Method and apparatus for welding and cutting polymeric films transparent to visible light using a laser source
The method and apparatus address the limitations of existing laser welding by employing a visible laser source with a vacuum system to uniformly distribute pressure and minimize air pockets, enabling efficient welding and cutting of transparent polymers.
Patent Information
- Application Number
- PCT/IB2026/054380
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-05-04
- Publication Date
- 2026-11-12
AI Technical Summary
Existing laser welding techniques for transparent polymers fail to minimize air pockets, distribute clamping pressure uniformly, and utilize a single laser source for both welding and cutting, especially when using visible light sources.
A method and apparatus using a low-cost laser source in the visible range, combined with a vacuum system and laminated film containment, ensures uniform clamping pressure and minimizes air pockets by evacuating gases, allowing both welding and cutting of transparent polymers.
Achieves high-quality welds with enhanced mechanical strength and uniform pressure distribution, using a cost-effective visible laser source that can perform both welding and cutting without modifying the polymer layers.
Smart Images

Figure IB2026054380_12112026_PF_FP_ABST
Abstract
Description
[0001] Method and apparatus for welding and cutting polymeric films transparent to visible light using a laser source
[0002] Applicant : Universita degli Studi "La Sapienza" Inventors : Giovanni De Bellis, Fabrizio Sarasini, Luciano Fattore, Gabriele Galbato Muscio
[0003] The present invention relates to a method and an apparatus for welding and cutting polymeric films transparent to visible light using a laser source .
[0004] Background
[0005] The welding of thermoplastic films finds application mainly in the food packaging and biomedical fields, with important applications also in the aeronautical and automotive sectors, as well as in the production of electronic devices and in microfluidics
[0001] . Traditionally, this particular type of welding is carried out using two assembly approaches : cold or hot . While cold welding involves the use of pressure-sensitive adhesives (PSAs )
[0002] , the techniques used for hot welding fundamentally involve the use of a constant heat source applied to the interfaces to be welded . Heat transfer can occur by conduction through direct contact, for example by means of a metal element (blade, wire) , or by ultrasound
[0003] , or by convection in hot air sealers or even by irradiation with infrared radiation or localized induction heating . In any case, these techniques involve melting thepolymeric films to maximize the performance of the obtained welds, both in terms of mechanical strength and hermetic sealing
[0004] . In recent years, laser welding has established itself over traditional techniques for creating joints on polymeric materials, especially in the field of thermoplastic polymers (although the possibility of forming a welded joint between thermoplastics and thermosets using a laser beam was already demonstrated in the early 1980s ) . Laser welding involves focusing a coherent light beam on the joint, to be carried out according to two main modes :
[0006] 1 ) In so-called "direct" laser welding (Direct Laser Welding) , the laser beam is projected directly onto the joint to be welded, placing the two surfaces of the joint face to face;
[0007] 2 ) In the technique known as transmission laser welding (TLW) , the two parts to be welded are positioned one on top of the other and the beam passes through the upper one, which must therefore be transparent to the wavelength of the source, and is then absorbed by the lower layer which must instead be able to absorb the same incident radiation to give rise to localized melting, resulting in the formation of the joint . The operating principle of the second mode, schematized in Fig . 1, is based on the difference between the optical properties of the two polymer layers 20, 30 to be welded and brought into contact with a pressure 40 : the upper layer 20 must be transparent to the laser beam 11, whilethe lower layer 30 must be opaque or, in general, absorbent to the same type of radiation (absorption can be partial and can be determined depending on the materials to be welded and the laser power) . A further possibility involves using a thin absorbent layer 50, positioned at the interface between the two polymeric layers 20, 30 to be welded, especially if the two layers to be welded are transparent .
[0008] Since the laser welding phenomenon is based on the thermo-optical correlation between the laser beam and the material to be welded, the latter must not be highly reflective to the radiation used . The unreflected portion of radiation is absorbed and propagates in the material, transferring energy in the form of heat and causing various modifications in the material that can include its melting and vaporization . Most polymers are transparent or, at most, translucent to visible or near-infrared (NIR) radiation, but they can be capable of absorbing the incident radiation if appropriately loaded with pigments or dyes . Absorption of laser radiation can be described by the well-known Beer-Lambert law, which well describes the attenuation phenomena of the radiation intensity :
[0009] / (z) = loe(~az)
[0010] wherein Io represents the intensity of the incident radiation, z the penetration depth and a the attenuation coefficient, comprising both absorption and scatteringphenomena
[0005] . The attenuation coefficient therefore also depends on the "color" of the absorbing medium, its composition, and characteristics of the incident radiation, such as its intensity and wavelength . The extent of laser radiation absorption in the absorbing polymer is determined by the absorption coefficient : a high value leads to absorption of laser energy on the surface or within a few microns of depth ( surface absorption) , while lower values cause volumetric absorption in deeper layers . Adequate contact between the parts to be joined is fundamental to ensure heat transfer from the absorbing polymer to the transparent part . The heat generated is transferred by thermal conduction, causing the softening or melting of both polymers at the interface when their glass transition temperature ( for amorphous polymers ) or melting temperature ( for semi-crystalline polymers ) is reached .
[0011] The heat at the interface forms a melt pool where molecular diffusion occurs; once the molten layer has solidified, a solid joint is formed . Most polymers have low absorption to radiation with a wavelength between 350 nm and 1 . 4 pm. For this reason, Nd : YAG (Neodymium-doped Yttrium Aluminum Garnet ) type lasers with wavelengths between 800 and 1100 nm are often used to weld polymers according to the TLW technique, being able to weld even within thicknesses of several millimeters . Nd : YAG lasers with 532 nm emission have been used for welding high-density polyethylene layers , but modifying the lowerabsorbent layer by introducing pigments or coloring elements into such layer (as indicated in paragraph 3 . 1 of ref .
[0006] , the additives that modify absorption are mainly dyes - soluble in the polymer - and pigments - insoluble in the polymer and in powder form, of both organic and inorganic origin) . The most recent diode lasers have further extended the interest in laser welding of polymers, relying on lower cost, greater flexibility, and superior electro-optical conversion efficiency . Due to the high absorption of polymers to radiation with a wavelength of 10 . 6 pm, CO2 lasers are mostly used today for welding polymer films in the packaging industry . Lasers with wavelengths between 1 . 4 and 2 .2 pm are instead used for welding transparent polymers without using an absorbent layer . Among these lasers, diode lasers should be mentioned, such as InGaAsP ( Indium-Gallium-Arsenide-Phosphide) and InGaAsSb ( Indium-Gallium-Arsenide-antimonide ) types operating in the 1 . 4-1 . 94 pm range, and Erbium and Thulium fiber lasers, with wavelengths between 1 . 53-1 . 65 pm and 1 . 9-2 . 05 pm, respectively
[0005] .
[0012] Laser welding between different polymers requires both physical compatibility (melting temperatures in the same range) and chemical compatibility, based on similar molecular structures and viscosities . It is feasible primarily between amorphous polymers, which have disordered structures and a wide softening range . Semicrystalline polymers, with ordered structures and sharp melting, usually only weld to themselves, andincompatibility prevents melting between different materials
[0006] .
[0013] At the patent level, US 2011 / 036817 Al describes the development of a welding station for polymeric films, with dedicated applications to the packaging industry for controlled atmosphere "trays" . In this case, the vacuum is used only to evacuate the oxygen that would degrade the products to be preserved in the tray and replace it with a possible protective atmosphere, while the problem of air evacuation is not solved, preventing the formation of trapped bubbles in the welding seal . Furthermore, in the prior art document, the contact pressure is guaranteed by an additional external clamping system. A modification of the films is indicated by including absorbers (except in the variation shown in Figs . 5 and 6) , an arrangement which however does not prevent optical / structural modifications to the films themselves .
[0014] US 2012 / 183748 Al relates to a method for welding polymeric sheets, preferably using infrared absorbing elements, integrated in various configurations and, mostly, directly into the sheets to be welded . Nearinfrared lasers (with wavelengths in the range between 800 and 1200 nm) or broad-spectrum infrared lamps are used, and the problem of evacuating air bubbles is not solved .
[0015] Although JP 2011 031587 A also concerns the welding of sheets of thermoplastic material with thicknesses less than 1 mm, the source used is also in this case infrared ( 980 nm) and the welding mechanism involves the use of anauxiliary lower plate, absorbent in the incident radiation range, having protruding portions (protrusions ) that reproduce the shape of the desired weld and onto which the incident radiation is directed. The shape of this auxiliary plate must be replaced every time the geometry of the weld bead is to be changed . Again, no mention is made of using vacuum to achieve the clamping pressure necessary for the welding process .
[0016] JP 2011 240586 A relates to laser welding of polymeric films based on the shaping of an absorbing region arranged along the planned welding line, with particular attention to varying the width of this region to locally modulate the joint resistance and obtain, in certain portions , "peelability" and "weldability" . The document does not describe a hermetically sealed assembly, nor a predetermined pressure between the transparent sheet and the lower support, in order to minimize air pockets . The document is oriented towards the use of near-infrared radiation, as confirmed by the reference to a graphite sheet as the preferred material for high laser light absorption in that spectral region.
[0017] In summary, the transparent polymer welding techniques currently available involve the use of sources with wavelengths only in the near infrared (between 1 . 4 and 2 .2 pm) and / or the modification of the films to be welded to allow absorption of the laser beam . Furthermore, known techniques fail to :
[0018] • minimize the air pockets that typically form betweenthe various layers of the weld;
[0019] • distribute the clamping pressure over the entire area of the films, in particular also in the zone affected by the optical path of the laser beam;
[0020] • use the same laser source for welding and cutting polymeric films .
[0021] There is therefore a need in the art for a solution that overcomes the aforementioned drawbacks .
[0022] Object and subject matter of the invention
[0023] The object of the present invention is to provide a system and method for welding and cutting polymeric films transparent to visible light using a laser source that overcomes the drawbacks and solves the problems of the prior art .
[0024] The subject matter of the present invention is a method and a system according to the attached claims .
[0025] Detailed description of the invention
[0026] List of figures
[0027] The invention will now be described for illustrative but non-limiting purposes, with particular reference to the drawings of the attached figures, wherein :
[0028] • figure 1 shows a known diagram of transmission laser welding operation, reproduced from the prior art reference
[0006] ;• figure 2 shows in (A) a representative diagram of a section of the laser welding system according to the invention ;
[0029] • in (B) an exploded view of the laminate in (A) ;
[0030] • figure 3 shows a general protocol for TLW welding of thermoplastic materials, according to the prior art
[0006] ;
[0031] • figure 4 shows an optical micrograph of the weld bead on a POF sample with a thickness of 15 pm (a) and its load curve (b) obtained by tearing according to the ASTM F088M standard, according to an example of the invention ;
[0032] • figure 5 shows an example of a micrograph of the Mylar weld bead in polarized light, according to the invention ;
[0033] • figure 6 shows an example of the tensile strength of the seal, which increases as the chamber pressure decreases, according to the invention .
[0034] It is specified here that elements of different embodiments can be combined together to provide further embodiments without limits respecting the technical concept of the invention, as a person skilled in the art will readily understand from what is described . The present description also refers to the prior art for its implementation, regarding the detailed characteristics not described, such as for example elements of minor importance usually used in the prior art in solutions of the sametype . When introducing an element, it always means that it can be "at least one" or "one or more" .
[0035] When a list of elements or features is listed in this description, it means that the invention "comprises" or alternatively "consists of" such elements . When features are listed within the same sentence or bulleted list, one or more of the individual features can be included in the invention without connection to the other features of the list .
[0036] Two or more of the parts (elements, devices, systems ) described below can be freely associated and considered as a kit of parts according to the invention .
[0037] Embodiment s
[0038] The present patent application represents an evolution of the TLW described above . The invention mainly consists in the development of a method aimed at welding and possibly also cutting polymeric films transparent to visible light, using for example a low-cost laser source for hobby use . An apparatus 1000 for carrying out the method may comprise three main components :
[0039] 1 ) A laser source, for example with any wavelength (the important thing is to transfer heat ) , preferably in the visible range ( solely for economic reasons ) , for example at 450 nm ( for example, without limitation, in the range of ±10%) , and a related movement and control system;2 ) A vacuum pump, for example a low-cost Venturi-type water pump;
[0040] 3 ) A laminated and hermetically sealed film containment system with a sealing gasket, connected to the vacuum pump .
[0041] The "laminated" system 100 comprises the superposition of different layers, between which the two (or more) polymeric films to be welded are enclosed . Referring to the example of Figs . 2A and 2B, respectively for the cross-sectional and exploded view, from top to bottom there are :
[0042] • an upper glass plate 91, for example of the float type (i . e . an "extra-flat" glass, obtained by floating molten glass on a metal bath, usually Sn) ;
[0043] • or of the extra-clear type (with greater transparency to visible light ) , transparent to the wavelength of 450 nm and with structural requirements necessary to apply the pressure required to clamp the films (therefore with variable thickness depending on the vacuum level applied) ;
[0044] • the two polymeric films 20, 30 to be welded : for example, in the case of co-extruded films having a heat-sealable layer (i . e . , with a softening point at a lower temperature than the bulk polymer) , this must face inwards for both films;
[0045] • a (highly) absorbent layer 50 at the wavelength of the laser light 11 emitted by the source 10 : for example, a red silicone plate capable of withstanding temperatures of 230 °C can be used;• instead of the absorbent layer, a pigment or dye can be used, provided it is of sufficient thickness / concent ration to guarantee the necessary absorption;
[0046] • also in this case, we will refer to an "absorbent layer" ;
[0047] • a lower plate 92 of suitable material ensuring good flatness and mechanical strength : in a specific case, a second float glass plate was used, whose function is to support and simultaneously back the sealing gasket 70 .
[0048] The sealing gasket 70 is placed on the outer perimeter of the laminated system 100 and allows connection 80 to the vacuum pump 85 , via a hose barb inserted in a specially made sleeve 80 . Instead of silicone, any material can be used that is resistant to temperatures higher than those required to make the joint, and absorbent (thanks , for example, to adequate pigmentation) at the appropriate wavelength (including "rigid" materials, although silicone has the undeniable advantage of mitigating unevenness in the assembly thickness ) .
[0049] In the laser welding process known as Transmission Laser Welding (TLW) , the two components to be welded are overlapped and it is necessary that the upper component , placed first in the laser ' s optical path, is transparent to the wavelength of the source used . It is also essential that an adequate clamping pressure is applied between the parts, necessary to ensure intimate contact between thecomponents . In general, in TLW processes it is possible to identify the four phases indicated in Fig . 3
[0001] which are also common to prior art :
[0050] 1 . Positioning of the components 20, 30 to be welded; 2 . Heating of the interface 25 (optional) between components 20, 30 by selective absorption of the laser source;
[0051] 3 . Application of the necessary pressure;
[0052] 4 . Cooling and consolidation of the welded joint .
[0053] Preferably according to the invention, an absorbent layer 50 is positioned on the lower planar plate 92 (made for example of float glass or other planar material with a glossy finish, to ensure hermetic sealing) , i . e . , for example a red-colored silicone plate, in the specific case of using a blue light laser source . The two films 20 , 30 are placed above the absorbent layer 50, using for example a roller that allows the elimination of any air pockets . Finally, the system can be completed by placing a float glass plate 91 transparent to the wavelength of the laser source on top of the films .
[0054] Once the sealing gasket is inserted and the desired degree of vacuum is reached, the system allows the films to be welded, exploiting the vacuum to apply pressure homogeneously between the films themselves (by the upper glass plate 91 ) and simultaneously eliminate any air pockets , which would reduce the efficiency of the heat exchange necessary for the films themselves to melt . The use of vacuum is not found in the prior art .The heating to the melting point of the thermoplastic films 20, 30 occurs, preferably according to the invention, thanks to the presence of the absorbent layer 50 placed beneath them. The melting and re-solidification process can be controlled, for a given polymer, as a function of the laser process parameters . Briefly, TLW welding involves passing the laser energy through the upper layers 91, 20, 30 of the assembly 100, which are transparent to the wavelength of the source, and transferring it to the absorbent layer 50 placed below them, where absorption and conversion into thermal energy take place . Part of the thermal energy generated in the absorbent layer 50 is transferred to the upper polymeric films 20, 30 by conduction, causing them to melt and giving rise, after an appropriate cooling phase, to a weld bead, thanks to molecular diffusion .
[0055] Below are some examples of system utilization, together with the evaluation of welding performance, carried out by means of welding mechanical resistance measurements .
[0056] EXAMPLE 1 - Welding of heat-sealable POF films with a total thickness of 15 pm
[0057] The vacuum setup consists of a rectangular float glass plate with dimensions 250x250x8 mm and an absorbent layer consisting of a red-colored silicone baking sheet produced by Silikomart s . r . l . , with dimensions 230x230 mm and a thickness of about 1 . 4 mm. The films to be welded, placed between the upper float glass plate and the absorbentsilicone layer, are made of coextruded POF (with the interface created by the contact zone between them) with polyethylene and polypropylene layers produced by The NewPack Ltd . The nominal thickness is 15 pm. The seal is guaranteed by a cast silicone gasket made in the laboratory (Prochima GLS Pro-20 ) . The welds were performed using a commercial laser engraver (Ortur Laser Master 2 Pro s2 ) equipped with laser sources of 1600 mW (Ortur LU 2-2 , spot diameter of 70 pm x 60 pm) and 5500 mW (Ortur LU 2-4 SF, spot diameter of 170 pm x 250 pm) both emitting at 450±5 nm . The vacuum setup is placed within the xy frame of the laser, which measures approximately 400x400 mm. Welds were successfully obtained with both sources . For simplicity, only the 5 .5 W source will be referred to below .
[0058] The weld bead consists of rectangular patterns measuring 75 x5 mm, from which to extract 5 samples for subsequent mechanical tests with a rectangular area measuring 15x5 mm, prepared according to the ASTM F088M standard .
[0059] Both welding and cutting of the samples were performed in a single operation, using the following parameters :
[0060] • Optical power : 23% for welding (corresponding to about 1265 mW) and 24% for cutting (corresponding to about 1320 mW) ;
[0061] • Scanning speed : 600 mm / min ( 10 mm / s ) for welding and 120 mm / min ( 2 mm / s ) for cutting;
[0062] • Line spacing (corresponding to the pitch between one scan line and the next ) , variable between 30 and 300 pm .The samples thus obtained were subjected to peel testing according to the ASTM F088M standard (Standard Test Method for Seal Strength of Flexible Barrier Material ) , using a Zwick / Roell Z2 . 5 mechanical testing machine with a 100 N load cell in displacement control at a speed of 200 mm / min . The strength of the observed welds varies between 3 and 4 . 8 N / 15 mm, with values generally higher than those of thermally obtained welds . Fig . 4a shows the optical micrograph of one of the weld beads made, before undergoing mechanical testing : as an example, figure 4b shows one of the obtained load curves .
[0063] EXAMPLE 2 - Welding of heat-sealable POF films with a total thickness of 25 pm
[0064] The vacuum setup consists of a rectangular float glass plate with dimensions 250x250x8 mm and an absorbent layer consisting of a red-colored silicone baking sheet produced by Silikomart s . r . l . , with dimensions 230x230 mm and a thickness of about 1 . 4 mm. The films to be welded, placed between the upper float glass plate and the absorbent silicone layer, are made of coextruded POF with polyethylene and polypropylene layers produced by The NewPack Ltd . The nominal thickness is 25 pm. The seal is guaranteed by a cast silicone gasket made in the laboratory (Prochima GLS Pro-20 ) . The welds were performed using a commercial laser engraver (Ortur Laser Master 2 Pro s2 ) equipped with laser sources of 1600 mW (Ortur LU 2-2 , spot diameter of 70 pm x 60 pm) and 5500 mW (Ortur LU 2-4 SF,spot diameter of 170 pm x 250 pm) both emitting at 450±5 nm . The vacuum setup is placed within the xy frame of the laser, which measures approximately 400x400 mm. Welds were successfully obtained with both sources . For simplicity, only the 1 . 6 W source will be referred to below .
[0065] The weld bead consists of rectangular patterns measuring 75 x5 mm, from which to extract 5 samples for subsequent mechanical tests with a rectangular area measuring 15x5 mm, prepared according to the ASTM F088M standard .
[0066] Both welding and cutting of the samples were performed in a single operation, using the following parameters :
[0067] • Optical power : 33% for both welding and cutting (corresponding to about 530 mW) ;
[0068] • Scanning speed : 800 mm / min ( 13 .33 mm / s ) for welding and 100 mm / min ( 1 . 67 mm / s ) for cutting;
[0069] • Line spacing (corresponding to the pitch between one scan line and the next ) , variable between 25 and 100 pm .
[0070] The obtained samples were subjected to peel testing according to the ASTM F088M standard (Standard Test Method for Seal Strength of Flexible Barrier Material ) , using a Zwick / Roell Z2 . 5 mechanical testing machine with a 100 N load cell in displacement control at a speed of 200 mm / min . The strength of the observed welds varies between 7 . 6 and 12 .3 N / 15 mm, with values generally higher than thermally obtained welds .EXAMPLE 3 - Welding of non-heat-sealable "plain" BOPP films with a thickness of 25 pm
[0071] The vacuum setup consists of a rectangular float glass plate with dimensions 250x250x8 mm and an absorbent layer consisting of a red-colored silicone baking sheet produced by Silikomart s . r . l . , with dimensions 230x230 mm and a thickness of about 1 . 4 mm. The films to be welded, placed between the upper float glass plate and the absorbent silicone layer, are made of homopolymer BOPP (a single homogeneous layer, without coextrusion with layers having lower melt ing / sof tening temperatures ) . The nominal thickness is 25 pm. The seal is guaranteed by a cast silicone gasket made in the laboratory (Prochima GLS Pro-20 ) . The welds are performed using a commercial laser engraver (Ortur Laser Master 2 Pro s2 ) equipped with a 5500 mW laser source (Ortur LU 2-4 SF, spot diameter of 170 pm x 250 pm) emitting at 450±5 nm. The vacuum setup is placed within the xy frame of the laser, which measures approximately 400 x400 mm.
[0072] The weld bead consists of rectangular patterns measuring 75 x5 mm, from which to extract 5 samples for subsequent mechanical tests with a rectangular area measuring 15x5 mm, made according to the ASTM F088M standard .
[0073] Both welding and cutting of the samples were performed in a single operation, using the following parameters :
[0074] • Optical power : 25% for both welding and cutting (corresponding to about 1375 mW) ;• Scanning speed : 600 mm / min ( 10 mm / s) for welding and 80 mm / min ( 1 .33 mm / s) for cutting;
[0075] • Line spacing (corresponding to the pitch between one scan line and the next ) , variable between 25 and 100 pm .
[0076] The obtained samples were subjected to peel testing according to the ASTM F088M standard (Standard Test Method for Seal Strength of Flexible Barrier Material ) , using a Zwick / Roell Z2 . 5 mechanical testing machine with a 100 N load cell in displacement control at a speed of 200 mm / min . The strength of the observed welds varies between 6 .2 and 12 . 9 N / 15 mm, with values higher than the corresponding ones obtainable on BOPP films with a heat-sealable layer
[0077] EXAMPLE 4 - Welding of non-heat-sealable Mylar films with a thickness of 3 pm
[0078] The vacuum setup consists of a rectangular float glass plate with dimensions 250x250x8 mm and an absorbent layer consisting of a red-colored silicone baking sheet produced by Silikomart s . r . l . , with dimensions 230x230 mm and a thickness of about 1 . 4 mm. The films to be welded, placed between the upper float glass plate and the absorbent silicone layer, are made of commercial PET . The nominal thickness is 3 pm. The seal is guaranteed by a cast silicone gasket made in the laboratory (Prochima GLS Pro-20 ) . The welds are performed using a commercial laser engraver (Ortur Laser Master 2 Pro s2 ) equipped with a 1600 mW laser source (Ortur LU 2-2 , spot diameter of 70 pm x 60 pm)emitting at 450±5 nm. The vacuum setup is placed within the xy frame of the laser, which measures approximately 400x400 mm.
[0079] The weld bead consists of rectangular patterns measuring 12 x2 mm (Fig . 5 ) . Only welding is performed using the following parameters :
[0080] - Optical power : 45% (corresponding to about 720 mW) ; - Scanning speed : 2000 mm / min ( 33 .33 mm / s ) ;
[0081] - Line spacing of about 33 pm.
[0082] According to some aspects of the invention, the technique described above can have three variations :
[0083] - use of a source with the same wavelength described above, but using a galvanomet ric mirror system to move the beam, with the possibility of reaching much higher scanning speeds (even above 10000 mm / s ) , provided the source has sufficient optical power to deposit the same energy;
[0084] - welding between films that exhibit a curvature (not excessive, in particular for "inextensible" thermoplastic films ) , using a glass plate with the desired curvature and a 4- or 5-axis handling system; - Welding of more than two polymeric films ( in any embodiment ) , provided their overall thickness does not exceed a few hundred microns and provided they are compatible, as previously described, from a chemical-physical point of view .EXAMPLE 5 - Effect of vacuum level on the weld bead strength of heat-sealable POE films with a total thickness of 25 pm The vacuum setup consists of a rectangular float glass plate with dimensions 250x250x8 mm and an absorbent layer consisting of a red-colored silicone baking sheet produced by Silikomart s . r . l . , with dimensions 230x230 mm and a thickness of about 1 . 4 mm. The films to be welded, placed between the upper float glass plate and the absorbent silicone layer, are made of coextruded POE with polyethylene and polypropylene layers produced by The NewPack Ltd . The nominal thickness is 25 pm. The seal is guaranteed by a cast silicone gasket made in the laboratory (Prochima GLS Pro-20 ) . The welds are performed using a commercial laser engraver (Ortur Laser Master 2 Pro s2 ) equipped with a 5500 mW laser source (Ortur LU 2-4 SF, spot diameter of 170 pm x 250 pm) emitting at 450±5 nm . The vacuum setup is placed within the xy frame of the laser, which measures approximately 400 x400 mm. The desired vacuum is obtained through the use of a KNF N 816. 3 . KT . 18 diaphragm pump, connected to the assembly via a silicone tube . The vacuum level in the chamber is regulated by a manual valve, depending on the absolute pressure reading obtained thanks to a Thyracont VD81 digital vacuum gauge with a resolution of 1 mbar .
[0085] The weld bead consists of rectangular patterns measuring 75 x5 mm, from which to extract 5 samples for subsequent mechanical tests with a rectangular area measuring 15x5 mm, made according to the ASTM F088M standard .Both welding and cutting of the samples are performed in a single operation, using the following parameters :
[0086] • Optical power : 23% for welding and 24% for cutting (corresponding to about 1265 mW) ;
[0087] • Scanning speed : 600 mm / min ( lOmm / s ) for welding and 120 mm / min ( 2 mm / s ) for cutting;
[0088] • Line spacing (corresponding to the pitch between one scan line and the next ) of 120 pm.
[0089] The obtained samples were subjected to peel testing according to the ASTM F088M standard (Standard Test Method for Seal Strength of Flexible Barrier Material ) , using a Zwick / Roell Z2 . 5 mechanical testing machine with a 100 N load cell in displacement control at a speed of 200 mm / min . The strength of the observed welds varies between 0 . 44 and 8 . 8 N / 15 mm depending on the absolute pressure in the chamber . The tests at 1000 mbar correspond to welds obtained at atmospheric pressure, using as the only source of pressure the weight force of the upper glass plate resting on the two films (about 12 N, corresponding to a clamping pressure between the films of about 190 / 200 Pa) . The weld beads were obtained by varying the pressure between 1000 mbar and the maximum vacuum degree obtainable with the diaphragm pump (corresponding to about 22 mbar of absolute pressure) , varying the pressure in steps of 100 mbar . The results obtained, summarized in Fig . 6, show that the resistance of the welding seal increases as the pressure in the chamber decreases, although not in a monotonic manner : in particular, to obtain a resistant beadit is sufficient that the absolute pressure in the chamber is less than 900 mbar, corresponding to a clamping pressure between the films of about 10 kPa . For each pressure, 5 samples were made and the vertical bars in the figure indicate the standard deviation of the series .
[0090] Advantages of the invention
[0091] Among the main advantages of the proposed method compared to existing ones are :
[0092] 1 . The possibility of also using a laser source in the visible range (e . g . , at 450 nm) at low optical power, which is economical and easily available commercially, and with a shorter wavelength than the sources traditionally used (and therefore with a lower diffraction limit and the possibility of reaching higher resolution) ;
[0093] 2 . The possibility of avoiding the use of pigments or absorbing elements in the lower film layer (or at the interface) , which modify its characteristics of laser energy absorption, thanks to the use of an absorber placed beneath both layers of film to be welded;
[0094] 3 . The possibility of performing both welding and cutting of the polymeric films using the same setup, thanks to the simple regulation of the laser scanning parameters ;
[0095] 4 . The possibility of homogeneously distributing the clamping pressure over the entire area of the films , in particular also in the zone affected by the opticalpath of the laser beam, thanks to the use of a vacuum system with pressure that can be adjusted as desired (provided it is lower than the pressure of the external environment ) ;
[0096] 5 . The minimization of air pockets present between the films and between the films and the lower absorbent layer, which are detrimental to heat exchange, thanks to the use of the vacuum and possibly to the simultaneous reduction of humidity (by evacuating the gases in the chamber with the vacuum, the water vapor present is also removed) .
[0097] Among the target markets are industrial packaging, microfluidics and biomedical sector, for which welding in sterile conditions is often required . The method has been successfully validated on a laboratory scale on different geometries and areas and on two different polymers , successfully creating welds even of 3 overlapping layers of film .
[0098] List of reference numerals for the figures
[0099] 10 : Laser Source
[0100] 11 : Laser light
[0101] 20 : First polymeric film
[0102] 25 : Interface between the two polymeric films
[0103] 30 : Second polymeric film
[0104] 40 : Clamping pressure
[0105] 50 : Absorber
[0106] 60 : Welding zone70 : Perimeter gasket
[0107] 80 : Connection to the vacuum pump
[0108] 85 : Vacuum pump
[0109] 91 : Glas s transparent to the laser
[0110] 92 : Lower support
[0111] 100 : Laser welding as sembly
[0112] 1000 : Laser welding apparatus
[0113] Bibliographic References
[0114]
[0001] L . F . F . F . Gonpalves , F . M . Duarte , C . I . Martins , and M . C . Paiva , "Laser welding of thermoplastics : An overview on lasers , materials , proces se s and quality, " Infrared Phys . Technol . , vol . 119 , no . August , p . 103931 , 2021 , doi : 10 . 1016 / j . inf rared . 2021 . 103931
[0115]
[0002] Qiu, J . ; Zhang, G . ; Sakai , E . ; Liu , W . ; Zang, L . Thermal Welding by the Third Phase Between Polymers : A Review for Ultrasonic Weld Technology Development s . Polymers 2020 , 12 , 759 . https : / / doi . org / 10 . 3390 / polyml 2040759
[0116]
[0003] Wang, D . , Li , J . , Jin, J . , Pan, Y . , Liang, H . , Ji , X . and Jiang, W . , 2024 . Chlorosulfonated Poly (propylene carbonate ) -Based Pres sure-Sensit ive Adhesive s with Improved Thermal Stability and Peel St rength . ACS Applied Polymer Materials , 6 ( 15 ) , pp . 8896-8904
[0117]
[0004] Ranvi j ay Kumar . " Solid-State Welding Technique s for Polymeric Materials : A State of The Art Review And Future Prospective" International Journal of Engineering Trends and Technology 69 . 1 ( 2021 ) : 139-146 . DOI : 10 . 14445 / 22315381 / I JETT-V69 I1P222
[0005] Bamps B, Bunt inx M, Peeters R . Seal materials in flexible plastic food packaging : A review . Packag Technol Sci . 2023 ; 36 ( 7 ) : 507-532 . doi : 10 . 1002 / pt s . 2732
[0118]
[0006] Acher j ee B . , Laser transmis sion welding of polymers-a review on proces s fundamentals , material att ributes , weldability, and welding techniques . JManufProce s s , 60 ( 2020 ) , pp . 227-246 . doi . org / 10 . 1016 / j . jmapro . 2022 . 05 . 026
[0119] In the foregoing, preferred embodiment s have been de scribed and variations of the pre sent invention have been suggested, but it is to be understood that those skilled in the art may make modif icat ions and changes without thereby departing from the relevant scope of protection , as defined by the attached claims .
Claims
CLAIMS1 . Method for welding transparent polymeric films us ing a source ( 10 ) of laser light ( 11 ) , the method compris ing the following steps :• positioning an absorbent layer ( 50 ) on a lower support plate ( 92 ) , the absorbent layer being conf igured to absorb at least a portion of the laser light ( 11 ) ;• positioning a second transparent polymeric film ( 30 ) and a first transparent polymeric film ( 20 ) above the absorbent layer ( 50 ) , in sequence ;• positioning a transparent glas s plate ( 91 ) above the first transparent polymeric film ( 20 ) ;• sealing the as sembly ( 100 ) comprising the lower support plate ( 92 ) , the absorbent layer ( 50 ) , the second ( 30 ) and the first ( 20 ) transparent polymeric film and the transparent glas s plate ( 91 ) with a perimeter gasket ( 70 ) to create a hermetic chamber;• applying a vacuum to the hermetic chamber by means of a vacuum pump ( 85 ) connected ( 80 ) to said hermetic chamber to generate a predetermined pres sure between the t ransparent glas s plate ( 91 ) and the lower support plate ( 92 ) , thereby pre s s ing the first ( 20 ) and the second ( 30 ) transparent polymeric film together and with the absorbent layer ( 50 ) , and thereby minimi zing any air pocket s ;irradiating the transparent glas s plate ( 91 ) with said laser light ( 11 ) .
2. Method according to claim 1 , wherein the absorbent layer ( 50 ) i s made of a silicone material .
3. Method according to claim 1 or 2 , wherein at least a further third polymeric layer is positioned above the first polymeric layer ( 20 ) .
4. Method according to one of claims 1 to 3 , wherein the absorbent layer ( 50 ) cons ist s of or comprises a pigment or a dye .
5. Method according to one of claims 1 to 4 , wherein the laser source ( 10 ) has a wavelength in the visible range , in particular of about 450 nm .
6. Method according to one of claims 1 to 5 , wherein the transparent glas s plate ( 91 ) i s a float glas s with st ructural requirement s for applying said predetermined pres sure .
7. Method according to one of claims 1 to 6 , wherein the step of irradiating laser light ( 11 ) include s regulat ing an optical power of the laser light source ( 10 ) and a scanning speed of the laser light source ( 10 ) to simultaneous ly perform welding and cutting of the first ( 20 ) and second ( 30 ) t ransparent polymeric f ilm .
8. Method according to one of claims 1 to 7 , wherein the first ( 20 ) and second ( 30 ) transparent polymeric films are selected from the group consisting of polyethylene , polypropylene and polyethylene terephthalate (PET ) .
9. Method according to one of claims 1 to 8 , wherein the as sembly ( 100 ) is allowed to cool after irradiat ion with the laser source .
10. Apparatus ( 1000 ) for welding transparent polymeric films using a source ( 10 ) of laser light ( 11 ) , the apparatus compris ing :• a lower support plate ( 92 ) configured to support an absorbent layer ( 50 ) ;• an absorbent layer ( 50 ) positioned on the lower support plate ( 92 ) , configured to absorb at least a port ion of the laser light ( 11 ) ;• a second transparent polymeric film ( 30 ) and a first transparent polymeric film ( 20 ) positioned, in this order, above the absorbent layer ( 50 ) ;• a transparent glas s plate ( 91 ) pos itioned above the first transparent polymeric film ( 20 ) ;• a perimeter gasket ( 70 ) configured to seal the as sembly ( 100 ) comprising the lower support plate ( 92 ) , the absorbent layer ( 50 ) , the second ( 30 ) and the first ( 20 ) t ransparent polymeric film and thetransparent glas s plate ( 91 ) , to create a hermetic chamber;• a vacuum pump ( 85 ) connected ( 80 ) to the hermetic chamber to generate a predetermined pres sure between the t ransparent glas s plate ( 91 ) and the lower support plate ( 92 ) , thereby pre s s ing the first ( 20 ) and the second ( 30 ) transparent polymeric film together and with the absorbent layer ( 50 ) , and thereby minimi zing any air pocket s ;• the source ( 10 ) of laser light ( 11 ) .
11. Apparatus according to claim 10 , wherein the laser light ( 11 ) source ( 10 ) is configured to apply di f ferentiated powers or differentiated speeds for the welding and for the cutting of said first ( 20 ) and second ( 30 ) transparent polymeric film .
12. Apparatus according to one of claims 10 or 11 , wherein the laser light ( 11 ) has a wavelength in the vi sible range , in part icular of about 450 nm .
13. Apparatus according to one of claims 10 to 12 , wherein the perimeter gasket ( 70 ) comprises a connect ion ( 80 ) to the vacuum pump ( 85 ) .
14. Apparatus according to one of claims 10 to 13 , compris ing a beam steering system with galvanomet ric mirrors , configured to steer said laser light ( 11 ) .
15. Apparatus according to one of claims 10 to 14 , wherein at least a further third polymeric layer is positioned above the first polymeric layer ( 20 ) .
16. Apparatus according to one of claims 10 to 15, wherein the absorbent layer (50 ) consists of or comprises a pigment or a dye .