Heterogeneous catalyst for co 2 hydrogenation, its process of preparation, and use thereof

A ternary mixed metal oxide catalyst addresses the inefficiencies of existing CO2 hydrogenation catalysts by achieving high selectivity and yield of methanol and dimethyl ether through a novel preparation process, enabling stable industrial-scale production.

WO2026234703A1PCT designated stage Publication Date: 2026-11-12COUNCIL OF SCI & IND RES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IN2026/050778
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing heterogeneous catalysts for CO2 hydrogenation suffer from low efficiency, selectivity, and yield in producing methanol and dimethyl ether, necessitating the development of compositionally tuned, mixed-oxide frameworks for selective conversion at low temperatures and pressures.

Method used

A heterogeneous catalyst comprising ternary mixed metal oxides represented by the formula (AwByCx-y)Oz, where A is a d-block element, B and C are p-block or inner transition elements, is prepared through a process involving precipitation, aging, washing, drying, and calcination, and used for CO2 hydrogenation under mild conditions to enhance catalytic performance.

Benefits of technology

The catalyst achieves high selectivity and yield of methanol and dimethyl ether, with CO2 conversion rates up to 30% and selectivity exceeding 95% for methanol, demonstrating stability and efficiency for industrial-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000002_0001
    Figure IMGF000002_0001
  • Figure IMGF000013_0001_TABLE
    Figure IMGF000013_0001_TABLE
  • Figure IMGF000014_0001_TABLE
    Figure IMGF000014_0001_TABLE
Patent Text Reader

Abstract

The present invention generally relates to metal chemistry specifically for the catalytic reactions. Particularly, the present invention relates to a heterogeneous catalyst comprising ternary mixed metal oxides for hydrogenation of CO2 and / or CO, and a process of preparation thereof. The present invention also relates to a process of preparation of value-added products specifically formation of C1-C3 oxygenated products (e.g. methanol, dimethyl ether, etc.), by hydrogenating CO2 and / or CO in presence of said heterogeneous catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] PT / 2026 / 12077

[0002] HETEROGENEOUS CATALYST FOR CO2HYDROGENATION, ITS PROCESS OF PREPARATION, AND USE THEREOF

[0003] FIELD OF THE INVENTION

[0004] The present invention generally relates to catalyst chemistry specifically for crucial industrial reactions. Particularly, the present invention relates to a heterogeneous catalyst comprising ternary mixed metal oxides for hydrogenation of CO2 and / or CO, and a process of preparation thereof. The present invention also relates to the process of preparation of value-added products, specifically the formation of C1-C3 oxygenated products (e. g. methanol, dimethyl ether, etc.), by hydrogenating CO2 and / or CO in the presence of ternary heterogeneous catalysts.

[0005] BACKGROUND OF THE INVENTION

[0006] According to the Intergovernmental Panel on Climate Change (IPCC), by the end of the twenty-first century, greenhouse gas (GHG) emissions will have caused the mean global temperature to rise from 1.1° to 6.4 °C. Reducing GHG emissions into the environment and seeking alternative carbon sources for energy and chemicals are essential challenges, as climate change and the depletion of fossil fuels are major problems today. Both issues can be resolved by developing methods for converting CO2, a typical greenhouse gas, into useful compounds. As a result, research into catalysts for CO2 utilization is expanding globally. CO2 is a thermodynamically stable molecule that requires extensive energy to break the O=C=O bonds (799 kJ / mol) and convert them into fine chemicals. Methanol is one of the most promising conversion targets for CO2 because it can be used as a raw material for various fine chemicals, fuel additives, and energy carriers. Considering the methanol process and industrial syngas are similar, Cu-based and Pd-based catalysts have been studied at high pressures and temperatures (250-300 °C and 3-10 MPa) for CO2 hydrogenation to methanol (refer, Saeidi, S.; Amin, N. A. S.; Rahimpour, M. R, J. CO2 Util. 2014, 5, 66-81).

[0007] A high reaction temperature is also detrimental in thermodynamics because the hydrogenation of CO2 to methanol and methanol to DME are exothermic processes (equations 1 and 2). Moreover, the direct conversion of CO2 into methane (equation 3) and olefins (equation 4) is also challenging and interesting to evaluate. However, no ideal catalyst will selectivelyPT / 2026 / 12077

[0008] produce methanol, DME, or olefins due to the specific requirement of different active sites for these distinct reactions.

[0009] > CO2m-I2CI-hOH + H2O ARH°- -50kJ mor[> > 2CO2+ 6H22CH?OH + 2H2O CH,OCH, + 3 H2O ARH° = -123 kJ mol’5(2) COo + 4H-> CH4+ 2H-0z-\ pH0= -165 kJ mol4> (3) x CO, y - **" CnILt)+ CnlLn+ z FhO

[0010]

[0011] A > (4)

[0012] Thus, there has been an intense effort to design catalysts that allow for low -temperature action. Even though there have been numerous reports of successful low-temperature methanol synthesis (<100 °C) using homogeneous catalysts (refer, Du, X. L.; Jiang, Z.; Su, D. S.; Wang, J. Q, ChemSusChem 2016, 9, 322-332; and Porosoff, M. D.; Yan, B.; Chen, J. G, Energy Environ. Sci. 2016, 9, 62-73) in terms of product separation, catalyst stability, and the difficulty of catalyst synthesis, hence, heterogeneous catalysts may be better suited for real-world applications than homogeneous catalysts.

[0013] As a result, reports of heterogeneous catalysts that remain active at room temperature (<30 °C) have just recently started to surface (refer, Weststrate, C. J.; Sharma, D.; Garcia Rodriguez, D.; Gleeson, M. A.; Fredriksson, H. O. A.; Niemantsverdriet, J. W. Nat. Commun.

[0014] 2020, 11, No. 750). Without uncertainty, the ability to perform large-scale CO2conversion at low temperatures (<250 °C) and low pressure (<40 bar) is appealing because of its costeffectiveness and commercialization. However, these catalyst's conversion efficiency is incredibly low (15 -17%) and with lower selectivity towards methanol and DME production (around 30-50%), necessitating the employment of far more active catalysts beyond the academic level of CO2 hydrogenation [additionally refer, US20230234039A1 and a research article by Pechenkin, Alexey, et al., Green Processing and Synthesis 10.1 (2021): 594-605]. A requirement for compositionally tuned, single-phase or strongly interacting mixed-oxide framework are being researched for creating well-defined electronic and structural environments at the active sites for selective conversion of CO2 . In the article by Liu, Hao et. al, Applied Catalysis B: Environmental Volume 48, Issue 1, 8 March 2004, Pages 37-48PT / 2026 / 12077

[0015] Co-In / A12O3 catalysts are disclosed, however, for the selective reduction of NO by propene. Moreover, the catalysts are not mixed oxide heterogeneous catalysts, but Coilm supported on alumina.

[0016] There is, therefore, a need in the art for heterogeneous catalysts which can effectively produce CO2 hydrogenated products like methanol, DME, etc. with greater yield, selectivity and efficiency, thus addressing the aforesaid and other problems of prior art.

[0017] OBJECTIVES OF THE INVENTION

[0018] An object of the present invention is to provide a heterogeneous catalyst comprising ternary mixed metal oxides.

[0019] Another object of the present invention is to provide a process of preparation of said heterogeneous catalyst.

[0020] Yet another object of the present invention is to provide a process of preparation of value-added products by reacting CO2 and or CO with the heterogeneous catalyst comprising ternary mixed metal oxides.

[0021] Another object of the present invention is to provide for the large-scale production of methanol and methanol-derived products with high selectivity and yield.

[0022] SUMMARY OF THE INVENTION

[0023] In an aspect, the present invention relates to heterogeneous catalysts being represented by:

[0024] (Aw ByCX-y)Oz

[0025] Formula (I)

[0026] wherein

[0027] A is a metal selected from d-block element;

[0028] B is a metal selected from p-block element and inner transition element;

[0029] C is a metal selected from p-block element and inner transition element;

[0030] w is in the range of 0.5 to 1.5;

[0031] x is in the range of 0.01 to 1;PT / 2026 / 12077

[0032] y is in the range of 0.01 to 1; and

[0033] z is in the range of 1 to 4.

[0034] In an embodiment, the present invention relates to heterogeneous catalysts having Formula (I): AiByCx-yOz,

[0035] wherein A is selected from Cu, Mn, Co, Ir, , Zn, Pt, Pd, Rh, Ru, Mg and Sr;

[0036] B and C are selected from Al, Ga, In, Ce, Zr, Nb, Ti, Si, Fe and P

[0037] and wherein x= 0.01 to 1, y= 0.01 to 1 and z=l to 4.

[0038] In an embodiment the heterogenous catalyst is selected from a group comprising cobaltindium- aluminium (CoInAlO), copper-indium- aluminium (CuInAlO), cobalt-zirconium-aluminium (CoZrAlO), cobalt-indium-iron (CoInFeO), cobalt-gallium-aluminium (CoGaAlO), and cobalt-cerium-aluminium (CoCeAlO).

[0039] In another aspect, the present disclosure relates to a process of preparation of the heterogeneous catalyst, comprising steps of:

[0040] a. preparing and providing metal precursor solution comprising precursors of metal A, B and C;

[0041] b. providing base solution comprising a base in water as solvent;

[0042] c. co-precipitating and forming oxides of metals by dropwise adding and mixing the metals precursor solution of step (a) into step (b) to obtain precipitated material;

[0043] d. aging the precipitated material of step (c), followed by washing, drying the precipitate to obtain dried precipitate and

[0044] e. calcining the dried precipitate of step (d) to obtain the heterogeneous catalyst.

[0045] In another aspect the present invention relates to a process of CO2 hydrogenation in the presence of a heterogenous catalyst comprising the steps of

[0046] a) reducing the heterogeneous catalyst in a reactor; andPT / 2026 / 12077

[0047] b) treating and reacting CO2 and H2 supplied separately in said reactor to react and reduce the CO2 in the presence of said reduced heterogeneous catalyst of step a);

[0048] wherein the heterogeneous catalyst is AiByCx-yOz,

[0049] having A selected from Cu, Mn, Co, Ir, Zn, Pt, Pd, Rh, Ru, Mg and Sr; B and C selected from Al, Ga, In, Ce, Zr, Ti, Nb, Si, Fe and P and where x= 1 to 0.01, y= 0.01 to 1 and z=l to 4.

[0050] In an embodiment of the process of CO2 hydrogenation, the temperature is in the range of 180-300 °C and the pressure is in the range of 1-60 bar in step (b).

[0051] BRIEF DESCRIPTION OF THE DRAWINGS:

[0052] Figure 1 illustrates XRD patterns of different heterogeneous catalysts of formula I at various scales.

[0053] Figure 2 shows TPR profiles of the CIA-30 catalyst (of present disclosure), and CIA-0 catalyst (for comparison).

[0054] Figure 3 shows NH3-TPD profiles of CIA-30 catalyst (of present disclosure), and CIA-0 catalyst (for comparison).

[0055] Figure 4 shows Py-DRIFT pattern of the prepared catalysts.

[0056] Figure 5 shows HRTEM micrographs and elemental mapping of CIA-30 catalyst.

[0057] Figure 6 shows catalytic performance of CO2 hydrogenation using D2 over CIA-30 catalyst under the condition of 220 °C, 30 bar, CO2 to H2 ratio of 1:3 and GHSV of 3000 h1.

[0058] Figure 7 shows TOS of CO2 hydrogenation over CIA-30 catalysts under the condition of 220 °C, 30 bar, CO2to H2ratio of 1:3, and GHSV of 3000-6000 h1.

[0059] Figure 8 shows XRD patterns of the fresh and spent CIA-30 catalysts.PT / 2026 / 12077

[0060] DETAILED DESCRIPTION OF THE INVENTION

[0061] In an aspect, the present invention relates to heterogeneous catalysts being represented by:

[0062] (Aw ByCX-y)Oz

[0063] Formula (I)

[0064] wherein

[0065] A is a metal selected from d-block element;

[0066] B is a metal selected from p-block element and inner transition element;

[0067] C is a metal selected from p-block element and inner transition element;

[0068] w is in the range of 0.5 to 1.5;

[0069] x is in the range of 0.01 to 1;

[0070] y is in the range of 0.01 to 1; and

[0071] z is in the range of 1 to 4.

[0072] In an embodiment, the present invention relates to heterogeneous catalysts having Formula (I): AiByCx-yOz,

[0073] wherein A is selected from Cu, Mn, Co, Ir, Zn, Pt, Pd, Rh, Ru, Mg and Sr; B and C are selected from Al, Ga, In, Ce, Zr, Nb, Ti, Si, Fe and P and wherein x= 0.01 to 1, y= 0.01 to 1 and z=l to 4.

[0074] In another embodiment, the heterogenous catalyst of the present invention is a mixed ternary catalyst having a formula: (AwByCx-y)Oz;

[0075] wherein A is selected from Cu, Mn, Co, Ir, Zn, Pt, Pd, Rh, Ru, Mg and Sr;

[0076] B and C are selected from Al, Ga, In, Ce, Zr, Nb, Si, Ti, Fe and P and

[0077] wherein w= 0.5 to 1.5; x= 0.01 to 1, y= 0.01 to 1 and z=l to 4, and has been particularly designed to enhance the catalytic performance through the synergistic effect of the three cations leading to improved oxygen mobility, increased vacancies, and higher surface area.PT / 2026 / 12077

[0078] In an embodiment, A is a transition metal cation having an oxidation state of at least +2 in the present invention. B and C are post transition metal cations having an oxidation state of at least +3 in the present invention.

[0079] In another embodiment, the heterogeneous catalyst comprising said metals A, B and C are in metal oxide or mixed metal oxides form.

[0080] In an embodiment, the d-block cation represented by A is selected from but not limited to copper, manganese, cobalt, iridium, zinc, platinum, ruthenium, magnesium, and strontium. In a specific embodiment, the metal A is selected from but not limited to cobalt and copper. Preferably, A is cobalt.

[0081] In an embodiment, the p-block cation represented by B and C are selected from but not limited to aluminium, gallium, indium, cerium, zirconium, niobium, titanium, silicon, iron and phosphorous. In a specific embodiment, the metal B is selected from but not limited to indium, zirconium, gallium, iron and cerium. In a specific embodiment, the metal C is selected from but not limited to aluminium and iron. Preferably B is Indium and C is aluminium.

[0082] In a specific embodiment, the weight % of the metal oxide of A is in the range of 30-60 wt%; the metal oxide of B is in the range of 10-20 wt% ; and the metal oxide of C is in the range of 20-40 wt% of the heterogenous catalysts as per the present invention.

[0083] In an embodiment, the heterogeneous catalyst comprises particles with uniform morphology and undefined spherical clusters. In another embodiment, the heterogeneous catalyst comprises pseudo spherical particles.

[0084] The catalyst comprises metal A, B, and / or C particles having an average particle size in the range of 10-14 nm, as determined by high-resolution TEM (HR-TEM), X-ray diffraction (XRD) line broadening analysis using the Scherrer equation. In another embodiment, the particle size of the heterogeneous catalyst as per the present invention is in the range of 10-14 nm. In another specific embodiment, the average particle size of the heterogeneous catalyst as per the present invention is 12 nm.PT / 2026 / 12077

[0085] In a specific embodiment, the heterogeneous catalyst of formula I are selected from but not limited to cobalt- indium-aluminium (CoInAlO), copper- indium- aluminium (CuInAlO), cobalt-zirconium-aluminium (CoZrAlO), cobalt-indium-iron (CoInFeO), cobalt-gallium-aluminium (CoGaAlO), and cobalt-cerium- aluminium (CoCeAlO).

[0086] The heterogeneous catalyst is in crystalline form with a spinel structure. The term “spinel” used herein is in the context of crystal, and refer to a cubic crystal system where the oxygen anions are arranged in a face-centered cubic lattice, and cations occupy tetrahedral and octahedral sites. In an embodiment, the metal B of the heterogeneous catalyst enhances the surface metal A species by being dispersed on the spinel structure, leading to improved hydrogen activation. Preferably, the B cation is Indium cation dispersed on the crystalline spinel structure of the catalyst.

[0087] Weak acidic sites on catalysts, including weak Brpnsted (proton donor) and Lewis (electron acceptor) sites, are critical for selective chemical transformations. They facilitate reactant activation while minimizing undesirable side reactions like excessive coking or overcracking. They promote dehydrogenation reactions, particularly by facilitating product desorption, improving selectivity, and reducing coke formation compared to strong acid sites The heterogenous catalyst of the present invention has a higher number of weak acidic active sites as compared to strong acidic active sites.

[0088] In a specific embodiment the present invention relates to a mixed ternary catalyst as per Formula (I) being Co-In-AlO. In an embodiment, the complete reduction of Co2+and In3+cations takes place at 650 °C, however during the reaction in the present invention, the catalyst is reduced at 400 °C to make the partially reduced catalyst (e.g. Co+ / 0-InOx-A12O3).

[0089] In another specific embodiment, in the case of CoInAl catalyst, the catalytically active sites comprise Co+-Co°-InOx-A12O3 interface.

[0090] In an embodiment, the molar ratio of A, B and C in the heterogeneous catalyst is in the range of 0.5: 0.15: 0.35 to 1.5: 0.45: 1.05. In a specific embodiment, the molar ratio of A, B and C in the heterogeneous catalyst is in the range of 1: 0.3: 0.7.

[0091] In another aspect, the present disclosure relates to a process of preparation of the heterogeneous catalyst, comprising steps of:PT / 2026 / 12077

[0092] a) preparing and providing metal precursor solution comprising precursors of metal A, B and C;

[0093] b) providing base solution comprising a base in water as solvent;

[0094] c) co-precipitating and forming oxides of metals by dropwise adding and mixing the metals precursor solution of step (a) into step (b) to obtain precipitated material;

[0095] d) aging the precipitated material of step (c), followed by washing, drying the precipitate to obtain dried precipitate and

[0096] e) calcining the dried precipitate of step (d) to obtain the heterogeneous catalyst.

[0097] In an embodiment, the co -precipitation is done under stirring at a temperature in the range of 25-35 °C and at a pH in the range of 9-10 for a time period in the range of 1-2 h to obtain the precipitated material.

[0098] In another embodiment, the precipitated material of step c) is aged at a temperature in the range of 25-35 °C for a period in the range of 11-13 h, followed by washing and drying the precipitate to obtain dried precipitate.

[0099] In an embodiment the calcining of the dried precipitate of step (d) is done at a temperature in the range of 425-635 °C for 4-7h, in step (e).

[0100] In a specific embodiment, the weight % of the metal oxide of A is in the range of 30-60 wt%; the metal oxide of B is in the range of 10-20 wt%; and the metal oxide of C is in the range of 20-40 wt% of the heterogenous catalysts as per the present invention.

[0101] In an embodiment, the precursors of metal A, B and C are selected from but not limited to sulphate, nitrate, and acetate of metal A. The metal(s) precursor solution of step a) is prepared by mixing precursor of metal A, precursor of metal B and precursor of metal C in water. Preferably the precursors to A is a nitrate , B is a nitrate, C is a nitrate.PT / 2026 / 12077

[0102] In an embodiment, the base is selected from but not limited to sodium hydroxide, potassium hydroxide, ammonium hydroxide, and so on. The base can act as a precipitating agent.

[0103] In an embodiment, the washing in step d) is done by warm water to remove the base from the precipitate.

[0104] In an embodiment, the drying in step d) is done by heating the precipitate in a hot air oven with a constant airflow of 25 ml min1for a time period in the range of 11- 13h at a temperature in the range of 100-120 °C.

[0105] In an embodiment, the calcining of step e) is done at a temperature in the range of 400-600 °C for 5-7 h with a heating rate of 1.8 °C min-1.

[0106] In a specific embodiment, the process of preparation of the heterogeneous catalyst comprises: precipitating a specific concentration of metal solutions containing specific p and d block elements against the base solution with specific molarity in the range from 0.01 to 10.0, and the whole precipitation process is carried out at pH = 9.3+0.7 by adjusting the addition of metal and base solutions concurrently. The formed precipitate is then washed with -2000 mL of warm deionized water until a neutralized decantation of water was obtained. Then, the obtained solids are dried at 100 °C for 12 hours, followed by the calcination process in the range from 500 to 600 °C with 3.5 °C per minute of ramping.

[0107] In another aspect, the present invention provides a process of hydrogenation of a CO2 comprising steps of:

[0108] a) reducing the heterogeneous catalyst in a reactor; and

[0109] b) treating and reacting CO2 and H2 supplied separately in said reactor to react and reduce the CO2 in presence of said reduced heterogeneous catalyst of step a) under one or more reaction condition(s) to obtain value-added products.

[0110] In an embodiment, the heterogeneous catalysts in the process of hydrogenation of a CO2 comprise Formula (I): AiByCx-yOz, wherein A is selected from Cu, Mn, Co, Ir, Zn, Pt, Pd, Rh, Ru, Mg and Sr; B and C are selected from Al, Ga, In, Ce, Zr, Nb, Ti, Si, Fe and P andPT / 2026 / 12077

[0111] wherein x= 0.01 to 1, y= 0.01 to 1 and z=l to 4. In another embodiment, the pellet size of heterogeneous catalyst loaded in the reactor for the process of hydrogenation of a CO2 is in the range of 0.5-0.8 mm. Preferably, the sieved pellet size of heterogeneous catalyst loaded in the reactor is 0.5-0.8 mm.

[0112] The reduction of step a) is done by treating the heterogeneous catalyst at temperature in the range of 400-600 °C in the presence of H2 gas flow for time period in the range of 1-3 h. In a specific embodiment the process of hydrogenation of a CO2 comprises reducing a heterogenous catalyst by way of the mixed ternary catalyst as per Formula (I) being Co-In- A1O. In an embodiment, the complete reduction of Co2+and In3+cations takes place at 650 °C, however during the reaction in step (a), the catalyst is reduced at 400 °C to make the partially reduced catalyst (e.g. Co-t / O-InOx-AhCh). In an embodiment the Co-In-Al ternary mixed oxide, functions as a stable and effective catalyst for the hydrogenation of CO2 at low operating temperatures.

[0113] In an embodiment, the one or more reaction condition(s) of step (b) includes the following:

[0114] i.a temperature in the range of 180-300 °C;

[0115] ii.a pressure in the range of 1-60 bar;

[0116] iii.a time period of the process is in the range of 1 to 600h;

[0117] iv.a weight ratio of CO2 to H2 is in the range of 0.5: 1.5 to 1.5: 4.5; and / or 5

[0118] v.a gas hourly space velocity of CO2 and H2 supplied separately in said reactor is in the range of 1000-12000 h1.

[0119] In specific embodiment, the pressure is in the range of 20-60 bar. The value-added products comprise C1-C3 oxygenated product / compound. In an embodiment, the C1-C3 oxygenated product / compound is selected from but not limited to methanol, ethanol, dimethyl ether, formaldehyde, acetaldehyde and formic acid.

[0120] The process of hydrogenation of CO2 is carried out in a reactor is selected from fixed bed reactor, a continuous flow reactor, batch reactor, parallel continuous flow reactor, and so on. Preferably it is a fixed bed reactor.PT / 2026 / 12077

[0121] Space-time yield (STY) is a critical performance metric in chemical engineering and bioprocessing that measures the amount of product produced per unit of bioreactor or reactor volume over a specific time. It is defined as the amount of product formed per unit time and reactor volume. In an embodiment, the space time yield of methanol is in the range of 200-400 GraniMeOH Kg cat 1 h 1.

[0122] It is observed that the conversion of CO2 into methanol by the process as per the present invention is in the range of 8-30 %. In an embodiment, the conversion of CO2 into methanol by said process is in the range of 11-26 %.

[0123] Surprisingly, it has been observed that the process of CO2 hydrogenation as per the present invention in the presence of the heterogenous catalyst of Formula (I), leads to a significantly high selectivity towards methanol under mild reaction conditions leading to a high yield of methanol. In an embodiment, the selectivity towards methanol in the process of CO2 hydrogenation as per the present invention is in the range of 95-98 %. In a specific embodiment, the yield of methanol is lower or higher than 5,600 mol / Kg cat / h of methanol. Dimethyl ether is also an important obtained by the process of CO2 hydrogenation as per the present invention. In an embodiment, the selectivity of formation of dimethyl ether by said process and catalyst is in the range of 0.5-20%.

[0124] The present invention based on the heterogenous catalyst (AvB,Cx / )O_z demonstrably provides an unexpected synergistic improvement in CO2 conversion, methanol selectivity, and stability over binary ImCh-based systems, simply supported Co-In / AbCh as it is the result of a unified, stoichiometrically governed (AvB ,Cx / )O_z lattice in which the roles of A, B, and C are co-engineered to modulate oxygen vacancies, adsorption sites, and hydrogen activation in a cooperative manner.

[0125] EXAMPLES

[0126] Following examples are given by way of illustration and therefore should not be construed to limit the scope of the invention.

[0127] Details of Materials and Equipment Used:PT / 2026 / 12077

[0128] All reagents and solvents were of commercial reagent grade procured or bought from Sigma Aldrich (India), Merck Millipore (India), and Baker and Baker (India), and were used without further purification unless otherwise noted.

[0129] EXAMPLE 1:

[0130] A) General procedure for the preparation of heterogeneous catalyst material with ternary metal oxides:

[0131] The ternary mixed oxide catalysts were synthesized by the co -precipitation method at room temperature. In a typical synthesis, a calculated molar ratio of metal precursor solution A was prepared by dissolving it in double-distilled water. Precipitating base solution B was prepared by dissolving a known amount of NaOH in double distilled water. The co -precipitation was done by dropwise addition of metal precursor solution A and base solution B simultaneously into a beaker with gentle stirring. The pH was maintained at 9.5 ± 0.3, and the solution was further stirred for an hour; subsequently, the solution was further stirred for an hour. Subsequently, the slurry was allowed for aging at room temperature for 12 h. The obtained precipitate was washed thoroughly with warm deionised water to remove the base. Then, the sample was dried in a hot air oven with a constant airflow of 25 ml min1for 12 h at 110 °C. Finally, the obtained sample was calcined at 400-600 °C for 6 h with a heating rate of 1.8 °C min-1. The obtained final catalysts are denoted as CIA-X, where X is the molar ratio of metal cation B multiplied by 10 times. The prepared catalysts as per the present invention are provided in Table 1

[0132] TABLE 1

[0133] S. No Inventive Catalyst Catalyst code

[0134] 1 CoInAlO CIA-20

[0135] 2 CoInAlO CIA-25

[0136] 3 CoInAlO CIA-30

[0137] 4 CoInAlO CIA-35

[0138] 5 CuInAlO CuIA-30

[0139] 6 CoZrAlO CZA-30

[0140]

[0141] PT / 2026 / 12077

[0142] 7 CoInFeO CIF-30

[0143] 8 CoGaAlO CGA-30

[0144] 9 CoCeAlO CCA-25

[0145]

[0146] B) General Procedure for the preparation of catalyst material without ternary metal oxides (for comparison purpose):

[0147] A catalyst without metal cation B was synthesized using the same procedure without adding an indium precursor and the obtained sample is denoted as CIA-0. In addition, a catalyst with the same molar ratio of all three metals were also prepared by sol-gel and impregnation methods and the sample were denoted as SG-X and IMP-X, where X is the malar ratio of indium multiplied by 10 times.

[0148] EXAMPLE 2: Characterization

[0149] The powder X-ray diffraction of the synthesized catalysts demonstrated a well-resolved high crystalline pattern for the final catalyst materials, as shown in Figure 1. The observed XRD reflections at different 29 values that correspond to the lattice planes are well-matched with the diffraction values of the spinel type materials. The XRD reflections at different production scales show no considerable change in its crystallinity and the observation of any other peaks. The absence of any InOxfeatures in all XRD patterns corroborates the high dispersion or the successful comprising of the indium ions in the spinel structures. Furthermore, the appearance of the XRD patterns at all scale-up syntheses exhibits that the crystalline size of the spinels remains the same, which substantiates the reproducibility of the employed synthesis methodology.

[0150] To determine the reduction nature of the prepared materials, the catalysts are subjected to the H2-TPR studies, and the obtained results are shown in Figure 2. As shown in the figure, the ternary mixed oxide catalyst CIA-30 displays three distinguishable reduction profiles that correspond to the reduction of cobalt oxides at different temperatures. The peak at 310 °C could be ascribed to the reduction of cobalt ions on the spinel surface, and the second reduction peak at a higher temperature (600 °C) could be assigned to the reduction of CoO to metallic cobalt species (Co0). Another noticeable peak at 700 °C might be due to the bulk Co-PT / 2026 / 12077

[0151] In-Al structure. On the other hand, the catalyst prepared without indium exhibits only two high-temperature reduction peaks that correspond to the reduction of bulk Co2+to CoO and further reduction into metallic cobalt. This concludes that the addition of indium in the catalyst enhances the surface cobalt species with a spinel structure that consequently improves the consumption of hydrogen.

[0152] The presence of surface acidic sites on both CIA-30 and CIA-0 catalysts was estimated through the NH3-TPD measurements. As depicted in Figure 3, CIA-0 exhibits two desorption peaks at 200 °C and 600 °C that could be speculated to the presence of weak and strong acidic sites, respectively. The origin of these weak and strong acidic sites could be related to the Al3+and surface hydroxyl groups, respectively. However, the presence of a relatively weak desorption peak located around 600 °C that corresponds to strong acidic sites for CIA-30 underpins the inclusion of indium, and suppresses the strong basic sites on the catalyst. Furthermore, the presence of Lewis acidic sites was also confirmed by the Pyridine-DRIFT analysis (Figure 4).

[0153] GENERAL PROCEDURE OF CO2 HYDROGENATION

[0154] The process of preparation of the value-added products by hydrogenating CO2 comprised finely grounded heterogenous catalyst was pelletized and sieved (0.8 mm) prior to loading. The catalyst (1 to 5g) was loaded in the reactor with suitable diluents and inert material selected from ceramic beats and silicon carbide (SiC). Before the reaction, the catalyst was reduced to a desired temperature (300-450 °C) for 2 hours. At a desired reaction temperature (200 - 3000 °C), both CO2 and H2 gases were fed into the reactor to start the reaction at a set pressure (10-40 bar).

[0155] EXAMPLE 3:

[0156] Hydrogenation of CO2 was carried out in a vertical downflow fixed bed reactor at different temperatures and pressures. The pelletized and sieved (size: 0.5-0.8 mm) catalyst was placed at the centre of the Inconel alloy reactor between two layers of ceramic beads and quartz wool. The catalyst was pre-reduced for 2 h at different temperatures, i.e. 400-600 °C, in the presence of H2 flow at high contact time, which is controlled by Brooks (5850S) make mass flow controller. After that, the reactor was cooled down to the desired reaction temperature in the presence of the same hydrogen flow. A suitable flow of CO2 and H2 was fedPT / 2026 / 12077

[0157] continuously from the high-precision Mass Flow Controllers (MFC) into the reactor to attain the target pressure. The initial reaction time was noted when the desired reaction conditions were achieved, and the outlet gas analysis was performed every hour.

[0158] The outlet gases were analysed online by a ThermoScientific Trace 1110 GC connected to TCD and FID. The non-condensable gasses (e.g., CFU and CO2) were detected and analysed by TCD. The hydrocarbons and liquid mixtures were analysed using the same GC connected to FID. The condensable liquid products (e.g., Methanol and water) were also confirmed and using HPLC using an H+ organic acid column with 0.005M H2SO4 as a mobile phase.

[0159] Conversion of CO2 (Xco2) and selectivity of products (Si) is based on the moles of carbon, which were calculated by the equation as follows:

[0160] CO2 Conversion

[0161] „ • ,[C02]in-[C02] out ,

[0162] Conversion (

[0163] v%)

[0164] 7= (

[0165] v- ; — - ) x 100 %

[0166] [C02] in7

[0167] Selectivity to the desired product

[0168] c i moles of desired product ,

[0169] Selectivity (%) = ( - ; — ; - — -£-- - ) x 100 %

[0170] total moles or products

[0171] This process of CO2 hydrogenation was experimental conducted with catalysts that are conventionally available as per prior art. The experimental data with the inventive catalysts and the comparative examples based on other catalysts represented in Table 1.

[0172] TABLE 3: Catalytic results of CO2 hydrogenation over various AiByCx-yOz catalysts as per the present invention and compared to catalytic results of CO2 hydrogenation over comparative catalyst examples:

[0173] s. Catalyst Catalyst Conversion Selectivity (%)

[0174] No code (%) Methanol Methane DME 1 CoInAlO CIA-20 7.2 73.1 21.2 5.7 2 CoInAlO CIA-25 18.8 94.8 1.6 3.5

[0175]

[0176] PT / 2026 / 12077

[0177] 3 CoInAlO CIA-30 21.2 97.2 0.6 2.2 4 CoInAlO CIA-35 13.4 89.8 5.5 4.4 5 CuInAlO CuIA-30 13.7 73.4 24.3 1.3 6 CoZrAlO CZA-30 16.1 76.3 19.7 1.0 7 CoInFeO CIF-30 12.3 72.7 18.9 0.8 8 CoGaAlO CGA-30 14.4 82.6 7.2 1.2 9 CoCeAlO CCA-25 11.2 67.5 32.4 0.7 10 Comparative CIA-0 32.6 2.3 97.3 0.4 example

[0178] CoAlO

[0179]

[0180] The CO2 hydrogenation results for different catalysts are given in Table 3. Under optimized conditions, CIA-25 catalyst exhibitsl8.8% CO2 conversion with 94.8% methanol selectivity. The best catalytic activity was achieved over the CIA-30 catalyst with 21.2% and of conversion, and 97.2% of selectivity towards methanol. The catalyst CIA-0 with only Co-Al (O) demonstrated a CO2 conversion of 32.6.% and notably the product selectivity was completely shifted towards methane (97.3%). This result indicates the reaction is more favour towards CH4 formation when indium is not present in the catalyst composition. Notably, DME is observed as a by-product for all catalysts which profoundly suggests the favour of dehydration due to the acidic sites present in the catalyst.

[0181] The CO2 hydrogenation performance of the CIA-30 catalyst was observed under different reaction temperatures. It showed the monotonous increment in the CO2 conversion concerning the elevated temperatures was observed; however, a drastic change in the product distribution was observed. Hence the parameters of the present process of CO2 hydrogentation favour mild conditions that is also thermodynamically favourable for the reaction.

[0182] The influence of reaction pressure on CO2 hydrogenation over the CIA-30 catalyst was analysed. The total reaction pressure was in direct correlation with the conversion. As the pressure increased that monotonous increment in the conversion from 14% to 25% was observed up to 50 bar pressure. While the product selectivity varied, methanol selectivity (>95%) was achieved at 30 bar pressure. The obtained results were in good correlation withPT / 2026 / 12077

[0183] the equilibrium conversion values reported recently. The studies have also concentrated for the CO2 hydrogenation reaction using deuterated hydrogen (D2) to produce methanol-d4, which is used as a solvent in nuclear magnetic resonance (NMR) spectroscopy and found diverse applications in various sectors. As shown in Figure 6, the CO2 hydrogenation using D2 as a hydrogen source also rendered almost similar results as H2 with more than 95% methanol selectivity up to 24 of the reaction streams.

[0184] The reaction was studied for a longer time on stream (TOS) under optimized conditions at different GHSVs. As depicted in Figure 7, the CIA-30 catalyst is extremely active for CO2 hydrogenation under all space velocities and renders more than 22% conversion as maximum. Worth noting that increasing the GHSV facilitated the reaction towards more methanol production as it reached 99% methanol selectivity at a GHSV of 6000 h1. Moreover, the obtained results conferred that the developed ternary mixed oxide catalysts are tremendously stable over 300 hours of TOS with sustained catalytic results. The XRD analysis of the spent catalyst (Figure 8) also demonstrated that there is no change in the catalyst phase even after 300 hours of the reaction, which further substantiated the stability of this catalyst and its significant candidature for industrial-scale methanol production. CIA-30 demonstrated catalytic performance with 21.2% CO2 conversion and more than 94.8% selectivity. On the other hand, CIA-25 exhibited 18.8% conversion with methanol selectivity of 97.2%.

[0185] EXAMPLE 4:

[0186] The estimated BET surface area for the CIA-0 is about 131.6 m2 / g, whereas the indium containing CIA-30 showed a slightly high surface area of about 142.3 m2 / g. The increment in the BET surface area for CIA-30 is due to the development of additional surface sites after indium loading. The HRTEM micrographs at different magnifications are shown in Figure 5, the prepared materials were found to have uniform morphology with undefined spherical clusters. As depicted from elemental mapping, the cobalt and indium oxides are highly dispersed crystalline phases which are also in great agreement with the XRD results.

[0187] The influence of different M2+and M3+cations in the AwByCx-yOzcatalysts during CO2 hydrogenation was evaluated under optimized reaction conditions. During the optimization of the catalyst composition the M2+(Cu, Co, Ni) and M3+(Al, Ga, Fe, Zr (IV)) were used for the study. Despite all the catalysts showing more than 10% CO2 conversion, the selectivity ofPT / 2026 / 12077

[0188] the methanol was achieved for CIA-X catalysts. The Table 1 presented that the product selectivity significantly varied with the change in the M2+and M3+metals in the catalyst composition under optimized reaction conditions. Among the tested catalysts, Co-In-Al (O) catalyst rendered the best catalytic results with excellent conversion of -19% and >97% selectivity towards methanol.

[0189] ADVANTAGES OF THE INVENTION

[0190] • The present invention provides highly stable methanol production (>300 hours) under mild reaction conditions (220 °C and 30 bar) with 95-97% methanol selectivity and DME selectivity (>40%) by altering the reaction conditions due to the introduction of novel heterogenous ternary catalysts for carbon dioxide hydrogenation.

[0191] • The catalysts of the present invention are simple, inexpensive, surface tunable and have highly reproducible heterogeneous catalyst synthesis methodology.

[0192] • The present invention is critical to create a carbon-neutral society, and the capture, compression, and conversion of industrially produced CO2, a potential greenhouse gas (GHG) into chemicals and feedstock is made possible due to the same.

[0193] • The present invention reduces the complications of stringent reaction parameters in conventional methanol production process and develop an efficient and robust ternary mixed oxide catalyst for enhanced production of methanol and methanol-derived products.

[0194] • The developed catalyst facilitates CO2 hydrogenation via a formate mechanism, bypassing the reverse water-gas shift (RWGS) route that typically demands elevated temperatures and pressures due to its higher energy barriers. In the formate pathway, CO2 is hydrogenated through direct interaction with the catalyst surface formates (HCOO*), enabling sequential hydrogenation steps to methanol at remarkably low temperatures and pressures. Moreover, the formate mechanism is inherently exothermic, releasing heat that thermodynamically favors the forward reaction under mild conditions, further enhancing catalyst efficiency and selectivity by minimizing energy input requirements and suppressing endothermic side pathways like RWGS. This kinetic advantage stems fromPT / 2026 / 12077

[0195] the catalyst's tailored active sites, which lower the activation energy for H2 dissociation and CO2 hydrogenation while suppressing CO production from RWGS, thus achieving high selectivity and turnover numbers under mild conditions.

[0196] • These insights delivered an efficient and durable catalyst for scalable CO2 to methanol processes, achieving benchmarked results with the space time yield (STY) of 389 gMeoH / kgcat / h.

Claims

PT / 2026 / 12077WE CLAIM:

1. A heterogeneous catalyst having Formula (I)(Aw ByCX-y)OzFormula (I)whereinA is a metal selected from d-block element;B is a metal selected from p-block element and inner transition element;C is a metal selected from p-block element and inner transition element;w is in the range of 0.5 to 1.5;x is in the range of 0.01 to 1;y is in the range of 0.01 to 1; andz is in the range of 1 to 4.

2. A heterogeneous catalyst having Formula (I)AlByCx-yOz,Formula (I)wherein:A is selected from Cu, Mn, Co, Ir, Zn, Pt, Pd, Rh, Ru, Mg and Sr;B and C are selected from Al, Ga, In, Ce, Zr, Nb, Ti, Si, Fe and P andwhere x= 0.01 to 1, y= 0.01 to 1 and z=l to 4.

3. The heterogenous catalyst as claimed in claim 1, wherein the surface of the catalyst has a higher number of weak acidic active sites as compared to strong acidic active sites.

4. The heterogenous catalyst as claimed in claim 1, wherein the catalyst has a crystalline spinel structure.

5. The heterogenous catalyst as claimed in claim 1, wherein particle size of heterogeneous catalyst is in the range of 10-14 nm.PT / 2026 / 120776. The heterogenous catalyst as claimed in claim 1, wherein the catalyst comprises the cation B ions dispersed in the crystalline phase.

7. The heterogenous catalyst as claimed in claim 1, wherein the molar ratio of A, B and C in the heterogeneous catalyst is in the range of 0.5: 0.15: 0.35 to 1.5: 0.45: 1.05.

8. The heterogenous catalyst as claimed in claim 1 is selected from a group comprising cobalt-indium-aluminium (CoInAlO), copper-indium-aluminium (CuInAlO), cobaltzirconium- aluminium (CoZrAlO), cobalt-indium-iron (CoInFeO), cobalt-gallium-aluminium (CoGaAlO), and cobalt-cerium-aluminium (CoCeAlO).

9. A process of preparation of the heterogeneous catalyst as claimed in claim 1, comprising the steps of:a. preparing and providing metal precursor solution comprising precursor of metal A, B and C;b. providing base solution comprising a base in water as solvent;c. co-precipitating and forming oxides of metals by dropwise adding and mixing the metals precursor solution of step (a) into step (b) to obtain precipitated material;d. aging the precipitated material of step (c), followed by washing, drying the precipitate to obtain dried precipitate ande. calcining the dried precipitate of step (d) to obtain the heterogeneous catalyst.

10. A process of CO2 hydrogenation in the presence of a heterogenous catalyst comprising the steps ofa) reducing the heterogeneous catalyst in a reactor; andb) treating and reacting CO2 and H2 supplied separately in said reactor to react and reduce the CO2 in presence of said reduced heterogeneous catalyst of step a);PT / 2026 / 12077wherein the heterogeneous catalyst is AiByCx.yOz,having A selected from Cu, Mn, Co, Ir, Ni, Zn, Pt, Ru, Mg and Sr; B and C selected from Al, Ga, In, Ce, Zr, Nb, Si and P and where x= 1 to 0.01, y= 0.01 to 1 and z=l to 4.

11. The process of CO2 hydrogenation as claimed in claim 9, wherein the temperature is in the range of 180-300 °C and a pressure in the range of 1-60 bar in step (b).