Na2mnfe(CN)6-carbon nanotube composite positive electrode material composition for secondary battery

The integration of carbon nanotubes into the cathode material composition for sodium ion batteries addresses the limitations of Prussian blue-based batteries by enhancing conductivity and yield, resulting in improved electrochemical performance.

WO2024248184A1PCT designated stage expired Publication Date: 2024-12-05ENERGY11 CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/007540
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Prussian blue-based sodium ion batteries face issues with low electrical conductivity, reduced charging and discharging efficiency, and limited solubility due to the common ion effect of NaCl, leading to poor manufacturing yield and component homogeneity.

Method used

A carbon nanotube composite cathode material composition is developed by mixing carbon nanotubes with the initial mixture of NaCl and MnCl aqueous solutions, followed by a secondary mixing process with Na4Fe(CN)6, enhancing the distribution and conductivity of the cathode material, with a preferred component ratio of MnCl2:NaCl:Na4Fe(CN)6 = 2:2.5:1, and using a pneumatic aerosol sprayer for improved mixing.

Benefits of technology

The approach increases the yield and homogeneity of the cathode material, significantly improving electrical conductivity and the overall quality of secondary batteries, resulting in enhanced charging and discharging efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023007540_05122024_PF_FP_ABST
    Figure KR2023007540_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a Na2MnFe(CN)6-carbon nanotube composite positive electrode material composition for a secondary battery. According to the present invention, the yield of a positive electrode material used in a Prussian blue-based sodium ion battery can be improved by changing a process sequence when manufacturing same. Additionally, by adding carbon nanotubes to a primary solution, the components of particles are not only mixed more uniformly, but electrical conductivity is also improved such that a secondary battery with improved charge / discharge efficiency and quality may be provided.
Need to check novelty before this filing date? Find Prior Art

Description

NA2MNFE(CN)6-carbon nanotube composite cathode material composition for secondary batteries

[0001] The present invention relates to a Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, and more particularly, to a Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, which can not only improve the process yield in manufacturing a cathode material used in a Prussian blue-based sodium ion battery, but also improve the charge / discharge efficiency and quality of a secondary battery by homogeneously mixing the components and increasing the electrical conductivity.

[0002]

[0003] In general, as the use of electronic devices such as smartphones becomes more widespread and miniaturized, secondary batteries are also becoming smaller, and among secondary batteries, lithium secondary batteries that use organic electrolytes and exhibit a discharge voltage more than twice as high and high energy density as batteries that use conventional alkaline aqueous solutions are widely used.

[0004] The lithium secondary battery described above is composed of a positive electrode, an electrolyte, and an anode. Commercially available lithium secondary batteries have a structure in which a 15-25 ㎛ thick polymer separator is added to a liquid electrolyte composed of an organic solvent and a lithium salt. When discharging, Li+ ions move from the negative electrode to the positive electrode, and electrons generated when Li is ionized also move from the negative electrode to the positive electrode. When charging, they move in the opposite direction.

[0005] The driving force behind this Li+ ion movement is the chemical stability of the two electrodes, which is determined by the potential difference between them. The capacity (Ah) of the battery is determined by the amount of Li+ ions moving from the negative electrode to the positive electrode and vice versa. Since this movement of Li+ ions occurs through the electrolyte, the Li+ ion conductivity of the electrolyte is known to affect the charge / discharge rate of the battery.

[0006] Meanwhile, the all-solid-state secondary battery replaces the liquid electrolyte among the above battery components with a solid electrolyte. Compared to liquid electrolytes, it has no risk of explosion or fire, simplifies the manufacturing process, and has the potential for high energy density, making it a next-generation secondary battery.

[0007] However, while solid-state secondary batteries have higher safety than liquid electrolytes due to the use of solid electrolytes, they have the problem of reduced ionic conductivity due to the reduced ionic conduction path caused by reduced interfacial contact with the electrodes.

[0008] Meanwhile, sodium secondary batteries have recently been developed, using sodium metal oxide as the positive active material and metals, sodium metal alloys, etc. as the negative active material. These sodium secondary batteries are charged and discharged through repeated processes of intercalation and deintercalation of sodium ions from the positive sodium metal oxide to the negative graphite electrode.

[0009] For example, as mentioned above, Na2MnFe(CN)6, also known as Prussian blue, is used as a cathode material for sodium secondary batteries.

[0010] The above-mentioned Na2MnFe(CN)6 is generally manufactured by forming a primary solution by adding 0.03M Na4Fe(CN)6 and 6M NaCl aqueous solution to a stirring tank, slowly dropping a secondary solution (0.06M MnCl2 aqueous solution) into the stirring tank containing the primary solution (0.03M Na4Fe(CN)6 + 6M NaCl aqueous solution) and stirring for more than 6 hours, and then separating the solid and liquid.

[0011] However, as is well known, the above-mentioned Prussian blue has a relatively low electrical conductivity, which causes a problem in that the charge / discharge efficiency is reduced when manufactured into a secondary battery.

[0012] In addition, the manufacturing method described above has a problem in that it cannot increase the solubility due to the limit of the solubility of Na+, which is the common ion of Na4Fe(CN)6 and NaCl constituting the primary solution, and has a limitation in that the charging / discharging efficiency and quality are further reduced due to the low mixing homogeneity of the main components.

[0013]

[0014] The present invention has been devised to solve the above problems, and its purpose is to provide a Na2MnFe(CN)6-carbon nanotube composite cathode material composition for secondary batteries, which can not only improve the yield in manufacturing cathode materials used in Prussian blue-based sodium ion batteries, but also homogeneously mix the components and increase electrical conductivity.

[0015]

[0016] The present invention is intended to solve the above-mentioned object, and provides a Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, which is manufactured from a slurry prepared by mixing carbon nanotubes together in a first mixture of MnCl2 and NaCl aqueous solutions so that the carbon nanotubes are homogeneously distributed in the first mixture, and then mixing Na4Fe(CN)6 aqueous solution for a second time.

[0017] In addition, the content ratio (M) of each component included in the composite cathode material composition is characterized as MnCl2: NaCl: Na4Fe(CN)6= 2:2.5:1.

[0018] The present invention is intended to achieve the above object, and provides a Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, which is manufactured from a slurry obtained by mixing carbon nanotubes together in a first mixture of MnCl2 and NaCl aqueous solutions so that the carbon nanotubes are homogeneously distributed in the first mixture, and then dropping Na4Fe(CN)6 aqueous solution into the first mixture at a rate of 2 mL / min to 5 mL / min to mix the second mixture.

[0019] In addition, the content ratio (M) of each component included in the composite cathode material composition is characterized as MnCl2: NaCl: Na4Fe(CN)6= 2:2.5:1.

[0020] In addition, the above Na4Fe(CN)6 aqueous solution is characterized in that it is dropped into the primary mixture at a rate of 2 mL / min to 5 mL / min using a pneumatic aerosol sprayer.

[0021] In addition, the injection pressure of the pneumatic aerosol injector is characterized by being in the range of 0.5 bar to 2 bar.

[0022] In addition, the particle size of the slurry is characterized by being in the range of 20 nm to 1 μm.

[0023] In addition, the carbon nanotubes are characterized in that they are mixed in an amount of 5 to 10 wt% relative to the total weight of the primary mixture.

[0024]

[0025] Figure 1 is a graph showing the electrochemical characteristics of a secondary battery according to Comparative Example 1 and Figure 2 is a graph showing the electrochemical characteristics of a secondary battery according to Example 1.

[0026] Figure 3 is a graph showing the electrochemical characteristics of a secondary battery according to Comparative Example 2 and Figure 4 is a graph showing the electrochemical characteristics of a secondary battery according to Example 1.

[0027] Figure 5 is a schematic process diagram for explaining a method for manufacturing a cathode material for a secondary battery according to one embodiment of the present invention.

[0028]

[0029] The present invention relates to a Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery.

[0030]

[0031] Hereinafter, the present invention will be described in detail with reference to the attached drawings.

[0032]

[0033] The present invention improves the yield by changing the process sequence in the manufacture of a cathode material used in a Prussian blue-based sodium ion battery, and improves the quality of a secondary battery by adding carbon nanotubes from the initial mixing stage of the components, thereby mixing each component of the particles more homogeneously and increasing electrical conductivity.

[0034] Specifically, according to one embodiment of the present invention, a Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery is manufactured from a slurry prepared by mixing carbon nanotubes together with a first mixture of MnCl2 and NaCl aqueous solutions so that the carbon nanotubes are homogeneously distributed in the first mixture, and then mixing Na4Fe(CN)6 aqueous solution for a second time.

[0035] According to another aspect of the present invention, a Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery is manufactured from a slurry obtained by mixing carbon nanotubes together in a first mixture of MnCl2 and NaCl aqueous solutions so that the carbon nanotubes are homogeneously distributed in the first mixture, and then dropping a Na4Fe(CN)6 aqueous solution into the first mixture at a rate of 2 mL / min to 5 mL / min to mix it a second time.

[0036] The above composite cathode material composition is manufactured in two steps: a first step of mixing carbon nanotubes into a primary mixture of MnCl2 and NaCl aqueous solutions so that the carbon nanotubes are homogeneously distributed in the primary mixture; and a second step of mixing Na4Fe(CN)6 aqueous solution. This is to overcome the drawback of the prior art in that when Na4Fe(CN)6 and NaCl are dissolved together to manufacture the primary solution, sodium ions are co-incorporated, limiting the solubility of Na4Fe(CN)6 to a maximum of 0.03 M, thereby lowering the yield of the final product. Therefore, by mixing Na4Fe(CN)6 aqueous solution into the primary mixture of MnCl2 and NaCl aqueous solutions sufficiently mixed in the first step as the second step, the final product can be obtained with the maximum yield.

[0037] In addition, the carbon nanotubes were introduced from the beginning into the first process of manufacturing the first mixture of MnCl2 and NaCl aqueous solutions. This can significantly improve electrical conductivity by increasing the uniformity of distribution of carbon nanotubes within the cathode material composition, compared to the conventional technique of introducing conductive materials such as carbon nanotubes after the manufacture of cathode material slurry is completed.

[0038] From the differences due to the process differences, the content ratio (M) of each component included in the final product can be MnCl2: NaCl: Na4Fe(CN)6= 2:2.5:1.

[0039] In addition, in order to ensure that each component material can be uniformly distributed, it is preferable to mix the Na4Fe(CN)6 aqueous solution by using a pneumatic aerosol sprayer while adding it to the first mixed solution in the second process.

[0040] In one embodiment of the present invention, the operating speed of the pneumatic aerosol injector is preferably in the range of 2 mL / min to 5 mL / min. If it is less than 2 mL / min, the injection speed is slow, which is not preferable because the production time becomes long, and if it is more than 5 mL / min, the injection time can be shortened, but the particles of the reaction product, Prussian flu, become too large, which is not preferable.

[0041] In addition, the injection pressure of the pneumatic aerosol injector is preferably in the range of 0.5 bar to 2 bar. If it is less than 0.5 bar, it is not preferable because the pressure is low and it is difficult to react uniformly, and if it is more than 2 bar, it is not preferable because the problem of overflowing the reactor during small-scale production and the phenomenon of moisture evaporating due to high pressure are intensified, causing a problem of concentration change.

[0042] It is preferable that the particle size of the cathode material composition slurry according to one embodiment of the present invention manufactured by such a process be in the range of 20 nm to 1 ㎛. If it is less than 20 nm, the volume becomes relatively large, which is not preferable because the energy density per volume becomes low. If it is more than 1 ㎛, it is not preferable because it is difficult to implement performance due to low electrical conductivity when the particle size becomes large.

[0043] The present invention forms a primary solution by mixing 2M MnCl2 and 2.5M NaCl aqueous solutions, and thus has the advantage of superior solubility compared to the case where components having Na+ ions are mixed as in the conventional manufacturing method described in the background art.

[0044] In addition, the secondary battery cathode material composition of the present invention can more homogeneously mix each component of the particles by adding carbon-based conductive particles, and can increase the electrical conductivity of the secondary battery cathode material, thereby having the effect of improving the quality of the secondary battery.

[0045]

[0046] A cathode material for a secondary battery according to one embodiment of the present invention can be manufactured by the following manufacturing method (Fig. 5).

[0047] A method for manufacturing a cathode material for a Prussian blue type sodium ion battery comprises sequentially performing a first solution composition step (s1), a second solution composition step (s2), a solid-liquid separation step (s3), a washing step (s4), a dehydration step (s5), a drying step (s6), and a crushing step (s7).

[0048] The first solution composition step (s1) is 2M MnCl 2+ A step of mixing 2.5M NaCl aqueous solution to form a primary solution, 2M MnCl in the first mixing tank 2+ It is prepared by adding 2.5M NaCl aqueous solution and then operating the first stirrer to stir.

[0049] The secondary solution composition step (s2) is a step of creating a secondary solution by mixing a 1M Na4Fe(CN)6 aqueous solution into the primary solution created by the primary solution composition step (s1). The primary solution is introduced into a second mixing tank, and the secondary solution is introduced at a rate of 1 to 5 ml per minute (min), and then the second stirrer is operated to stir for 5 hours or more.

[0050] Here, it is preferable to prepare the secondary solution by adding it at a rate of 1 ml per minute (min) for homogeneous mixing and stirring for more than 12 hours.

[0051] And, the method for manufacturing a cathode material for a secondary battery according to one embodiment of the present invention is characterized by performing a carbon-based conductive material particle introduction step (s12) of introducing and mixing carbon-based conductive material particles to improve the electrical conductivity of the cathode material for a secondary battery.

[0052] The carbon-based conductive particle injection step (s12) is injected in the primary solution composition step (s1) that performs the primary solution composition process so that a more homogeneous mixture can be achieved through repeated stirring and high-pressure spraying through a multi-stage mixing process.

[0053] Additionally, it is preferable to add carbon-based conductive particles in an amount ranging from 5 to 10 wt% of the total weight of the primary solution. This composition ratio is obtained by repeatedly testing secondary batteries using cathode material test products and measuring their quality.

[0054] In addition, it is desirable to use carbon nanotubes (CNTs) as carbon-based conductive particles that can increase electrical conductivity.

[0055] Meanwhile, the solid-liquid separation step (s3) is a step of obtaining a solid secondary battery cathode material by removing the solvent through solid-liquid separation of the secondary solution formed by the secondary solution composition step.

[0056] And the wastewater, which is the solvent separated in the high-liquid separation stage (s3), is moved to the wastewater treatment unit and discharged after going through a purification process.

[0057] In addition, the high-liquid separation step (s3) can be applied without limitation to various high-liquid separation means such as a filter press, but in this embodiment, it is performed using a centrifuge as described below.

[0058] The washing step (s4) is a step for washing the cathode material for a secondary battery that has undergone the solid-liquid separation step (s3). The cathode material for a secondary battery is placed in a washing tank, washing water is supplied, and a washing mixer is operated to mix the material so that any remaining foreign substances are dissolved in the washing water.

[0059] The dehydration step (s5) is a step for removing the washing water included in the process of performing the washing step (s4), and is a step for dehydrating the washing water through a solid-liquid separation process using a centrifuge, dehydrator, etc.

[0060] The aforementioned washing step (s4) and dehydration step (s5) can be performed two or more times without limitation to obtain a clean cathode material for secondary batteries. However, after analyzing the quality of the cathode material for secondary batteries through repeated test manufacturing, it was confirmed that performing the process three times is preferable.

[0061] The drying step (s6) is a step for drying the cathode material for secondary batteries that has undergone the dehydration step (s5), and it is preferable to vacuum-dry at a temperature range of 80 to 100°C.

[0062] For example, the drying step (s6) is performed by placing the secondary battery cathode material that has gone through the dehydration step (s5) into a vacuum oven, setting the drying temperature to a range of 80 to 100°C, and drying for 12 hours or more.

[0063] The crushing step (s7) is a step of crushing the cathode material for secondary batteries that has gone through the drying step (s6), and is performed using a crushing means such as a ball mill.

[0064]

[0065] Hereinafter, the present invention will be described in more detail through examples. However, these examples are intended solely to illustrate the present invention, and the scope of the present invention is not to be construed as being limited by these examples. Those skilled in the art will understand that some of the examples can be substituted or modified without departing from the technical spirit of the present invention.

[0066]

[0067] [Example]

[0068] [Example 1]

[0069] After adding CNT (10 wt%) to the primary solution containing a mixture of 2 M MnCl2 and 2.5 M NaCl aqueous solutions, the first stirrer is operated to stir.

[0070] The first solution containing the above-described carbon nanotubes is added to the second mixing tank, and a 1M Na4Fe(CN)6 aqueous solution is dropped at a rate of 1 ml / min using a pneumatic aerosol sprayer and stirred for 12 hours or more.

[0071] The Prussian blue, after the reaction is complete, is separated from the solvent using centrifugation.

[0072] Afterwards, the secondary battery cathode material is placed in the washing tank, washing water is supplied, and the washing agitator is operated to wash it three times.

[0073] After separation by centrifugation, vacuum dry at 80-100℃ for more than 12 hours.

[0074] Use after grinding using a ball mill.

[0075]

[0076] [Comparative example]

[0077] [Comparative Example 1]

[0078] The same method as Example 1 is performed except that CNT is not added to the primary solution.

[0079]

[0080] [Comparative Example 2]

[0081] The same method as Example 1 is used, except that CNTs are added in the electrode manufacturing step rather than in the primary solution.

[0082]

[0083] [Comparative Example 3]

[0084] After adding CNT (..wt%) to the primary solution containing 0.03M Na4Fe(CN)6 and 6M NaCl aqueous solution, the first stirrer is operated to stir.

[0085] The primary solution containing the above-described carbon nanotubes is added to the second mixing tank, and a 0.06 M MnCl2 aqueous solution is dropped at a rate of 1 ml / min using a pneumatic aerosol sprayer and stirred for more than 12 hours.

[0086] The Prussian blue, after the reaction is complete, is separated from the solvent using centrifugation.

[0087] Afterwards, the cathode material for secondary batteries is placed in the washing tank, washing water is supplied, and the washing agitator is operated to wash it three times.

[0088] After separation by centrifugation, vacuum dry at 80-100℃ for more than 12 hours.

[0089] Use after grinding using a ball mill.

[0090]

[0091] [Experimental Example]

[0092] Fig. 1 is a graph showing the electrochemical characteristics of a secondary battery according to Comparative Example 1 and Fig. 2 is a graph showing the electrochemical characteristics of a secondary battery according to Example 1. Referring to Figs. 1 and 2, in the case of Comparative Example 1 (Fig. 1), the initial capacity is about 120 mAh / g, and in the case of Example 1 (Fig. 2), the initial capacity is about 135 mAh / g.

[0093] Figures 3, 4, and Table 1 show the results of electrochemical characteristics of secondary batteries according to Comparative Example 2 (Figure 3) and Example 1 (Figure 4). Referring to these, it can be seen that the electrochemical characteristics are superior when carbon nanotubes are mixed into the primary solution of Example 1 compared to when carbon nanotubes are added in the electrode manufacturing step of Comparative Example 2.

[0094] Test type Electrolyte active material weight (mg) Active material loading amount (mg / cm 2 ) Condition Example 1HalfPC90:EC93.872.510.116mAh (based on 150mAh / g) Comparative Example 2HalfTEP90:PC9:VC13.742.430.112mAh (based on 150mAh / g)

[0095] Table 2 shows the results showing the production amount of Example 1 according to the present invention and Comparative Example 3 according to the conventional method in manufacturing a Prussian blue cathode material. In the case of Comparative Example 3, when Na4Fe(CN)6 and NaCl were dissolved together to prepare the first solution, the solubility of the main reactant, Na4Fe(CN)6, did not dissolve up to a maximum of 0.03 M due to the dissolution phenomenon of the co-ion of the sodium ion, so that the final product could be produced in an amount of up to 10 g per 1 L of water. On the other hand, in the case of the Example, NaCl was dissolved together with MnCl2, so that the co-ion reaction of Cl occurred, but the solubility of MnCl2 was at most 73.9 g / 100 mL at room temperature, so even if NaCl was dissolved together with MnCl2, the amount for reacting by dissolving Na4Fe(CN)6 alone to the maximum was sufficient, so that up to 100 g could be produced when up to 1 L of water was used. Therefore, it can be seen that a production amount more than 10 times that of the conventional method can be obtained.

[0096] Na2MnFe(CN)6 production amount (based on 1L of water) Example 1100g Comparative example 310g

[0097]

[0098] According to the Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery according to the present invention, the primary solution is formed by mixing MnCl2 and NaCl aqueous solutions instead of first mixing components having Na+ ions as in the prior art, so that solubility can be improved, and by adding carbon nanotubes to the primary solution, each component of the particles can be mixed more homogeneously and electrical conductivity can be increased, thereby having the effect of improving the quality of the secondary battery.

Claims

1. A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery manufactured from a slurry prepared by mixing carbon nanotubes together in a first mixture of MnCl2 and NaCl aqueous solutions so that the carbon nanotubes are homogeneously distributed in the first mixture, and then mixing Na4Fe(CN)6 aqueous solution for a second time.

2. In paragraph 1, A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, characterized in that the content ratio (M) of each component included in the composite cathode material composition is MnCl2: NaCl: Na4Fe(CN)6= 2:2.5:

1.

3. In paragraph 2, A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, characterized in that the carbon nanotubes are mixed in an amount of 5 to 10 wt% relative to the total weight of the primary mixture.

4. A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery manufactured from a slurry obtained by mixing carbon nanotubes together in a first mixture of MnCl2 and NaCl aqueous solutions so that the carbon nanotubes are homogeneously distributed in the first mixture, and then dropping Na4Fe(CN)6 aqueous solution into the first mixture at a rate of 2 mL / min to 5 mL / min to mix the second mixture.

5. In paragraph 4, A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, characterized in that the above Na4Fe(CN)6 aqueous solution is dropped into the primary mixture at a rate of 2 mL / min to 5 mL / min using a pneumatic aerosol sprayer.

6. In paragraph 5, A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, characterized in that the spray pressure of the above pneumatic aerosol sprayer is in the range of 0.5 bar to 2 bar.

7. A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, characterized in that the particle size of the slurry in the 6th paragraph is in the range of 20 nm to 1 μm.

8. In paragraph 4, A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, characterized in that the content ratio (M) of each component included in the composite cathode material composition is MnCl2: NaCl: Na4Fe(CN)6= 2:2.5:

1.

9. In paragraph 8, A Na2MnFe(CN)6-carbon nanotube composite cathode material composition for a secondary battery, characterized in that the carbon nanotubes are mixed in an amount of 5 to 10 wt% relative to the total weight of the primary mixture.

Citation Information

Patent Citations

  • Method for preparing Prussian blue positive electrode material, and sodium ion battery

    CN107364875A

  • Sodium-ion battery anode material as well as preparation method and application thereof

    CN108258239A

  • Method for preparing Prussian blue positive electrode material and sodium ion battery

    CN109599558A

  • Prussian blue cathode material with high sodium content, preparation method and applications thereof, and sodium ion battery

    CN110235292A

  • Method for producing electrode material, battery and electrode member

    JP2014026805A