Medium-manganese wear-resistant steel, manufacturing method therefor, and steel product

By optimizing the composition ratio and preparation process of medium-manganese wear-resistant steel, the comprehensive performance problems of medium-manganese wear-resistant steel in terms of hardness, strength and plasticity have been solved, and the wear resistance and toughness in high-wear environments have been improved, reducing the failure risk and maintenance cost of equipment.

WO2026232820A1PCT designated stage Publication Date: 2026-11-12HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/143726
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2025-12-19
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing medium-manganese wear-resistant steels cannot simultaneously meet the comprehensive requirements for hardness, strength, and plasticity, leading to frequent premature wear and fracture failures under high wear and high stress environments, increasing equipment maintenance costs and reducing production efficiency.

Method used

By controlling the composition ratio of medium-manganese wear-resistant steel, adding appropriate amounts of C, Mn, Mo, V and Nb elements, and combining continuous casting, heating, hot rolling, cold rolling and tempering processes, the hardness, strength and plasticity of the steel are optimized, and medium-manganese wear-resistant steel with good comprehensive performance is prepared.

Benefits of technology

This technology achieves good plasticity while maintaining high strength and hardness in medium-manganese wear-resistant steel, thereby improving the service life and production efficiency of equipment and reducing equipment maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2025143726-APPB-I100001
    Figure PCTCN2025143726-APPB-I100001
  • Figure PCTCN2025143726-APPB-I100002
    Figure PCTCN2025143726-APPB-I100002
Patent Text Reader

Abstract

Disclosed in the present application are a medium-manganese wear-resistant steel, a manufacturing method therefor, and a steel product. The medium-manganese wear-resistant steel comprises the following components in percentage by mass: C 0.05%-0.22%, Si 0.18%-0.44%, Mn 6.4%-11.3%, Mo 0.3%-0.6%, Cr 0.2%-0.6%, V 0.13%-0.26%, Nb 0.07%-0.16%, S 0-0.01%, and P 0-0.008%, with the balance being Fe and unavoidable impurities. In the medium-manganese wear-resistant steel, the components are coordinated with each other by means of controlling the proportions of the components, and then an extremely thin medium-manganese wear-resistant steel having good overall performance in hardness, strength and plasticity is obtained on the basis of a cold rolling process.
Need to check novelty before this filing date? Find Prior Art

Description

Medium manganese wear-resistant steel and its preparation method, steel products Technical Field

[0001] This application belongs to the field of steel processing technology, and in particular relates to a medium-manganese wear-resistant steel, its preparation method, and steel products. Background Technology

[0002] Medium-manganese wear-resistant steel has attracted much attention due to its potential in wear-resistant applications. However, existing medium-manganese wear-resistant steel technologies struggle to simultaneously meet the comprehensive requirements for hardness, strength, and ductility. On one hand, increasing hardness and strength often involves increasing the content of hard phases such as carbides, but this significantly reduces the steel's ductility, making it prone to brittle fracture under impact or complex stress, thus limiting its application in conditions requiring high material toughness. On the other hand, focusing on improving ductility inevitably sacrifices hardness and strength, making it unable to effectively resist wear and shortening its service life. For example, in mining machinery and construction machinery, equipment components often operate in high-wear, high-stress environments. Existing medium-manganese wear-resistant steels, unable to balance hardness, strength, and ductility, frequently experience premature wear and fracture failures, increasing equipment maintenance costs and reducing production efficiency. Developing a new technology that can simultaneously optimize the hardness, strength, and ductility of medium-manganese wear-resistant steel is of significant practical importance and urgently needed. Summary of the Invention

[0003] In view of this, this application provides a medium-manganese wear-resistant steel with good comprehensive properties of hardness, strength and plasticity, and a method for preparing the same; further, it provides a steel product.

[0004] The first aspect of this application provides a medium-manganese wear-resistant steel, which, by mass percentage, comprises the following components: C 0.05%~0.22%, Si 0.18%~0.44%, Mn 6.4%~11.3%, Mo 0.3%~0.6%, Cr 0.2%~0.6%, V 0.13%~0.26%, Nb 0.07%~0.16%, S 0~0.01%, P 0~0.008%, with the remainder being Fe and unavoidable impurities.

[0005] In the aforementioned medium-manganese wear-resistant steel, by controlling the proportions of each component to achieve synergistic effects, a medium-manganese wear-resistant steel with good overall properties of hardness, strength, and plasticity is obtained. Specifically, in the above-mentioned medium-manganese wear-resistant steel, the C content is moderate, not exceeding 0.22%, the Mn content is moderate, ranging from 6.4% to 11.3%, and the addition of 0.3% to 0.6% Mo allows the steel to possess high strength and hardness while maintaining good plasticity after cold rolling. Simultaneously, the addition of trace amounts of V and Nb elements can achieve tempering precipitation, improving the plasticity of the steel while preventing a decrease in strength and hardness; thus, a medium-manganese wear-resistant steel with good hardness, strength, and plasticity can be obtained.

[0006] In some embodiments, medium-manganese wear-resistant steel is a plate.

[0007] In some embodiments, the thickness of the medium-manganese wear-resistant steel is 0.4 mm to 2.9 mm.

[0008] In some embodiments, medium-manganese wear-resistant steel meets at least one of the following conditions:

[0009] (1) The surface Brinell hardness of medium manganese wear-resistant steel is 390HBW~470HBW;

[0010] (2) The tensile strength of medium manganese wear-resistant steel is ≥1250MPa;

[0011] (3) The elongation after fracture of medium manganese wear-resistant steel, A50, is ≥7%;

[0012] (4) The average flatness of medium manganese wear-resistant steel is ≤2mm / m.

[0013] The second aspect of this application provides a method for preparing medium-manganese wear-resistant steel, comprising the following steps:

[0014] Molten steel is supplied according to the proportions of each component in the medium-manganese wear-resistant steel;

[0015] The molten steel is subjected to continuous casting, heating, hot rolling, cold rolling and tempering in sequence; the tempering temperature is 220℃~350℃ and the tempering time is 18min~36min.

[0016] In some embodiments, the continuous casting process conditions include at least one of the following:

[0017] (1) During the continuous casting process, the superheat of the molten steel is 10℃~20℃;

[0018] (2) The casting speed of continuous casting is 1.0 m / min to 1.5 m / min;

[0019] (3) The thickness of the billet prepared by continuous casting is 190mm~230mm and the width is 900mm~2080mm;

[0020] (4) During the continuous casting process, an acidic covering agent is used to cover the tundish.

[0021] In some embodiments, the heating step includes:

[0022] The billet, with a temperature of 560℃~820℃, is placed in a heating furnace and then heated to 1180~1250℃ at a heating rate of 1℃ / min~5℃ / min. After holding at this temperature for 20min~40min, it is removed from the furnace.

[0023] In some embodiments, the hot rolling step includes performing five passes of rough rolling and seven passes of finish rolling in sequence;

[0024] Preferably, the hot rolling meets at least one of the following conditions:

[0025] (1) The total reduction rate of rough rolling is ≥74%;

[0026] (2) The total reduction rate of finishing rolling is ≥86.9%;

[0027] (3) The exit temperature of the finishing mill is 860℃~950℃;

[0028] (4) The exit thickness of the finishing mill is 3mm~6mm.

[0029] In some embodiments, cold rolling satisfies at least one of the following conditions:

[0030] (1) The cold rolling process involves 3 to 4 passes of cold rolling;

[0031] (2) The exit thickness of cold rolling is 0.4mm~2.9mm.

[0032] This application provides a steel article comprising the medium-manganese wear-resistant steel provided in the first aspect, or the medium-manganese wear-resistant steel prepared by the preparation method provided in the second aspect. Detailed Implementation

[0033] To better understand the above-mentioned objectives, features, and advantages of this application, the solution of this application will be further described below. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be combined with each other.

[0034] Numerous specific details are set forth in the following description in order to provide a full understanding of this disclosure, but this application may also be implemented in other ways different from those described herein; obviously, the embodiments in the specification are only some embodiments of this application, and not all embodiments.

[0035] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60~120 and 80~110 are listed for a specific parameter, it is also expected that ranges of 60~110 and 80~120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1~3, 1~4, 1~5, 2~3, 2~4, and 2~5. In this application, unless otherwise stated, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0~5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0036] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.

[0037] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure of this application.

[0038] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0039] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.

[0040] Unless otherwise specified, this application uses conventional testing methods or testing methods recommended by the instrument.

[0041] Conventional wear-resistant steel plates are high-strength, high-hardness steel plates with martensite as the main matrix structure. The heat treatment process for conventional wear-resistant steel plates is generally quenching followed by tempering. However, when the hardness reaches 400 HBW or higher, the phase transformation stress during the quenching process can cause waviness in the wear-resistant steel plate. The more thin the steel plate, the greater the number and size of the waviness. Therefore, the production of extremely thin wear-resistant steel, especially plates with a thickness of <3mm, is extremely difficult, and conventional production processes cannot produce wear-resistant steel with a thickness of less than 3mm.

[0042] Research has shown that cold rolling of medium-manganese steel can simultaneously achieve extremely thin thickness, ultra-high strength, and good sheet shape. However, the plasticity of cold-rolled medium-manganese steel is unstable; continuous cold deformation causes an increase in the strength and hardness of the steel sheet, while decreasing its toughness and plasticity. Based on this, this application provides a medium-manganese wear-resistant steel with good comprehensive properties of hardness, strength, and plasticity, and its preparation method. Details are as follows:

[0043] medium manganese wear-resistant steel

[0044] One embodiment of this application provides a medium-manganese wear-resistant steel, which, by mass percentage, comprises the following components: C 0.05%~0.22%, Si 0.18%~0.44%, Mn 6.4%~11.3%, Mo 0.3%~0.6%, Cr 0.2%~0.6%, V 0.13%~0.26%, Nb 0.07%~0.16%, S 0~0.01%, P 0~0.008%, with the remainder being Fe and unavoidable impurities.

[0045] In the aforementioned medium-manganese wear-resistant steel, by controlling the proportions of each component to achieve synergistic effects, a medium-manganese wear-resistant steel with good overall properties of hardness, strength, and plasticity is obtained. Specifically, in the above-mentioned medium-manganese wear-resistant steel, the C content is moderate, not exceeding 0.22%, the Mn content is moderate, ranging from 6.4% to 11.3%, and the addition of 0.3% to 0.6% Mo allows the steel to possess high strength and hardness while maintaining good plasticity after cold rolling. Simultaneously, the addition of trace amounts of V and Nb elements can achieve tempering precipitation, improving the plasticity of the steel while preventing a decrease in strength and hardness; thus, a medium-manganese wear-resistant steel with good hardness, strength, and plasticity can be obtained.

[0046] As an example, the C content in medium manganese wear-resistant steel can be 0.05%, 0.1%, 0.12%, 0.14%, 0.15%, 0.16%, 0.18%, 0.19%, 0.20%, 0.21%, or 0.22%, or any value within the range formed by any two of the above point values ​​as endpoints.

[0047] As an example, the Si content in medium manganese wear-resistant steel can be 0.18%, 0.20%, 0.22%, 0.25%, 0.26%, 0.28%, 0.30%, 0.32%, 0.34%, 0.35%, 0.36%, 0.38%, 0.40%, 0.42%, or 0.44%, or any value within the range formed by any two of the above point values ​​as endpoints.

[0048] As an example, the Mn content in medium manganese wear-resistant steel can be 6.4%, 6.8%, 7.0%, 7.4%, 7.5%, 7.6%, 7.8%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, 10.5%, 11.0%, or 11.3%, or any value within the range formed by any two of the above point values ​​as endpoints.

[0049] As an example, the Mo content in medium manganese wear-resistant steel can be 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, or 0.6%, or any value within the range formed by any two of the above point values ​​as endpoints.

[0050] As an example, the Cr content in medium manganese wear-resistant steel can be 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, or 0.6%, or any value within the range formed by any two of the above point values ​​as endpoints.

[0051] As an example, the V content in medium manganese wear-resistant steel can be 0.13%, 0.15%, 0.16%, 0.18%, 0.20%, 0.22%, 0.24%, 0.25%, or 0.26%, or any value within the range formed by any two of the above point values ​​as endpoints.

[0052] As an example, the Nb content in medium manganese wear-resistant steel can be 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, or 0.16%, or any value within the range formed by any two of the above point values ​​as endpoints.

[0053] In some embodiments, medium-manganese wear-resistant steel is a plate.

[0054] In some embodiments, the thickness of the medium-manganese wear-resistant steel plate is 0.4 mm to 2.9 mm. Further, the thickness of the medium-manganese wear-resistant steel plate can be 0.4 mm, 0.5 mm, 0.8 mm, 1.0 mm, 1.2 mm, 1.5 mm, 1.8 mm, 2.0 mm, 2.2 mm, 2.5 mm, 2.8 mm, or 2.9 mm, or any value within the range formed by any two of the above point values ​​as endpoints.

[0055] In some embodiments, the average flatness of the medium-manganese wear-resistant steel plate is ≤2mm / m. Further, the average flatness of the medium-manganese wear-resistant steel plate is 0.2mm / m to 2mm / m.

[0056] In some embodiments, the surface Brinell hardness of medium-manganese wear-resistant steel is 390HBW~470HBW.

[0057] In some embodiments, the tensile strength of medium-manganese wear-resistant steel is ≥1250MPa; further, the tensile strength of medium-manganese wear-resistant steel is 1250MPa~1690MPa.

[0058] In some embodiments, the elongation after fracture (A50) of the medium-manganese wear-resistant steel is ≥7%; further, the elongation after fracture (A50) of the medium-manganese wear-resistant steel is 7%~26%.

[0059] Preparation method of medium manganese wear-resistant steel

[0060] In one embodiment, a method for preparing medium-manganese wear-resistant steel is provided, comprising the following steps S10 to S20.

[0061] S10. Provide molten steel according to the proportions of each component of medium manganese wear-resistant steel.

[0062] S20 involves sequentially casting, heating, hot rolling, cold rolling, and tempering of molten steel.

[0063] The tempering temperature is 220℃~350℃, and the tempering time is 18min~36min.

[0064] After the molten steel undergoes continuous casting, heating, hot rolling, cold rolling and tempering in sequence, its component elements and content remain basically unchanged. Therefore, the component ratio of each element in the molten steel provided in step S10 is the same as the component ratio of each element in the manganese wear-resistant steel in the finished product.

[0065] By continuously casting molten steel with a specific component ratio, a billet with a suitable shape can be obtained. Then, by combining hot rolling and cold rolling, extremely thin specifications, ultra-high strength, and good plate shape quality can be obtained. Then, low-temperature tempering is used to further improve the toughness and plasticity of the steel plate and obtain a suitable hardness range. This ensures that the extremely thin wear-resistant steel plate simultaneously obtains good wear resistance, excellent plate shape, and suitable strength and toughness, thereby improving the product qualification rate.

[0066] As an example, the tempering temperature can be 220℃, 230℃, 240℃, 250℃, 260℃, 270℃, 280℃, 290℃, 300℃, 310℃, 320℃, 33℃, 340℃, or 350℃, or any value within the range defined by any two of the above point values ​​as endpoints. Further, the tempering temperature is 220℃~280℃.

[0067] As an example, the tempering time can be 18 min, 20 min, 22 min, 25 min, 26 min, 28 min, 30 min, 32 min, 34 min, 35 min, or 36 min, or any value within the range formed by any two of the above point values ​​as endpoints. Further, the tempering time is 20 min to 36 min.

[0068] In some embodiments, step S10, which provides molten steel according to the composition ratio of medium-manganese wear-resistant steel, includes the following steps S11 to S14:

[0069] S11. Desulfurize the molten iron, control the sulfur content of the molten iron leaving the station to be ≤0.005%, and the cleanliness of the desulfurization slag to be ≥90%.

[0070] S12. The desulfurized molten iron is introduced into the converter, and manganese metal, ferrosilicon and ferrosilicon are added for deoxidation and alloying to obtain molten steel; then the steel is tapped; during the tapping process, argon gas is blown to stir and the temperature of the tapping argon station is controlled to be ≥1550℃.

[0071] In some embodiments, the manganese-containing metal may be at least one of low-carbon ferromanganese, low-carbon manganese, and metallic manganese.

[0072] In some embodiments, before tapping, slag washing is performed by adding 1.5 kg to 3.5 kg of slag washing material per ton of molten steel. Further, the slag washing material is a conventionally used slag washing material, including but not limited to lime.

[0073] S13. Perform LF refining for ≥50 min; then desulfurize; alloy by adding manganese, molybdenum alloy, vanadium alloy and niobium alloy.

[0074] It is understandable that in step S13, when alloying is carried out by adding metallic manganese, molybdenum alloy, vanadium alloy and niobium alloy, the content of Mn, Mo, V and Nb elements in the steel plate is controlled.

[0075] S14. Perform RH refining, add aluminum during the refining process, and quench after breaking the air; the quenching time is ≥8min.

[0076] In some embodiments, during step S20, when continuously casting molten steel, the superheat of the molten steel is 10°C to 20°C.

[0077] In some embodiments, when continuously casting molten steel, the billet pulling speed is 1.0 m / min to 1.5 m / min. By controlling the pulling speed, the internal structure of the cast billet is ensured to be uniform, and defects such as cracks are avoided.

[0078] In some embodiments, when continuously casting molten steel, the tundish may be covered with an acidic coating agent.

[0079] In some embodiments, when continuously casting molten steel, a high-manganese steel protective slag is used to protect the surface of the molten steel in the crystallizer. The high-manganese steel used is the conventional high-manganese steel used in the art.

[0080] In some embodiments, the heating step in step S20 includes:

[0081] The billet, initially heated to 560℃~820℃, is placed in a heating furnace and then heated to 1180~1250℃ at a rate of 1℃ / min~5℃ / min, holding for 20min~40min before removal from the furnace. Preheating the billet before hot rolling significantly improves its machinability. Heating increases the metal's plasticity, reduces deformation resistance, decreases the risk of rolling cracks, and lowers energy consumption. Uniform heating temperature ensures stable rolling, avoids poor sheet shape, and improves production efficiency. Simultaneously, high temperature heals internal defects in the billet, reduces compositional segregation, refines coarse as-cast grains, and creates conditions for subsequent dynamic recrystallization.

[0082] In some embodiments, the above preparation method further includes a high-pressure descaling step on the heated billet before the hot rolling step. Further, the high-pressure descaling can employ conventional high-pressure descaling methods in the art, including but not limited to impacting the surface of the high-temperature billet with high-pressure water (150~400 bar). High-pressure descaling removes the iron oxide scale from the billet surface, ensuring a smooth surface during subsequent rolling and preventing rolling defects from being pressed in.

[0083] In some embodiments, the hot rolling step S20 includes performing five passes of rough rolling and seven passes of finish rolling in sequence.

[0084] In some embodiments, the finishing mill exit temperature is 860°C to 950°C. The finishing mill exit temperature refers to the temperature of the hot-rolled steel strip obtained when finishing milling is completed.

[0085] In some embodiments, the total reduction rate of the roughing roll is ≥74%. Further, the total reduction rate of the roughing roll is 74%~82.6%.

[0086] In some embodiments, the total reduction rate of finishing rolling is ≥86.9%. Further, the total reduction rate of finishing rolling is 86.9%~95%.

[0087] In some embodiments, the exit thickness of the finishing mill is 3 mm to 6 mm. The exit thickness of the finishing mill refers to the thickness of the hot-rolled steel strip obtained when the finishing mill is completed.

[0088] In some embodiments, the above-described preparation method further includes the step of coiling the hot-rolled steel strip obtained after hot rolling. Coiling allows the steel strip to be formed into a hot-rolled steel coil, facilitating storage and transportation.

[0089] Furthermore, the coiling temperature is ≤200℃. The coiling temperature refers to the temperature of the hot-rolled steel strip during coiling. Further, the coiling temperature is 60℃~200℃.

[0090] In some embodiments, in step S20, the cold rolling step includes performing 3 to 4 passes of cold rolling on the steel strip to be processed; further, the cold rolling step includes performing 3 passes of cold rolling.

[0091] In some embodiments, the exit thickness of the cold-rolled strip is 0.4 mm to 2.9 mm. The exit thickness of the cold-rolled strip is the thickness of the cold-rolled steel strip obtained after cold rolling.

[0092] In some embodiments, a pickling step is included before the cold rolling step for the hot-rolled steel strip or hot-rolled steel coil. Pickling can remove impurities such as iron oxide scale that form on the surface of the steel strip after high-temperature hot rolling.

[0093] Furthermore, the pickling solution used during pickling is an aqueous solution of hydrochloric acid with a concentration of 70 g / L to 140 g / L.

[0094] Furthermore, the pickling temperature is 65℃~75℃.

[0095] Furthermore, the pickling speed is 35 m / min to 45 m / min.

[0096] In some embodiments, a leveling step of the hot-rolled steel coil is included before the pickling step. This leveling step is a conventional leveling step.

[0097] In some embodiments, the above preparation method further includes a step of cross-cutting and leveling the cold-rolled steel strip before tempering, thereby further improving the flatness of the steel strip.

[0098] steel products

[0099] In one embodiment, a steel product is provided, which includes the above-mentioned medium-manganese wear-resistant steel, or medium-manganese wear-resistant steel prepared according to the above-mentioned preparation method.

[0100] In some embodiments, the steel products mentioned above include, but are not limited to, crusher jaw plates, ball mill liners, bulldozer blades, and fan blades.

[0101] Example

[0102] The following embodiments describe the disclosure of this application in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on weight, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.

[0103] Example 1

[0104] The ultra-thin, medium-manganese wear-resistant steel plate provided in this embodiment has the following chemical composition by weight percentage: C 0.11%, Si 0.26%, Mn 8.6%, Mo 0.42%, Cr 0.44%, V 0.18%, Nb 0.10%, S 0.001%, P 0.007%, with the remainder being Fe and unavoidable impurities. The specific production steps are as follows:

[0105] (1) Desulfurization of molten iron: Desulfurize the molten iron, control the S content of the molten iron leaving the station to be 0.001%, and the cleanliness of the desulfurization slag to be 95%.

[0106] (2) Converter blowing: The desulfurized molten iron is introduced into the converter and low-carbon ferromanganese, metallic manganese, ferrosilicon and ferroaluminum are added for deoxidation and alloying treatment. Slag washing is carried out before tapping, and lime slag washing material is added at a ratio of 3 kg of slag washing material per ton of molten steel; then the steel is tapped, and argon gas is blown to stir during the tapping process, and the temperature of the argon station at the tapping is controlled at 1588℃.

[0107] (3) LF refining: The molten steel from the converter is introduced into the LF refining furnace to desulfurize it. Then, manganese, molybdenum alloy, vanadium alloy and niobium alloy are added to alloy the molten steel so that the element content in the melt meets the content of the target product. The LF refining time is controlled to be 56 min.

[0108] (4) RH refining: RH refining is carried out in an RH refining furnace, and 40 kg of aluminum is added during the RH refining process. The settling time after breaking the air is 11 min.

[0109] (5) Continuous casting: When continuous casting is carried out, acidic covering agent is used for the tundish and high manganese steel protective slag is used; the superheat of molten steel is controlled at 16℃ and the continuous casting speed is 1.2m / min to obtain a continuous casting slab with a thickness of 230mm and a width of 1250mm.

[0110] (6) Slab heating: Place the 620℃ continuous casting slab in the heating furnace, and then heat it to 1220℃ at a heating rate of 4℃ / min. After holding it at that temperature for 35 minutes, remove it from the furnace and then perform high-pressure descaling.

[0111] (7) Hot rolling and coiling: The slab after dephosphorization is subjected to 5 passes of rough rolling and 7 passes of finish rolling. The total reduction rate of rough rolling is controlled at 80%, the total reduction rate of finish rolling is controlled at 87%, and the exit temperature of finish rolling is 930℃ to obtain a hot-rolled coil with a thickness of 6mm; then it is cooled to 200℃ for coiling.

[0112] (8) Leveling: The hot-rolled coil is leveled.

[0113] (9) Pickling and cold rolling: The steel coil after leveling is pickled and cold rolled in three passes to obtain a cold-rolled steel strip with a thickness of 2.5 mm.

[0114] (10) Cross-cutting and leveling: Cross-cutting and leveling the cold-rolled steel strip.

[0115] (11) Tempering: The tempering temperature is controlled at 240℃ and the tempering time is 25min; medium manganese wear-resistant steel plate is obtained.

[0116] Examples 2-3

[0117] The preparation methods of Examples 2 and 3 are basically the same as those of Example 1, except that the chemical composition of the prepared steel plate and the tempering temperature and time are different, as detailed in Table 1 below.

[0118] Comparative Example 1

[0119] The ultra-thin, medium-manganese wear-resistant steel plate provided in this embodiment has the following chemical composition by weight percentage: C 0.26%, Si 0.27%, Mn 3.5%, Mo 0.32%, Cr 0.56%, V 0.15%, Nb 0.11%, S 0.001%, P 0.008%, with the remainder being Fe and unavoidable impurities. The specific production steps are as follows:

[0120] (1) Desulfurization of molten iron: Desulfurize the molten iron, control the S content of the molten iron leaving the station to be 0.001%, and the cleanliness of the desulfurization slag to be 94%.

[0121] (2) Converter blowing: The desulfurized molten iron is introduced into the converter and low-carbon ferromanganese, metallic manganese, ferrosilicon and ferroaluminum are added for deoxidation and alloying treatment. Before tapping, slag washing is carried out, and lime slag washing material is added at a ratio of 3 kg per ton of molten steel. Then the steel is tapped. Argon gas is blown to stir during the tapping process, and the temperature of the argon station at the tapping is controlled at 1579℃.

[0122] (3) LF refining: The molten steel from the converter is introduced into the LF refining furnace to desulfurize it. Then, manganese, molybdenum alloy, vanadium alloy and niobium alloy are added to alloy the molten steel so that the element content in the melt meets the content of the target product. The LF refining time is controlled to be 59 min.

[0123] (4) RH refining: RH refining is carried out, and 40 kg of aluminum is added during the RH refining process. After breaking the air, the calming time is 10 min.

[0124] (5) Continuous casting: When continuous casting is carried out, acidic covering agent is used for the tundish and high manganese steel protective slag is used; the superheat of molten steel is controlled at 20℃ and the continuous casting speed is 1.2m / min to obtain a continuous casting slab with a thickness of 230mm and a width of 1250mm.

[0125] (6) Slab heating: Place the 606℃ continuous casting slab in the heating furnace, and then heat it to 1216℃ at a heating rate of 3.5℃ / min. After holding it at that temperature for 30 minutes, remove it from the furnace and then perform high-pressure descaling.

[0126] (7) Hot rolling and coiling: The slab after dephosphorization is subjected to 5 passes of rough rolling and 7 passes of finish rolling. The total reduction rate of rough rolling is controlled at 80%, the total reduction rate of finish rolling is controlled at 87%, and the exit temperature of finish rolling is 910℃ to obtain a hot-rolled steel strip with a thickness of 6mm. Then it is cooled to 200℃ for coiling.

[0127] (8) Leveling: The hot-rolled coil is leveled.

[0128] (9) Pickling and cold rolling: The hot-rolled coil after leveling is pickled and cold-rolled in three passes to obtain a cold-rolled steel strip with a thickness of 2.5 mm.

[0129] (10) Cross-cutting and leveling: Cross-cutting and leveling the cold-rolled steel strip.

[0130] (11) Tempering: The tempering temperature is controlled at 240℃ and the tempering time is 25min; medium manganese wear-resistant steel plate is obtained.

[0131] Comparative Example 2

[0132] The ultra-thin, medium-manganese wear-resistant steel plate provided in this embodiment has the following chemical composition by weight percentage: C 0.13%, Si 0.36%, Mn 9.8%, Mo 0.40%, Cr 0.39%, V 0.16%, Nb 0.11%, S 0.001%, P 0.006%, with the remainder being Fe and unavoidable impurities. The specific production steps are as follows:

[0133] (1) Desulfurization of molten iron: Desulfurize the molten iron obtained from blast furnace smelting, control the S content of the molten iron leaving the station to be 0.001%, and the cleanliness of the desulfurized slag to be 95%.

[0134] (2) Converter blowing: The desulfurized molten iron is introduced into the converter and low-carbon ferromanganese, metallic manganese, ferrosilicon and ferroaluminum are added for deoxidation and alloying treatment. Slag washing is carried out before tapping, and lime slag washing material is added at a ratio of 3 kg of slag washing material per ton of molten steel; then the steel is tapped, and argon gas is blown to stir during the tapping process, and the temperature of the argon station at the tapping is controlled at 1594℃.

[0135] (3) LF refining: The molten steel from the converter is introduced into the LF refining furnace to desulfurize it. Then, manganese, molybdenum alloy, vanadium alloy and niobium alloy are added to alloy the molten steel so that the element content in the melt meets the content of the target product. The LF refining time is controlled to be 58 min.

[0136] (4) RH refining: After LF refining is completed, the melt is introduced into the RH refining furnace for RH refining, and 40 kg of aluminum is added during the RH refining process. After breaking the air, the settling time is 12 min.

[0137] (5) Continuous casting: When continuous casting is carried out, acidic covering agent is used for the tundish and high manganese steel protective slag is used; the superheat of molten steel is controlled at 20℃ and the continuous casting speed is 1.2m / min to obtain a continuous casting slab with a thickness of 230mm and a width of 1250mm.

[0138] (6) Slab heating: When the continuous casting slab temperature is 598℃, it is placed in a heating furnace and then heated to 1205℃ at a heating rate of 3.5℃ / min. After holding at the temperature for 30 minutes, it is taken out of the furnace and then subjected to high-pressure descaling.

[0139] (7) Hot rolling and coiling: After high pressure descaling, the slab is subjected to 5 passes of rough rolling and 7 passes of finish rolling. The total reduction rate of rough rolling is controlled at 82.6%, the total reduction rate of finish rolling is 95%, and the exit temperature of finish rolling is 910℃ to obtain a hot-rolled steel strip with a thickness of 2mm. Then it is cooled to 200℃ and coiled.

[0140] (8) Leveling: The hot-rolled coil is leveled.

[0141] (9) Cross-cutting and leveling: The hot-rolled coil after leveling is cross-cut and leveled to obtain plate steel.

[0142] (10) Quenching: Quenching temperature 900℃, holding time 15min.

[0143] (11) Tempering: The tempering temperature is controlled at 240℃ and the tempering time is 25min; medium manganese wear-resistant steel plate is obtained.

[0144] Comparative Example 3

[0145] The preparation method of Comparative Example 3 is substantially the same as that of Example 1, with the only difference lying in the tempering temperature and tempering time; the tempering temperature of Comparative Example 3 is 360°C, and the tempering time is 8 minutes.

[0146] The component ratios and process conditions of the medium-manganese wear-resistant steel plates prepared in each Example and Comparative Example are shown in Table 1 below:

[0147] Table 1

[0148]

[0149] Performance Testing

[0150] Brinell hardness: The surface Brinell hardness of the medium-manganese wear-resistant steel plates prepared in each Example and Comparative Example is tested according to the method specified in GB / T 231.1-2018 "Metallic materials - Brinell hardness test - Part 1: Test method".

[0151] Tensile strength: The tensile strength of the medium-manganese wear-resistant steel plates prepared in each Example and Comparative Example is tested according to the method specified in GB / T 228.1-2021 "Metallic materials - Tensile testing - Part 1: Method of test at room temperature".

[0152] Elongation after fracture A50: The elongation after fracture A50 of the steel plates prepared in each Example and Comparative Example is tested according to the method specified in GB / T 228.1-2021 "Metallic materials - Tensile testing - Part 1: Method of test at room temperature".

[0153] Average flatness: The average flatness of the medium-manganese wear-resistant steel plates prepared in each Example and Comparative Example is tested according to the method specified in GB / T 709-2019 "Dimensions, shape, weight and permissible tolerances of hot-rolled steel plates and strips".

[0154] Wear resistance: The wear resistance of the medium-manganese wear-resistant steel plates prepared in each Example and Comparative Example is tested according to the method specified in ASTM G65-16 "Standard Test Method for Measuring Abrasion Using the Dry Sand / Rubber Wheel Apparatus".

[0155] The performance test data of the steel plates prepared in each Example and Comparative Example are shown in Table 2.

[0156] Table 2

[0157]

[0158] Note: A product is judged as qualified when its hardness reaches 390HBW to 470HBW, elongation is ≥7%, tensile strength is ≥1250MPa, and flatness is ≤3mm / m, and the qualification rate = weight of qualified products / total production volume.

[0159] The relative wear resistance in the table refers to the wear resistance relative to Q355 steel, where the wear resistance of Q355 steel is defined as 1.

[0160] According to Tables 1 and 2, the steel plates prepared by the technical solution of this application in Examples 1-3 all have high values ​​of surface Brinell hardness, tensile strength and elongation after fracture. This application provides comprehensive properties of hardness, strength and plasticity of steel plates.

[0161] The C content added in Comparative Example 1 is higher than the range of this application, and the Mn content is lower than the range of this application. Although the steel plate prepared by it has good hardness, its plasticity is poor, and it fails to improve the comprehensive performance of medium manganese wear-resistant steel plate. The material is unqualified.

[0162] In Comparative Example 2, during the preparation of medium-manganese wear-resistant steel plates, a quenching and tempering process was used. The phase transformation stress in the quenching process caused wavy patterns in the medium-manganese wear-resistant steel plates. As the thickness of the steel plate decreased, the number of wavy patterns increased and the wavy patterns became larger. This resulted in the average surface roughness of the 2mm thick medium-manganese wear-resistant steel plate reaching 35mm / m, thus reducing the quality of the medium-manganese wear-resistant steel plate.

[0163] In Comparative Example 3, when the medium manganese wear-resistant steel plate was prepared, tempering was carried out at a relatively high temperature, which significantly reduced the hardness and strength of the steel plate and reduced its wear resistance.

[0164] The above description is merely a specific implementation of this application. Those skilled in the art will clearly understand that, for the sake of convenience and brevity, the specific working processes of the systems, modules, and units described above can be referred to the corresponding processes in the foregoing method embodiments, and will not be repeated here. It should be understood that the protection scope of this application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and these modifications or substitutions should all be covered within the protection scope of this application.

Claims

1. A medium-manganese wear-resistant steel, characterized in that, The medium-manganese wear-resistant steel comprises the following components by mass percentage: C 0.05%~0.22%, Si 0.18%~0.44%, Mn 6.4%~11.3%, Mo 0.3%~0.6%, Cr 0.2%~0.6%, V 0.13%~0.26%, Nb 0.07%~0.16%, S 0~0.01%, P 0~0.008%, with the remainder being Fe and unavoidable impurities.

2. The medium-manganese wear-resistant steel according to claim 1, characterized in that, The medium-manganese wear-resistant steel is in the form of plates.

3. The medium-manganese wear-resistant steel according to claim 2, characterized in that, The thickness of the medium manganese wear-resistant steel is 0.4mm to 2.9mm.

4. The medium-manganese wear-resistant steel according to any one of claims 2 to 3, characterized in that, The medium-manganese wear-resistant steel meets at least one of the following conditions: (1) The surface Brinell hardness of the medium manganese wear-resistant steel is 390HBW~470HBW; (2) The tensile strength of the medium-manganese wear-resistant steel is ≥1250MPa; (3) The elongation after fracture of the medium-manganese wear-resistant steel, A50, is ≥7%; (4) The average flatness of the medium manganese wear-resistant steel is ≤2mm / m.

5. The method for preparing medium-manganese wear-resistant steel according to any one of claims 1 to 4, characterized in that, Includes the following steps: Molten steel is supplied according to the component proportions of the medium-manganese wear-resistant steel; The molten steel is subjected to continuous casting, heating, hot rolling, cold rolling and tempering in sequence; the tempering temperature is 220℃~350℃ and the tempering time is 18min~36min.

6. The method for preparing medium-manganese wear-resistant steel according to claim 5, characterized in that, The continuous casting process conditions include at least one of the following: (1) During the continuous casting process, the superheat of the molten steel is 10℃~20℃; (2) The casting speed of the continuous casting is 1.0 m / min to 1.5 m / min; (3) The thickness of the billet prepared by continuous casting is 190mm~230mm and the width is 900mm~2080mm; (4) In the continuous casting process, the tundish is covered with an acidic covering agent.

7. The method for preparing medium-manganese wear-resistant steel according to claim 5, characterized in that, The heating step includes: The billet, with a temperature of 560℃~820℃, is placed in a heating furnace and then heated to 1180~1250℃ at a heating rate of 1℃ / min~5℃ / min. After holding at this temperature for 20min~40min, it is removed from the furnace.

8. The method for preparing medium-manganese wear-resistant steel according to claim 5, characterized in that, The hot rolling process includes performing five passes of rough rolling and seven passes of finish rolling. The hot rolling satisfies at least one of the following conditions: (1) The total reduction rate of the rough rolling is ≥74%; (2) The total reduction rate of the finishing mill is ≥86.9%; (3) The exit temperature of the finishing mill is 860℃~950℃; (4) The exit thickness of the finishing mill is 3mm~6mm.

9. The method for preparing medium-manganese wear-resistant steel according to claim 5, characterized in that, The cold rolling process satisfies at least one of the following conditions: (1) The cold rolling process involves 3 to 4 passes of cold rolling; (2) The cold-rolled exit thickness is 0.4mm~2.9mm.

10. A steel product, characterized in that, The steel product includes medium-manganese wear-resistant steel as described in any one of claims 1 to 4, or medium-manganese wear-resistant steel prepared by the preparation method described in any one of claims 5 to 9.