Monolayer coating and method for manufacturing articles with black appearance
The monolayer coating addresses mechanical and chemical limitations of existing deep black coatings by using a top-area with low absorption and a gradual absorber-area, achieving high gloss and improved resistance with minimal interference.
Patent Information
- Application Number
- PCT/EP2026/076414
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-09-03
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-12
AI Technical Summary
Existing deep black high gloss PVD coatings suffer from mechanical and chemical limitations due to density gradients and amorphous carbon structures, leading to low abrasion resistance and inhomogeneous appearance on 3D-surfaces, with CIELab L* values typically below 30, and interference effects from sudden refractive index changes.
A monolayer coating design with a top-area of low absorption and an absorber-area with a gradual absorption coefficient increase, avoiding internal optical reflection interfaces, using materials like SiO2 for the top-area and adding absorber elements to achieve high gloss and mechanical stability.
The monolayer coating achieves deep black surfaces with high gloss and improved mechanical and chemical resistance, minimizing interference effects and maintaining surface smoothness, with CIELab L* values potentially exceeding 28.
Smart Images

Figure EP2026076414_12112026_PF_FP_ABST
Abstract
Description
Monolayer Coating and method for manufacturing articles with black appearance.
[0001] Coatings may be used to enhance aesthetic appearance and / or color of the surfaces of objects. In particular deep black is one application area where PVD coatings are successfully utilized. Reflectance and gloss are important parameters with which the optical appearance of essentially unstructured surfaces is described.
[0002] In order to achieve deep black surfaces, the reflection percentage of the light which impinges onto the surface needs to be low and well adopted to the spectral intensity distribution of such light. For example if only red light is impinging onto the surface of an object and the surface efficiently absorbs red light the object will appear black. If white light impinges onto the surface of an object efficiently absorbing red and blue light, but not or less efficiently absorbs green light the object will appear green.
[0003] Existing deep black high gloss PVD coatings are often based on density gradients and / or high amounts of carbon incorporated into the coating to reduce difference in the refractive index of the coating at the interface between air and coating and to achieve sufficient absorption in the visible spectrum. This limits the chemical, mechanical and optical properties that such coatings can achieve due to the reduced density and / or amorphous carbon structures created. Typically the lower the reflection, the lower the mechanical properties and the oxidation resistance. Existing decorative black coatings are known to have low abrasion resistance due to low surface hardness caused by density gradient. Existing decorative black PVD coatings often suffer from inhomogeneous appearance of 3D-surfaces due to bias effects or gas-availability effects.
[0004] Typically the minimum D65 (SCI) CIELab L* value of PVD / CVD coatings according to state of the art is about 30 where lower L*-values are being achieved by nanostructured surfaces that are even more fragile from mechanical and chemical perspectives.
[0005] Hereby D65 is the standard illuminant with a color temperature of about 6504 K, representing the average daylight. SCI (Specular Component Included) is the measurement mode in which specular refections are included – commonly used in color measurement to minimize the influence of surface textures.CIELab L*is the lightness component in the CIELab color space, ranging from0(perfect black) to100(perfect diffuse white under D65). Decorative PVD / CVD black coatings compatible with high gloss appearance with CIELab SCI L*-values < 28 are not known.
[0006] Gloss level is a quantitative measure of how much light is reflected in a specular (mirror-like) direction from a surface compared to a reference standard. It describes the surface’s ability to produce distinct, mirror-like reflections rather than scattering light diffusely.
[0007] In order to measure the gloss level a so called glossmeter is used. A glossmeter directs a beam of light onto the surface at a fixed incident angle (commonly 20°, 60°, or 85°).
[0008] A detector measures the intensity of the light reflected at the equal but opposite specular angle. The result is compared to a calibrated reference standard — usually a piece of polished black glass defined as 100 gloss units (GU) at 60°.
[0009] As mentioned different measurement angles may be used. Standards such as ISO 2813 and ASTM D523 define the following:
[0010] 60° – universal angle for medium-gloss surfaces.
[0011] 20° – used for high-gloss surfaces to improve differentiation in the upper range.
[0012] 85°– used for low-gloss or matte surfaces to improve sensitivity.
[0013] The measurement results are expressed in Gloss Units (GU).
[0014] The following classification is typically used:
[0015] < 10 GU (at 60°) matte finish
[0016] 10–70 GU (at 60°) semi-gloss or satin
[0017] > 70 GU** (at 60°) high gloss
[0018] The scale is relative: a reading of 100 GU matches the polished glass standard, and higher values are possible for extremely reflective materials like mirrors or polished metals.
[0019] WO2024133736 does describe a coating system consisting of a deep black layer combined with a hard and transparent toplayer. However, achieving the deep black combined with high gloss without generating unwanted interference effects detrimental for the decorative purpose, is still a challenge. The disclosed example in WO2024133736 wherein the deep black absorber layer has a different O:N ratio as compared to the ratio in the hard and transparent toplayer has shown limited compatibility on low roughness (mirror polished) surfaces. It is assumed that somewhere within the deep black absorber an optically relevant interface is created leading to a sudden variation of the index of refraction and therefore in combination with the air / coating interface potentially leading to visible interference effects.
[0020] Such sudden variation might be made visible with a calocut, showing a clear and fine circle within the area of the deep black absorber where actually a smooth change of shading is ideally expeced.
[0021] Practically, the method as suggested in WO2024133736 for producing these coatings reaches its limits when the cathodes operate near to the transition zone as this will always cause a fast non-continuous change of coating composition and thereby may induce optical interfaces.
[0022] One approach to address these issues would be to avoid smooth interfaces as such interface roughnesses decrease specular reflection and to a certain level counteract and prohibit interference effect. In such case however the objects fail to appear as high gloss objects.
[0023] Inspection of the calocut of such a coating might show a smeared out area of transition as is typical for non-polished interfaces.
[0024] US2002146570A1 describes a functional film with a transition layer comprising a first constituent and a second constituent. The first constituent is at least one dielectric material selected from the group consisting of SiOx (x>1), MgF2, CaF2, Al2O3, SnO2, In2O3and ITO, and the second constituent is at least one material selected from the group consisting of iron (Fe), cobalt (Co), titanium (Ti), vanadium (V), aluminium (Al), silver (Ag), silicon (Si), germanium (Ge), yttrium (Y), zinc (Zn), zirconium (Zr), tungsten (W) and tantalum (Ta).
[0025] To overcome these issues, a new inventive coating design is presented and a method is described to produce gradient absorber coating areas transferring into dense transparent or semitransparent top areas, both areas together forming an inventive monolayer with minimal and preferably no visible interference effects. A main purpose is to create as compared to the state of the art improved deep black surfaces with high gloss and good mechanical and chemical resistance.
[0026] The objective of the invention is solved by providing an inventive monolayer coating according to main claim. Dependent claims represent favorable embodiments. Disclosed is as well a method for producing the monolayer coating and the use, primarily for decorative purposes on substrates.
[0027] In general, the perception of black is minimization of reflection for all relevant wavelengths of visible light. One way to achieve a minimum of reflection the change of refractive index at an interface needs to be small. The refraction index (RI) taking into account absorption is described as a complex term according to the formula
[0028] RI = n +ik
[0029] where the real part n is the refractive index and the imaginary part k is the extinction coefficient.
[0030] Refractive index n and absorption coefficient k are wavelength (more exactly frequency dependent and depend on each other via the Kramers-Kronig relations. Without going into further detail it might be stated that a material with a strictly frequency-independent refractive index cannot absorb light, because otherwise n(ω) would have to show frequency dispersion. Absorption and dispersion are inseparably linked.
[0031] The special case n(ω)≡1 corresponds to vacuum.
[0032] Another constant value n=1 is mathematically admissible, but physically unrealistic, since no material can be simultaneously transparent and dispersion-free across all frequencies (except vacuum).
[0033] For practically fully transparent materials in the visible spectrum (wavelenth range of from about 400nm to about 700nm), the extinction coefficient k needs to be almost 0. An example for a material coming close to this is SiO2.
[0034] One of the coating materials used in thin film optics with lower refractive index and very low absorption values in the visible regime is MgF2. Its refractive index at 500nm wavelength is about n=1.38 with practically no absorption. A representation for the dispersion relation of this material is plotted in
[0035] Another broadly used coating material is SiO2. With an index of refraction of 1.465 at a wavelength of 500nm, the index is rather low and the material itself and its use is broadly spread. A representation for the dispersion relation of this material is plotted inAlthough it seems to be the first impression, the absorption coefficient of this material is not identical to zero as the representation as given inshows. However for our purposes here it may be assumed to be zero.
[0036] Roughly the air / coating interface with an SiO2 coating provides a jump of index of refraction from approximately 1 to approximately 1.5. This reflection at the interface air / coating by itself therefore would lead for perpendicular incident light in the visible range to a reflection of about 4% (at 0° angle) while the rest of the light is transmitted into the coating.
[0037] When a thin transparent or semitransparent monolayer coating is applied on a substrate it does result in two optical reflection effective interfaces: the first optical reflection effective interface would be air / coating surface and the second optical reflection effective interface would be coating / substrate. The situation is illustrated inThis combination of these two optical reflection effective interfaces can result into unwanted interference effects when applying thin film coatings, especially if these interfaces provide for minor roughness and in particular if the substrate was polished and the outer surface was polished as well after coating, decreasing the roughness.
[0038] In order to clarify terminology, throughout this specification a coating layer is defined as an overlay over an object with essentially homogeneous thickness, such thickness being defined by a first optical reflection effective interface essentially parallel to the original surface of the object and spaced apart from this a second optical reflection effective interface but as well parallel to the original surface of the object.
[0039] “Optical reflection effective interface” hereby means that if light with a wavelength within the visible range impinges on such interface at least some measurable percentage of the light is reflected at the interface. If in contrast there is an effect of absorption only (without reflection) this in the broad sense might as well be an optical effect, however the respective interface does not count as optical reflection effective interface of this specification.
[0040] In addition it is clear that the wavelength of electromagnetic waves depends on the medium it is propagating in, which means that propagating from one medium into another medium might cause a change in the actual wavelength. What remains unchanged is the frequency (as long as the relative velocity of the observer to the medium is not altered and no Dopplereffect occurs). Taking this into account it is hereby stated that whenever throughout this description a wavelength or a wavelength range is adressed, the wavelength or wavelength range of electromagnetic waves propagating in vacuum is meant.
[0041] Absorption properties with respect to electromagnetic waves play a major role within this description. Reflection and / or absorption of light by pure bulk metals or alloys and / or thin pure metal or alloy films might be due to the free moving of valence electrons of these metals or alloys. This however is not true for some compound materials comprising metal atoms and / or ions as chemical elements but not forming metallic surfaces. These might lead to electrically isolating materials (indicating that no metallic character is present) but never the less showing some considerable optical absorption coefficient. In addition, physical vapor deposition might result in small clustering leading locally to metallic behaviour, however on a macroscopic scale not showing metallic character. Whatever the case may be, this will not be discussed in detail in this specification and might even not be relevant for the purpose of this invention. Relevant however is that adding chemical elements, in particular metallic halfmetallic or semiconductor elements to a coating material which previously essentially did not show absorption at all in this visible spectrum could lead to an optical material now showing absorption. In most cases, the more such element is added to, the higher is the absorption coefficient of the material created (and due to the Kramers-Kronig relations as well influencing the index of reflection of the material). If throughout this specification an absorber element and its concentration is described, the actual purpose is to qualitatively describe the absorption properties of the material created by such addition of such chemical element.
[0042] The inventor realized that if he manages to absorb most of the light (and preferably all of it) which transmitted into the coating (as decribed before) before such light itself on its way in direction to the substrate encounters this second optical reflection effective interface, unwanted interference effects can be avoided up to a high degree.
[0043] According to the present invention the inventive monolayer coating along its layer thickness comprises two optically different areas: The first area, forming the air / coating interface can be named as top-area of the inventive monolayer coating. This area essentially consists only of material or materials with an absorption coefficient of essentially zero value in the visible range of the electromagnetic spectrum. Adjacent to this first area and between the original surface of the object and the first area is a second area. This can be named as absorber-area of the inventive monolayer coating. This second area is a material with in direction to the original surface of the object changing material composition thereby gradually increasing the means absorption coefficient. By this a soft gradient of absorption coefficient is formed. It should be noted that the transition from the first area to the second area does not form an optical reflection effective interface according to the definition as given above. It should be noted as well that the gradient as described is not chosen to be so steep that it gives reasons for reflections of light. It should be noted in addition that such gradient needs not to lead to a monotonical increase and / or strictly monotonically increase of the absorption coefficient in direction to the original surface of the object throughout the thickness of the second area of the inventive monolayer coating. Preferred however is a monoton increase and especially prefered is a strictly monoton increase
[0044] Therefore, first area and second area together do not internally comprise an optical reflection effective interface and as such first and second area form a monolayer coating in the sense of the definition as given above.
[0045] The choice of the word object indicates that this is not limited to an uncoated substrate. For example there might be an adhesion layer provided between a substrate and the inventive monolayer coating. As such the substrate together with the adhesion layer can form the object.
[0046] The absorber area is preferably located closer to the substrate than the top area. The coating design enables the coating of a wide variety of substrates and substrate materials, without dependency on optical properties of the substrate. Substrates may be optically intransparent. As described above, most of the light or all of the light which is transmitted into the coating is absorbed on its way in direction to the substrate.
[0047] It should be noted as well that the top-area of the coating preferably provides for tribological and / or mechanical and / or chemical stability against for example wear and or other environmental challenges. SiO2is an excellent choice to provide these properties. However the interface formed by the top-area may as well be an interface to additional materials and especially coatings and / or coating systems. Alternating thin film optical coating systems on the to-area may for example provide for additional multiple optical reflection effective interfaces resulting for example in broadband antireflection coatings in order to further decrease the fresnel reflections significantly below 4%. Alternating thin film multilayer coatings on the top-area can as well provide color filters selectively reflecting specific wavelengths and / or wavelength bands. In the attempt however of realizing such optical thin film coating systems including the inventive monolayer coating it needs to be taken into account that with increase of complexity of the overall coating system the complexity of calculating the optical response of the respective surfaces increases as well and the simple picture as drawn above with respect to the inventive monolayer coating alone might not be straight forward valid any more. However the basic design principle of the inventive monolayer still holds and for its combination with more complex coating systems strong simulation software such as for example Optilayer exist since decades to calculate and optimize a coating system once good starting values are given.
[0048] Coming back to the state of the art as given by WO2024133736 by Keraudy it might be that the intention of Keraudy was to realize a similar coating system as described above. However the inventive monolayer coating not internally comprising an optical reflection effective interface according to the present invention was neither described by Keraudy nor was it realized because the boundary conditions of the method and coating technology as used and described in WO2024133736 did by no way allow such realization.
[0049] Reiterating what was described above: Practically, the method as suggested in WO2024133736 for producing these coatings reaches its limits when the cathodes operate near to the transition zone as this will always cause a fast non-continuous change of coating composition and thereby may induce optical interfaces.
[0050] It is therefore one preferred aspect of the present invention to take measures that if a similar technology as described in WO2024133636 is used it needs to be prohibited that the cathodes operate near to the transition zone.
[0051] The inventors found that preferably sources that provide the transparent or semitransparent part of the coating are not allowed to exhibit a change of operating mode from e.g. metal- to oxide- or even from metal to transition mode as this causes too steep changes in the optical properties of the deposited coating. The inventors found that can be solved by for example two different approaches: i) using a deposition source for the principal element A that does not exhibit such behavior or ii) using one or more source for the principal element A that is constantly in the transition- or oxidemode and a second (or more) source for provision absorber element.
[0052] The inventors found that this for example can be avoided by choosing the absorbing element to be different from the principle element constituting the main part of non-absorbing and therefore transparent part of the coating. Especially for example if two different coating sources are used and the attractiveness of the principal element is higher for the reactive gas as it is for the absorber element and if the gas flow of the reactive gas is limited, the cathode providing the absorber material will be less prone to be poisoned, leading to a stable process with this cathode operating stable in the metallic mode.
[0053] By this for the first time and in contrast to what was described in WO2024133636 a gradual and smooth transition from an absorbing area to a non-absorbing top-area without creating an internal optical reflection effective interface could be realised.
[0054] One embodiment of the present invention therefore relates to a monolayer coating comprising a top-area and an absorber-area characterised in that the top-area is adjacent to the absorber-area and both areas together form a volume not comprising an internal optical reflection effective interface.
[0055] If such a monolayer coating is applied onto a polished substrate, it will, due to the missing surface roughness show high gloss which is desirable. Preferably the coating will be realised in such a manner that a calotest performed on the substrate coated with the inventive monolayer coating will neither show a clear and fine circle defining the transition between the absorber-area and the top-area, nor will it show the smeared out areas as typical for the coatings applied on unpolished surfaces. Most preferably the calotest of such an inventive coating will not optically show any defined transition zone between absorber-area and top-area.
[0056] The increased extinction coefficient is preferably coming from an added absorber element with an extinction coefficient k > 0 in the application relevant wavelength range.
[0057] The core principles are:
[0058] - As long as the change of RI =n+ik (referring to the differential coefficient d(RI) / d(thickness)) inside the coating volume is continuous and sufficiently moderate there is no internal optical reflection effective interface realised and the light propagating within the coating in direction to the original surface of the object is more and more absorbed without being reflected.
[0059] If there are any discontinuities caused by e.g. the production technique, the “RI-steps” from one depth to the next, these discontinuities need to be small enough in order not to give effect to significant residual reflection. Preferably, a coating design without discontinuities should be realized.
[0060] - The combination of absorption strength of the respective k(depth) profile and the overall minimum thickness of the absorber-area needs to be chosen that preferably all light that enters into the coating volume will be absorbed before reaching the interface coating / substrate.
[0061] In other words the amount and / or thickness required of the absorber-area will depend on the value and profile of the extinction coefficient k as a function of distance from the air / coating interface. With material within the absorber-area providing for high k values the thickness / amount of the absorber area can be chosen smaller compared to a material with lower value of k, however always taking into account that the change in k along the path of the propagating light must be chosen so moderate that it may not establish an internal optical reflection effective interface.
[0062] By applying these design principles virtually no light will reach an optical reflection effective internal interface and there will be no influence of such light on the reflection caused by the top-area / air interface.
[0063] The material of the top-area of the inventive monolayer coating may preferably be selected among materials which are transparent or semitransparent. Suitable materials for the top layer may therefore include oxides and / or nitrides and / or fluorides or combinations thereof formed with one or several elements among for example Mg, Na, Nb, Si, Al, Zr, Y, Hf, Ti, Ta, and / or Ga. In particular, oxides, oxynitrides and nitrides of Si are particularly useful for black appearance, as these compounds on the basis of Si show a low refractive index n resp. RI which can be easily adjusted by the oxygen to nitrogen ratio in the compound. In a particularly preferred embodiment, the top-area is formed by SiO2.
[0064] In other embodiments, the top-area may include oxynitrides and / or nitrides formed with one or several elements among Si, Al, and Ga. These elements are known to form transparent or semitransparent oxynitrides and nitrides.
[0065] The top layer may also be a carbide, an oxycarbide, a carbonitride or an oxycarbonitride of Si, which are transparent.
[0066] The main chemical element or combination of chemical elements present in the top-area of the inventive monolayer coating is referred to as the principal element and designated letter A. Possible principal elements are described in Table 1. Preferably, the top-area can therefore be an oxide, an oxynitride or a nitride of the principal element in the case of Si, Al, Zr, Y, Hf, Ti, Ta and / or Ga. However Mg and Nb (not shown in the table should be taken into account as well. The top-area can be an oxynitride or a nitride of the principal element in the case of Si, Al, and / or Ga. If the principal element is Si, then the compound of the top-area may also be a carbide, an oxycarbide, a carbonitride or an oxycarbonitride.
[0067] The absorber-area is located below the top-area and in direct contact with the top-area layer, thus contiguous with the top-area. To avoid sudden changes in the optical properties, it is preferable that the absorber-area is based on the same principal element as the principle element in the top-area.
[0068] It is preferred for the continuity of optical properties that the absorber-area comprises oxygen, when the top-area is an oxide, or that the absorber-area comprises oxygen and nitrogen when the top-area is an oxynitride, or that the absorber-area comprises nitrogen when the top-area is a nitride, or that the absorber-area comprises carbon when the top-area is a carbide, or that the absorber-area comprises oxygen and carbon when the top-area is an oxycarbide, or that the absorber-area comprises oxygen, carbon and nitrogen when the top-area is an oxycarbonitride, or that the absorber-area comprises carbon and nitrogen when the top-area is a carbonitride.
[0069] In some embodiments, the absorber-area may comprise sub-stoichiometric oxides. Coating designs may in such embodiments include an oxide of the principal element as described above. The absorber area may then include oxygen containing compounds of the same principal element, where, however, the content of oxygen is lower. Such designs can enable a fine graduation of optical properties and help avoid effective internal optical reflection interfaces. Example coating designs include a top area with an oxide of Si and / or Al, with an absorber area comprising sub-stoichiometric oxides of Si and / or Al. In particular, a top area with an oxide of Si may be advantageously combined with an absorber-area comprising sub-stoichiometric oxides of Si.
[0070] The oxygen content may be varying along the depth, i.e. thickness or growth direction, of the absorber area. As such the compositional profiles of oxygen and the principal element may follow different trajectories within the absorber area. Analogous design principles may be applied in coating designs comprising nitrides, carbides, oxynitrides, oxycarbide, carbonitirdes and oxycarbonitrides. It may such be that the compositional profile of the principal element and the compositional profiles of O, N, and C follow different trajectories within the absorber area. Some examples are illustrated inthrough, highlighting the possibility to adjust the elemental compositional profiles to enhance absorption and avoid effective internal optical reflection interfaces. In particular, the content of the principal element may be decreasing over the top area in the direction from the side opposite the top area towards the top area, and the composition profile of O, N, and / or C may be increasing in the same direction.
[0071] In addition to the principal element A and its chemical compounds, the absorber-area comprises an absorber element which is selected to form a compound with a positive extinction coefficient (k > 0). Preferably the absorber element is a different element than the principal element A. The criteria of a positive extinction coefficient is relevant for the wavelength range the coating layer system is designed to optically absorb.
[0072] The wavelength range may be the range of visible light from 400 nm to 700 nm, Examples of absorber elements and preferred combinations with top-layers are given in Table 1.
[0073] Preferred absorber elements (and / or)Preferred transparent or semitransparent top-areaPrincipal element ATi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfSi-O, Si-N, Si-O-NSiTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfAl-O, Al-N, Al-O-NAlTi, Ag, Cr, Zr, Cu, Nb, Ta, HfSi-O-C, Si-N-C, Si-C, Si-O-N-CSiTi, Ag, Cr, Zr, Cu, C, Nb, TaY-OYTi, Ag, Cr, Zr, Cu, C, Nb, TaHf-OHfTi, Ag, Cr, Cu, C, Nb, TaZr-OZrTi, Ag, Cr, Zr, Cu, C, Nb,Ta-OTaTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfGa-NGaAg, Cr, Zr, Cu, C, Nb, Ta, HfTi-OTiAg, Cr, Zr, Cu, C, Nb, TaTi-Hf-OTi + HfTi, Ag, Cr, Zr, Cu, C, Ta, HfNb-ONbTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfGe-OGeTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfMg-OMgTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfMo-OMoTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfV-OVTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfW-OWTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfZn-OZnTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfB-NBTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfGa-NGaTi, Ag, Cr, Zr, Cu, C, Nb, Ta, HfBe-OBe
[0074] It should be noted however that absorber element and principle element can as well be the same if in the absorber-area such element concentration is increased in a manner over the top of stoechiometry thereby introducing an increased absorption coefficient into the absorber-area as compared to the top-area.
[0075] For the ease of manufacturing it is preferrable however that the top-area does not comprise the absorber element. Depending on the method for manufacturing the monolayer coating, it may however be the case that the top-area comprises traces of the absorber element. In any case, it is preferred that the concentration of the absorber element in the top-area does not exceed 5 at%. In case absorber element and principle element of the top-area are the same it is preferred that this element is not present in the top-area in a manner exceeding stoechiometry by more than 5 at%, more preferrably is not over the stocheometry at all in the top-area.
[0076] The chemical composition profiles within the inventive monolayer coating should preferably be continuous in the sense that no sudden changes in the refractive index are created due to changing chemical composition. As mentioned an internal optical reflection effective interface must not be present. In particular, when the chemical composition within an area within the inventive monolayer coating is adjusted, it is preferred that the change is gradual. Furthermore, it is preferred that transitions from one area to an adjacent, contiguous area within the monolayer coating are designed with a continuous composition profile at the transition area from the top-area to the absorber area inside the coating volume. The chemical composition close to the the mentioned transition area should therefore be adjusted to be same or similar in both of the adjoining areas, namely the top-area and the absorber area.
[0077] The inventive monolayer coating may in some embodiments comprise an absorber block as a coating layer located between the substrate and the absorber-area. Such absorber block is characterized that it comprises the principal element A and the absorber element in constant composition over the thickness of the absorber block. This means that the material composition within the absorber block essentially as a function of depth does not change. In case the absorber-area of the monolayer coating comprises such an absorber block, in order to omit an internal optical reflection effective interface
[0078] The inventive monolayer coating may in some embodiments be applied on an adhesion layer coated on the substrate. Substrate and adhesion layer then form the object as already described. The adhesion layer may include elements present in the substrate and / or the absorber-area of the monolayer coating.
[0079] In some embodiments, the absorber-area is realized in a design with at least one gradient portion, wherein the concentration of the absorber element is changing over the thickness of the gradient portion, as well as the concentration of oxygen and / or nitrogen and / or carbon are changing over the thickness of the gradient portion. The concentration of the absorber element is thereby preferably decreasing in the direction from the object on which the monolayer coating is placed towards the top-area. The gradient of oxygen and / or nitrogen and / or carbon is preferably in the opposite direction compared to the gradient of the absorber element, thus the concentration of oxygen and / or nitrogen and / or carbon is lowest in the beginning of the gradient portion closest to the object and higher in the end of the gradient portion further away from the substrate and closer to the top-area.
[0080] An example of an embodiment is illustrated in, wherein the absorber-area 200, located below the top-area 100 consists of one gradient portion 201. Within the gradient portion 201, the composition of the absorber element is decreasing in direction from substrate towards the top-area, and the concentration of (O + N + C) is increasing.
[0081] It is preferrable that the composition profile of oxygen, nitrogen and carbon are continuous across the volume from the absorber-area to the top-area to avoid adverse effects on optical properties.
[0082] In some embodiments, the absorber-area is realized in a design with three portions, adjacent to each other and aligned with the direction of increasing depth (along the propagation direction of the light)of the absorber layer. The first portion is closer to the objectthan the following two portions. The second portion is in the middle of the three portions. The third portion is closer to the top-area than the preceding two portions. The foregoing arrangement can be described as forming a motive of three adjacent portions within the absorber-area, wherein the second portion is the central portion and the first and third portion are peripheral portions. It is preferrable that the peripheral portions – the first and the third portion – are gradient portions wherein the concentration of the absorber element decreases in the direction from the object towards the top-area (counterdirection of the propagation direction of the light not yet absorbed). The central portion may have a concentration of the absorber element which is constant across the thickness of the central portion, therefore forming an absorber block. In other embodiments, the central portion may display a compositional profile wherein the concentration of the absorber element decreases across the central portion in direction from the substrate towards the top-area, however with a rate of decrease which is lower compared with the rate of decrease in the two peripheral portions.
[0083] The inventors have found that the aforementioned design with three portions is an advantageous way to achieve high absorption in the absorber-area with limited area thickness. The three portion design thus achieves higher absorption compared to a design of same thickness with only a gradient profile.
[0084] In some further embodiments, the absorber area is realized in a design with a plurality of portions. The plurality may comprise five portions, seven portions or even further number of portions. The portions are arranged to form motives of three sequential portions adjacent to each other in the direction of increasing depth (along the propagation direction of the light) of the absorber-area, i.e. the growth direction of the coating. Within each motive, the portion arranged between the other two portions is referred to as the central portion and the other two portions are referred to as peripheral portions. Within each motive, the two peripheral portions are gradient portions where the concentration of the absorber element decreases in the direction from the object towards the top-area. Within each motive, the central portion can have either a constant concentration of the absorber element, or a concentration of absorber element which decreases in direction from the object towards the top-area. When the absorber element within the central portion is decreasing, the rate of decrease is lower compared to the rate of decrease in both of the peripheral portions within the motive.
[0085] The number of motives within the absorber area may be two, three, four or a larger number. The inventors have found that the aforementioned design with a plurality of portions forming at least two motives within the absorber-area advantageously contributes to increasing the absorption efficiency of the absorber-area within limited layer thickness of the inventive monolayer coating. A set amount of absorption can thus be achieved with a lower thickness of the absorber-area compared to, for example, an absorber-area with only one portion.
[0086] In some embodiments, a gradient portion within the absorber-area may be member of two motives. This situation can be illustrated with examples as follows. In, the portions 211, 212 and 213 are forming one motive where the portions 211 and 213 are peripheral portions with decreasing concentration of absorber elements and portion 212 is the central portion with constant composition of absorber element. Furthermore, a second motive is formed by the portions 213, 214, and 215, wherein the portions 213 and 215 are peripheral portions with decreasing composition of absorber element and portion 214 is the central portion with constant composition of the absorber element.
[0087] One further example is illustrated in, wherein the portions 221, 222 and 223 are forming one motive where the portions 221 and 223 are peripheral portions with decreasing concentration of absorber elements. The portion 212 is the central portion where the concentration of absorber element is decreasing, however at lower rate of decrease with respect to thickness compared to portions 221 and 223. Further in this example, the portions 223, 224 and 225 are forming a second motive where the portions 223 and 225 are peripheral portions with decreasing concentration of absorber elements. The portion 224 is the central portion within the motive where the concentration of absorber element is decreasing, however at lower rate of decrease with respect to thickness compared to portions 223 and 225.
[0088] One further example is illustrated in, wherein the portions 231, 232 and 233 are forming one motive where the portions 231 and 233 are peripheral portions and portion 232 is the central portion. A second motive in this example is formed by the portions 233, 234 and 235, wherein the portions 233 and 235 are peripheral portions and the portion 234 is the central portion.
[0089] A method to deposit the inventive monolayer coating onto an object according to the invention uses vacuum coating methods. Vacuum coating methods may include PVD, PECVD and / or CVD methods operated at typical pressures between 0.01 Pa and 100 Pa. A coater unit is provided with means for holding the substrate. Such means may include mechanical or magnetic fixturing of the substrates to be coated and may include rotational motions to equally expose different sides and surfaces of the substrates to the deposition flux.
[0090] The exemplary inventive method as presented here includes the provision and / or use of means for supplying the principal element A, which may include a plasma source based on evaporation of solid material through e.g. sputtering or arc evaporation, and / or may include providing the principal element from the gas phase in a reactive or non-reactive way.
[0091] The method includes the provision and / or use of means for supplying the absorber element, which may include a plasma source based on evaporation of solid material through e.g. sputtering or arc evaporation, or may include providing the principal element from the gas phase in a reactive or non-reactive way.
[0092] The method includes the provision and / or means for supplying oxygen and / or nitrogen and / or carbon, which may include gas supply through one or several gas inlets into the coating system.
[0093] During the vacuum coating process, the temperature inside the coater unit is preferably controlled, for example according to a predefined setpoint value. Means for heating or cooling the coater unit may be applied, such as resistive heating element, plasma heating sources, or water-cooling circuits may be employed.
[0094] The method to produce a monolayer coating according to the invention may comprises at least one step or steps for depositing an absorber-area, wherein the absorber-area comprises at least one gradient portion, and at least one step or steps for depositing a top-area.
[0095] Possible steps of the inventive method can be described for example as follows.
[0096] 1) In a step 1, a gradient portion of the absorber-area layer is deposited during which means for supplying the principal element A are operated to provide a constant flux of element A, and other means for supplying absorber element are operated to provide a decreasing flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide an increasing or constant flux of oxygen and / or nitrogen and / or carbon. ,
[0097] 2) In a step 2, a top-area is deposited during which the means for supplying the prinicpal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are not operated, and means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a constant flux of oxygen and / or nitrogen and / or carbon
[0098] Preferably step 1) is performed before step 2).
[0099] In step 1) and 2), the principal element A may be selected as one or more elements selected from the list of Mg, Nb, Si, Al, Zr, Y, Hf, Ti, Ta, and Ga. Furthermore, the absorber element is preferably a different element than the principal element A and the absorber element leading in the absorber area to a material with an extinction coefficient k > 0 over the defined wavelength range, preferably the visible range.
[0100] According to one embodiment, the means to supply the absorber element is operated such that the concentration of the absorber element is maximum 5 at% in the top area.
[0101] According to one embodiment if the principal element A is Si, then the means for supplying oxygen and / or nitrogen and / or carbon may be operated to supply carbon, or alternatively to supply carbon and nitrogen, or alternatively to supply carbon and nitrogen and oxygen.
[0102] According to another embodiment if the principal element A is one or more elements selected from the list of Si, Al and Ga, then the means for supplying oxygen and / or nitrogen and / or carbon may be operated to supply nitrogen, or oxygen and nitrogen.
[0103] According to another embodiment if the principal element A is one or more elements selected from the list of Si, Al, Zr, Y, Hf, Ti, Ta, and Ga, then the means for supplying oxygen and / or nitrogen and / or carbon may be operated to supply oxygen.
[0104] The method according to the invention may include performing step 1) two or multiple times, preferably including an intermediate step between each repetition of step 1).
[0105] The intermediate step may be a step of
[0106] 1a) of depositing an intermediary portion of the absorber-area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a constant flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a constant flux of oxygen and / or nitrogen and / or carbon.
[0107] In other embodiments, the intermediary step may be a step of
[0108] 1b) of depositing an intermediary portion of the absorber-area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a constant flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide an increasing flux of oxygen and / or nitrogen and / or carbon.
[0109] The sequence of step 1) and intermediate steps may be performed several times, preferably forming a sequence of steps according to … 1), 1a), 1), 1a), 1) …. or according to … 1), 1b), 1), 1b), 1) ….
[0110] The starting values at the beginning of steps within the method, such as steps 1), 2), 1a) and 1b) described above, are preferably selected to match the end values of the preceding step, as to not cause internal optical reflection effective interfaces in the monolayer coating which means to really keep realizing a monolayer coating.
[0111] For example, in the sequence of step 1) and step 2), the flux of element A at the beginning of step 2) is preferably adjusted to be same or very similar as the flux of element A at the end of step 1). The same principle applies for the absorber element and for oxygen, nitrogen and carbon.
[0112] When a step is repeated two or multiple times during the method, the starting values at each repetition is preferably selected to match the end values of the immediately preceding step. The starting values for each repetition of the same step is thus preferably not the same.
[0113] As an example if a step 1) is performed two times: S11and S12with a step 1b) inbetween S1a, according to the sequence S11-S1b-S12, then the starting values at the beginning of S12are preferably the same as the end values of S1b, thereby differing from the starting values of S11. Such values could be for example the flux of element A and / or the flux of the absorber element.Description of figures
[0114] shows schematically potential light reflections in a transparent or semi-transparent coating 1 on a substrate 2. An incident ray 3 may be reflected on the interface air / coating 7 and may give reflected ray 4. Light transmitted into the coating may give rise to a ray 5 reflected at the coating / substrate interface 8, and a ray 6 transmitted back to air after a second reflection on the coating / air interface 7.
[0115] illustrates the objective of the present invention to isolate the reflected ray 4 of the reflection at the interface air / coating 7, and to absorb the transmitted light inside the coating 1 to prevent reflection at the interface coating / object 8.
[0116] illustrates schematically the monolyer coating according to the invention with a top-area 100, an absorber-area comprising a gradient portion 200 and an optional absorber block 300. Shown as well is an optional adhesion layer 400, on a substrate 500 forming the object to be coated with the monolayer coating.
[0117] illustrates an exemplary compositional profile of a monolayer coating according to the invention. The horizontal thickness scale increases with distance from the substrate / object. The depicted monolayer coating comprises a top-area 100 and an absorber-area 200 with a gradient portion 201.
[0118] illustrates an exemplary compositional profile of a monolayer coating according to the invention. The horizontal thickness scale increases with distance from the substrate / object. The depicted monolayer coating comprises a top-area 100 and an absorber-area, the absorber area comprising a profile portion 200 with a gradient portion 201, and the absorber area comprising an absorber block 300.
[0119] illustrates an exemplary compositional profile of a monolayer coating according to the invention. The horizontal thickness scale increases with distance from the substrate. The depicted monolayer coating comprises a top-area 100 and an absorber-area, the absorber-area comprising a gradient portion 200 with five subportions 211-215 and the absorber-area comprising an absorber block 300. The concentration of absorber element is decreasing along a gradient in direction of increasing coating thickness in portions 211, 213, and 215. In portions 212 and 214, the composition of absorber element is constant.
[0120] illustrates an exemplary compositional profile of a monolayer coating according to the invention. The horizontal thickness scale increases with distance from the substrate. The depicted coating layer system comprises a top-area layer 100 and an absorber-area, the absorber area comprising a profile portion 200 with five subportions portions 221-225, wherein subportions 221, 223 and 225 are gradient portions, and the absorber-area comprising as well an absorber block 300. The concentration of the absorber element is decreasing along a gradient in direction of increasing coating thickness in portions 221, 223, and 225. In portions 222 and 224, the absorber element concentration is decreasing along a gradient in direction of increasing coating thickness, at a lower rate compared to the adjacent portions. The rate of decrease of the absorber element in portion 222 is thus lower than the rate of decrease in portions 221 and 223. Analogously, the rate of decrease of the absorber element in portion 224 is thus lower than the rate of decrease in portions 223 and 225.
[0121] illustrates an exemplary compositional profile of a monolayer coating according to the invention. The horizontal thickness scale increases with distance from the substrate. The depicted monolayer coating comprises a top-area 100 and an absorber-area, the absorber-area comprising a grardient portion 200 with five subportions 231-235 and the absorber-area comprising an absorber block 300. In this design subportions 231, 233 and 235 are gradient portions. The concentration of the absorber element is decreasing along a gradient in direction of increasing coating thickness in portions 231, 233, and 235. In portions 232 and 234, the composition of absorber element is constant.
[0122] shows a SCI reflection profiles of an exemplary monolayer coating according to the invention. Both samples are from the same batch and therefore essentially have seen the same deposition process. The deposition process uses 4 consecutive motives with variation of concentration slope. The difference is that one is from a 2fold and the other from a 3fold rotation fixturing. This is to show the capability to coat complex parts with inventive monolayer coating.
[0123] The reflection spectrum was measured with a Konica Minolta Spectrophotometer CM-2600d, utilizing an aperture of 3mm and an observer angle of 8°. The sample measured was a flat polished surface. Slight indications of residual interference effects can be seen.
[0124] shows the dispersion relation of MgF2in the visible range.
[0125] shows the dispersion relation of SiO2in a wavelength range from 400nm up to 3000nm.
[0126] shows the estimated absorption coefficient for SiO2.
[0127] shows the picture of a calotest of a sample where aluminum was deposited with an increasing oxide flux, operating the cathode from metallic mode through the transition mode to oxide mode. The diameter of the calosphere was 20mm. The sphere entered the substrate to a depth of 0.84 µm. Overall thickness of the coating was 5.15 µm. There clearly is an inner circle area which shows the substrate. Connected to this an inner ring appears of about 1.18 µm thickness and separated by presumably interference effects is seen an outer ring with about 3.97 µm thickness. The inner ring is attributed to the metallic mode operation of the cathode, the outer ring is attributed to the oxide mode operation of the cathode. Even though the ramp stepness of oxide flow increase was chosen to be moderate, sudden transition and thereby creation of an optically reflection effective interface could not be avoided.
[0128] shows the calotest as performed on the sample from which the reflection spectrum ofwas measured. The diameter of the calosphere was 20mm. The sphere entered the substrate to a depth of 1.07 µm. Overall thickness of the monolayer coating was 2.25 µm. The absorber- area directly deposited onto the substrate comprised Ti with decreasing percentage of Ti-concentration in direction away from the substrate. The top-area finally forming an interface to the environment did not comprise Ti. As can be seen there is no defined transition circle withing the monolayer formed by the absorber-area and top-area. As a consequence and in contrast tothere is as well no sign for interference effects.
[0129] shows the dispersions of the three materials SiO2, Si3N4and Si2N2O corresponding to the materials as listed in the first line of table 1, however limited to stochiometric compounds.Examples
[0130] The invention is now further and in more detail described with examples. The examples are provided to facilitate the understanding of the invention and should not be construed as limiting.
[0131] Example 1
[0132] In a first example, a monolayer coating according to the invention was deposited utilizing a low voltage arc driven PECVD process with a Silane source (i.e. gas supply of SiH4) and Oxygen to deposit Si resp. SiOxNy. The pressure in the coating chamber was chosen to be between 7E-3 mbar to 2E-2 mbar. To add the absorber element two Titanium-targets with two respective pDC-Magnetronsources were utilized. “pDC” hereby means “pulsed direct current sputter source. This is a magnetron sputter source which is operated with a timedependent rectangular power supply rather than constant power. The deposition was done at 300°C process temperature. The substrates were placed on a 12 tree carousel with a 3-fold rotating flicker driven fixture. “Flicker driven fixture” hereby means a discontinuous drive, which is available in some coating equipment. Normally a continuous two fold planetary system (sun and planets) is realised in coating equipment. The flicker (sometimes as well named “kicker”) add a third rotation axis, such rotation however being discontinuous. Such a flicker driven fixture is for example described in EP1256637 by Kunz et al. The carousel was run with 5 rpm center axis speed. In transfer from one step to the next all relevant sources and gasflows were kept constant with their respective set values to prevent the formation of non-continuous interfaces.
[0133] The carousel run with 5 rpm center axis speed had a rotation transfer ratio of at least 4. In other words, the two-fold rotation of planetary holders occurred at an axis rotation speed of the planetaries which were at least 4 times the center axis speed.
[0134] A low voltage arc was first ignited and run with an Ar-gasflow of 240sccm to form a plasma source for the PECVD process. This Ar-gasflow and low voltage arc was maintained for the whole process.
[0135] In a second step, an adhesion layer was deposited by running the pulsed DC driven Ti-targets with 2kW average power (P_avg) each for 300s. After these 300s, a flow of 20sccm SiH4was let in accompanied by an oxygenflow of 8 sccm. Over the next 600s, the flow of SiH4was linearly increased to 200sccm with the Oxygen being kept constant. All this was done while keeping the Ti-targets running at the 2kW P_avg.
[0136] For the PVD equipment used the used 2kW average power applied to the Ti-targets were equivalent to a growth rate of 270 nm / h of Ti on the substrate and the 200 sccm SiH4were of an equivalent of 700 nm / h growth rate of Si on the substrate.
[0137] In a third step the absorber-area was formed. The flow of SiH4was set to 200 sccm throughout the whole absorber layer deposition duration of 4200s. In parallel the oxygen flow was linearly increased from 10 to 400sccm over the whole absorber-area deposition duration of 4200s. The step of forming the absorber-area was divided into sub-steps where different power was used on the titanium targets, in order to create different portions in the absorber-area. In a first sub-step, the power (P_avg) was reduced linearly with a total reduction of 400W over a duration of 600s, i.e. a decrease from 2kW at beginning of the first sub-step to 1.6 kW at the end of the first sub-step. In a second sub-step, P_avg on the titanium targets was kept constant at 1.6 kW for 300s. In a third sub-step P_avg on the titanium targets were decreased again linearly at a rate of 400W per 600s for a duration of 600s. The power was thus decreased from 1.6 kW at the beginning of the third sub-step to 1.2 kW at the end of the third sub-step. In a fourth sub-step, P_avg was held constant at 1.2 kW for 300s. In a fifth sub-step P_avg on the titanium targets were decreased again linearly at a rate of 400W per 600s for a duration of 600s, thus with power of 1.2 kW at the beginning of the fifth sub-step decreasing to 0.8 kW at the end of the fifth sub-step. In a sixth sub-step, P_avg was held constant at 0.8 kW for 300s. In a sixth sub-step P_avg on the titanium targets were decreased again linearly at a rate of 400W per 600s for a duration of 600s, thus with power of 0.8 kW at the beginning of the sixth sub-step decreasing to 0.4 kW at the end of the sixth sub-step. In a seventh sub-step, P_avg was held constant at 0.4 kW for 300s. In an eighth sub-step P_avg on the titanium targets were decreased again linearly at a rate of 400W per 600s for a duration of 600s, thus with power of 0.4 kW at the beginning of the eighth sub-step decreasing to 0 kW at the end of the eighth sub-step. The end of the eighth sub-step concluded the third step of forming the absorber-area. P_avg reached 0W which was after the defined 4200s when the Oxygenflow had reached 400sccm.
[0138] In a fourth and final step, the top-area of SiOxwas deposited for 1800s. This was achieved by keeping the set low voltage arc, Ar-flow, carousel speed, Silaneflow and Oxygen constant for further 1800s.
[0139] After this duration first the Silaneflow was stopped, then the Oxygen and finally the Argon and the low-voltage Arc were stopped.
[0140] This whole coating process did result in a deposition of ca. 100nm adhesion layer, ca. 0.6µm absorber-area and ca. 1.4µm top-area, absorber-area and top-area forming together the inventive monolayer coating. The coating thickness was measured on samples mounted in 2-fold rotation as well as on samples mounted in 3-fold rotation.
[0141] The optical properties were determined and favorably low L* values were measured, as shown in Table 2.shows the reflection profile, which confirmed reflection of about 3.5% in the wavelength range from 360 nm to 740 nm which is in expectation for a single interface reflection from air to dense and amorphous SiO2. The amplitude of residual interference was found to be low enough to not have any visible effect on the appearance.
[0142] Sample mountingGloss componentL*(D65)a*(D65)b*(D65)2-fold rotationSCI21.810.05-0.13-fold rotationSCI21.750.06-0.07
[0143] Example 2:
[0144] In a second example, the same procedure as described in the first example was followed except that a mixture of Oxygen and Nitrogen in the ratio 20sccm:180sccm was used instead of pure Oxygen. This resulted in a higher reflectivity, respective higher L*-value, as is expected by a higher SiNx content in the top layer. The measured optical properties are shown in Table 3.
[0145] Sample mountingGloss componentL*(D65)a*(D65)b*(D65)2-fold rotationSCI31.660.140.023-fold rotationSCI31.680.250.16
[0146] Example 3:
[0147] In a third example Copper (Cu) was utilized as absorber element. The general process procedure was done in a similar way as the described implementation with Titanium in example 1, except for that only one pulsed DC source equipped with Copper was used. At first a deposition with 100 sccm SiH4together with 200 sccm O2 were done for 15min. After these 15min the copper was deposited starting with 2kW average power for 30min followed by a 10min linear ramp down to 1kW which was then held constant for a further 10min. This constant segment was followed by a 10min linear ramp to 630W, followed by a 30min linear ramp to 0W. Throughout the deposition of Copper the Silane and Oxygen deposition was run in parallel with constant parameters. These parameters were then continued to be held constant for a further 60min.
[0148] This implementation resulted in the following color value as shown in Table 4, which is essentially the same as when utilizing Titanium as absorber element.
[0149] sample mountinggloss componentL*(D65)a*(D65)b*(D65)2-fold rotationSCI21.770.46-0.12
[0150] The disclosure according to this specification is focused on applications for visible light. However in applications in the infrared or even radar applications, in other words wherever electromagnetic waves are used and play a role, the same idea (using a monolayer coating with an absorber-area and a top-area, whereby within the monolayer coating no reflectivity effective interface is realised) can be applied mutatis mutandis. These applications are as well to be regarded as within the scope of the present invention. The one skilled in the art will know how to adopt the materials as well as the thicknesses of the areas as well as the gradient profiles accordingly.
[0151] Monolayer coating according to the invention may be used in diverse applications and on a variety of substrates. Use cases and substrates may in particular be decorative articles, such as jewelry, watches, ornaments, figurines, sculptures, commemorative items, trophies, jewelry, fashion accessories, or architectural decorative elements. The inventive monolayer coating may as well be used on sports equipment including articles, accessories and components for athletic or recreational activities. In particular bats, racquets, clubs, sticks, protective gear, and apparel. The inventive monolayer coating may as well be used on kitchen utensils including any articles used configured for use in the preparation, processing, handling, storage, serving, cooking, heating, cooling, mixing, measuring, dispensing, cutting, or presentation of food, beverages, ingredients, or consumable products.
[0152] In some embodiments, the monolayer coating according to the invention may be applied onto optically intransparent substrates.
[0153] A monolayer coating was disclosed comprising an absorber-area and adjacent to the absorber-area a top-area, with the absorber-area comprising material with an absorption coefficient for visible light above the absorption coefficient of SiO2 for visible light and with the top-area comprising less material with an absorption coefficient for visible light above the absorption coefficent of SiO2 for visible light as compared to the absorber-area, preferably the top-area comprising a maximum 5at% of material with absorption coefficient above the absorption coefficient for SiO2 for visible light, characterized in that within volume of the monolayer coating and parallel to the interfaces of the monolayer coating to its environment no internal optical reflection effective interface is present.
[0154] The monolayer coating may have the characteristic that a calotest on the monolayer coating does not show a visible transition area between the absorber-area and the top-area thereby proving the absence of an internal optical reflection effective interface.
[0155] The top area of the monolayer coating may comprise one or more materials of members of the group formed by SiO2, Si3N4and Si2N2O
[0156] The monolayer coating may have the characteristic that the material with an absorption coefficient for visible light above the absorption coefficient of SiO2comprises at least one element selected from the list of Ti, Ag, Cr, Zr, Cu, C, Nb, Ta, Al, and Hf.
[0157] The monolayer coating may have the characteristic that the material with an absorption coefficient for visible light above the absorption coefficient of SiO2comprises Ti and / or Cu.
[0158] The monolayer coating may have the characteristic that the material with an absorption coefficient for visible light above the absorption coefficient of SiO2consists of Ti or Cu, or a mixture of Ti and Cu.
[0159] The monolayer coating may have the characteristic that the material with an absorption coefficient for visible light above the absorption coefficient of SiO2consists of Ti.
[0160] The monolayer coating may be deposited on a substrate, and the absorber area may be located closer to the substrate than the top area.
[0161] The monolayer coating may have the characteristic that the absorber area comprises at least one gradient portion, wherein the concentration profile of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is continuous, wherein the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light decreases in the direction from the substrate towards the top area.
[0162] The gradient portion of the absorber area may have the characteristic that concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light continuously approaches zero at the side of the gradient portion closest to the top area.
[0163] The monolayer coating may have the characteristic that the thickness of the absorber area is at least 0.3 µm.
[0164] The monolayer coating may have the characteristic that the top area is a compound of a principal element A, and the absorber-area comprises the principal element A, wherein the principal element A is one or more elements selected from the list of Si, Al, Zr, Y, Hf, Ti, Ta, and Ga, and the compound of the top area is an oxide, and the composition profiles of O are continuous within the absorber area, across the interface from the absorber area to the top area and within the top area. These characteristics may in particular be combined with the characteristics that the material with an absorption coefficient for visible light above the absorption coefficient of SiO2comprise at least one element selected from the list of Ti, Ag, Cr, Zr, Cu, C, Nb, Ta, Al, and Hf, preferably comprise or consist of Ti and / or Cu.
[0165] The monolayer coating may have the characteristic that the top area is a compound of a principal element A, and the absorber-area comprises the principal element A the principal element A is one or more elements selected from the list of Si, Al, and Ga, and the compound of the top area is an oxynitride or a nitride, and the composition profiles of O and N are continuous within the absorber area, across the interface from the absorber area to the top area and within the top area. These characteristics may in particular be combined with the characteristics that the material with an absorption coefficient for visible light above the absorption coefficient of SiO2comprise at least one element selected from the list of Ti, Ag, Cr, Zr, Cu, C, Nb, Ta, Al, and Hf, preferably comprise or consist of Ti and / or Cu.
[0166] The monolayer coating may have the characteristic that the top area is a compound of a principal element A, and the absorber-area comprises the principal element A, the principal element A is Si, and the compound of the top area is a carbide or an oxycarbide or an oxycarbonitride or a carbonitride, and the composition profiles of C, O and N are continuous within the absorber area, across the interface from the absorber area to the top area and within the top area. These characteristics may in particular be combined with the characteristics that the material with an absorption coefficient for visible light above the absorption coefficient of SiO2comprise at least one element selected from the list of Ti, Ag, Cr, Zr, Cu, C, Nb, Ta, Al, and Hf, preferably comprise or consist of Ti and / or Cu.
[0167] The monolayer coating may have the characteristic that the top area is a compound of a principal element A, and the absorber-area comprises the principal element A, wherein the principal element A is Si, Al, or a mixture of Si and Al, and the compound of the top area is an oxide. These characteristics may in particular be combined with the characteristics that the material with an absorption coefficient for visible light above the absorption coefficient of SiO2comprise or consist of Ti and / or Cu.
[0168] The monolayer coating may have the characteristic that the composition profile of the principal element A and the composition profile of O, N and C follow different trajectories within the absorber area.
[0169] The monolayer coating may have the characteristic that the composition profile of the principal element A is decreasing in the direction from the side opposite the top area towards the top area and the composition profile of O is increasing in the direction from the side opposite the top area towards the top area over at least part of the absorber area, preferably over the entire absorber area.
[0170] The monolayer coating may have the characteristic that the absorber area comprises sub-stoichiometric oxides of the principal element A. The compound of the top area may be an oxide and the principal element A may be Si, Al, or a mixture of Si and Al, preferably is Si.
[0171] The monolayer coating may have the characteristic that the compound of the top area is a nitride, a carbide or a carbonitride and wherein preferably the coating is essentially free of oxygen.
[0172] The monolayer coating may be deposited on a substrate and may have the characteristic that the absorber area comprises three sequential portions adjacent to each other, wherein the portion closest to the substrate and the portion closest to the top area form peripheral portions and the portion between the peripheral portions forms a central portion, wherein the concentration profile of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is continuous across the interfaces between adjacent portions, wherein the two peripheral portions are gradient portions where the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light decreases in the direction from the substrate towards the top area, wherein the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is constant across the central portion.
[0173] The monolayer coating may be deposited on a substrate and may have the characteristic that the absorber area comprises three sequential portions adjacent to each other, wherein the portion closest to the substrate and the portion closest to the top area form peripheral portions and the portion between the peripheral portions forms a central portion, wherein the concentration profile of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is continuous across the interfaces between adjacent portions, wherein the two peripheral portions are gradient portions where the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light decreases in the direction from the substrate towards the top area, wherein the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light in the central portion decreases across the central portion in direction from the substrate towards the top area with a rate of decrease that is lower than the rate of decrease in each of the two peripheral portions.
[0174] The monolayer coating may be deposited on a substrate and may have the characteristic that the absorber area comprises a plurality of at least five portions, arranged to form at least two motives of three sequential portions adjacent to each other, wherein the concentration profile of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is continuous across the interfaces between adjacent portions, wherein the two peripheral portions within each motive are gradient portions where the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light decreases in the direction from the substrate towards the top area, wherein within each motive, the central portion has a concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light which is constant across the central portion or decreases across the central portion in direction from the substrate towards the top area, where the rate of decrease is lower than the rate of decrease in each of the peripheral portions within the motive.
[0175] The monolayer coating may be deposited on a substrate and may have the characteristic that he plurality of portions includes at least seven portions forming at least three motives.
[0176] The monolayer coating may be deposited on a substrate which may be optically intransparent.
[0177] The monolayer coating may be deposited on a substrate which may be a decorative article or a part of a decorative article, a sports equipment or a part of a sports equipment, a kitchen utensil or part of a kitchen utensil.
[0178] Disclosed is a vacuum coating method for producing a monolayer coating on a substrate, with a top area comprising a principal element A, and an absorber area comprising and an absorber element, wherein the absorber area comprises at least one gradient portion, providing a coater unit with means for holding the substrate, providing means for supplying the principal element A, providing means for supplying the absorber element, providing means for supplying oxygen and / or nitrogen and / or carbon, wherein the method comprises the steps ofdepositing the gradient portion of the absorber area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a decreasing flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide an increasing or constant flux of oxygen and / or nitrogen and / or carbon,depositing the top area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are not operated or are operated to provide a constant flux of the absorber element which is lower compared to the flux of element A, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a constant flux of oxygen and / or nitrogen and / or carbon
[0179] wherein step 1) is performed before step 2), and the principal element A is one or more elements selected from the list of Si, Al, Zr, Y, Hf, Ti, Ta, and Ga, and the absorber element is a different element than the principal element A and the absorber element is an element with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light, and the means for supplying oxygen and / or nitrogen and / or carbon is operated to provide oxygen.
[0180] Disclosed is as well a vacuum coating method for producing a monolayer coating on a substrate, with a top area comprising a principal element A, and an absorber area comprising and an absorber element, wherein the absorber area comprises at least one gradient portion, providing a coater unit with means for holding the substrate, providing means for supplying the principal element A, providing means for supplying the absorber element, providing means for supplying oxygen and / or nitrogen and / or carbon, wherein the method comprises the steps ofdepositing the gradient portion of the absorber area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a decreasing flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide an increasing or constant flux of oxygen and / or nitrogen and / or carbon,depositing the top area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are not operated or are operated to provide a constant flux of the absorber element which is lower compared to the flux of element A, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a constant flux of oxygen and / or nitrogen and / or carbon
[0181] wherein step 1) is performed before step 2), and the principal element A is one or more elements selected from the list of Si, Al, and Ga, and the absorber element is a different element than the principal element A and the absorber element is an element with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light, and the means for supplying oxygen and / or nitrogen and / or carbon is operated to provide oxygen and / or nitrogen.
[0182] Disclosed is as well a vacuum coating method for producing a monolayer coating on a substrate, with a top area comprising a principal element A, and an absorber area comprising and an absorber element, wherein the absorber area comprises at least one gradient portion, providing a coater unit with means for holding the substrate, providing means for supplying the principal element A, providing means for supplying the absorber element, providing means for supplying oxygen and / or nitrogen and / or carbon, wherein the method comprises the steps ofdepositing the gradient portion of the absorber area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a decreasing flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide an increasing or constant flux of oxygen and / or nitrogen and / or carbon,depositing the top area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are not operated or are operated to provide a constant flux of the absorber element which is lower compared to the flux of element A, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a constant flux of oxygen and / or nitrogen and / or carbon
[0183] wherein step 1) is performed before step 2), and the principal element A is Si, and the absorber element is a different element than the principal element A and the absorber element is an element with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light, and the means for supplying oxygen and / or nitrogen and / or carbon is operated to provide carbon, or carbon and nitrogen, or carbon and oxygen, or carbon and nitrogen and oxygen.
[0184] The vacuum deposition method may have the characteristic that in that step 1) is performed at least two times, wherein between each repetition of step 1) a further step 1a) of depositing an intermediary portion of the absorber area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a constant flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a constant flux of oxygen and / or nitrogen and / or carbon is performed.
[0185] The vacuum deposition method may have the characteristic that step 1 is performed at least three times, resulting in a step sequence of … 1), 1a), 1), 1a), 1) …
[0186] The vacuum deposition method may have the characteristic that in that step 1) is performed at least two times, wherein between each repetition of step 1) a further step 1b) of depositing an intermediary portion of the absorber area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a constant flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a decreasing flux of oxygen and / or nitrogen and / or carbon is performed.
[0187] The vacuum deposition method may have the characteristic that step 1 is performed at least three times, resulting in a step sequence of … 1), 1b), 1), 1b), 1) …
[0188] The vacuum deposition method may have the characteristic that the means for supplying the principal element A is a PVD deposition source or a PECVD deposition source and the means for supplying the absorber element is a PVD deposition source, preferably a magnetron sputtering source.
[0189] The vacuum deposition method may have the characteristic that the principal element A is Si and the absorber element is Ti.
Claims
Monolayer coating comprising an absorber-area and adjacent to the absorber-area a top-area, with the absorber-area comprising material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light and with the top-area comprising less material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light as compared to the absorber-area, preferably the top-area comprising a maximum 5at% of material with absorption coefficient above the absorption coefficient for SiO2for visible light, characterized in that within volume of the monolayer coating and parallel to the interfaces of the monolayer coating to its environment no internal optical reflection effective interface is present.Monolayer coating according to claim 1 characterized in that a calotest on the monolayer coating does not show a visible transition area between the absorber-area and the top-area thereby proving the absence of an internal optical reflection effective interface.Monolayer coating according to claim 1 or 2, wherein the material with an absorption coefficient for visible light above the absorption coefficient of SiO2comprises at least one element selected from the list of Ti, Ag, Cr, Zr, Cu, C, Nb, Ta, Al, and Hf.Monolayer coating according to claim 3, wherein the material with an absorption coefficient for visible light above the absorption coefficient of SiO2comprises Ti and / or Cu.Monolayer coating according to claim 4, wherein the material with an absorption coefficient for visible light above the absorption coefficient of SiO2consists of Ti or Cu, or a mixture of Ti and Cu.Monolayer coating according to claim 5, wherein the material with an absorption coefficient for visible light above the absorption coefficient of SiO2consists of Ti.Monolayer coating according to any one of the preceding claims, wherein the monolayer coating is deposited on a substrate, characterized in that the absorber area is located closer to the substrate than the top area.Monolayer coating according to claim 7, wherein the monolayer coating is deposited on a substrate, characterized in that the absorber area comprises at least one gradient portion, wherein the concentration profile of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is continuous, wherein the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light decreases in the direction from the substrate towards the top area.Monolayer coating according to claim 8, wherein the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light continuously approaches zero at the side of the gradient portion closest to the top area.Monolayer coating according to any one of the preceding claims, wherein the thickness of the absorber area is at least 0.3 µm.Monolayer coating according to any one of the preceding claims, characterized in that the top area is a compound of a principal element A, and the absorber-area comprises the principal element A, wherein eitheri) the principal element A is one or more elements selected from the list of Si, Al, Zr, Y, Hf, Ti, Ta, and Ga, andthe compound of the top area is an oxide, andthe composition profiles of O are continuous within the absorber area, across the interface from the absorber area to the top area and within the top area,orii) the principal element A is one or more elements selected from the list of Si, Al, and Ga, andthe compound of the top area is an oxynitride or a nitride, andthe composition profiles of O and N are continuous within the absorber area, across the interface from the absorber area to the top area and within the top area,oriii) the principal element A is Si, andthe compound of the top area is a carbide or an oxycarbide or an oxycarbonitride or a carbonitride, andthe composition profiles of C, O and N are continuous within the absorber area, across the interface from the absorber area to the top area and within the top area.Monolayer coating according to claim 11, wherein the principal element A is Si, Al, or a mixture of Si and Al, and the compound of the top area is an oxide.Monolayer coating according to claim 11, wherein the composition profile of the principal element A and the composition profile of O, N and C follow different trajectories within the absorber area.Monolayer coating according to claim 13, wherein the composition profile of the principal element A is decreasing in the direction from the side opposite the top area towards the top area and the composition profile of O is increasing in the direction from the side opposite the top area towards the top area over at least part of the absorber area, preferably over the entire absorber area.Monolayer coating according to claim 11, wherein the absorber area comprises sub-stoichiometric oxides of the principal element A.Monolayer coating according to claim 15, wherein the compound of the top area is an oxide.Monolayer coating according to claim 16, wherein the principal element A is Si, Al, or a mixture of Si and Al, preferably is Si.Monolayer coating according to claim 11, characterized that the compound of the top area is a nitride, a carbide or a carbonitride and wherein preferably the coating is essentially free of oxygen.Monolayer coating according to any one of the preceding claims, wherein the monolayer coating is deposited on a substrate, characterized in that the absorber area comprises three sequential portions adjacent to each other, wherein the portion closest to the substrate and the portion closest to the top area form peripheral portions and the portion between the peripheral portions forms a central portion, wherein the concentration profile of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is continuous across the interfaces between adjacent portions, wherein the two peripheral portions are gradient portions where the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light decreases in the direction from the substrate towards the top area, wherein eitherthe concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is constant across the central portion or the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light in the central portion decreases across the central portion in direction from the substrate towards the top area with a rate of decrease that is lower than the rate of decrease in each of the two peripheral portions.Monolayer coating according to any one of the preceding claims, wherein the monolayer coating is deposited on a substrate, characterized in that the absorber area comprises a plurality of at least five portions, arranged to form at least two motives of three sequential portions adjacent to each other,wherein the concentration profile of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light is continuous across the interfaces between adjacent portions,wherein the two peripheral portions within each motive are gradient portions where the concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light decreases in the direction from the substrate towards the top area,wherein within each motive, the central portion has a concentration of the material with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light which is constant across the central portion or decreases across the central portion in direction from the substrate towards the top area, where the rate of decrease is lower than the rate of decrease in each of the peripheral portions within the motive.Monolayer coating according to claim 20, wherein the plurality of portions includes at least seven portions forming at least three motives.Monolayer coating according to claim 1, characterized in that the top-area of the monolayer coating comprises one or more materials of members of the group formed by SiO2, Si3N4and Si2N2OMonolayer coating according to any one of the preceding claims, wherein the monolayer coating is deposited on a substrate, characterized in that the substrate is optically intransparent.Monolayer coating according to any one of the preceding claims, wherein the monolayer coating is deposited on a substrate, wherein the substrate is a decorative article or a part of a decorative article, a sports equipment or a part of a sports equipment, a kitchen utensil or part of a kitchen utensil.Vacuum coating method for producing a monolayer coating on a substrate, with a top area comprising a principal element A, and an absorber area comprising and an absorber element, wherein the absorber area comprises at least one gradient portion,providing a coater unit with means for holding the substrate,providing means for supplying the principal element A,providing means for supplying the absorber element,providing means for supplying oxygen and / or nitrogen and / or carbon,wherein the method comprises the steps of1) depositing the gradient portion of the absorber area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a decreasing flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide an increasing or constant flux of oxygen and / or nitrogen and / or carbon,2) depositing the top area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are not operated or are operated to provide a constant flux of the absorber element which is lower compared to the flux of element A, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a constant flux of oxygen and / or nitrogen and / or carbonwherein step 1) is performed before step 2), andwherein eitheri) the principal element A is one or more elements selected from the list of Si, Al, Zr, Y, Hf, Ti, Ta, and Ga, andthe absorber element is a different element than the principal element A and the absorber element is an element with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light , andthe means for supplying oxygen and / or nitrogen and / or carbon is operated to provide oxygen,orii) the principal element A is one or more elements selected from the list of Si, Al, and Ga, andthe absorber element is a different element than the principal element A and the absorber element is an element with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light, andthe means for supplying oxygen and / or nitrogen and / or carbon is operated to provide oxygen and / or nitrogen,oriii) the principal element A is Si, andthe absorber element is a different element than the principal element A and the absorber element is an element with an absorption coefficient for visible light above the absorption coefficient of SiO2for visible light, andthe means for supplying oxygen and / or nitrogen and / or carbon is operated to provide carbon, orcarbon and nitrogen, orcarbon and oxygen, orcarbon and nitrogen and oxygen.Method according to claim 25, characterized in that step 1) is performed at least two times, wherein between each repetition of step 1) a further step1a) of depositing an intermediary portion of the absorber area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a constant flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a constant flux of oxygen and / or nitrogen and / or carbon,is performed.Method according to claim 26, wherein step 1 is performed at least three times, resulting in a step sequence of … 1), 1a), 1), 1a), 1) …Method according to claim 25, characterized in that step 1) is performed at least two times, wherein between each repetition of step 1) a further step1b) of depositing an intermediary portion of the absorber area during which the means for supplying the principal element A are operated to provide a constant flux of element A, and the means for supplying absorber element are operated to provide a constant flux of the absorber element, and the means for supplying oxygen and / or nitrogen and / or carbon are operated to provide a decreasing flux of oxygen and / or nitrogen and / or carbon,is performed.Method according to claim 28, wherein step 1 is performed at least three times, resulting ina step sequence of … 1), 1b), 1), 1b), 1) …Method according to any one of claims 25-29, wherein the means for supplying the principal element A is a PVD deposition source or a PECVD deposition source and the means for supplying the absorber element is a PVD deposition source, preferably a magnetron sputtering source.Method according to any one of claims 25-30, wherein the principal element A is Si and the absorber element is Ti.