One-pack type heat-curable resin composition and use thereof
The one-component thermosetting resin composition, featuring an epoxy resin, core-shell polymer particles, and specific additives, addresses the low-temperature curing challenge by achieving superior T-peel adhesive strength while reducing energy and emissions, aligning with sustainable development goals.
Patent Information
- Application Number
- PCT/JP2024/019321
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-27
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional thermosetting resin compositions fail to achieve sufficient T-peel adhesive strength when cured at low temperatures, necessitating the development of a novel one-component thermosetting resin composition that maintains excellent adhesive properties even under low-temperature curing conditions.
A one-component thermosetting resin composition comprising an epoxy resin, polymer particles with a core-shell structure, blocked urethane, rubber modification, dicyandiamide, and monocarboxylic acid or its metal salt, which provides enhanced T-peel adhesive strength by optimizing the ratio and content of these components.
The composition achieves high T-peel adhesive strength at both low and normal temperatures, reducing energy consumption and greenhouse gas emissions, aligning with sustainable development goals by minimizing energy requirements and carbon footprint.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
One-component thermosetting resin composition and its use
[0001] The present invention relates to a one-component thermosetting resin composition and its use.
[0002] Thermosetting resin compositions containing epoxy resins are used in a wide range of fields, as described in Patent Documents 1 to 3. For example, Patent Documents 1 and 3 disclose them as structural adhesives.
[0003] Incidentally, in the field of structural adhesives, low temperature curing is currently required from the viewpoint of carbon neutrality.
[0004] International Publication WO2022 / 114073 A1 International Publication WO2022 / 045329 A1 International Publication WO2022 / 039121 A2
[0005] Conventional thermosetting resin compositions are insufficient in terms of T-peel adhesive strength of the cured product obtained when cured at low temperatures, and there is room for further improvement.
[0006] One embodiment of the present invention has been made in consideration of the current situation as described above, and its object is to provide a novel one-component thermosetting resin composition that can provide a cured product having excellent T-peel adhesive strength even when cured at a low temperature.
[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.
[0008] That is, a one-component thermosetting resin composition according to one embodiment of the present invention contains (A) an epoxy resin, (B) one or more resins selected from the group consisting of polymer particles having a core-shell structure comprising a core layer and a shell layer, blocked urethane, a rubber-modified epoxy resin, and a urethane-modified epoxy resin, (C) dicyandiamide, and (D) a monocarboxylic acid and / or a monocarboxylic acid metal salt, wherein, relative to 100 parts by mass of the component (A), (a) the content of the component (B) is 1 part by mass to 100 parts by mass, (b) the content of the component (C) is 3.5 parts by mass to 19.0 parts by mass, and (c) the content of the component (D) is 0.01 parts by mass to 30.00 parts by mass.
[0009] According to one embodiment of the present invention, it is possible to provide a novel one-component thermosetting resin composition that can provide a cured product that has excellent T-peel adhesive strength even when cured at low temperatures.
[0010] One embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to the respective configurations described below, and various modifications are possible within the scope of the claims. Embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments and examples are also included in the technical scope of the present invention. Furthermore, all academic literature and patent documents described in this specification are incorporated herein by reference. Furthermore, unless otherwise specified in this specification, "A to B" representing a numerical range means "greater than or equal to A and less than or equal to B."
[0011] In this specification, the term "X unit" contained in a polymer, copolymer, or resin refers to a "structural unit derived from an X monomer." For example, the term "butadiene unit" refers to a "structural unit derived from a butadiene monomer."
[0012] [1. Curable Resin Composition] A one-component thermosetting resin composition according to one embodiment of the present invention contains (A) an epoxy resin, (B) one or more resins selected from the group consisting of polymer particles having a core-shell structure including a core layer and a shell layer, blocked urethane, rubber-modified epoxy resin, and urethane-modified epoxy resin, (C) dicyandiamide, and (D) a monocarboxylic acid and / or a monocarboxylic acid metal salt, wherein, relative to 100 parts by mass of the component (A), (a) the content of the component (B) is 1 part by mass to 100 parts by mass, (b) the content of the component (C) is 3.5 parts by mass to 19.0 parts by mass, and (c) the content of the component (D) is 0.01 parts by mass to 30.00 parts by mass.
[0013] In this specification, "(A) epoxy resin," "(B) one or more selected from the group consisting of polymer particles having a core-shell structure containing a core layer and a shell layer, blocked urethane, rubber-modified epoxy resin, and urethane-modified epoxy resin," "(C) dicyandiamide," "(D) monocarboxylic acid and / or monocarboxylic acid metal salt," "(E) epoxy-based reactive diluent," "(F) amine adduct curing agent that is solid at room temperature," and "(G) urea compound" may be referred to as "(A) component," "(B) component," "(C) component," "(D) component," "(E) component," "(F) component," and "(G) component," respectively. Furthermore, in this specification, a "one-component thermosetting resin composition" may be referred to as "composition," and a "one-component thermosetting resin composition according to one embodiment of the present invention" may be referred to as "the composition."
[0014] Because of the above-described configuration, the present composition has the advantage of being able to provide a cured product having excellent T-peel adhesive strength even when cured at low temperatures. Furthermore, because of the above-described configuration, the present composition has the advantage of being able to provide a cured product having excellent T-peel adhesive strength even when cured at normal temperatures (e.g., 170°C). That is, because of the above-described configuration, the present composition can provide a cured product having excellent T-peel adhesive strength whether cured at normal temperatures or low temperatures, and can provide a cured product having excellent T-peel adhesive strength especially when cured at low temperatures.
[0015] In this specification, the phrase "can provide a cured product having excellent T-peel adhesive strength even when cured at low temperatures" means that the composition is cured at low temperatures (e.g., 120°C to 140°C) for a curing time of, for example, 20 minutes, resulting in a cured product having a high T-peel adhesive strength (e.g., 100 N / 25 mm or more). The method for measuring the T-peel adhesive strength of the cured product will be described in detail in the Examples below.
[0016] The higher the T-peel adhesive strength of the cured product, the better the T-peel adhesive strength of the cured product. In one embodiment of the present invention, the T-peel adhesive strength of the cured product obtained by low-temperature curing of the composition (e.g., curing at a curing temperature of 120°C to 140°C for a curing time of 20 minutes) is preferably 100 N / 25 mm or more, more preferably 101 N / 25 mm or more, even more preferably 102 N / 25 mm or more, even more preferably 103 N / 25 mm or more, and particularly preferably 104 N / 25 mm or more. The upper limit of the T-peel adhesive strength of the cured product obtained by low-temperature curing of the composition is not particularly limited, but is, for example, 400 N / 25 mm or less.
[0017] The present composition can provide a cured product with excellent T-peel adhesive strength even when cured at low temperatures. Therefore, one embodiment of the present invention can reduce the amount of energy required to cure the composition, thereby lowering production costs. This effect contributes to the achievement of, for example, Goal 7 of the United Nations' Sustainable Development Goals (SDGs), "Ensure access to affordable, reliable, sustainable, and modern energy for all." The present composition also has the advantage of reducing carbon dioxide emissions associated with the curing of the composition, thereby reducing greenhouse gas emissions. This effect also contributes to the achievement of, for example, Goal 13 of the United Nations, "Take urgent action to combat climate change and its impacts."
[0018] <(A) Epoxy Resin> The present composition contains an epoxy resin as component (A). In this specification, "epoxy resin" refers to "a resin having at least one epoxy group per molecule." The epoxy resin as component (A) is preferably a resin having two or more epoxy groups per molecule. In this specification, "rubber-modified epoxy resins" and "urethane-modified epoxy resins" are not included in component (A), but are included in component (B). In other words, component (A) can be said to be "an epoxy resin other than components (A) and (B)." Various epoxy resins can be used as the epoxy resin.
[0019] A resin having X epoxy groups per molecule is sometimes referred to as an "X-functional epoxy resin." For example, a resin having one epoxy group per molecule is called a "monofunctional epoxy resin," and a resin having two epoxy groups per molecule is called a "difunctional epoxy resin." Furthermore, a resin having two or more epoxy groups per molecule is sometimes called a "multifunctional epoxy resin."
[0020] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD type epoxy resins, bisphenol S type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, novolac type epoxy resins, glycidyl ether type epoxy resins of bisphenol A propylene oxide adducts, hydrogenated bisphenol A (or F) type epoxy resins, fluorinated epoxy resins, flame-retardant epoxy resins such as glycidyl ether of tetrabromobisphenol A, and p-oxybenzoic acid glycidyl ether ester type epoxy resins. resins, m-aminophenol type epoxy resins, diaminodiphenylmethane type epoxy resins, various alicyclic epoxy resins, N,N-diglycidylaniline, N,N-diglycidyl-o-toluidine, triglycidyl isocyanurate, divinylbenzene dioxide, resorcinol diglycidyl ether, chelate-modified epoxy resins, hydantoin type epoxy resins, epoxidized products of unsaturated polymers such as petroleum resins, aminoglycidyl ether resins, and epoxy compounds obtained by addition reaction of the above epoxy resins with bisphenol A (or F) or polybasic acids, etc.
[0021] Examples of epoxy compounds obtained by subjecting an epoxy resin to an addition reaction with a polybasic acid or the like include an addition reaction product of a dimer of tall oil fatty acid (dimer acid) with a bisphenol A-type epoxy resin, as described in WO 2010-098950.
[0022] The epoxy resin is not limited to these, and any commonly used epoxy resin may be used. These epoxy resins may be used alone or in combination of two or more.
[0023] Here, in this specification, polyalkylene glycol diglycidyl ethers, glycol diglycidyl ethers, diglycidyl esters of aliphatic polybasic acids, glycidyl ethers of dihydric or higher polyhydric aliphatic alcohols, and monoepoxides are not included in the term "epoxy resins." These polyalkylene glycol diglycidyl ethers, glycol diglycidyl ethers, diglycidyl esters of aliphatic polybasic acids, glycidyl ethers of dihydric or higher polyhydric aliphatic alcohols, and monoepoxides have relatively low viscosities (e.g., 500 mPa·s or less at 25°C) compared to the above-mentioned epoxy resins. In this specification, epoxy resins with a viscosity of 500 mPa·s or less at 25°C are not included in component (A). In other words, component (A) in this specification can also be said to be "epoxy resins with a viscosity of more than 500 mPa·s at 25°C."
[0024] As the chelate-modified epoxy resin, for example, the resins described in paragraphs
[0018] to
[0019] of WO2016-163491 can be used.
[0025] Among these epoxy resins, polyfunctional epoxy resins having at least two epoxy groups per molecule have high curability, produce cured products with excellent flexibility, and are excellent in improving the T-peel adhesive strength of the cured products when polymer particles, as described below, are incorporated. Furthermore, among polyfunctional epoxy resins, bifunctional epoxy resins produce cured products with high strength and an excellent balance between elastic modulus and elongation. Therefore, component (A) preferably contains a polyfunctional epoxy resin, more preferably consists solely of a polyfunctional epoxy resin, more preferably contains a bifunctional epoxy resin, and even more preferably is (consists solely of) a bifunctional epoxy resin.
[0026] The epoxy equivalent of the epoxy resin is preferably less than 220 g / eq, more preferably from 90 g / eq to less than 210 g / eq, and even more preferably from 135 g / eq to less than 200 g / eq. This configuration has the advantage of being able to obtain a cured product with high elastic modulus and heat resistance.
[0027] In this specification, the term "epoxy equivalent" refers to the molecular weight per epoxy group contained in a compound having an epoxy group, and specifically, is a value calculated based on the following formula: Epoxy equivalent (g / eq) = mass average molecular weight (Mw) of compound / number of epoxy groups per molecule of compound (average number). The epoxy equivalent can also be measured in accordance with JIS K7236.
[0028] Among the above-mentioned epoxy resins, bisphenol A epoxy resins and bisphenol F epoxy resins provide cured products with high elastic modulus, excellent heat resistance and adhesion, and are relatively inexpensive. Therefore, component (A) preferably contains bisphenol A epoxy resin and / or bisphenol F epoxy resin, and more preferably is (consists only of) bisphenol A epoxy resin and / or bisphenol F epoxy resin. Furthermore, since a curable resin composition capable of providing a cured product with excellent heat resistance can be obtained at a low cost, component (A) more preferably contains bisphenol A epoxy resin, and particularly preferably is (consists only of) bisphenol A epoxy resin.
[0029] From the viewpoints of the balance between elastic modulus and elongation, and strength, component (A) more preferably contains a difunctional bisphenol A type epoxy resin and / or a difunctional bisphenol F type epoxy resin, and even more preferably is (consists solely of) a difunctional bisphenol A type epoxy resin and / or a difunctional bisphenol F type epoxy resin.
[0030] From the viewpoints of the balance between elastic modulus and elongation, and strength, the present composition preferably contains a smaller amount of tri- or higher functional epoxy resin as component (A). In the present composition, the total amount of tri- or higher functional epoxy resins per 100% by mass of component (A) is preferably 40% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 0% to 5% by mass. In the present composition, the total amount of tri- or higher functional epoxy resins per 100% by mass of component (A) may be 0% by mass. In other words, the present composition does not need to contain a tri- or higher functional epoxy resin as component (A).
[0031] Examples of commercially available bisphenol A type epoxy resins include those commercially available under the trade name jER from Mitsubishi Chemical Corporation (e.g., jER828, jER825, jER827, jER828EL, jER828US, jER828XA, jER834, jER1001, jER1002, jER1004, jER1007, jER1009, jER1010), and those commercially available under the trade name jER from Momentive Specialty Chemicals, Inc. those commercially available under the trade name EPON from Olin Epoxy Co. (e.g., EPON 1510, EPON 1310, EPON 828, EPON 872, EPON 1001, EPON 1004, EPON 2004); Examples of suitable resins include, but are not limited to, resins commercially available under the trade name DER from Epson Corporation (e.g., DER 331, DER 332, DER 336, and DER 439), resins commercially available under the trade name ADEKA RESIN from ADEKA Corporation (e.g., EP-4100, EP-4300, EP-4400, EP-4530, and EP-4504), and resins commercially available under the trade name EPICLON from DIC Corporation (e.g., EPICLON 840 and EPICLON 850).
[0032] Examples of commercially available bisphenol F epoxy resins include, but are not limited to, those commercially available under the trade name jER from Mitsubishi Chemical Corporation (e.g., jER806, jER806H, jER807, jER4005P, jER4007P, jER4010P), those commercially available under the trade name DER from Olin Epoxy Co. (e.g., DER 334), those commercially available under the trade name ADEKA RESIN from ADEKA Corporation (e.g., EP-4901, EP-4901E), and those commercially available under the trade name EPICLON from DIC Corporation (e.g., EPICLON 830).
[0033] The total content of the bisphenol A epoxy resin and the bisphenol F epoxy resin in 100% by mass of the component (A) is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 90% by mass to 100% by mass. This configuration has the advantage that the resulting cured product has excellent T-peel adhesive strength, impact resistance, heat resistance, and adhesiveness. The total content of the bisphenol A epoxy resin and the bisphenol F epoxy resin in 100% by mass of the component (A) may be 100% by mass. In other words, the component (A) may be (or may consist solely of) a bisphenol A epoxy resin and / or a bisphenol F epoxy resin.
[0034] Both bisphenol A epoxy resins having an epoxy equivalent of less than 220 g / eq and bisphenol F epoxy resins having an epoxy equivalent of less than 220 g / eq are liquid at room temperature and have excellent handleability. Therefore, it is particularly preferable that component (A) contains a bisphenol A epoxy resin having an epoxy equivalent of less than 220 g / eq and / or a bisphenol F epoxy resin having an epoxy equivalent of less than 220 g / eq. This configuration has the advantage of further improving the storage stability of the resulting composition.
[0035] The total content of the bisphenol A epoxy resin having an epoxy equivalent of less than 220 g / eq and the bisphenol F epoxy resin having an epoxy equivalent of less than 220 g / eq per 100% by mass of component (A) is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 90% by mass to 100% by mass. This configuration has the advantages of providing a cured product with excellent T-peel adhesion strength, impact resistance, heat resistance, and adhesiveness, and of providing a composition with excellent storage stability. The total content of the bisphenol A epoxy resin having an epoxy equivalent of less than 220 g / eq per 100% by mass of component (A) may be 100% by mass. In other words, component (A) may be (or may consist solely of) a bisphenol A type epoxy resin having an epoxy equivalent of less than 220 g / eq and / or a bisphenol F type epoxy resin having an epoxy equivalent of less than 220 g / eq.
[0036] From the viewpoint of T-peel adhesive strength, the content of component (A) in 100% by mass of the total amount of components (A) to (G) is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 60% by mass or more, and even more preferably 60% by mass to 80% by mass.
[0037] <Component (B)> The present composition includes, as component (B), one or more selected from the group consisting of polymer particles having a core-shell structure containing a core layer and a shell layer, blocked urethane, rubber-modified epoxy resin, and urethane-modified epoxy resin. The present composition only needs to include, as component (B), at least polymer particles having a core-shell structure containing a core layer and a shell layer, blocked urethane, rubber-modified epoxy resin, or urethane-modified epoxy resin. The present composition does not necessarily need to include, as component (B), all of polymer particles having a core-shell structure containing a core layer and a shell layer, blocked urethane, rubber-modified epoxy resin, and urethane-modified epoxy resin.
[0038] (Polymer particles) In this specification, "polymer particles having a core-shell structure comprising a core layer and a shell layer" refers to particles in which a core layer made of a core polymer and a shell layer made of a shell polymer form a layer structure. In this specification, "polymer particles having a core-shell structure comprising a core layer and a shell layer" may also be referred to as "core-shell polymer particles" or simply "polymer particles."
[0039] When the present composition contains polymer particles as component (B), the polymer particles can exhibit a toughness-improving effect in the composition. As a result, by including polymer particles as component (B), the present composition has the advantage of being able to provide a cured product (e.g., an adhesive layer) with excellent T-peel adhesive strength even when cured at low temperatures. Furthermore, when the present composition contains polymer particles as component (B), the adhesive strength (e.g., T-peel adhesive strength) of the resulting cured product tends to be excellent.
[0040] The polymer particles can be obtained by graft polymerizing a graft-copolymerizable monomer (a monomer for forming a shell layer) in the presence of a core layer to form a shell layer. More specifically, this polymerization operation can be carried out by adding a monomer for forming a shell layer (shell polymer) to a latex of a core polymer prepared in an aqueous polymer latex state and polymerizing it. In the polymer particles, it is preferable that the core polymer and the shell polymer are substantially chemically bonded. Note that in the polymer particles, the core layer and the shell layer do not need to form a complete layer structure. The shell layer (shell polymer) only needs to cover at least a portion of the core layer (core polymer), and does not need to cover the entire core layer. Furthermore, a portion of the shell layer may penetrate into the core layer.
[0041] Each layer of the polymer particles will be specifically described below.
[0042] <<Core Layer>> The core layer is preferably an elastic core layer having rubber properties in order to enhance the toughness of the cured product of the composition.
[0043] The core layer preferably contains a diene rubber because it effectively improves the toughness of the resulting cured product, effectively improves the T-peel adhesion strength of the resulting cured product, and is less likely to experience an increase in viscosity over time due to swelling of the core layer due to its low affinity with component (A). The core layer preferably contains a (meth)acrylate rubber because a wide range of polymer compositions can be designed by combining a variety of monomers. Furthermore, when attempting to improve low-temperature impact resistance without reducing the heat resistance of the cured product, the core layer preferably contains an organosiloxane rubber. In other words, the core layer preferably contains one or more rubbers selected from the group consisting of diene rubbers, (meth)acrylate rubbers, and organosiloxane rubbers.
[0044] (Diene Rubber) The diene rubber is preferably a polymer containing 50% by mass to 100% by mass of conjugated diene units and 0% by mass to 50% by mass of structural units derived from vinyl monomers other than conjugated diene monomers copolymerizable with the conjugated diene monomers.
[0045] Examples of the conjugated diene monomer from which the conjugated diene units are derived include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), and 2-chloro-1,3-butadiene.
[0046] These conjugated diene monomers may be used alone or in combination of two or more.
[0047] The content of conjugated diene units in the core layer (e.g., diene rubber) is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass, based on 100% by mass of all structural units constituting the core layer. When the content of conjugated diene units in the core layer (e.g., diene rubber) is 50% by mass or more, the T-peel adhesion strength of the resulting cured product can be improved.
[0048] Examples of vinyl monomers other than conjugated diene monomers copolymerizable with conjugated diene monomers include vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; vinyl carboxylic acids such as acrylic acid and methacrylic acid; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; vinyl acetate; alkenes such as ethylene, propylene, butylene, and isobutylene; and polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.
[0049] These vinyl monomers may be used alone or in combination of two or more. As the vinyl monomer other than the conjugated diene monomer copolymerizable with the conjugated diene monomer, styrene is particularly preferred.
[0050] Among diene rubbers, the core layer preferably contains butadiene rubber, which is a homopolymer of 1,3-butadiene, and / or butadiene-styrene rubber, which is a copolymer of 1,3-butadiene and styrene, from the viewpoints of a greater effect of improving the toughness of the resulting cured product, a greater effect of improving the T-peel adhesion strength of the resulting cured product, and a lower affinity with the (A) epoxy resin, making it less likely that the viscosity will increase over time due to swelling of the core layer. It is more preferable that the core layer is (consisting only of) butadiene rubber and / or butadiene-styrene rubber, even more preferable that it contains butadiene rubber, and particularly preferable that it is (consisting only of) butadiene rubber. Butadiene-styrene rubber is also preferred because it can enhance the transparency of the resulting cured product by adjusting the refractive index.
[0051] ((Meth)acrylate Rubber) The (meth)acrylate rubber is preferably a polymer obtained by polymerizing a monomer mixture containing 50% by mass to 100% by mass of (meth)acrylate units and 0% by mass to 50% by mass of structural units derived from vinyl monomers other than (meth)acrylate monomers that are copolymerizable with the (meth)acrylate monomers. In this specification, "(meth)acrylate" means acrylate and / or methacrylate.
[0052] Examples of the (meth)acrylate monomer from which the (meth)acrylate unit is derived include: (i) alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; (ii) aromatic ring-containing (meth)acrylates such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; and (iii) hydroxyalkanol (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate. (iv) glycidyl (meth)acrylates such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; (v) alkoxyalkyl (meth)acrylates; (vi) allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; (vii) polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and the like.
[0053] Examples of hydroxyalkyl (meth)acrylates include hydroxy linear alkyl (meth)acrylates (particularly, hydroxy linear C1-6 alkyl (meth)acrylates) such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates; hydroxy branched alkyl (meth)acrylates such as methyl α-(hydroxymethyl)acrylate and ethyl α-(hydroxymethyl)acrylate; and hydroxyl group-containing (meth)acrylates such as mono(meth)acrylates of polyester diols (particularly saturated polyester diols) obtained from divalent carboxylic acids (such as phthalic acid) and dihydric alcohols (such as propylene glycol).
[0054] These (meth)acrylate monomers may be used alone or in combination of two or more. The (meth)acrylate unit is preferably at least one selected from the group consisting of an ethyl (meth)acrylate unit, a butyl (meth)acrylate unit, and a 2-ethylhexyl (meth)acrylate unit.
[0055] Examples of vinyl monomers copolymerizable with (meth)acrylate monomers other than (meth)acrylate monomers include (i) vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; (ii) vinyl carboxylic acids such as acrylic acid and methacrylic acid; (iii) vinyl cyanides such as acrylonitrile and methacrylonitrile; (iv) vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; (v) vinyl acetate; (vi) alkenes such as ethylene, propylene, butylene, and isobutylene; and (vii) polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.
[0056] The vinyl monomer other than the (meth)acrylate monomer copolymerizable with the (meth)acrylate monomer may be used alone or in combination of two or more. Styrene is particularly preferred as the vinyl monomer other than the (meth)acrylate monomer copolymerizable with the (meth)acrylate monomer, since it can easily increase the refractive index.
[0057] (Organosiloxane-Based Rubber) Examples of the organosiloxane-based rubber include (i) polysiloxane-based polymers composed of alkyl or aryl di-substituted silyloxy units, such as dimethylsilyloxy, diethylsilyloxy, methylphenylsilyloxy, diphenylsilyloxy, and dimethylsilyloxy-diphenylsilyloxy; and (ii) polysiloxane-based polymers composed of alkyl or aryl mono-substituted silyloxy units, such as organohydrogensilyloxy in which some of the alkyl groups in the side chains are substituted with hydrogen atoms.
[0058] These polysiloxane polymers may be used alone or in combination of two or more. Among these, dimethylsilyloxy, methylphenylsilyloxy, and dimethylsilyloxy-diphenylsilyloxy are preferred because they can impart heat resistance to the cured product, and dimethylsilyloxy is most preferred because it is easily available.
[0059] The glass transition temperature (hereinafter, sometimes simply referred to as "Tg") of the core layer is preferably 0°C or lower, more preferably -20°C or lower, even more preferably -40°C or lower, and particularly preferably -60°C or lower, in order to enhance the toughness of the resulting cured product.
[0060] The volume average particle diameter of the core layer is not particularly limited, but is preferably 0.03 μm to 2.00 μm, more preferably 0.05 μm to 1.00 μm, more preferably 0.12 μm to 0.50 μm, more preferably 0.12 μm to 0.28 μm, and even more preferably 0.14 to 0.25 μm. When the volume average particle diameter of the core layer is within this range, the core layer can be produced stably, and the cured product can have good heat resistance and T-peel adhesive strength. The method for measuring the volume average particle diameter of the core layer will be described in detail in the Examples below.
[0061] The core layer may have a single layer structure or a multilayer structure consisting of multiple layers each having rubber elasticity. When the core layer has a multilayer structure, the polymer compositions of the layers may be different from each other within the ranges disclosed above.
[0062] The composition of the structural units of the core layer depends on the composition of the monomer for forming the core layer. When the polymerization conversion rate is 100%, the obtained core layer contains structural units derived from all of the monomers contained in the monomer for forming the core layer.
[0063] In one embodiment of the present invention, an intermediate layer, for example, as described in paragraphs
[0046] to
[0049] of WO2016-163491, can be provided between the core layer and the shell layer.
[0064] <Shell Layer> The shell layer is a polymer obtained by polymerizing a monomer for forming the shell layer. The polymer constituting the shell layer (shell polymer) plays a role of improving the compatibility between the polymer particles and component (A) and enabling the polymer particles to be dispersed in the form of primary particles in the composition and / or a cured product of the composition.
[0065] The type and content ratio of the structural unit contained in the shell layer are not particularly limited. In terms of compatibility and dispersibility of the polymer particles in the composition, the shell layer preferably contains one or more structural units selected from the group consisting of aromatic vinyl units, vinylcyan units, and (meth)acrylate units, and more preferably contains (meth)acrylate units. In particular, the shell layer preferably contains methyl methacrylate units.
[0066] The composition of the structural units of the shell layer depends on the composition of the monomer for forming the shell layer. When the polymerization conversion rate is 100%, the obtained shell layer contains structural units derived from all of the monomers contained in the monomer for forming the shell layer.
[0067] The total content of one or more structural units selected from the group consisting of aromatic vinyl units, vinylcyan units, and (meth)acrylate units in the shell layer is preferably 10.0% by mass to 99.5% by mass, more preferably 50.0% by mass to 99.0% by mass, even more preferably 65.0% by mass to 98.0% by mass, particularly preferably 67.0% by mass to 80.0% by mass, and most preferably 67.0% by mass to 85.0% by mass, based on 100% by mass of the shell layer (shell polymer).
[0068] Specific examples of the aromatic vinyl monomer from which the aromatic vinyl unit is derived include vinylbenzenes such as styrene, α-methylstyrene, p-methylstyrene, and divinylbenzene.
[0069] Specific examples of the vinylcyanide monomer from which the vinylcyanide unit is derived include acrylonitrile and methacrylonitrile.
[0070] Specific examples of the (meth)acrylate monomers from which the (meth)acrylate units are derived are the same as those described in the section "Core Layer" above, and therefore, the description therein is incorporated by reference and will not be repeated here.
[0071] In order to maintain a good dispersion state without aggregation of the polymer particles in the cured product and the composition, it is preferable to chemically bond the polymer particles to the component (A). In order to chemically bond the polymer particles to the component (A), it is preferable that the shell layer has a structural unit derived from a reactive group-containing monomer. In other words, it is preferable that the shell layer contains a reactive group.
[0072] The reactive group is preferably at least one selected from the group consisting of, for example, an epoxy group, an oxetane group, a hydroxyl group, an amino group, an imide group, a carboxylic acid group, a carboxylic anhydride group, a cyclic ester, a cyclic amide, a benzoxazine group, and a cyanate ester group.
[0073] The reactive group is preferably an epoxy group. In other words, the shell layer preferably has a structural unit derived from a monomer having an epoxy group, that is, preferably has an epoxy group. When the shell layer of the polymer particle has an epoxy group, the composition has excellent storage stability, and has the advantage that a cured product having excellent T-peel adhesive strength can be provided even when the composition is cured at a low temperature.
[0074] Specific examples of the monomer having an epoxy group include glycidyl group-containing vinyl monomers such as glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and allyl glycidyl ether.
[0075] When the shell layer of the polymer particle contains epoxy groups, the content (mmol) of epoxy groups in the shell layer relative to the total mass (g) of the shell layer of the polymer particle is preferably more than 0 mmol / g and not more than 2.0 mmol / g, more preferably 0.1 mmol / g to 2.0 mmol / g, and even more preferably 0.3 mmol / g to 1.5 mmol / g. This configuration suppresses aggregation of the polymer particles, allowing the polymer particles to be dispersed in the cured product in the state of primary particles, and as a result, it is presumed that the T-peel adhesion strength of the cured product can be improved even when cured at low temperatures.
[0076] The monomer having an epoxy group is preferably used to form the shell layer, and more preferably used only to form the shell layer. In other words, it is preferable that the core layer and the intermediate layer do not have an epoxy group.
[0077] From the viewpoint of storage stability of the composition, it is preferable that the shell layer of the polymer particle does not have an epoxy group.
[0078] Specific examples of the reactive group-containing monomer having a hydroxyl group include the above-mentioned hydroxyalkyl (meth)acrylates.
[0079] When the shell layer contains a structural unit derived from a polyfunctional monomer having two or more radically polymerizable double bonds, swelling of the polymer particles in the composition is prevented, and the viscosity of the composition tends to be low, making it easier to handle. Therefore, it is preferable that the shell layer contains a structural unit derived from the polyfunctional monomer. On the other hand, from the viewpoint of excellent effects of improving the toughness and T-peel adhesion strength of the resulting cured product, it is preferable that the shell layer does not contain a structural unit derived from the polyfunctional monomer.
[0080] Specific examples of the polyfunctional monomer do not include conjugated diene monomers such as butadiene, and include allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; allyloxyalkyl (meth)acrylates; polyfunctional (meth)acrylates having two or more (meth)acrylic groups such as (poly)ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate; diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.
[0081] Among these polyfunctional monomers, allyl methacrylate and triallyl isocyanurate are preferred.
[0082] The shell layer is preferably a polymer composed only of the following structural units: (a) aromatic vinyl units (particularly preferably styrene units) 0% to 50% by mass (preferably 0% to 35% by mass, more preferably 0% to 20% by mass), (b) vinylcyan units (particularly preferably acrylonitrile units) 0% to 50% by mass (preferably 0% to 30% by mass, more preferably 0% to 20% by mass), (c) (meth)acrylate units ((i) preferably one or more structural units selected from the group consisting of methyl acrylate units, butyl acrylate units, and methyl methacrylate units, (ii) particularly preferably methyl methacrylate units) 0% to 100% by mass (preferably 5% to 100% by mass, more preferably 70% to 95% by mass), and (d) structural units derived from a monomer having an epoxy group (particularly glycidyl methacrylate units) 0% to 50% by mass (preferably 1% to 35% by mass, more preferably 3% to 20% by mass). However, (i) the total of the aromatic vinyl-based units, vinylcyan-based units, (meth)acrylate-based units, and structural units derived from monomers having an epoxy group is 100% by mass, and (ii) 0% by mass means that the structural units may not be included.
[0083] The above-mentioned monomer components may be used alone or in combination of two or more. The shell layer may contain a structural unit derived from a monomer other than the above-mentioned monomers.
[0084] The shell layer may have a single layer structure or a multi-layer structure, and when the shell layer has a multi-layer structure, the polymer compositions of the layers may be different from each other within the ranges disclosed above.
[0085] <Volume average particle diameter (Mv) of polymer particles> The volume average particle diameter (Mv) of the polymer particles is not particularly limited, but from the viewpoint of industrial productivity and workability of the curable resin composition, it is preferably 0.01 μm to 2.00 μm, more preferably 0.02 μm to 1.00 μm, more preferably 0.03 μm to 0.60 μm, more preferably 0.05 μm to 0.40 μm, more preferably 0.10 μm to 0.30 μm, more preferably 0.15 μm to 0.30 μm, more preferably 0.16 μm to 0.28 μm, more preferably 0.17 μm to 0.27 μm, and even more preferably 0.18 μm to 0.25 μm. When the volume average particle diameter (Mv) of the polymer particles is (a) 0.01 μm or more, the viscosity of the composition is reduced, which is advantageous in that workability is improved, and when it is (b) 2.00 μm or less, the polymerization time of the polymer particles is shortened, which is advantageous in that industrial productivity is increased. The method for measuring the volume average particle diameter (Mv) of the polymer particles will be described in detail in the Examples below.
[0086] When the composition contains polymer particles as component (B), the polymer particles are preferably dispersed in the composition in the form of primary particles. In this specification, "polymer particles dispersed in the form of primary particles" (hereinafter also referred to as "primary dispersion") means that the polymer particles are dispersed substantially independently (without contact) with each other. The dispersion state of the polymer particles in the composition can be confirmed, for example, by mixing a portion of the composition with a solvent such as methyl ethyl ketone, subjecting the resulting mixture to a particle size measurement device using laser light scattering, or the like, and measuring the particle size of the polymer particles in the mixture.
[0087] Furthermore, the term "stable dispersion" of polymer particles means a state in which the polymer particles are dispersed steadily under normal conditions for a long period of time without agglomeration, separation, or precipitation in the continuous layer. It is also preferable that the distribution of the polymer particles in the continuous layer does not change substantially, and that the "stable dispersion" can be maintained even when the composition is heated within a safe range to reduce the viscosity and stirred.
[0088] The polymer particles may be used alone or in combination of two or more kinds.
[0089] <<Method for Producing Polymer Particles>> (Method for Producing Core Layer) The core layer constituting the polymer particles can be formed by, for example, emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. As the methods such as emulsion polymerization, suspension polymerization, and microsuspension polymerization, for example, the methods described in WO 2005 / 028546 and WO 2006 / 070664 can be appropriately used.
[0090] (Method for forming shell layer and intermediate layer) When the polymer particles include an intermediate layer, the intermediate layer can be formed by polymerizing a monomer for forming the intermediate layer by known radical polymerization. When the rubber elastic material constituting the core layer is obtained as an emulsion, it is preferable to polymerize the monomer for forming the intermediate layer by emulsion polymerization.
[0091] The shell layer can be formed by polymerizing a monomer for forming the shell layer by known radical polymerization. When the core layer or the polymer particle precursor formed by coating the core layer with an intermediate layer is obtained as an emulsion, the polymerization of the monomer for forming the shell layer is preferably carried out by emulsion polymerization. For example, the method described in WO 2005 / 028546 can be appropriately used as the emulsion polymerization method.
[0092] In emulsion polymerization, an emulsifier (dispersant) is used.
[0093] Examples of the emulsifier include (i) (i-1) various acids such as alkyl or aryl sulfonic acids typified by dioctylsulfosuccinic acid and dodecylbenzenesulfonic acid; alkyl or aryl ether sulfonic acids; alkyl or aryl sulfuric acids typified by dodecyl sulfate; alkyl or aryl ether sulfuric acids; alkyl or aryl substituted phosphoric acids; alkyl or aryl ether substituted phosphoric acids; N-alkyl or aryl sarcosinic acids typified by dodecyl sarcosinic acid; alkyl or aryl carboxylic acids typified by oleic acid and stearic acid; and alkyl or aryl ether carboxylic acids; and (i-2) anionic emulsifiers (dispersants) such as alkali metal salts or ammonium salts of these acids, (ii) nonionic emulsifiers (dispersants) such as alkyl or aryl substituted polyethylene glycol, and (iii) dispersants such as polyvinyl alcohol, alkyl substituted cellulose, polyvinylpyrrolidone, and polyacrylic acid derivatives.
[0094] These emulsifiers (dispersants) may be used alone or in combination of two or more.
[0095] It is preferable to use a small amount of emulsifier (dispersant) as long as it does not impair the dispersion stability of the aqueous latex of polymer particles. Furthermore, the higher the water solubility of the emulsifier (dispersant), the more preferable it is. High water solubility makes it easier to wash off the emulsifier (dispersant) with water, and can easily prevent adverse effects on the final cured product.
[0096] When emulsion polymerization is employed, peroxides (for example, organic peroxides), chain transfer agents, surfactants, and the like may be used as needed.
[0097] The polymerization conditions such as polymerization temperature, pressure, deoxidation, etc., may be within known ranges.
[0098] The present composition preferably contains at least polymer particles as component (B) because this provides an excellent balance between the storage stability of the resulting composition and the toughness-improving effect and T-peel adhesion strength of the resulting cured product.
[0099] When the composition contains polymer particles as component (B), the content of the polymer particles in the composition is preferably 1 to 100 parts by mass, more preferably 5 to 90 parts by mass, even more preferably 10 to 80 parts by mass, even more preferably 20 to 70 parts by mass, and particularly preferably 30 to 60 parts by mass, per 100 parts by mass of component (A). This configuration has the advantage of providing an excellent balance between the storage stability of the resulting composition and the toughness-improving effect and T-peel adhesion strength of the resulting cured product.
[0100] <Blocked Urethane> In this specification, the term "blocked urethane" refers to an "elastomeric compound containing a urethane group and / or a urea group and having a terminal isocyanate group," in which all or some of the terminal isocyanate groups have been capped with various blocking agents having active hydrogen groups. The compound capped with a blocking agent, i.e., the blocked urethane itself, may be an elastomer. As the blocked urethane, a compound in which all of the terminal isocyanate groups have been capped with a blocking agent is particularly preferred. Blocked urethanes can be obtained, for example, by the following methods: (A) (A-1) reacting an organic polymer having an active hydrogen-containing group at its terminal with an excess of a polyisocyanate compound to obtain a polymer (urethane prepolymer) having urethane groups and / or urea groups in the main chain and isocyanate groups at its terminal; (A-2) subsequently capping all or some of the isocyanate groups with a blocking agent having an active hydrogen group; or (B) reacting an organic polymer having an active hydrogen-containing group at its terminal with an excess of a polyisocyanate compound and simultaneously reacting it with a blocking agent, thereby capping all or some of the isocyanate groups of the urethane prepolymer with the blocking agent having an active hydrogen group.
[0101] Specific examples of blocked urethanes include compounds described in WO 2016 / 163491.
[0102] The number average molecular weight of the blocked urethane, in terms of polystyrene equivalent molecular weight measured by GPC, is preferably 2,000 to 40,000, more preferably 3,000 to 30,000, and particularly preferably 4,000 to 20,000. The molecular weight distribution (weight average molecular weight / number average molecular weight) of the blocked urethane is preferably 1.0 to 4.0, more preferably 1.2 to 3.0, and particularly preferably 1.5 to 2.5.
[0103] The blocked urethane may be used alone or in combination of two or more.
[0104] From the viewpoint of improving the toughness, impact resistance, and adhesive properties (for example, T-peel adhesion strength) of the resulting cured product, the present composition preferably contains at least a blocked urethane as component (B).
[0105] When the composition contains a blocked urethane as component (B), the content of the blocked urethane in the composition is, from the above-mentioned viewpoints, preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, and particularly preferably 5 to 30 parts by mass, per 100 parts by mass of component (A). When the content of the blocked urethane in the composition is (a) 1 part by mass or more per 100 parts by mass of component (A), the toughness, impact resistance, and adhesive properties (e.g., T-peel adhesion strength) of the cured product obtained by curing the resulting composition are favorably improved, and when the content is (b) 50 parts by mass or less, the resulting cured product has the advantage of being excellent in heat resistance and having a high modulus of elasticity.
[0106] <Rubber-Modified Epoxy Resin> The rubber-modified epoxy resin is a reaction product obtained by reacting rubber with an epoxy group-containing compound (e.g., an epoxy resin). The rubber-modified epoxy resin preferably has an average of 1.1 or more epoxy groups per molecule, and more preferably 2 or more epoxy groups.
[0107] Examples of rubber include rubber-based polymers such as acrylonitrile-butadiene rubber (NBR), styrene-butadiene rubber (SBR), hydrogenated nitrile rubber (HNBR), ethylene-propylene rubber (EPDM), acrylic rubber (ACM), butyl rubber (IIR), butadiene rubber, and polyoxyalkylene (e.g., polypropylene oxide, polyethylene oxide, polytetramethylene oxide, etc.). The rubber-based polymer preferably has a terminal reactive group (a functional group capable of reacting with an epoxy group), such as an amino group, a hydroxy group, or a carboxyl group. The rubber-modified epoxy resin used in one embodiment of the present invention is a reaction product obtained by reacting these rubber-based polymers with an epoxy group-containing compound (e.g., an epoxy resin) in an appropriate blending ratio using a known method. Among these, from the viewpoints of the adhesiveness and impact peel adhesion resistance of the resulting curable resin composition, acrylonitrile-butadiene rubber-modified epoxy resins and polyoxyalkylene-modified epoxy resins are preferred, with acrylonitrile-butadiene rubber-modified epoxy resins being more preferred. The acrylonitrile-butadiene rubber modified epoxy resin can be obtained, for example, by reacting carboxyl-terminated NBR (CTBN) with bisphenol A type epoxy resin.
[0108] The content of the acrylonitrile monomer component (acrylonitrile unit) in the acrylonitrile-butadiene rubber (100% by mass) is preferably 5% by mass to 40% by mass, more preferably 10% by mass to 35% by mass, and even more preferably 15% by mass to 30% by mass, from the viewpoint of the adhesiveness and impact peel adhesion resistance of the resulting curable resin composition. The content of the acrylonitrile monomer component (acrylonitrile unit) in the acrylonitrile-butadiene rubber (100% by mass) is particularly preferably 20% by mass to 30% by mass, from the viewpoint of the workability of the resulting curable resin composition.
[0109] Furthermore, rubber-modified epoxy resins also include, for example, addition reaction products (hereinafter also referred to as "adducts") between amino-terminated polyoxyalkylenes and epoxy resins. The adducts can be easily produced by known methods, as described in, for example, U.S. Pat. Nos. 5,084,532 and 6,015,865. Examples of the epoxy resins used in producing the adducts include the specific examples of component (A) described above. As the epoxy resins used in producing the adducts, bisphenol A epoxy resins and bisphenol F epoxy resins are preferred, with bisphenol A epoxy resins being more preferred. Commercially available amino-terminated polyoxyalkylenes used in producing the adduct include, for example, Jeffamine (registered trademark) D-230, Jeffamine (registered trademark) D-400, Jeffamine (registered trademark) D-2000, Jeffamine (registered trademark) D-4000, and Jeffamine (registered trademark) T-5000, all of which are manufactured by Huntsman.
[0110] The reactive groups contained in the molecular terminals of the rubber are sometimes referred to as "epoxide reactive end groups." The average number of epoxide reactive end groups contained per rubber molecule is preferably 1.5 to 2.5, more preferably 1.8 to 2.2. The number average molecular weight of the rubber, as measured by GPC in terms of polystyrene, is preferably 1,000 to 10,000, more preferably 2,000 to 8,000, and particularly preferably 3,000 to 6,000.
[0111] There are no particular limitations on the method for producing rubber-modified epoxy resins. For example, rubber-modified epoxy resins can be produced by reacting rubber with an epoxy group-containing compound in a large amount of epoxy group-containing compound. Specifically, rubber-modified epoxy resins are preferably produced by reacting two or more equivalents of epoxy group-containing compound per equivalent of epoxy-reactive terminal groups in the rubber. It is more preferable to react a sufficient amount of epoxy group-containing compound with rubber so that the resulting product is a mixture of an adduct of rubber and epoxy group-containing compound and free epoxy group-containing compound. For example, rubber-modified epoxy resins can be produced by heating a mixture of rubber and epoxy group-containing compound to a temperature of 100°C to 250°C in the presence of a catalyst such as phenyldimethylurea and triphenylphosphine. While there are no particular limitations on the epoxy group-containing compound used in producing rubber-modified epoxy resins, bisphenol A epoxy resins and bisphenol F epoxy resins are preferred, with bisphenol A epoxy resins being more preferred.
[0112] In the case of rubber-modified epoxy resins, the epoxy resin can be modified by pre-reacting a bisphenol component with rubber. The amount of the bisphenol component used for modification is preferably 3 to 35 parts by mass, more preferably 5 to 25 parts by mass, per 100 parts by mass of the rubber component in the rubber-modified epoxy resin. The cured product obtained by curing a curable resin composition containing the modified rubber-modified epoxy resin has excellent adhesion durability after exposure to high temperatures and also excellent impact resistance at low temperatures.
[0113] The glass transition temperature (Tg) of the rubber-modified epoxy resin is not particularly limited, but is preferably −25° C. or lower, more preferably −35° C. or lower, even more preferably −40° C. or lower, and particularly preferably −50° C. or lower.
[0114] The number average molecular weight of the rubber-modified epoxy resin, as measured by GPC in terms of polystyrene, is preferably 1,500 to 40,000, more preferably 3,000 to 30,000, and particularly preferably 4,000 to 20,000. The molecular weight distribution (ratio of weight average molecular weight to number average molecular weight (weight average molecular weight / number average molecular weight)) of the rubber-modified epoxy resin is preferably 1 to 4, more preferably 1.2 to 3, and particularly preferably 1.5 to 2.5.
[0115] From the viewpoint of the balance of toughness, impact peel adhesion, heat resistance, and modulus of elasticity (rigidity) of the cured product, the present composition preferably contains at least a rubber-modified epoxy resin as component (B).
[0116] When the present composition contains a rubber-modified epoxy resin as component (B), the content of the rubber-modified epoxy resin in the composition is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, even more preferably 5 to 30 parts by mass, and particularly preferably 10 to 20 parts by mass, per 100 parts by mass of component (A). When the content of the rubber-modified epoxy resin in the composition is (a) 1 part by mass or more per 100 parts by mass of component (A), the obtained cured product has the advantage of excellent toughness and good impact peel adhesion, and when the content is (b) 50 parts by mass or less, the obtained cured product has the advantage of good heat resistance and / or elastic modulus (rigidity).
[0117] The rubber-modified epoxy resins may be used alone or in combination of two or more.
[0118] <Urethane-modified epoxy resin> The urethane-modified epoxy resin is a reaction product obtained by reacting (i) a compound containing an epoxy group and a group reactive with an isocyanate group with (ii) a urethane prepolymer containing an isocyanate group. The urethane-modified epoxy resin preferably has an average of 1.1 or more epoxy groups per molecule, more preferably 2 or more. For example, a urethane-modified epoxy resin can be obtained by reacting a hydroxyl-containing epoxy compound with a urethane prepolymer.
[0119] The number average molecular weight of the urethane-modified epoxy resin, as measured by GPC in terms of polystyrene, is preferably 1,500 to 40,000, more preferably 3,000 to 30,000, and particularly preferably 4,000 to 20,000. The molecular weight distribution (ratio of weight average molecular weight to number average molecular weight (weight average molecular weight / number average molecular weight)) of the urethane-modified epoxy resin is preferably 1 to 4, more preferably 1.2 to 3, and particularly preferably 1.5 to 2.5.
[0120] From the viewpoint of the balance between toughness and heat resistance of the cured product, the present composition preferably contains at least a rubber-modified epoxy resin as component (B).
[0121] When the present composition contains a urethane-modified epoxy resin as component (B), the content of the urethane-modified epoxy resin in the composition is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, even more preferably 5 to 30 parts by mass, and particularly preferably 10 to 20 parts by mass, per 100 parts by mass of component (A). When the content of the urethane-modified epoxy resin in the composition is (a) 1 part by mass or more per 100 parts by mass of component (A), the obtained cured product has the advantage of excellent toughness, and when (b) 50 parts by mass or less, the obtained cured product has the advantage of good heat resistance.
[0122] The urethane-modified epoxy resin may be used alone or in combination of two or more.
[0123] In this composition, the content of component (B) is 1 to 100 parts by mass, more preferably 5 to 90 parts by mass, even more preferably 10 to 80 parts by mass, even more preferably 20 to 70 parts by mass, and particularly preferably 30 to 60 parts by mass, per 100 parts by mass of component (A). This configuration has the advantage that the resulting cured product has excellent toughness, impact resistance, and adhesion (e.g., T-peel adhesion strength). Note that the "content of component (B)" refers to the total content of polymer particles having a core-shell structure containing a core layer and a shell layer, blocked urethane, rubber-modified epoxy resin, and urethane-modified epoxy resin contained in the composition.
[0124] <(C) Dicyandiamide> The present composition contains dicyandiamide as component (C). In the present composition, dicyandiamide, which is component (C), can function as a curing agent that cures the composition. Dicyandiamide does not exhibit a curing action at temperatures below 100°C, or, even if it does exhibit a curing action, the curing reaction proceeds very slowly. On the other hand, when dicyandiamide is heated to a temperature of 100°C or higher (preferably 120°C), it rapidly exhibits a curing action and can rapidly cure the composition. Therefore, dicyandiamide is sometimes referred to as a latent curing agent.
[0125] As described above, dicyandiamide does not exhibit a curing effect at temperatures around room temperature, or if it does, the curing reaction proceeds very slowly. Therefore, even though the present composition is a one-component thermosetting resin composition, there is no risk of the composition unintentionally curing during storage. In other words, the present composition has excellent storage stability due to the inclusion of dicyandiamide as a curing agent.
[0126] In the present composition, the content of component (C) per 100 parts by mass of component (A) is 3.5 to 19.0 parts by mass, preferably 3.5 to 18.0 parts by mass, more preferably 4.0 to 16.0 parts by mass, more preferably 4.5 to 14.0 parts by mass, even more preferably 5.0 to 12.0 parts by mass, even more preferably 6.0 to 10.0 parts by mass, and particularly preferably 7.0 to 8.5 parts by mass. When the content of component (C) per 100 parts by mass of component (A) is (a) 3.5 parts by mass or more, there is an advantage that the cured product obtained by curing the present composition at low temperature has sufficient T-peel adhesive strength, and when it is (b) 19.0 parts by mass or less, there is an advantage that the storage stability of the present composition is good.
[0127] <(D) Monocarboxylic Acid and / or Metal Salt of Monocarboxylic Acid> The present composition contains, as component (D), (i) a monocarboxylic acid but no metal salt of monocarboxylic acid, (ii) a metal salt of monocarboxylic acid but no monocarboxylic acid, or (iii) both a monocarboxylic acid and a metal salt of monocarboxylic acid.
[0128] Through extensive research, the present inventors independently and independently discovered the novel finding that the addition of component (D) to a composition containing the aforementioned components (A), (B), and (C) surprisingly improves the T-peel adhesive strength of the cured product obtained by low-temperature curing of the resulting composition. While the reason why the addition of component (D) improves T-peel adhesive strength is unclear, it is speculated as follows: The curing process of component (A) (epoxy resin) using component (C) dicyandiamide as a curing agent is speculated as follows (see Takashi Kamon et al., Polymers Review, Vol. 34, No. 7, pp. 537-543). When a composition containing component (A) (epoxy resin) and component (C) (dicyandiamide) is heated, cyanamide produced from component (C) (dicyandiamide) first reacts with component (A) (epoxy resin) to form a linear polymer having hydroxyl and cyano groups. Next, the hydroxyl groups and cyano groups in the linear polymers react to form a three-dimensional crosslinked structure, which causes the composition to harden. At this time, if component (D) is present, the carboxyl groups and / or —C(═O)O groups of component (D) react to form a three-dimensional crosslinked structure, which causes the composition to harden. - The ions react with some of the cyano groups, inhibiting some of the reactions between the hydroxyl groups and cyano groups of the linear polymer and reducing the crosslink density of the three-dimensional crosslinked structure. This increases the molecular weight between crosslink points in the cured product, making the cured product more susceptible to plastic deformation and improving the T-peel adhesive strength. However, the present invention is not limited to this assumption.
[0129] The monocarboxylic acid is not particularly limited, and examples thereof include formic acid, acetic acid, propionic acid, butyric acid, naphthenic acid, fatty acids, aromatic monocarboxylic acids, amino acids, hydroxy acids, and keto acids.
[0130] In this specification, the term "fatty acid" refers to an organic acid having a carbonyl group and having 4 or more carbon atoms in the portion other than the carbonyl group.
[0131] Fatty acids include saturated fatty acids and unsaturated fatty acids. Saturated fatty acids include hexanoic acid, 2-ethylhexanoic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, eicosanoic acid, behenic acid, and lignoceric acid. Unsaturated fatty acids include oleic acid, linoleic acid, linolenic acid, arachidonic acid, and sorbic acid. Aromatic monocarboxylic acids include benzoic acid, salicylic acid, mellitic acid, and cinnamic acid. Hydroxy acids include lactic acid. Keto acids include pyruvic acid and acetoacetic acid.
[0132] Monocarboxylic acids also include α,β-unsaturated fatty acids, such as methacrylic acid, acrylic acid, and cinnamic acid.
[0133] As the monocarboxylic acid, one type may be used alone, or two or more types may be used in combination.
[0134] The monocarboxylic acid metal salt is not particularly limited. As the monocarboxylic acid metal salt, metal salts of the monocarboxylic acids exemplified above are preferred. Examples of the monocarboxylic acid metal salt include divalent tin salts of monocarboxylic acids (e.g., tin octoate, tin versatate, tin stearate, etc.), tetravalent tin salts (e.g., dibutyltin dilaurate, etc.), magnesium salts (e.g., magnesium octoate, magnesium naphthenate, magnesium stearate, etc.), iron salts (e.g., iron octoate, iron naphthenate, iron stearate, etc.), titanium salts (e.g., titanium octoate, titanium naphthenate, titanium stearate, etc.), aluminum salts (e.g., aluminum octoate, aluminum naphthenate, aluminum tristearate ((C 17 H 35 COO) 3 Al), aluminum distearate ((C 17 H 35 COO)2 Al(OH)) and aluminum monostearate ((C 17 H 35 COO)Al(OH) 2 ), cobalt salts (e.g., cobalt octylate, etc.), manganese salts (e.g., manganese octylate, etc.), lead salts (e.g., lead octylate, etc.), zinc salts (e.g., zinc octylate, etc.), zirconium salts (e.g., zirconium octylate, etc.), calcium salts (e.g., calcium octylate, etc.), nickel salts (e.g., nickel octylate, etc.), potassium salts (e.g., potassium octylate, etc.), lithium salts (e.g., lithium octylate, etc.), and bismuth salts (e.g., bismuth octylate, bismuth versatate, bismuth stearate, etc.).
[0135] In order to provide a composition with excellent workability (handling properties) and a cured product with excellent heat resistance, the molecular weight of the monocarboxylic acid is not particularly limited, but is preferably 60 to 700, more preferably 100 to 500, even more preferably 140 to 400, even more preferably 250 to 350, and particularly preferably 300 to 350.
[0136] In order to provide a composition with excellent workability (handling properties) and a cured product with excellent heat resistance, the molecular weight of the monocarboxylic acid metal salt is not particularly limited, but is preferably 60 to 2,000, more preferably 100 to 1,000, even more preferably 200 to 800, and particularly preferably 300 to 600.
[0137] The total content of the monocarboxylic acid having a molecular weight of 60 to 700 and the metal salt of a monocarboxylic acid having a molecular weight of 60 to 2,000 is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and particularly preferably 99 to 100% by mass, based on 100% by mass of component (D). This configuration has the advantages of providing a composition with superior workability (handling properties) and providing a cured product with superior heat resistance. Component (D) may be composed solely of a monocarboxylic acid having a molecular weight of 60 to 700 and / or a metal salt of a monocarboxylic acid having a molecular weight of 60 to 2,000.
[0138] The melting point of component (D) is not particularly limited, but is preferably 60°C or higher, more preferably 70°C or higher, more preferably 80°C or higher, even more preferably 100°C or higher, and particularly preferably 120°C or higher. This configuration has the advantage of improving the storage stability of the composition. The melting point of component (D) may be 145°C or higher. The upper limit of the melting point of component (D) is not particularly limited, but is, for example, 180°C or lower.
[0139] The content of component (D) having a melting point of 60°C or higher, relative to 100% by mass of component (D), is preferably 80% by mass to 100% by mass, more preferably 90% by mass to 100% by mass, even more preferably 95% by mass to 100% by mass, and particularly preferably 99% by mass to 100% by mass. This configuration has the advantage of improving the storage stability of the composition.
[0140] From the viewpoint of the balance between the storage stability of the composition and the T-peel adhesive strength of the resulting cured product, the composition preferably contains at least a monocarboxylic acid metal salt as component (D). The content of the monocarboxylic acid metal salt, based on 100% by mass of component (D), is preferably 50% to 100% by mass, more preferably 80% to 100% by mass, even more preferably 90% to 100% by mass, and particularly preferably 100% by mass. In other words, it is particularly preferable that component (D) is composed solely of a monocarboxylic acid metal salt. This configuration offers the advantages of good storage stability of the composition and excellent T-peel adhesive strength of the resulting cured product.
[0141] Since a cured product having excellent T-peel adhesive strength can be obtained, the metal salt of monocarboxylic acid preferably contains one or more metal salts selected from the group consisting of divalent tin salts, magnesium salts, iron salts, titanium salts, and aluminum salts of monocarboxylic acids, more preferably contains one or more metal salts selected from the group consisting of divalent tin salts, magnesium salts, and aluminum salts of monocarboxylic acids, even more preferably contains one or more metal salts selected from the group consisting of magnesium salts and aluminum salts of monocarboxylic acids, and particularly preferably contains an aluminum salt of monocarboxylic acids.
[0142] The total content of one or more metal salts selected from the group consisting of divalent tin salts, magnesium salts, iron salts, titanium salts, and aluminum salts of monocarboxylic acids, relative to 100% by mass of component (D), is preferably 80% to 100% by mass, more preferably 90% to 100% by mass, even more preferably 95% to 100% by mass, and particularly preferably 99% to 100% by mass. This configuration has the advantage that the cured product has superior T-peel adhesive strength.
[0143] It is particularly preferred that the monocarboxylic acid contains at least a fatty acid, as this is easily available and gives a cured product with excellent T-peel adhesive strength.
[0144] The content of fatty acids in 100% by mass of monocarboxylic acids is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 99% by mass or more. This configuration has the advantage that the cured product has superior T-peel adhesive strength.
[0145] It is particularly preferred that the monocarboxylic acid metal salt contains at least a fatty acid metal salt, since the fatty acid as a raw material is easily available and a cured product having excellent T-peel adhesive strength can be obtained.
[0146] The content of the fatty acid metal salt in 100% by mass of the monocarboxylic acid metal salt is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 99% by mass or more. This configuration has the advantage that the cured product has superior T-peel adhesive strength.
[0147] From the viewpoint of the workability (handleability) of the composition, the monocarboxylic acid may contain an α,β-unsaturated carboxylic acid. When the monocarboxylic acid contains an α,β-unsaturated carboxylic acid, the content of the α,β-unsaturated carboxylic acid, relative to 100% by mass of the monocarboxylic acid, is preferably more than 0% by mass and not more than 0.10% by mass, more preferably 0.01% by mass to 0.10% by mass, even more preferably 0.01% by mass to 0.08% by mass, and particularly preferably 0.01% by mass to 0.05% by mass. This configuration has the advantage of low volatility and excellent workability of the composition.
[0148] Since a cured product having excellent adhesive strength can be obtained, the lower the content of α,β-unsaturated carboxylic acid in the monocarboxylic acid, the more preferable. In one embodiment of the present invention, the content of α,β-unsaturated carboxylic acid in 100% by mass of monocarboxylic acid is preferably 0.010% by mass or less, more preferably 0.005% by mass or less, even more preferably 0% by mass to 0.005% by mass, and particularly preferably 0% by mass. In other words, it is particularly preferable that the monocarboxylic acid does not contain α,β-unsaturated carboxylic acid.
[0149] Through extensive research, the present inventors independently and surprisingly discovered that the amount of component (D) relative to the amount of component (C) affects the T-peel adhesive strength of the cured product obtained by low-temperature curing. The present inventors further independently and independently discovered that when the ratio of the molar amount of component (D) to twice the molar amount of component (C) in the composition (the molar amount of component (D) / twice the molar amount of component (C)) is 0.001 to 0.400, the composition achieves a particularly excellent balance between the storage stability and the T-peel adhesive strength of the cured product obtained by low-temperature curing.
[0150] In order to provide a composition with excellent storage stability and a cured product obtained by low-temperature curing with excellent T-peel adhesive strength, the molar amount of component (D) / twice the molar amount of component (C) is more preferably 0.001 to 0.350, more preferably 0.002 to 0.300, more preferably 0.003 to 0.250, more preferably 0.004 to 0.250, more preferably 0.005 to 0.200, more preferably 0.007 to 0.200, even more preferably 0.009 to 0.180, and particularly preferably 0.010 to 0.150.
[0151] In the present composition, the content of component (D) per 100 parts by mass of component (A) is 0.01 to 30.00 parts by mass, preferably 0.03 to 20.00 parts by mass, more preferably 0.05 to 15.00 parts by mass, more preferably 0.10 to 10.00 parts by mass, and particularly preferably 0.30 to 8.00 parts by mass. When the content of component (C) per 100 parts by mass of component (A) is (a) 0.01 part by mass or more, there is an advantage that the cured product obtained by curing the composition at low temperature has sufficient T-peel adhesive strength, and when it is (b) 30.00 parts by mass or less, there is an advantage that the storage stability of the composition is good. The term "content of component (D)" refers to (i) the content of monocarboxylic acid when the composition contains a monocarboxylic acid as component (D) but does not contain a monocarboxylic acid metal salt, (ii) the content of monocarboxylic acid metal salt when the composition contains a monocarboxylic acid as component (D) but does not contain a monocarboxylic acid, and (iii) the total content of monocarboxylic acid and monocarboxylic acid metal salt when the composition contains both a monocarboxylic acid and a monocarboxylic acid metal salt as component (D).
[0152] <Monocarboxylic Acid-Amine Complex> From the viewpoint of balancing the storage stability of the composition and the T-peel adhesive strength of the cured product, the composition may further contain a monocarboxylic acid-amine complex. When the composition contains a monocarboxylic acid-amine complex, the content of the monocarboxylic acid-amine complex in the composition is preferably more than 0 parts by mass and not more than 0.10 parts by mass, more preferably 0.01 parts by mass to 0.10 parts by mass, even more preferably 0.01 parts by mass to 0.08 parts by mass, and particularly preferably 0.01 parts by mass to 0.05 parts by mass, per 100 parts by mass of component (A). This configuration has the advantages of providing the composition with excellent storage stability and providing the cured product with excellent T-peel adhesive strength.
[0153] Since the composition has excellent storage stability, the smaller the content of the monocarboxylic acid-amine complex in the composition, the better. In the present composition, the content of the monocarboxylic acid-amine complex per 100 parts by mass of component (A) is preferably 0.010 parts by mass or less, more preferably 0.005 parts by mass or less, even more preferably 0 to 0.005 parts by mass, and particularly preferably 0 part by mass. In other words, it is particularly preferable that the present composition does not contain a monocarboxylic acid-amine complex.
[0154] <(E) Epoxy-based reactive diluent> The present composition preferably further comprises an epoxy-based reactive diluent as component (E). In this specification, the term "epoxy-based reactive diluent" refers to a compound that has an epoxy group and a viscosity of 500 mPa·s or less at 25°C. When the composition comprises component (E), i.e., an epoxy-based reactive diluent, there is an advantage that the cured product obtained by curing the composition at low temperature has superior T-peel adhesive strength.
[0155] Examples of the epoxy-based reactive diluent include polyalkylene glycol diglycidyl ether, glycol diglycidyl ether, diglycidyl ester of an aliphatic polybasic acid, glycidyl ether of a dihydric or higher polyhydric aliphatic alcohol, and monoepoxide.
[0156] More specific examples of the polyalkylene glycol diglycidyl ether include polyethylene glycol diglycidyl ether and polypropylene glycol diglycidyl ether. More specific examples of the glycol diglycidyl ether include neopentyl glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and cyclohexanedimethanol diglycidyl ether. More specific examples of the diglycidyl esters of aliphatic polybasic acids include dimer acid diglycidyl ester, adipic acid diglycidyl ester, sebacic acid diglycidyl ester, and maleic acid diglycidyl ester. More specific examples of the glycidyl ethers of dihydric or higher polyhydric aliphatic alcohols include trimethylolpropane triglycidyl ether, trimethylolethane triglycidyl ether, castor oil-modified polyglycidyl ether, propoxylated glycerin triglycidyl ether, and sorbitol polyglycidyl ether.
[0157] Examples of monoepoxides include aliphatic glycidyl ethers such as butyl glycidyl ether; aromatic glycidyl ethers such as phenyl glycidyl ether and cresyl glycidyl ether (o-cresyl glycidyl ether); ethers containing a glycidyl group and an alkyl group having 8 to 10 carbon atoms, such as 2-ethylhexyl glycidyl ether; ethers containing a glycidyl group and a phenyl group having 6 to 12 carbon atoms, which may be substituted with an alkyl group having 2 to 8 carbon atoms, such as p-tert-butylphenyl glycidyl ether; ethers containing a glycidyl group and an alkyl group having 12 to 14 carbon atoms, such as dodecyl glycidyl ether (alkyl C12-C14 glycidyl ether); aliphatic glycidyl esters such as glycidyl (meth)acrylate and glycidyl maleate; glycidyl esters of aliphatic carboxylic acids having 8 to 12 carbon atoms, such as versatic acid glycidyl ester, neodecanoic acid glycidyl ester, and lauric acid glycidyl ester; and p-t-butylbenzoic acid glycidyl ester.
[0158] The epoxy-based reactive diluent preferably contains an epoxy-based reactive diluent having one epoxy group per molecule. This configuration has the advantages of providing a cured product with excellent impact peel adhesion resistance and a composition with excellent storage stability. Examples of epoxy-based reactive diluents having one epoxy group per molecule include neodecanoic acid glycidyl ester, phenyl glycidyl ether, cresyl glycidyl ether, 4-tert-butylphenyl glycidyl ether, and 2-ethylhexyl glycidyl ether.
[0159] The component (E) in the present composition preferably contains, based on 100 mass% of the component (E), 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and particularly preferably 90 mass% to 100 mass% of an epoxy-based reactive diluent having one epoxy group per molecule. The component (E) may contain, based on 100 mass% of the component (E), 100 mass% of an epoxy-based reactive diluent having one epoxy group per molecule; in other words, the component (E) may be composed solely of an epoxy-based reactive diluent having one epoxy group per molecule.
[0160] Commercially available epoxy-based reactive diluents can also be used. Examples of commercially available epoxy-based reactive diluents include YED216M (manufactured by Mitsubishi Chemical, 1,6-hexanediol diglycidyl ether), Cardura (registered trademark) E10P (manufactured by Hexion, neodecanoic acid glycidyl ester), ERISYS (registered trademark) GE-10 (manufactured by Huntsman, o-cresyl glycidyl ether), 4-tert-butylphenyl glycidyl ether (manufactured by Tokyo Chemical Industry Co., Ltd.), ERISYS (registered trademark) GE-6 (manufactured by Huntsman, 2-ethylhexyl glycidyl ether), ERISYS (registered trademark) GE-8 (manufactured by Huntsman, alkyl C12-C14 glycidyl ether), ERISYS (registered trademark) GE-20 (manufactured by Huntsman, neopentyl glycol diglycidyl ether), and ERISYS (registered trademark). Examples of such diluents include GE-21 (1,4-butanediol diglycidyl ether, manufactured by Huntsman) and ERISYS (registered trademark) GE-24 (polypropylene glycol diglycidyl ether, manufactured by Huntsman). Note that Cardura (registered trademark) E10P, ERISYS (registered trademark) GE-10, 4-tert-butylphenyl glycidyl ether, ERISYS (registered trademark) GE-6, and ERISYS (registered trademark) GE-8 are each epoxy-based reactive diluents having one epoxy group per molecule.
[0161] In the present composition, the amount of component (E) per 100 parts by mass of component (A) is preferably 1.0 part to 20.0 parts by mass, more preferably 2.0 parts to 18.0 parts by mass, more preferably 4.0 parts to 16.0 parts by mass, even more preferably 6.0 parts to 14.0 parts by mass, and particularly preferably 8.0 parts to 12.0 parts by mass. When the amount of component (E) per 100 parts by mass of component (A) is within the above-mentioned range, the composition has the advantage of exhibiting excellent T-peel adhesive strength when cured at low temperatures.
[0162] <(F) Amine Adduct Curing Agent> The present composition preferably further comprises, as component (F), an amine adduct curing agent that is solid at room temperature. In the present composition, the amine adduct curing agent can function as a curing agent that cures the composition. In the present composition, the amine adduct curing agent contained as component (F) is solid at room temperature. More specifically, in the present composition, the amine adduct curing agent contained as component (F) is a solid that is insoluble in component (A) at room temperature (e.g., 25°C), and is a compound that becomes soluble in component (A) upon heating and functions as a curing agent for component (A). The amine adduct curing agent can also be referred to as a latent curing agent, and more specifically, as a latent modified polyamine-based curing agent that is solid at room temperature.
[0163] The amine adduct curing agent of component (F) does not exhibit a curing effect at temperatures below 80° C., or if it does exhibit a curing effect, the curing reaction proceeds very slowly. On the other hand, when heated to a temperature of 80° C. or higher (preferably 120° C.), the amine adduct curing agent of component (F) exhibits a rapid curing effect, allowing the composition to cure rapidly.
[0164] As described above, component (F) does not exhibit a curing effect at room temperature, or if it does, the curing reaction proceeds very slowly. Therefore, even though the present composition is a one-component thermosetting resin composition, there is no risk of the composition unintentionally curing during storage. In other words, the present composition has excellent storage stability due to the inclusion of component (F) as a curing agent.
[0165] Examples of the amine adduct curing agent (G) contained as component (F) in the present composition include amine-epoxy adduct curing agents which are reaction products of amine compounds and epoxy compounds (e.g., Amicure (registered trademark) PN23, PN31, PN40, PN50, PN-H manufactured by Ajinomoto Fine-Techno Co., Ltd.; AJICURE (registered trademark) manufactured by Ajinomoto Fine-Techno Co., Ltd.) PN23, PN31, PN40, PN50, PN-H: Hardener X-3661S, X-3670S manufactured by ACR Corporation; Novacure (registered trademark) HX-3742, HX-3721 manufactured by Asahi Kasei Corporation; ADEKA Hardener (registered trademark) EH3293S, EH3366S, EH4346S manufactured by ADEKA Corporation; urea-type adduct curing agents which are reaction products of amine compounds and isocyanate compounds or urea compounds (e.g., Fujicure FXR-1020, FXR-1121, FXR-1081, 1061, 1171, etc. manufactured by T&K TOKA (Fuji Chemical Industry Co., Ltd.)), etc. Amine-epoxy adduct curing agents are sometimes referred to as epoxy compound adduct curing agents.
[0166] The component (F) preferably contains, as the amine adduct curing agent, one or more selected from the group consisting of amine-epoxy adduct curing agents and urea adduct curing agents, and particularly preferably contains one or more selected from amine-epoxy adduct curing agents, because this provides the composition with excellent fast-curing properties at low temperatures and the cured product obtained by curing with the composition with excellent heat resistance.
[0167] The component (F) preferably contains one or more selected from the group consisting of amine-epoxy adduct curing agents in an amount of 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 90 to 100% by mass, based on 100% by mass of the component (F).
[0168] The component (F) may be composed of only one or more selected from the group consisting of amine-epoxy adduct curing agents and urea adduct curing agents, or may be composed of only one or more selected from the group consisting of urea adduct curing agents, or may be composed of only one or more selected from the group consisting of amine-epoxy adduct curing agents.
[0169] Component (F) preferably contains an amine adduct curing agent having a softening temperature of 80° C. to 140° C. This configuration has the advantage of providing an excellent balance between the T-peel adhesive strength and storage stability of the cured product. Examples of amine adduct curing agents having a softening temperature of 80°C to 140°C include: (i) Amicure (registered trademark) PN-23 (95°C), Amicure (registered trademark) PN-23J (95°C), Amicure (registered trademark) PN-H (102°C), Amicure (registered trademark) PN-40 (108°C), Amicure (registered trademark) PN-40J (106°C), Amicure (registered trademark) PN-31J (109°C), Amicure (registered trademark) PN-50 (115°C), Amicure (registered trademark) MY-24 (120°C), Ajicure PN-23 (95°C), Ajicure PN-23J (95°C), Ajicure PN-H (102°C), and Ajic ...50 (115°C), all manufactured by Ajinomoto Fine-Techno Co., Ltd. PN-40 (108°C), Ajicure PN-40J (106°C), Ajicure PN-31J (109°C), Ajicure PN-50 (115°C), and Ajicure MY-24 (120°C); and (ii) Fujicure FXR-1020 (120°C to 130°C), Fujicure FXR-1081 (115°C to 125°C), Fujicure 1061 (90°C to 110°C), Fujicure FXR-1121 (128°C to 138°C), and Fujicure 1171 (105°C to 115°C), manufactured by T&K TOKA (Fuji Chemical Industry Co., Ltd.) (the temperature in parentheses indicates the softening temperature).
[0170] In the present composition, the content of component (F) per 100 parts by mass of component (A) is preferably 0.3 parts by mass to 10.0 parts by mass, more preferably 0.5 parts by mass to 8.0 parts by mass, more preferably 0.8 parts by mass to 6.0 parts by mass, more preferably 1.0 parts by mass to 4.0 parts by mass, even more preferably 1.0 parts by mass to 3.0 parts by mass, and particularly preferably 1.5 parts by mass to 2.0 parts by mass. When the content of component (F) in the present composition per 100 parts by mass of component (A) is (a) 0.3 parts by mass or more, there is an advantage that the cured product obtained by curing the present composition at low temperatures has excellent T-peel adhesive strength, and when it is (b) 10.0 parts by mass or less, there is an advantage that the storage stability of the present composition is good.
[0171] The present composition may contain a curing agent other than components (C) and (F). For example, the present composition may contain a latent curing agent other than components (C) and (F). Examples of latent curing agents other than components (C) and (F) include N-containing curing agents such as certain amine-based curing agents (including imine-based curing agents). Examples of N-containing curing agents other than components (C) and (F) include boron trichloride / amine complexes, boron trifluoride / amine complexes, melamine, diallylmelamine, guanamine, aminotriazole, hydrazide, cyanoacetamide, imidazole, and aromatic polyamines.
[0172] In order to achieve a particularly excellent balance between the T-peel adhesive strength and storage stability of the cured product, the content of curing agents other than components (C) and (F) in the composition is preferably 5.0% by mass or less, more preferably 2.0% by mass or less, even more preferably 1.0% by mass or less, even more preferably 0.5% by mass or less, and particularly preferably 0% by mass to 0.5% by mass, based on 100% by mass of the composition. The content of curing agents other than components (C) and (F) in the composition may be 0% by mass, based on 100% by mass of the composition. In other words, the curing agent in the composition may be composed only of components (C) and (F).
[0173] <(G) Urea Compound> The present composition preferably further comprises a urea compound as component (G). The urea compound is preferably a substance (compound) that contains a urea bond in the molecule and can accelerate the curing of the composition. The urea compound can also be considered a curing accelerator.
[0174] The urea compound is represented by the general formula (1): 1 -NH-C(=O)-NR 2 2 ...(1) (wherein, R 1 is a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, and two R 2 are each independently a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms.
[0175] In this specification, amine adduct curing agents such as urea adduct curing agents are included in the component (F) but not in the component (G).
[0176] Examples of urea compounds include 3-(3,4-dichlorophenyl)-1,1-dimethylurea (e.g., Dyhard® UR200 manufactured by AlzChem), 3,3′-[methylenebis(4,1-phenylene)]bis(1,1-dimethylurea) (e.g., Omicure 52 manufactured by Huntsman), and 1,1′-(4-methyl-1,3-phenylene)bis(3,3-dimethylurea) (e.g., Dyhard® manufactured by AlzChem). Suitable examples of the methylurea include 4,4'-methylenebisphenyldimethylurea, p-chlorophenyl-N,N-dimethylurea (for example, trade name: Monoron), N-(3-chloro-4-methylphenyl)-N',N'-dimethylurea (for example, trade name: Chlortoluron), 1,1-dimethylphenylurea (for example, Dyhard (registered trademark) UR300 manufactured by AlzChem), and the like.
[0177] The urea compound preferably contains one or more selected from the group consisting of 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3,3'-[methylenebis(4,1-phenylene)]bis(1,1-dimethylurea), and 1,1'-(4-methyl-1,3-phenylene)bis(3,3-dimethylurea), more preferably 3-(3,4-dichlorophenyl)-1,1-dimethylurea and / or 3,3'-[methylenebis(4,1-phenylene)]bis(1,1-dimethylurea), and particularly preferably 3-(3,4-dichlorophenyl)-1,1-dimethylurea. This configuration has the advantage of providing an excellent balance between T-peel adhesion strength and storage stability of the cured product.
[0178] The urea compound preferably contains 70% by mass or more, more preferably 80% by mass or more, still more preferably 90% by mass or more, and particularly preferably 90% by mass to 100% by mass of one or more selected from the group consisting of 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3,3'-[methylenebis(4,1-phenylene)]bis(1,1-dimethylurea), and 1,1'-(4-methyl-1,3-phenylene)bis(3,3-dimethylurea) based on 100% by mass of the urea compound. The urea compound may contain 100% by mass of one or more compounds selected from the group consisting of 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3,3'-[methylenebis(4,1-phenylene)]bis(1,1-dimethylurea), and 1,1'-(4-methyl-1,3-phenylene)bis(3,3-dimethylurea) in 100% by mass of the urea compound; in other words, the urea compound may consist of only one or more compounds selected from the group consisting of 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3,3'-[methylenebis(4,1-phenylene)]bis(1,1-dimethylurea), and 1,1'-(4-methyl-1,3-phenylene)bis(3,3-dimethylurea). Furthermore, the urea compound may be composed solely of 3-(3,4-dichlorophenyl)-1,1-dimethylurea and / or 3,3'-[methylenebis(4,1-phenylene)]bis(1,1-dimethylurea), or may be composed solely of 3-(3,4-dichlorophenyl)-1,1-dimethylurea.
[0179] In the present composition, the content of component (G) per 100 parts by mass of component (A) is preferably 0.5 to 15.0 parts by mass, more preferably 0.7 to 13.0 parts by mass, more preferably 1.0 to 11.0 parts by mass, more preferably 2.0 to 10.0 parts by mass, even more preferably 3.0 to 9.0 parts by mass, even more preferably 4.0 to 7.0 parts by mass, and particularly preferably 5.0 to 6.0 parts by mass. When the content of component (G) in the present composition is (a) 0.5 parts by mass or more per 100 parts by mass of component (A), there is an advantage that the cured product obtained by curing the present composition at low temperatures has sufficient T-peel adhesive strength, and when it is (b) 15.0 parts by mass or less, there is an advantage that the storage stability of the present composition is good.
[0180] In the present composition, the total content of components (F) and (G) is preferably 0.8 parts by mass to 25.0 parts by mass, more preferably 1.0 parts by mass to 16.5 parts by mass, more preferably 2.0 parts by mass to 14.5 parts by mass, more preferably 3.0 parts by mass to 12.3 parts by mass, more preferably 4.0 parts by mass to 11.3 parts by mass, more preferably 5.0 parts by mass to 9.8 parts by mass, even more preferably 6.0 parts by mass to 8.3 parts by mass, and particularly preferably 7.0 parts by mass to 7.8 parts by mass, relative to 100 parts by mass of component (A). When the total content of components (F) and (G) in the present composition is (a) 0.8 parts by mass or more relative to 100 parts by mass of component (A), there is an advantage that the cured product obtained by curing the present composition at low temperatures has excellent T-peel adhesive strength, and when it is (b) 25.0 parts by mass or less, there is an advantage that the storage stability of the present composition is good. Through extensive research, the present inventors independently discovered that the storage stability of the composition is particularly good when the total amount of the components (F) and (G) in the composition is 7.8 parts by mass or less per 100 parts by mass of the component (A).
[0181] The present composition may contain a curing accelerator other than component (G). Examples of the curing accelerator other than component (G) include latent curing accelerators obtained by microencapsulating a curing accelerator such as tertiary amines, imidazoles, 6-caprolactam, and imidazoles or tertiary amines (e.g., Novacure (registered trademark) HX-3722, Novacure (registered trademark) HX-3742, and Novacure (registered trademark) HX-3088, manufactured by Asahi Kasei Corporation).
[0182] In order to achieve a particularly excellent balance between the T-peel adhesive strength and storage stability of the cured product, the content of curing accelerators other than component (G) in this composition is preferably 5.0% by mass or less, more preferably 2.0% by mass or less, even more preferably 1.0% by mass or less, even more preferably 0.5% by mass or less, and particularly preferably 0% by mass to 0.5% by mass, based on 100% by mass of the composition. The content of curing accelerators other than component (G) in this composition may be 0% by mass based on 100% by mass of the composition. In other words, the curing accelerator in this composition may consist solely of component (G).
[0183] The composition may contain water. To reduce the risk of a decrease in T-peel adhesive strength due to water evaporation during thermal curing, the water content in the composition is preferably as low as possible. For example, the water content is preferably 1 part by mass or less, more preferably 0.1 parts by mass or less, even more preferably 0.05 parts by mass or less, even more preferably 0.01 parts by mass or less, and particularly preferably 0 parts by mass to 0.01 parts by mass, per 100 parts by mass of component (A).
[0184] <Inorganic Filler> The present composition preferably contains an inorganic filler. When the present composition contains an inorganic filler, the obtained cured product has the effect of exhibiting superior rigidity at high temperatures.
[0185] Examples of inorganic fillers include silicic acid and / or silicates such as dry silica, wet silica, aluminum silicate, magnesium silicate, and calcium silicate; reinforcing fillers such as wollastonite, talc, dolomite, and carbon black; ground calcium carbonate; colloidal calcium carbonate; magnesium carbonate; titanium oxide; ferric oxide; fine aluminum powder; zinc oxide; and activated zinc oxide.
[0186] Among these, wollastonite is preferred because it has the advantage that the resulting cured product has excellent rigidity at high temperatures. Fumed silica and calcium carbonate are also preferred inorganic fillers. Of the above-mentioned inorganic fillers, one type may be used alone, or two or more types may be used in combination.
[0187] The dry silica is also called fumed silica, and includes hydrophilic fumed silica with no surface treatment and hydrophobic fumed silica produced by chemically treating the silanol group portion of hydrophilic fumed silica with silane or siloxane. As the fumed silica, hydrophobic fumed silica is preferred from the viewpoint of dispersibility in (A) epoxy resin.
[0188] The inorganic filler is preferably surface-treated with a surface treatment agent, which improves the dispersibility of the inorganic filler in the composition, thereby improving various physical properties of the resulting cured product.
[0189] The content of the inorganic filler in the composition is preferably 1 to 300 parts by mass, more preferably 5 to 200 parts by mass, and even more preferably 10 to 150 parts by mass, per 100 parts by mass of component (A). When the content of the inorganic filler is within the above range, the resulting cured product has the advantage of being even better in rigidity and T-peel adhesive strength at high temperatures.
[0190] In this specification, calcium oxide, which will be described later, is not included in the inorganic filler. In other words, when the present composition contains an inorganic filler and calcium oxide, the amount of calcium oxide is not included in the content of the inorganic filler.
[0191] <Calcium Oxide> The present composition preferably contains calcium oxide. When the present composition contains calcium oxide, calcium oxide reacts with moisture in the composition to remove moisture from the composition, thereby solving various problems with physical properties caused by the presence of moisture. For example, calcium oxide functions as a bubble inhibitor due to moisture removal, and can suppress a decrease in the T-peel adhesive strength of the resulting cured product.
[0192] Calcium oxide can be surface-treated with a surface treatment agent. The surface treatment improves the dispersibility of calcium oxide in the composition. As a result, the use of surface-treated calcium oxide has the advantage of improving the physical properties of the resulting cured product, such as the T-peel adhesive strength, compared to the use of calcium oxide that has not been surface-treated. The surface treatment agent is not particularly limited, but a fatty acid is preferred.
[0193] One type of calcium oxide may be used alone, or two or more types may be used in combination. Also, surface-treated calcium oxide and non-surface-treated calcium oxide may be used in combination.
[0194] The content of calcium oxide in the composition is preferably 0.1 to 10.0 parts by mass, more preferably 0.2 to 5.0 parts by mass, even more preferably 0.5 to 3.0 parts by mass, and particularly preferably 1.0 to 2.0 parts by mass, per 100 parts by mass of component (A). When the content of calcium oxide in the composition is 0.1 part by mass or more, the moisture removal effect is good, and when it is 10.0 parts by mass or less, the strength of the resulting cured product is high.
[0195] <Other Components> The composition may contain other components as necessary. Examples of other components include phenolic compounds, reinforcing agents, radical-curing resins, monoepoxides, photopolymerization initiators, expansion agents such as azo-type chemical foaming agents and thermally expandable microballoons, fiber pulp such as aramid pulp, colorants such as pigments and dyes, extender pigments, UV absorbers, antioxidants, stabilizers (antigelling agents), plasticizers, leveling agents, defoamers, silane coupling agents, antistatic agents, flame retardants, lubricants, viscosity reducers, low-shrinkage agents, organic fillers, thermoplastic resins, desiccants, and dispersants.
[0196] <Method for producing the composition> The method for producing the composition is not particularly limited, and various methods can be used. Hereinafter, the method for producing the composition will be described using an example in which the composition contains at least polymer particles as component (B).
[0197] First, a dispersion in which polymer particles, which are component (B), are dispersed in component (A) can be obtained by the following methods: a method in which polymer particles obtained in an aqueous latex state are brought into contact with component (A) and then unnecessary components such as water are removed, a method in which the polymer particles are once extracted with an organic solvent and then mixed with component (A), and then the organic solvent is removed, etc. Specifically, the method described in WO 2005 / 028546 is preferably used as a production method for obtaining such a dispersion. More specifically, the dispersion is preferably prepared by a production method including the following first to third steps in order: a first step of mixing an aqueous latex containing polymer particles (specifically, a reaction mixture obtained after producing polymer particles by emulsion polymerization) with an organic solvent having a solubility in water of 5% by mass to 40% by mass at 20°C, and then mixing the resulting mixture with excess water to aggregate the polymer particles; a second step of separating and recovering the aggregated polymer particles from the liquid phase, and then mixing them again with an organic solvent to obtain an organic solvent dispersion of polymer particles; and a third step of mixing the organic solvent dispersion of polymer particles with component (A), and then distilling off the organic solvent from the resulting mixture.
[0198] Component (A) is preferably liquid at 23°C, as this facilitates the third step. "Liquid at 23°C" means that the softening point is 23°C or lower and that the component is fluid at 23°C.
[0199] The present composition can also be produced by methods other than those including the above steps (Steps 1 to 3). For example, there is a method using powdery polymer particles as component (B). Specifically, an aqueous latex containing polymer particles is first used to coagulate the polymer particles by a method such as salting out, and the resulting coagulate is then dried. This produces powdery polymer particles. The powdery polymer particles can be redispersed in component (A) by subjecting a mixture containing the powdery polymer particles and component (A) to a dispersing machine with high mechanical shear force, such as a triple paint roll, roll mill, or kneader. In this way, a polymer particle-containing composition can also be produced using powdery polymer particles as component (B). In this case, the polymer particles can be efficiently dispersed in component (A) by applying mechanical shear force at high temperature to the mixture of polymer particles (components (A) and (B)). The temperature during dispersion (the temperature at which shear force is applied) is preferably 50° C. to 200° C., more preferably 70° C. to 170° C., even more preferably 80° C. to 150° C., and particularly preferably 90° C. to 120° C. When the temperature during dispersion is (a) 50° C. or higher, the polymer particles of component (B) can be sufficiently dispersed in component (A), and when the temperature is (b) 200° C. or lower, there is no risk of thermal degradation of the polymer particles of components (A) and (B).
[0200] The present composition can be obtained by mixing the dispersion of component (B) polymer particles dispersed in the state of primary particles in component (A) obtained through steps 1 to 3 above with components (C) and (D), and, if necessary, additional components (A), (B) blocked urethane, (E), (F), (G), inorganic filler, calcium oxide, and other components. Furthermore, this production method can obtain the present composition in which the polymer particles are dispersed in the state of primary particles. When the present composition contains polymer particles as component (B) and the polymer particles are dispersed in the composition in the state of primary particles, the resulting cured product has the advantage of having even better T-peel adhesion strength.
[0201] When the composition contains component (F), a preferred method for producing the composition includes mixing all components except component (F) and then adding component (F) last. For example, a one-component thermosetting resin composition can be obtained by mixing components (C) and (D), as well as additional components (A), (B) blocked urethane, (E), (G), inorganic filler, calcium oxide, and other components, with a dispersion of component (B) in the form of primary particles obtained through steps 1 to 3 described above. The resulting mixture is then mixed with component (F) to obtain a one-component thermosetting resin composition. The amine adduct curing agent (F) has a low softening temperature. Furthermore, high-viscosity structural adhesives are prone to temperature increases due to shear heat during mixing in a mixer. Therefore, adding component (F) last minimizes shear heat during mixing, which tends to improve the storage stability of the resulting composition.
[0202] [Cured Product] In one embodiment of the present invention, a cured product is provided by curing the present composition. In this specification, the "cured product according to one embodiment of the present invention" may be referred to as the "present cured product."
[0203] The present cured product has the above-mentioned structure and therefore has the advantage of excellent T-peel adhesive strength.
[0204] [Others] <Application Method> The present composition can be applied to a substrate by any method. According to a preferred embodiment, it can be applied at low temperatures around room temperature (e.g., 5°C to 40°C), and can also be applied after heating (e.g., 45°C to 80°C) as needed. The present composition has excellent storage stability and is therefore particularly useful for application methods in which it is heated.
[0205] The two substrates can be joined by applying the present composition to one or both of the substrates, bringing the substrates into contact with each other so that the present composition is disposed between the two substrates, and then curing the present composition in that state.
[0206] When the curable resin composition is used as a structural adhesive for joining structural members of a vehicle or the like, the joining can be strengthened by applying spot welding as appropriate after the application of the curable resin composition as a weld bond method.
[0207] [Adhesive] In one embodiment of the present invention, an adhesive containing the present composition is provided. An adhesive containing the present composition has the advantage of being able to provide a cured product (adhesive layer) with excellent T-peel adhesive strength by low-temperature curing. Furthermore, an adhesive containing the present composition also has the advantage of excellent storage stability. When the present composition is used as an adhesive to bond various substrates, for example, substrates such as wood, metal, plastic, and glass can be bonded. Bonding of automobile parts is preferred, and bonding of automobile frames to each other or bonding of an automobile frame to other automobile parts is more preferred. Examples of substrates include various plastic substrates, such as steel materials such as cold-rolled steel and hot-dip galvanized steel, aluminum materials such as aluminum and coated aluminum, general-purpose plastics, engineering plastics, and composite materials such as CFRP and GFRP. The present curable resin composition may be used alone as an adhesive, or, if necessary, a mixture of the present composition and other components may be used as an adhesive.
[0208] The adhesive according to one embodiment of the present invention is applied to one or both of two substrates, the two substrates are brought into contact with each other so that the adhesive is disposed between the two substrates, and the adhesive is then cured, thereby bonding the two substrates together with the resulting cured product (adhesive layer). That is, in one embodiment of the present invention, there is provided a laminate comprising at least two substrates and an adhesive layer formed by curing the adhesive according to one embodiment of the present invention, which bonds the at least two substrates together.
[0209] A laminate according to one embodiment of the present invention can also be expressed as follows: A laminate comprising two substrates and an adhesive layer formed between the two substrates by curing an adhesive according to one embodiment of the present invention.
[0210] The laminate according to one embodiment of the present invention can also be expressed as follows: A laminate formed by laminating a first substrate, a cured product obtained by curing an adhesive according to one embodiment of the present invention, and a second substrate in this order.
[0211] The present composition has excellent T-peel adhesive strength, and therefore a laminate obtained by sandwiching the present composition between at least two substrates, laminating them together, and then curing the composition to bond the resulting member is preferred because it exhibits excellent T-peel adhesive strength.
[0212] In recent years, there has been a trend toward the widespread use of aluminum materials as substrates for automobile parts in order to reduce weight. At least one of the two substrates is preferably an aluminum material. Both of the two substrates may be aluminum materials. Aluminum materials and steel materials have significantly different linear expansion coefficients. Generally, when bonding dissimilar substrates having significantly different linear expansion coefficients with an adhesive, the bonded portion may be significantly distorted when the adhesive is cured at high temperatures (e.g., 170°C to 190°C) and then cooled to room temperature. The present composition can be cured at low temperatures (e.g., 120°C to 140°C) and has excellent toughness. Therefore, as described above, even when bonding dissimilar substrates having different linear expansion coefficients, bonding them using an adhesive according to one embodiment of the present invention has the advantage of improving the distortion of the bonded portion. In other words, when at least two substrates have different linear expansion coefficients (e.g., the difference in linear expansion coefficients is 5×10 or more), the adhesive can be cured at low temperatures (e.g., 120°C to 140°C). -6 It is preferable that the temperature is at least two substrates (temperature is 100°C or higher).
[0213] The compositions can also be used to join aerospace components, particularly exterior metal components.
[0214] <Curing Temperature> The curing temperature of the present composition (for example, the curing temperature of the composition when producing the laminate) is not particularly limited as long as it is 100°C or higher, but is preferably low, for example, preferably 115°C to 145°C, more preferably 117°C to 140°C, even more preferably 118°C to 135°C, and particularly preferably 120°C to 130°C. A curing temperature of 145°C or lower can be said to be a "low temperature." In other words, a curing temperature of 145°C or lower can be said to be low-temperature curing.
[0215] <Curing Time> The curing time of the present composition (for example, the curing time of the composition when producing the laminate) is preferably 10 to 60 minutes, more preferably 12 to 40 minutes, even more preferably 13 to 30 minutes, and particularly preferably 15 to 25 minutes.
[0216] In other words, the method for producing a laminate according to one embodiment of the present invention preferably includes a step of curing the one-component thermosetting resin composition at a curing temperature of 115°C to 145°C for a curing time of 10 minutes to 60 minutes.
[0217] When the present composition is used as an automotive adhesive, it is preferable from the viewpoint of shortening and simplifying the process to apply the adhesive to an automotive part, then apply a coating such as electrodeposition coating, and bake and cure the coating while curing the adhesive at the same time.
[0218] <Applications> The composition is preferably used in applications such as adhesives, such as structural adhesives for vehicles and aircraft, and structural adhesives for wind power generation; paints; lamination materials with glass fibers; materials for printed wiring boards; solder resists; interlayer insulating films; build-up materials; adhesives for FPCs; electrical insulating materials, such as encapsulants for electronic components, such as semiconductors and LEDs; die bond materials; underfills; semiconductor mounting materials, such as ACF, ACP, NCF, and NCP; and encapsulants for display devices and lighting devices, such as liquid crystal panels, OLED lighting, and OLED displays.
[0219] An embodiment of the present invention may have the following configuration.
[0220] [1] A one-component thermosetting resin composition comprising: (A) an epoxy resin; (B) one or more polymer particles having a core-shell structure comprising a core layer and a shell layer, a blocked urethane, a rubber-modified epoxy resin, and a urethane-modified epoxy resin; (C) dicyandiamide; and (D) a monocarboxylic acid and / or a monocarboxylic acid metal salt, wherein, relative to 100 parts by mass of the component (A), (a) the content of the component (B) is 1 part by mass to 100 parts by mass, (b) the content of the component (C) is 3.5 parts by mass to 19.0 parts by mass, and (c) the content of the component (D) is 0.01 parts by mass to 30.00 parts by mass.
[0221] [2] The one-component thermosetting resin composition according to [1], wherein the component (A) contains a difunctional bisphenol A type epoxy resin and / or a difunctional bisphenol F type epoxy resin.
[0222] [3] The one-component thermosetting resin composition according to [2], wherein the total content of the difunctional bisphenol A epoxy resin and the difunctional bisphenol F epoxy resin is 60 mass% or more in 100 mass% of the component (A).
[0223] [4] In the component (D), the molecular weight of the monocarboxylic acid is 60 to 700, and the molecular weight of the monocarboxylic acid metal salt is 60 to 2000. [1] The one-component thermosetting resin composition according to any one of [1] to [3].
[0224] [5] The one-component thermosetting resin composition according to any one of [1] to [4], wherein the ratio of the molar amount of the component (D) to twice the molar amount of the component (C) (the molar amount of the component (D) / twice the molar amount of the component (C)) is 0.001 to 0.400. [6] The one-component thermosetting resin composition according to any one of [1] to [5], wherein the melting point of the component (D) is 60°C or higher.
[0225] [7] The one-component thermosetting resin composition according to any one of [1] to [6], wherein in the component (D), the monocarboxylic acid metal salt includes a fatty acid metal salt.
[0226] [8] The one-component thermosetting resin composition according to any one of [1] to [7], wherein in the component (D), the monocarboxylic acid includes a fatty acid.
[0227] [9] In the component (D), the monocarboxylic acid contains an α,β-unsaturated carboxylic acid, and the content of the α,β-unsaturated carboxylic acid in 100% by mass of the monocarboxylic acid is more than 0% by mass and 0.10% by mass or less.
[10] The one-component thermosetting resin composition according to any one of [1] to [8].
[0228]
[10] The one-component thermosetting resin composition according to any one of [1] to [8], wherein in the component (D), the monocarboxylic acid does not contain an α,β-unsaturated carboxylic acid.
[0229]
[11] The one-component thermosetting resin composition according to any one of [1] to
[10] , wherein the component (D) contains a monocarboxylic acid metal salt.
[0230]
[12] The one-component thermosetting resin composition according to
[11] , wherein the metal salt of monocarboxylic acid includes one or more metal salts selected from the group consisting of divalent tin salts, magnesium salts, iron salts, titanium salts, and aluminum salts of monocarboxylic acids.
[0231]
[13] The one-component thermosetting resin composition according to any one of [1] to [7], wherein the component (D) is composed solely of a monocarboxylic acid metal salt.
[0232]
[14] The one-component thermosetting resin composition according to
[13] , wherein the metal salt of monocarboxylic acid includes one or more metal salts selected from the group consisting of divalent tin salts, magnesium salts, iron salts, titanium salts, and aluminum salts of monocarboxylic acids.
[0233]
[15] The one-component thermosetting resin composition according to any one of [1] to
[14] , further comprising a monocarboxylic acid-amine complex, and the content of the monocarboxylic acid-amine complex is more than 0 parts by mass and not more than 0.10 parts by mass per 100 parts by mass of the component (A).
[0234]
[16] The one-component thermosetting resin composition according to any one of [1] to
[14] , wherein the one-component thermosetting resin composition does not contain a monocarboxylic acid-amine complex.
[0235]
[17] The one-component thermosetting resin composition according to any one of [1] to
[16] , further comprising (E) an epoxy-based reactive diluent, and the content of the component (E) is 1.0 parts by mass to 20.0 parts by mass per 100 parts by mass of the component (A).
[0236]
[18] The one-component thermosetting resin composition according to any one of [1] to
[17] , further comprising (F) an amine adduct curing agent that is solid at room temperature, and the content of the component (F) is 0.3 parts by mass to 10.0 parts by mass per 100 parts by mass of the component (A).
[0237]
[19] The one-component thermosetting resin composition according to any one of [1] to
[18] , further comprising a urea compound (G), and the content of the component (G) is 0.5 parts by mass to 15.0 parts by mass per 100 parts by mass of the component (A).
[0238]
[20] The one-component thermosetting resin composition according to any one of [1] to
[19] , wherein the content of the component (A) is 60% by mass or more in 100% by mass of the total amount of the components (A) to (G).
[0239]
[21] The one-component thermosetting resin composition according to any one of [1] to
[20] , wherein the water content is 1 part by mass or less per 100 parts by mass of the component (A).
[0240]
[22] A cured product obtained by curing the one-component thermosetting resin composition according to any one of [1] to
[21] .
[0241]
[23] An adhesive comprising the one-component thermosetting resin composition according to any one of [1] to
[21] .
[0242]
[24] A laminate comprising two substrates and an adhesive layer formed between the two substrates by curing the adhesive according to
[23] .
[0243] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited thereto. One embodiment of the present invention can be carried out by appropriately modifying the following examples within the scope that can comply with the above-mentioned and below-mentioned aims. All embodiments carried out by appropriately modifying the following examples are included within the technical scope of the present invention. In the following examples, comparative examples, and tables, "parts" and "%" mean parts by mass and % by mass, respectively.
[0244] [Materials] First, the materials used in the examples and comparative examples are listed below.
[0245] <Component (A)> A-1: JER828 (manufactured by Mitsubishi Chemical Corporation, a bifunctional bisphenol A epoxy resin (BisA epoxy resin) that is liquid at room temperature, epoxy equivalent: 184 g / eq to 194 g / eq) A-2: JER1001 (manufactured by Mitsubishi Chemical Corporation, a bifunctional bisphenol A epoxy resin (BisA epoxy resin) that is solid at room temperature, epoxy equivalent: 450 g / eq to 500 g / eq) <Component (B)> (Polymer Particles) As the polymer particles of component (B), polymer particles prepared by the following method were used. As described below, dispersions (M-1 to M-2) in which the prepared component (B) (polymer particles) was dispersed in component (A-1) were prepared and used in the examples.
[0246] 1. Formation of Core Layer Production Example 1-1: Preparation of Polybutadiene Rubber Latex (R-1) Into a 100 L pressure-resistant polymerization reactor, 200 parts by mass of deionized water, 0.03 parts by mass of tripotassium phosphate, 0.25 parts by mass of potassium dihydrogen phosphate, 0.002 parts by mass of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts by mass of ferrous sulfate heptahydrate (FE), and 1.5 parts by mass of sodium dodecylbenzenesulfonate (SDS) as an emulsifier were charged. Next, the gas inside the pressure-resistant polymerization reactor was replaced with nitrogen while stirring the charged raw materials, thereby thoroughly removing oxygen from inside the pressure-resistant polymerization reactor. Thereafter, 100 parts by mass of butadiene (BD) was charged into the pressure-resistant polymerization reactor, and the temperature inside the pressure-resistant polymerization reactor was raised to 45 ° C. Next, 0.015 parts by mass of paramenthane hydroperoxide (PHP) was charged into the pressure-resistant polymerization reactor, followed by 0.04 parts by mass of sodium formaldehyde sulfoxylate (SFS) to initiate polymerization. Ten hours after the start of polymerization, the polymerization was terminated by devolatilization under reduced pressure to remove remaining monomers that had not been used in the polymerization. During the polymerization, PHP, EDTA, and FE were each added to the pressure-resistant polymerization reactor in desired amounts and at desired times. This polymerization procedure yielded a latex (R-1) containing a core layer (polybutadiene rubber particles) primarily composed of polybutadiene rubber. The volume average particle diameter of the polybutadiene rubber particles contained in the resulting latex was 0.10 μm.
[0247] Production Example 1-2: Preparation of Polybutadiene Rubber Latex (R-2) 21 parts by mass of the polybutadiene rubber latex (R-1) obtained in Production Example 1-1 (containing 7 parts by mass of polybutadiene rubber particles), 200 parts by mass of deionized water, 0.03 parts by mass of tripotassium phosphate, 0.002 parts by mass of EDTA, and 0.001 parts by mass of FE were charged into a 100 L pressure-resistant polymerization reactor. Next, the gas inside the pressure-resistant polymerization reactor was replaced with nitrogen while stirring the charged raw materials, thereby thoroughly removing oxygen from inside the pressure-resistant polymerization reactor. Thereafter, 93 parts by mass of BD were charged into the pressure-resistant polymerization reactor, and the temperature inside the pressure-resistant polymerization reactor was raised to 45°C. Next, 0.02 parts by mass of PHP was charged into the pressure-resistant polymerization reactor, followed by 0.10 parts by mass of SFS, to initiate polymerization. Thirty hours after the start of polymerization, volatilization was carried out under reduced pressure to remove remaining monomers that were not used in the polymerization, thereby terminating the polymerization. During the polymerization, PHP, EDTA, and FE were each added to the pressure-resistant polymerization reactor in desired amounts and at desired times. This polymerization procedure yielded a latex (R-2) containing a core layer (polybutadiene rubber particles) composed primarily of polybutadiene rubber. The volume average particle diameter of the polybutadiene rubber particles contained in the obtained latex was 0.20 μm.
[0248] 2. Preparation of Polymer Particles Having a Core-Shell Structure (Formation of Shell Layer) Production Example 2-1: Preparation of Aqueous Latex (L-1) Containing Polymer Particles 262 parts by mass of the polybutadiene rubber latex (R-2) prepared in Production Example 1-2 (containing 87 parts by mass of polybutadiene rubber particles) and 57 parts by mass of deionized water were charged into a glass reactor. The glass reactor was equipped with a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device. The gas in the glass reactor was replaced with nitrogen, and the charged raw materials were stirred at 60°C while the nitrogen replacement was being carried out. Next, 0.004 parts by mass of EDTA, 0.001 parts by mass of FE, and 0.2 parts by mass of SFS were added to the glass reactor. Thereafter, a mixture of shell layer-forming monomers (8 parts by mass of methyl acrylate (MA), 3.5 parts by mass of butyl acrylate (BA), and 1.5 parts by mass of glycidyl methacrylate (GMA)) and 0.04 parts by mass of cumene hydroperoxide (CHP) was continuously added to the glass reactor over a period of 120 minutes. After completion of the addition, 0.04 parts by mass of CHP was added to the glass reactor, and the mixture in the glass reactor was continuously stirred for an additional 2 hours to complete the polymerization. Through the above operations, an aqueous latex (L-1) containing polymer particles having a core-shell structure was obtained. The polymerization conversion rate of the monomer components was 99% or more. The volume average particle diameter of the polymer particles contained in the obtained aqueous latex (L-1) was 0.21 μm.
[0249] Production Example 2-2: Preparation of aqueous latex (L-2) containing polymer particles
[0063] An aqueous latex (L-2) containing polymer particles having a core-shell structure was obtained in the same manner as in Production Example 2-1, except that <6 parts by mass of styrene (ST), 1 part by mass of methyl methacrylate (MMA), 2 parts by mass of acrylonitrile (AN), and 4 parts by mass of GMA> were used instead of <8 parts by mass of MA, 3.5 parts by mass of BA, and 1.5 parts by mass of GMA> as the shell layer-forming monomers in Production Example 2-1. The volume average particle diameter of the polymer particles contained in the obtained aqueous latex was 0.21 μm.
[0250] 3. (A) Preparation of Dispersion (M) in which Polymer Particles are Dispersed in Epoxy Resin Production Example 3-1: Preparation of Dispersion (M-1) 132 g of methyl ethyl ketone (MEK) was introduced into a 1 L mixing tank at 25°C. Next, while stirring the MEK, 132 g of the aqueous latex (L-1) containing polymer particles obtained in Production Example 2-1 (containing 40 g of polymer particles) was added to the mixing tank. After the raw materials in the mixing tank were uniformly mixed, 200 g of water was added to the mixing tank at a feed rate of 80 g / min while stirring the raw materials in the mixing tank. After the water supply was completed, stirring was promptly stopped to obtain a slurry liquid consisting of aggregates containing polymer particles and an aqueous phase containing a small amount of organic solvent. The aggregates were floatable. Next, 360 g of the aqueous phase was discharged from a discharge port at the bottom of the mixing tank, leaving a portion of the aggregates containing the aqueous phase in the mixing tank. 90 g of MEK was added to the obtained aggregates and mixed uniformly to obtain a dispersion in which polymer particles were uniformly dispersed in MEK. 60 g of epoxy resin (A-1), component (A), was added to the obtained dispersion and mixed uniformly. The epoxy resin (A-1) is described in detail below. MEK was removed from the obtained mixture using a rotary evaporator. In this way, a dispersion (M-1) in which polymer particles were dispersed in epoxy resin (A) was obtained.
[0251] Production Example 3-2: Preparation of Dispersion (M-2) A dispersion (M-2) in which polymer particles were dispersed in epoxy resin (A) was obtained in the same manner as in Production Example 3-1, except that 132 g of (L-2) (containing 40 g of polymer particles) was used instead of 132 g of (L-1) as the aqueous latex containing polymer particles in Production Example 3-1.
[0252] The following were used as component (B) other than the polymer particles: (Urethane-modified epoxy resin) B-1: EPU-73B (manufactured by ADEKA, urethane-modified epoxy resin, epoxy equivalent: 245 g / eq) (Blocked urethane) B-2: Flexibilizer DY 965 (manufactured by Huntsman, blocked urethane containing a polytetramethylene glycol structure, GPC (apparatus: Tosoh HLC-8420, column: Tosoh TSKgel Super HZ column, mobile phase: THF, column temperature: 40°C, flow rate: 0.35 ml / min, injection volume: 10 μL, detector: differential refractometer) polystyrene-equivalent number average molecular weight (Mn): 11,800, molecular weight distribution (Mw / Mn): 2.1) (Rubber-modified epoxy resin) B-3: Hypox RA 1340 (manufactured by Huntsman, rubber-modified epoxy resin, epoxy equivalent: 325 g / eq to 375 g / eq).
[0253] <Component (C)> Dyhard (registered trademark) 100S (manufactured by AlzChem, dicyandiamide) <Component (D)> TFA-140F (manufactured by Tsuno Foods Industries, a fatty acid mixture that is liquid at 25°C and contains oleic acid (51% by weight), linoleic acid (36% by weight), and linolenic acid (8% by weight), and has a melting point of less than 25°C) NAA-173K powder (manufactured by NOF Corporation, a fatty acid mixture that contains stearic acid (93% by weight) and palmitic acid (6% by weight), and has a melting point of 65°C to 69°C) NAA-222K powder (manufactured by NOF Corporation, a fatty acid mixture that contains behenic acid (85% by weight), saturated fatty acids having 16 to 20 carbon atoms (13% by weight), and lignoceric acid (2% by weight), and has a melting point of 74°C to 78°C) Neostan U-28 (manufactured by Nitto Kasei, 2-ethylhexanoic acid tin (II), liquid at 25°C, melting point below 25°C) Magnesium Stearate GP (manufactured by NOF Corp., magnesium stearate, melting point 120°C to 140°C) Aluminum Stearate 900 (manufactured by NOF Corp., aluminum tristearate, melting point 110°C to 125°C) Aluminum Stearate 300 (manufactured by NOF Corp., aluminum monostearate, melting point 150°C to 165°C)) <Component (E)> Cardura (registered trademark) E10P (manufactured by Hexion, neodecanoic acid glycidyl ester) ERISYS (registered trademark) GE-10 (manufactured by Huntsman, o-cresyl glycidyl ether) <Component (F)> Ajicure PN-40 (manufactured by Ajinomoto Fine-Techno, amine-epoxy adduct curing agent (imidazole group-containing modified polyamine), softening temperature: 108°C, particle size: 11.6 μm) <Component (G)> Dyhard (registered trademark) UR200 (manufactured by AlzChem, 3-(3,4-dichlorophenyl)-1,1-dimethylurea) <Other components> (Phenol compound) IRGANOX (registered trademark) 245 (manufactured by BASF Japan, bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylenebis(oxyethylene)]) (fumed silica) CAB-O-SIL TS-720 (manufactured by CABOT, fumed silica surface-treated with polydimethylsiloxane) (referred to as "TS-720" in the table), (wollastonite) NYAD 400 (manufactured by NYCO Minerals, untreated wollastonite) (calcium carbonate) Whiten SB (manufactured by Shiraishi Calcium, untreated heavy calcium carbonate) (calcium oxide) CML#31 (manufactured by Omi Chemical Industry, calcium oxide surface-treated with fatty acid).
[0254] (Silane Coupling Agent) DOWSIL (registered trademark) SH 6040 Silane (manufactured by Dow, 3-glycidoxypropyltrimethoxysilane).
[0255] [Measurement and Evaluation Methods] The measurement and evaluation methods for each physical property measured in the examples are shown below.
[0256] [Measurement of Volume Average Particle Diameter] The volume average particle diameter (Mv) of the polymer particles (B) dispersed in the aqueous latex was measured using a Microtrac UPA150 (manufactured by Nikkiso Co., Ltd.). A sample prepared by diluting the aqueous latex with deionized water was used. The measurement was performed by inputting the refractive index of water and the refractive index of each polymer particle, adjusting the sample concentration so that the measurement time was 600 seconds, and the signal level was within the range of 0.6 to 0.8.
[0257] [Measurement of Water Content in Composition] The water content in the composition was measured using a Karl Fischer moisture meter (MK-II, manufactured by Kyoto Electronics Manufacturing Co., Ltd.).
[0258] [Measurement of T-Peel Adhesion Strength] The T-peel adhesion strength of the cured composition was measured as follows: The composition was applied to two cold-rolled steel plates (SPCC steel plates) measuring 25 mm wide x 200 mm long x 0.5 mm thick, and the two cold-rolled steel plates were then stacked together to form an adhesive layer thickness of 0.25 mm. The compositions in Tables 1 to 3 (Examples 1 to 15, Comparative Examples 1 to 4) were then cured (low-temperature cured) at a curing temperature of 120°C for 20 minutes to obtain a laminate in which the two steel plates were bonded together. The compositions in Table 4 (Examples 16 to 18, Comparative Examples 5 and 6) were cured (low-temperature cured) at a curing temperature of 140°C for 20 minutes to obtain a laminate in which the two steel plates were bonded together. These laminates can be said to be laminates including two steel plates (substrates) and an adhesive layer formed between the two steel plates by curing an adhesive containing the composition. The resulting laminates were used as samples to measure T-peel adhesive strength (N / 25 mm) according to JIS K6854. The measurement conditions were a measurement temperature of 23°C and a test speed of 254 mm / min.
[0259] [Measurement of Viscosity Increase Rate (Storage Stability)] The viscosity increase rate of the composition was measured by the following methods (1) to (4): (1) The viscosity of the composition at 50°C was measured using a rheometer at a shear rate of 5 s -1 (2) The composition was then stored (left to stand) at 40°C for 7 days; (3) After storage, the viscosity of the composition at 50°C was measured using a rheometer at a shear rate of 5 s -1 (4) Subsequently, the ratio of the viscosity of the composition before storage to the viscosity of the composition after storage (viscosity of the composition after storage / viscosity of the composition before storage) was calculated, and the obtained value was taken as the viscosity increase rate. The closer the viscosity increase rate is to 1, the more excellent the storage stability is intended to be.
[0260] (Examples 1 to 18, Comparative Examples 1 to 6) One-component thermosetting resin compositions were obtained by weighing each component and thoroughly mixing them to obtain the formulations shown in Tables 1 to 4. In all of Examples 1 to 18 and Comparative Examples 1 to 6, the water content in the resulting composition was 0.1 parts by mass or less per 100 parts by mass of component (A). The T-peel adhesive strength and viscosity increase rate of the resulting compositions were measured and evaluated according to the methods described above. The results are shown in Tables 1 to 4.
[0261] According to one embodiment of the present invention, it is possible to provide a one-component thermosetting resin composition that can provide a cured product having excellent T-peel adhesive strength even when cured at low temperatures. Therefore, this embodiment of the present invention can be suitably used as an adhesive, particularly as a structural adhesive for vehicles.
Claims
1. A one-component thermosetting resin composition comprising: (A) an epoxy resin; (B) one or more selected from the group consisting of polymer particles having a core-shell structure including a core layer and a shell layer, blocked urethane, a rubber-modified epoxy resin, and a urethane-modified epoxy resin; (C) dicyandiamide; and (D) a monocarboxylic acid and / or a monocarboxylic acid metal salt, wherein, relative to 100 parts by mass of the component (A), (a) the content of the component (B) is 1 part by mass to 100 parts by mass; (b) the content of the component (C) is 3.5 parts by mass to 19.0 parts by mass; and (c) the content of the component (D) is 0.01 parts by mass to 30.00 parts by mass.
2. The one-component thermosetting resin composition according to claim 1, wherein the component (A) contains a difunctional bisphenol A type epoxy resin and / or a difunctional bisphenol F type epoxy resin.
3. A one-component thermosetting resin composition as described in claim 2, wherein the total content of the difunctional bisphenol A type epoxy resin and the difunctional bisphenol F type epoxy resin is 60 mass% or more in 100 mass% of the (A) component.
4. The one-component thermosetting resin composition according to claim 1, wherein in component (D), the molecular weight of the monocarboxylic acid is 60 to 700, and the molecular weight of the monocarboxylic acid metal salt is 60 to 2,000.
5. The one-component thermosetting resin composition according to claim 1, wherein the ratio of the molar amount of the (D) component to twice the molar amount of the (C) component (the molar amount of the (D) component / the molar amount of the (C) component) is 0.001 to 0.
400.
6. The one-component thermosetting resin composition according to claim 1, wherein the melting point of component (D) is 60°C or higher.
7. The one-component thermosetting resin composition according to claim 1, wherein in component (D), the monocarboxylic acid metal salt includes a fatty acid metal salt.
8. The one-component thermosetting resin composition according to claim 1, wherein in component (D), the monocarboxylic acid comprises a fatty acid.
9. The one-component thermosetting resin composition according to claim 1, wherein in the component (D), the monocarboxylic acid contains an α,β-unsaturated carboxylic acid, and the content of the α,β-unsaturated carboxylic acid in 100% by mass of the monocarboxylic acid is greater than 0% by mass and 0.10% by mass or less.
10. The one-component thermosetting resin composition according to claim 1, wherein in component (D), the monocarboxylic acid does not contain an α,β-unsaturated carboxylic acid.
11. The one-component thermosetting resin composition according to claim 1, wherein the component (D) comprises a metal salt of a monocarboxylate.
12. The one-component thermosetting resin composition according to claim 11, wherein the metal salt of a monocarboxylic acid comprises one or more metal salts selected from the group consisting of divalent tin salts, magnesium salts, iron salts, titanium salts and aluminum salts of a monocarboxylic acid.
13. The one-component thermosetting resin composition according to claim 1, wherein the component (D) consists solely of a monocarboxylic acid metal salt.
14. The one-component thermosetting resin composition according to claim 13, wherein the metal salt of a monocarboxylic acid comprises one or more metal salts selected from the group consisting of divalent tin salts, magnesium salts, iron salts, titanium salts and aluminum salts of a monocarboxylic acid.
15. The one-component thermosetting resin composition according to claim 1, further comprising a monocarboxylic acid-amine complex, and the content of the monocarboxylic acid-amine complex per 100 parts by mass of component (A) is more than 0 parts by mass and not more than 0.10 parts by mass.
16. The one-component thermosetting resin composition according to claim 1, wherein the one-component thermosetting resin composition does not contain a monocarboxylic acid-amine complex.
17. The one-component thermosetting resin composition according to claim 1, further comprising (E) an epoxy-based reactive diluent, and the content of the component (E) is 1.0 part by mass to 20.0 parts by mass per 100 parts by mass of the component (A).
18. The one-component thermosetting resin composition according to claim 1, further comprising (F) an amine adduct curing agent that is solid at room temperature, and the content of the component (F) is 0.3 parts by mass to 10.0 parts by mass per 100 parts by mass of the component (A).
19. The one-component thermosetting resin composition according to claim 1, further comprising a urea compound (G), and the content of the component (G) is 0.5 parts by mass to 15.0 parts by mass per 100 parts by mass of the component (A).
20. A one-component thermosetting resin composition according to claim 1, wherein the content of component (A) is 60 mass% or more out of a total of 100 mass% of components (A) to (G).
21. The one-component thermosetting resin composition according to claim 1, wherein the water content is 1 part by mass or less per 100 parts by mass of the component (A).
22. A cured product obtained by curing the one-component thermosetting resin composition according to any one of claims 1 to 21.
23. An adhesive comprising the one-component thermosetting resin composition according to any one of claims 1 to 21.
24. A laminate comprising two substrates and an adhesive layer formed by curing the adhesive according to claim 23 between the two substrates.
Citation Information
Patent Citations
Single-component epoxy adhesive for automobile manufacturing
CN112358839A
Self-adhesive structural adhesive tape and preparation method thereof
CN115216230A
Structural adhesive sheet used in the mirror base of an automobile inner rearview mirror and method for manufacturing the same
JP2014532801A
Polymer fine particle-containing curable resin composition improved in peel adhesion and impact-resistant peel adhesion