Nanocomposite based on porous carrier, and preparation method therefor and use thereof
By adding organic additives to the synthesis process of porous supports, the distribution of nanoparticles can be regulated and a synergistic catalytic system can be formed, which solves the problem of the distribution of platinum-based catalysts in the mesopores of porous supports, improves the activity and high-temperature stability of the catalyst, and makes it suitable for high-temperature proton exchange membrane fuel cell applications.
Patent Information
- Application Number
- PCT/CN2026/075200
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-01-27
- Publication Date
- 2026-11-12
AI Technical Summary
The distribution of existing platinum-based catalysts in the mesopores of porous supports is difficult to control, resulting in insufficient catalytic activity and high-temperature stability, which cannot meet the requirements of high-temperature proton exchange membrane fuel cells.
By adding organic additives to the synthesis process of porous supports, the distribution of nanoparticles can be regulated to form a synergistic catalytic system of metal compounds and nanoparticles, enabling the controllable enrichment of nanoparticles in mesopores. Furthermore, the dopant elements can be retained through etching, simplifying the synthesis process.
It achieves controllable loading of nanoparticles on porous supports, improves catalytic performance and high-temperature operation stability, meets the requirements of high-temperature proton exchange membrane fuel cells, and has a catalyst activity of up to 720 mA/mgPt. The performance degradation rate after 30,000 durability cycles is less than 10%.
Smart Images

Figure CN2026075200_12112026_PF_FP_ABST
Abstract
Description
Nanocomposites based on porous supports, their preparation methods and applications
[0001] This application is based on and claims priority to Chinese Patent Application No. 202510592826.X, filed on May 9, 2025, entitled "Nanocomposite Materials Based on Porous Carriers and Their Preparation Methods and Applications". Technical Field
[0002] This application relates to nanocomposite materials, specifically to a nanocomposite material based on a porous carrier, its preparation method, and its application, belonging to the field of materials science. Background Technology
[0003] Due to their unique structural advantages such as high specific surface area, tunable pore size, excellent conductivity and mechanical adaptability, porous carrier-based nanocomposites have shown broad application potential in many fields such as clean energy production, environmental and energy conversion, chemical energy storage, and wearable and implantable bioelectronic devices. In particular, in the field of high-temperature fuel cells, the development of catalyst materials with high activity and high stability is of great significance.
[0004] For nanocomposites based on porous supports, the loading sites of active nanoparticles are of great significance. Taking platinum-based catalysts as an example, the proportion of platinum particles in the mesopores of the porous support significantly affects their catalytic activity and anti-poisoning performance. However, current technologies cannot controllably adjust the proportion of platinum particles in the mesopores of the porous support. Specifically, common synthesis processes for platinum-based catalysts include polyol methods, ion exchange methods, and colloidal methods. However, these processes use reaction solvents with excessive surface tension, preventing the metal precursor from effectively wetting the mesopores. Platinum nanoparticles are mainly distributed in the channels outside the mesopores, leading to direct contact between the nanoparticles and poisoning substances, resulting in the deactivation of active sites and affecting catalytic performance. Researchers have successfully loaded nanoparticles of different proportions onto the inner and outer surfaces of Ketjen black supports using different synthesis methods such as the initial wetting method and the polyol reduction method. Among these, the catalyst nanoparticles prepared by the polyol method are mainly deposited on the outer surface of the Ketjen black support. Currently, no process has been reported that can achieve a controllable distribution of the proportion of mesoporous nanoparticles on the same carbon support.
[0005] Furthermore, existing platinum-based catalysts are generally only suitable for cryogenic proton exchange membrane fuel cell devices operating at temperatures below 100°C. To further improve energy conversion efficiency, reduce hydrogen purity, and lower water management requirements, the application of cryogenic proton exchange membrane fuel cell devices at higher temperatures is gradually becoming the most promising development direction. However, existing platinum-based catalysts are prone to metal dissolution and detachment during operation at temperatures above 100°C, resulting in rapid performance degradation. Summary of the Invention
[0006] The main objective of this application is to provide a nanocomposite material based on a porous carrier, its preparation method, and its application, in order to solve the aforementioned problems in the prior art.
[0007] To achieve the aforementioned objectives, the technical solution adopted in this application includes:
[0008] The first aspect of this application provides a nanocomposite material based on a porous support, comprising a porous support and nanoparticles supported on the porous support, wherein the nanocomposite material further satisfies the following conditions:
[0009] (1.1) The porous carrier has mesopores and other channels besides mesopores, wherein the volume ratio of the mesopores is 50% to 90%;
[0010] (1.2) The nanoparticles are loaded in the mesopores and other channels outside the mesopores. The mass of the nanoparticles in the mesopores is defined as M, and the mass of the nanoparticles in other channels outside the mesopores is defined as N. Then Fx≥0.3, Fx=M / (M+N).
[0011] (1.3) The nanoparticles comprise a metal and a metal compound, wherein the mass ratio of the metal compound to the metal is 0.02 to 0.2, and the metal element in the metal compound is the same as at least a portion of the metal element in the metal;
[0012] (1.4) The nanocomposite material further comprises a dopant element, wherein a portion of the dopant element is used to form the metal compound, and the mass ratio of the dopant element to the metal element contained in the nanoparticle is 0.1 to 0.3.
[0013] A second aspect of this application provides a method for preparing a nanocomposite material based on a porous support, comprising:
[0014] A liquid-phase mixed reaction system containing a metal source, an organic additive, and a solvent is allowed to react fully at room temperature to form a precursor liquid. The molar ratio of the organic additive to the metal source is 1:3 to 1:1, and the organic additive contains a dopant element.
[0015] The porous support is dispersed in the precursor liquid and thoroughly mixed and reacted at room temperature. The resulting reaction product is then dried and reduced sequentially. After the reduction treatment is completed, it is directly etched to obtain the nanocomposite material based on the porous support.
[0016] The third aspect of this application provides the use of the aforementioned porous support-based nanocomposite material in the preparation of fuel cell catalysts or fuel cells.
[0017] A fourth aspect of this application provides a fuel cell catalyst comprising the aforementioned porous support-based nanocomposite material.
[0018] A fifth aspect of this application provides a fuel cell that includes the aforementioned fuel cell catalyst.
[0019] Compared with the prior art, this application has at least the following beneficial effects:
[0020] Firstly, in the porous support-based nanocomposite material provided in this application, the nanoparticles, serving as the active material, are controllably enriched within the mesopores of the porous support, thus achieving controllable loading of nanoparticles on the porous support. This results in the nanocomposite material exhibiting advantages such as controllable catalytic performance, high mass activity, low susceptibility to poisoning, and high cycle stability when used as a catalyst. Simultaneously, doping elements are introduced into the nanocomposite material. These doping elements, combined with some metal elements in the nanoparticles, form metal compounds that can cooperate with the metals in the nanoparticles to form a synergistic catalytic system, improving the metal electron cloud structure and further significantly enhancing the activity and stability of the nanocomposite material as a catalyst under high-temperature operating conditions. For example, the porous support-based nanocomposite material provided in this application is a platinum-based catalyst with a mass activity as high as 720 mA / mg. Pt (0.9V vs. RHE), the performance degradation rate after 30,000 durability cycles is less than 10%. During high-temperature operation above 105°C, the peak power of the membrane electrode can reach 1.55 W / cm². 2 It meets the high-temperature application requirements of low-temperature proton exchange membrane fuel cells, caters to the future development of new proton exchange membrane fuel cells, and can provide strong support for the commercial application of proton exchange membrane fuel cells.
[0021] Secondly, in the nanocomposite material synthesis process based on porous carriers provided in this application, by adding organic additives to the raw material system, on the one hand, the charge on the surface of the porous carrier can be controlled to achieve enrichment and control of metal colloidal particles as precursors of nanoparticles, so that the nanoparticles can be controllably loaded on the porous carrier; on the other hand, the doping elements introduced by the organic additives are combined with some of the metal elements used to form nanoparticles to form metal compounds, so that the metal in the nanoparticles can form a synergistic catalytic system with the metal compounds.
[0022] Thirdly, the synthesis process of the porous support-based nanocomposite material provided in this application simplifies the synthesis process by directly etching in an air atmosphere after drying and reducing the reaction product of the nanoparticle precursor and the porous support, without undergoing a high-temperature treatment process of 600-1000℃. This process also ensures that the dopant elements are well retained in the nanocomposite material, thereby allowing the aforementioned synergistic catalytic system to fully exert its effectiveness. The synthesis process of this application breaks through the limitations of existing catalyst preparation technologies and can provide a new technical solution and implementation paradigm for the design of high-performance catalysts in fields such as fuel cells and chemical catalysis. Attached Figure Description
[0023] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 is a SEM image of the nanocomposite material prepared in Example 3e of this application;
[0025] Figure 2 is a TEM image of the nanocomposite material prepared in Example 3e of this application;
[0026] Figure 3 is a schematic diagram of the structure of the nanocomposite material obtained in Example 3e of this application;
[0027] Figure 4 is a TEM image of the nanocomposite material prepared in Example 5 of this application;
[0028] Figure 5 is an elemental scan diagram of the nanocomposite material prepared in Example 5 of this application;
[0029] Figure 6 is a TEM image of the nanocomposite material prepared in Comparative Example 3;
[0030] Figure 7 shows the SEM image of the nanocomposite material prepared in Comparative Example 4.
[0031] Figure 8 is a TEM image of the nanocomposite material prepared in Comparative Example 4;
[0032] Figure 9 is a schematic diagram of the structure of the nanocomposite material prepared in Comparative Example 4;
[0033] Figure 10 shows the linear relationship between the single-cell membrane electrode voltage power density and current density of the catalysts prepared in Examples 2, 4, 5, Comparative Example 1, and Comparative Example 5 of this application.
[0034] Figure 11 shows the XRD diffraction patterns of the nanocomposites prepared in Examples 1-4 and Comparative Example 3 of this application. Detailed Implementation
[0035] As mentioned earlier, existing nanocomposites based on porous supports, such as those synthesized with platinum-based catalysts, generally suffer from drawbacks such as difficulty in adapting to high-temperature operating environments and difficulty in controlling the distribution of nanoparticles within the support during their synthesis. In view of this, the inventors of this application, through long-term research and extensive practice, have proposed the technical solution of this application. In summary, this application mainly involves adding an excess of organic additives to the raw material system during the synthesis process of nanocomposites based on porous supports. On the one hand, the organic additives alter the surface electronegativity of the porous support, driving the infiltration of metal colloids (precursors to nanoparticles), dynamic confinement and fixation of solvent evaporation, and synergistic effects between the support and particles, thereby achieving precise control over the proportion of mesoporous nanoparticles. On the other hand, the organic additives introduce dopant elements, allowing the metal compounds formed by the reaction of the dopant elements with some of the metal elements constituting the nanoparticles to form a synergistic catalytic system with the metal in the nanoparticles, thus significantly improving the activity, stability, and mass transfer efficiency of the nanocomposites.
[0036] The technical solution, implementation process, and principles of this application will be further explained below.
[0037] Specifically, as one aspect of the technical solution of this application, a nanocomposite material based on a porous carrier includes a porous carrier and multiple nanoparticles supported by the porous carrier, wherein the nanoparticles include metal compounds and metals.
[0038] In some embodiments, the porous carrier has mesopores and other channels besides mesopores, wherein the volume fraction of the mesopores is 50%–90%, preferably 60%–90%, and more preferably 80%–85%. If the volume fraction of the mesopores is too small, the internal space of the mesopores cannot accommodate a sufficient number of nanoparticles. If the volume fraction of the mesopores is too large, most of the nanoparticles are inside the mesopores of the porous carrier, resulting in excessive resistance to oxygen permeation through the channels, which also affects performance.
[0039] In some embodiments, the nanoparticles are loaded in the mesopores and other pores. If the mass of the nanoparticles in the mesopores is defined as M, the mass of the nanoparticles in the other pores is defined as N, and the total mass of the nanoparticles in the porous carrier is M+N, then M and N satisfy Fx=M / (M+N) and Fx≥0.3.
[0040] Furthermore, the mass of the nanoparticles within the mesopores and the mass of the nanoparticles in other pores outside the mesopores satisfy 0.3 ≤ Fx ≤ 0.9, preferably 0.5–0.6. If the proportion of nanoparticles within the mesopores is too high, the resistance to the reactants reaching the metal active sites will be too great, affecting performance. If the proportion of nanoparticles within the mesopores is too low, the metal active sites will directly contact the ionomer, poisoning the active sites and affecting performance.
[0041] In some embodiments, the average particle size of the nanoparticles is 1–5 nm. The nanoparticles in the porous carrier-based nanocomposite material synthesized in this application are characterized by their small size.
[0042] In some embodiments, the nanocomposite material further comprises dopant elements, some of which are used to combine with some of the metal elements within the nanoparticles to form the metal compound. In some cases, some of the dopant elements may also be distributed in locations such as the pore walls within the porous carrier.
[0043] In some preferred embodiments, the metallic elements contained in the nanoparticles include one or more combinations of Pt, Al, Ti, V, Cr, Mn, Co, Ni, etc., but are not limited thereto.
[0044] In some more preferred embodiments, the metallic element is Pt, or the metallic element includes one or more of Al, Ti, V, Cr, Mn, Co, Ni and other combinations with Pt.
[0045] In some preferred embodiments, the mass ratio of the dopant element to the metal element contained in the nanoparticles is 0.1 to 0.3, preferably 0.2 to 0.3. Too much dopant element can cause pore blockage, while too little dopant element will result in a larger size of the synthesized nanocomposite material, thereby reducing catalyst activity.
[0046] Furthermore, the doping element may include one or more combinations of N, P, S, etc., but is not limited to this.
[0047] Taking Pt as an example, when N is selected as the dopant element, the lone pair electrons of N form Pt-N coordination bonds with Pt, stabilizing Pt nanoparticles and regulating their electronic structure. Specifically, the electron-donating effect of N increases the d-band center of Pt, enhancing the adsorption of reactants (such as H2 and O2) and improving hydrogen evolution reaction (HER) and orthogonal reaction (ORR) activities. N-containing sites can form localized positively charged sites, promoting the adsorption and activation of O2.
[0048] When P is selected as the dopant element, the lone pair electrons of P form Pt-P bonds with Pt, which inhibits sintering and reduces the d-band center. P has a lower electronegativity than C, so it feeds electrons back to Pt, which reduces intermediate poisoning (such as CO) and enhances corrosion resistance. P doping improves the oxidation resistance of the support and extends the catalyst lifetime.
[0049] When sulfur (S) is chosen as the dopant, S forms a PtS2 compound with Pt, altering the electron cloud distribution and improving stability. Furthermore, defect sites can be introduced; S doping causes carbon lattice distortion, increasing the density of active sites. It also exhibits a bifunctional catalytic effect, as S sites can adsorb H2. + Or O2, synergistically with Pt to promote reactions (such as ORR).
[0050] In some more preferred embodiments, the metal compound includes, but is not limited to, one or more combinations of metal sulfides, metal nitrides, metal phosphides, etc.
[0051] Taking Pt as an example, the metal in the nanoparticles can be platinum, and the metal compound can be one or more of platinum sulfide, platinum phosphide, platinum nitride, etc., but is not limited to these.
[0052] In some embodiments, the mass ratio of the metal compound to the metal is 0.02 to 0.2, preferably 0.05 to 0.15, and the metal element in the metal compound is at least partially the same as the metal element in the metal. For example, the metal may be platinum or an alloy of platinum with metals such as Al, Ti, V, Cr, Mn, Co, or Ni, while the metal compound may be platinum sulfide. Too much metal compound can cause the loss of metal active sites, affecting performance; too little metal compound has too weak an effect on inducing changes in the electronic structure of the metal.
[0053] In some embodiments, the porous support is made of one or more of carbon, metal oxides, silicon, silicon carbide, and silicon nitride, but is not limited thereto. For example, the porous support may include one or more of porous graphite, porous graphene, SiC, SnO2, ZrO2, etc., but is not limited thereto.
[0054] In some preferred embodiments, the porous carrier is made of carbon, which has excellent electronic transport properties and good compatibility with nanoparticles whose main component is metal.
[0055] In some embodiments, the mass ratio of the metal element contained in the nanocomposite material to the mass of the porous carrier is 1:4 to 3:2.
[0056] As another aspect of the technical solution of this application, it also relates to a method for preparing the aforementioned porous carrier-based nanocomposite material, including:
[0057] A liquid-phase mixed reaction system containing a metal source, an organic additive, and a solvent is fully reacted at room temperature to form a precursor liquid, wherein the organic additive contains a dopant element;
[0058] The porous support is dispersed in the precursor liquid and thoroughly mixed and reacted at room temperature. The resulting reaction product is then dried and reduced sequentially. After the reduction treatment is completed, the product is directly etched to obtain the nanocomposite material based on the porous support.
[0059] The organic additive contains at least one active group, wherein one or more active groups have a coordination function and are used to coordinate with metal ions derived from a metal source to form metal colloids. Such active group can be defined as the first group.
[0060] Furthermore, the doping element may be distributed within the first group, and may be selected from, but not limited to, one or more combinations of N, P, S, etc.
[0061] By allowing the organic auxiliaries to exist in excess and maintaining the molar ratio with the metal source within a suitable range, it is possible not only to promote the reduction of at least some metal ions provided by the metal source to form metal colloids as precursors for nanoparticles, but also to allow dopant elements to combine with some metal elements in the nanoparticles to form metal compounds, thereby changing the electronic structure of the metal in the nanoparticles and thus improving their catalytic activity and durability.
[0062] Furthermore, the molar ratio of the organic auxiliary agent to the metal source is 1:3 to 1:1. If the molar ratio of the organic auxiliary agent to the metal source is greater than 1:1, the organic auxiliary agent will cause partial blockage of the pores within the porous support, affecting the contact between the active sites inside the pores and the reactants. If the molar ratio of the organic auxiliary agent to the metal source is less than 1:3, the organic auxiliary agent is too small, which will result in incomplete reduction of metal ions and excessively large nanoparticle size.
[0063] Meanwhile, one or more active groups in the organic additive are hydrophilic groups, which can be defined as second groups.
[0064] The first and second groups may include one or more combinations of groups selected from thiocarboxyl, mercapto, sulfonic acid, hydroxyl, amino, nitro, phosphate, carboxyl, and aldehyde groups. Furthermore, the first and second groups may be of the same or different types. For example, both the first and second groups may be mercapto groups.
[0065] When the porous support is porous carbon particles or the like, the amphiphilic hydrophobic groups of the organic additive, such as its alkyl backbone, can combine with the hydrophobic surface of the support, while its hydrophilic groups can interact with solvents such as water to form a hydrophilic layer, making the support easier to wet with solvents.
[0066] In some embodiments, the organic auxiliaries may include any one or more combinations of mercaptoacetic acid or its salts, L-cysteine or its salts, ethylenediamine, glutathione, penicillamine, dithiothreitol, adenosine triphosphate, etc., but are not limited thereto. For example, the organic auxiliaries may preferably be mercaptoacetic acid salts such as STG (sodium mercaptoacetate). The thiol groups contained in STG have a strong coordinating ability and can combine with metal ions provided by the metal source to form complexes. At the same time, STG has a mild reducing ability to slowly nucleate metal atoms, inhibiting excessive reduction and aggregation of metal ions, thereby effectively controlling the size of nanoparticles with metal as the main component. In addition, STG can chemically bond to modify the surface of porous supports, increasing the active sites on the surface of porous supports and promoting the uniform distribution of nanoparticles.
[0067] In some embodiments, the metal source may be a soluble metal salt. Furthermore, the metal element contained in the metal salt may include any one or a combination of two or more of Pt, Al, Ti, V, Cr, Mn, Co, and Ni, for example, it may be Pt, or a combination of one or more of Al, Ti, V, Cr, Mn, Co, and Ni with Pt, and is not limited thereto.
[0068] For example, the metal source may be an acid (such as chloroplatinic acid) or salt containing the aforementioned metal element. Further, the metal source may be a nitrate, hydrochloride, sulfate or other form of salt, such as potassium chloroplatinate, sodium chloroplatinate, platinum nitrate, platinum acetylacetonate, platinum sulfate, ammonium chloroplatinate, etc.
[0069] In some embodiments, the solvent includes water or a combination of water and an organic solvent. For example, the organic solvent may include, but is not limited to, acetone, methanol, ethanol, isopropanol, or acetonitrile.
[0070] In some embodiments, the preparation method may specifically include: reacting the liquid-phase mixed reaction system at room temperature for more than 1 hour, for example, 1 hour to 2 hours, thereby forming the precursor liquid.
[0071] In some embodiments, the preparation method may specifically include: uniformly dispersing the porous support in the precursor liquid and reacting it fully at room temperature, wherein the residual organic additives in the precursor liquid can change the electronegativity of the porous support surface, thereby causing a specified mass ratio of metal colloidal particles in the precursor liquid to enter the mesopores within the porous support and further transform into nanoparticles within the mesopores, thereby achieving controllable loading of nanoparticles within the porous support.
[0072] If the nanoparticles loaded in the mesopores are defined as mesoporous nanoparticles, then generally speaking, the proportion of mesoporous nanoparticles is positively correlated with the immersion time of the porous carrier in the precursor fluid.
[0073] Furthermore, the porous support can be dispersed in the precursor liquid and reacted at room temperature for at least 6 hours, preferably 6 to 36 hours, after which the reaction product can be separated from the reaction mixture. During this reaction, as the reaction time increases, the porous support continuously attracts metal colloidal particles into its interior, resulting in a gradual increase in the number of mesoporous nanoparticles. When the reaction time exceeds 36 hours, the internal enrichment force reaches saturation, and the mesoporous nanoparticles no longer accumulate with further time. At this point, the proportion of mesoporous nanoparticles is 0.7 to 0.9%.
[0074] In some embodiments, during the drying process, only the solvent in the reaction mixture is evaporated and removed, while the remaining components are retained in the final reaction product.
[0075] In some embodiments, the reduction treatment is carried out in an atmosphere containing a reducing gas, at a temperature of 200–500°C, for a time of 1–5 hours. Through this reduction treatment, the platinum precursor can be completely converted into metallic Pt. 0 This ensures sufficient exposure of the catalytic active sites. If the reduction treatment temperature is too high, irreversible sintering will occur; if the reduction treatment temperature is too low, the reduction will be insufficient.
[0076] In some embodiments, the etching process is performed in an air atmosphere at a temperature of 200–500°C for 1–6 hours. This air etching process can remove amorphous carbon, clear pores, and improve mass transfer efficiency. If the etching temperature is too high or the time is too long, the carrier structure may collapse; if the etching temperature is too low or the time is too short, the effects of removing amorphous carbon and clearing pores will not be achieved.
[0077] In the preparation method of this application, after reducing the reaction product, air etching is performed directly without high-temperature annealing or other processes. This allows the metal compound to be stably retained in the nanoparticles, forming a synergistic catalytic system with the metal components in the nanoparticles. At the same time, it can avoid damage to the porous support structure and migration of nanoparticles caused by high-temperature treatment, making the distribution position of nanoparticles in the porous support more controllable.
[0078] The preparation process described in this application is process-compatible and can be adapted to a variety of porous supports and metal precursors. It optimizes the activity, stability and mass transfer efficiency of the catalyst. This strategy provides a new paradigm for the design of high-performance catalysts in fields such as fuel cells and chemical catalysis.
[0079] Furthermore, the preparation method of this application can synthesize small-sized, highly dispersible nanoparticles with metal as the main component, thereby improving catalytic activity and stability. It also has the advantages of simple process (fewer steps and lower equipment requirements), economic efficiency (low raw material and energy costs, suitable for large-scale application), and environmental friendliness (low solvent and by-product pollution, in line with green chemistry principles).
[0080] As another aspect of the technical solution of this application, it also relates to the use of the aforementioned porous carrier-based nanocomposite materials in the fields of preparing fuel cell catalysts or fuel cells.
[0081] Correspondingly, another aspect of the technical solution of this application also provides a fuel cell catalyst comprising the aforementioned porous carrier-based nanocomposite material.
[0082] Another aspect of the technical solution of this application provides a fuel cell that includes the aforementioned fuel cell catalyst.
[0083] To provide a clearer understanding of the purpose, technical solution, and advantages of this application, the following embodiments will further explain and illustrate the technical solution, its implementation process, and principles. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to enable a more thorough and comprehensive understanding of the disclosure of this application.
[0084] The carriers used in the following embodiments have a mesoporous content of ≥50%, and the specific types can be porous carbon carriers (CMK1-C12-FA), tin oxide (Tiannai Technology-688116), silicon carbide (Beijing Deco Island Gold Technology Co., Ltd.-DK-SiC-001), etc.
[0085] Example 1
[0086] The preparation method of a platinum-carbon catalyst in this embodiment includes:
[0087] S1. Sodium mercaptoacetate and chloroplatinic acid in a molar ratio of approximately 1:1 are added to deionized water at room temperature and stirred at room temperature for about 2 hours to form a precursor solution.
[0088] S2. Add a porous carbon support (CMK1-C12-FA-2400) with a mesoporous content of about 50% to the precursor liquid obtained in step S1, and control the mass ratio of the metal element in the metal source to the carbon support to be about 1:4. Stir at room temperature for about 6 hours, and then dry the obtained reaction mixture at a temperature of about 70°C to obtain powder.
[0089] S3. Place the powder obtained in step S2 in a tube furnace and heat it for reduction. The reduction conditions are: temperature about 200℃, time about 1 hour, and reaction atmosphere is 5% H2 / Ar mixed gas to obtain the reduction product.
[0090] S4. Wash the reduction product obtained in step S3 with clean water and by vacuum filtration until the conductivity of the filtrate is about 5 μs / cm to obtain the washed powder.
[0091] S5. The cleaned powder obtained in step S4 is subjected to air etching under the following conditions: temperature of about 200°C and time of about 1 hour, to obtain the target product.
[0092] Example 1a
[0093] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 1, except that: in S2, a porous carbon support (CMK1-C12-FA-2000) with a mesoporous content of about 60% is used.
[0094] Example 1b
[0095] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 1, except that: in S2, a porous carbon support (CMK1-C12-FA-1600) with a mesoporous content of about 70% is used.
[0096] Example 1c
[0097] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 1, except that: in S2, a porous carbon support (CMK1-C12-FA-1200) with a mesoporous content of about 80% is used.
[0098] Example 1d
[0099] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 1, except that: in S2, a porous carbon support (CMK1-C12-FA-900) with a mesoporous content of about 85% is used.
[0100] Example 1e
[0101] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 1, except that: in S2, a porous carbon support (CMK1-C12-FA) with a mesoporous content of about 90% is used.
[0102] Example 2
[0103] The preparation method of a platinum-carbon catalyst in this embodiment includes:
[0104] S1. Sodium mercaptoacetate and chloroplatinic acid in a molar ratio of approximately 1:2 are added to deionized water at room temperature and stirred at room temperature for about 2 hours to form a precursor solution.
[0105] S2. Add a porous carbon support (CMK1-C12-FA-1200) with a mesoporous content of about 80% to the precursor liquid obtained in step S1, and control the mass ratio of the metal element in the metal source to the carbon support to be about 1:4. Stir at room temperature for about 12 hours, and then dry the obtained reaction mixture at a temperature of about 70°C to obtain powder.
[0106] S3. Place the powder obtained in step S2 in a tube furnace and heat it for reduction. The reduction conditions are: temperature about 300℃, time about 3h, and reaction atmosphere is 5% H2 / Ar mixed gas to obtain the reduction product.
[0107] S4. Wash the reduction product obtained in step S3 with clean water and by vacuum filtration until the conductivity of the filtrate is about 5 μs / cm to obtain the washed powder.
[0108] S5. The cleaned powder obtained in step S4 is subjected to air etching under the following conditions: temperature of about 300°C and time of about 3 hours, to obtain the target product.
[0109] Example 2a
[0110] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 2, except that in S1, the molar ratio of sodium mercaptoacetate to chloroplatinic acid is 1:3.
[0111] Example 2b
[0112] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 2, except that in S1, the molar ratio of sodium mercaptoacetate to chloroplatinic acid is 1:1.
[0113] Example 3
[0114] The preparation method of a platinum-carbon catalyst in this embodiment includes:
[0115] S1. Sodium mercaptoacetate and chloroplatinic acid in a molar ratio of approximately 1:3 are added to deionized water at room temperature and stirred at room temperature for about 2 hours to form a precursor solution.
[0116] S2. Add a porous carbon support (CMK1-C12-FA-1200) with a mesoporous content of about 80% to the precursor liquid obtained in step S1, and control the mass ratio of the metal element in the metal source to the carbon support to be about 1:4. Stir at room temperature for about 20 hours, and then dry the obtained reaction mixture at a temperature of about 70°C to obtain powder.
[0117] S3. Place the powder obtained in step S2 in a tube furnace and heat it for reduction. The reduction conditions are: temperature about 400℃, time about 5h, and reaction atmosphere is 5% H2 / Ar mixed gas to obtain the reduction product.
[0118] S4. Wash the reduction product obtained in step S3 with clean water and by vacuum filtration until the conductivity of the filtrate is about 5 μs / cm to obtain the washed powder.
[0119] S5. The cleaned powder obtained in step S4 is subjected to air etching under the following conditions: temperature of about 500°C and time of about 5 hours, to obtain the target product.
[0120] Example 3a
[0121] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that: S2, a porous carbon support (CMK1-C12-FA-1200) with a mesoporous ratio of about 80% is added to the precursor liquid, and then stirred at room temperature for about 6 hours.
[0122] Example 3b
[0123] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that: S2, a porous carbon support (CMK1-C12-FA-1200) with a mesoporous ratio of about 80% is added to the precursor liquid, and then stirred at room temperature for about 12 hours.
[0124] Example 3c
[0125] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that: S2, a porous carbon support (CMK1-C12-FA-1200) with a mesoporous ratio of about 80% is added to the precursor liquid, and then stirred at room temperature for about 18 hours.
[0126] Example 3d
[0127] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that: S2, a porous carbon support (CMK1-C12-FA-1200) with a mesoporous ratio of about 80% is added to the precursor liquid, and then stirred at room temperature for about 30 hours.
[0128] Example 3e
[0129] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that: S2, a porous carbon support (CMK1-C12-FA-1200) with a mesoporous ratio of about 80% is added to the precursor liquid, and then stirred at room temperature for about 36 hours.
[0130] Example 4
[0131] The preparation method of a platinum-carbon catalyst in this embodiment includes:
[0132] S1. Sodium mercaptoacetate and chloroplatinic acid in a molar ratio of approximately 1:2 are added to deionized water at room temperature and stirred at room temperature for about 2 hours to form a precursor solution.
[0133] S2. Add a porous carbon support (CMK1-C12-FA-1200) with a mesoporous content of about 80% to the precursor liquid obtained in step S1, and control the mass ratio of the metal element in the metal source to the carbon support to be about 1:3. Stir at room temperature for about 20 hours, and then dry the obtained reaction mixture at a temperature of about 70°C to obtain powder.
[0134] S3. Place the powder obtained in step S2 in a tube furnace and heat it for reduction. The reduction conditions are: temperature about 400℃, time about 5h, and reaction atmosphere is 5% H2 / Ar mixed gas to obtain the reduction product.
[0135] S4. Wash the reduction product obtained in step S3 with clean water and by vacuum filtration until the conductivity of the filtrate is about 5 μs / cm to obtain the washed powder.
[0136] S5. The cleaned powder obtained in step S4 is subjected to air etching under the following conditions: temperature of about 500°C and time of about 5 hours, to obtain the target product.
[0137] Example 4a
[0138] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that: in S2, the mass ratio of the metal element in the metal source to the carbon support is controlled to be about 1:2.
[0139] Example 4b
[0140] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that: in S2, the mass ratio of the metal element in the metal source to the carbon support is controlled to be about 1:1.
[0141] Example 4c
[0142] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that the mass ratio of the metal element in the metal source to the carbon support is controlled to be about 2:1 in S2.
[0143] Example 4d
[0144] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 3, except that the mass ratio of the metal element in the metal source to the carbon support is controlled to be about 3:2 in S2.
[0145] Example 5
[0146] The preparation method of a platinum-carbon catalyst in this embodiment includes:
[0147] S1. Sodium thioglycolate, chloroplatinic acid and CoCl2 are added to deionized water at room temperature. The molar ratio of the sum of the molar amounts of chloroplatinic acid and CoCl2 to sodium thioglycolate is approximately 2:1. The mixture is stirred at room temperature for about 2 hours to form a precursor solution.
[0148] S2. Add a porous carbon support (CMK1-C12-FA-1200) with a mesoporous content of about 80% to the precursor liquid obtained in step S1, and control the mass ratio of the metal element in the metal source to the carbon support to be about 1:1. Stir at room temperature for about 20 hours, and then dry the obtained reaction mixture at a temperature of about 70°C to obtain powder.
[0149] S3. Place the powder obtained in step S2 in a tube furnace and heat it for reduction. The reduction conditions are: temperature about 500℃, time about 2h, and reaction atmosphere is 5% H2 / Ar mixed gas to obtain the reduction product.
[0150] S4. Wash the reduction product obtained in step S3 with clean water and by vacuum filtration until the conductivity of the filtrate is about 5 μs / cm to obtain the washed powder.
[0151] S5. The cleaned powder obtained in step S4 is subjected to air etching under the following conditions: temperature of about 200°C and time of about 5 hours, to obtain the target product.
[0152] Example 6
[0153] The preparation method of a platinum-carbon catalyst in this embodiment includes:
[0154] S1. Sodium mercaptoacetate, chloroplatinic acid and MnSO4 are added to deionized water at room temperature, wherein the molar ratio of the sum of the molar amounts of chloroplatinic acid and MnSO4 to sodium mercaptoacetate is approximately 2:1, and the mixture is stirred at room temperature for about 2 hours to form a precursor solution.
[0155] S2. Add silicon carbide with a mesoporous content of about 80% to the precursor liquid obtained in step S1, and control the mass ratio of the metal element in the metal source to the carbon support to be about 1:1. After stirring at room temperature for about 20 hours, dry the obtained reaction mixture at a temperature of about 70°C to obtain powder.
[0156] S3. Place the powder obtained in step S2 in a tube furnace and heat it for reduction. The reduction conditions are: temperature about 500℃, time about 2h, and reaction atmosphere is 5% H2 / Ar mixed gas to obtain the reduction product.
[0157] S4. Wash the reduction product obtained in step S3 with clean water and by vacuum filtration until the conductivity of the filtrate is about 5 μs / cm to obtain the washed powder.
[0158] S5. The cleaned powder obtained in step S4 is subjected to air etching under the following conditions: temperature of about 200°C and time of about 3 hours, to obtain the target product.
[0159] Example 7
[0160] The preparation method of a platinum-carbon catalyst in this embodiment includes:
[0161] S1. Sodium mercaptoacetate, chloroplatinic acid and TiCl4 are added to deionized water at room temperature. The molar ratio of the sum of the molar amounts of chloroplatinic acid and TiCl4 to sodium mercaptoacetate is approximately 2:1. The mixture is stirred at room temperature for about 2 hours to form a precursor solution.
[0162] S2. Add tin oxide with a mesoporous content of about 85% to the precursor liquid obtained in step S1, and control the mass ratio of the metal element in the metal source to the carbon support to be about 1:1. Stir at room temperature for about 20 hours, and then dry the obtained reaction mixture at a temperature of about 70°C to obtain powder.
[0163] S3. Place the powder obtained in step S2 in a tube furnace and heat it for reduction. The reduction conditions are: temperature about 500℃, time about 2h, and reaction atmosphere is 5% H2 / Ar mixed gas to obtain the reduction product.
[0164] S4. Wash the reduction product obtained in step S3 with clean water and by vacuum filtration until the conductivity of the filtrate is about 5 μs / cm to obtain the washed powder.
[0165] S5. The cleaned powder obtained in step S4 is subjected to air etching under the following conditions: temperature of about 200°C and time of about 6 hours, to obtain the target product.
[0166] Example 8
[0167] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 4, except that sodium mercaptoacetate is replaced with dithiothreitol.
[0168] Example 9
[0169] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 4, except that sodium mercaptoacetate is replaced with L-cysteine.
[0170] Example 10
[0171] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 4, except that sodium mercaptoacetate is replaced with penicillamine.
[0172] Example 11
[0173] The preparation method of the platinum-carbon catalyst provided in this embodiment is basically the same as that in Example 4, except that sodium mercaptoacetate is replaced with adenosine triphosphate.
[0174] Comparative Example 1
[0175] The preparation method of the platinum-based catalyst provided in this comparative example is basically the same as that in Example 5, except that:
[0176] In step S1, an excess of chloroplatinic acid is added, with a molar ratio of sodium mercaptoacetate to chloroplatinic acid of approximately 1:5, and the mixture is stirred at room temperature for about 2 hours to form a precursor fluid.
[0177] Comparative Example 2
[0178] The preparation method of the platinum-based catalyst provided in this comparative example is basically the same as that in Example 5, except that:
[0179] In step S1, an excess of sodium thioglycolate is added, with a molar ratio of sodium thioglycolate to chloroplatinic acid of approximately 2:1, and the mixture is stirred at room temperature for about 2 hours to form a precursor solution.
[0180] Comparative Example 3
[0181] The preparation method of the platinum-based catalyst provided in this comparative example is basically the same as that in Example 5, except that sodium mercaptoacetate is not added in step S1.
[0182] Comparative Example 4
[0183] The preparation method of the platinum-based catalyst provided in this comparative example is basically the same as that in Example 5, except that:
[0184] In step S2, a carbon support is added to the precursor fluid obtained in step S1, and then stirred at room temperature for about 2 hours.
[0185] Comparative Example 5
[0186] The preparation method of the platinum-based catalyst provided in this comparative example is basically the same as that in Example 5, except that the mesoporous content of the porous carbon support used in step S2 is 30%.
[0187] Figures 1, 2, and 3 are SEM images, TEM images, and structural schematic diagrams of the nanocomposite material prepared in Example 3e, respectively. It can be seen that Example 3e achieved the enrichment of platinum nanoparticles inside the mesopores.
[0188] Figure 4 is a TEM image of the nanocomposite material prepared in Example 5, and Figure 5 is an elemental scan of the nanocomposite material. It can be seen that sulfur and platinum overlap and have an anchoring effect.
[0189] Figure 6 is a TEM image of the nanocomposite material prepared in Comparative Example 3. Comparing the transmission electron microscope schematic diagrams in Figure 4 and Figure 6, it can be seen that the size of the nanoparticles gradually increases from the presence to the absence of organic additives in Example 5 and Comparative Example 3. Therefore, the content of organic additives will significantly affect the size of the metal nanoparticles.
[0190] Figures 7, 8, and 9 show the SEM images, TEM images, and structural schematic diagrams of the nanocomposite material prepared in Comparative Example 4, respectively. It can be seen that Comparative Example 4 cannot achieve the enrichment and loading of platinum nanoparticles inside the mesopores, and the proportion of platinum nanoparticles inside the mesopores is less than 0.3%.
[0191] Figure 10 shows the linear relationship between the single-cell membrane electrode voltage power density and current density of the catalysts prepared in Examples 2, 4, 5, Comparative Example 1, and Comparative Example 5. It shows that the performance of the examples is much higher than that of the comparative examples, and the performance of Example 5 shows a peak.
[0192] Figure 11 shows the XRD diffraction patterns of the nanocomposites prepared in Examples 1-4 and Comparative Example 3, indicating that the organic additives promote the presence of the metal compounds.
[0193] The test methods for the catalyst performance data shown in Table 2 are as follows: The electrochemical workstation was a Biologic-50e, and the RDE device was a PINE electrode kit sold by Hong Kong Li & Fung Company, employing a three-electrode system: the working electrode was a glassy carbon electrode (PINE) with catalyst supported, the reference electrode was a saturated calomel electrode (SCE), and the counter electrode was a Pt carbon rod. The perchloric acid solution used in this test was 0.1M. The scanning potential range of the cyclic voltammetry was set from 0.05V vs. RHE to 1.05V vs. RHE, and the scan rate was 50mV s.-1 The electrochemical specific surface area (ECSA) of platinum can be calculated by potentiometrically depositing the hydrogen adsorption region. The LSV of the LSV test is measured in the potential range of 0.05 V vs. RHE to 1.05 V vs. RHE, with a scan rate of 10 mV / s. -1 The rotating disk electrode was rotated at 1600 rpm, and the ORR performance was evaluated using half-wave potential and mass activity (MA). Durability testing: In N2-saturated 0.1M HClO4, a constant potential of 0.6V / vs.RHE was first applied for 30 seconds, followed by square wave cycling at 0.95V vs.RHE–0.6V vs.RHE, with each potential lasting 3 seconds and each cycle lasting 6 seconds, for a total of 100,000 cycles. Activation and polarization curve tests of the membrane electrode were conducted in a hydrogen-air environment at 80℃ and 90% RH, with a single-cell back pressure of 70 kPa. Before testing, the membrane electrode was activated at a constant voltage of 0.3V until the current density reached a stable state. After stabilization, subsequent tests were performed, and the current density-voltage curve of the fuel cell was measured within a certain current range to obtain the peak power density of the material. The activation and polarization curve tests of the high-temperature membrane electrode were all conducted in a hydrogen-air environment at a temperature of 105°C or higher. The raw materials and amounts used in Examples 1-11 and Comparative Examples 1-5 are shown in Table 1, and the structural data of the obtained catalysts are shown in Table 2.
[0194] Table 1. Raw materials and amounts used in Examples 1-11 and Comparative Examples 1-5
[0195] Table 2 Catalyst structural data for Examples 1-11 and Comparative Examples 1-5 Note: The proportion of mesoporous nanoparticles = the mass of nanoparticles within mesopores / (the mass of nanoparticles within mesopores + the mass of nanoparticles in other channels outside mesopores); the proportion of doped elements = the mass of doped elements / the mass of the metal; the proportion of metal compounds = the mass of metal compounds / the mass of the metal.
[0196] When the catalyst of this application is used in a fuel cell, the test performance data of the corresponding cell are shown in Table 3.
[0197] Table 3 Battery Test Performance
[0198] The activity of the catalysts in Examples 1 to 11 of this application was tested, and the results showed that the mass activity (MA) of these catalysts could be increased to 720 mA / mgPt (0.9V vs. RHE), which is much higher than the 200 mA / mgPt of current commercial catalysts. This may be attributed to the high dispersion of the internal nanoparticles and the intrinsic activity enhanced by the confinement effect.
[0199] The stability of the catalysts in Examples 1 to 11 of this application was tested, and the results showed that in the accelerated aging test (ADT), the ECSA decay rate of these catalysts could be reduced to 6%, which is far lower than 50% of the current commercial catalysts. This should be due to the significant confinement effect of the support, which effectively inhibits platinum dissolution and agglomeration.
[0200] Furthermore, the half-cells prepared based on the catalysts of Examples 1-11 of this application have a mass activity of 400-720.04 mA / mg. Pt (0.9V vs. RHE), the peak power density of a single cell at an operating temperature of 80°C is 1.06–2.0 W / cm³. 2 Furthermore, the peak power density of the single cell at an operating temperature of 105°C is 0.93–1.55 W / cm². 2 .
[0201] In addition, the applicant also conducted experiments using other raw materials and process conditions listed in this specification, referring to the preparation methods of Examples 1-11 above. The composition, structure, and application performance of the products obtained from these experiments were tested using a series of characterization methods described above, revealing good performance in catalytic activity and stability. For example, the applicant replaced the porous carbon support in Example 4 with graphene (NanoXplore-XG-Porous), graphitic carbon nitride (carbon nitride-Xi'an Ruixi Biotechnology Co., Ltd.-RC-1220), and metal-organic framework materials (BASF-CALF-20), respectively. The mass activity of the obtained catalyst products was all above 450 mA / mgPt (0.9V vs. RHE), and the ECSA attenuation rate was all below 15%.
[0202] Although the embodiments of this application have been described in detail above, those skilled in the art, upon understanding the inventive content and concepts, may make deletions and modifications, all of which fall within the scope of protection of this application. Therefore, the scope of protection of this patent application shall be determined by the appended claims.
[0203] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
Claims
1. A nanocomposite material based on a porous carrier, comprising a porous carrier and nanoparticles supported on the porous carrier, characterized in that, The nanocomposite material also meets the following conditions: (1.1) The porous carrier has mesopores and other channels besides mesopores, wherein the volume ratio of the mesopores is 50% to 90%; (1.2) The nanoparticles are loaded in the mesopores and other channels outside the mesopores. The mass of the nanoparticles in the mesopores is defined as M, and the mass of the nanoparticles in other channels outside the mesopores is defined as N. Then Fx≥0.3, Fx=M / (M+N). (1.3) The nanoparticles comprise a metal and a metal compound, wherein the mass ratio of the metal compound to the metal is 0.02 to 0.2, and the metal element in the metal compound is the same as at least a portion of the metal element in the metal; (1.4) The nanocomposite material further comprises a dopant element, wherein a portion of the dopant element is used to form the metal compound, and the mass ratio of the dopant element to the metal element contained in the nanoparticle is 0.1 to 0.
3.
2. The nanocomposite material based on a porous carrier according to claim 1, characterized in that: Fx is 0.3 to 0.
9.
3. The nanocomposite material based on a porous carrier according to claim 1, characterized in that: The average particle size of the nanoparticles is 1–5 nm.
4. The nanocomposite material based on a porous carrier according to claim 1, characterized in that: The metallic element includes any one or more combinations of Pt, Al, Ti, V, Cr, Mn, Co, and Ni, and the doping element includes one or more combinations of N, P, and S.
5. The nanocomposite material based on a porous carrier according to claim 4, characterized in that: The metallic element is Pt, or the metallic element includes one or more of Al, Ti, V, Cr, Mn, Co, and Ni combined with Pt.
6. The nanocomposite material based on a porous carrier according to claim 5, characterized in that: The metal compound includes one or more combinations of metal sulfides, metal nitrides, and metal phosphides.
7. The nanocomposite material based on a porous carrier according to claim 1, characterized in that: The porous carrier is made of one or more of the following materials: carbon, metal oxide, silicon, silicon carbide, and silicon nitride.
8. A method for preparing the porous carrier-based nanocomposite material according to any one of claims 1 to 7, characterized in that, include: A liquid-phase mixed reaction system containing a metal source, an organic additive, and a solvent is allowed to react fully at room temperature to form a precursor liquid. The molar ratio of the organic additive to the metal source is 1:3 to 1:1, and the organic additive contains a dopant element. The porous support is dispersed in the precursor liquid and thoroughly mixed and reacted at room temperature. The resulting reaction product is then dried and reduced sequentially. After the reduction treatment is completed, it is directly etched to obtain the nanocomposite material based on the porous support.
9. The method according to claim 8, characterized in that: The organic additive contains a first group and a second group, wherein the first group and the second group include one or more combinations of thiocarboxyl, mercapto, sulfonic acid, hydroxyl, amino, nitro, phosphate, carboxyl, and aldehyde groups.
10. The method according to any one of claims 8 to 9, characterized in that: The organic adjuvants include one or more combinations of thioglycolic acid or its salts, L-cysteine or its salts, ethylenediamine, glutathione, penicillamine, dithiothreitol, and adenosine triphosphate.
11. The method according to claim 8, characterized in that: The metal source includes a soluble metal salt, wherein the metal element contained in the metal salt includes any one or a combination of two or more of Pt, Al, Ti, V, Cr, Mn, Co, and Ni; and / or, the solvent includes water or a combination of water and an organic solvent.
12. The method according to claim 8, characterized in that, Specifically, it includes: The liquid-phase mixed reaction system is reacted at room temperature for more than 1 hour to form the precursor liquid.
13. The method according to claim 8, characterized in that, Specifically, it includes: The porous support was dispersed in the precursor liquid and mixed and reacted at room temperature for more than 6 hours, after which the reaction product was obtained by separation from the reaction mixture.
14. The method according to claim 8, characterized in that: The reduction treatment is carried out in an atmosphere containing reducing gas, at a temperature of 200–500°C, for a time of 1–5 hours.
15. The method according to claim 8, characterized in that: The etching process is carried out in an air atmosphere at a temperature of 200–500°C for 1–6 hours.
16. Use of the porous support-based nanocomposite material according to any one of claims 1 to 7 in the preparation of fuel cell catalysts or fuel cells.
17. A fuel cell catalyst, characterized in that, The nanocomposite material based on a porous carrier, as described in any one of claims 1 to 7.