Method for separating and recovering rare earth element
By forming rare earth carbonates and using electrolysis with molten salts, the method simplifies the recovery of praseodymium and neodymium from alloys, addressing the complexity of existing methods and enhancing efficiency.
Patent Information
- Application Number
- PCT/JP2026/010201
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-03-16
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for recovering rare earth elements from alloys with nickel require additional steps to separate the rare earth elements, increasing complexity and cost.
A method involving contacting a rare earth element-containing material with an acid medium to form a rare earth carbonate, followed by electrolysis using a molten salt containing alkali or alkaline earth metal carbonates to precipitate praseodymium and neodymium as metals.
Enables direct deposition of rare earth elements as metals on an electrode, simplifying the recovery process and reducing the need for additional separation steps.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Methods for separating and recovering rare earth elements
[0001] This invention relates to a method for separating and recovering rare earth elements.
[0002] Rare earth elements are indispensable for improving the performance and efficiency of high-tech products. For example, rare earth magnets (such as neodymium (Nd) magnets), which are powerful permanent magnets, are used in electric vehicles, wind turbine motors, and computer hard disk drives, enabling improved energy efficiency and miniaturization for high performance. In recent years, the demand for rare earth elements has increased with the proliferation of these high-tech products. However, rare earth elements are produced in limited locations, their output is low, and their prices are soaring. Therefore, there is a need to develop and improve technologies for separating and recovering rare earth elements from discarded high-tech products.
[0003] One such technology involves recovering rare earth elements from molten salts containing them by electrolytic extraction. For example, Japanese Patent Publication No. 6234160 discloses a method for separating and obtaining rare earth elements from a treatment material containing iron and one or more rare earth elements by molten salt electrolysis. The method comprises the steps of: adding and dissolving metal A, which is more noble than the rare earth elements contained in the treatment material, to a molten salt; providing a cathode electrode and an anode electrode made of the treatment material to the molten salt containing dissolved metal A, and performing electrolysis to dissolve at least the iron and one or more rare earth elements from the constituent elements of the treatment material into the molten salt; providing a pair of electrodes in the molten salt containing dissolved metal A and at least the iron and one or more rare earth elements from the constituent elements of the treatment material, and controlling the potential of the cathode electrode so that both the metal ions of metal A dissolved in the molten salt and the iron ions dissolved from the treatment material precipitate or alloy simultaneously or separately, thereby recovering the metal ions of metal A and the iron ions dissolved from the treatment material from the molten salt; and providing a pair of electrodes in the molten salt and applying a voltage between the electrodes to generate a potential difference, thereby precipitating or alloying the rare earth elements derived from the treatment material dissolved in the molten salt onto the surface of one of the electrodes. According to the document, the above configuration makes it possible to provide a method for producing rare earth metals that separates each rare earth element from a processing material such as a rare earth magnet with high purity through easy operation.
[0004] However, the technology described in the above-mentioned literature uses a nickel electrode as the cathode and recovers the target rare earth element in the form of an alloy with nickel (Ni) (for example, an alloy of dysprosium (Dy) and Ni, or an alloy of Nd, praseodymium (Pr), and Ni). Therefore, in order to reuse the rare earth element, an additional step was required to separate the rare earth element from Ni in the above alloy.
[0005] Therefore, the object of the present invention is to provide a method for separating and recovering rare earth elements using electrolytic deposition, which allows at least one of the rare earth elements to be deposited as a metal on an electrode.
[0006] The inventors diligently studied to solve the above problems. As a result, they found that the above problems can be solved by contacting a rare earth element-containing material with an acid medium to dissolve the rare earth element into the acid medium, then forming a rare earth carbonate via a double sulfate containing the rare earth element, and then performing electrolysis using a molten salt containing the rare earth carbonate and at least one alkali metal carbonate or alkaline earth metal carbonate, thus completing the present invention.
[0007] In other words, a method for separating and recovering rare earth elements according to one embodiment of the present invention relates to a method for separating and recovering rare earth elements from a rare earth element-containing material containing at least one selected from the group consisting of praseodymium and neodymium. The method comprises: contacting the rare earth element-containing material with an acidic medium to obtain an eluate containing rare earth ions; adding an alkali metal sulfate to the eluate to obtain a double salt of rare earth ions, alkali metal ions, and sulfate ions; adding the double salt to an aqueous solution containing carbonate ions and alkali metal ions to obtain a rare earth carbonate; and precipitating at least one selected from the group consisting of praseodymium and neodymium as a metal from a molten salt containing the rare earth carbonate and at least one selected from the group consisting of alkali metal carbonates and alkaline earth metal carbonates by electrolysis.
[0008] Figure 1 shows the XPS spectrum of the electrodeposit obtained in Example 1. Figure 2 shows the XPS spectrum of the electrodeposit obtained in Example 5.
[0009] The embodiments of the present invention will be described below, but the technical scope of the present invention should be determined based on the claims and is not limited to the following forms. Note that "X to Y" indicating the range means "X or more and Y or less".
[0010] One embodiment of the present invention is a method for separating and recovering rare earth elements from a rare earth element-containing material containing at least one selected from the group consisting of praseodymium and neodymium, comprising: contacting the rare earth element-containing material with an acidic medium to obtain an eluate containing rare earth ions (hereinafter also referred to as the "acid elution step"); adding an alkali metal sulfate to the eluate to obtain a double salt of rare earth ions, alkali metal ions, and sulfate ions (hereinafter also referred to as the "sulfate double salt" step) (hereinafter also referred to as the "sulfate double salt production step"); adding the double salt to an aqueous solution containing carbonate ions and alkali metal ions to obtain a rare earth carbonate (hereinafter also referred to as the "carbonate production step"); and precipitating at least one selected from the group consisting of praseodymium and neodymium as a metal from a molten salt of the rare earth carbonate and at least one selected from the group consisting of alkali metal carbonates and alkaline earth metal carbonates by electrolysis (hereinafter also referred to as the "electrolysis extraction step"). According to this embodiment, in a method for separating and recovering rare earth elements using electrolytic deposition, at least one of the rare earth elements can be deposited as a metal on the electrode. In this specification, "depositing at least one selected from the group consisting of praseodymium and neodymium as a metal" includes the form in which praseodymium metal is deposited; the form in which neodymium metal is deposited; and the form in which a mixture consisting of praseodymium metal and neodymium metal is deposited.
[0011] The following describes in detail each step of the method for separating and recovering rare earth elements according to this embodiment.
[0012] <Acid Elution Process> In this process, the rare earth element-containing material is brought into contact with an acid medium to obtain an eluate containing rare earth ions.
[0013] [Rare Earth Element-Containing Material] The rare earth element-containing material contains at least one selected from the group consisting of praseodymium (Pr) and neodymium (Nd). The rare earth element-containing material may further contain one or more rare earth elements other than praseodymium and neodymium (i.e., scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu)). In one preferred embodiment, the rare earth element-containing material contains at least Pr and Nd, more preferably at least Pr, Nd, Tb, and Dy, and even more preferably Pr, Nd, Tb, and Dy.
[0014] The rare earth element-containing material may also contain elements other than rare earth elements. According to the separation and recovery method of this embodiment, even if the rare earth element-containing material contains elements other than rare earth elements, most of these elements can be removed in the acid elution step, the sulfate double salt formation step, and / or the carbonate formation step. Examples of elements other than rare earth elements include, but are not limited to, iron (Fe), cobalt (Co), nickel (Ni), boron (B), copper (Cu), sodium (Na), manganese (Mn), aluminum (Al), silicon (Si), and sulfur (S).
[0015] The rare earth element-containing material is preferably a rare earth magnet (including sludge generated during its production) that is rich in rare earth elements. The rare earth magnet is not particularly limited as long as it is a magnet using an alloy containing one or more rare earth elements. Specific examples of rare earth magnets include neodymium magnets, samarium-cobalt magnets, praseodymium magnets, and samarium-iron-nitrogen magnets. Among these, neodymium magnets or praseodymium magnets are preferred, and neodymium magnets are more preferred. Neodymium magnets using rare metals such as rare earth elements (e.g., Pr, Nd, Tb, Dy) are used in the drive and power generation motors of environmentally friendly electric vehicles (EVs) and hybrid electric vehicles (HEVs). Given the procurement risks associated with rare earth elements and the expected increase in demand for environmentally friendly vehicles in Japan, a country poor in natural resources, recycling rare earth elements from neodymium magnets is crucial. Recycling rare earth elements from neodymium magnets is advantageous because it reduces the procurement risks associated with rare earth elements. Typically, neodymium magnets are defined as rare-earth magnets whose main components are neodymium, iron, and boron. However, in this specification, neodymium magnets are defined as magnets of an R-T-B alloy having R, T, and B (wherein R must include at least one selected from the group consisting of Pr, Nd, Tb, and Dy; T is a transition metal in which Fe is essential; and B is boron, which can be partially substituted with carbon or nitrogen).
[0016] Rare earth element-containing materials can include products made using materials containing rare earth elements, waste products or semi-finished products, scraps and defective products generated during the manufacturing process, and intermediates obtained during the recycling of these materials. Furthermore, the form in which rare earth elements exist in rare earth element-containing materials is not particularly limited and can take various forms such as metals, alloys, oxides, salts, and combinations thereof. If elements other than rare earth elements are included in rare earth element-containing materials, the form in which those elements exist is also not particularly limited and can take various forms such as metals, alloys, oxides, salts, and combinations thereof.
[0017] When the rare earth element-containing material contains a transition metal (e.g., Fe, Co, Ni, Cu, Mn) as an element other than the rare earth element, it is preferable that at least a part of the transition metal is contained in the rare earth element-containing material in the form of a transition metal oxide. By adopting the form of transition metal oxide, elution of the transition metal can be suppressed in the acid elution step, and the transition metal contained in the rare earth element-containing material can be separated. From the viewpoint of improving the separation efficiency of the transition metal, it is preferable that more of the transition metal contained in the rare earth element-containing material is in the form of a transition metal oxide. Specifically, the ratio of the substance amount of the transition metal in the form of an oxide to the substance amount of the transition metal contained in the rare earth element-containing material is preferably 50 to 100%, more preferably 75 to 100%, and preferably 90 to 100%. In particular, when the rare earth element-containing material contains a large amount of Fe like a neodymium magnet, Fe is Fe 2 O 3 is preferably contained in the rare earth element-containing material. Fe 2 O 3 is sparingly soluble in an acid medium, so that Fe contained in the rare earth element-containing material can be separated in this step. That is, according to a preferred embodiment of the present invention, the rare earth element-containing material contains iron, and at least a part of the iron (preferably 50 to 100%, more preferably 75 to 100%, further preferably 90 to 100%) is Fe 2 O 3 . When iron is in the form of Fe 3 O 4 , when the rare earth element-containing material is brought into contact with an acid medium, iron can be eluted mainly in the form of Fe 3+ by the following elution reaction.
[0018]
[0019] When a substance containing a transition metal (particularly Fe) in a non-oxide form is subjected to the separation and recovery method according to the present embodiment, it is preferable to subject the substance to an oxidation treatment in advance and use the obtained oxidized product as the rare earth element-containing material according to the present embodiment. The oxidation treatment method converts a non-oxide transition metal (particularly Fe) into a transition metal oxide (particularly Fe 2 O 3While there are no particular restrictions as long as the material can be converted to (a), a method of heating at a high temperature in an oxygen-containing gas atmosphere (e.g., in air) (oxidative roasting) is preferred because it is simple. Note that if a substance containing transition metals (especially Fe) in a non-oxide form is brought into direct contact with an acid medium, the transition metal may leach out, and the composition of the transition metal in the eluate may increase. Even in such cases, since much of the transition metal (especially Fe) remains in the eluate during the sulfate double salt production process described later, separation of rare earth elements and transition metals can be sufficiently achieved.
[0020] [Acid medium] The acid medium is not particularly limited as long as it can dissolve rare earth elements from the rare earth element-containing material, but it is preferable that it contains a strong acid. Examples of strong acids include hydrochloric acid (HCl) and nitric acid (HNO). 3 ), sulfuric acid (H 2 SO 4 ), perchloric acid (HClO 4 Examples include hydrobromic acid (HBr) and hydroiodic acid (HI). Among these, hydrochloric acid, nitric acid, and sulfuric acid are preferred, with hydrochloric acid being more preferred.
[0021] The elution reaction of rare earth elements proceeds according to the following reaction equation.
[0022]
[0023] The elution status of rare earth elements and their separation from transition metals can be determined from the pH and ORP (oxidation-reduction potential) of the eluate and the Pourbaix Diagram. For example, if the pH and ORP of the eluate after elution are pH = 1.00 and ORP = 606.7 mV vs. Ag / AgCl, then in the Pourbaix Diagram, Fe 2 O 3 , Nd 3+ Since this is within the specified region, it can be confirmed that rare earth elements are selectively eluted.
[0024] When hydrochloric acid is used as the acid medium, the concentration of hydrochloric acid is not particularly limited as long as the Fe-based compound does not hinder solid-liquid separation after elution, but is preferably 3.0 mol / L or less, more preferably 1.5 mol / L or less, even more preferably 1.2 mol / L or less, particularly preferably 0.1 to 1.2 mol / L, and most preferably 0.5 to 1.2 mol / L. In particular, when the rare earth element-containing material contains a large amount of boron (B), by setting the concentration of hydrochloric acid to 1.2 mol / L or less, B 2 O 3 By crystallizing it, the elution of B can be suppressed. Also, B 2 O 3 By utilizing the temperature dependence of solubility, for example, by performing filtration at a temperature below room temperature, B 2 O 3 Because it recrystallizes, the amount of B that elutes can be further suppressed. In this way, B 2 O 3 By crystallizing and separating the components, the viscosity of the eluate can be reduced, thereby minimizing the impact on the subsequent precipitation and separation reaction. As a result, B can be separated by this process. The volume of the acid medium is not particularly limited as long as the pH and ORP of the eluate change according to the weight of the rare earth element-containing material, as long as the pH and ORP that selectively leach the rare earth elements mentioned above can be maintained. However, it is preferably 5 to 100 mL per gram of rare earth element-containing material, and more preferably 10 to 50 mL.
[0025] By contacting a rare earth element-containing material with an acid medium, the rare earth elements contained in the material are ionized and eluted into the acid medium. Contact between the rare earth element-containing material and the acid medium can be carried out preferably at a temperature of 10 to 90°C, more preferably 25 to 80°C, for 1 to 48 hours, more preferably 6 to 24 hours. To promote the elution of rare earth elements, the mixture of the rare earth element-containing material and the acid medium may be stirred as needed. Furthermore, if the concentration of rare earth elements in the eluate is dilute, or if the concentration of transition metals is significantly high, the elution process may be repeated until the pH and ORP range described above is reached.
[0026] <Sulfate Double Salt Formation Process> In this process, alkali metal sulfates are added to the eluate obtained in the above acid elution process to obtain a double salt of rare earth ions, alkali metal ions, and sulfate ions.
[0027] [Alkali metal sulfates] Examples of alkali metal sulfates include lithium sulfate (Li 2 SO 4 ), sodium sulfate (Na 2 SO 4 ), potassium sulfate (K 2 SO 4 ), rubidium sulfate (Rb 2 SO 4 ), cesium sulfate (Cs 2 SO 4 ) are some examples. Among them, sodium sulfate (Na 2 SO 4 ), potassium sulfate (K 2 SO 4 ) is preferred, and sodium sulfate (Na 2 SO 4 ) is preferable.
[0028] Rare earth elements form double salts with alkali metal sulfates through the following reaction. This reaction system requires a considerable amount of time to reach equilibrium. Therefore, based on Le Chatelier's principle, alkali metal sulfates (e.g., Na) 2 SO 4 Increasing the amount of added ) promotes the chemical equilibrium of the forward reaction (to the right).
[0029]
[0030] The amount of alkali metal sulfate added is not particularly limited, as long as it is at least the stoichiometric amount relative to the amount of rare earth elements contained in the eluate (i.e., 2.0 moles or more per 1.0 mole of rare earth elements (Ln)). From the viewpoint of improving the recovery rate of double sulfates, the ratio of the amount of alkali metal sulfate to the amount of rare earth elements contained in the eluate is preferably 6.0 to 14.0, more preferably 6.0 to 12.0, even more preferably 8.0 to 12.0, and particularly preferably 10.0 to 12.0. The amount of rare earth elements contained in the eluate can be determined by performing ICP-AES analysis on the eluate.
[0031] When alkali metal sulfates are added to the eluate, double salts are formed of rare earth ions, alkali metal ions, and sulfate ions. The resulting double sulfates may be in the form of hydrates (double sulfate hydrates). In the above double sulfate formation reaction, increasing the temperature can accelerate the chemical equilibrium of the forward reaction (rightward). The double sulfate formation reaction can be carried out at a temperature of preferably 10 to 90°C, more preferably 25 to 80°C, for preferably 1 to 48 hours, more preferably 6 to 24 hours. To promote the elution of rare earth elements, the mixture of the rare earth element-containing material and the acid medium may be stirred as needed. Since the double sulfates precipitate in the reaction solution, they can be recovered by solid-liquid separation (e.g., centrifugation, filtration, etc.).
[0032] This process allows for the separation of elements contained in the eluate by utilizing the differences in the ease with which each element forms double sulfate salts. More specifically, rare earth elements form double sulfate salts more readily than other elements. Furthermore, since Fe remains in the solution as a highly soluble sulfate, the elemental composition of the double sulfate salt can be richer in rare earth elements compared to the elemental composition of the rare earth element-containing material. In addition, among the rare earth elements, the double sulfate salts of light rare earth elements (La, Ce, Pr, Nd, Pm, Sm, Eu) are sparingly soluble, while the double sulfate salts of heavy rare earth elements (Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu) are highly soluble, making it easier to form double sulfate salts of light rare earth elements. Therefore, the composition of rare earth elements contained in the double sulfate salt can be richer in light rare earth elements compared to the composition of rare earth elements contained in the rare earth element-containing material.
[0033] Furthermore, in order to further separate light rare earth elements from heavy rare earth elements, it is also preferable to perform multi-stage extraction using an acidic extractant or a solvating extractant on the solid component (double sulfate) or liquid component obtained in the double sulfate production step. Multi-stage extraction refers to a method of extraction in which new aqueous or organic phases are added step by step until the components to be extracted are sufficiently separated. By using multi-stage extraction, the target components can be separated with high efficiency, and as a result, the recovery rate of rare earth elements in the electrolytic extraction step can be further improved.
[0034] <Carbonate Production Process> In this process, the sulfate double salt obtained in the sulfate double salt production process described above is added to an aqueous solution containing carbonate ions and alkali metal ions to obtain rare earth carbonates through the following reaction. If the reaction does not proceed smoothly in accordance with the stoichiometric ratios in this reaction system, the chemical equilibrium of the forward reaction (rightward) can be promoted by increasing the temperature or increasing the addition ratio of alkali metal carbonates.
[0035]
[0036] [Aqueous solutions containing carbonate ions and alkali metal ions] Aqueous solutions containing carbonate ions and alkali metal ions are typically prepared by dissolving alkali metal carbonates in water, but they may also be prepared by dissolving alkali metal salts other than alkali metal carbonates in water and bubbling carbon dioxide into the solution, and are not particularly limited. Examples of alkali metals include lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and cesium (Cs). Among these, sodium (Na) and potassium (K) are preferred, and sodium (Na) is more preferred.
[0037] When an aqueous solution containing carbonate ions and alkali metal ions is an aqueous solution of alkali metal carbonate, the amount of alkali metal carbonate added to prepare the aqueous solution is not particularly limited, as long as it is at least a stoichiometric amount relative to the amount of double sulfate (i.e., 3 moles or more for every 2 moles of double sulfate). In one preferred embodiment, the ratio of the amount of alkali metal carbonate to the amount of double sulfate is 1.5 to 3.0, more preferably 2.0 to 3.0, and even more preferably 2.5 to 3.0. This configuration can improve the yield of rare earth carbonates. Furthermore, this configuration can reduce the sulfur (S) content in the obtained rare earth carbonates.
[0038] When a double sulfate is added to an aqueous solution containing carbonate ions and alkali metal ions, rare earth carbonates are produced. The rare earth carbonates produced may be in the form of hydrates (rare earth carbonate hydrates). The rare earth carbonate production reaction may be carried out at a temperature of preferably 10 to 90°C, more preferably 25 to 80°C, and even more preferably 40 to 60°C, for preferably 1 to 48 hours, and more preferably 6 to 24 hours. To promote the rare earth carbonate production reaction, the reaction solution may be stirred as needed. Since the rare earth carbonate precipitates in the reaction solution, it can be recovered by solid-liquid separation (e.g., centrifugation, filtration, etc.).
[0039] <Electrolytic Deposition Process> In this process, at least one metal selected from the group consisting of praseodymium and neodymium is precipitated as a metal (Pr metal, Nd metal, or a mixture of Pr metal and Nd metal) by electrolytic deposition from the molten salt of the rare earth carbonate obtained in the carbonate production process above and at least one selected from the group consisting of alkali metal carbonates and alkaline earth metal carbonates. In the following, "Pr metal, Nd metal, or a mixture of Pr metal and Nd metal" will also be simply referred to as Pr / Nd metal.
[0040] [Molten Salt] The molten salt comprises a rare earth carbonate and at least one selected from the group consisting of alkali metal carbonates and alkaline earth metal carbonates, and is obtained by melting these carbonates.
[0041] The alkali metal carbonate used in this process is lithium carbonate (Li 2 CO 3 ), sodium carbonate (Na 2 CO 3 ), potassium carbonate (K 2 CO 3 ), rubidium carbonate (Rb 2 CO 3 ), cesium carbonate (Cs 2 CO 3 Examples include magnesium carbonate (MgCO3). 3 ), calcium carbonate (CaCO3) 3 ), strontium carbonate (SrCO 3 ), barium carbonate (BaCO2) 3 Examples include the following. These carbonates may be used individually or in combination of two or more. In one preferred embodiment, the molten salt comprises two or more selected from the group consisting of alkali metal carbonates and alkaline earth metal carbonates, more preferably three to five, and even more preferably four to five. With such a configuration, it is possible to lower the melting point of the molten salt and reduce the energy cost of electrolysis.
[0042] According to one preferred embodiment, the molten salt is given by formula: xLi 2 CO3 -(1-x)Na 2 CO 3 The solution contains a carbonate having the composition shown in the formula (wherein 0.37 < x < 0.52). The melting point of the carbonate having this composition may be around 498 to 550°C. In particular, when depositing Pr metal in the electrolytic deposition process, it is preferable to use a molten salt containing a carbonate having this composition. When the molten salt contains a carbonate having this composition, the ratio of the rare earth carbonate to 100 mol% of the carbonate having this composition is preferably 10.0 mol% or less, more preferably 5.0 mol% or less, even more preferably 0.1 to 5.0 mol%, particularly preferably 1.0 to 5.0 mol%, and most preferably 1.0 to 3.0 mol%. Based on the Nernst formula, the higher the dissolved concentration of the rare earth carbonate in the electrolytic bath, the more the potential shifts in the noble direction. Therefore, from the viewpoint of overpotential in constant potential electrolysis, a higher dissolved concentration of the rare earth carbonate is desirable. On the other hand, from the viewpoint of solubility in the electrolytic bath, the amount of rare earth carbonate is preferably 1.0 to 5.0 mol%, and more preferably 1.0 to 3.0 mol%.
[0043] According to another preferred form, the molten salt is given by formula: xLi 2 CO 3 -(1-x)BaCO 3The solution contains a carbonate having the composition shown in the formula (wherein 0.50 < x < 0.75). In particular, when depositing Pr metal in the electrolytic deposition process, it is preferable to use a molten salt containing a carbonate having the said composition. The melting point of the carbonate having the said composition may be around 609 to 650°C. When the molten salt contains a carbonate having the said composition, the ratio of the rare earth carbonate to 100 mol% of the carbonate having the said composition is preferably 10.0 mol% or less, more preferably 5.0 mol% or less, even more preferably 0.1 to 5.0 mol%, particularly preferably 1.0 to 5.0 mol%, and most preferably 1.0 to 3.0 mol%. Based on the Nernst formula, the higher the dissolved concentration of the rare earth carbonate in the electrolytic bath, the more the potential shifts in the noble direction; therefore, from the viewpoint of overpotential in constant potential electrolysis, a higher dissolved concentration of the rare earth carbonate is desirable. On the other hand, from the viewpoint of solubility in the electrolytic bath, the amount of rare earth carbonate is preferably 1.0 to 5.0 mol%, and more preferably 1.0 to 3.0 mol%.
[0044] According to a more preferred embodiment, the molten salt is given by the formula: (1-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xMCO 3The present invention provides a carbonate having the composition shown in the formula (wherein 0 < x ≤ 0.15 is satisfied, and M represents Ca or Ba). In particular, when Pr metal is precipitated in the electrolytic deposition process, it is preferable to use a molten salt containing a carbonate having the said composition. The melting point of the carbonate having the said composition may be 390°C to 395°C. By using a carbonate with such a low melting point, the energy cost of electrolytic deposition can be reduced. Therefore, the present invention also provides a carbonate having the said composition. When the molten salt contains a carbonate having the said composition, the ratio of the rare earth carbonate to 100 mol% of the carbonate having the said composition is preferably 10.0 mol% or less, more preferably 5.0 mol% or less, even more preferably 0.1 to 5.0 mol%, particularly preferably 1.0 to 5.0 mol%, and most preferably 1.0 to 3.0 mol%. According to the Nernst equation, the higher the dissolved concentration of rare earth carbonates in the electrolytic bath, the more the potential shifts towards the noble direction. Therefore, from the viewpoint of overpotential in constant-potential electrolysis, a higher dissolved concentration of rare earth carbonates is desirable. On the other hand, from the viewpoint of solubility in the electrolytic bath, a concentration of 1.0 to 5.0 mol% of rare earth carbonates is desirable, and 1.0 to 3.0 mol% is more desirable.
[0045] According to another more preferred form, the molten salt is of the formula: 0.07MCO 3 -(0.93-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xCs 2 CO 3The present invention provides a carbonate having the composition shown in the formula (wherein 0 ≤ x ≤ 0.07 is satisfied, and M represents Ca or Ba). In particular, when Pr metal is precipitated in the electrolytic deposition process, it is preferable to use a molten salt containing a carbonate having the said composition. The melting point of the carbonate having the said composition may be 390°C to 395°C. By using a carbonate with such a low melting point, the energy cost of electrolytic deposition can be reduced. Therefore, the present invention also provides a carbonate having the said composition. When the molten salt contains a carbonate having the said composition, the ratio of the rare earth carbonate to 100 mol% of the carbonate having the said composition is preferably 10.0 mol% or less, more preferably 5.0 mol% or less, even more preferably 0.1 to 5.0 mol%, particularly preferably 1.0 to 5.0 mol%, and most preferably 1.0 to 3.0 mol%. According to the Nernst equation, the higher the dissolved concentration of rare earth carbonates in the electrolytic bath, the more the potential shifts towards the noble direction. Therefore, from the viewpoint of overpotential in constant-potential electrolysis, a higher dissolved concentration of rare earth carbonates is desirable. On the other hand, from the viewpoint of solubility in the electrolytic bath, a concentration of 1.0 to 5.0 mol% of rare earth carbonates is desirable, and 1.0 to 3.0 mol% is more desirable.
[0046] According to a more preferred embodiment, the molten salt is given by the formula: (1-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xCs 2 CO 3The present invention provides a carbonate having a composition represented by (wherein 0 < x ≤ 0.07). In particular, when Nd metal is precipitated in the electrolytic deposition process, it is preferable to use a molten salt containing a carbonate having said composition. The melting point of the carbonate having said composition may be 390°C to 395°C. By using a carbonate with such a low melting point, the energy cost of electrolytic deposition can be reduced. Therefore, the present invention also provides a carbonate having said composition. When the molten salt contains a carbonate having said composition, the ratio of the rare earth carbonate to 100 mol% of the carbonate having said composition is preferably 10.0 mol% or less, more preferably 5.0 mol% or less, even more preferably 0.1 to 5.0 mol%, particularly preferably 1.0 to 5.0 mol%, and most preferably 1.0 to 3.0 mol%. According to the Nernst equation, the higher the dissolved concentration of rare earth carbonates in the electrolytic bath, the more the potential shifts towards the noble direction. Therefore, from the viewpoint of overpotential in constant-potential electrolysis, a higher dissolved concentration of rare earth carbonates is desirable. On the other hand, from the viewpoint of solubility in the electrolytic bath, a concentration of 1.0 to 5.0 mol% of rare earth carbonates is desirable, and 1.0 to 3.0 mol% is more desirable.
[0047] If the carbonate contained in the molten salt contains hydrates, it is preferable to dehydrate the molten salt before electrolysis. The method of dehydration is not particularly limited, but it is carried out by heating the molten salt to a temperature above its melting point (for example, 50 to 120°C higher than its melting point) under reduced pressure. If the carbonate contained in the molten salt contains trace amounts of impurities, it is preferable to pre-electrolyze the molten salt before electrolysis. The method of pre-electrolysis is not particularly limited, but it is carried out by applying a potential nobler than the deposition potential of the target rare earth element (for example, -1.5V to -1.1V relative to a Pt pseudo-reference electrode).
[0048] [Electrolytic deposition] The above molten salt is used as an electrolytic bath to deposit Pr / Nd metal by electrolytic deposition. The temperature of the electrolytic bath is not particularly limited as long as it is above the melting point of the molten salt, but it is preferably 20 to 80°C higher than the melting point, and more preferably 40 to 60°C higher than the melting point.
[0049] The anode electrode used in electrodeposition is not particularly limited as long as it is a material that does not hinder CO generation and is electrochemically stable, or a material in which the metal component of the anode electrode dissolves via an anode reaction by applying an electric potential in molten carbonate, and can be appropriately selected by those skilled in the art. Examples of such anode materials include platinum (Pt), NdFeB, glassy carbon, graphite and the like. The cathode electrode is also not particularly limited as long as it is a material that is electrochemically stable in molten carbonate and does not hinder the deposition of the target Pr / Nd metal, and can be appropriately selected by those skilled in the art. Examples of such cathode materials include copper (Cu), niobium (Nb), molybdenum (Mo), tantalum (Ta), tungsten (W) and the like, among which niobium (Nb), molybdenum (Mo), tantalum (Ta), and tungsten (W) are preferred. According to a preferred example, platinum (Pt) is used as the anode, molybdenum (Mo) or tungsten (W) is used as the cathode, and platinum (Pt) is used as the pseudo reference electrode. According to another preferred embodiment, an NdFeB rod is used as the anode, Mo or W is used as the cathode, and Pt is used as the pseudo reference electrode. In this embodiment, in order to prevent the iron-based compound from diffusing from the anode into the electrolytic bath, it is preferable to separate the anode and the electrolytic bath with a suitable filter. To prepare for falling electrodeposits at the cathode electrode, it is desirable to separate the cathode and the electrolytic bath with a suitable filter and provide a receiver at the bottom. 2
[0050] The potential (overpotential) applied to the electrode is not particularly limited as long as it is a potential (overpotential) that does not cause the electrolytic bath to decompose, and can be appropriately set by those skilled in the art depending on the type of metal to be recovered (Pr, Nd, or both Pr and Nd). For example, when the purpose is to recover Pr, it is preferable to apply an overpotential to the cathode such that the cathode potential is 0.5 V or more lower than the reduction potential of praseodymium, and to set the potential such that the difference between the cathode potential and the anode potential is smaller than the decomposition voltage of the molten salt. More specifically, when Pt is used as a pseudo-reference electrode, praseodymium can be deposited as a metal by applying an overpotential of -2.0 V to -2.5 V relative to the pseudo-platinum reference electrode. When the purpose is to recover Nd, it is preferable to apply an overpotential to the cathode such that the cathode potential is 0.5 V or more lower than the reduction potential of neodymium, and to set the potential such that the difference between the cathode potential and the anode potential is smaller than the decomposition voltage of the molten salt. More specifically, when Pt is used as a pseudo-reference electrode, neodymium can be deposited as a metal by applying an overvoltage of -2.6V to -3.0V relative to the pseudo-platinum reference electrode. As shown in Example 8 below, if the ratio of the amount of praseodymium to the total amount of praseodymium and neodymium contained in the rare-earth carbonate is large, a mixture of neodymium metal and praseodymium metal may be deposited when an overvoltage of -2.6V to -3.0V is applied. The time for electrolysis is not particularly limited, as long as the rare-earth complex species to be recovered proceeds in a diffusion-limited process or the rare-earth metal species deposited at the electrode interface do not settle in the electrolytic bath, but it is preferably 1 to 48 hours, more preferably 6 to 24 hours.
[0051] Furthermore, the following items are also included in the scope of the present invention: Item 1: A method for separating and recovering rare earth elements from a rare earth element-containing material containing at least one selected from the group consisting of praseodymium and neodymium, comprising: contacting the rare earth element-containing material with an acidic medium to obtain an eluate containing rare earth ions; adding an alkali metal sulfate to the eluate to obtain a double salt of rare earth ions, alkali metal ions, and sulfate ions; adding the double salt to an aqueous solution containing carbonate ions and alkali metal ions to obtain a rare earth carbonate; and precipitating at least one selected from the group consisting of praseodymium and neodymium as a metal from a molten salt containing the rare earth carbonate and at least one selected from the group consisting of alkali metal carbonates and alkaline earth metal carbonates by electrolysis; Item 2: The method for separating and recovering rare earth elements according to Item 1, wherein the rare earth element-containing material contains a transition metal element, and at least a portion of the transition metal element is in the form of a transition metal oxide; Item 3: The method for separating and recovering rare earth elements according to Item 1 or 2, wherein the acid medium is hydrochloric acid with a concentration of 1.2 mol / L or less; Item 4: The method for separating and recovering rare earth elements according to any one of Items 1 to 3, wherein in the electrolytic emission, an overvoltage is applied to the cathode such that the cathode potential is 0.5 V or more lower than the reduction potential of praseodymium, and the potential is set such that the difference between the cathode potential and the anode potential is smaller than the decomposition voltage of the molten salt; Item 5: The method for separating and recovering rare earth elements according to any one of Items 1 to 4, wherein in the electrolytic emission, an overvoltage of -2.0 V to -2.5 V relative to a pseudo-platinum reference electrode is applied; Item 6: A method for separating and recovering rare earth elements according to any one of Items 1 to 5, wherein in the electrolytic emission, an overvoltage is applied to the cathode such that the cathode potential is 0.5 V or more lower than the reduction potential of neodymium, and the potential is set such that the difference between the cathode potential and the anode potential is smaller than the decomposition voltage of the molten salt; Item 7: A method for separating and recovering rare earth elements according to any one of Items 1 to 6, wherein in the electrolytic emission, an overvoltage of -2.6 V to -3.0 V is applied with respect to a pseudo-platinum reference electrode;Item 8: The method for separating and recovering a rare earth element according to any one of Items 1 to 7, wherein in the electrolytic deposition, the cathode material is at least one selected from the group consisting of copper (Cu), niobium (Nb), molybdenum (Mo), tantalum (Ta), and tungsten (W); Item 9: The method for separating and recovering a rare earth element according to any one of Items 1 to 8, wherein the ratio of the substance amount of the alkali metal sulfate to the substance amount of the rare earth element contained in the eluate is 6.0 to 12.0; Item 10: The aqueous solution containing carbonate ions and alkali metal ions is an aqueous solution of an alkali metal carbonate, and the ratio of the substance amount of the alkali metal carbonate to the substance amount of the double salt is 1.5 to 3.0, the method for separating and recovering a rare earth element according to any one of Items 1 to 9; Item 11: The molten salt includes the rare earth carbonate and a carbonate having a composition represented by the formula: xLi; 2 CO 3 -(1-x)Na 2 CO 3 (wherein 0.37 < x < 0.52 is satisfied), the method for separating and recovering a rare earth element according to any one of Items 1 to 10; Item 12: The molten salt includes the rare earth carbonate and a carbonate having a composition represented by the formula: xLi 2 CO 3 -(1-x)BaCO 3 (wherein 0.50 < x < 0.75 is satisfied), the method for separating and recovering a rare earth element according to any one of Items 1 to 10; Item 13: The molten salt includes the rare earth carbonate and a carbonate having a composition represented by the formula: (1-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 )-xMCO 3 (wherein 0 < x ≤ 0.15 is satisfied, and M represents Ca or Ba), the method for separating and recovering a rare earth element according to any one of Items 1 to 10; Item 14: The molten salt includes the rare earth carbonate and a carbonate having a composition represented by the formula: 0.07MCO 3 -(0.93-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K2 CO 3 ) - xCs 2 CO 3 A method for separating and recovering rare earth elements according to any one of items 1 to 10, comprising a carbonate having the composition shown in the formula: (1-x)(0.476Li) (wherein 0 ≤ x ≤ 0.07, and M represents Ca or Ba); Item 15: The molten salt comprises the rare earth carbonate and a carbonate having the composition shown in the formula: (1-x)(0.476Li) 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xCs 2 CO 3 A method for separating and recovering rare earth elements according to any one of items 1 to 10, comprising a carbonate having a composition represented by the formula: (1-x)(0.476Li) 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xCs 2 CO 3 A method for separating and recovering rare earth elements according to any one of claims 1 to 10, comprising precipitating neodymium as a metal from a molten salt containing a carbonate having a composition represented by (wherein the formula satisfies 0 < x ≤ 0.07).
[0052] The present invention will be described in more detail below with reference to examples. However, the technical scope of the present invention is not limited to the following examples.
[0053] 《Separation and Recovery of Praseodymium》 [Example 1] <ICP-AES Analysis of Rare Earth Element-Containing Precursor (Magnet A)> A demagnetized Nd-Fe-B magnet (referred to as "Magnet A"), used as a rare earth element-containing precursor, was immersed in 20 mL of aqua regia and dissolved at 70°C for 5 hours. The resulting solution was filtered, and the filtrate was diluted with distilled water to prepare a 100 mL standard solution. This standard solution was further diluted at dilution ratios of 1 / 10, 1 / 25, 1 / 50, 1 / 100, 1 / 200, 1 / 400, 1 / 800, 1 / 1600, and 1 / 3200, and ICP-AES analysis (inductively coupled plasma emission spectroscopy) was performed using each dilution. For each element, an appropriate concentration range was selected in which the dilution ratio and the quantitative analysis value were consistent. Finally, the average value of the appropriate concentration range was adopted as the quantitative analysis value. The results are shown in Table 1 below.
[0054]
[0055] <Oxidation Treatment Process> The above-mentioned demagnetized Nd-Fe-B magnet (Magnet A, Pr:Nd (molar ratio) = 26.0:74.0) (thickness 2 mm) was subjected to six oxidation roasting cycles at 900°C for 3 hours. The sample after oxidation roasting was pulverized in an automatic mortar to obtain oxidized magnetic powder (containing rare earth elements). XRD (X-ray crystal structure analysis) was performed on the oxidized magnetic powder to determine Fe 2 O 3 I checked the layers.
[0056] <Acid Elution Process> 5 g of the above-mentioned oxide magnetic powder containing rare earth elements was mixed with 100 mL of 1.2 mol / L hydrochloric acid as the acid medium, and the mixture was stirred at 75°C and 500 rpm for 12 hours to induce elution. During this process, the rare earth elements (Ln = Pr, Nd, Tb, Dy) eluted into the acid medium by the reaction shown in Formula 1 below. The obtained eluate was filtered, and the filtrate was progressively diluted with distilled water in the range of 1 / 40 to 1 / 640. ICP-AES analysis was performed using each dilution. The results are shown in Table 2 below.
[0057]
[0058]
[0059] As shown in Table 2, the proportion of Fe among the elements contained in the eluate is smaller than the proportion of Fe among the elements contained in the rare earth element-containing material. Therefore, the oxidation treatment process removes Fe. 2 O 3 It can be seen that a large portion of the Fe can be separated by performing an acid elution process after morphology.
[0060] <Sulfate Double Salt Production Process> Add sodium sulfate (Na) to 50 mL of the above eluate in amounts 6.0 times, 8.0 times, 10.0 times, 12.0 times, and 14.0 times relative to the molar amount of the rare earth element (3.0 times, 4.0 times, 5.0 times, 6.0 times, and 7.0 times the stoichiometric amount). 2 SO 4 Add ) and stir at 25°C and 500 rpm, Na 2 SO 4 The elements were dissolved. The pH of each solution at this time was 0.12 to 0.17. The solutions were then stirred at 80°C and 500 rpm for 12 hours. During this time, the rare earth elements (Ln=Pr, Nd, Tb, Dy) formed double sulfates through the reaction shown in the following formula. The pH of each solution after the reaction was 0.12 to 0.17. The obtained solutions were centrifuged at 9840 G for 3 minutes to separate the solids from the liquids. The solids were dried at room temperature (25°C) for 24 hours, and then their weight was measured. Furthermore, XRD (X-ray crystallography) was performed on the dried solids, and it was determined that the solids were double sulfates (LnNa(SO)). 4 ) 2 6H 2 It was confirmed that the ratio was O(Ln=Pr,Nd,Tb,Dy). The yield of the double sulfate in each example is shown in Table 3 below. In addition, 0.1 g of the double sulfate was mixed with 1.0 mol / L nitric acid (HNO). 3 The solution was completely dissolved in 50 mL of aqueous solution. The resulting solution was gradually diluted with distilled water in the range of 1 / 2 to 1 / 20, and ICP-AES analysis was performed using each dilution. 10.0 times the amount of rare earth element (5.0 times the stoichiometric amount) of sodium sulfate (Na) was added. 2 SO 4 The results of the ICP-AES analysis in the example where () was added are shown in Table 4 below.
[0061]
[0062]
[0063]
[0064] As shown in Table 3, Na is the molar mass of rare earth elements. 2 SO 4 It can be seen that the yield of sulfate double salts is particularly high when the amount of additive is about 10.0 times the normal amount. Also, as shown in Table 4, rare earth elements tend to form double salts more readily than other elements (Fe, B, Na), so it can be seen that many other elements can be separated and removed by this process. It can also be seen that light rare earth elements (Pr and Nd) tend to form double salts more readily than heavy rare earth elements (Tb and Dy).
[0065] <Carbonate Production Process> In the above <Sulfate Double Salt Production Process>, 10.0 times the amount of sodium sulfate (Na) relative to the amount of rare earth element (5.0 times the stoichiometric amount) is added. 2 SO 4 In the example where sodium carbonate (Na) was added, 1 g of the resulting double sulfate was weighed. The amount of sodium carbonate (Na) was used relative to the amount of substance of the double sulfate. 2 CO 3 The amount of ) was weighed out to 1.5 times, 2.0 times, 2.5 times, and 3.0 times (equal amounts, 1.33 times, 1.67 times, and 2.00 times the stoichiometric amount), and each was completely dissolved in 100 mL of distilled water. At this time, each Na 2 CO 3 The pH of the aqueous solution was 11.2–11.7. 2 CO 3 One g of double sulfate was added to an aqueous solution and stirred at 60°C and 350 rpm for four hours. During this time, the double sulfate formed a carbonate through the reaction shown in the following formula. The pH of each solution after the reaction was 9.74, 9.84, 10.42, and 10.70. The obtained solutions were centrifuged at 9840 G for three minutes to separate the solid from the liquid. After drying the solid at room temperature (25°C) for 24 hours, XRD (X-ray crystallography) was performed on the solid, and it was determined that the solid was a carbonate (Ln 2 (CO 3 ) 3 8H 2It was confirmed that the carbonate was O(Ln=Pr,Nd,Tb,Dy). Differential scanning calorimetry (DSC) was performed on the carbonate, and it was found to have a melting point in the range of 109.2 to 110.2°C. The yield of the carbonate in each example is shown in Table 5 below. In addition, 0.1 g of the carbonate was mixed with 1.0 mol / L nitric acid (HNO). 3 The solution was completely dissolved in 50 mL of aqueous solution. The resulting solution was gradually diluted with distilled water in the range of 1 / 2 to 1 / 20, and ICP-AES analysis was performed using each dilution. 3.0 times the amount of rare earth element (2.00 times the stoichiometric amount) of sodium carbonate (Na) was used. 2 CO 3 The results of the ICP-AES analysis in the example where () was added are shown in Table 6 below.
[0066]
[0067]
[0068]
[0069] As shown in Table 5, Na is the molar mass of rare earth elements. 2 CO 3 As the amount of additive approaches 3.0 times the original amount, it can be seen that the sulfur (S) content in the carbonate decreases and the yield improves.
[0070] <Electrolytic deposition process> [(Li, Na) 2 CO 3 [Electrolytic emission using electrolytic bath] Lithium carbonate (Li 2 CO 3 ) and sodium carbonate (Na 2 CO 3 ) and, formula: 0.42Li 2 CO 3 -0.58Na 2 CO 3 The ingredients were weighed to achieve the composition shown and mixed in an alumina container. The mixture in the alumina container was placed in an electric furnace and N 2A molten carbonate was prepared by melting the mixture at 700°C under atmospheric conditions, and then cooling and solidifying it. Differential scanning calorimetry (DSC) was performed on the molten carbonate, and the melting point was found to be 498°C. For 100 mol% of the molten carbonate, in the above <carbonate production process>, 3.0 times the amount of sodium carbonate (Na) relative to the amount of double sulfate (2.00 times the stoichiometric amount) was added. 2 CO 3 The carbonate obtained in the example where () was added was added at a rate of 1 mol%, and dehydration treatment was carried out at 500°C for 12 hours under reduced pressure of -0.1 MPa. Then, using a Pt wire as the anode, a Cu substrate as the cathode, and a Pt wire as the pseudo-reference electrode, a potential (overpotential) of -2.4 V relative to the pseudo-platinum reference electrode was applied, and constant potential electrolysis was carried out at an electrolytic bath temperature of 550°C for 10 hours. The outermost layer of the black electrodeposited on the Cu substrate (cathode) was ground to the order of nm by Ar sputtering, and then analyzed by X-ray photoelectron spectroscopy (XPS). Figure 1 shows the XPS spectra of each electrodeposited obtained when the overpotential relative to the pseudo-platinum reference electrode was changed to -2.0 V, -2.1 V, -2.2 V, -2.3 V, and -2.4 V. As shown in Figure 1, a peak with a peak top in the range of 931.4 to 931.7 eV was observed. According to JF Moulder et al., “Handbook of X-ray photo-electron spectroscopy”, Perkin-Elmer Corp., (1992), in the XPS spectrum, the peak of metallic Pr appears in the range of 931.1–931.5 eV, and Pr 2 O 3 The peak appears in the range of 933.0–933.5 eV, and ProO 2 The peak appears in the range of 935.0–935.5 eV. Furthermore, peaks for Nd metal and Nd oxides, Tb metal and Tb oxides, and Dy metal and Dy oxides were not observed. Therefore, it was confirmed that the electrodeposited material is Pr metal.
[0071] [Example 2] The above [(Li, Na) 2 CO 3Instead of using an electrolytic bath for electrolysis, the electrolysis process was performed using the following method. Otherwise, the separation and recovery of praseodymium was attempted in the same manner as in Example 1.
[0072] [(Li 2 , Ba) CO 3 [Electrolytic emission using electrolytic bath] Lithium carbonate (Li 2 CO 3 ) and barium carbonate (BaCO2) 3 ) and, formula: 0.55Li 2 CO 3 -0.45 BaCO 3 The ingredients were weighed to achieve the composition shown and mixed in an alumina container. The mixture in the alumina container was placed in an electric furnace and N 2 A molten carbonate was prepared by melting the mixture at 700°C under atmospheric conditions, and then cooling and solidifying it. Differential scanning calorimetry (DSC) was performed on the molten carbonate, and the melting point was found to be 609°C. To 100 mol% of the molten carbonate, in the above <carbonate production process>, 3.0 times the amount of sodium carbonate (Na) relative to the amount of double sulfate (2.00 times the stoichiometric amount) was added. 2 CO 3 The carbonate obtained in the example where () was added was added at a rate of 1 mol%, and dehydration treatment was carried out at 650°C for 12 hours under reduced pressure of -0.1 MPa. Subsequently, a Pt wire was used as the anode, a Cu substrate as the cathode, and a Pt wire as the pseudo-reference electrode, and a potential (overpotential) of -2.4 V was applied relative to the pseudo-platinum reference electrode, and constant potential electrolysis was carried out at 650°C for 10 hours. The outermost layer of the black electrodeposited on the Cu substrate (cathode) was ground to the order of nm by Ar sputtering, and then analyzed by X-ray photoelectron spectroscopy (XPS). A peak with a peak top in the range of 931.4 to 931.7 eV was observed. Furthermore, peaks of Nd metal and Nd oxide, Tb metal and Tb oxide, and Dy metal and Dy oxide were not observed. From this, it was confirmed that the electrodeposited material was Pr metal.
[0073] [Example 3] The above [(Li, Na) 2 CO 3Instead of using an electrolytic bath for electrolysis, the electrolysis process was performed using the following method. Otherwise, the separation and recovery of praseodymium was attempted in the same manner as in Example 1.
[0074] [(Li 2 , Na 2 , K 2 , Ba) CO 3 [Electrolytic emission using electrolytic bath] Lithium carbonate (Li 2 CO 3 ) and sodium carbonate (Na 2 CO 3 ) and potassium carbonate (K 2 CO 3 ) and barium carbonate (BaCO2) 3 ) and, formula: 0.85(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 )-0.15BaCO 3 The ingredients were weighed to achieve the composition shown and mixed in an alumina container. The mixture in the alumina container was placed in an electric furnace and N 2 A molten carbonate was prepared by melting the mixture at 700°C under atmospheric conditions, and then cooling and solidifying it. Differential scanning calorimetry (DSC) was performed on the molten carbonate, and the melting point was found to be 390°C to 395°C. For 100 mol% of the molten carbonate, in the above <carbonate production process>, 3.0 times the amount of sodium carbonate (Na) relative to the amount of double sulfate (2.00 times the stoichiometric amount) was added. 2 CO 3The carbonate obtained in the example with the addition of ( ) was added at a rate of 1 mol%, and dehydration treatment was carried out at 500°C for 12 hours under reduced pressure of -0.1 MPa. Subsequently, an NdFeB rod was used as the anode, a Cu substrate as the cathode, and a Pt wire as the pseudo-reference electrode. The electrolytic bath and the anode were separated by a G3 filter to prevent the diffusion of Fe-based compounds into the electrolytic bath. A potential (overpotential) of -2.5 V was applied relative to the pseudo-platinum reference electrode, and constant potential electrolysis was performed at an electrolytic bath temperature of 450°C for 10 hours. The outermost layer of the black electrodeposited material on the Cu substrate (cathode) was ground to the order of nm by Ar sputtering, and then analyzed by X-ray photoelectron spectroscopy (XPS). A peak with a peak top in the range of 931.2 to 931.7 eV was observed. Furthermore, no peaks of Nd metal and Nd oxide, Tb metal and Tb oxide, or Dy metal and Dy oxide were observed. From this, it was confirmed that the electrodeposited material was Pr metal.
[0075] [Example 4] The above [(Li, Na) 2 CO 3 Instead of using an electrolytic bath for electrolysis, the electrolysis process was performed using the following method. Otherwise, the separation and recovery of praseodymium was attempted in the same manner as in Example 1.
[0076] [(Li 2 , Na 2 , K 2 , Ca, (Cs 2 )) CO 3 [Electrolytic emission using electrolytic bath] Lithium carbonate (Li 2 CO 3 ) and sodium carbonate (Na 2 CO 3 ) and potassium carbonate (K 2 CO 3 ) and calcium carbonate (CaCO3) 3 ) and cesium carbonate (Cs 2 CO 3 ) and, formula: 0.07CaCO 3 -(0.93-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3) - xCs 2 CO 3 The mixture was weighed to the composition shown (where x is 0, 0.03, 0.04, 0.05, 0.06, or 0.07) and mixed in an alumina container. The mixture in the alumina container was placed in an electric furnace and N 2 Molten carbonate was prepared by melting the mixture at 700°C under atmospheric conditions, and then cooling and solidifying it. Differential scanning calorimetry (DSC) was performed on the molten carbonate, and the melting points of the molten carbonate with x = 0.03, 0.04, 0.05, 0.06, or 0.07 were 390°C to 395°C, and the melting point of the molten carbonate with x = 0 was 395°C. For 100 mol% of the molten carbonate, in the above <carbonate production process>, 3.0 times the amount of sodium carbonate (Na) relative to the amount of double sulfate (2.00 times the stoichiometric amount) was added. 2 CO 3 The carbonate obtained in the example with the addition of ( ) was added at a rate of 1 mol%, and dehydration treatment was carried out at 500°C for 12 hours under reduced pressure of -0.1 MPa. Subsequently, an NdFeB rod was used as the anode, a Cu substrate as the cathode, and a Pt wire as the pseudo-reference electrode. The electrolytic bath and the anode were separated by a G3 filter to prevent Fe from diffusing into the electrolytic bath. A potential (overpotential) of -2.5 V was applied relative to the pseudo-platinum reference electrode, and constant potential electrolysis was performed at an electrolytic bath temperature of 450°C for 10 hours. The outermost layer of the black electrodeposited material on the Cu substrate (cathode) was ground to the order of nm by Ar sputtering, and then analyzed by X-ray photoelectron spectroscopy (XPS). A peak with a peak top in the range of 931.2 to 931.7 eV was observed. Furthermore, no peaks of Nd metal and Nd oxide, Tb metal and Tb oxide, or Dy metal and Dy oxide were observed. From this, it was confirmed that the electrodeposited material was Pr metal.
[0077] [Separation and Recovery of Neodymium, or a Mixture of Praseodymium Metal and Neodymium Metal] [Example 5] <ICP-AES Analysis of Rare Earth Element-Containing Precursor (Magnet B)> A demagnetized Nd-Fe-B magnet (referred to as "Magnet B"), used as a rare earth element-containing precursor, was immersed in 20 mL of aqua regia and dissolved at 70°C for 5 hours. The resulting solution was filtered, and the filtrate was diluted with distilled water to prepare a 100 mL standard solution. This standard solution was further diluted stepwise at dilution ratios from 1 / 10 to 1 / 1280, and ICP-AES analysis (inductively coupled plasma emission spectroscopy) was performed using each dilution. For each element, an appropriate concentration range was selected in which the dilution ratio and the quantitative analysis value were consistent. Finally, the average value of the appropriate concentration range was adopted as the quantitative analysis value. The results are shown in Table 7 below.
[0078]
[0079] <Oxidation Treatment Process> The demagnetized Nd-Fe-B magnet (magnet B, Pr:Nd (molar ratio) = 6.82:93.18) was subjected to oxidative roasting nine times at 900°C for 3 hours. The sample after oxidative roasting was pulverized in an automatic mortar to obtain oxidized magnetic powder (containing rare earth elements). XRD (X-ray crystal structure analysis) was performed on the oxidized magnetic powder to determine Fe 2 O 3 I checked the layers.
[0080] <Acid Elution Process> 5.0 g of the above-mentioned oxide magnetic powder containing rare earth elements was mixed with 100 mL of 1.2 mol / L hydrochloric acid as the acid medium, and the mixture was stirred at 75°C and 500 rpm for 12 hours to eluate the elements. The resulting eluate was filtered, and the filtrate was progressively diluted with distilled water in the range of 1 / 25 to 1 / 400. ICP-AES analysis was performed using each dilution. The results are shown in Table 8 below. The pH and ORP (oxidation-reduction potential) of the eluate were pH = 0.22 to 0.26 and ORP = 621.8 to 634.6 mV vs. Ag / AgCl, respectively. In the Pourbaix Diagram (potential-pH diagram), this range of pH and ORP is mainly due to Fe. 2 O 3 It is stable as a rare earth element, Ln 3+This corresponds to the region where it is dissolved. Therefore, it was confirmed that under these conditions, rare earth elements can be selectively eluted while Fe remains as a solid phase.
[0081]
[0082] <Sulfate Double Salt Formation Process> Add 10.0 times the amount of sodium sulfate (Na) relative to the amount of rare earth element (5.0 times the stoichiometric amount) to 50 mL of the above eluate. 2 SO 4 Add ) and stir at 25°C and 500 rpm, Na 2 SO 4 The solution was dissolved. The solution was then stirred at 80°C and 500 rpm for 12 hours. The pH of the solution after the reaction was 0.12. The resulting solution was centrifuged at 9840 G for 3 minutes to separate the solid from the liquid. The solid was dried at room temperature (25°C) for 24 hours, and its weight was measured. XRD measurement was also performed on the dried solid, and it was determined that the solid was a double sulfate [LnNa(SO4)]. 4 ) 2 6H 2 We confirmed that O(Ln = Pr, Nd, Tb, Dy).
[0083] <Carbonate Production Process> In the above <Sulfate Double Salt Production Process>, 10.0 times the amount of sodium sulfate (Na) relative to the amount of rare earth element (5.0 times the stoichiometric amount) is added. 2 SO 4 5.0 g of the double sulfate obtained in the example where ) was added was weighed. Relative to the amount of substance of the double sulfate, sodium carbonate (Na 2 CO 3 The amount of ) was weighed out to be 3.0 times the amount (2.0 times the stoichiometric amount), and each was completely dissolved in 100 mL of distilled water. 2 CO 3 The pH of the aqueous solution was 11.7. 2 CO 3 5.0 g of double sulfate was added to the aqueous solution and stirred at 60°C and 350 rpm for 4 hours. The resulting solution was centrifuged at 9840 G for 3 minutes to separate the solid from the liquid. After drying the solid at room temperature (25°C) for 24 hours, the solid was subjected to XRD measurement, and the carbonate [Ln] of the solid was determined.2 (CO 3 ) 3 ・xH 2 We confirmed that O(Ln = Pr, Nd, Tb, Dy).
[0084] <Electrolytic deposition process> [(Li 2 , Na 2 , K 2 , Cs 2 ) CO 3 [Electrolytic emission using electrolytic bath] Lithium carbonate (Li 2 CO 3 ) and sodium carbonate (Na 2 CO 3 ) and potassium carbonate (K 2 CO 3 ) and cesium carbonate (Cs 2 CO 3 ) and, formula: 0.93(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) -0.07Cs 2 CO 3 The ingredients were weighed to achieve the composition shown and mixed in an alumina container. The mixture in the alumina container was placed in an electric furnace and N 2A molten carbonate was prepared by melting the mixture at 700°C under atmospheric conditions and then cooling and solidifying it. Differential scanning calorimetry (DSC) was performed on the molten carbonate, and the melting point was found to be 390-395°C. 1 mol% of the carbonate obtained in the above <carbonate production process> was added to 100 mol% of the molten carbonate, and dehydration was performed at 500°C for 12 hours under reduced pressure of -0.1 MPa. Before electrolysis, a preliminary electrolysis was performed for 3 hours by applying an overvoltage of -1.5V to the cathode side using a Pt pseudo-reference electrode as a reference, to remove trace amounts of impurities in the electrolytic bath. All electrodes used in the preliminary electrolysis were replaced before the constant potential electrolysis. In the constant potential electrolysis after the preliminary electrolysis, an NdFeB rod was used as the anode, a Mo substrate as the cathode, and a Pt wire as the pseudo-reference electrode. To prevent the electrodeposited material from diffusing into the electrolytic bath and remaining near the electrode even if it falls onto the cathode, the electrolytic bath and the cathode were separated by a G3 filter. To prevent Fe from diffusing into the electrolytic bath, the electrolytic bath and the anode were separated by a G3 filter. A potential of -2.6V (overpotential) was applied with a pseudo-platinum reference electrode as the reference, and constant potential electrolysis was performed for 12 hours at an electrolytic bath temperature of 450°C. The outermost layer of the black electrodeposited material on the Mo substrate (cathode) and the fallen material was ground to the order of nm by Ar sputtering, and then analyzed by X-ray photoelectron spectroscopy (XPS). Figure 2 shows the XPS spectra of the electrodeposited material obtained in this embodiment. In Figure 2, the red spectrum shows the measurement results of the outermost layer that was not ground by Ar sputtering. The orange spectrum shows the measurement results at a position 0.25 μm from the outermost layer ground by Ar sputtering. Furthermore, the yellow-green, green, light blue, blue, and purple spectra show the measurement results at positions where the material was sequentially ground by Ar sputtering in increments of several tens of nanometers in the depth direction from the 0.25 μm position mentioned above. The grinding depth for each position was calculated based on the sputtering rate determined from the sputtering conditions. As shown in Figure 2, a peak with its peak top in the range of 980.5–981.0 eV was observed. Also, no peaks for Pr metal and Pr oxide, Tb metal and Tb oxide, or Dy metal and Dy oxide were observed. From this, it was confirmed that the electrodeposited material was Nd metal.Table 9 shows the results of energy-dispersive X-ray spectroscopy (EDX) analysis of the electrodeposit obtained in this embodiment. As shown in Table 9, the Nd content was 85.0% by mass or more, and the oxygen content was 10.0% by mass or less, confirming that the majority of the electrodeposit is Nd metal. Generally, light elements such as C, N, and Li cannot be quantified by EDX measurement. Also, the detected oxygen may include that which is due to adsorption to the carbon tape used to hold the sample. Furthermore, since Pr, Tb, and Dy have X-ray energy levels close to Nd, trace levels of signals tend to be detected.
[0085]
[0086] [Example 6] In the <Acid Elution Step>, replace "5.0 g of the above-mentioned magnetic oxide powder" with "5.0 g of the above-mentioned magnetic oxide powder and Pr 2 O 3 A mixed powder was prepared by mixing the two components to achieve a Pr:Nd molar ratio of 9.81:90.19 and a total mass of 5.0 g. This mixed powder was used as the rare earth element-containing material. In the electrolytic extraction process, 2.5 mol% of the carbonate obtained in the carbonate generation process was added to 100 mol% of the molten carbonate. A W substrate was used as the cathode instead of the Mo substrate. The applied overpotential was set to a potential of -2.85 V relative to the pseudo-platinum reference electrode. Otherwise, the separation and recovery of neodymium was attempted using the same method as in Example 5. As a result, an electrodeposit consisting of Nd metal was obtained, similar to Example 5. Table 10 shows the EDX analysis results of the electrodeposit obtained in this example. As shown in Table 10, the Nd content was 85.0 mass% or more and the oxygen content was 10.0 mass% or less, confirming that the majority of the electrodeposit is Nd metal.
[0087]
[0088] [Example 7] In the <Acid Elution Step>, replace "5.0 g of the above-mentioned magnetic oxide powder" with "5.0 g of the above-mentioned magnetic oxide powder and Pr 2 O 3A mixed powder was prepared by mixing the two substances to achieve a Pr:Nd molar ratio of 12.26:87.74 and a total mass of 5.0 g. This mixed powder was used as the rare earth element-containing material. In the electrolytic extraction process, 5.0 mol% of the carbonate obtained in the carbonate generation process was added to 100 mol% of the molten carbonate. A W substrate was used as the cathode instead of the Mo substrate. The applied overpotential was set to a potential of -3.0 V relative to the pseudo-platinum reference electrode. Otherwise, the separation and recovery of neodymium was attempted using the same method as in Example 5. As a result, an electrodeposit consisting of Nd metal was obtained, similar to Example 5. Table 11 shows the EDX analysis results of the electrodeposit obtained in this example. As shown in Table 11, the Nd content was 85.0 mass% or more and the oxygen content was 10.0 mass% or less, confirming that the majority of the electrodeposit is Nd metal.
[0089]
[0090] [Example 8] In the <Acid Elution Step>, replace "5.0 g of the above-mentioned magnetic oxide powder" with "5.0 g of the above-mentioned magnetic oxide powder and Pr 2 O 3 A mixed powder was prepared by mixing the two components to achieve a Pr:Nd molar ratio of 19.23:80.77 and a total mass of 5.0 g. This mixed powder was used as the rare earth element-containing material. In the electrolysis extraction process, 5.0 mol% of the carbonate obtained in the carbonate generation process was added to 100 mol% of the molten carbonate. A W substrate was used as the cathode instead of the Mo substrate. The applied overpotential was set to a potential of -3.0 V relative to the pseudo-platinum reference electrode. Otherwise, the separation and recovery of neodymium was attempted using the same method as in Example 5. As a result, a peak with a peak top in the range of 980.5 to 981.0 eV was observed in the XPS spectrum of the electrodeposited material. Although no peaks for Tb metal and Tb oxide, or Dy metal and Dy oxide were observed, a weak peak was observed in the range of 931.5 to 931.9 eV. From this, it was concluded that the electrodeposit obtained in this embodiment is a mixture containing Nd metal and a small amount of Pr metal.
[0091] As shown in the above examples, according to the present invention, in a method for separating and recovering rare earth elements using electrolytic deposition, Pr can be deposited as a metal on the electrode. Furthermore, Nd can be deposited as a metal on the electrode, or Nd and Pr can be deposited as a mixture of metals on the electrode.
[0092] This application is based on Japanese Patent Application No. 2025-78380, filed on 9 May 2025, the disclosures of which are referenced and incorporated in whole.
Claims
1. A method for separating and recovering rare earth elements from a rare earth element-containing material containing at least one selected from the group consisting of praseodymium and neodymium, comprising: contacting the rare earth element-containing material with an acidic medium to obtain an eluate containing rare earth ions; adding an alkali metal sulfate to the eluate to obtain a double salt of rare earth ions, alkali metal ions, and sulfate ions; adding the double salt to an aqueous solution containing carbonate ions and alkali metal ions to obtain a rare earth carbonate; and precipitating at least one selected from the group consisting of praseodymium and neodymium as a metal from a molten salt containing the rare earth carbonate and at least one selected from the group consisting of alkali metal carbonates and alkaline earth metal carbonates by electrolysis.
2. The method for separating and recovering rare earth elements according to claim 1, wherein the rare earth element-containing material includes a transition metal element, and at least a portion of the transition metal element is in the form of a transition metal oxide.
3. The method for separating and recovering rare earth elements according to claim 1 or 2, wherein the acid medium is hydrochloric acid with a concentration of 1.2 mol / L or less.
4. The method for separating and recovering rare earth elements according to claim 1 or 2, wherein in the electrolytic extraction, an overvoltage is applied to the cathode such that the cathode potential is 0.5 V or more lower than the reduction potential of praseodymium, and the potential is set such that the difference between the cathode potential and the anode potential is smaller than the decomposition voltage of the molten salt.
5. The method for separating and recovering rare earth elements according to claim 1 or 2, comprising applying an overvoltage of -2.0V to -2.5V with respect to a pseudo-platinum reference electrode in the electrolytic extraction.
6. The method for separating and recovering rare earth elements according to claim 1 or 2, wherein in the electrolytic extraction, an overvoltage is applied to the cathode such that the cathode potential is 0.5 V or more lower than the reduction potential of neodymium, and the potential is set such that the difference between the cathode potential and the anode potential is smaller than the decomposition voltage of the molten salt.
7. The method for separating and recovering rare earth elements according to claim 1 or 2, comprising applying an overvoltage of -2.6V to -3.0V with respect to a pseudo-platinum reference electrode in the electrolytic extraction.
8. The method for separating and recovering rare earth elements according to claim 1 or 2, wherein in the electrolytic emission, the cathode material is at least one selected from the group consisting of copper (Cu), niobium (Nb), molybdenum (Mo), tantalum (Ta), and tungsten (W).
9. The method for separating and recovering rare earth elements according to claim 1 or 2, wherein the ratio of the amount of substance of the alkali metal sulfate to the amount of substance of the rare earth elements contained in the eluate is 6.0 to 12.
0.
10. The method for separating and recovering rare earth elements according to claim 1 or 2, wherein the aqueous solution containing carbonate ions and alkali metal ions is an aqueous solution of alkali metal carbonate, and the ratio of the amount of substance of the alkali metal carbonate to the amount of substance of the double salt is 1.5 to 3.
0.
11. The molten salt is the rare earth carbonate and the formula: xLi 2 CO 3 -(1-x)Na 2 CO 3 A method for separating and recovering rare earth elements according to claim 1 or 2, comprising a carbonate having a composition represented by the formula (wherein 0.37 < x < 0.52).
12. The molten salt is the rare earth carbonate and the formula: xLi 2 CO 3 -(1-x)BaCO 3 A method for separating and recovering rare earth elements according to claim 1 or 2, comprising a carbonate having a composition represented by the formula (wherein 0.50 < x < 0.75).
13. The molten salt comprises the rare earth carbonate and a carbonate having a composition represented by the formula: (1-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 )-xMCO 3 (wherein 0 < x ≤ 0.15 is satisfied, and M represents Ca or Ba). The method for separating and recovering a rare earth element according to claim 1 or 2.
14. The molten salt is the rare earth carbonate and the formula: 0.07 MCO 3 -(0.93-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xCs 2 CO 3 A method for separating and recovering rare earth elements according to claim 1 or 2, comprising a carbonate having a composition represented by the formula (wherein 0 ≤ x ≤ 0.07, and M represents Ca or Ba).
15. The molten salt is the rare earth carbonate and the formula: (1-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xCs 2 CO 3 A method for separating and recovering rare earth elements according to claim 1 or 2, comprising a carbonate having a composition represented by the formula (wherein 0 < x ≤ 0.07).
16. Formula: (1-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xMCO 3 A carbonate having the composition shown in the formula (wherein 0 < x ≤ 0.15 is satisfied, and M represents Ca or Ba).
17. Formula: (1-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xCs 2 CO 3 A carbonate having the composition shown in the formula (wherein 0 < x ≤ 0.07).
18. Formula: 0.07MCO 3 -(0.93-x)(0.476Li 2 CO 3 -0.279Na 2 CO 3 -0.245K 2 CO 3 ) - xCs 2 CO 3 A carbonate having the composition shown in the formula (wherein 0 ≤ x ≤ 0.07 is satisfied, and M represents Ca or Ba).