Cooling member production method
Thermal diffusion bonding with specific ratios and R-shaped joints addresses the complexity and cost issues in cooling member manufacturing, resulting in improved cooling performance and reduced manufacturing costs.
Patent Information
- Application Number
- PCT/JP2026/008516
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-03-05
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for manufacturing cooling members for heating elements, such as electronic components, are costly due to complex work processes and reduced cooling performance due to the use of bonding materials that act as heat transfer resistance.
A method involving thermal diffusion bonding to join a flow path forming member, a heat sink, and a heat conductive member, with specific surface area and thickness ratios, and R-shaped joints to improve manufacturing efficiency and cooling performance.
The method allows for low-cost production of cooling members with enhanced cooling performance and simplified manufacturing processes, reducing heat transfer resistance and enabling easier assembly of dissimilar metals.
Smart Images

Figure JP2026008516_12112026_PF_FP_ABST
Abstract
Description
Method for manufacturing cooling member
[0001] The present invention relates to the technical field of a method for manufacturing a cooling member that cools a heating element such as an electronic component.
[0002] Conventionally, techniques for methods of manufacturing cooling members that cool heating elements such as electronic components are publicly known. For example, as described in Patent Document 1.
[0003] Patent Document 1 discloses a water jacket (cooler) that forms a fluid flow path by a bottom portion and side walls provided upright on the bottom portion, and a heat sink (cooling fin base) that is joined to the side walls and has a plurality of fins formed on the flow path side, and discloses a water jacket type heat sink (cooling member) on which a heating element (power semiconductor device) is mounted on the surface of the heat sink opposite to the fins. Such a water jacket type heat sink can cool the heating element (power semiconductor device). Further, in such a water jacket type heat sink, a technique is known in which a heat spreader is provided between the heat sink and the heating element to improve heat dissipation performance.
[0004] Here, in the configuration described in Patent Document 1, the water jacket (cooler) and the heat sink (cooling fin base) are metal-bonded with a bonding material, and a brazing material such as solder or a sintered material containing metal particles is used as the bonding material.
[0005] In this way, when separate metal materials (for example, the water jacket and heat sink as described above, or the heat spreader and heat sink) are joined by a bonding material, the work process becomes complicated, which may increase the manufacturing cost of the cooling member. In addition, since the bonding material acts as resistance to heat transfer, the cooling performance of the cooling member may be reduced.
[0006] Japanese Unexamined Patent Application Publication No. 2017-5181
[0007] The present invention has been made in view of the circumstances as described above, and the problem to be solved is to provide a method for manufacturing a cooling member that can be manufactured at low cost and has improved cooling performance.
[0008] The problems that this invention aims to solve are as described above, and the means for solving these problems will now be explained.
[0009] That is, the present invention provides a method for manufacturing a cooling member, comprising: a flow path forming member that forms a fluid flow path with a bottom and side walls erected on the bottom; a heat sink joined to the side walls, separating the flow path from the outside of the flow path forming member, and having a plurality of fins on the flow path side; and a heat conductive member joined to an exposed portion of the heat sink that is exposed on the outside side of the flow path forming member, and in contact with a heating element, wherein the method for manufacturing a cooling member comprises a joining step of joining the flow path forming member, the heat sink, and the heat conductive member using thermal diffusion bonding.
[0010] Furthermore, the ratio of the total surface area A of the joint between the heat conductive member and the heat sink, the total surface area B of the joint between the heat sink and the side wall, and the total surface area C of the joint between the fin and the bottom is A:B:C = 1:0.5 to 5:0.5 to 5.
[0011] Furthermore, the ratio of the total area A to the total area C is A:C = 1:0.5 to 1.
[0012] Furthermore, the ratio of the thicknesses t1, t2, and t3 in the vertical direction of the side walls of the heat conductive member, the portion of the heat sink excluding the fins, and the bottom portion is t1:t2:t3 = 1:1 to 3:1 to 10.
[0013] Furthermore, the left-right width d of the side wall is set to 1 to 20 [mm].
[0014] Furthermore, the joint between the fin and the bottom portion is formed to have an R-shape.
[0015] The present invention provides the following effects:
[0016] The present invention provides a method for manufacturing a cooling member that can be produced inexpensively and improves cooling performance.
[0017] In the method for manufacturing a cooling member of the present invention, the flow path forming member, the heat sink, and the heat conducting member can be easily joined together.
[0018] In the method for manufacturing a cooling member of the present invention, the flow path forming member, the heat sink, and the heat conducting member can be joined together more easily.
[0019] In the method for manufacturing a cooling member of the present invention, the cooling performance of the cooling member can be further improved.
[0020] The present invention provides a method for manufacturing a cooling member that allows for greater freedom in determining the shape of the cooling member.
[0021] In the method for manufacturing the cooling member of the present invention, the strength of the joint between the fins and the bottom can be improved.
[0022] A front cross-sectional view showing a cooling member manufactured by a method for manufacturing a cooling member according to one embodiment of the present invention. A flowchart showing each step of the method for manufacturing a cooling member according to one embodiment of the present invention. (a) A front cross-sectional view showing the water jacket and heat sink after the first contact step. (b) A front cross-sectional view showing the water jacket, heat sink and copper spread after the second contact step. (a) A front cross-sectional view showing the state in which the copper spread and the heat sink, and the side wall of the water jacket and the heat sink are joined in the joining step. (b) A front cross-sectional view showing the state in which the bottom of the water jacket and the fins of the heat sink are further joined in the joining step.
[0023] In the following explanation, the directions indicated by arrows U, D, L, and R in the diagram will be defined as upward, downward, left, and right, respectively.
[0024] The following outlines the configuration of the cooling member 1 according to the first embodiment of the present invention, using Figure 1. The cooling member 1 is a water jacket type heat sink that cools a heat-generating element by circulating a fluid. The heat-generating element is, for example, an electronic component. In this embodiment, the cooling member 1 is formed to cool the electronic component E by circulating cooling water.
[0025] Figure 1 is a cross-sectional view of the cooling member 1, showing a cross-section perpendicular to the direction of cooling water flow. In the example, the cooling member 1 is shown such that the direction of cooling water flow is the depth direction of the paper. In the example, the left direction (left side of the paper) in the view of the cooling water flow direction is indicated as the left direction, and the right direction (right side of the paper) in the view of the cooling water flow direction is indicated as the right direction.
[0026] The cooling component 1 mainly comprises a water jacket 10, a heat sink 20, and a copper spreader 30.
[0027] The water jacket 10 forms a flow path P for the cooling water. The water jacket 10 is formed to extend along the direction of flow of the cooling water. The water jacket 10 is made of aluminum. The water jacket 10 has a bottom portion 11 and side walls 12.
[0028] The bottom portion 11 constitutes the lower part of the water jacket 10. The bottom portion 11 is formed in a plate shape with its plate surface oriented vertically.
[0029] The side walls 12 are formed to be erected at the left and right ends of the bottom portion 11. The side walls 12 are formed in a rectangular shape when viewed in a front cross-section. The left-right width d of each side wall 12 (the width of the side wall 12 in the left-right direction when viewed in the direction of extension of the flow path P (direction of cooling water flow)) is preferably set to 1 to 20 [mm].
[0030] The water jacket 10 configured in this way forms a fluid flow path P with its bottom portion 11 and side walls 12.
[0031] The heat sink 20 dissipates heat from the electronic component E. The heat sink 20, like the water jacket 10, is formed to extend along the direction of the cooling water flow. The heat sink 20 is made of aluminum. In this specification, "aluminum" includes aluminum and aluminum alloys. The heat sink 20 comprises a main body 21 and fins 22.
[0032] The main body portion 21 constitutes the main structure of the heat sink 20. The main body portion 21 is formed in a plate shape with its plate surface oriented vertically. The length of the main body portion 21 in the left-right direction is formed to be approximately the same as the length of the water jacket 10 in the left-right direction. The main body portion 21 is provided so that its lower surface is in contact with the upper surface of the side wall 12 of the water jacket 10, and is joined to the side wall 12 of the water jacket 10 using thermal diffusion bonding. By being joined to the side wall 12 of the water jacket 10, the main body portion 21 separates the flow path P from the outside of the water jacket 10.
[0033] An exposed surface 21a is formed on the main body portion 21. The exposed surface 21a is the upper surface of the main body portion 21 and is formed to be exposed to the outside side of the water jacket 10.
[0034] The fins 22 are formed to extend from the lower surface of the main body 21 toward the flow path P side (downward). Multiple fins 22 are provided at intervals in the left-right direction. The tips of the fins 22 are joined to the bottom 11 of the water jacket 10 using thermal diffusion bonding. The fins 22 configured in this way increase the surface area of the heat sink 20, thereby improving the heat dissipation effect.
[0035] The copper spreader 30 is a heat dissipation spreader that dissipates heat from the electronic component E. The copper spreader 30 is formed in a plate shape with its plate surface oriented vertically. The copper spreader 30 is made of copper. In this specification, the term "copper" includes copper and copper alloys. The copper spreader 30 is provided so that its lower surface is in contact with the exposed surface 21a of the heat sink 20, and is joined to the exposed surface 21a using thermal diffusion bonding. The copper spreader 30 is positioned in the left-right center of the main body 21 of the heat sink 20.
[0036] As described above, the water jacket 10, heat sink 20, and copper spreader 30 are not all made of the same metal material, but are made of two different metal materials: aluminum and copper. The water jacket 10, heat sink 20, and copper spreader 30 are joined together using thermal diffusion bonding.
[0037] Next, a method for manufacturing the cooling member 1 according to one embodiment of the present invention will be described using Figures 2 to 4. Note that the joints of each member (the first joint 40, the second joint 50, and the third joint 60, which will be described later) do not actually have thickness, but are shown as having thickness in order to clearly indicate the position of each joint.
[0038] First, the first contact step S1 shown in Figure 2 is performed. The first contact step is the process of bringing the heat sink 20 into contact with the side wall 12 of the water jacket 10 with the multiple fins 22 spaced apart from the bottom 11 of the water jacket 10. As shown in Figure 3(a), in the first contact step, the heat sink 20 is placed on the side wall 12 of the water jacket 10 with the surface on which the fins 22 are provided facing downwards. The component dimensions (mm) of the water jacket 10 and heat sink 20 before joining are set to satisfy the following equation 1.
[0039] a - b > X 1 ...(Formula 1)
[0040] In Equation 1, "a" represents the height (length in the vertical direction) of the side wall 12 of the water jacket 10 before joining from the bottom 11 [mm]. "b" represents the height (length of the fin 22 in the vertical direction of the side wall 12) of the fin 22 of the heat sink 20 before joining from the main body 21 [mm]. 1 This value is a predetermined positive value, preferably greater than 0 [mm] and set to any value less than or equal to 0.1 [mm].
[0041] In this way, before joining, the height a of the side wall 12 is set to be greater than the height b of the fin 22 (satisfying equation 1), so that, as shown in Figure 3(a), when the heat sink 20 is in contact with the side wall 12, the fin 22 and the bottom 11 do not come into contact, and there is a gap between the fin 22 and the bottom 11. The value of "a-b" is set to a value that satisfies the conditions of equation 1 and allows the fin 22 and the bottom 11 to be joined in the joining process described later.
[0042] Next, the second contact step of step S2 is performed. The second contact step is a step of bringing the copper spreader 30 into contact with the exposed surface 21a of the heat sink 20. As shown in FIG. 3(b), in the second contact step, the copper spreader 30 is placed at the left-right center of the exposed surface 21a of the heat sink 20. The second contact step (step S2) may be performed before the first contact step (step S1), or may be performed simultaneously with the first contact step (step S1).
[0043] Here, the respective thicknesses (thicknesses in the direction in which the side walls 12 are erected) t1, t2 and t3 of the copper spreader 30, the main body portion 21 of the heat sink 20, and the bottom portion 11 of the water jacket 10 are set so as to satisfy the following formula 2.
[0044] t1:t2:t3=1:1 to 3:1 to 10 (Formula 2)
[0045] Next, the bonding step of step S3 is performed. The bonding step is a step of bonding the water jacket 10, the heat sink 20 and the copper spreader 30 to each other by thermal diffusion bonding after the first contact step (step S1) and the second contact step (step S2) are performed. In the bonding step, the water jacket 10, the heat sink 20 and the copper spreader 30 arranged by the first contact step (step S1) and the second contact step (step S2) are heated and pressurized to perform thermal diffusion bonding at the same time. More specifically, in thermal diffusion bonding, a load is applied so that the bonding surfaces are brought into close contact with each other while the bonding surfaces are heated. The applied heat and load are set to appropriate values according to the material, size and the like of each member.
[0046] Thereby, as shown in FIG. 4(a), the lower surface of the copper spreader 30 and the exposed surface 21a of the heat sink 20 are bonded by thermal diffusion. Hereinafter, the bonding portion between the lower surface of the copper spreader 30 and the exposed surface 21a of the heat sink 20 is referred to as a first bonding portion 40.
[0047] Further, as shown in FIG. 4(a), the lower surface of the heat sink 20 and the upper surface of the side wall 12 of the water jacket 10 are bonded by thermal diffusion. Hereinafter, the bonding portion between the lower surface of the heat sink 20 and the upper surface of each side wall 12 of the water jacket 10 is referred to as a second bonding portion 50.
[0048] As described above, before the formation of the second joint 50, the height a of the side wall 12 is set to be greater than the height b of the fin 22, and the fin 22 and the bottom 11 are separated. On the other hand, as the second joint 50 is formed, the lower surface of the heat sink 20 and the upper surface of the side wall 12 of the water jacket 10 deform. As a result, the lower surface of the fin 22 of the heat sink 20 and the upper surface of the bottom 11 of the water jacket 10 come into contact.
[0049] Therefore, as the fins 22 of the heat sink 20 and the bottom 11 of the water jacket 10 are heated and pressurized, the lower surface of the fins 22 and the upper surface of the bottom 11 are thermally diffusively bonded, as shown in Figure 4(b). Hereinafter, the joint between the lower surface of each fin 22 of the heat sink 20 and the upper surface of the bottom 11 of the water jacket 10 will be referred to as the third joint 60.
[0050] In the cooling member 1 configured in this way, the ratio of the area of the joints of each member is set to satisfy the following equation 3.
[0051] A:B:C=1:0.5~5:0.5~5...(Formula 3)
[0052] In Equation 3, "A" represents the area of the first joint 40 (the joint surface between the copper spreader 30 and the main body 21 of the heat sink 20). If multiple first joints 40 are formed, "A" represents the sum of the areas of each first joint 40 (total area). "B" represents the sum of the areas of each second joint 50 (the joint surface between the main body 21 of the heat sink 20 and each side wall 12 of the water jacket 10). "C" represents the sum of the areas of each third joint 60 (the joint surface between each fin 22 of the heat sink 20 and the bottom 11 of the water jacket 10).
[0053] More preferably, the ratio of the total area A of the first joint 40 to the total area C of the third joint 60 is set to satisfy the following equation 4.
[0054] A:C=1:0.5~1...(Formula 4)
[0055] Furthermore, more preferably, the total area C of the third joint 60 and the total area B of the second joint 50 are set to satisfy the following formula 5.
[0056] (C / 2)<B<(C×2)...(Formula 5)
[0057] In this way, the copper spreader 30 and the main body 21 of the heat sink 20, the main body 21 of the heat sink 20 and the side wall 12 of the water jacket 10, and the fins 22 of the heat sink 20 and the bottom 11 of the water jacket 10 are joined using thermal diffusion bonding, thereby enabling the manufacture of the cooling member 1 shown in Figure 1.
[0058] In the cooling member 1 manufactured in this manner, the joint portion (orthogonal portion) between the fin 22 and the bottom portion 11 is formed to have an R shape (see a partially enlarged view of Figure 1). This improves the strength of the joint between the fin 22 and the bottom portion 11.
[0059] As described above, in the manufacturing method of the cooling member 1 according to this embodiment, even when the number of parts to be joined (joining locations) is relatively large, each joining location can be joined at once by thermal diffusion bonding, thus simplifying the joining process. Furthermore, the cooling member 1 can be manufactured at a lower cost than when brazing, welding, or adhesive bonding is used as the joining method. In addition, compared to brazing, welding, and adhesive bonding, resistance to heat transfer can be reduced, and cooling performance can be improved.
[0060] Furthermore, since the main body 21 of the heat sink 20 and the side wall 12 of the water jacket 10 are joined using thermal diffusion bonding, the left-right width d of the side wall 12 can be made smaller (for example, 1 to 20 mm) compared to the case where the main body 21 and the side wall 12 are bolted together. Therefore, the degree of freedom in the shape of the cooling member 1 can be improved. In addition, the width of the flow path P can be made larger, and consequently, the cooling performance can be improved.
[0061] Furthermore, in the manufacturing method of the cooling member 1 according to this embodiment, the contact process (first contact process and second contact process) is completed when the heat sink 20 is in contact with the side wall 12 of the water jacket 10 and the fins 22 are separated from the bottom 11 of the water jacket 10. After that, the water jacket 10, heat sink 20, and copper spreader 30 that were positioned in the contact process are heated and pressurized to start thermal diffusion bonding. Due to the pressurization, the side wall 12 of the water jacket 10 contracts appropriately, and the separated fins 22 and the bottom 11 of the water jacket 10 come into contact. As a result, excessive force is suppressed on the fins 22 during bonding, and contact is made, allowing for thermal diffusion bonding, and consequently, deformation or damage to the fins 22 can be suppressed.
[0062] Furthermore, in the manufacturing method of the cooling member 1 according to this embodiment, since thermal diffusion bonding is used to join each member, dissimilar metals can be easily joined. Also, the water jacket 10 and the heat sink 20 come into contact not only with the side wall 12 and the main body 21, but also with the bottom 11 and the fins 22 during the joining process. This suppresses the occurrence of deformation of the entire cooling member 1 due to heating and pressurization. Moreover, by adjusting the total area C of the third joint 60 and the total area B of the second joint 50 to satisfy "(C / 2) < B < (C × 2)", deformation of the entire cooling member 1 due to heating and pressurization can be further suppressed.
[0063] Furthermore, the thicknesses t1, t2, and t3 of the copper spreader 30, the main body 21 of the heat sink 20, and the bottom 11 of the water jacket 10 are set to t1:t2:t3 = 1:1 to 3:1 to 10. By setting the ratio of each thickness t1, t2, and t3 in this way, the cooling performance can be improved.
[0064] Furthermore, the ratio of the total area A of the first joint 40, the total area B of the second joint 50, and the total area C of the third joint 60 is set to A:B:C = 1:0.5 to 5:0.5 to 5, preferably A:C = 1:0.5 to 1. By setting the ratio of the total areas A, B, and C in this way, it is possible to make it easier to join the water jacket 10, the heat sink 20, and the copper spreader 30. In addition, it is possible to further suppress the occurrence of deformation of the entire cooling member 1 due to heating and pressurization.
[0065] As described above, the method for manufacturing the cooling member 1 according to this embodiment is a method for manufacturing the cooling member 1 comprising: a water jacket 10 (flow channel forming member) that forms a fluid flow channel P with a bottom portion 11 and a side wall 12 erected on the bottom portion 11; a heat sink 20 that is joined to the side wall 12, demarcates the flow channel P from the outside of the water jacket 10, and has a plurality of fins 22 on the flow channel P side; and a copper spreader 30 (heat conducting member) that is joined to an exposed surface 21a (exposed portion) of the heat sink 20 that is exposed to the outside of the water jacket 10, and to which an electronic component E (heating element) is in contact; and the method for manufacturing the cooling member 1 comprises a joining step (step S3 in Figure 2) in which the water jacket 10, the heat sink 20, and the copper spreader 30 are joined using thermal diffusion bonding.
[0066] By configuring the components in this way, the water jacket 10, heat sink 20, and copper spreader 30 are joined to each other by thermal diffusion bonding. This simplifies the manufacturing process compared to joining components using solder or other brazing materials, or sintered materials containing metal particles, and consequently reduces manufacturing costs. Furthermore, because the components are joined by thermal diffusion bonding, the resistance to heat transfer is reduced compared to joining components using the aforementioned materials. In other words, the cooling component 1 can be manufactured at a low cost, and its cooling performance can be improved.
[0067] Furthermore, the ratio of the total surface area A of the joint between the copper spreader 30 and the heat sink 20, the total surface area B of the joint between the heat sink 20 and the side wall 12, and the total surface area C of the joint between the fin 22 and the bottom portion 11 is A:B:C = 1:0.5 to 5:0.5 to 5.
[0068] This configuration makes it easier to join the water jacket 10, heat sink 20, and copper spreader 30. This simplifies the manufacturing process and, consequently, allows the cooling component 1 to be manufactured at a lower cost.
[0069] Furthermore, the ratio of the total area A to the total area C is A:C = 1:0.5 to 1.
[0070] This configuration makes it easier to join the water jacket 10, heat sink 20, and copper spreader 30. This simplifies the manufacturing process and, consequently, allows the cooling component 1 to be manufactured at a lower cost.
[0071] Furthermore, the ratio of the thicknesses t1, t2, and t3 of the side walls 12 in the vertical direction for the copper spreader 30, the main body 21 (the portion of the heat sink 20 excluding the fins 22), and the bottom portion 11 is t1:t2:t3 = 1:1 to 3:1 to 10.
[0072] By configuring it in this way, the cooling performance of the cooling component 1 can be further improved.
[0073] Furthermore, the width d of the side walls in the left-right direction when viewed in the direction of extension of the flow path P is 1 to 20 [mm].
[0074] This configuration allows for greater flexibility in the shape of the cooling element 1.
[0075] Furthermore, the joint between the fin 22 and the bottom portion 11 (third joint portion 60) is formed to have an R shape.
[0076] This configuration improves the strength of the joint between the fin 22 and the bottom portion 11.
[0077] Although embodiments of the present invention have been described above, the present invention is not limited to the above configuration, and various modifications are possible within the scope of the invention as described in the claims.
[0078] For example, in this embodiment, the side wall 12 is provided on the water jacket 10, but it may also be provided on the heat sink 20.
[0079] Furthermore, in this embodiment, all fins 22 are in contact with and joined to the bottom 11, but it is also possible that only a portion of the fins 22 are in contact with and joined to the bottom 11.
[0080] Furthermore, the metal materials constituting the water jacket 10, heat sink 20, and copper spreader 30 are not limited to those of this embodiment, and other metal materials may be used. Also, the metal materials constituting the water jacket 10, heat sink 20, and copper spreader 30 may consist of three different types (i.e., each may be made of a different metal material).
[0081] This invention can be applied to the technology of a method for manufacturing a cooling member for cooling heat-generating elements such as electronic components.
[0082] 1 Cooling component 10 Water jacket 11 Bottom 12 Side wall 20 Heat sink 21a Exposed surface 22 Fin 30 Copper spreader
Claims
1. A method for manufacturing a cooling member comprising: a flow path forming member that forms a fluid flow path by a bottom and a side wall erected on the bottom; a heat sink joined to the side wall, separating the flow path from the outside of the flow path forming member, and having a plurality of fins on the flow path side; and a heat conductive member joined to an exposed portion of the heat sink that is exposed on the outside side of the flow path forming member, and in contact with a heating element, the method comprising a joining step of joining the flow path forming member, the heat sink, and the heat conductive member using thermal diffusion bonding.
2. The method for manufacturing a cooling member according to claim 1, wherein the ratio of the total area A of the joint surfaces between the heat conductive member and the heat sink, the total area B of the joint surfaces between the heat sink and the side wall, and the total area C of the joint surfaces between the fin and the bottom is A:B:C = 1:0.5 to 5:0.5 to 5.
3. The method for manufacturing a cooling member according to claim 2, wherein the ratio of the total area A to the total area C is A:C = 1:0.5 to 1.
4. The method for manufacturing a cooling member according to claim 1, wherein the ratio of the thicknesses t1, t2, and t3 in the vertical direction of the side wall of the heat conductive member, the portion of the heat sink excluding the fins, and the bottom portion is t1:t2:t3 = 1:1 to 3:1 to 10.
5. The left-right width d of the side wall is set to 1 to 20 [mm], the method for manufacturing a cooling member according to any one of claims 1 to 4.