1A from entering the colored layer 52, thereby making it difficult for the colored layer 52 to deteriorate due to ultraviolet rays.

[0063] Here, the ultraviolet ray shielding rate is a value measured and calculated based on JIS L1925:2019, and is expressed as a value (%) obtained by subtracting the average transmittance (%) in the wavelength range of 290 to 400 nm from 100%.

[0064] 1 as the first embodiment also serves as a substrate. The thickness of the ultraviolet-shielding layer 51 is not particularly limited, but is preferably in the range of 10 to 100 μm. The thickness of each layer included in the surface protection member 5 can be determined by observing a cross section of the surface protection member 5 parallel to the thickness direction with a microscope such as an electron microscope.

[0065] The ultraviolet ray blocking layer 51 includes a transparent material having ultraviolet ray absorbing properties, or includes a transparent material having or not having ultraviolet ray absorbing properties and an ultraviolet ray absorbing agent.

[0066] Transparent materials that can be used for the ultraviolet shielding layer 51 include polyolefins such as polyethylene and polypropylene, polyesters such as polybutylene terephthalate and polyethylene naphthalate, polyacrylates such as polymethyl methacrylate, polyamides such as nylon 6 and nylon 66, polyimides, polyarylates, polycarbonates, triacetyl cellulose, polyacrylates, polyvinyl alcohol, polyvinyl chloride, cycloolefin copolymers, norbornene-containing resins, polyether sulfones, polysulfones, and transparent resins, as well as inorganic glass. Among these, films made of polyethylene terephthalate (PET), films made of triacetyl cellulose (TAC), films made of polymethyl methacrylate (PMMA), and films made of polyesters can be preferably used.

[0067] The ultraviolet absorber is not particularly limited, but benzophenone-based, benzotriazole-based, triazine-based, oxalic acid anilide-based, and cyanoacrylate-based compounds can be used. As a benzotriazole-based ultraviolet absorber, for example, 2-(2H-benzotriazol-2-yl)-4-methylphenol can be used. As a triazine-based ultraviolet absorber, for example, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol can be used.

[0068] The colored layer 52 is located between the display panel DPA and the ultraviolet blocking layer 51. The colored layer 52 exhibits low transmittance in one or more wavelength ranges in the visible range and high transmittance in one or more other wavelength ranges in the visible range. Specifically, the colored layer 52 exhibits high transmittance in the wavelength range of light emitted by each subpixel of the display panel DPA and low transmittance in at least part of the other wavelength ranges. In addition to serving as such an optical filter, the colored layer 52 may also serve as an adhesive layer.

[0069] The thickness of the colored layer 52 is preferably in the range of 0.5 to 10 μm. Increasing the thickness of the colored layer 52 reduces the effect of the coloring material (described later) on the smoothness of the colored layer 52 and increases the uniformity of the distribution of the coloring material in the colored layer 52. Furthermore, a thin colored layer 52 is advantageous for reducing the thickness of the display device 1A.

[0070] The colored layer 52 includes a first color material. The colored layer 52 can further include at least one of a second color material and a third color material. Here, as an example, the colored layer 52 includes all of the first color material, the second color material, and the third color material.

[0071] The colored layer 52 further contains a transparent material that dissolves or disperses the color material in. The transparent material is, for example, a cured resin obtained by curing an active energy ray curable resin, which will be described later.

[0072] The colored layer 52 can be obtained, for example, by applying a colored layer-forming composition to one main surface of the ultraviolet-shielding layer 51 and curing the coating. The colored layer-forming composition contains, for example, an active energy ray-curable resin and the above-mentioned coloring material. When such a colored layer-forming composition is used, the coating can be cured by irradiating it with active energy rays such as ultraviolet rays and electron beams.

[0073] The first colorant has a maximum absorption wavelength in the range of 560 to 620 nm and a half-width of the absorption spectrum in the range of 15 to 55 nm. Here, the maximum absorption wavelength refers to the wavelength that gives the maximum of the maximum values ​​of light absorptance in the light absorptance spectrum (absorption spectrum). This maximum absorption wavelength is the wavelength that gives the smallest of the minimum values ​​in the light transmittance spectrum. The same applies hereinafter to the maximum absorption wavelength.

[0074] If the maximum absorption wavelength of the first coloring material is less than the lower limit, the green light emitted by the second wavelength-converter 36G is absorbed by the coloring layer 52 to a large extent, resulting in a decrease in the luminance efficiency of the green light emitted. If the maximum absorption wavelength of the first coloring material is greater than the upper limit, the red light emitted by the first wavelength-converter 36R is absorbed by the coloring layer 52 to a large extent, resulting in a decrease in the luminance efficiency of the red light emitted.

[0075] If the half width of the absorption spectrum of the first coloring material is less than the lower limit, the effect of suppressing reflection of external light is reduced. If the half width of the absorption spectrum of the first coloring material is greater than the upper limit, the luminance efficiency is reduced.

[0076] The second coloring material has a maximum absorption wavelength in the range of 470 to 530 nm and an absorption spectrum half width in the range of 15 to 45 nm.

[0077] If the maximum absorption wavelength of the second coloring material is less than the lower limit, the blue light emitted from the filling section 36B is absorbed by the coloring layer 52 to a large extent, resulting in a decrease in the luminance efficiency of the blue light emitted. If the maximum absorption wavelength of the second coloring material is greater than the upper limit, the green light emitted from the second wavelength-converting section 36G is absorbed by the coloring layer 52 to a large extent, resulting in a decrease in the luminance efficiency of the green light emitted.

[0078] If the half width of the absorption spectrum of the second coloring material is less than the lower limit, the effect of suppressing reflection of external light is reduced, whereas if the half width of the absorption spectrum of the second coloring material is greater than the upper limit, the luminance efficiency is reduced.

[0079] The third coloring material has a wavelength in the range of 650 to 780 nm at which the transmittance is lowest within the wavelength range of 400 to 780 nm. The half width of the absorption spectrum of the third coloring material is, for example, in the range of 10 to 300 nm, but is not particularly limited thereto.

[0080] If the wavelength at which the third coloring material exhibits the lowest transmittance in the wavelength range of 400 to 780 nm is set below the lower limit, the red light emitted by the first wavelength converter 36R is absorbed by the coloring layer 52 to a large extent, reducing the luminance efficiency of the red light emission. If the wavelength at which the third coloring material exhibits the lowest transmittance in the wavelength range of 400 to 780 nm is set above the upper limit, the effect of suppressing reflection of external light is reduced.

[0081] The colored layer 52 may contain, as at least one of the first color material, the second color material, and the third color material, one or more compounds selected from the group consisting of compounds having any of a porphyrin structure, a merocyanine structure, a phthalocyanine structure, an azo structure, a cyanine structure, a squarylium structure, a coumarin structure, a polyene structure, a quinone structure, a tetradiporphyrin structure, a pyrromethene structure, and an indigo structure, and metal complexes thereof. In particular, it is preferable to use a compound having a porphyrin structure, a pyrromethene structure, a phthalocyanine structure, or a squarylium structure in its molecule.

[0082] These compounds or metal complexes thereof may be contained in the first coloring material, the second coloring material, the third coloring material, or two or more of these coloring materials.

[0083] For the purpose of adjusting color tone or transmittance, in addition to the first, second, and third coloring materials, coloring materials with wide half-widths or pigments without selective wavelength-selective absorption properties may be used in combination, as long as they do not significantly affect the light emission.

[0084] An active energy ray-curable resin is a resin that polymerizes and hardens when irradiated with active energy rays such as ultraviolet rays or electron beams. The active energy ray-curable resin may contain, for example, a monofunctional, difunctional, trifunctional or higher functional (meth)acrylate monomer, a urethane (meth)acrylate, etc. Here, "(meth)acrylate" means both or either one of "acrylate" and "methacrylate."

[0085] Examples of monofunctional (meth)acrylate compounds that can be contained in the active energy ray-curable resin include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfuryl acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and the like. ) acrylate, isobornyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phosphate (meth)acrylate, ethylene oxide-modified phosphate (meth)acrylate, phenoxy (meth)arylate, ethylene oxide-modified phenoxy (meth)acrylate ) acrylate, propylene oxide modified phenoxy (meth)acrylate, nonylphenol (meth)acrylate, ethylene oxide modified nonylphenol (meth)acrylate, propylene oxide modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl (meth ) acrylate, 2-(meth)acryloyloxyethyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hexahydrohydrogen phthalate, 2-(meth)acryloyloxypropyl tetrahydrohydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate,Examples include adamantane derivative mono(meth)acrylates such as adamantyl acrylate having a monovalent mono(meth)acrylate derived from 2-adamantane or adamantanediol. Here, "(meth)acryloyl" means both or either "acryloyl" and "methacryloyl."

[0086] Examples of bifunctional (meth)acrylate compounds that can be contained in the active energy ray-curable resin include di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate.

[0087] Examples of trifunctional or higher (meth)acrylate compounds that can be contained in the active energy ray-curable resin include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris-2-hydroxyethyl isocyanurate tri(meth)acrylate, and glycerin tri(meth)acrylate, and trifunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate. Examples of the (meth)acrylate compound include tri- or higher functional (meth)acrylate compounds such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ditrimethylolpropane hexa(meth)acrylate, as well as polyfunctional (meth)acrylate compounds in which a portion of these (meth)acrylates is substituted with an alkyl group or ε-caprolactone.

[0088] Urethane (meth)acrylate can also be used as a resin that can be contained in the active energy ray-curable resin. Examples of the urethane (meth)acrylate include those obtained by reacting a product obtained by reacting a polyester polyol with an isocyanate monomer or prepolymer, and then reacting the product with a (meth)acrylate monomer having a hydroxyl group.

[0089] Examples of urethane (meth)acrylates include pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate toluene diisocyanate urethane prepolymer, pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, and dipentaerythritol pentaacrylate isophorone diisocyanate urethane prepolymer.

[0090] The monofunctional, difunctional, trifunctional or higher functional (meth)acrylate monomers, urethane (meth)acrylates, etc. may be used alone or in combination of two or more thereof. They may also be partially polymerized oligomers.

[0091] The color layer-forming composition and the color layer 52 may contain one or more of a radical scavenger, a singlet oxygen quencher, and a peroxide decomposer.

[0092] The radical scavenger captures radicals that occur when the coloring material is oxidized and deteriorates, thereby suppressing autoxidation. Therefore, by including a radical scavenger in the coloring layer 52, deterioration of the coloring material, i.e., fading of the coloring layer 52, can be suppressed.

[0093] The radical scavenger may be an additive or resin having an amine structure. Here, the "amine structure" refers to a structure in which the hydrogen atom of ammonia is substituted with a hydrocarbon group or an aromatic atomic group. Examples of the amine structure include primary amines, secondary amines, and tertiary amines, and may also be quaternary ammonium cations.

[0094] For example, when a hindered amine light stabilizer with a molecular weight of 2000 or more is used as an additive having an amine structure as a radical scavenger, a high anti-fading effect can be obtained. If the molecular weight of the radical scavenger is low, it is likely to volatilize. Therefore, in this case, few molecules remain in the colored layer, making it difficult to obtain a sufficient anti-fading effect. The molecular weight of the hindered amine light stabilizer is, for example, about 200,000, but the upper limit is not particularly limited. In this specification, "molecular weight" means the "mass average molecular weight" measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0095] Examples of additives having an amine structure that are preferably used as radical scavengers include Chimassorb (registered trademark) 2020FDL, Chimassorb (registered trademark) 944FDL, and Tinuvin (registered trademark) 622, all manufactured by BASF, and LA-63P, all manufactured by ADEKA Corporation.

[0096] The active energy ray-curable resin, the colored layer-forming composition, and the colored layer 52 preferably contain, as at least a part of the radical scavenger, a polymer whose repeating unit contains a structure represented by the following formula (i):

[0097]

[0098] Here, R 12 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 13represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.

[0099] R 12 is preferably a hydrogen atom, a hydroxy group, or an alkyl group having 10 or less carbon atoms. The number of carbon atoms in the alkyl group is preferably in the range of 1 to 6, and more preferably in the range of 1 to 3.

[0100] R 13 is preferably a hydrogen atom or an alkyl group having 10 or less carbon atoms. The number of carbon atoms in the alkyl group is preferably in the range of 1 to 6, and more preferably in the range of 1 to 3.

[0101] X is preferably a single bond or an aliphatic alkyl chain having 30 or less carbon atoms. The number of carbon atoms in the aliphatic alkyl chain is preferably 10 or less, more preferably in the range of 1 to 6, and even more preferably in the range of 2 to 4.

[0102] The polymer having a repeating unit containing the structure shown in formula (i) may be a copolymer further containing any of the repeating units described below. By including the additional repeating unit, the compatibility with other components can be controlled.

[0103] Examples of the additional repeating unit include (meth)acrylate repeating units, olefin repeating units, halogen atom-containing repeating units, styrene repeating units, vinyl acetate repeating units, and vinyl alcohol repeating units.

[0104] Examples of the (meth)acrylate repeating unit include a repeating unit derived from a (meth)acrylate monomer having a linear or branched alkyl group on the side chain, and a repeating unit derived from a (meth)acrylate monomer having a hydroxyl group on the side chain.

[0105] Examples of repeating units derived from (meth)acrylate monomers having a linear or branched alkyl group on the side chain include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, and isooctyl (meth)acrylate. Examples of monomer-derived components include octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, myristyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, and octadecyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above, (meth)acrylate-based repeating units having a linear or branched alkyl group having 1 to 4 carbon atoms on the side chain are preferred.

[0106] Examples of repeating units derived from (meth)acrylic monomers having a hydroxyl group in the side chain include components derived from monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxyphenyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0107] Examples of the olefin repeating unit include components derived from olefin monomers such as ethylene, propylene, isoprene, butadiene, etc. These may be used alone or in combination of two or more.

[0108] Examples of the halogen atom-containing repeating unit include components derived from monomers such as vinyl chloride, vinylidene chloride, etc. These may be used alone or in combination of two or more.

[0109] Examples of the styrene repeating unit include components derived from styrene monomers such as styrene, α-methylstyrene, vinyltoluene, etc. These may be used alone or in combination of two or more.

[0110] Examples of vinyl acetate repeating units include esters of saturated carboxylic acids with vinyl alcohol, such as vinyl acetate and vinyl propionate. These may be used alone or in combination of two or more.

[0111] An example of the vinyl alcohol repeating unit is vinyl alcohol, which may have a 1,2-glycol bond in the side chain.

[0112] The copolymer may have any of a random copolymer, an alternating copolymer, a block copolymer, and a graft copolymer structure. If the copolymer has a random copolymer structure, the manufacturing process and preparation with other components are easy. Therefore, a random copolymer is preferable to other copolymers.

[0113] Radical polymerization can be used as a polymerization method for obtaining the copolymer. Radical polymerization is preferred because it is easy to produce industrially. Radical polymerization may be a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a suspension polymerization method, or the like. For radical polymerization, it is preferable to use a solution polymerization method. By using a solution polymerization method, it is easy to control the molecular weight of the copolymer.

[0114] In the radical polymerization, the above-mentioned monomer may be diluted with a solvent, and then a polymerization initiator may be added to polymerize the monomer.

[0115] The solvent may be, for example, an ester-based solvent, an alcohol ether-based solvent, a ketone-based solvent, an aromatic solvent, an amide-based solvent, or an alcohol-based solvent. Examples of the ester-based solvent include methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, t-butyl acetate, methyl lactate, and ethyl lactate. Examples of the alcohol ether-based solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, 3-methoxy-1-butanol, and 3-methoxy-3-methyl-1-butanol. Examples of the ketone-based solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. Examples of the aromatic solvent include benzene, toluene, and xylene. Examples of the amide-based solvent include formamide and dimethylformamide. The alcohol-based solvent may be, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, s-butanol, t-butanol, diacetone alcohol, 2-methyl-2-butanol, etc. Among the above-mentioned solvents, one type may be used alone, or two or more types may be mixed and used.

[0116] The radical polymerization initiator may be, for example, a peroxide or an azo compound. The peroxide may be, for example, benzoyl peroxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, di-t-butyl peroxide, etc. The azo compound may be, for example, azobisisobutyronitrile, azobisamidinopropane salt, azobiscyanovaleric acid (salt), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], etc.

[0117] The amount of radical polymerization initiator used is preferably in the range of 0.0001 to 20 parts by mass, more preferably in the range of 0.001 to 15 parts by mass, and even more preferably in the range of 0.005 to 10 parts by mass, relative to 100 parts by mass of the total amount of monomers. The radical polymerization initiator may be added to the monomers and solvent before the start of polymerization, or may be added dropwise to the polymerization reaction system. Adding the radical polymerization initiator dropwise to the monomers and solvent in the polymerization reaction system is preferred in that heat generation due to polymerization can be suppressed.

[0118] The reaction temperature for the radical polymerization is appropriately selected depending on the type of radical polymerization initiator and solvent, and is preferably in the range of 60 to 110° C. from the viewpoints of ease of production and reaction controllability.

[0119] When the resin having an amine structure with radical scavenging ability is a polymer containing a structural unit represented by formula (i), the content of the structural unit represented by formula (i) is preferably in the range of 1 to 95 mol %, and more preferably in the range of 10 to 90 mol %, relative to the total molar amount of the monomers constituting the active energy ray-curable resin. When the content of the structural unit represented by formula (i) is within the above numerical range, the light resistance and heat resistance of the colored layer 52 are improved, and fading is easily suppressed.

[0120] The singlet oxygen quencher inactivates highly reactive singlet oxygen, which tends to oxidize and deteriorate color materials. Therefore, by incorporating a singlet oxygen quencher into the active energy ray-curable resin, it is possible to suppress deterioration of the color material, i.e., to suppress fading of the color layer 52.

[0121] Examples of singlet oxygen quenchers include transition metal complexes, dyes, amines, phenols, and sulfides. A suitable material is a transition metal complex of dialkyl phosphate, dialkyl dithiocarbamate, or benzenedithiol, and nickel, copper, or cobalt is preferably used as the central metal. Examples include NKX1199, NKX113, and NKX114 manufactured by Hayashibara Biochemical Laboratories, Inc., and D1781, B1350, B4360, and T3204 manufactured by Tokyo Chemical Industry Co., Ltd.

[0122] Furthermore, a compound represented by the following formula (ii) can also be suitably used as the singlet oxygen quencher.

[0123]

[0124] Here, R 1 each independently represents an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, R 9 CO-, R 10 SO 2 - and R 11 NHCO—, and R 9 , R 10 , and R 11 are each independently an alkyl group, an alkenyl group, an aryl group, or a heterocyclic group; R 2 and R 3 are each independently any one of a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, and an alkenyloxy group, and R 4 ~R 8 are each independently any of a hydrogen atom, an alkyl group, an alkenyl group, and an aryl group.

[0125] The peroxide decomposer decomposes the peroxide generated when the coloring material is oxidized and deteriorates, thereby stopping the auto-oxidation cycle. Therefore, by including an oxide decomposer in the coloring layer 52, deterioration of the coloring material, i.e., fading of the coloring layer 52, can be suppressed.

[0126] As the peroxide decomposer, for example, a phosphorus-based antioxidant or a sulfur-based antioxidant can be used.

[0127] Examples of phosphorus-based antioxidants include 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]dioxaphosphepine.

[0128] Examples of sulfur-based antioxidants include 2,2-bis({[3-(dodecylthio)propionyl]oxy}methyl)-1,3-propanediyl-bis[3-(dodecylthio)propionate], 2-mercaptobenzimidazole, dilauryl-3,3′-thiodipropionate, dimyristyl-3,3′-thiodipropionate, distearyl-3,3′-thiodipropionate, pentaerythrityl-tetrakis(3-laurylthiopropionate), and 2-mercaptobenzothiazole.

[0129] The content of the active energy ray-curable resin is preferably 20 to 80 mass %, more preferably 30 to 70 mass %, relative to the total mass of the color layer-forming composition. When the content of the active energy ray-curable resin is equal to or greater than the above-mentioned lower limit, the effect of inhibiting fading can be further enhanced. When the content of the active energy ray-curable resin is equal to or less than the above-mentioned upper limit, the handleability of the color layer-forming composition can be further enhanced.

[0130] The first surface layer 53 is provided on the ultraviolet ray blocking layer 51. The first surface layer 53 faces the colored layer 52 with the ultraviolet ray blocking layer 51 sandwiched therebetween.

[0131] The second surface layer 54 is provided on the first surface layer 53. The second surface layer 54 faces the ultraviolet blocking layer 51 with the first surface layer 53 sandwiched therebetween.

[0132] In the surface protection member 5, the ultraviolet-shielding layer 51, the first surface layer 53, and the second surface layer 54 constitute a functional layer. The functional layer is a layer that exhibits an ultraviolet-absorbing function and, optionally, one or more other functions. The one or more other functions may be, for example, one or more of an anti-reflection function, an anti-glare function, an anti-static function, an anti-fouling function, and a strengthening function.

[0133] The functional layer may have a single-layer structure or a multi-layer structure. When the functional layer has a multi-layer structure, the layers included in the functional layer may exhibit different functions or the same function. Each layer included in the functional layer may exhibit only one function or may exhibit multiple functions.

[0134] The functional layer may not include one or both of the first surface layer 53 and the second surface layer 54. That is, the surface protection member 5 may not include one or both of the first surface layer 53 and the second surface layer 54. Alternatively, the surface protection member 5 may further include one or more other layers.

[0135] Here, the first surface layer 53 is a hard coat layer that exhibits a reinforcing function. Examples of the hard coat layer include a layer formed of a hard coat agent containing a monofunctional, bifunctional, trifunctional or higher functional (meth)acrylate or urethane (meth)acrylate.

[0136] In this example, the second surface layer 54 is a low-refractive index layer that exhibits an anti-reflection function. The low-refractive index layer has a refractive index in the visible range that is lower than that of the layer in contact with the surface facing the display panel DPA.

[0137] The low refractive index layer contains lithium fluoride (LiF) and magnesium fluoride (MgF 2 ), sodium hexafluoroaluminum (cryolite, cryolite, 3NaF·AlF 3 , Na 3 AlF 6 ), aluminum fluoride (AlF 3), silica fine particles, etc. may be blended. As the silica fine particles, the use of porous silica fine particles or hollow silica fine particles having voids inside the particles is effective in lowering the refractive index of the low refractive index layer. Furthermore, the composition for forming the low refractive index layer (composition for forming the low refractive index layer) may be appropriately blended with the photopolymerization initiator, solvent, and additives described above for the colored layer.

[0138] The low refractive index layer preferably has a refractive index in the visible range of 1.20 to 1.55.

[0139] The thickness of the low refractive index layer is not particularly limited, but is preferably in the range of 40 nm to 1 μm.

[0140] When the functional layer exhibits an antiglare function, it can include an antiglare layer. The antiglare layer has fine irregularities on its surface, which scatter external light and reduce glare, improving display quality. When the antiglare layer is combined with a low refractive index layer, the combination of these forms an antireflection layer.

[0141] The antiglare layer contains one or more kinds of particles selected from organic fine particles and inorganic fine particles, as needed.

[0142] Organic fine particles are materials that form fine irregularities on the surface and impart the function of scattering external light. Examples of organic fine particles include resin particles made of light-transmitting resin materials such as acrylic resin, polystyrene resin, styrene-(meth)acrylic acid ester copolymer, polyethylene resin, epoxy resin, silicone resin, polyvinylidene fluoride, and polyethylene fluoride resin. In order to adjust the refractive index and dispersibility of the resin particles, two or more types of resin particles made of different materials (refractive indexes) may be mixed and used.

[0143] Inorganic fine particles are materials that control the sedimentation and aggregation of organic fine particles. Examples of inorganic fine particles that can be used include silica fine particles, metal oxide fine particles, and various mineral fine particles. Examples of silica fine particles that can be used include colloidal silica and silica fine particles surface-modified with reactive functional groups such as (meth)acryloyl groups.

[0144] As the metal oxide fine particles, for example, fine particles made of alumina (aluminum oxide), zinc oxide, tin oxide, antimony oxide, indium oxide, titania (titanium dioxide), zirconia (zirconium dioxide), etc. can be used.

[0145] Examples of mineral fine particles that can be used include fine particles made of mica, synthetic mica, vermiculite, montmorillonite, iron-montmorillonite, bentonite, beidellite, saponite, hectorite, stevensite, nontronite, magadiite, ailalite, kanemite, layered titanic acid, smectite, synthetic smectite, etc. The mineral fine particles may be either natural or synthetic (including substituted products and derivatives), or a mixture of both.

[0146] Among mineral fine particles, layered organic clay is particularly preferred. Layered organic clay refers to a swelling clay in which organic onium ions are introduced between the layers. The organic onium ions are not limited as long as they can be organized by utilizing the cation exchange property of the swelling clay. When a layered organic clay mineral is used as the mineral fine particles, the above-mentioned synthetic smectite can be preferably used. Synthetic smectite has the function of increasing the viscosity of the coating liquid for forming the antiglare layer, suppressing the sedimentation of resin particles and inorganic fine particles, and adjusting the uneven shape of the surface of the antiglare layer.

[0147] When the functional layer exhibits an antistatic function, it may include an antistatic layer, such as a layer containing fine particles of metal oxides such as antimony-doped tin oxide (ATO) and tin-doped indium oxide (ITO), a polymer-type conductive composition, or an antistatic agent such as a quaternary ammonium salt.

[0148] When the functional layer has a multilayer structure including an antistatic layer, the antistatic layer may be the outermost layer of the functional layer, or may be interposed between the ultraviolet-shielding layer and one or more other layers included in the functional layer. Alternatively, when the functional layer includes a layer that exhibits a function other than antistatic, an antistatic agent may be blended into this layer to allow this layer to further exhibit an antistatic function.

[0149] When the surface protective member 5 includes a layer that exhibits an antistatic function, the surface resistance value of the surface protective member 5 is 1.0×10 6 ~1.0×10 12 It is preferably in the range of Ω / cm.

[0150] When the functional layer exhibits an anti-fouling function, it may include an anti-fouling layer as the outermost layer. The anti-fouling layer enhances the anti-fouling properties of the surface protective member 5 by imparting water repellency and / or oil repellency to the surface protective member 5. Examples of the anti-fouling layer include layers containing an anti-fouling agent such as silicon oxide, a fluorine-containing silane compound, a fluoroalkylsilazane, a fluoroalkylsilane, a fluorine-containing silicon compound, or a perfluoropolyether group-containing silane coupling agent. When the functional layer includes a layer exhibiting a function other than anti-fouling as the outermost layer, an anti-fouling agent may be blended into this outermost layer to further enhance the anti-fouling function of this layer.

[0151] The adhesive layer 6 is interposed between the display panel DPA and the surface protection member 5. The adhesive layer 6 bonds the surface protection member 5 to the display panel DPA. The adhesive layer 6 is, for example, a colorless and transparent layer. The adhesive layer 6 is made of an adhesive or a pressure-sensitive adhesive. If the colored layer 52 also functions as an adhesive or a pressure-sensitive adhesive layer, the adhesive layer 6 can be omitted.

[0152] The display device 1A described above is capable of suppressing a decrease in brightness and displaying images with high color reproducibility even after long-term use, as will be described below.

[0153] The phosphor contained in the wavelength conversion layer generally has a wide half-width of light emission, which makes it difficult for a display device including the wavelength conversion layer to display images with high color reproducibility, even when using a color filter.

[0154] High color reproducibility can be achieved by incorporating a coloring material (specific wavelength absorbing dye) that absorbs light in a specific wavelength range into the wavelength conversion layer and narrowing the half-width of the light emitted from the wavelength conversion layer. However, the inventors have found that the specific wavelength absorbing dye has low light resistance and heat resistance, and therefore, when the above-mentioned configuration is adopted, the specific wavelength absorbing dye is deteriorated by heat applied to the wavelength conversion layer during the manufacturing process of the display device, heat applied to the wavelength conversion layer from elements included in the display device, such as light-emitting diodes, during use, and external light incident on the wavelength conversion layer during use.

[0155] Quantum dot phosphors have a narrower half-width of emission compared to general phosphors. Therefore, it is believed that high color reproducibility can be achieved by incorporating quantum dot phosphors into a wavelength conversion layer. However, quantum dot phosphors are prone to deterioration in luminescence characteristics during processes such as exposure and firing during wavelength conversion layer formation, and are also prone to oxidative degradation in the air. Therefore, wavelength conversion layers containing quantum dot phosphors have the problem of being difficult to stably manufacture with high luminous efficiency.

[0156] In the display device 1A, the phosphor contained in the wavelength conversion layer is Eu 2+ Use activated phosphor. Eu 2+ The activated phosphor has a wide half-value width of emission, but is less likely to suffer from deterioration in emission characteristics during processes such as exposure and firing when forming the wavelength conversion layer, and is also less likely to suffer from oxidation degradation in the air atmosphere.

[0157] Furthermore, in the display device 1A, a colored layer 52 is disposed between the wavelength conversion layer and the viewer, and the colored layer 52 contains a specific wavelength absorbing pigment. The colored layer 52 can reduce the half-width of light emitted by sub-pixels corresponding to one or more of the first wavelength conversion section 36R, the second wavelength conversion section 36G, and the filler section 36B. For example, the colored layer 52 reduces the half-width of light emitted by each of the sub-pixels corresponding to the first wavelength conversion section 36R, the second wavelength conversion section 36G, and the filler section 36B.

[0158] Furthermore, in the display device 1A, the coloring layer 52 can be provided after the wavelength conversion layer is formed, which prevents the specific wavelength absorbing dye from being deteriorated by heat applied when the wavelength conversion layer is formed.

[0159] Furthermore, in the display device 1A, a wavelength conversion layer, a color filter 33, etc. are interposed between the colored layer 52 and the light-emitting diode 23. In this structure, the distance from the heat source such as the light-emitting diode 23 to the specific wavelength absorbing pigment is large, so that the specific wavelength absorbing pigment is less likely to deteriorate due to heat applied from elements included in the display device such as the light-emitting diode during use.

[0160] In the display device 1A, the ultraviolet ray blocking layer 51 is disposed between the colored layer 52 and the viewer, so that the specific wavelength absorbing dye is less likely to be deteriorated by ultraviolet rays incident on the wavelength conversion layer during use.

[0161] Therefore, the display device 1A is capable of suppressing a decrease in brightness and displaying images with high color reproducibility even after long-term use. For example, the display device 1A may have the following display characteristics.

[0162] That is, CIE1976 L * u * v * The coverage of the BT.2020 color gamut in the color system and the coverage of the BT.2020 color gamut in the CIE 1931 u'v' color system are each 90% or more. RY is the stimulus value Y in the CIE 1931 color system of light incident on the surface of the red filter portion 33R facing the light-emitting diode 23; RY' is the stimulus value Y in the CIE 1931 color system of light emitted from the surface of the red filter portion 33R opposite to the surface facing the light-emitting diode 23; GY is the stimulus value Y in the CIE 1931 color system of light incident on the surface of the green filter portion 33G facing the light-emitting diode 23; GY', which is the stimulus value Y in the CIE 1931 color system of light emitted from the surface opposite to the surface facing the diode 23, BY, which is the stimulus value Y in the CIE 1931 color system of light incident on the surface of the blue filter portion 33B facing the light-emitting diode 23, and BY', which is the stimulus value Y in the CIE 1931 color system of light emitted from the surface of the blue filter portion 33B opposite to the surface facing the light-emitting diode 23, satisfy the relationship shown in inequality (1) below.

[0163]

[0164] Here, CIE 1976 L * u * v * The BT.2020 color gamut in the color system is the color gamut surrounded by the dashed line in Figure 2. That is, CIE1976 L * u * v * The BT.2020 color gamut in the color system is the area enclosed by the line segments connecting the red coordinates (u', v') = (0.557, 0.517), green coordinates (u', v') = (0.056, 0.587), and blue coordinates (u', v') = (0.159, 0.126), which correspond to the three primary colors of the BT.2020 standard values ​​expressed in the CIE (International Commission on Illumination) 1976 color system. In FIG. 2, the solid lines represent the monochromatic light locus and the pure purple locus.

[0165] <2> Second Embodiment FIG. 3 is a cross-sectional view of a display device according to a second embodiment of the present invention.

[0166] 3 is similar to the display device 1A described above, except that it includes a display panel DPB instead of the display panel DPA. The display panel DPB is similar to the display panel DPA, except for the following points.

[0167] That is, the display panel DPB does not include the black matrix substrate 3 and the adhesive layer 4. The display panel DPB includes a dimming device 2B instead of the dimming device 2A. The dimming device 2B is similar to the dimming device 2A except that it further includes a black matrix 32, a color filter 33, a partition layer 34, a first wavelength-converting section 36R, a second wavelength-converting section 36G, a filling section 36B, a planarizing layer 37, and a protective layer 38.

[0168] The partition layer is provided on the multi-layer wiring layer 22. The light-emitting diodes are located in through holes provided in the partition layer .

[0169] The first wavelength-converting portion 36R, the second wavelength-converting portion 36G, and the filling portion 36B fill the through-holes provided in the partition layer 34. The light-emitting diodes 23 are embedded in the first wavelength-converting portion 36R, the second wavelength-converting portion 36G, and the filling portion 36B.

[0170] The planarization layer 37 covers the partition layer 34, the first wavelength-converting portion 36R, the second wavelength-converting portion 36G, and the filling portion 36B. The planarization layer 37 is made of, for example, a colorless and transparent resin. The planarization layer 37 provides a flat base for the black matrix 32 and the color filter 33.

[0171] The black matrix 32 is provided on the planarizing layer 37. The black matrix 32 has openings at the positions of the through holes provided in the partition wall layer .

[0172] The color filter 33 is provided on the planarizing layer 37 and the black matrix 32. The red filter portion 33R, the green filter portion 33G, and the blue filter portion 33B face the first wavelength converting portion 36R, the second wavelength converting portion 36G, and the filling portion 36B, respectively, with the planarizing layer 37 sandwiched therebetween.

[0173] The protective layer 38 is provided on the color filter 33. The protective layer 38 is made of, for example, a colorless and transparent material.

[0174] The display device 1B is substantially the same as the display device 1A, except that the black matrix substrate 3 and the adhesive layer 4 are omitted, and the black matrix 32, the color filter 33, the partition layer 34, the first wavelength-converting section 36R, the second wavelength-converting section 36G, the filling section 36B, the planarizing layer 37, and the protective layer 38 are provided as parts of the light control device. Therefore, the display device 1B can achieve the effects described above for the display device 1A.

[0175] Tests conducted in connection with the present invention will be described below. In the following, "parts" represent parts by mass.

[0176] (1) Preparation of Photosensitive Composition The photosensitive composition used for forming the color filter layer was prepared by the method described below.

[0177] (1.1) Preparation of Micronized Pigment (1.1.1) Preparation of Micronized Pigment R-1 A red micronized pigment R-1 was prepared by the following method. That is, 500 parts of an anthraquinone-based red pigment C.I. Pigment Red 177 (Cinilex (registered trademark) Red SR3C manufactured by Cinilex), 500 parts of sodium chloride, and 250 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 120°C for 8 hours. Next, this kneaded mixture was added to 5 liters of warm water and stirred for 1 hour while heating to 70°C to form a slurry. Thereafter, filtration and washing with water were repeated to remove sodium chloride and diethylene glycol, and the mixture was dried at 80°C for 24 hours. In this manner, a micronized pigment R-1 was obtained.

[0178] (1.1.2) Preparation of Micronized Pigment G-1 Micronized pigment G-1 was prepared by the following method. That is, 100 parts of halogenated zinc phthalocyanine pigment C.I. Pigment Green 58 ("FASTOGEN (registered trademark) GREEN A110" manufactured by DIC Corporation), 1,200 parts of sodium chloride, and 120 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho) and kneaded at 70°C for 6 hours. This kneaded mixture was added to 3,000 parts of warm water and stirred for 1 hour while heating to 70°C to form a slurry. Thereafter, the mixture was repeatedly filtered and washed with water to remove sodium chloride and diethylene glycol, and then dried at 80°C for 24 hours. In this manner, micronized pigment G-1 was obtained.

[0179] (1.1.3) Preparation of Micronized Pigment G-2 Micronized pigment G-2 was obtained in the same manner as described above for micronized pigment G-1, except that halogenated zinc phthalocyanine pigment C.I. Pigment Green 59 (manufactured by DIC Corporation, "FASTOGEN (registered trademark) GREEN C100") was used instead of halogenated zinc phthalocyanine pigment C.I. Pigment Green 58.

[0180] (1.1.4) Preparation of Micronized Pigment Y-1 Micronized pigment Y-1 was prepared by the following method. That is, 100 parts of a metal complex yellow pigment C.I. Pigment Yellow 150 ("Yellow Pigment E4GN" manufactured by Lanxess), 1,600 parts of sodium chloride, and 190 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 60°C for 10 hours. Next, this mixture was added to 3 liters of warm water, and stirred with a high-speed mixer for about 1 hour while heating to about 80°C to form a slurry. Thereafter, filtration and washing with water were repeated to remove sodium chloride and the solvent, and the mixture was dried at 80°C for 24 hours. In this manner, micronized pigment Y-1 was obtained.

[0181] (1.1.5) Preparation of Micronized Pigment B-1 Micronized pigment B-1 was prepared by the following method. That is, 100 parts of C.I. Pigment Blue 15:3 ("Lionol (registered trademark) Blue FG-7351" manufactured by Toyocolor Co., Ltd.), 1,000 parts of ground salt, and 100 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho) and kneaded at 50°C for 12 hours. This mixture was added to 3,000 parts of warm water, and stirred with a high-speed mixer for about 1 hour while heating to about 70°C to form a slurry. Thereafter, the mixture was repeatedly filtered and washed with water to remove the salt and solvent, and then dried at 80°C for 24 hours. In this manner, micronized pigment B-1 was obtained.

[0182] (1.2) Preparation of Resin Dispersant Solution A resin dispersant solution was prepared by the following method. A reaction vessel equipped with a gas inlet tube, a condenser, a stirring blade, and a thermometer was charged with 3 parts of trimellitic anhydride, 1 part of 3-mercapto-1,2-propanediol, 50 parts of propylene glycol monomethyl ether acetate, and 0.1 parts of dimethylbenzylamine. The gas in the reaction vessel was replaced with nitrogen gas, and then the liquid in the reaction vessel was heated at 120°C for 4 hours, and then heated at 80°C for 2 hours. Next, 30 parts of tertiary butyl acrylate, 20 parts of ETERNACOLL (registered trademark) OXMA ((3-ethyloxetan-3-yl)methyl methacrylate, manufactured by Ube Industries, Ltd.), 5 parts of methacrylic acid, 40 parts of ethyl acrylate, and 10 parts of propylene glycol monomethyl ether acetate were charged into a reaction vessel, and while the liquid in the reaction vessel was maintained at 80°C, 0.2 parts of 2,2'-azobisisobutyronitrile was added to this liquid in 15 portions every 30 minutes. The nonvolatile content was measured one hour after the final addition, and it was confirmed that 95% of the monomers had reacted. Thereafter, propylene glycol monomethyl ether acetate was added to this so that the nonvolatile content was 20% by mass. This resulted in a 20% solution of a resin-type dispersant having a carboxyl group, an acid value per nonvolatile content of 51 mgKOH / g, and a weight average molecular weight (Mw) of 24,000.

[0183] (1.3) Preparation of Binder Resin Solution The binder resin solution was prepared by the following method. That is, 196 parts of cyclohexanone were charged into a reaction vessel consisting of a separable four-neck flask equipped with a thermometer, a condenser, a nitrogen gas inlet tube, a dropping tube, and a stirrer, and the temperature was raised to 80 ° C. After the gas in the reaction vessel was replaced with nitrogen, a mixture consisting of 37.2 parts of n-butyl methacrylate, 12.9 parts of 2-hydroxyethyl methacrylate, 12.0 parts of methacrylic acid, 20.7 parts of paracumylphenol ethylene oxide-modified acrylate ("Aronix (registered trademark) M110" manufactured by Toagosei Co., Ltd.), and 1.1 parts of 2,2'-azobisisobutyronitrile was added dropwise to the liquid in the reaction vessel from the dropping tube over 2 hours. After the completion of the dropping, the reaction was continued for 3 hours to obtain a solution of binder resin (non-photosensitive randomly polymerized acrylic resin). After cooling to room temperature, approximately 2 parts of the solution was sampled and heated at 180°C for 20 minutes to measure the nonvolatile content. Propylene glycol monomethyl ether acetate was then added to the remaining solution to achieve a nonvolatile content of 20% by weight. This resulted in a binder resin solution with a nonvolatile content of 20%. The weight-average molecular weight (Mw) of the binder resin was 26,000.

[0184] (1.4) Preparation of Micronized Pigment Dispersion (1.4.1) Preparation of Dispersion R-1 Dispersion R1 was prepared as a micronized pigment dispersion by the following method. That is, the following materials were mixed by stirring. Next, zirconia beads with a diameter of 0.5 mm were added to this mixture, and a dispersion treatment was carried out for 3 hours using an Eiger mill ("Mini Model M-250 MKII" manufactured by Eiger Japan Co., Ltd.). Thereafter, this was filtered through a filter with a pore size of 5.0 μm to obtain a micronized pigment dispersion with a non-volatile component content of 20% by mass.

[0185] Finely divided pigment R-1: 15.0 parts Resin type dispersant solution (non-volatile content 20%): 10.0 parts Binder resin solution (non-volatile content 20%): 15.0 parts Propylene glycol monomethyl ether acetate: 55.0 parts

[0186] (1.4.2) Preparation of Other Dispersions Dispersions G-1, G-2, Y-1, and B-1 were prepared in the same manner as described above for Dispersion R1, except that micronized pigments G-1, G-2, Y-1, and B-1, respectively, were used in place of micronized pigment R-1.

[0187] (1.5) Preparation of Acrylic Resin Solution An acrylic resin solution was prepared by the following method. 100 parts of propylene glycol monomethyl ether acetate was placed in a reaction vessel consisting of a separable four-neck flask equipped with a thermometer, a condenser, a nitrogen gas inlet tube, and a stirrer. The liquid in the reaction vessel was heated to 120°C while nitrogen gas was injected into the reaction vessel. Next, while maintaining the temperature at 120°C, a mixture consisting of 5.2 parts of styrene, 35.5 parts of glycidyl methacrylate, 41.0 parts of dicyclopentanyl methacrylate, and 1.0 part of azobisisobutyronitrile was added dropwise to the reaction vessel through a dropping tube over 2.5 hours to cause a polymerization reaction.

[0188] Next, the gas in the reaction vessel was replaced with air, and 17.0 parts of acrylic acid, 0.3 parts of tris(dimethylaminomethyl)phenol, and 0.3 parts of hydroquinone were added to the reaction vessel. The reaction was continued at 120°C for 5 hours, and was terminated when the solid acid value reached 0.8. This resulted in a resin solution with a weight average molecular weight of approximately 12,000 (measured by GPC).

[0189] Next, 30.4 parts of tetrahydrophthalic anhydride and 0.5 parts of triethylamine were added to this resin solution, and the mixture was allowed to react for 4 hours at 120° C. After that, propylene glycol monomethyl ether acetate was added to this liquid to obtain an acrylic resin solution with a nonvolatile content of 20% by mass.

[0190] (1.6) Preparation of Photosensitive Composition (1.6.1) Preparation of Photosensitive Composition PR-1 The materials for photosensitive composition PR-1 were mixed by stirring in the formulation shown in Table 1. Then, this mixture was filtered through a filter with a pore size of 1.0 μm to obtain photosensitive composition PR-1.

[0191] (1.6.2) Preparation of Other Photosensitive Compositions Photosensitive compositions PR-2, PR-3, PG-1, PG-2, PG-3, and PB-1 were prepared in the same manner as described above for photosensitive composition PR-1, except that the formulation of materials was changed as shown in Table 1.

[0192]

[0193] The material names listed in Table 1 represent the following materials: FDG007: tetraazaporphyrin copper complex dye (manufactured by Yamada Chemical Co., Ltd., "FDG007," maximum absorption wavelength 595 nm, half-width 22 nm) M309: trimethylolpropane triacrylate (manufactured by Toagosei Co., Ltd., "Aronix (registered trademark) M-309") M402: dipentaerythritol hexaacrylate (manufactured by Toagosei Co., Ltd., "Aronix (registered trademark) M-402") OXE02: ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) (manufactured by BASF, "IRGACURE (registered trademark) OXE02")

[0194] (2) Manufacturing of Display Panel (2.1) Manufacturing of Display Panel DPA-1 As the display panel DPA-1, the display panel DPA described with reference to Fig. 1 was manufactured. As the light control device 2A, a device in which the light emitting diode 23 emitted blue light with a wavelength of 450 nm was used. As the transparent substrate 31, a glass substrate was used.

[0195] The red filter portion 33R, green filter portion 33G, and blue filter portion 33B were formed using photosensitive compositions PR-1, PG-1, and PB-1, respectively. Specifically, the red filter portion 33R, green filter portion 33G, and blue filter portion 33B were each formed by the following method. That is, a photosensitive composition was applied to a transparent substrate 31 on which a black matrix 32 had been formed, using a spin coater, so that the thickness after curing would be 2.5 μm. Next, this coating film was exposed to ultraviolet light through a pattern mask, and the unexposed areas were removed by alkaline development. The coating film was then cured by heating at 230°C for 15 minutes in a heating oven. By this method, the red filter portion 33R, green filter portion 33G, and blue filter portion 33B were each formed. The partition wall layer 34 was formed to a thickness of 30 μm.

[0196] The first wavelength conversion portion 36R is made of 30 parts Eu 2+ A layer was formed by curing a mixture of an activated phosphor and 100 parts of a silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd.). 2+ The activated phosphor is SrCaAlSiN 3 : Eu (particle diameter 5.4 nm) was used.

[0197] The second wavelength conversion portion 36G is made of Eu 2+ As an activator phosphor, SrCaAlSiN 3 : (Ba, Sr)Ga instead of Eu (particle diameter 5.4 nm) 2 S 4 A layer similar to that of the first wavelength-converting portion 36R was formed, except that Eu (particle diameter: 4.6 μm) was used.

[0198] The filling portion 36B is Eu 2+ A layer similar to that of the first wavelength-converting portion 36R was formed, except that the activated phosphor was omitted and the entire amount was silicone resin.

[0199] (2.2) Fabrication of Display Panel DPA-2 Display panel DPA-2 was fabricated in the same manner as described above for display panel DPA-1, except for the following: instead of using photosensitive compositions PR-1 and PG-1, photosensitive compositions PR-2 and PG-2 were used, respectively.

[0200] (2.3) Fabrication of Display Panel DPA-3 Display panel DPA-2 was fabricated in the same manner as described above for display panel DPA-1, except for the following: instead of using photosensitive compositions PR-1 and PG-1, photosensitive compositions PR-3 and PG-3 were used, respectively.

[0201] (3) Manufacture of Surface Protecting Member (3.1) Manufacture of Surface Protecting Member SWA1 As the surface protecting member SWA1, the surface protecting member 5 described with reference to FIG. 1 was manufactured.

[0202] As the ultraviolet ray blocking layer 51, a TAC (triacetyl cellulose film) (manufactured by Fujifilm Corporation, TG60UL, thickness 60 μm, ultraviolet ray blocking rate 92.9%) was used.

[0203] The colored layer 52 was formed by the following method. First, a colored layer-forming composition CR1 having the formulation shown in Table 2 below was prepared. Next, the colored layer-forming composition CR1 was applied to one surface of the ultraviolet-shielding layer 51 so that the thickness after curing would be 5.0 μm. This coating film was dried in an oven at 80° C. for 60 seconds. The dried coating film was irradiated with 150 mJ / cm using an ultraviolet irradiator (manufactured by Fusion UV Systems Japan, light source H bulb). 2 The coating film was cured by irradiating it with ultraviolet light at an exposure dose of 1000 kJ / cm.sup.2. The colored layer 52 was thus obtained.

[0204]

[0205] The material names listed in Table 2 represent the following materials: FDG-007: tetraazaporphyrin copper complex dye (Yamada Chemical Co., Ltd., "FDG007," maximum absorption wavelength 595 nm, half-width 22 nm) Dye-1: dipyrromethene cobalt complex dye (maximum absorption wavelength 493 nm, half-width 26 nm) Dye-2: phthalocyanine copper complex dye (Yamada Chemical Co., Ltd., "FDN002," minimum transmittance wavelength 780 nm in the 400-780 nm range) UA-306H: pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer (Kyoeisha Chemical Co., Ltd., "UA-306H") DPHA: dipentaerythritol hexaacrylate PETA: pentaerythritol triacrylate T1477: 3,3,3',3'-tetramethyl-5,5',6,6'-tetrapropoxy-1,1'-spirobiindane ("T1477" manufactured by Tokyo Chemical Industry Co., Ltd.) D1781: bis(dibutyldithiocarbamate)nickel(II) ("D1781" manufactured by Tokyo Chemical Industry Co., Ltd.) Tinuvin 479: hydroxyphenyltriazine-based ultraviolet absorber ("Tinuvin 479" manufactured by BASF Japan Ltd.) LA-36: benzotriazole-based ultraviolet absorber ("ADEKA STAB LA-36" manufactured by ADEKA Corporation) Omnirad TPO: manufactured by IGM Resins B.V. (acylphosphine oxide-based photopolymerization initiator) MEK: methyl ethyl ketone

[0206] Resin RS1 was produced by the following method. 2.4 g of 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate (FA-711MM, manufactured by Showa Denko Materials Co., Ltd.), 5.6 g of methyl methacrylate (manufactured by Kanto Chemical Co., Ltd.), 31 g of cyclohexanone (manufactured by Kanto Chemical Co., Ltd.), and 0.11 g of 2,2'-azobis(isobutyronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed in a reaction vessel and heated at 70°C for 8 hours with stirring under a nitrogen gas atmosphere. The mixture was then further heated at 100°C for 1 hour with stirring to obtain a polymer solution. This polymer solution was poured into 400 mL of methanol (manufactured by Kanto Chemical Co., Ltd.), and the resulting precipitate was filtered off and dried. In this manner, a resin RS1 was obtained by copolymerizing 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate and methyl methacrylate in a molar ratio of 15:85.

[0207] Dye-1 was produced by the following method. Specifically, 2.5 g of ethyl 5-formyl-2,4-dimethyl-1H-pyrrole-3-carboxylate was placed in a reaction vessel and dissolved in 50 mL of methanol. 45 g of 47% hydrobromic acid was added to this solution, and the mixture was refluxed for 1 hour. The precipitated solid was filtered off to obtain 2.6 g of 3,3',5,5'-tetramethyl-4,4'-die-ethoxycarbonyl-2,2'-dipyrromethene hydrobromide. Next, 0.6 g of 3,3',5,5'-tetramethyl-4,4'-die-ethoxycarbonyl-2,2'-dipyrromethene hydrobromide was placed in a reaction vessel, and 5 mL of methanol, 0.17 g of triethylamine, and 0.18 g of cobalt acetate tetrahydrate were added thereto, and the mixture was refluxed for 2 hours. The precipitated solid was filtered off to obtain 0.42 g of Dye-1.

[0208] Next, a hard coat layer was formed as a first surface layer 53 on the surface of the ultraviolet-shielding layer 51 opposite to the surface on which the colored layer 52 was formed. This hard coat layer was formed in the same manner as described above for the colored layer 52, except that the colored layer-forming composition CR1 was replaced with the hard coat layer-forming composition HC1, the formulation of which is shown in Table 3 below.

[0209]

[0210] The material names listed in Table 3 represent the following materials: UA-306H: Pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer (manufactured by Kyoeisha Chemical Co., Ltd., "UA-306H") DPHA: Dipentaerythritol hexaacrylate PETA: Pentaerythritol triacrylate Omnirad TPO: Manufactured by IGM Resins B.V. (Acylphosphine oxide photopolymerization initiator) MEK: Methyl ethyl ketone

[0211] Next, a low refractive index layer was formed as the second surface layer 54 on the first surface layer 53 by the following method.

[0212] First, the following materials were mixed to prepare a composition LR for forming a low refractive index layer. Refractive index adjuster: porous silica fine particles (average particle size 75 nm, solid content 20%) methyl isobutyl ketone dispersion 8.5 parts Antifouling agent: Optool (registered trademark) AR-110 (manufactured by Daikin Industries, Ltd., solid content 15%, solvent: methyl isobutyl ketone) 5.6 parts Active energy ray curable resin: pentaerythritol triacrylate (PETA) 0.4 parts Photopolymerization initiator: Omnirad TPO (manufactured by IGM Resins B.V.) 0.07 parts Leveling agent: RS-77 (manufactured by DIC Corporation) 1.7 parts Solvent: methyl isobutyl ketone 83.73 parts

[0213] Next, the composition LR for forming a low refractive index layer was applied onto the first surface layer 53 so that the thickness after curing would be 100 nm. This coating film was dried for 60 seconds in an oven at 80°C. The dried coating film was irradiated with 200 mJ / cm using an ultraviolet irradiator (manufactured by Fusion UV Systems Japan, light source H bulb). 2 The coating was cured by irradiating with ultraviolet light at an exposure dose of 1000 kJ / cm 2 , thereby obtaining a low refractive index layer as the second surface layer 54. In this manner, the surface protection member SWA1 was produced.

[0214] (3.2) Production of surface protection members SWA2 to SWA7 Surface protection members SWA2 to SWA7 were produced by the same method as described above for surface protection member SWA1, except that colored layer-forming compositions CR2 to CR7 having the compositions shown in Table 2 above were used instead of colored layer-forming composition CR1.

[0215] (3.3) Production of Surface Protective Members SWA8 and SWA9 Surface protective members SWA8 and SWA9 were produced by the same method as described above for surface protective member SWA1, except for the following points. That is, instead of using TAC as the ultraviolet-shielding layer 51, a PMMA:polymethyl methacrylate film (W002N80 manufactured by Sumitomo Chemical Co., Ltd., thickness 80 μm, ultraviolet shielding rate 13.9%) was used. In the production of surface protective member SWA8, colored layer-forming composition CR1 having the composition shown in Table 2 above was used instead of colored layer-forming composition CR1. In the production of surface protective member SWA9, colored layer-forming composition CR8 having the composition shown in Table 2 above was used instead of colored layer-forming composition CR1.

[0216] (4) Manufacturing of Display Device (4.1) Examples 1 to 7 The display device 1A described with reference to Fig. 1 was manufactured. In Example 1, as shown in Table 4 below, the display panel DPA-1 described above was used as the display panel DPA, and the surface protective member SWA1 described above was used as the surface protective member 5. The display panel DPA and the surface protective member 5 were bonded together via an adhesive layer.

[0217] (4.2) Examples 2 to 7 As shown in Table 4, the display devices 1A of Examples 2 to 7 were manufactured in the same manner as described above for the display device 1A of Example 1, except that the display panel DPA-2 was used instead of the display panel DPA-1, and the surface protection members SWA2 to SWA7 were used instead of the surface protection member SWA1, respectively.

[0218]

[0219] (4.3) Comparative Example 1 As shown in Table 5 below, the above-described display panel DPA-1 was used as the display panel DPA, and the surface protection member 5 and the adhesive layer for bonding it to the display panel DPA were omitted. In other words, the display panel DPA-1 was used as a display device.

[0220] (4.4) Comparative Examples 2 and 3 As shown in Table 5, display devices according to Comparative Examples 2 and 3 were manufactured by the same method as described above for the display device 1A according to Example 1, except that surface protection members SWA8 and SWA9 were used instead of surface protection member SWA1, respectively.

[0221] (4.5) Comparative Example 4 As shown in Table 5 below, the above-described display panel DPA-3 was used as the display panel DPA, and the surface protection member 5 and the adhesive layer for bonding it to the display panel DPA were omitted. In other words, the display panel DPA-3 was used as the display device.

[0222]

[0223] (5) Evaluation The display devices according to Examples 1 to 7 and Comparative Examples 1 to 4 were evaluated as follows.

[0224] (5.1) BT.2020 Coverage Ratio For each display device, the coverage ratio of the BT.2020 color gamut in the CIE 1976 u'v' color system (BT.2020 coverage ratio) was determined as an index of color reproducibility.

[0225] (5.2) Luminance Efficiency Y' / Y For each display device, the value of the left side of the above inequality (1) was calculated as the luminance efficiency Y' / Y.

[0226] (5.3) Reliability For each display device, the initial spectrum when displaying white and the light having a wavelength of 300 nm to 400 nm were measured at 60 W / m using a Xe lamp under the conditions of a temperature of 45°C and a humidity of 50% RH. 2 The color difference ΔE before and after irradiation was calculated from the spectrum during white display after irradiation for 120 hours at an illuminance of * ab The color difference ΔE was calculated. * ab If the color difference ΔE was 3 or more, the evaluation was "B".* ab If the color difference ΔE was within the range of 1 or more and less than 3, it was evaluated as "A". * ab When the value was less than 1, the evaluation was "AA".

[0227] (5.4) Results The evaluation results are shown in Tables 6 and 7 below.

[0228]

[0229]

[0230] As shown in Table 7, in Comparative Examples 1 and 4, in which the surface protective member was omitted, the BT.2020 coverage or reliability was insufficient. Furthermore, in Comparative Example 2, in which a substrate without ultraviolet shielding ability was used instead of the ultraviolet shielding layer in the surface protective member, the reliability was insufficient. Furthermore, in Comparative Example 3, in which a substrate without ultraviolet shielding ability was used instead of the ultraviolet shielding layer in the surface protective member and an ultraviolet absorber was added to the colored layer, the reliability was also insufficient. In contrast, Examples 1 to 7, in which a surface protective member with an ultraviolet shielding layer was used, showed high performance in all of the BT.2020 coverage, luminance efficiency Y' / Y, and reliability.

[0231] 1A...display device, 1B...display device, 2A...dimming device, 2B...dimming device, 3...black matrix substrate, 4...adhesive layer, 5...surface protective member, 6...adhesive layer, 21...substrate, 22...multilayer wiring layer, 23...light-emitting diode, 31...transparent substrate, 32...black matrix, 33...color filter, 33B...blue filter portion, 33G...green filter portion, 33R...red filter portion, 34...partition layer, 36B...filling portion, 36G...second wavelength conversion portion, 36R...first wavelength conversion portion, 37...planarizing layer, 38...protective layer, 51...ultraviolet shielding layer, 52...colored layer, 53...first surface layer, 54...second surface layer, DPA...display panel, DPB...display panel.

Claims

1. A substrate; a plurality of light emitting diodes arranged on the substrate and having the same emission spectrum; and a plurality of filter sections including a red filter section, a green filter section, and a blue filter section, the plurality of filter sections including color filters facing the plurality of light emitting diodes, a first wavelength conversion section positioned between the red filter section and the light emitting diode facing it, and a second wavelength conversion section positioned between the green filter section and the light emitting diode facing it, each of the first wavelength conversion section and the second wavelength conversion section being made of Eu. 2+ a wavelength conversion layer containing an activated phosphor; a functional layer including an ultraviolet shielding layer having an ultraviolet shielding rate of 85% or more in accordance with JIS L1925:2019, the functional layer sandwiching the color filter and the wavelength conversion layer between the light emitting diodes; and a coloring layer interposed between the functional layer and the color filter, the coloring layer including a first color material having a maximum absorption wavelength in the range of 560 to 620 nm and a half width of an absorption spectrum in the range of 15 to 55 nm.

2. The plurality of light emitting diodes are near-ultraviolet light emitting diodes, and the wavelength conversion layer further includes a third wavelength conversion portion located between the blue filter portion and the light emitting diode facing the blue filter portion, and the third wavelength conversion portion is made of Eu. 2+ 2. The display device according to claim 1, further comprising an activated phosphor.

3. The display device according to claim 1, wherein said plurality of light emitting diodes are blue light emitting diodes.

4. CIE 1976 L * u * v * The coverage of the BT.2020 color gamut in the color system and the coverage of the BT.2020 color gamut in the CIE1976 u'v' color system are each 90% or more; 4. The display device according to claim 1, wherein RY is a stimulus value Y in the CIE 1931 color system of light incident on a surface of the red filter portion facing the light emitting diode, RY' is a stimulus value Y in the CIE 1931 color system of light emitted from a surface opposite to the surface of the red filter portion facing the light emitting diode, GY is a stimulus value Y in the CIE 1931 color system of light incident on the surface of the green filter portion facing the light emitting diode, GY' is a stimulus value Y in the CIE 1931 color system of light emitted from a surface opposite to the surface of the green filter portion facing the light emitting diode, BY is a stimulus value Y in the CIE 1931 color system of light incident on the surface of the blue filter portion facing the light emitting diode, and BY' is a stimulus value Y in the CIE 1931 color system of light emitted from a surface opposite to the surface of the blue filter portion facing the light emitting diode, satisfying a relationship shown in the following inequality (1).

5. The Eu contained in the wavelength conversion layer 2+ 5. The display device according to claim 1, wherein the activated phosphor has a particle size in the range of 0.1 to 15 [mu]m.

6. A display device as claimed in any one of claims 1 to 5, wherein the coloured layer further comprises at least one of a second colour material having a maximum absorption wavelength in the range of 470 to 530 nm and a half width of an absorption spectrum in the range of 15 to 45 nm, and a third colour material having a wavelength with the lowest transmittance in the wavelength range of 400 to 780 nm in the range of 650 to 780 nm.

7. The display device according to any one of claims 1 to 6, wherein the colored layer further contains one or more selected from the group consisting of a radical scavenger, a singlet oxygen quencher, and a peroxide decomposer.

8. The display device according to any one of claims 1 to 7, wherein the colored layer contains a polymer having a repeating unit represented by the following formula (i): Here, R 12 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 13 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.

9. The display device according to any one of claims 1 to 8, wherein the colored layer contains one or more compounds selected from the group consisting of dialkyldithiophosphates, dialkyldithiocarbanates, benzenedithiols, transition metal complexes thereof, and compounds represented by the following formula (ii): Here, R 1 each independently represents an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, or R 9 CO - , R 10 SO 2 - Or R 11 N.H.C.O. - R represents a group represented by 9 , R 10 , and R 11 R each independently represents an alkyl group, an alkenyl group, an aryl group, or a heterocyclic group. 2 and R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, or an alkenyloxy group; R 4 ~R 8 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an aryl group.

10. A display device according to any one of claims 1 to 9, wherein the colored layer contains one or more compounds selected from the group consisting of compounds having any one of a porphyrin structure, a merocyanine structure, a phthalocyanine structure, an azo structure, a cyanine structure, a squarylium structure, a coumarin structure, a polyene structure, a quinone structure, a tetradiporphyrin structure, a pyrromethene structure and an indigo structure, and metal complexes thereof.

11. The display device according to any one of claims 1 to 10, wherein the functional layer functions as an anti-reflection layer or an anti-glare layer.

12. The display device according to any one of claims 1 to 11, wherein the functional layer further includes an antistatic layer or an antifouling layer facing the colored layer with the ultraviolet ray blocking layer sandwiched therebetween.

Citation Information

Patent Citations

  • Photosensitive resin composition and production of color filter using the same

    JP1993005987A

  • Display device and manufacturing method thereof

    JP2018523848A

  • Display

    JP2023054570A

  • Optical film and display device

    JP7207598B1

  • Laminate, display device, and organic electroluminescence display device

    WO2021162115A1