Method for producing a decorated profile body having portions with different surface properties

The method of applying a curable coating to a substrate and differentially treating surface sections addresses the challenge of creating angle-dependent surface variations in decorated profile bodies, achieving cost-effective and visually distinct results.

WO2026233718A1PCT designated stage Publication Date: 2026-11-12REHAU IND SE & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/061536
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-22
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for producing decorated profile bodies with sectionally different surface properties, such as those used in furniture and wall coverings, result in uniformly visible effects and are costly, lacking the ability to create subtle, angle-dependent surface variations.

Method used

A method involving the application of a curable coating to a substrate, followed by partial gelling and differential treatment of surface sections using additive manufacturing and controlled irradiation to achieve varying gloss and tactile properties.

Benefits of technology

Creates a subtle surface effect that is inconspicuous at first glance but becomes apparent under specific angles or touch, allowing for cost-effective production of decorated profile bodies with differentiated surface optics and haptics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026061536_12112026_PF_FP_ABST
    Figure EP2026061536_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a decorated profile body (1) having portions with different surface properties, in particular for the furniture industry, comprising the steps of: step A: providing a substrate (2); step B: applying a curable coating (3) to the substrate (2); step C: partially gelling the coating (3); step D: treating at least two surface portions (4, 5) of the partially gelled coating (3) in different ways so that the surface properties of the coating (3) in the differently treated surface portions (4, 5) differ when fully cured.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0002] Method for producing a decorated profile body with section-by-section different surface properties

[0003] The present invention relates to a method for producing a decorated profile body with sectionally different surface properties.

[0004] Decorated profile bodies can be, for example, decorative foils used for furniture fronts, wall coverings, niche coverings or roller shutters (slats).

[0005] Decorated profile bodies can also be edge strips or wall connection profiles with a decorated surface.

[0006] A continuing and increasing trend in the furniture industry is matt surfaces, for which excimer technology (lacquer micro-folding) has prevailed in terms of the achievable qualities.

[0007] Furthermore, the gelation of surfaces using special emitters (PAC, UV Ga, LED) is known to achieve a soft surface feel and at the same time influence the sheene effect, i.e. a glossiness under shallow angles.

[0008] To create glossy effects, foils are used as a structuring agent.

[0009] Corresponding techniques for producing matt surfaces are known from EP 2794 126 B1 or EP 3453463 B1.

[0010] A disadvantage of excimer technology (micro-folding of lacquer) is that it produces purely homogeneous surface appearances. Furthermore, the use of films is expensive, and the effect is uniformly visible from all viewing angles.

[0011] The present invention is based on the objective of providing a method for producing a decorated profile body in order to create different surface properties section by section with minimal effort.

[0012] To solve this problem, the present invention provides the method according to claim 1.

[0013] A process for manufacturing a decorated profile body with sectionally different surface properties, particularly for the furniture industry, is disclosed, comprising the following steps: REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0014] Step A: Providing a substrate;

[0015] Step B: Applying a curable, especially radiation-curable, coating such as UV varnish to the substrate;

[0016] Step C: Gelling or hardening of the coating;

[0017] Step D: Treat at least two surface sections of the gelled coating in different ways, so that the surface properties of the coating differ in the differently treated surface sections in the cured state.

[0018] The surface properties can differ, particularly in terms of appearance, especially regarding the gloss behavior at a shallow angle and / or the feel and / or the softness.

[0019] In step B, the coating is preferably applied to the entire surface of the substrate. In step C, the coating is preferably gelled over the entire surface.

[0020] The solution according to the invention essentially consists of generating a subtle surface effect or doubling, which only becomes apparent from defined angles. This creates a shading effect. The present invention makes use of the properties of the curable coating material.

[0021] The curable coating material does not harden instantly, but rather in a process that is usually controllable over time, in which the state of the coating material changes from flowable and malleable to hard and fixed in shape.

[0022] An increase in the viscosity of the gelled coating material is barely measurable, as only a very thin top layer is gelled. However, the conversion of double bonds is measurable, e.g., via ATR-FT-IR. While a peak (100%) is still displayed at the C-C band in liquid lacquer, this peak is only between 50-60% during gelling and close to 0 upon final curing.

[0023] This means a double bond turnover of >95%.

[0024] In the gelled transition state, the coating material remains malleable, for example, through the application of external force and / or energy. The gelled state can be "frozen" by fully curing the coating material to ensure its permanent effect. Thus, different surface properties or effects can be created by treating already gelled surface sections differently, and these effects are retained even after the coating has fully cured.

[0025] Ideally, a coating material such as a UV lacquer is first applied to the substrate and allowed to gel over the entire surface. REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj Subsequently, for example, a partial application of the same or a different coating material – wet-on-wet – can be carried out using additive manufacturing processes such as flexographic printing, inkjet printing, or other techniques. Thus, material is applied to a portion of the gelled coating, while, for example, another portion remains untreated.

[0026] The entire surface can then be subjected to excimer curing, whereby the areas applied after pre-gelling have a different gloss behavior at a shallow angle as well as a different feel / softness.

[0027] Alternatively, other treatments of the gelled surface sections are also conceivable, whereby, for example, partial material removal or external force causes a partial displacement of the coating material.

[0028] Different irradiations of different surface sections are also possible.

[0029] The main advantage of the present invention lies in the creation of a surface effect that is very inconspicuous at first glance, which only becomes apparent under certain lighting conditions and viewing angles, or can be felt through the differences in softness.

[0030] The contrast can be adjusted by controlling the gelation energy, e.g. by using a different number of PAG emitters.

[0031] Advantageous embodiments of the invention are the subject of the dependent claims.

[0032] It can be advantageous if, in step A, the substrate is made of a polymeric material, preferably plastic, preferably as an extruded or calendered profile, particularly preferably as an edge banding or wall connection profile, or as a film, for example with a layer thickness of less than 0.5 mm, particularly less than 0.3 mm. Such substrates are inexpensive to produce and versatile in their applications.

[0033] Decorative films are particularly versatile and can be applied to different surfaces.

[0034] Suitable plastics for the substrate include polyolefins such as high- and low-density polyethylene (PE) or polypropylene (PP). Other suitable materials include polyvinyl chloride (PVC), polystyrene (PS), polyester, polycarbonate (PC), polyethylene terephthalate (PET), and many others.

[0035] It can prove practical if, in step B, the coating is applied to the substrate in a layer thickness in the range of > 5 pm to < 500 pm, preferably in the range of > 10 pm to < 100 pm, preferably in the range of > 20 pm to < 50 pm, preferably as a radiation-curable varnish, preferably as a UV varnish. With such layer thicknesses, REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0036] Opaque decorative effects with a depth of field can be created. Furthermore, the layer thickness in the stressed area proves particularly advantageous with regard to the intended treatment. The layer thickness tends to determine the possibilities for treating the gelled coating.

[0037] A relatively thick coating generally requires a high material input and a long curing time. A relatively thin coating reduces material input but may not provide satisfactory coverage or depth of penetration. Considering various requirements, the selected layer thickness range represents an optimum.

[0038] It can be useful if, in step C, the coating is gelled by irradiation, preferably by irradiation with one of the following radiation sources:

[0039] a. UV emitters with a wavelength of > 200 nm to < 420 nm, preferably > 280 nm to < 420 nm and / or with a radiation dose of > 25 to < 120 mJ / cm² 2 , preferably from > 50 to < 100 mJ / cm² 2 , preferably from > 60 to < 80 mJ / cm² 2, and / or b. low-pressure mercury emitters with (short-wave, monochromatic radiation with) emission lines at 185 and 254 nm and doses of 15 to 600 mJ / cm² 2

[0040] c. Xenon-iodine excimer emitters with a wavelength of 253 nm and / or a preferably adjustable irradiance of 6 to 60 mW / cm² 2 .

[0041] Such radiation sources allow the coating material to be brought into a gelled state on the surface particularly easily and controllably. The wavelength of classic mercury (Hg)-doped UV emitters lies in a broad spectrum of 200–400 nm (especially 250–330 nm).

[0042] It can be advantageous if, in step C, the gloss value of the profile body according to DIN EN ISO 2813: 2015-02, 85° is reduced by at least 10 gloss units, preferably by at least 20 gloss units, and particularly by at least 30 gloss units. This design proves to be particularly advantageous for producing matte surfaces.

[0043] It can prove practical if, in step D, one, several, or all of the surface sections of the gelled coating are mechanically, pneumatically, and / or hydraulically processed, for example, by applying force such as with a roller or compressed air, to disrupt, alter, or break up the gelled surface, particularly by material removal and / or displacement. These methods allow for the creation of three-dimensional, haptically perceptible surface effects that are permanently retained after the coating has fully cured and, in particular, also structure or profile the surface.

[0044] It can be advantageous if, in step D, material is applied to one, several or all of the surface sections of the gelled coating, preferably using an additive process, preferably using a printing process, and particularly preferably using flexographic or inkjet printing.

[0045] This can also result in advantageous shading effects.

[0046] It can prove helpful if the material application is carried out by applying a further coating, the further coating being preferably identical or different to the underlying coating.

[0047] Preferably, the subsequent coating consists of the same coating material as the underlying coating.

[0048] When using an identical coating material, the superimposed coatings are chemically and physically optimally compatible in order to bond well with each other during curing and to behave similarly over a long period of use (aging).

[0049] It may be advantageous if, in step D, one, several, or all of the surface sections are treated by irradiation with at least one radiation source, preferably by irradiation with radiation of different wavelengths and / or different radiation doses, preferably while one, several, or all of the other surface sections are covered with a mask / stencil, wherein the irradiation is particularly preferably carried out by:

[0050] a. UV emitters with a wavelength of > 120 nm to < 230 nm, preferably > 150 nm to < 225 nm, and / or

[0051] b. Low-pressure mercury lamps (preferably for photochemical matting using short-wave, monochromatic radiation), with a wavelength of 185 nm and / or a radiation dose of > 100 to < 1000 mJ / cm² 2 .

[0052] Irradiation can take place before or after material application, material removal, or material redistribution in the respective surface section.

[0053] Irradiating surface sections can produce different surface effects even without physical intervention. The use of REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0054] Masks are particularly advantageous for selectively avoiding unwanted radiation exposure to surface areas other than those being treated.

[0055] It can prove useful if, in step D, one, several or all of the surface sections are microstructured by excimer folding.

[0056] Excimer folding allows for the creation of particularly sophisticated surface effects. Excimer irradiation results in finer folding (softer feel) and a change in gloss level at an 85° angle. Excimer folding can be performed before or after material application, material removal, or material redistribution within the respective surface area.

[0057] It may be advantageous to initiate excimer folding by irradiation with monochromatic light of wavelength p < 200 nm (and optionally subsequently by irradiation with monochromatic light), preferably by an excimer emitter with emission lines in the range of 172 to 222 nm and / or with doses of 0.5 to 10 mJ / cm² 2This occurs. Such radiation parameters have proven particularly advantageous for excimer folding.

[0058] It can prove beneficial to subsequently cure the coating microstructured using excimer technology by means of UV or electron irradiation.

[0059] It can be practical if at least one of the surface sections is left untreated to harden in step D.

[0060] It can prove advantageous if the at least two surface sections of the gelled coating form a regular or arbitrary pattern, preferably in at least one of the following embodiments:

[0061] a. one, several or all of the surface sections is / are striped, mottled, polygonal, circular, oval or dot-like.

[0062] b. one, several or all of the surface sections extend parallel to the profile axis of the profile.

[0063] c. one or more of the surface sections is / are island-shaped and surrounded by one or more of the other surface sections.

[0064] d. The surface sections imitate a wood grain or marbling. REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0065] A surface section can have several separate sub-areas, which are preferably processed in the same way in step D.

[0066] It is also advantageous if one or more of the surface sections exhibit different surface roughness according to DIN EN ISO 25178-2:2023-09. Surface roughness, as defined in the invention, is characterized by a sequence of peaks and valleys with varying heights, depths, and spacings on the surface sections. Surface roughness is defined as the shorter frequency of the actual surface area relative to the valleys. DIN EN ISO 25178-2:2023-09 comprises a collection of international standards for the analysis of surface roughness, in particular two measurement methods: a contact measurement method (using a probe) and a non-contact measurement method (using an optical probe). This dual approach solves problems previously encountered with the profile method, namely the variation in measurement results depending on the measuring side and the scanning device.

[0067] It is further advantageous that the at least two surface sections have a surface roughness S a (mean arithmetic height) of approximately 1 pm to 25 pm, preferably 2 pm to 25 pm, particularly preferably 2 to 20 pm according to DIN EN ISO 25178-2:2023-09. This allows for the cost-effective and economical production of different optics and / or haptics of the surface sections. This can be very well characterized by the measured value S a The so-called mean arithmetic height is a parameter that extends the line roughness parameter Ra (arithmetic mean) to the surface. It represents the magnitude of the height difference at each point compared to the arithmetic mean of the surface. This parameter is generally used to assess surface roughness.

[0068] It is also advantageous that the at least two surface sections have a surface roughness Spc (arithmetic mean of the specific curvature) of approximately 2.5 1 / mm to 401 / mm, preferably 5.0 1 / mm to 35 1 / mm, particularly preferably 5.0 to 301 / mm according to DIN EN ISO 25178-2:2023-09. This can be determined by the characteristic value S pc , the arithmetic mean of the specific curvature. This parameter represents the arithmetic mean of the principal curvature of the peaks on the surface. A small value means that the contact points with other objects have a rounded shape. A larger value means that the contact points with other objects are pointed. REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0069] A further advantage is that the surface sections have different surface structures. It has proven advantageous that the surface sections have a maximum roughness depth R. t or R max from approximately 5 pm to 200 pm, preferably 10 pm to 150 pm, particularly preferably 15 to 100 pm, preferably a maximum of 10 pm according to ISO 21920-2:2021-12. The maximum roughness depth Rtbzw.

[0070] Rmax is the vertical difference between the deepest groove and the highest peak within the total measuring distance.

[0071] It is also advantageous that surface sections can be produced using the method according to the invention, which have a surface structure similar to food.

[0072] Graining refers to the structuring of a surface, which is essential for its haptic and visual properties. It is characterized by an irregular geometric variation in the surface topography / surface texture.

[0073] Further advantageous embodiments result from combinations of the features disclosed in the claims, the description and the figures.

[0074] Terms and definitions

[0075] Fishing

[0076] Gelling is a term from the field of surface coating and means pre-hardening or partial drying, so that the coating is no longer fluid but not yet fully cured. Gelling is used, among other things, in powder coating, the application of inks, paints, varnishes, etc.

[0077] Depending on the coating material, heat or radiation sources used for gelling include, for example, hot air generators, IR radiation, and UV radiation. By controlling the heat / radiation intensity and / or the exposure time to the coating, gelling of the coating is achieved instead of complete curing.

[0078] Brief description of the characters

[0079] They show:

[0080] Fig. 1: A schematic perspective view of a semi-finished product, intermediate product, or final product of the inventive process, wherein a radiation-curable coating is applied over the entire surface of an extruded plastic substrate. REHAU Industries SE & Co. KG 08.05.2025 Int. Mark: 25.042 / 1 dr.rin-aj

[0081] is angled, wherein the coating has two strip-shaped surface sections extending parallel to the profile axis, wherein in one of the angled surface sections a further coating is applied in an additive process.

[0082] Fig. 2: a schematic perspective view of another semi-finished product or

[0083] intermediate or end product of the process according to the invention, wherein a radiation-curable coating is applied over the entire surface of an extruded plastic substrate and gelled, wherein the coating has two strip-shaped surface sections extending parallel to the profile axis, wherein material is removed in one of the gelled surface sections.

[0084] Fig. 3 shows a schematic perspective view of another semi-finished product or...

[0085] intermediate or end product of the inventive method, wherein a radiation-curable coating is applied over the entire surface of an extruded plastic substrate and gelled, wherein the coating has a surface section with island-shaped sub-areas that are completely surrounded by the other surface section, wherein the surface section with island-shaped sub-areas has been subjected to further radiation treatment after the gelling of the coating, while the other surface section is covered by a radiation-impermeable mask / stencil (not shown).

[0086] Fig. 4 in view (a) is a top view of a pattern of a decorated profile body produced according to the invention (designation “PAG stencil 1 (# 132) Micro”), wherein, for the production of the pattern, in steps C and D, partial gelation of the coating was carried out using a PAC emitter, in particular through openings (in areas 2, 3 and 5) of a stencil arranged on the coating, while the other surface areas of the coating (areas 2 and 4) were covered by the stencil, wherein (full) surface excimer irradiation of the coating then took place, wherein surface roughness values ​​were subsequently measured in five different surface areas of the coating, which are designated “Area 1” to “Area 5”; wherein view (b) shows the corresponding measured values ​​of the surface roughness according to ISO 25178 in areas 1 to 5. REHAU Industries SE & Co. KG 08.05.2025 Int. Mark: 25.042 / 1 dr.rin-aj

[0087] Fig. 5 in view (a) shows a top view of another pattern of a decorated profile body produced according to the invention (designation “PAC stencil 1 (# 123) Micro”), wherein, for the production of the pattern, in steps C and D, a partial gelation of the coating was carried out using a PAC emitter, in particular through openings (in areas 2 and 4) of a stencil arranged on the coating, while the other surface areas of the coating (areas 1 and 3) were covered by the stencil, wherein a (full) surface excimer irradiation of the coating then took place, wherein surface roughness values ​​were subsequently measured in four different surface areas of the coating, which are designated as “area 1” to “area 4”; wherein view (b) shows the corresponding measured values ​​of the surface roughness according to ISO 25178 in areas 1 to 4.

[0088] Detailed description of preferred embodiments

[0089] The preferred embodiments of the invention are described in detail below with reference to the accompanying figures.

[0090] The invention relates to a method for producing a decorated profile body 1 in the form of a decorated furniture foil. The method comprises the following steps:

[0091] Step A

[0092] In step A of this process, an extruded plastic film is first provided as substrate 2. The film has, for example, a thickness of 0.2 mm or 200 µm. The plastic film is produced, for example, using a known extrusion process. The film can be single-layered or multi-layered.

[0093] To facilitate attachment to furniture, the foil can be provided on the underside, i.e. on the side facing away from coating 3, with an adhesive layer such as a thermally activated hot melt adhesive layer (not shown).

[0094] The profile axis PA of substrate 2 corresponds to the extrusion direction and runs along the X-axis. The thickness of substrate 2 and coating 3 is measured along the Z-axis. The surface of substrate 2 and the resulting profile body 1 lies in the X-Y plane. Suitable plastics for substrate 2 include PE, PP, PVC, PS, polyester, PC, PET, and many others.

[0095] Step BREHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0096] In step B, a radiation-curable coating 3, e.g. in a layer thickness of 0.04 mm or 40 pm, is then applied over the entire surface of the substrate 2.

[0097] The thickness of substrate 2 is therefore several times, in this case five times, the thickness of coating 3. Substrate 2 is thus the structural element of the decorated profile body 1. Suitable coatings include, for example, all common UV lacquers.

[0098] Step C

[0099] In step C, the coating 3 is fully gelled or cured, for example by irradiation with a radiation source. UV light with a wavelength between 280 nm and 420 nm at a radiation dose of 60 to 80 mJ / cm² is particularly suitable for UV coatings. 2 . . . It is also possible, for example, to irradiate the coating 3 using a low-pressure mercury emitter with emission lines at 185 and 254 nm and doses of 15 to 600 mJ / cm². 2 .

[0100] This process brings the coating 3 into a partially malleable, honey-like, and not yet fully cured state, in which a surface effect on individual surface sections 4, 5 is retained even in the fully cured state, in order to achieve different surface effects. During gelling, the gloss value Y of the coating 3 can be reduced by more than 30 gloss units GU according to DIN EN ISO 2813: 2015-02, 85°. This allows matte surfaces to be created.

[0101] Other exemplary radiation sources for irradiating coating 3 in step C and / or individual, several or all surface sections 4, 5 in step D are:

[0102] PAC spotlight:

[0103] A PAC emitter is a monochromatic, low-pressure mercury emitter with an emitting wavelength of 254 nm, preferably adapted to classic photoinitiators used in UV coatings. A PAC emitter is generally not adjustable. Different energy levels are preferably achieved by switching a specific number of emitters on and off. Typically, 8-10 emitters are contained in a single unit.

[0104] In comparison to classic Hg-UV lamps used for curing paints, a PAC lamp also has a very low power of 1 V / cm and a very low power of 50-60 mW / cm. 2 Hg-UV lamps typically operate at 2000-3000 mW / cm². 2and result in 95-100% double bond conversion, which means complete polymerization of the coating. A double bond conversion of only 50-60% means that the coating does not harden completely. The coating remains liquid or honey-like; the viscosity is only increased superficially. REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0105] The increase in viscosity is barely measurable, however, as the penetration depth of the PAC emitter is only a few millimeters. With increasing viscosity, the folding decreases under subsequent excimer irradiation at 172 nm. Instead of becoming rough, the texture becomes soft, and the gloss increases at an 85° angle, while remaining almost constant at a 60° angle.

[0106] Xenon-iodine excimer emitter 253nm:

[0107] The advantage of an excimer lamp compared to a PAC lies in its superior adjustability, as the lamp can be regulated via a potentiometer. Furthermore, the lamp requires less space and can be operated under an inert atmosphere in an excimer tunnel using a 172 nm excimer lamp. In contrast, a PAC lamp can only be operated in an atmospheric environment.

[0108] The radiation dose and polymerization degree of the xenon-iodine excimer lamp are analogous to those of the PAC lamp. In contrast to the excimer lamp, which contains only xenon molecules and emits at 172 nm, resulting in a 95-100% double bond conversion and thus wrinkling the paint surface (penetration depth, however, is only 1.5 pm compared to the classic UV lamp), this PAC alternative contains xenon-iodine molecules that emit at 253 nm and thus lead to an increase in the viscosity of the paint surface, similar to PAC.

[0109] Ga-spotlights:

[0110] However, a disadvantage of the gas emitter for gelling the paint is its high power output, which is often not sufficiently controllable / throttleable.

[0111] LED:

[0112] A disadvantage of LED spotlights is their strong dependence on the surface, e.g., different reflection depending on whether the surface is white or black.

[0113] The effect of the gelation in step C with a xenon-iodine excimer emitter corresponds to that of the PAC emitter: The radiation is monochromatic at a wavelength of 253 nm.

[0114] The irradiance is adjustable from 6 to 60 mW / cm² 2 , possibly also via a gap, since the surface of the radiator only has a temperature of 40 °C.

[0115] Step D

[0116] In step D, at least two surface sections 4, 5 of the gelled coating 3 are treated differently before complete curing, such that the surface properties of the coating 3 in the differently treated surface sections 4, 5 differ in the cured state, particularly visually, especially with regard to the gloss behavior at a shallow angle and / or the feel and / or the softness. REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0117] Different treatments of surface sections 4, 5 are explained below by way of example using the variants shown in Figures 1, 2 and 3.

[0118] Fig. 1 shows a schematic perspective view of a substrate 2 with a coating 3 applied over the entire surface and gelled.

[0119] Substrate 2 is a plastic extrusion profile that was extruded in one extrusion direction along a profile axis PA.

[0120] Coating 3 is a UV-curable lacquer containing conventional photoinitiators that cure upon exposure to UV light. Coating 3 comprises two strip-shaped surface sections 4 and 5 extending parallel to the profile axis PA.

[0121] In one of the strip-shaped surface sections 5, a further coating 6 made of identical coating material is applied to the already gelled coating 3 using an additive process, e.g. flexographic printing, inkjet technology.

[0122] No material is applied to the other surface section 4.

[0123] As a result, the surfaces of the two surface sections 4 and 5 are slightly offset from each other, as shown. The entire coating 3, including the two angled surface sections 4 and 5, as well as the further coating 6, is subsequently subjected to excimer curing.

[0124] The additional coating 6 applied after the gelation exhibits a different gloss behavior at a shallow angle as well as a different feel / softness than the untreated surface section 4.

[0125] Fig. 2 shows - like Fig. 1 - a schematic perspective view of a substrate 2 with a coating 3 applied over the entire surface and gelled.

[0126] The coating 3 also includes two strip-shaped surface sections 4, 5, which extend parallel to the profile axis PA.

[0127] In contrast to Fig. 1, however, in one of the strip-shaped surface sections 4 material has been removed or displaced, in particular by the application of force such as by a roller or by compressed air, in order to destroy, alter or break up the gelled surface.

[0128] No material removal takes place in the other surface section 5.

[0129] As a result, the surfaces of the two surface sections 4 and 5 are slightly offset from each other, as shown. REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0130] Analogous to Fig. 1, the entire coating 3 is again subjected to subsequent excimer curing. The surface section 4 treated by material removal after gelation therefore also exhibits a different gloss behavior at shallow angles as well as a different feel / softness than the untreated surface section 5.

[0131] In the variants of Figures 1 and 2, the differently treated surface sections 4, 5 of the gelled coating 3 form a regular striped pattern.

[0132] However, other patterns can also be represented. For example, it is possible for a surface section 5 to have several separate sub-areas with identical surface properties, as shown in Fig. 3.

[0133] Fig. 3 shows - like Fig. 1 and 2 - a schematic perspective view of a substrate 2 with a coating 3 applied over the entire surface and gelled.

[0134] Unlike Figures 1 and 2, the coating 3 in Figure 3 has a surface section 5 with island-shaped sub-areas, each of which is completely surrounded by the other surface section 4. After the coating 3 has gelled, the surface section 5 with the island-shaped sub-areas is subjected to further radiation treatment, e.g., excimer curing.

[0135] To precisely limit the irradiation of coating 3 to the surface section 5 to be treated and its sub-areas, the other, surrounding surface section 4 is covered by a radiation-impermeable mask / stencil (not shown) during irradiation. Subsequently, both surface sections 4 and 5 are cured, e.g., by irradiation with UV light.

[0136] The different treatment of the surface sections 4, 5 in step D of the inventive method results in a subtle surface effect or

[0137] It creates a décolletage effect that only appears from defined angles.

[0138] This creates a shading effect. This effect remains permanently after the coating 3 has fully cured. In this way, a decorated profile body with differently textured surface properties can be produced with minimal effort.

[0139] Surface roughness

[0140] Figures 4 and 5 show surface roughness measurements according to ISO 25178 on two different samples of decorated profile bodies produced according to the inventive method. In steps C and D of the manufacturing process, the coating was partially gelled using a PAC emitter through a stencil positioned on the coating. This was followed by full-surface excimer irradiation of the partially gelled coating. The stencil had (circular) openings in areas 2, 3, and 5 of the sample in Figure 4 and in areas 2 and 4 of the sample in Figure 5. Thus, the coating of the sample in Figure 4 was gelled by PAC irradiation only in areas 2, 3, and 5, and the coating of the sample in Figure 5 was gelled only in area 2. Areas 1 and 4 of the pattern according to Fig. 4 and areas 1 and 3 of the pattern according to Fig.Five areas were obscured by the template. Therefore, no gelation from PAC irradiation occurred in these areas.

[0141] The following parameters were determined on the two samples shown in Figs. 4 and 5 when measuring the surface roughness according to ISO 25178:

[0142] Sa (mean arithmetic height)

[0143] This parameter is an extension of the line roughness parameter Ra (arithmetic mean) to the surface. It represents the magnitude of the height difference at each point compared to the arithmetic mean of the surface. This parameter is generally used to assess surface roughness.

[0144] Sz (maximum height)

[0145] This parameter is defined as the sum of the height value of the highest peak and the height value of the deepest depression within the definition area.

[0146] Str (aspect ratio of the surface texture)

[0147] This parameter is a measure of the uniformity of the surface texture. This value is obtained by dividing the horizontal distance in the direction where the automatic correlation function decays most rapidly (according to Sal) to the value [s] (default: 0.2) by the horizontal distance in the direction where the automatic correlation function decays most slowly to the value [s].

[0148] Spc (arithmetic mean of tip curvature)

[0149] This parameter represents the arithmetic mean of the principal curvature of the peaks on the surface. A small value means that the contact points with other objects have a rounded shape. A larger value means that the contact points with other objects are pointed. REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0150] Sdr (Developed Interface Ratio)

[0151] This parameter represents the percentage of the additional area of ​​the definition domain attributable to the texture, compared to a perfectly flat definition domain. The Sdr value of a completely flat surface is 0. If a surface has a slope, the Sdr value increases. For an example reference surface defined as a plane with a 45-degree slope, the Sdr value is 0.414. This means that the surface area is increased by slightly more than 40%.

[0152] Gloss measurement

[0153] In a further experiment, five samples of decorated profile bodies produced according to the invention were subjected to a gloss measurement:

[0154] 1 Additive application Flexographic printing (RV crystal titanio)

[0155] Additive application with a structured rubber roller (flexo roller) onto a gelled surface - followed by excimer coating across the entire surface.

[0156] 2 Subtractive application. Flexographic printing (RV crystal titan.)

[0157] Subtractive application with a structured rubber roller (flexo roller) into a gelled surface - followed by excimer coating over the entire surface

[0158] 3 PAC template 1

[0159] Partial PAC gelation using a template - followed by PAC+excimer over the entire area

[0160] 4 PAC template 2 (#123)

[0161] Partial PAC gelation using a template - followed by full-surface excimer gel application.

[0162] 5 PAC template 3 (#132)

[0163] Partial PAC gelation using a template - followed by full-surface excimer gel application.

[0164] The gloss level was determined according to DIN EN ISO 2813* (02 / 2015) as an average of five values ​​(BYK micro TRI gloss).

[0165] The measuring device was positioned so that it detected either a small amount of structure (e.g., within a circle) or a larger amount (e.g., at the edge of the circle) in the center. Since the length of the measuring range is approximately 6 cm, both structures are always within the measurement range. REHAU Industries SE & Co. KG 08.05.2025 Int. Ref: 25.042 / 1 dr.rin-aj

[0166] For info:

[0167] - 20° -> For high-gloss coatings that exhibit gloss values ​​greater than approximately 70 GU (gloss units) at the 60° measurement geometry

[0168] - 85° -> For matte coatings that exhibit gloss values ​​lower than approximately 10 GU (gloss units) at the 60° measurement geometry

[0169] Table 1 below contains the test results of the gloss measurement according to DIN EN ISO 2813* (02 / 2015) at 20°, 60° and 85°:

[0170] Pattern 20° 60° 85°

[0171] 1-1 little structure 1.4 4.6 36.3

[0172] 1-2 more structure 1.4 4.7 33.7

[0173] 1-3 more structure 1.3 4.4 28.8

[0174] 1-4 more structure 1.3 4.4 28.0

[0175] 1-5 little structure 1.4 4.4 36.7

[0176] 2-1 little structure 1.5 5.0 39.5

[0177] 2-2 more structure 1.7 5.7 37.9

[0178] 2-3 more structure 1.7 5.7 37.5

[0179] 2-4 little structure 1.6 5.2 36.8

[0180] 3-1 little structure 0.2 2.8 28.6

[0181] 3-2 little structure 0.2 2.8 26.7

[0182] 3-3 more structure 0.2 3.0 36.8

[0183] 3-4 more structure 0.2 3.1 37.6

[0184] 4-1 little structure 0.2 2.9 36.0

[0185] 4-2 little structure 0.2 3.0 33.6

[0186] 4-3 more structure 0.2 3.2 5.7

[0187] 4-4 more structure 0.2 3.2 6.2

[0188] 5-1 little structure 0.2 2.9 38.3

[0189] 5-2 little structure 0.2 2.8 20.9

[0190] 5-3 more structure 0.3 3.3 6.5

[0191]

[0192] 5-4 more structure 0.2 3.2 6.3

[0193] Table 1 Test results of the gloss measurement according to DIN EN ISO 2813* (02 / 2015)

[0194] The exemplary embodiments are not to be understood as limiting. Any further exemplary embodiments are possible within the scope of the claims. REHAU Industries SE & Co. KG 08.05.2025

[0195] International reference: 25,042 / 1 dr.rin-aj

[0196] Reference symbol list

[0197] 1 Profile body

[0198] 2 Substrat

[0199] 3 coating

[0200] 4 First surface section of the coating 5 Second surface section of the coating 6 Further coating

[0201] PA profile axle

[0202] X X-axis (extrusion direction)

[0203] X Y-axis (width)

[0204] Z Z-axis (height)

Claims

REHAU Industries SE & Co. KG Rehau, May 8, 2025 Int. Ref: 25.042 / 1 dr.rin-aj Patent claims 1. Method for producing a decorated profile body (1) with sectionally different surface properties, especially for the furniture industry, comprising the steps: Step A: Providing a substrate (2); Step B: Applying a curable coating (3) to the substrate (2); Step C: Angeling the coating (3); Step D: Treating at least two surface sections (4, 5) of the gelled coating (3) in different ways, such that the surface properties of the coating (3) differ in the differently treated surface sections (4, 5) in the cured state.

2. Method according to the preceding claim, characterized in that in step A the substrate (2) is made from a polymeric material, preferably from plastic, preferably as an extruded or calendered profile, particularly preferably as an edge banding or wall connection profile, or as a film, for example with a layer thickness of less than 0.5 mm, in particular less than 0.3 mm.

3. Method according to one of the preceding claims, characterized in that in step B the coating (3) is applied to the substrate (2) in a layer thickness in the range of > 5 pm to < 500 pm, preferably in the range of > 10 pm to < 100 pm, preferably in the range of > 20 pm to < 50 pm, preferably as a radiation-curable varnish, preferably as a UV varnish.

4. Method according to one of the preceding claims, characterized in that in step C the coating (3) is gelled by irradiation, preferably by irradiation with at least one of the following radiation sources: a. UV emitters at a wavelength of > 200 nm to < 420 nm, preferably from > 280 nm to < 420 nm and / or at a radiation dose of > 25 to <REHAU Industries SE & Co. KG Rehau, den 08.05.2025 Int. Zeichen: 25.042 / 1 dr.rin-aj 120 mJ / cm 2 , preferably from > 50 to < 100 mJ / cm² 2 , preferably from > 60 to < 80 mJ / cm² 2 . b. Low-pressure mercury emitters with emission lines at 185 and 254 nm and doses of 15 to 600 mJ / cm² 2 c. Xenon-iodine excimer emitters with a wavelength of 253 nm and / or a preferably adjustable irradiance of 6 to 60 mW / cm² 2 .

5. Method according to one of the preceding claims, characterized in that in step C the gloss value (Y) of the profile body (1) according to DIN EN ISO 2813 : 2015-02, 85° is reduced by at least 10 gloss units (GU), preferably by at least 20 gloss units (GU), in particular by at least 30 gloss units (GU).

6. A method according to one of the preceding claims, wherein in step D one, several or all of the surface sections (4, 5) of the gelled coating (3) are mechanically and / or pneumatically and / or hydraulically processed, for example by applying force such as by a roller or by compressed air, in order to destroy, alter or break up the gelled surface, in particular by material removal and / or material displacement.

7. Method according to one of the preceding claims, characterized in that in step D a material is applied to one, several or all of the surface sections (4, 5, 6) of the gelled coating (3), preferably by printing, preferably by flexographic printing or inkjet printing.

8. Method according to the preceding claim, characterized in that the material application is carried out by applying a further coating (7), wherein the further coating (7) is preferably identical or different to the underlying coating (4).

9. Method according to one of the preceding claims, characterized in that in step D one, several or all of the surface sections (4, 5) are treated by irradiation with at least one radiation source, preferably by irradiation with radiation of different wavelengths and / or different radiation doses, preferably during one, several or REHAU Industries SE & Co. KG Rehau, May 8, 2025 Int. Ref: 25.042 / 1 dr.rin-aj all of the other surface sections (4, 5) are covered with a mask / stencil, the irradiation being particularly preferably carried out by one of the following radiation sources: a. UV lamps with a wavelength of > 120 nm to < 230 nm, preferably > 150 nm to < 225 nm, and / or b. low-pressure mercury lamps, preferably for photochemical matting, preferably with a wavelength of 185 nm and / or a radiation dose of > 100 to < 1000 mJ / cm² 2 .

10. Method according to one of the preceding claims, characterized in that in step D one, several or all of the surface sections (4, 5) are microstructured by excimer folding.

11. Method according to the preceding claim, characterized in that the excimer folding is carried out by irradiation with monochromatic light of wavelength p < 200 nm and / or with doses of 0.5 to 10 mJ / cm² 2 This is done preferably by an excimer emitter with emission lines in the range of 172 to 222 nm.

12. Method according to the preceding claim, characterized in that the coating microstructured by excimer technology is subsequently cured by UV or electron irradiation.

13. Method according to one of the preceding claims, characterized in that in step D at least one of the surface sections (4, 5) is left untreated to harden.

14. Method according to one of the preceding claims, characterized in that the at least two surface sections (4, 5) of the gelled coating (3) form a regular or random pattern, preferably in at least one of the following embodiments: a. one, several or all of the surface sections (4, 5) is / are striped, mottled, polygonal, circular, oval or dot-like. b. one, several or all of the surface sections (4, 5) extend parallel to the profile axis (PA) of the profile (1). REHAU Industries SE & Co. KG Rehau, May 8, 2025 Int. Ref: 25.042 / 1 dr.rin-aj c. one or more of the surface sections (4, 5) is / are island-shaped and surrounded by one or more of the other surface sections (4, 5). d. the surface sections (4, 5) imitate a wood grain or marbling.