Modified molecular sieve-based solid electrolyte, preparation method therefor, and use thereof
By dispersing modified substances in molecular sieve-based solid electrolytes, changing the coordination environment of carriers, and improving their activity and migration capabilities, the problems of poor electrochemical performance and short cycle life of existing solid electrolytes in solid batteries are solved. Achieves high-performance and low-cost solid-state batteries.
Patent Information
- Application Number
- PCT/CN2023/117384
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-14
- Filing Date
- 2023-09-07
- Publication Date
- 2025-02-20
AI Technical Summary
The existing solid-state electrolytes face problems such as poor electrochemical performance, short cycle life and high cost when assembling solid-state batteries, which limit the application and development of solid-state energy storage systems.
Using modified molecular sieve-based solid electrolyte, by dispersing modified substances in the pore structure of molecular sieve-based solid electrolyte, the modified substances can have a coordination effect with carriers, change the coordination environment of carriers, and improve their activity and migration. ability.
Modified molecular sieve-based solid electrolytes significantly improve the electrochemical performance of solid-state batteries, extend the cycle life, and reduce costs, achieving a superior electrochemical performance with the use of organic electrolyte batteries.
Smart Images

Figure CN2023117384_20022025_PF_FP_ABST
Abstract
Description
A modified molecular sieve-based solid electrolyte and its preparation method and application
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on August 14, 2023, with application number 202311013483.4 and invention name “A modified molecular sieve-based solid electrolyte, its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention relates to the field of solid-state energy storage technology, and in particular to a modified molecular sieve-based solid electrolyte and a preparation method and application thereof. Background Art
[0003] The development of high-performance secondary batteries is of great strategic significance in many aspects such as environmental protection and efficient energy utilization. Secondary battery systems usually use liquid electrolytes, which are prone to leakage and short circuits, which can lead to dangerous accidents such as battery combustion and explosion. The use of solid-state electrolytes can, to a certain extent, inhibit the formation of negative electrode dendrites to avoid short circuits and reduce the proportion of combustible materials in the battery. Therefore, batteries using solid-state electrolytes are safer than batteries using liquid electrolytes. However, solid-state batteries assembled using existing solid-state electrolytes usually face problems such as poor electrochemical performance, short cycle life and high cost, which seriously restrict the application and development of solid-state energy storage systems.
[0004] In comparison, molecular sieve-based solid electrolytes have a simple preparation process, low cost, high stability, and good application prospects. However, the ion conductivity and interfacial compatibility with positive and negative electrodes of existing molecular sieve-based solid electrolytes still need to be improved.
[0005] Summary of the Invention
[0006] The purpose of the present invention is to provide a modified molecular sieve-based solid electrolyte and its preparation method and application. The modified molecular sieve-based solid electrolyte can well meet the requirements of assembling all-solid-state batteries, so that the electrochemical performance of the all-solid-state batteries exceeds the electrochemical performance of batteries using organic electrolytes.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a modified molecular sieve-based solid electrolyte, comprising a molecular sieve-based solid electrolyte and a modifying substance dispersed in the pore structure of the molecular sieve-based solid electrolyte;
[0009] The modified substance can produce a coordination effect with the carriers in the molecular sieve-based solid electrolyte;
[0010] The modified substance contains one or more of nitrogen, oxygen and sulfur elements.
[0011] Preferably, the modifying substance is a nitrogen-oxygen double bond-containing compound, a carbon-oxygen double bond-containing compound, a sulfur-oxygen double bond-containing compound, a phosphorus-oxygen double bond-containing compound, a carbon-sulfur double bond-containing compound, or water.
[0012] Preferably, the modifying substance is a sulfonyl-containing metal salt and / or a sulfonyl-containing non-metal salt.
[0013] Preferably, the difference between the maximum window diameter of the pore structure of the molecular sieve-based solid electrolyte and the longest diameter of the modifying substance filled in the pore structure is ≤±1 nm.
[0014] Preferably, the volume ratio of the pore volume of the largest pores of the molecular sieve-based solid electrolyte to the volume of the modifying substance is 1:(0.1-0.7).
[0015] The present invention also provides a method for preparing the modified molecular sieve-based solid electrolyte described in the above technical solution, comprising the following steps:
[0016] The modified substance is dispersed and loaded in the pore structure of the molecular sieve-based solid electrolyte to obtain the modified molecular sieve-based solid electrolyte.
[0017] Preferably, the method of dispersing the load is vacuum impregnation, grinding or negative pressure adsorption.
[0018] Preferably, the temperature for dispersing the load is from room temperature to 350°C.
[0019] The present invention also provides the use of the modified molecular sieve-based solid electrolyte described in the above technical solution or the modified molecular sieve-based solid electrolyte prepared by the preparation method described in the above technical solution in energy storage devices.
[0020] Preferably, the energy storage device includes a primary battery, a secondary battery or a capacitor.
[0021] The present invention provides a modified molecular sieve-based solid electrolyte, comprising a molecular sieve-based solid electrolyte and a modifying substance dispersed in the pore structure of the molecular sieve-based solid electrolyte; the modifying substance is capable of generating a coordination effect with charge carriers in the molecular sieve-based solid electrolyte; and the modifying substance contains one or more of nitrogen, oxygen, and sulfur. The modifying substance is capable of generating a coordination effect with the charge carriers, thereby changing the coordination environment and solid solvation structure of the charge carrier cations in the molecular sieve-based solid electrolyte, reducing the constraint of the molecular sieve framework on the charge carrier cations, thereby maintaining a highly active and easily mobile state, and promoting smoother conduction in the bulk of the modified molecular sieve-based solid electrolyte and at the interfaces between the positive and negative electrodes and the solid electrolyte. The modified molecular sieve-based solid electrolyte of the present invention has a dense structure. When applied to solid-state metal-air batteries, it can effectively prevent the air at the positive electrode from corroding the metal negative electrode (such as active metals such as lithium and sodium) through the electrolyte. The modified molecular sieve-based solid electrolyte of the present invention has excellent chemical and electrochemical stability, is not prone to side reactions, and is conducive to the stable operation of high-activity systems such as light-assisted batteries and metal-air batteries. The modified molecular sieve-based solid electrolyte of the present invention can change the type of internal carrier cations through ion exchange and can be used in a variety of solid-state energy storage systems. The modified molecular sieve-based solid electrolyte of the present invention can be prepared into an ultra-thin film. The solid-state energy storage device using the modified molecular sieve-based solid electrolyte is light in weight, low in thickness, and has a higher energy density. The solid-state battery using the modified molecular sieve-based solid electrolyte of the present invention has excellent performance, operates stably under high current conditions, and has better performance than a liquid electrolyte battery. At the same time, the modified molecular sieve-based solid electrolyte of the present invention is environmentally friendly, has a short preparation cycle, and is low in cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] FIG1 is a SEM image of the solid electrolyte described in Example 5;
[0023] FIG2 is an energy dispersive X-ray spectrum of a cross section of the solid electrolyte described in Example 8;
[0024] FIG3 is a charge and discharge curve diagram of the solid-state sodium metal battery described in Example 9;
[0025] FIG4 is a cycle performance curve of the all-solid-state lithium-ion battery described in Example 4;
[0026] FIG5 shows the all-solid-state lithium-air battery of Example 5 at 0.2 A·g -1 Cyclic performance curves at current density of ;
[0027] FIG6 shows the all-solid-state lithium-air battery of Example 5 at 0.1-2 A·g -1 Rate performance curves at multiple current densities;
[0028] FIG. 7 shows the all-solid-state lithium-air battery of Comparative Example 1 at 0.5 A·g -1 Charge and discharge curves at current density of ;
[0029] FIG8 is a graph showing the all-solid-state lithium-air battery of Comparative Example 2 at 0.5 A·g -1 Charge and discharge curves at current density of ;
[0030] FIG9 is a graph showing the organic electrolyte solution of the lithium-air battery in Comparative Example 3 at 0.2 A·g -1 Cycling performance at current density. DETAILED DESCRIPTION
[0031] The present invention provides a modified molecular sieve-based solid electrolyte, comprising a molecular sieve-based solid electrolyte and a modifying substance dispersed in the pore structure of the molecular sieve-based solid electrolyte;
[0032] The modified substance can produce a coordination effect with the carriers in the molecular sieve-based solid electrolyte;
[0033] The modified substance contains one or more of nitrogen, oxygen and sulfur elements.
[0034] In the present invention, the type of the carrier is preferably lithium ion, sodium ion, magnesium ion, calcium ion, potassium ion, zinc ion, iron ion, aluminum ion or proton.
[0035] In the present invention, the modifying substance contains one or more of nitrogen, oxygen, and sulfur; more preferably, it is a nitrogen-oxygen double bond compound, a carbon-oxygen double bond compound, a sulfur-oxygen double bond compound, a phosphorus-oxygen double bond compound, a carbon-sulfur double bond compound, or water; further preferably, it is a sulfonyl-containing metal salt and / or a sulfonyl-containing non-metallic salt; most preferably, it is one or more of bis(trifluoromethanesulfonylimide)lithium, bis(trifluoromethanesulfonylimide)sodium, bis(trifluoromethanesulfonylimide)potassium, bis(trifluoromethanesulfonylimide)zinc, bis(trifluoromethanesulfonylimide)magnesium, 1-ethyl-3-methylimidazolinebis(trifluoromethylsulfonyl)imide, and 1-methyl-1-propylpiperidiniumbis(trifluoromethylsulfonyl)imide.
[0036] In the present invention, the difference between the maximum window diameter of the pore structure of the molecular sieve-based solid electrolyte and the longest diameter of the modifying material filled in the pore structure is preferably ≤±1nm, more preferably ≤±0.5nm. In the present invention, the structure of the molecular sieve-based solid electrolyte is preferably RHO, FAU, LTL, RWY, EMT, IWS, LTA, TSC or NAT. In the present invention, ion migration behavior can occur in the molecular sieve-based solid electrolyte.
[0037] In the present invention, the volume ratio of the pore volume of the largest pores of the molecular sieve-based solid electrolyte to the volume of the modifying substance is preferably 1:(0.1-0.7).
[0038] The present invention also provides a method for preparing the modified molecular sieve-based solid electrolyte described in the above technical solution, comprising the following steps:
[0039] The modified substance is dispersed and loaded in the pore structure of the molecular sieve-based solid electrolyte to obtain the modified molecular sieve-based solid electrolyte.
[0040] In the present invention, the molecular sieve-based solid electrolyte is preferably prepared by a preparation method well known to those skilled in the art. The preparation method of the molecular sieve-based solid electrolyte is preferably prepared with reference to the Chinese patent or paper "Chi, X. et al. A highly stable and flexible zeolite electrolyte solid-state Li-air battery. Nature 592,551-557 (2021)" with publication number CN112864456A. In the present invention, the molecular sieve-based solid electrolyte is preferably a molecular sieve-based solid electrolyte powder or a molecular sieve-based solid electrolyte membrane. When the molecular sieve-based solid electrolyte is a molecular sieve-based solid electrolyte powder, the modified molecular sieve-based solid electrolyte prepared is preferably pressed into a tablet and then applied.
[0041] In the present invention, the method for dispersing the load is preferably vacuum impregnation, grinding or negative pressure adsorption.
[0042] In the present invention, the temperature for dispersing the load is preferably room temperature to 350° C., more preferably 121 to 170° C. The present invention does not have any particular limitation on the process of vacuum impregnation, grinding or negative pressure adsorption, and any process well known to those skilled in the art can be used.
[0043] The present invention also provides the use of the modified molecular sieve-based solid electrolyte described in the above technical solution or the modified molecular sieve-based solid electrolyte prepared by the preparation method described in the above technical solution in energy storage devices.
[0044] In the present invention, the energy storage device preferably includes a primary battery, a secondary battery, or a capacitor. The present invention does not have any special restrictions on the type of the primary battery, secondary battery, or capacitor, and any type familiar to those skilled in the art can be used. In an embodiment of the present invention, the secondary battery is specifically an all-solid-state sodium metal battery, an all-solid-state sodium ion battery, an all-solid-state lithium metal battery, an all-solid-state lithium ion battery, an all-solid-state lithium-air battery, an all-solid-state zinc battery, or a quasi-solid-state magnesium metal battery.
[0045] The modified molecular sieve-based solid electrolyte, its preparation method and application provided by the present invention are described in detail below with reference to the following examples, but they should not be construed as limiting the scope of protection of the present invention.
[0046] Example 1
[0047] According to 4.0NaOH:0.3Cs2O:1.0Al2O3:6.0SiO2:0.5C 12 H 24 O6(18-crown ether-6):110H2O (molar ratio) to prepare reaction gel;
[0048] The reaction gel was heated at 120°C for 200 h using a seed crystal assisted method, and then washed and dried in sequence to obtain a membrane molecular sieve Na-RHO (molecular sieve window size is about The diameter of the supercage is approximately );
[0049] The membrane molecular sieve is subjected to ion exchange in a lithium chloride solution having a concentration of 2M to obtain an ion-exchanged membrane molecular sieve Li-RHO;
[0050] Under negative pressure, 0.2 mL of lithium-containing 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide (the longest diameter is about ) was dispersed in the pore structure of 1 g of molecular sieve (the dispersion temperature was 150 ° C and the time was 12 h) to obtain a film-like modified molecular sieve-based solid electrolyte;
[0051] Lithium iron phosphate active material, PVDF binder and acetylene black were mixed in a mass ratio of 8:1:1 to prepare a slurry;
[0052] The slurry was coated on the surface of the film-like modified molecular sieve-based solid electrolyte (active material loading was 3 mg cm -2 ), to obtain a positive electrode-modified molecular sieve-based solid electrolyte structure;
[0053] The lithium metal negative electrode was heated and then bonded to the positive electrode-modified molecular sieve-based solid electrolyte structure to form an all-solid-state lithium metal battery. The all-solid-state lithium metal battery was subjected to light-assisted charging and discharging under 500W xenon lamp irradiation.
[0054] Example 2
[0055] The reaction gel was prepared according to the ratio (molar ratio) of 4.7Na2O:1.0Al2O3:2.9SiO2:175H2O;
[0056] The reaction gel was heated at 100°C for 5 h using a seed-assisted method, and then washed and dried in sequence to obtain powdered molecular sieves and membrane molecular sieves Na-FAU (molecular sieve window size is approximately The diameter of the supercage is approximately );
[0057] Under negative pressure, 0.08 mL of sodium 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt (the longest diameter is about ) was dispersed in 1 g of molecular sieve (the dispersion temperature was 120° C. and the time was 24 h) to obtain a powdered modified molecular sieve-based solid electrolyte and a film-like modified molecular sieve-based solid electrolyte;
[0058] Sodium vanadium fluorophosphate active material, PVDF binder, acetylene black and powdered modified molecular sieve-based solid electrolyte were mixed in a mass ratio of 8:1:1:1 to prepare a slurry;
[0059] The slurry was coated on the upper and lower surfaces of the film-shaped modified molecular sieve-based solid electrolyte (active material loading was 3 mg cm -2 ), assembled into an all-solid-state sodium-ion battery.
[0060] Example 3
[0061] The reaction gel was prepared according to the ratio (molar ratio) of 10.2Na2O:1.0Al2O3:6.2SiO2:210H2O;
[0062] The reaction gel was heated at 70°C for 6 h and then at 95°C for 7 h to obtain powdered molecular sieve Na-FAU (molecular sieve window size is approximately The diameter of the supercage is approximately );
[0063] The powdered molecular sieve is ion exchanged in a lithium chloride solution having a concentration of 1 M to obtain an ion-exchanged powdered molecular sieve Li-FAU;
[0064] 0.1 mL of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide (the longest diameter is about ) and 1 g of powdered molecular sieve and ball milled to uniformly disperse the 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide in the pores of the powdered molecular sieve to obtain a powdered modified molecular sieve-based solid electrolyte;
[0065] Pressing the powdered modified molecular sieve-based solid electrolyte into sheets to obtain sheet-like modified molecular sieve-based solid electrolyte;
[0066] NCM-811 active material, PVDF binder, and Super P were mixed in a mass ratio of 7:2:1 to prepare a slurry;
[0067] The slurry was coated on the surface of the sheet-like modified molecular sieve-based solid electrolyte (active material loading was 4 mg cm -2 ), to obtain a positive electrode-modified molecular sieve-based solid electrolyte structure;
[0068] The metallic lithium negative electrode is heated and then bonded to the positive electrode-modified molecular sieve-based solid electrolyte structure to assemble an all-solid-state lithium metal battery.
[0069] Example 4
[0070] The reaction gel was prepared according to the ratio (molar ratio) of 3.5Na2O:1.0Al2O3:2.2SiO2:180H2O;
[0071] The reaction gel was heated at 95° C. for 5 h, and a film-like molecular sieve was prepared on the surface of the graphite negative electrode using a seed-assisted method, and a powdered molecular sieve (Na-FAU, with a window size of approximately The diameter of the supercage is approximately );
[0072] Ion exchange is performed on the membrane molecular sieve and the powdered molecular sieve in a 2M lithium chloride solution to obtain an ion-exchanged Li-FAU membrane molecular sieve;
[0073] By vacuum impregnation, 0.08 mL of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide (with the longest diameter of about 10.7) were mixed. ) is uniformly dispersed in the pores of 1 g of molecular sieve and dried to obtain a film-like and powder-like modified molecular sieve-based solid electrolyte;
[0074] Lithium cobalt oxide, PVDF binder, acetylene black, and powdered modified molecular sieve-based solid electrolyte were mixed in a mass ratio of 8:1:1:1 to prepare a slurry;
[0075] The slurry was coated on the surface of the film-like modified molecular sieve-based solid electrolyte on one side relative to the graphite negative electrode (active material loading was 8 mg cm -2 ), assembled into an all-solid-state lithium-ion battery.
[0076] Example 5
[0077] The reaction gel was prepared according to the ratio (molar ratio) of 3.5Na2O:1.0Al2O3:2.2SiO2:180H2O;
[0078] The reaction gel was heated at 95 ° C for 5 h, and a film-like molecular sieve Na-FAU (with a window size of approximately 100 nm) was grown on the carbon nanotube cathode (refer to Chi, X. et al. A highly stable and flexible zeolite electrolyte solid-state Li-air battery. Nature 592, 551-557, 2021) by a seed-assisted method. The diameter of the supercage is approximately );
[0079] The membrane molecular sieve is subjected to ion exchange in a 2M lithium chloride solution to obtain an ion-exchanged Li-FAU membrane molecular sieve;
[0080] By vacuum impregnation, 0.08 mL of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide (with the longest diameter of about 10.7) were mixed. ) is uniformly dispersed in the pores of 1 g of a membrane-like molecular sieve to obtain a membrane-like modified molecular sieve-based solid electrolyte;
[0081] The metallic lithium negative electrode is heated until softened and attached to the surface of the film-shaped modified molecular sieve-based solid electrolyte opposite to the carbon nanotube positive electrode to assemble an all-solid-state lithium-air battery, which is then allowed to stand in dry oxygen for 24 hours.
[0082] Example 6
[0083] The reaction gel was prepared according to the ratio (molar ratio) of 3.5Na2O:1.0Al2O3:2.2SiO2:190H2O;
[0084] The zinc negative electrode was placed in the reaction gel and heated at 95° C. for 6 h. A film-like molecular sieve Na-FAU (molecular sieve window size of about 100 nm) was grown on the zinc negative electrode. The diameter of the supercage is approximately );
[0085] performing ion exchange on the membrane molecular sieve in a 0.2M zinc chloride solution to obtain an ion-exchanged membrane molecular sieve;
[0086] Using the negative pressure adsorption method, 0.05 mL of water was evenly dispersed in the pores of 1 g of film-like molecular sieve to obtain a negative electrode-film-like modified molecular sieve-based solid electrolyte structure;
[0087] Prussian blue active material, PVDF binder and acetylene black were mixed in a mass ratio of 7:2:1 to prepare a slurry;
[0088] The slurry is coated on the other side of the surface of the film-shaped modified molecular sieve-based solid electrolyte relative to the zinc negative electrode, and an all-solid-state zinc battery is assembled and then packaged.
[0089] Example 7
[0090] The reaction gel was prepared according to the ratio (molar ratio) of 5.0Na2O:1.0Al2O3:5.2SiO2:185H2O;
[0091] The reaction gel was heated at 100°C for 7 h to obtain a membrane molecular sieve Na-FAU (with a window size of approximately The diameter of the supercage is approximately );
[0092] ion-exchange the membrane molecular sieve in a 0.2 M magnesium sulfate solution to obtain an ion-exchanged Mg-FAU membrane molecular sieve;
[0093] By vacuum impregnation, 0.1 mL of a mixture of 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide and N-butyl-N-methylpyrrolidinium bis(trifluoromethylsulfonyl)imide (the longest diameter is about 100 μm) was added. ) is uniformly dispersed in the pores of 1 g of a membrane-like molecular sieve to obtain a membrane-like modified molecular sieve-based solid electrolyte;
[0094] Nano-Mo6O8, PVDF binder (and acetylene black) were mixed in a mass ratio of 7:2:1 to prepare a slurry;
[0095] The slurry was coated on one side of the membrane-like modified molecular sieve-based solid electrolyte (active material loading was 3 mg cm -2 ), to obtain a positive electrode-modified molecular sieve-based solid electrolyte structure;
[0096] A small amount of ionic liquid electrolyte is dripped onto the surface of the metal magnesium negative electrode to infiltrate the interface between the negative electrode and the solid electrolyte, and is assembled with the positive electrode-modified molecular sieve-based solid electrolyte structure to form a quasi-solid-state magnesium metal battery.
[0097] Example 8
[0098] The reaction gel was prepared according to the ratio (molar ratio) of 3.3Na2O:1.0Al2O3:2.0SiO2:177H2O;
[0099] The reaction gel was heated at 100°C for 3 h, and a seed-assisted method was used to obtain membrane molecular sieves and powdered molecular sieves Na-LTA (with a window size of approximately The diameter of the supercage is approximately );
[0100] Using vacuum impregnation method, 0.2g sodium bis(trifluoromethylsulfonyl)imide (the longest diameter is about ) The prepared methanol solution is uniformly dispersed in the pores of 1 g of the membrane molecular sieve and the powdered molecular sieve to obtain a membrane modified molecular sieve-based solid electrolyte and a powdered modified molecular sieve-based solid electrolyte;
[0101] The sodium vanadium phosphate active material, the PVDF binder, the acetylene black and the powdered modified molecular sieve-based solid electrolyte were mixed in a mass ratio of 8:1:1:1 to prepare a slurry;
[0102] The slurry was coated on one side of the membrane-like modified molecular sieve-based solid electrolyte (active material loading was 4 mg cm -2 ), to obtain a positive electrode-modified molecular sieve-based solid electrolyte;
[0103] A layer of polymer sodium ion solid electrolyte is added between the metallic sodium negative electrode and the film-shaped modified molecular sieve-based solid electrolyte to assemble an all-solid-state sodium metal battery.
[0104] Example 9
[0105] The reaction gel was prepared according to the ratio (molar ratio) of 3.5Na2O:1.0Al2O3:2.2SiO2:180H2O;
[0106] The reaction gel was heated at 100°C for 5 h, and a seed-assisted method was used to obtain membrane molecular sieves and powdered molecular sieves Na-FAU (with a window size of approximately The diameter of the supercage is approximately );
[0107] Under negative pressure, a mixture of 0.07 mL of sodium bis(trifluoromethylsulfonyl)imide and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide (the longest diameter is about 100 mL) was added. ) were uniformly dispersed in the pores of 1 g of a membrane-like molecular sieve and a powdered molecular sieve, respectively, to obtain a membrane-like modified molecular sieve-based solid electrolyte and a powdered modified molecular sieve-based solid electrolyte;
[0108] The sodium vanadium phosphate active material, the PVDF binder, the acetylene black and the powdered modified molecular sieve-based solid electrolyte were mixed in a mass ratio of 8:1:1:1 to prepare a slurry;
[0109] The slurry was coated on one side of the membrane-like modified molecular sieve-based solid electrolyte (active material loading was 3 mg cm -2 ), to obtain a cathode-film-like modified molecular sieve-based solid electrolyte structure;
[0110] The sodium metal negative electrode is heated and bonded to the positive electrode-solid electrolyte structure to assemble an all-solid-state sodium metal battery.
[0111] Test Case
[0112] FIG1 is a SEM image of the solid electrolyte described in Example 5. As can be seen from FIG1 , the surface of the modified molecular sieve-based solid electrolyte is flat and uniform, and can form good contact with the electrode, forming an ideal interface structure; the crystals are tightly bonded to facilitate ion conduction; and there are no gaps, which can effectively prevent air from penetrating the solid electrolyte to corrode the negative electrode;
[0113] FIG2 is an energy dispersive X-ray spectrum of a cross-section of the solid electrolyte described in Example 8. As can be seen from FIG2 , the Na element is evenly distributed and rich in content, which is conducive to the construction of a high-conductivity solid electrolyte. In addition, the thickness of the film-shaped modified molecular sieve-based solid electrolyte is as low as 7 μm. Therefore, the solid electrolyte described in the present invention can be used to assemble a solid-state battery with a small mass and low thickness, and can achieve a higher energy density.
[0114] FIG3 is a charge and discharge curve diagram of the solid-state sodium metal battery described in Example 9. As can be seen from FIG3 , the capacity of the solid-state sodium metal battery hardly decays after multiple charge and discharge cycles. This indicates that the modified molecular sieve-based solid electrolyte of the present invention has good ion conductivity, ideal compatibility with the positive and negative interfaces, and excellent solid-state battery performance.
[0115] FIG4 is a cycle performance curve of the all-solid-state lithium-ion battery according to Example 4. As shown in FIG4 , the capacity retention rate of the all-solid-state lithium-ion battery is greater than 96% after 1000 cycles at a high current density of 1C.
[0116] FIG5 shows the all-solid-state lithium-air battery of Example 5 at 0.2 A·g -1 As shown in FIG5 , the discharge voltage of the all-solid-state lithium-air battery remains almost unchanged after 1000 cycles, and the battery has excellent cycle stability in an air environment.
[0117] FIG6 shows the all-solid-state lithium-air battery of Example 5 at 0.1-2 A·g -1 As shown in Figure 6, the solid-state battery using the modified molecular sieve-based solid electrolyte has excellent ion conductivity, and the assembled all-solid-state lithium-air battery has excellent rate performance and has very promising application prospects.
[0118] Comparative Example 1
[0119] Prepare the reaction mother solution according to the ratio (molar ratio) of 3.6Na2O:1.0Al2O3:2.4SiO2:178H2O;
[0120] placing the self-supporting carbon-based cathode in the reaction mother solution and heating it at 100° C. for 3 hours to grow a film-like molecular sieve on the carbon-based cathode;
[0121] performing ion exchange on the membrane molecular sieve in a lithium chloride solution to obtain an ion-exchanged membrane molecular sieve;
[0122] The metallic lithium negative electrode was heated to 330° C. and attached to the surface of the film-shaped modified molecular sieve-based solid electrolyte opposite to the carbon-based positive electrode. After assembling into an all-solid-state lithium-air battery, the battery was allowed to stand in dry oxygen for 24 hours.
[0123] The all-solid-state lithium-air battery was tested at 500 mA·g -1 The charge and discharge performance test was carried out in ambient air under the same conditions. The test results are shown in FIG7 . As can be seen from FIG7 , the all-solid-state lithium-air battery using the molecular sieve-based solid electrolyte (unmodified) has a large overpotential and poor battery performance.
[0124] Comparative Example 2
[0125] 6.097 g lithium carbonate, 2.550 g aluminum oxide, 15.693 g germanium oxide and 34.502 g ammonium dihydrogen phosphate were prepared by solid phase synthesis method. 1.5 Al 0.5 Ge 1.5 P3O 12 (LAGP) solid electrolyte;
[0126] CNT, 5% PVDF NMP solution and LAGP powder were fully mixed in a ratio of 1:20:50 to prepare a slurry;
[0127] The slurry was evenly applied to one side of the LAGP sheet and sintered at 705° C. under an argon atmosphere;
[0128] A metallic lithium negative electrode heated to soften is attached to the other surface of the lithium aluminum germanium phosphate solid electrolyte sheet to complete the assembly of the LAGP-based all-solid-state lithium-air battery;
[0129] The assembled all-solid-state lithium-air battery was placed in dry oxygen and allowed to stand for 24 hours.
[0130] The all-solid-state lithium-air battery was tested at 500 mA·g -1The charge and discharge performance test was carried out in ambient air under the same conditions. The test results are shown in FIG8 . Compared with the modified molecular sieve-based solid electrolyte described in the present invention, the preparation process of the lithium aluminum germanium phosphate solid electrolyte is complicated and the cost is high. The lithium aluminum germanium phosphate solid electrolyte is unstable to the metallic lithium negative electrode. The germanium element will be reduced by the metallic lithium, causing damage to the crystal structure. In addition, the mass transfer at the interface of the positive electrode structure of the all-solid-state lithium-air battery prepared by mechanical blending is difficult. As can be seen from FIG8 , the performance of the all-solid-state lithium-air battery is poor.
[0131] Comparative Example 3
[0132] The lithium-air battery with organic electrolyte assembled by carbon nanotube-based cathode, commercial lithium-air battery organic electrolyte (specifically 1M LiTFSI dissolved in TEGDME) and metal lithium anode was tested at 0.2A·g -1 The battery cycle performance test was carried out at a current density of , and the test results are shown in FIG9 . As can be seen from FIG9 , the cycle life of the lithium-air battery using the organic electrolyte is only 130 times (the discharge voltage is lower than 2 V, indicating battery failure), which is much lower than the cycle performance of the all-solid-state lithium-air battery using the modified molecular sieve-based solid electrolyte of the present invention.
[0133] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A modified molecular sieve-based solid electrolyte, characterized in that: It includes a molecular sieve-based solid electrolyte and a modified substance dispersed in the pore structure of the molecular sieve-based solid electrolyte; The modified substance can produce coordination effects with the carriers in the molecular sieve-based solid electrolyte; The modified substance contains one or more of nitrogen, oxygen and sulfur elements.
2. The modified molecular sieve-based solid electrolyte according to claim 1, characterized in that: The modified substance is a nitrogen-oxygen double bond-containing compound, a carbon-oxygen double bond-containing compound, a sulfur-oxygen double bond-containing compound, a phosphorus-oxygen double bond-containing compound, a carbon-sulfur double bond-containing compound or water.
3. The modified molecular sieve-based solid electrolyte according to claim 1 or 2, characterized in that: The modified substance is a sulfonyl-containing metal salt and / or a sulfonyl-containing non-metal salt.
4. The modified molecular sieve-based solid electrolyte according to claim 3, characterized in that: The modified substance is one or more of bis(trifluoromethanesulfonyl imide) lithium, bis(trifluoromethanesulfonyl imide) sodium, bis(trifluoromethanesulfonyl imide) potassium, bis(trifluoromethanesulfonyl imide) zinc, bis(trifluoromethanesulfonyl imide) magnesium, 1-ethyl-3-methylimidazoline bis(trifluoromethylsulfonyl) imide and 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl) imide.
5. The modified molecular sieve-based solid electrolyte according to claim 1, characterized in that: The difference between the maximum window diameter of the pore structure of the molecular sieve-based solid electrolyte and the longest diameter of the modified substance filled in the pore structure is ≤±1 nm.
6. The modified molecular sieve-based solid electrolyte according to claim 4 or 5, characterized in that: The volume ratio of the pore volume of the largest pores of the molecular sieve-based solid electrolyte to the volume of the modified substance is 1:(0.1-0.7).
7. The method for preparing a modified molecular sieve-based solid electrolyte according to any one of claims 1 to 6, characterized in that: The following steps are involved: The modified substance is dispersed and loaded in the pore structure of the molecular sieve-based solid electrolyte to obtain the modified molecular sieve-based solid electrolyte.
8. The preparation method according to claim 7, characterized in that: The method for dispersing the load is vacuum impregnation, grinding or negative pressure adsorption.
9. The preparation method according to claim 7 or 8, characterized in that: The temperature of the dispersed load is room temperature to 350°C.
10. Use of the modified molecular sieve-based solid electrolyte according to any one of claims 1 to 6 or the modified molecular sieve-based solid electrolyte prepared by the preparation method according to any one of claims 7 to 9 in energy storage devices.
11. The use according to claim 10, characterized in that The energy storage device includes a primary battery, a secondary battery or a capacitor.
12. The use according to claim 11, characterized in that The secondary battery is an all-solid-state sodium metal battery, an all-solid-state sodium ion battery, an all-solid-state lithium metal battery, an all-solid-state lithium ion battery, an all-solid-state lithium-air battery, an all-solid-state zinc battery or a quasi-solid-state magnesium metal battery.
Citation Information
Patent Citations
Lithium battery solid electrolyte based on MCM-41 molecular sieve solidified ionic liquid and preparation method thereof
CN111740154A
Molecular sieve supported sodium ion solid electrolyte and preparation method and application thereof
CN111755734A
Composite solid electrolyte and preparation method and application thereof
CN112599851A
Molecular sieve based solid electrolyte and preparation method thereof, and integrated solid electrolyte-electrode material
CN112864456A
Molecular sieve imidazole framework doped polymer solid electrolyte and preparation method thereof
CN114709475A
Cited By
Amine functionalized molecular sieve composite electrolyte membrane and preparation method and application thereof
CN120749222A