Compositions, systems and methods for removing impurities from lithium-containing aqueous solutions

The selective solvent extraction of magnesium and calcium impurities from lithium-containing solutions using a tailored reagent composition enhances lithium recovery by reducing impurity levels and minimizing losses, addressing the challenges of existing purification methods and improving processing efficiency.

WO2024249272A1PCT designated stage expired Publication Date: 2024-12-05ENERGY EXPLORATION TECHNOLOGIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/030852
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current methods for purifying lithium-containing aqueous solutions, such as those from brine evaporation or direct lithium extraction, often result in significant losses of lithium due to coprecipitation with impurities like magnesium and calcium, which are difficult and expensive to separate, leading to reduced lithium yields and processing bottlenecks.

Method used

The use of a selective reagent composition in solvent extraction systems that selectively extracts magnesium and calcium impurities from lithium-containing aqueous solutions, forming an impurity-depleted lithium solution and an impurity-rich organic stream, with subsequent stripping and recycling of the reagent to enhance lithium recovery processes.

Benefits of technology

This approach significantly increases lithium yield by reducing impurity levels to trace amounts, minimizing lithium losses, and simplifying the processing steps, thereby improving the economic viability of lithium recovery and production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024030852_05122024_PF_FP_ABST
    Figure US2024030852_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are methods of removing impurities (e.g., magnesium, calcium, or both) from an aqueous solution comprising lithium. The methods can include contacting the aqueous solution with a reagent composition that selectively extracts the impurities over the lithium; and forming an impurity depleted lithium aqueous solution and an impurity rich organic solution. Also disclosed are reagent compositions and related systems.
Need to check novelty before this filing date? Find Prior Art

Description

COMPOSITIONS, SYSTEMS AND METHODS FOR REMOVING IMPURITIES FROMLITHIUM-CONTAINING AQUEOUS SOLUTIONSFIELD

[0001] The disclosure relates to compositions, systems and methods for removing impurities, such as, calcium and magnesium, from lithium-containing aqueous solutions.BACKGROUND

[0002] In the world’s transition to clean energy, electricity storage platforms play an important role. Lithium batteries are at the forefront of electricity storage technologies because inter alia they charge faster, last longer and have a higher power density to provide more battery life in a lighter package than conventional batteries. Lithium storage devices are useful for electrification of the transportation sector, electric vehicles, battery storage for electric utilities and in many other applications to reduce carbon emissions and store electricity.

[0003] Lithium is typically extracted from underground deposits of brine water and ore made of compounds containing lithium. Brines from salars and salt lakes, as well as spodumene ores, are the primary sources of lithium, while geothermal brines represent secondary sources. Li- containing brine obtained from a source is initially concentrated to a suitable concentration (e.g., about 6,000 ppm Li) for viable recovery. Classical methods of lithium extraction rely on brine evaporation in open ponds to maximize element concentration for further purification; however, these methods are very slow (evaporation of ponds to the desired level can take up to 24 months) and strongly dependent on region-specific weather conditions that vary throughout the year. Newer technologies based on precipitation, adsorption, solvent extraction and membranes can beused for brine concentration and may increase the economic viability of minerals extracted from seawater and other geothermal brines. While all of these technologies are able to produce a purified lithium solution, impurities such as calcium and magnesium remain. There is a need for improved processes and compositions to further purify metal (e.g., lithium) containing aqueous solutions to remove unwanted impurities such as magnesium and / or calcium.BRIEF SUMMARY

[0007] Described herein are methods of removing impurities (e.g., magnesium, calcium, or both) from an aqueous solution comprising lithium. The methods include contacting the aqueous solution with a reagent composition that selectively extracts the impurities over the lithium; and forming an impurity depleted lithium aqueous solution and an impurity rich organic solution. In some embodiments, the impurity depleted lithium aqueous solution comprises trace amounts of the impurities, less than trace amounts of the impurities or no detectable amount of the impurities.

[0008] In one or more embodiments, the metal containing aqueous solution comprises a brine, a metal (e.g., lithium) product stream, a stream exiting a direct metal (e.g., lithium) extraction process, a purified and concentrated brine, a stream existing a pond system, feed stream to a metal (e.g., lithium) recovery plant, or combinations thereof. The metal containing aqueous solution may comprise lithium in an amount of about 200 ppmw to about 2,000 ppmw and further comprises sodium, potassium, magnesium, calcium, chlorine, sulfate, boron or combinations thereof. In some embodiments, the aqueous solution comprises a weight ratio of magnesium to lithium of about 50: 1 to about 1 :50, about 1 : 1 to about 20: 1, or any individual value or sub-range within these ranges, and / or the aqueous solution comprises a weight ratio of calcium to lithium of about 50: 1 to about 1 :50, about 1 :1 to about 20: 1, or any individual value or sub-range within theseranges. In some embodiments, the reagent composition comprises an impurity selective extractant in an amount of about 0.025 M to about 3 M, about 0.05 M to about 2 M, about 0.1 M to about 1M, or any individual value or sub-range within these ranges.

[0004] The reagent composition includes an extractant that is selective for the impurities over lithium. In some embodiments, the reagent composition further comprises a modifier. According to various embodiments, the reagent composition extracts only trace amounts of lithium, less than trace amounts of lithium or no detectable amount of lithium.

[0005] In one or more embodiments contacting the aqueous solution with the reagent composition comprises ion exchange, electrodialysis, solvent extraction, adsorption techniques, or combinations thereof. In some embodiments, contacting the aqueous solution with the reagent composition is in a solvent extraction system.

[0006] The methods can further include stripping in a stripping process the impurity rich organic stream of the impurities to form a fresh reagent composition and a concentrated impurity solution. The methods can further include returning the fresh reagent composition to the extraction process for contacting with the aqueous solution. The concentrated impurity solution may flow to a purification process to remove the impurities and form a fresh strip solution. In some embodiments, the fresh strip solution is returned to the stripping process.

[0007] The methods may further include extracting boron from the impurity depleted lithium aqueous solution.

[0009] According one or more embodiments, contacting the aqueous solution with the reagent composition is: at a pH of greater than 5, or greater than 5 to about 6, at a pH of greater than 6, or greater than 6 to about 9, at a pH of greater than 9, or greater than 9 to about 10, or at a pH of greater than 10, or greater than 10 to about 12.

[0010] In one or more embodiments, the impurity depleted lithium aqueous solution is fed to a lithium recovery process. Lithium yield from the lithium recovery process can, for example, increase by about 1% to about 99%, about 2% to about 95%, about 5% to about 80%, about 10% to about 50%, or any individual value or sub-range within these ranges. According to various embodiments, the lithium recovery process produces lithium carbonate.

[0011] Further disclosed herein are systems for removing impurities comprising magnesium, calcium, or both from an aqueous solution comprising lithium. In one or more embodiments, the systems include a solvent extraction stage, which may be a first solvent extraction stage, configured to receive the aqueous solution and contact the aqueous solution with a reagent composition that selectively extracts at least one of the impurities over the lithium; and form a first impurity depleted lithium aqueous solution and a first impurity rich organic solution.

[0012] According to one or more embodiments, systems further include a second solvent extraction stage configured to: receive the first impurity depleted lithium aqueous solution and contact the aqueous solution with a reagent composition that selectively extracts at least one of the impurities over the lithium; and form a second impurity depleted lithium aqueous solution and a second impurity rich organic solution. In some embodiments, the first solvent extraction stage substantially extracts calcium (or magnesium) and the second solvent extraction stage substantially extracts magnesium (or calcium).SUMMARY OF THE DRAWINGS

[0013] The present disclosure is illustrated by way of example, and not by way of limitation, in the figures of the accompanying drawings in which like references indicate similar elements.

[0014] FIG. 1 is a schematic of a lithium extraction system for a metal containing aqueous solution containing a high concentration of magnesium using a series of cascading ponds.

[0015] FIG. 2 is a schematic of a lithium extraction system containing a series of cascading ponds.

[0016] FIG. 3 is a schematic of a lithium extraction process from a concentrated metal containing aqueous solution containing lithium.

[0017] FIG. 4 is a schematic of an embodiment of a lithium extraction process from a concentrated lithium containing aqueous solution.

[0018] FIG. 5 is an isotherm chart showing extraction percentage as a function of time of calcium and magnesium from an aqueous solution at a pH of greater than 5.

[0019] FIG. 6 is an isotherm chart showing extraction percentage as a function of time of calcium and magnesium from an aqueous solution at a pH of greater than 6.

[0020] FIG. 7 is an isotherm chart showing extraction percentage as a function of time of calcium and magnesium from an aqueous solution at a pH of greater than 9.

[0021] FIG. 8 is an isotherm chart showing extraction percentage as a function of time of calcium and magnesium from an aqueous solution at a pH of greater than 10.

[0022] FIG. 9 is a schematic of an embodiment of a solvent extraction process for extracting lithium from an aqueous solution.

[0023] FIG. 10 is a schematic of an extraction system for removing magnesium and calcium from an aqueous solution containing lithium.

[0024] FIG. 11 is a schematic of a solvent extraction system according to one or more embodiments herein.Definitions

[0025] Reference throughout this specification to, for example, “one embodiment,” “certain embodiments,” “one or more embodiments” or “an embodiment” means that a particular feature, structure, material, or characteristic described in connection with the embodiment is included in at least one embodiment of the invention. Thus, the appearances of the phrases such as “in one or more embodiments,” “in certain embodiments,” “in one embodiment” or “In one or more embodiments” in various places throughout this specification are not necessarily referring to the same embodiment of the invention. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0026] As used herein, the singular forms “a,” “an,” and “the” include plural references unless the context clearly indicates otherwise. Thus, for example, reference to “a depurator vessel” includes a single depurator vessel as well as more than one depurator vessel.

[0027] As used herein, the term “about” in connection with a measured quantity, refers to the normal variations in that measured quantity as expected by one of ordinary skill in the art in making the measurement and exercising a level of care commensurate with the objective of measurement and the precision of the measuring equipment. In certain embodiments, the term “about” includes the recited number ±10%, such that “about 10” would include from 9 to 11.

[0028] The term “at least about” in connection with a measured quantity refers to the normal variations in the measured quantity, as expected by one of ordinary skill in the art in making the measurement and exercising a level of care commensurate with the objective of measurement and precisions of the measuring equipment and any quantities higher than that. In certain embodiments, the term “at least about” includes the recited number minus 10% and any quantity that is higher such that “at least about 10” would include 9 and anything greater than 9. This term can also be expressed as “about 10 or more.” Similarly, the term “less than about” typicallyincludes the recited number plus 10% and any quantity that is lower such that “less than about 10” would include 11 and anything less than 11. This term can also be expressed as “about 10 or less.”

[0029] Unless otherwise indicated, all parts and percentages are by weight. Weight percent (wt. %), if not otherwise indicated, is based on an entire composition free of any volatiles, that is, based on dry solids content.

[0030] Reference throughout this specification to a chemical element or a “metal” encompasses the basic chemical element or metal itself, ions, molecules containing the chemical element or metal, and / or ionic compounds containing the chemical element or metal, or combinations thereof. For example, “lithium” refers to the element lithium, lithium ions, lithium salts, lithium-containing molecules and lithium-containing ionic compounds, or combinations thereof.

[0031] The term “trace” or “trace amount” as used herein refers to the amount of a component in a solution being less than about 1 part per million by weight (ppmw).DETAILED DESCRIPTION

[0032] Embodiments of the disclosure are described more fully hereinafter with reference to the accompanying drawings, which form a part hereof, and which show, by way of illustration, example features. The features can, however, be embodied in many different forms and should not be construed as limited to the combinations set forth herein; rather, these combinations are provided so that this disclosure will be thorough and complete and will fully convey the scope. The following detailed description is, therefore, not to be taken in a limiting sense.

[0033] Nearly two-thirds of the lithium resources in the world reside in very high salinity brines having lithium concentrations of about 200 ppmw - 65,000 ppmw. Lithium in these brines is typically subterranean and associated with high levels of Na+, K+, Mg2+, Ca2+, C1‘, SCU2', B (ionicor molecular) and other ions (i.e., “impurity ions”). Each brine chemistry is unique. Calcium and magnesium are known impurities of significance because brines containing high Ca / Li and / or Mg / Li ratios are typically processed either in evaporation ponds or by direct lithium extraction in order to significantly lower these ratios.

[0034] Existing methods and systems for purifying and concentrating metal containing aqueous solutions are based on solar evaporation / concentration processes. In all such cases, major coprecipitation losses of lithium occur. In metal containing aqueous solutions having a high magnesium concentration, these losses occur mainly as a lithium carnallite precipitate (LiCl.MgCl2.7H2O). In high sulfate metal containing aqueous solutions, these losses occur mainly as lithium sulfate monohydrate (Li2SO4.H2O) and lithium schoenite (Li2SO4.K2SO4) precipitates.

[0035] According to one or more embodiments, lithium product streams as described herein can be, for example, a direct lithium extraction (DLE) concentrated aqueous solution (e.g., a purified and concentrated brine) and / or any feed to a processing plant that converts a metal containing aqueous solution into lithium products. Metal (e g., lithium) containing aqueous solutions may be purified using various methods to achieve a suitable concentration or level of impurities that makes conversion to lithium products in the ponds easier and economically attractive. See FIGs. 1 and 2. However, significant impurities still remain in these lithium product streams fed to the lithium conversion and / or recovery plants. The most troublesome impurities are magnesium (Mg / Mg2+) and calcium (Ca / Ca2+). These impurities must be chemically precipitated and separated from lithium in the processing plant. This is a difficult and expensive step that bottlenecks processing plants. Along with the removal of impurities, valuable lithium, up to 10%, is lost.

[0036] FIG. 1 shows a schematic representation of a conventional evaporation and concentration system 100 for forming a lithium product stream 110 (i.e., an aqueous stream that has been purifiedand concentrated with lithium). A metal containing aqueous solution feed (not shown) containing a high concentration of magnesium flows into a halite pond 102 wherein halite salts among others are precipitated and removed. From the halite pond 102, the halite purified aqueous stream flows into a sylvinite pond 104 where inter alia sylvinite salts are precipitated and removed. The sylvinite purified aqueous stream flows into a carnallite pond 106 where carnallite salts, among others, are precipitated and removed. The carnallite purified stream flows into a final lithium pond 108 where lithium carnallite and lithium sulfate monohydrate salts, among others, are precipitated and removed. The purified and concentrated lithium product stream 110 exits the pond system 100 and flows to a lithium plant for further recovery and processing (e.g., lithium carbonate recovery).

[0037] As shown in FIG. 1, prior to final evaporation, the lithium concentration may be at about 1.6% when it enters the processing plant. Even lower concentrations (as low as about 0.7% Li) may be fed to processing plants in some locations where the magnesium concentration in the metal containing aqueous feed is lower because the magnesium is chemically precipitated in the ponds at great expense and difficulty. In some processes, the metal containing aqueous solution is concentrated further, sacrificing 40-70% of valuable lithium (about 50% in FIG. 1) so that magnesium levels can be reduced from 5.36% to 1.5%. In other cases where lithium is separated from magnesium, continued evaporation of the metal containing aqueous solution can reconcentrate the magnesium along with the lithium to about 0.5 wt% magnesium.

[0038] FIG. 2 shows a schematic of another conventional evaporation pond system 200 for purifying and concentrating a metal containing aqueous solution to form a lithium product stream 210. A metal containing aqueous solution feed (not shown) containing a high concentration of magnesium flows into a halite pond 202 wherein sodium and halite salts among others areprecipitated and removed. From the halite pond 202, the halite purified aqueous stream flows into a sylvinite pond 204 where potassium and sylvinite salts among others are precipitated and removed. The sylvinite purified aqueous stream flows into a mixed salt pond 206 where halite, sylvinite, carnallite and kainite salts among others are precipitated and removed. The mixed salt purified stream flows into a final lithium sulfate pond 208 where halite and carnalite salts, among others, are precipitated and removed. The purified and concentrated lithium product stream 210 exits the pond system 200 and flows to a lithium plant for further recovery and processing (e.g., lithium carbonate recovery).

[0039] The metal containing aqueous feed to the pond system 200 of FIG. 2 had even higher ratios of magnesium to lithium (20: 1) and sulfate (SO4) to lithium (30: 1) than the feed in FIG. 1. Even upon lithium concentration, the magnesium to lithium ratios remained very high with the residual aqueous solution remaining unprocessable at a magnesium to lithium ratio of 18: 1. The lithium sulfate precipitate was, thus, chosen for production which still had a magnesium to lithium ratio of 4: 1. Because of these high Mg / Li ratios, this particular system 200 has produced very little lithium despite being the world’s largest resource with a pond and processing plant infrastructure. Removing magnesium in the evaporation pond or other direct lithium extraction (DLE) processes could substantially increase lithium yield.

[0040] Even after the metal containing aqueous solutions have been purified and concentrated in the pond system 100 or 200 to form a lithium product stream, calcium and / or magnesium impurities can persist in the product streams. Removing calcium and / or magnesium from lithium product streams (i.e., streams exiting a pond system and / or a DLE process) before or after conversion to a lithium product (e.g., lithium carbonate) may be process intensive and result in a loss of lithium yield.

[0041] In further conventional processes for processing metal containing aqueous solutions, lithium product streams may be further processed prior to lithium recovery. FIG. 3 is a flow chart depicting a conventional lime soda softening process 300 of a lithium product stream (e.g., a brine), an evaporated feed (e.g., exiting a pond system) and / or a DLE brine collectively 302. At block 304, boron is separated from the feed using solvent extraction. This is followed by, at block 306, the addition of lime (Ca(OH)2), which precipitates Mg(OH)2 and sulfate as CaSCM. This saturates the metal containing aqueous solution in calcium, which is removed by addition of soda ash (Na2CC>3) precipitating Ca as CaCCh. In the lime precipitation step, a very difficult to separate magnesium hydroxide and gypsum sludge is precipitated, which traps a large amount of high lithium concentrated aqueous. This may be separated and softened using a series of steps at blocks 308-312, for example, large filter presses with multiple washings. Still about 5-10% of the lithium remains in this sludge resulting in a loss of recovery. Calcium carbonate is easier to filter, but to ensure complete removal of Ca, a small excess of soda ash must be added. This excess soda ash results in precipitation of Li as Li2CC>3. This again represents a loss of recovery of lithium products 314.

[0042] It is desirable to remove calcium and magnesium impurities from metal (e.g., lithium) containing aqueous solutions (or product streams) using solvent extraction prior to metal (e.g., lithium) recovery processing. The compositions, systems and methods according to embodiments herein are suitable to remove such impurities from metal containing aqueous streams and / or metal containing product streams. Without being bound by any particular theory, it is believed that such impurity removal will ultimately lead to an increase in metal (e.g., lithium, lithium carbonate, lithium sulfate) yield. According to one or more embodiments, the methods utilize solvent extraction to remove the calcium and / or magnesium impurities.

[0043] In one or more embodiments, a solvent extraction system suitable for use in the selective isolation of a metal (e.g., calcium, magnesium) may be comprised of a dynamic system of extraction, scrubbing, and stripping stages. The solvent extraction stage receives an aqueous solution and combines it with an organic solution containing a target metal (e g., calcium and / or magnesium) selective extractant. Extraction stages are suitable to extract the target metal (e.g., lithium, lithium ions, lithium salts, etc.) from the metal containing aqueous feed solution. Scrubbing stages are suitable to reduce transfer of aqueous entrainment and impurities. Stripping stages are suitable to concentrate the metal with the desired counterion.

[0044] Depending on the pH of the metal containing aqueous solution and the pH at which the target metal (e g., calcium and / or magnesium) is extracted, and based on the pH isotherm of the metal selective extractant reagent (R), the reaction will proceed according to Equation 1. If enough acid is produced to stop the extraction, additional base can be added to maintain the extraction reaction. Stripping is accomplished by using a large excess of acid to push the equilibrium far to the right as in aqueous Equation 2. The anion counterion to the magnesium can be chloride or sulfate and is equivalent on the respective sides of the extraction and strip equations. Calcium may be substituted for magnesium in Equations 1 and 2.(R')2Mg2+- 2 H ^ 2 RH + [Mg2+] Eq. 2

[0045] Suitable solvent extraction reagents for extracting alkaline earth metals, such as magnesium and calcium, may have either anionic or neutral functional groups. The neutral reagents need to have a substantial dipole moment for their functional groups. Therefore, the more negative the functional group the more aggressively the attraction to cations. The charged extractants are those that are activated by removing a proton as in Equation 1, which leads to a fixed negative charge. The pKa at which this occurs is different for each extractant and isdependent on the acidity of the proton being abstracted. This is affected by the stability of the metal complex. Notably, the extractant does not have a specific pKa, such as is found in acid / base reactions with organic molecules. The one or more metals being extracted will affect how easily the proton is removed. The pH at which the extractant is activated for an ion is dependent on the complex being formed.

[0046] Solvent extraction works on the mass transfer of metals across the organic / aqueous interface. Increasing that interfacial surface area also increases the rate at which one or more target metals is transferred. This is because the extractant and the one or more metals being extracted must come into contact at the interface. An increased surface area is produced by breaking the initial interface and then breaking the droplets produced by the mixer. The continuous shearing of droplets results in smaller droplets and a shift of the distribution of droplet size. By increasing the shear of the impeller and increasing the speed of the mixer, the surface area of the emulsion will increase. In solvent extraction systems, there is a continuous phase where all the solution is contiguous and a droplet phase. The continuous phase is often the phase with the greater volume in the mixer (e.g., if the aqueous volume is in excess, it is often the case that the aqueous will be the continuous phase and the organic will be mostly composed of organic droplets).

[0047] Solvent extraction is agnostic to the metal containing aqueous solution being used; any aqueous solution that has a high content of standard salts may be used. This solution can come from natural sources or can be the result of recycling streams or produced water. The organic solution contains organic compounds that target the selective extraction of the desired one or more metals, over other metals in the solution. Therefore, so long as the extractant molecules are sufficiently selective, the contents of the metal containing aqueous solution are less impactful on the process.

[0048] When the organic and aqueous solutions are mixed, an emulsion forms. This dramatic increase in surface area increases the transfer rate of the one or more metals (e.g., magnesium ions, calcium ions, etc.) from the aqueous phase to the extractant in the organic. The extraction can be completed in less than 1 minute. The phases are then allowed to coalesce. The aqueous phase, mostly depleted of calcium and / or magnesium can be sent back to an industrial process or returned to the environment. The organic phase may be washed in the scrubbing stage and sent to stripping where the one or more metals may be removed from the organic. This can happen in one of two ways. Some extractants are activated for extraction and deactivated for stripping by adjusting pH and some are loaded. Some extractants can be stripped with water on an equilibrium basis. The stripped organic can then be sent back to the extraction stages to repeat the process.

[0049] To have a selective reagent for solvent extraction, the structure of the extractant molecule is synthesized to match the most preferred bonding for the desired one or more metals (e.g., calcium ions, magnesium ions, etc.). These chemical compounds can be formulated in a solvent, and different structures can be used depending on the conditions of the metal containing aqueous solution. For example, if the metal containing aqueous solution has a high pH, it might require a specific extractant structure. It is possible to optimize the efficiency of lithium recovery downstream by designing an appropriate the extractant structure. Higher recoveries are possible when impurity metals, such as calcium and magnesium, are removed by solvent extraction upstream.

[0050] During the solvent extraction processes according to embodiments herein, a calcium and / or magnesium selective reagent is employed to separate such impurities from the metal (e.g., lithium) containing aqueous stream and / or product stream. Suitable reagent compositions include a calcium and / or magnesium selective extractant. In some embodiments, the reagent compositionsmay further include a modifier to stabilize the magnesium and calcium complexes formed with the extractant.

[0051] FIG. 4 shows an embodiment of a system 400 for extracting magnesium and / or calcium impurities from a lithium containing aqueous feed 402 using a solvent extraction system. An organic reagent having a high selectivity for magnesium and / or calcium over lithium and any other metals in the solution is used as the extractant in the organic phase. In various embodiments, the separation of magnesium and / or calcium from lithium can be achieved using ion exchange, electrodialysis, solvent extraction, adsorption techniques and / or combinations thereof. In particular, solvent extraction is capable of purifying the feed in a single simple step.

[0052] The solvent extraction system 404 is suitable to remove magnesium and / or calcium from the aqueous feed solution to trace amounts in the aqueous raffinate exiting system 404 without the loss of lithium beyond possible trace amounts. Relying on solvent extraction to remove the magnesium and / or calcium from the aqueous solution may eliminate the need for multiple other difficult steps, any one of which may also entrap lithium, thereby minimizing lithium losses in the process. The compositions, systems and methods according to embodiments herein combine a separation process according to various embodiments (e.g., solvent extraction) together with a magnesium and calcium selective composition to separate these impurities from a lithium product stream. Solvent extraction processes may also include a stripping step to recover the magnesium and / or calcium contained in the complexes formed with the reagent composition. In some embodiments, the purified lithium stream exiting the separation process 404 is fed to a boron solvent exchange process to further remove boric acid and the resulting lithium product stream may then be fed to a lithium recovery plant (e.g., lithium carbonate processing).

[0053] Reagent compositions according to embodiments herein are selective for magnesium and / or calcium and are suitable for operation at a variety of pH ranges depending on the needs of the particular processing plant. Isotherm charts for magnesium and / or calcium extraction using reagent compositions as described herein that are selective for magnesium and calcium are shown in FIGs. 5-8. FIG. 5 shows the percent extraction of magnesium and calcium at constant temperature as a function of pH where the pH was greater than 5. FIG. 6 shows the percent extraction of magnesium and calcium at constant temperature as a function of pH where the pH was greater than 6. FIG. 7 shows the percent extraction of magnesium and calcium at constant temperature as a function of pH where the pH was greater than 9. FIG. 8 shows the percent extraction of magnesium and calcium at constant temperature as a function of pH where the pH was greater than 10. Although the magnesium and calcium selective extractants can extract lithium, the lithium extraction occurs a pH higher than that for magnesium and calcium extraction. The compositions, systems and methods, thus, are suitable to selectively extract the magnesium and calcium impurities from the aqueous lithium-containing solution.

[0054] According to various embodiments, the extracted impurities comprising magnesium and calcium may be selectively extract and isolated using a solvent extraction process as shown in FIGs. 9 and 10. FIG. 9 shows a solvent extraction system 900 suitable for selectively removing magnesium and / or calcium impurities from an aqueous solution containing lithium (e.g., a lithium product stream). The aqueous feed solution containing lithium, magnesium and calcium (among other metals) 902 contacts a reagent composition containing a magnesium and / or calcium selective reagent in the extraction system 904. Magnesium and / or calcium are extract from the aqueous phase into the organic phase in accordance with Equations 1 and 2 set forth above.

[0055] The magnesium and / or calcium depleted aqueous solution is returned to combine with the metal containing aqueous solution feed 908 and reused for subsequent processing. The magnesium and calcium rich organic stream (i.e., loaded organic after the extractant forms complexes with the Mg and / or Ca) 910 flows to a stripping process 912. During stripping, the magnesium and calcium components are removed to provide a free a reagent composition 914 (i.e., barren organic) that is returned to the extraction process 904. The stripped magnesium and calcium 916 are sent to a purification system 918 to remove the Mg and Ca and generate a fresh strip solution 920.

[0056] In FIG. 10, another embodiment of a solvent extraction and stripping system 1000 is shown. In this system 1000, an extraction circuit 1002 and a strip circuit 1004 are provided. An aqueous feed 1006 (e.g., a lithium product solution) flows into a mixer system 1008 of the extraction circuit 1002 wherein it is combined with a barren organic solution 1010. The extraction circuit 1002 further includes extraction settlers 1012. A raffinate 1014 exits the extraction settlers 1012 and a loaded organic solution 1016 flows into a mixer system 1018 of the strip circuit 1004. Loaded organic solution 1016 combines with the poor electrolyte 1020 of concentration cell 1022. The effluent 1026 from a strip settler 1024 flows into concentration cell 1022 which ultimately produces a further processed lithium product stream 1028.

[0057] Further described herein are methods of removing impurities such as divalents (e.g., calcium, magnesium, etc.) from an aqueous solution containing lithium. In one or more embodiments, methods include contacting the aqueous solution with a reagent composition that selectively extracts the impurities over the lithium; and forming an impurity depleted lithium aqueous solution and an impurity rich organic solution. In various embodiments as described herein, the aqueous solution is a brine, a lithium product stream, a stream exiting a direct lithium extraction process, a purified and concentrated brine, a stream existing a pond system, feed streamto a lithium recovery plant, and / or combinations thereof. In one or more embodiments, the aqueous feed solution includes lithium in an amount of about 200 ppmw to about 65,000 ppmw, or any individual value or sub-range within this range. In various embodiments, the aqueous solution further includes sodium, potassium, magnesium, calcium, chlorine, sulfate, boron or combinations thereof.

[0058] In one or more embodiments, the aqueous feed solution has a weight ratio of magnesium to lithium of about 50: 1 to about 1 :50, about 1 : 1 to about 20:1, or any individual value or subrange within these ranges. In various embodiments, the aqueous feed solution has a weight ratio of calcium to lithium of about 50: 1 to about 1 :50, about 1 : 1 to about 20: 1, or any individual value or sub-range within these ranges.

[0059] Methods for removing impurities from the aqueous solutions include contacting the solution with a reagent composition in a solvent extraction system. In various embodiments, suitable reagent compositions contain about 5% to about 100% of a calcium and / or magnesium selective organic extractant, or any individual value or sub-range within this range. The reagent composition comprises an impurity selective extractant in an amount of about 0.025 M to about 3 M, about 0.05 M to about 2 M, or about 0.1 to about 1 M, or any individual value or sub-range within these ranges. Extractants according to embodiments herein are selective for divalents such as calcium and / or magnesium over lithium. As such, the divalents are removed from the aqueous solution, leaving a lithium-enriched aqueous solution as the product. Such purified lithium-rich aqueous solutions (e.g., containing LiCl, or other lithium salts) may be suitable for battery grade processing.

[0060] Suitable extractants include, but are not limited to, organic phosphoric acid-based extractants and organic phosphinic acid-based extractants. Suitable organic phosphoric acid-basedextractants include, but are not limited to, C1-C20 straight or branched alkyl phosphoric acids, Ci- C20 straight or branched dialkyl phosphoric acids, C2-C20 straight or branched alkenyl phosphoric acids, C2-C20 straight or branched dialkenyl phosphoric acids, or any individual compound within these definitions. In some embodiments, the phosphinic acid-based extractants are branched C3- C10 dialkyl phosphoric acids, or any individual compound within this definition. Suitable organic phosphinic acid-based extractants include, but are not limited to, C1-C20 straight or branched alkyl phosphinic acids, C1-C20 straight or branched dialkyl phosphinic acids, C2-C20 straight or branched alkenyl phosphinic acids, C2-C20 straight or branched dialkenyl phosphinic acids, or any individual compound within these definitions. In some embodiments, the phosphinic acid-based extractants are branched C3-C10 dialkyl phosphinic acids, or any individual compound within this definition.

[0061] The reagent compositions may further include an organic solvent. Suitable organic solvents include, but are not limited to, an aliphatic hydrocarbon, aromatic hydrocarbon, amine, ester, ether, ketone, nitrated or chlorinated hydrocarbon, or combinations thereof. In some embodiments, the organic solvent contains kerosene, hexane, toluene, dichloromethane, diethyl ether, acetone, chloroform, petroleum distillates, hydrotreated light, and / or combinations thereof. The reagent composition may contain the organic solvent in amount of greater than 0 wt% to about 95 wt%, based on the total weight of the reagent composition, or any individual value or sub-range within this range.

[0062] In one or more embodiments, the reagent composition may further include a modifier. Some of the aforementioned organic solvents are suitable modifiers. Suitable modifiers include, but are not limited to, 1,6-di-t-butoxy hexane, N,N-dimethyldecanamide, di(ethylene glycol) dibutyl ether, N,N-dimethyldecanamide, N,N-diethyldodecanamide, N,N-diethyl-2-ethyl hexanamide, 1,4-bis-t-butoxy butane, 2-ethylhexyl succinimide, 4-t-butylcyclohexanone,industrial denatured alcohol, dodecanol, 2,2,4-trimethyl-l,3-pentanediol di isobutyrate, isotridecyl alcohol, cydecanol, 7-ethyl-2-methyl-undecanol, trimethyl nonanol, 4-isopropyl cyclohexanone, t-butyl octyl ether, and / or combinations thereof.

[0063] Methods according to embodiments herein may further include a stripping process to process the impurity rich organic stream. The impurity rich organic stream is stripped of the impurities to form a fresh reagent composition and a concentrated impurity solution. The fresh reagent composition may then be recycled to the solvent extraction process for further processing. In some embodiments, the concentrated impurity solution flows to a purification process to remove the impurities and form a fresh strip solution. The fresh strip solution may be returned to the stripping process. In various embodiments, the methods include extracting boron from the impurity depleted lithium aqueous solution.

[0064] According to various embodiments, the methods of purifying the lithium-containing electrolyte include contacting the aqueous solution with the reagent composition in the solvent extraction system at a pH of greater than 5, of greater than 5 to about 6, of greater than 6, of greater than 6 to about 9, of greater than 9, of greater than 9 to about 10, of greater than 10, or of greater than 10 to about 12, of above 5 to about 12, or any individual value or sub-range within these ranges. Methods as described herein may further include separating impurities from the aqueous solution using ion exchange, electrodialysis, a second solvent extraction process, adsorption techniques, or combinations thereof.

[0065] In some embodiments, the impurity depleted lithium aqueous solution comprises trace amounts (e.g., less than 10 ppm, or any individual value or sub-range within this range) of impurities. In embodiments, the lithium-rich electrolyte product has no detectable amount of the impurities. In some embodiments, the reagent composition extracts only trace amounts (e.g., lessthan 10 ppm, or any individual value or sub-range within this range) of lithium, less than trace amounts of lithium or no detectable amount of lithium.

[0066] According to various embodiments, the impurity depleted lithium aqueous solution is fed to a lithium recovery process. Suitable lithium recovery processes include, but are not limited to, lithium carbonate production processes. In one or more embodiments, the lithium yield from the lithium recovery process increases by about 1% to about 99%, about 2% to about 95%, about 5% to about 80%, about 10% to about 50%, or any individual value or sub-range within these ranges, when solvent extraction is used to produce a lithium-rich aqueous product stream containing reduced concentrations of divalents such as calcium and magnesium.

[0067] Further described herein are methods of removing impurities comprising magnesium, calcium, or both from an aqueous solution comprising lithium. Such methods include contacting the aqueous solution with a reagent composition as described herein that selectively extracts the impurities over the lithium. The methods may further include forming an impurity depleted lithium aqueous solution and an impurity rich organic solution.

[0068] In some embodiments, the method further includes removing the remaining impurities by precipitation, ion exchange, or a combination thereof. The removal of trace remaining divalents such as Ca and Mg may be accomplished with the addition of NaOH and / or Na2CO3. In some embodiments, removal of trace remaining Mg is by the addition of NaOH and of trace remaining Ca is by ion exchange. In some embodiments, an ion exchange process may be used to remove trace remaining Mg and Ca from the lithium-rich aqueous product stream.EXAMPLESExample 1

[0069] A magnesium removal circuit using feed brine was operated to selectively remove magnesium from a lithium containing aqueous solution. The reagent composition included a magnesium selective extractant and a complexation modifier. The extraction of magnesium, was accomplished in a continuous solvent extraction circuit where the configuration was lExlWxlS. The concentration of the extractant was about 0. IM. The flow rate was 1.5 mL / min and the organic to aqueous ratio was about 1.1 : 1. Lithium analysis error showed that the lithium was not lost to the magnesium extraction circuit. Calcium was also extracted from the brine.Table 1 - Magnesium, Calcium and Lithium concentrations in brine before and after solvent extractionExample 2

[0070] A pond concentrated brine containing a relatively high concentration of lithium was subjected to a process according to embodiments herein. As shown in Table 2, the Mg and Ca concentrations were significantly reduced by solvent extraction as shown by the comparison of the Brine / Feed and the Raffinate / Aqueous. The concentration of lithium was only slightly reduced by the solvent extraction process. Following the solvent extraction stage, the composition of the Raffinate / Aqueous stream was then suitable as a feed to a lithium carbonate or hydroxide production plant as the difficult and lithium yield loss inducing process steps of removing magnesium and calcium are now drastically reduced, altered or eliminated.

[0071] The remainder of the magnesium and calcium was removed by precipitating the small amount of magnesium remaining in the Raffinate / Aqueous with NaOH and the small amount of calcium with Na2C0.3 or by removing the Mg by NaOH precipitation and the Ca by ion exchange.Table 2 - Magnesium, Calcium and Lithium concentrations in brine before and after solvent extraction, precipitation and ion exchangeExample 3

[0072] Magnesium and calcium (i.e., divalents) were reduced in a lithium containing aqueous brine using a solvent extraction process to produce a rich electrolyte (RE) product containing lithium chloride. The target concentrations were less than 1 ppm magnesium and less than 5 ppm calcium in a 25 g / L lithium-rich electrolyte solution suitable for making battery grade lithium carbonate. In a static test, an aqueous solution was contacted multiple times to selectively remove divalents such as calcium and magnesium while monitoring the loss, if any, of lithium (e.g., lithium salts).

[0073] A divalent selective extractant was contacted at a 1 : 1 ratio with a produced strip solution at varying pH to determine at what separation the divalents were selectively extracted with minimal loss of lithium. Fifty (50) ml of an old strip solution was contacted with 50 ml of the divalent selective extractant, in a standard solvent extraction mixing vessel at a standard tip speed. The pHwas adjusted using a solution of NaOH to 10.5. The organic was stripped and the feed recontacted three times in the mixing vessel. The results are shown in Table 3.Table 3 - Composition of the feed and rich electrolyte following solvent extraction

[0074] The results demonstrate that in a static test, it was possible to reduce the Ca and Mg concentrations. However, there may be a limit to the amount of hardness that can be removed in the static test. The extracted lithium was not of major concern as the lithium losses were limited by the extractive capability of the reagent.Example 4

[0075] The brine as in Example 3 was evaluated in a continuous solvent extraction process configured to remove the divalents magnesium and calcium from a rich electrolyte (RE). The solvent extraction circuit had three countercurrent extraction stages (El, E2, E3). The solvent extraction configuration included three counter current extraction stages using a 1 L / hr flow rate for all aqueous streams and a 1.3L / hr flow rate for all organic streams. Continuity of the organic composition was maintained during the extraction process. Operation was at ambient temperature and pH was controlled in the mixbox using NaOH solutions. The results are shown in Table 4.Table 4 - Concentrations of Mg and Ca in the rich electrolyte, extraction stages and stripping stage

[0076] The continuous solvent extraction circuit containing a calcium and magnesium selective reagent suitably reduced the concentrations of calcium and magnesium in the electrolyte.Example 5

[0077] A dynamic solvent extraction system was used to remove magnesium and calcium from a lithium-rich electrolyte received from a lithium solvent extraction plant to nearly undetectable levels. At such low concentrations, the resulting lithium-rich electrolyte was of suitable quality for battery grade processing.

[0078] A dynamic system 1100 having a first solvent extraction stage and a second solvent extraction stage was constructed and operated to remove calcium and magnesium from a lithium- rich aqueous feed 1115. A schematic of system 1100 is shown in FIG. 11. The lithium-rich electrolyte 1115 (e.g., from a lithium solvent extraction plant) was received by the multi-stage solvent extraction system 1100 and contained 28,000 ppm lithium, 5000 ppm Na, 100 ppm Mg and 50 ppm Ca.

[0079] The first solvent extraction stage utilized an organic reagent composition 1107 containing 5% alkyl phosphoric acid extractant and 5% organic phosphate 1120 combined with an organic diluent 1122 containing petroleum distillates, hydrotreated light (Oroform® SX-12). Pumps 1124 and 1126 were utilized to transfer the organic extractant 1120 and the diluent 1122 through lines 1114 and 1110, respectively. The extractant 1120 and diluent 1122 were combined at mixer 1101. After mixing, the reagent composition 1106 flowed from mixer 1101 into settler 1102. In mixer 1103, the lithium-rich electrolyte feed 1115 was contacted with the organic reagent composition1107 to selectively extract divalents such as calcium from the aqueous feed phase 11 15 and into the organic reagent composition phase. The mixture 1108 was transferred from mixing vessel 1103 into settler 1104 where the lithium rich aqueous phase 1116 separated from the organic phase 1109. The first solvent extraction stage was suitable for extracting high levels of calcium from the lithium-rich aqueous feed.

[0080] In the second solvent extraction stage, an organic reagent composition 1128 was prepared containing 5% alkyl phosphinic acid as the organic extractant 1130 in 5% of an organic diluent 1132 containing petroleum distillates, hydrotreated light (Oroform® SX-12). The feed to the second solvent extraction system was the raffinate 1116 from the first solvent extraction system. Pumps 1134 and 1136 were utilized to transfer the organic extractant 1130 and the diluent 1132 through lines 1111 and 1105, respectively. The extractant 1130 and diluent 1132 were combined at mixer 1105. After mixing, the reagent composition 1128 flowed from mixer 1105 into settler 1106. In mixer 1107, the lithium-rich electrolyte feed 1116 was contacted with the organic reagent composition 1128 to selectively extract divalents such as magnesium from the aqueous feed phase 1116 and into the organic reagent composition phase. The mixture 1136 was transferred from mixing vessel 1107 into settler 1108 where the lithium rich aqueous phase 1117 separated from the organic phase 1138. The second solvent extraction stage was suitable for extracting high levels of magnesium from the lithium-rich aqueous feed 1116.

[0081] A strip solution comprised of 1 8M HC1 was used to recover the extractants 1113, 1112 for reuse in the solvent extraction stages. The system produced a lithium-rich aqueous solution 1 117. Following extraction, the calcium was concentration in solution 1113 and the magnesium was concentrated in solution 1112.

[0082] The combined system was configured to have aqueous flows of 12 ml / min and organic flows of 12 ml / min. The mixer 1101, 1103, 1105, 1107 retention times were roughly 3-4 min and the settler 1102, 1104, 1106, 1108 times were 20-25 min. The pH was controlled at 9.0 in the first solvent extraction system and at 6.5 in the second solvent extraction system. The temperature was ambient at about 20°C. Solvent extraction system 1100 was operated for several days and samples were taken at various times from streams 1112, 1113, 1115, 1116 and 1117. These samples were analyzed using inductively coupled plasma mass spectrometry. The results are shown in Table 5.Table 5 - Concentrations of metals in the collected samples

[0083] As shown in Table 5, the initial feed 1115 had a magnesium concentration of about 100 ppm and a calcium concentration of about 50 ppm. After being processed, the lithium-rich aqueousproduct had a reduced magnesium concentration of 0 ppm and a reduced calcium concentration of 2 ppm.

[0084] The foregoing description discloses example embodiments of the disclosure. Modifications of the above-disclosed assemblies, apparatus, and methods which fall within the scope of the disclosure will be readily apparent to those of ordinary skill in the art. Accordingly, while the present disclosure has been disclosed in connection with example embodiments, it should be understood that other embodiments may fall within the scope of the disclosure, as defined by the following claims.

[0085] Although the subject matter has been described in language specific to structural features and / or methodological acts, it is to be understood that the subject matter defined in the appended claims is not necessarily limited to the specific features or acts described above. Rather, the specific features and acts described above are disclosed as example forms of implementing the claims.

Claims

CLAIMSWhat is claimed is:

1. A method of removing impurities comprising magnesium, calcium, or both from an aqueous solution comprising lithium, the method comprising: contacting the aqueous solution with a reagent composition that selectively extracts the impurities over the lithium; and forming an impurity depleted lithium aqueous solution and an impurity rich organic solution.

2. The method of claim 1, wherein the aqueous solution comprises a brine, a lithium product stream, a stream exiting a direct lithium extraction process, a purified and concentrated brine, a stream existing a pond system, feed stream to a lithium recovery plant, or combinations thereof.

3. The method of claim 1 or 2, wherein the aqueous solution comprises lithium in an amount of about 200 ppmw to about 65,000 ppmw and further comprises sodium, potassium, magnesium, calcium, chlorine, sulfate, boron or combinations thereof.

4. The method of any preceding claim, wherein the aqueous solution comprises a weight ratio of magnesium to lithium of about 50: 1 to about 1 :50, about 1 : 1 to about 20:1, or any individual value or sub-range within these ranges, and / orwherein the aqueous solution comprises a weight ratio of calcium to lithium of about 50: 1 to about 1 :50, about 1 : 1 to about 20: 1, or any individual value or sub-range within these ranges.

5. The method of any preceding claim, wherein contacting the aqueous solution with the reagent composition is in a solvent extraction system.

6. The method of any preceding claim, wherein the reagent composition comprises an extractant that is selective for the impurities over lithium.

7. The method of any preceding claim, wherein the reagent composition further comprises a modifier.

8. The method of any preceding claim, further comprising stripping in a stripping process the impurity rich organic stream of the impurities to form a fresh reagent composition and a concentrated impurity solution.

9. The method of claim 8, wherein contacting the aqueous solution with a reagent composition is in an extraction process of a solvent extraction system, the method further comprising returning the fresh reagent composition to the extraction process for contacting with the aqueous solution.

10. The method of claim 9, wherein the concentrated impurity solution flows to a purification process to remove the impurities and form a fresh strip solution.

11. The method of claim 10, further comprising returning the fresh strip solution to the stripping process.

12. The method of any preceding claim, further comprising extracting boron from the impurity depleted lithium aqueous solution.

13. The method of any preceding claim, wherein contacting the aqueous solution with the reagent composition is: at a pH of greater than 5, or greater than 5 to about 6, at a pH of greater than 6, or greater than 6 to about 9, at a pH of greater than 9, or greater than 9 to about 10, or at a pH of greater than 10, or greater than 10 to about 12.

14. The method of any preceding claim, wherein the impurity depleted lithium aqueous solution comprises trace amounts of the impurities, less than trace amounts of the impurities or no detectable amount of the impurities.

15. The method of any preceding claim, wherein the reagent composition extracts only trace amounts of lithium, less than trace amounts of lithium or no detectable amount of lithium.

16. The method of any preceding claim, wherein the impurity depleted lithium aqueous solution is fed to a lithium recovery process.

17. The method of claim 14, wherein lithium yield from the lithium recovery process increases by about 1% to about 99%, about 2% to about 95%, about 5% to about 80%, about 10% to about 50%, or any individual value or sub-range within these ranges.

18. The method of claim 14 or 15, wherein the lithium recovery process produces lithium carbonate.

19. The method of any preceding claim, further separating the impurities from the aqueous solution using ion exchange, electrodialysis, solvent extraction, adsorption techniques, or combinations thereof.

20. The method of any preceding claim, wherein the reagent composition comprises an impurity selective extractant in an amount of about 0.025 M to about 3 M, about 0.05 M to about 2 M, or about 0.1 to about 1 M.

21. A method of removing impurities comprising magnesium, calcium, or both from an aqueous solution comprising lithium, the method comprising: contacting the aqueous solution with a reagent composition that selectively extracts the impurities over the lithium; and forming an impurity depleted lithium aqueous solution and an impurity rich organic solution.

22. The method of any preceding claim, wherein the impurity depleted lithium aqueous solution comprises a reduced concentration of remaining impurities, the method further comprising removing the remaining impurities by precipitation, ion exchange, or a combination thereof.

23. The method of any preceding claim, further comprising addition of NaOH and Ca using Na2CO3.

24. The method of any preceding claim, followed by removal of trace remaining Mg by NaOH and Ca by Ion Exchange.

25. The method of any preceding claim, followed by removal of trace remaining Mg and Ca by Ion Exchange.

26. A system for removing impurities comprising magnesium, calcium, or both from an aqueous solution comprising lithium, the system comprising: a first solvent extraction stage configured to: receive the aqueous solution and contact the aqueous solution with a reagent composition that selectively extracts at least one of the impurities over the lithium; and form a first impurity depleted lithium aqueous solution and a first impurity rich organic solution.

27. The system of claim 26, further comprising a second solvent extraction stage configured to:receive the first impurity depleted lithium aqueous solution and contact the aqueous solution with a reagent composition that selectively extracts at least one of the impurities over the lithium; and form a second impurity depleted lithium aqueous solution and a second impurity rich organic solution.

28. The system of claim 26 or 27, wherein the first solvent extraction stage selectively extracts calcium.

29. The system of any one of claims 26 to 28 wherein the second solvent extraction stage selectively extracts magnesium.

Citation Information

Patent Citations

  • An extraction method for separating calcium and extracting lithium from low-temperature calcium-containing brine and its application.

    CN113061722B

  • Method for co-producing ultra-high-purity lithium salt and 6Li isotope and application thereof

    CN115646190A

  • Lithium or magnesium extraction processes

    WO2021231894A1