Oil-resistant sheet

The oil-resistant sheet, made with hardwood pulp, wax, and resins, addresses the issue of inadequate edge resistance in food cups and packaging by providing comprehensive oil and water resistance, enhancing product integrity.

WO2026234989A1PCT designated stage Publication Date: 2026-11-12OJI HLDG CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/015927
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-21
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing oil-resistant sheets, such as those used in food cups and packaging, fail to provide adequate oil and water resistance on the sides and edges, leading to seepage and appearance issues.

Method used

An oil-resistant sheet composed of a paper substrate containing hardwood pulp, wax, and at least one of an olefin resin and a urethane resin, with specific ratios and distributions of components to enhance oil and water resistance on the surface and sides.

Benefits of technology

The sheet achieves excellent oil resistance on the surface and sides, as well as water resistance on the sides, preventing seepage and maintaining product appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026015927_12112026_PF_FP_ABST
    Figure JP2026015927_12112026_PF_FP_ABST
Patent Text Reader

Abstract

An oil-resistant sheet 10 consists of a paper substrate 11 containing: pulp; wax; and at least one of an olefin resin and a urethane resin. The pulp includes hardwood pulp. The basis weight of the paper substrate 11 is 150-1000 g / m2. The density of the paper substrate 11 is 0.6-1.0 g / cm3. The content (α) of the wax is 0.5-10 mass% relative to the total mass of the paper substrate 11. The ratio (α / β) of content (α) to content (β) of the wax in regions S11 and S12, which are up to 20 µm from surfaces 11a and 11b of the paper substrate, 11 is 0.5 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Oil-resistant sheet

[0001] This invention relates to an oil-resistant sheet. This application claims priority based on Japanese Patent Application No. 2025-078719, filed in Japan on May 9, 2025, the contents of which are incorporated herein by reference.

[0002] Paper food cups are used as containers for bento boxes and prepared foods such as pasta, curry, and fried rice. Paper food cups are made, for example, by using a laminated sheet made by laminating polyethylene onto a paper base to form a heat-seal layer, shaping the laminated sheet into a cylinder with the heat-seal layer on the inside, and joining the body, which is made by heat-sealing the overlapping parts, to the bottom. Because the inside of the food cup obtained in this way is laminated with polyethylene, it has oil resistance and water resistance.

[0003] Furthermore, oil-resistant paper, which is made by coating a paper base material with an oil-resistant agent to provide oil resistance, is used as packaging paper for wrapping foods such as hamburgers. Patent Document 1 discloses a water-based oil-resistant agent containing one or more resins selected from specific olefin resins and specific urethane resins, and paraffin wax.

[0004] Japanese Patent Publication No. 2022-188338

[0005] However, when food is stored in food cups, oils and other substances from the food can seep into the edges of the overlapping portions (sealed areas) of the laminated sheets on the inside of the food cup. These seeped areas can appear as streaks, affecting the appearance of the product. Even if an oil-resistant agent is coated onto a paper substrate, while it provides excellent oil resistance to the inner surface of the food cup, it is difficult to sufficiently prevent oil and moisture from seeping into the edges of the sealed area. Thus, the oil and water resistance of the sides (cross-section) of oil-resistant sheets has not been studied to date. The present invention aims to provide an oil-resistant sheet that is excellent in oil resistance on the surface and sides, and in water resistance on the sides.

[0006] The present invention has the following aspects: [1] An oil-resistant sheet made of a paper substrate comprising pulp, wax, and at least one of an olefin resin and a urethane resin, wherein the pulp comprises hardwood pulp, and the basis weight of the paper substrate is 150 to 1000 g / m² 2 The density of the paper substrate is 0.6 to 1.0 g / cm³. 3 [1] An oil-resistant sheet wherein the content of the wax (α) relative to the total mass of the paper substrate is 0.5 to 10% by mass, and the ratio of the content (α) to the content (β) of the wax in the region from the surface of the paper substrate up to 20 μm is 0.5 or more. [2] The oil-resistant sheet according to [1], wherein the wax comprises paraffin wax. [3] The oil-resistant sheet according to [1] or [2], wherein the disintegration-freeness of the pulp is 450 mL or less. [4] The oil-resistant sheet according to any one of [1] to [3], wherein the paper substrate further comprises poly(meth)acrylamide. [5] The oil-resistant sheet according to any one of [1] to [4], wherein the paper substrate is multilayer-formed with three or more layers. [6] The oil-resistant sheet according to any one of [1] to [5], for use in food cups.

[0007] According to the present invention, it is possible to provide an oil-resistant sheet that has excellent oil resistance on the surface and sides, as well as excellent water resistance on the sides.

[0008] This is a schematic cross-sectional view showing an example of the oil-resistant sheet of the present invention. This is a schematic cross-sectional view showing another example of the oil-resistant sheet of the present invention. This is a schematic perspective view showing an example of a food cup using the oil-resistant sheet of the present invention.

[0009] Hereinafter, an embodiment of the oil-resistant sheet according to the present invention will be described in detail with reference to Figure 1 as appropriate. In this specification, "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid. "(meth)acrylamide" is a general term for acrylamide and methacrylamide. "(meth)allyl" is a general term for allyl and methallyl. "(meth)acrylate" is a general term for acrylate and methacrylate. Furthermore, the "~" indicating a numerical range means that the values ​​described before and after it are included as the lower and upper limits. The numerical ranges of the content, various physical properties, and property values ​​disclosed in this specification can be changed to new numerical ranges by arbitrarily combining their lower and upper limits. In addition, in order to make the features easier to understand, the drawings used in the following description may be enlarged to show characteristic parts for convenience, and the dimensional ratios of each component may differ from those in reality. The materials, dimensions, etc. exemplified in the following description are examples, and the oil-resistant sheet according to the present invention is not limited to them, and can be implemented with appropriate modifications without departing from the gist of the present invention.

[0010] [Oil-resistant sheet] Figure 1 shows an example of the oil-resistant sheet of the present invention. The oil-resistant sheet 10 of this embodiment is made of a paper substrate 11. In this specification, one surface 11a of the paper substrate 11 is also called the "first surface," and the other surface 11b is also called the "second surface." In addition, the surface 11c of the paper substrate 11 that is perpendicular to the first surface 11a and the second surface 11b is also called the "side surface."

[0011] <Paper Substrate> The paper substrate 11 shown in Figure 1 is a single-layer paper made from one layer. The paper substrate 11 contains pulp, wax, and at least one of olefin resin and urethane resin. Preferably, the paper substrate 11 further contains poly(meth)acrylamide. The paper substrate 11 may further contain components other than pulp, wax, olefin resin, urethane resin, and poly(meth)acrylamide (hereinafter also referred to as "optional components") as needed, as long as it does not impair the effects of the present invention.

[0012] (Pulp) The pulp includes hardwood pulp. The inclusion of hardwood pulp provides excellent design qualities for printing. Hardwood pulp can be any pulp made from hardwoods, and its manufacturing method is not particularly limited. Examples of hardwood pulp include chemical pulps such as bleached hardwood kraft pulp (LBKP) and bleached hardwood sulfite pulp (LBSP). Other examples include unbleached pulps, semi-bleached pulps, and bleached pulps such as stone ground pulp (GP), pressure stone ground pulp (PGW), refiner ground pulp (RGP), chemigland pulp (CGP), thermomechanical pulp (TMP), and chemothermetic pulp (CTMP). Sulfite pulp and recycled paper pulp are also examples. Hardwood pulp may be used alone or in combination of two or more types.

[0013] The pulp may further contain pulps other than hardwood pulp (hereinafter also referred to as "other pulps"). Examples of other pulps include softwood pulp, non-wood pulp (such as hemp pulp), and synthetic pulp. Other pulps may be used individually or in combination of two or more types.

[0014] As for other types of pulp, softwood pulp is preferred because it increases tear strength. Softwood pulp can be made from softwood as a raw material, and its manufacturing method is not particularly limited. Examples include chemical pulps such as bleached softwood kraft pulp (NBKP) and bleached softwood sulfite pulp (NBSP). Other examples include unbleached pulps, semi-bleached pulps, and bleached pulps such as stone ground pulp (GP), pressure stone ground pulp (PGW), refiner ground pulp (RGP), chemigland pulp (CGP), thermomechanical pulp (TMP), and chemothermetic pulp (CTMP). Sulfite pulp and recycled paper pulp are also examples. Softwood pulp may be used alone or in combination of two or more types.

[0015] The hardwood pulp content is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and may be 100% by mass, based on the total mass of the pulp. If the pulp contains other pulps, the hardwood pulp content is preferably 90% by mass or less, and more preferably 80% by mass or less, based on the total mass of the pulp.

[0016] In the paper substrate 11, it is preferable that the content of hardwood pulp is 50 to 100% by mass and the content of softwood pulp is 0 to 50% by mass relative to the total mass of pulp, more preferably that the content of hardwood pulp is 60 to 100% by mass and the content of softwood pulp is 0 to 40% by mass, and even more preferably that the content of hardwood pulp is 70 to 100% by mass and the content of softwood pulp is 0 to 30% by mass.

[0017] The mass ratio expressed as [hardwood pulp content] / [softwood pulp content] is preferably 0.1 to 9, and more preferably 0.25 to 4. If the mass ratio is above the lower limit, the surface properties of the paper will be improved. If the mass ratio is below the upper limit, the strength will be improved.

[0018] The pulp may be dry pulp or wet pulp, but wet pulp is preferred from the viewpoint of increasing the tensile modulus of the paper substrate 11. Here, dry pulp is pulp whose moisture content has been adjusted to 3 to 10% by mass by drying. On the other hand, wet pulp is pulp whose moisture content has been adjusted to 40 to 60% by mass by drying. The moisture content of the pulp is a value measured in accordance with JIS P 8127:2010.

[0019] The Canadian standard freeness of the pulp (hereinafter also referred to as "disintegration freeness") is preferably 450 mL or less, more preferably 200 to 450 mL, and even more preferably 250 to 400 mL. When the disintegration freeness of the pulp is equal to or higher than the above lower limit, the tear strength of the paper base material 11 tends to be high, and the processability tends to be excellent. When the disintegration freeness of the pulp is equal to or lower than the above upper limit, the wax described later is more likely to remain in the paper base material 11, and the oil resistance is further improved. In particular, the oil resistance at the end face 31c of the overlapping portion (seal portion) H (hereinafter also referred to as "cross-sectional oil resistance") when the oil-resistant sheet 10 is processed into a cup shape as shown in, for example, FIG. 3 is further improved. The disintegration freeness of pulp is measured by the following method. That is, for the disintegrated pulp obtained by subjecting the paper base material 11 to disintegration treatment in accordance with JIS P 8220-1:2012 using a standard disintegrator, the freeness is measured in accordance with JIS P 8121-2:2012 using a Canadian standard freeness tester, and the measured freeness is defined as the disintegration freeness of the pulp. The disintegration freeness can be adjusted by the beating degree of the pulp.

[0020] The content of pulp in the paper base material 11 is preferably 89.9 to 99 mass%, more preferably 93 to 98.5 mass%, and even more preferably 95 to 98 mass%, relative to the total mass of the paper base material 11. The masses of the paper base material 11 and the pulp are absolute dry masses. The absolute dry mass is measured in accordance with JIS P 8203:2010. The total content of the pulp, the wax, olefin resin, urethane resin, poly(meth)acrylamide and optional components described later does not exceed 100 mass% relative to the total mass of the paper base material 11.

[0021] (Wax) The paper substrate 11 contains wax. The inclusion of wax provides excellent oil resistance on the surface and sides, as well as water resistance on the sides. Examples of waxes include paraffin wax, carboxyl group-containing paraffin wax, microcrystalline wax, polyethylene wax, carboxyl group-containing polyethylene wax, polypropylene wax, polyolefin waxes such as ethylene-propylene copolymer wax, candelilla wax, rice wax, montan wax, fatty acids such as stearic acid, fatty acid amides such as stearic acid amide, stearate bisamide, oleic acid amide, palmitic acid amide, fatty acid metal salts such as zinc stearate and calcium stearate, hydrogenated castor oil, rice wax, carnauba wax, hydrogenated palm oil, hydrogenated soybean oil, and fatty acid ester waxes such as beeswax. Among these, paraffin wax, carboxyl group-containing paraffin wax, and fatty acid ester waxes are preferred from the viewpoint of further improving oil resistance, with paraffin wax being more preferred. The wax may be used alone, or two or more may be used in combination.

[0022] It is preferable to use a wax that has been made into an aqueous emulsion using a dispersant. Examples of dispersants include nonionic surfactants, cationic surfactants, anionic surfactants, etc., as described in Japanese Patent Application Publication No. 2013-237941. The dispersant may be used alone or in combination of two or more types.

[0023] Paraffin wax is obtained by subjecting crude oil to reduced-pressure distillation, and separating and purifying hydrocarbons with good crystallinity from the resulting distillate. Paraffin wax is mainly composed of linear hydrocarbons (normal paraffins). As the paraffin wax, a synthetic product may be used, or a commercially available product may be used. Examples of solid commercially available paraffin wax products include, for example, trade names "Paraffin 115", "Paraffin 120", "Paraffin 125", "Paraffin 130", "Paraffin 135", "Paraffin 140", "Paraffin 145", "Paraffin 150", "Paraffin 155", "HNP-51" and the like manufactured by Nippon Seiro Co., Ltd. Paraffin wax may be used singly, or two or more types may be used in combination.

[0024] The content of the paraffin wax is preferably 50 mass% or more, more preferably 60 mass% or more, further preferably 70 mass% or more, and may be 100 mass%, relative to the total mass of the wax.

[0025] The melting point of the wax is preferably 40°C to 120°C, more preferably 40°C to 100°C, further preferably 45°C to 80°C, and particularly preferably 55°C to 80°C. When the melting point of the wax is not less than the above lower limit value, oil resistance can be more sufficiently easily exhibited even against high-temperature foods during actual use of the oil-resistant sheet 10. When the melting point of the wax is not more than the above upper limit value, the wax melts and spreads uniformly by heating during production, whereby more excellent oil resistance is easily obtained. The melting point of the wax is a value measured by the DSC method in accordance with JIS K 7121:2012. When a commercially available product is used as the wax, the catalog value may be adopted as the melting point for products that have a catalog value.

[0026] The content of the wax in the paper base material 11 is 0.5 to 10 mass%, preferably 0.6 to 5 mass%, more preferably 0.8 to 3 mass%, and further preferably 1 to 2 mass%, relative to the total mass of the paper base material 11. When the wax content is at least the above lower limit value, the oil resistance, particularly the cross-sectional oil resistance, is excellent. When the wax content is not more than the above upper limit value, excessive slipperiness caused by the wax is less likely to occur.

[0027] Furthermore, when the wax content in the paper substrate 11 is denoted as "content (α)" and the wax content in the region from the surface of the paper substrate 11 up to 20 μm is denoted as "content (β)", the ratio of content (α) to content (β) (α / β) is 0.5 or more. α / β is preferably 0.5 to 5, more preferably 0.7 to 3, and even more preferably 0.9 to 1.1. Specifically, as shown in Figure 1, when the wax content (β) in region (S11) relative to the total mass of the region (S11) from the first surface 11a to 20 μm of the paper substrate 11 is denoted as "content (β11)", the ratio of content (α) to content (β11) (α / β11) is 0.5 or more, preferably 0.5 to 5, more preferably 0.7 to 3, and even more preferably 0.9 to 1.1. Furthermore, when the content (β) of wax in the region (S12) relative to the total mass of the region (S12) from the second surface 11b of the paper substrate 11 to 20 μm is defined as "content (β12)", the ratio of content (α) to content (β12) (α / β12) is 0.5 or more, preferably 0.5 to 5, more preferably 0.7 to 3, and even more preferably 0.9 to 1.1. If the ratio (α / β), ratio (α / β11), and ratio (α / β12) are all within the above ranges, the wax is uniformly dispersed in the paper substrate 11. In particular, if the ratio (α / β), ratio (α / β11), and ratio (α / β12) are all above the lower limit, the wax is evenly distributed throughout the interior of the paper substrate 11, further improving the oil resistance of the cross-section. If the ratios (α / β), (α / β11), and (α / β12) are each below the above upper limit, the presence of wax on the surface of the paper substrate 11 makes it easier to obtain surface oil resistance.

[0028] (Olefin resin and urethane resin) The paper substrate 11 contains at least one of an olefin resin and a urethane resin. The inclusion of at least one of an olefin resin and a urethane resin provides excellent oil resistance to the surface and sides. (Olefin resin) Examples of olefin resins include homopolymers or copolymers of olefins, copolymers of olefins and other monomers, etc. Examples of olefins include compounds consisting only of carbon atoms and hydrogen atoms and having at least one double bond in the molecule. Among these, monoolefins having one double bond in the molecule are preferred. Examples of monoolefins include ethylene, propylene, 1-butene, 2-butene, 1-pentene, 2-pentene, 1-hexene, 2-hexene, 3-hexene, 1-heptene, 2-heptene, 3-heptene, 1-octene, 2-octene, 3-octene, 4-octene, isooctene, 1-decene, 2-decene, 3-decene, 4-decene, 1-dodecene, 2-dodecene, 3-dodecene, 1-tetradecene, 2-tetradecene, 3-tetradecene, 1- Linear olefins such as hexadecene, 2-hexadecene, 3-hexadecene, 1-octadecene, 2-octadecene, 3-octadecene, 1-eicosene, 1-tetracosene, and 1-triaconthene; 2-methylpropene (isobutene), 2,4,4-trimethyl-1-pentene, 2,4,4-trimethyl-2-pentene, and mixtures of 2,4,4-trimethyl-1-pentene and 2,4,4-trimethyl-2-pentene (hereinafter also referred to as "diisobutylene").Branched olefins such as 2-methyl-1-butene, 3-methyl-1-butene (isopentene), 2-methyl-1-pentene, 2-ethyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene (isohexene), 2-ethyl-1-pentene, 3-ethyl-1-pentene, 2-methyl-3-ethyl-1-pentene, 2-methyl-1-hexene, 3-methyl-1-hexene, 4-methyl-1-hexene, 2-ethyl-1-hexene, 3-ethyl-1-hexene, 2-methyl-1-octene, 3-methyl-1-octene; cyclic olefins such as cyclohexene, methylcyclohexene, vinylcyclohexane, 4-vinylcyclohexene, cyclopentene, and methylcyclopentene; and isomers of these olefins (cis and trans forms). Among these, monoolefins having 2 to 20 carbon atoms are preferred, and monoolefins having 4 to 20 carbon atoms are more preferred. In particular, from the viewpoint of further improving oil resistance, it is even more preferable to combine monoolefins having 4 to 10 carbon atoms with monoolefins having 12 to 20 carbon atoms, and it is especially preferable to combine monoolefins having 6 to 8 carbon atoms with monoolefins having 15 to 20 carbon atoms.

[0029] Other monomers are not particularly limited as long as they can copolymerize with olefins, but examples include α,β-unsaturated carboxylic acids, α,β-unsaturated monocarboxylate alkyl esters, and other polymerizable monomers (hereinafter also referred to as "other polymerizable monomers"). Among these, α,β-unsaturated carboxylic acids are preferred from the viewpoint of further improving oil resistance. Other monomers may be used individually or in combination of two or more.

[0030] Examples of α,β-unsaturated carboxylic acids include α,β-unsaturated dicarboxylic acids such as maleic acid, itaconic acid, fumaric acid, muconic acid, and citraconic acid; α,β-unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid; acid anhydrides of the unsaturated dicarboxylic acids, acid anhydrides of the unsaturated monocarboxylic acids, monoalkyl esters of the unsaturated dicarboxylic acids, and monoalkylamides of the unsaturated dicarboxylic acids. Among these, maleic anhydride is preferred. Examples of alkyl groups for monoalkyl esters of unsaturated dicarboxylic acids and monoalkylamides of unsaturated dicarboxylic acids include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, n-pentyl, isopentyl, n-hexyl, cyclohexyl, n-octyl, (2-ethylhexyl) group, n-decyl, n-dodecyl, n-tetradecyl, n-hexadecyl, n-octadecyl, n-nonadecyl, n-eicosyl, and n-docosyl groups. The α,β-unsaturated carboxylic acid may be used alone or in combination of two or more types.

[0031] α,β-unsaturated carboxylic acids may also be used in the form of neutralized salts. Examples of neutralized salts include alkali metal salts such as sodium salts and potassium salts; and ammonium salts. When preparing neutralized salts, examples of alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; inorganic amines such as ammonia and ammonium carbonate; alkylamines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, and n-butylamine; cycloalkylamines such as cyclohexylamine; and aromatic amines such as aniline can be used. These may be used individually or in combination of two or more.

[0032] Examples of α,β-unsaturated monocarboxylate alkyl esters include monoalkyl esters of α,β-unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid. Examples of alkyl groups in α,β-unsaturated monocarboxylate alkyl esters include alkyl groups having 1 to 20 carbon atoms. Examples of alkyl groups in α,β-unsaturated monocarboxylate alkyl esters include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, s-butyl group, t-butyl group, n-pentyl group, isopentyl group, neopentyl group, cyclopentyl group, n-hexyl group, isohexyl group, cyclohexyl group, n-heptyl group, isoheptyl group, n-octyl group, isooctyl group, n-nonyl group, isononyl group, n-decyl group, isodecyl group, n-undecyl group, n-dodecyl group, n-tridecyl group, n-tetradecyl group, n-pentadecyl group, n-hexadecyl group, n-heptadecyl group, n-octadecyl group, n-nonadecyl group, n-eicosyl group, and n-docosyl group. Among these, alkyl groups having 1 to 10 carbon atoms are preferred, and alkyl groups having 1 to 5 carbon atoms are more preferred. The α,β-unsaturated monocarboxylate alkyl ester may be used alone or in combination of two or more types.

[0033] Other polymerizable monomers (excluding α,β-unsaturated carboxylic acids and α,β-unsaturated monocarboxylate alkyl esters) include, for example, the following compounds: styrenes such as styrene, α-methylstyrene, t-butylstyrene, dimethylstyrene, acetoxystyrene, hydroxystyrene, vinyltoluene, and chlorovinyltoluene; (meth)acrylic acid esters having hydroxyl groups such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, glycerin mono(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol mono(meth)acrylate, and pentaerythritol di(meth)acrylate; (meth)acrylate aminoalkyls such as (meth)acrylate aminoethyl, (meth)acrylate aminopropyl, (meth)acrylate aminobutyl, (meth)acrylate N-methylaminoethyl, (meth)acrylate N-methylaminopropyl, (meth)acrylate N-methylaminobutyl, (meth)acrylate N,N-dimethylaminoethyl, (meth)acrylate N,N-dimethylaminopropyl, (meth)acrylate N,N-dimethylaminobutyl, (meth)acrylate N,N-diethylaminoethyl, (meth)acrylate N,N-diethylaminopropyl, (meth)acrylate N,N-diethylaminobutyl; monomers having a sulfo group, such as styrene sulfonic acid, α-methylstyrene sulfonic acid, vinyl sulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamide-N-methylsulfonic acid, (meth)acrylamide phenylpropanesulfonic acid, (meth)allylsulfonic acid, (meth)ethyl methacrylate, (meth)sulfopropyl methacrylate, and (meth)sulfo-2-hydroxypropyl methacrylate; divinyl esters such as divinyl adipate and divinyl sebacate; polyethylene glycol mono(meth)acrylates such as diethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, and tetraethylene glycol mono(meth)acrylate;Polyethylene glycol di(meth)acrylates such as ethylene glycol di(meth)acrylate and diethylene glycol di(meth)acrylate; polyalkylene glycol mono(meth)acrylates such as polypropylene glycol mono(meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, polytrimethylene glycol mono(meth)acrylate, polytetramethylene glycol mono(meth)acrylate, polyethylene glycol propylene glycol mono(meth)acrylate; (meth)acrylamide, N-methylol(meth)acrylamide, N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, N-octyl(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-ethoxymethyl(meth)acrylamide, N-propoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, N-2-hydroxyethyl(meth)acrylamide, N,N-dihydroxyethyl (meth)acrylamides such as (meth)acrylamide, N-(1,1-dimethyl-3-oxobutyl)acrylamide, N-allyl(meth)acrylamide, (meth)acrylamide glycolic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-diallyl(meth)acrylamide, N,N'-methylenebis(meth)acrylamide, N,N'-ethylenebis(meth)acrylamide; aromatic polyvinyls such as divinylbenzene, 1,3,5-triacryloylhexahydro-1,3,5-triazine, triallyl isocyanurate, triallyl trimellitate, triallylamine, tetramethylolmethane tetraacrylate, tetraallyl pyromellate; acrylonitrile, etc. Other polymerizable monomers may be used individually or in combination of two or more.

[0034] The content of monoolefin-derived structural units is preferably 20 to 70% by mass, and more preferably 30 to 60% by mass, relative to the total mass of the olefin resin. If the content of monoolefin-derived structural units is above the lower limit, oil resistance is improved. If the content of monoolefin-derived structural units is below the upper limit, air permeability is improved. The content of monoolefin-derived structural units having 4 to 10 carbon atoms is preferably 5 to 30% by mass, and more preferably 10 to 25% by mass, relative to the total mass of the olefin resin. If the content of monoolefin-derived structural units having 4 to 10 carbon atoms is above the lower limit, dispersibility and uniformity are improved. If the content of monoolefin-derived structural units having 4 to 10 carbon atoms is below the upper limit, oil resistance is improved. The content of monoolefin-derived structural units having 12 to 20 carbon atoms is preferably 10 to 45% by mass, and more preferably 15 to 35% by mass, relative to the total mass of the olefin resin. If the content of constituent units derived from monoolefins with 12 to 20 carbon atoms is above the lower limit, oil resistance will be improved. If the content of constituent units derived from monoolefins with 12 to 20 carbon atoms is below the upper limit, air permeability will be improved.

[0035] The mass ratio expressed as [content of constituent units derived from monoolefins having 4 to 10 carbon atoms] / [content of constituent units derived from monoolefins having 12 to 20 carbon atoms] is preferably 0.2 to 3, and more preferably 0.3 to 2. If the mass ratio is above the lower limit, the dispersibility of the resin is improved. If the mass ratio is below the upper limit, the oil resistance is improved.

[0036] The mass ratio expressed as (content of constituent units derived from monoolefins + content of constituent units derived from α,β-unsaturated monocarboxylate alkyl esters) / (content of constituent units derived from α,β-unsaturated dicarboxylic acids) is more preferably 0.8 to 3.5. If the mass ratio is above the lower limit, oil resistance is improved. If the mass ratio is below the upper limit, air permeability is improved.

[0037] Specific examples of olefin resins include ethylene homopolymers (polyethylene) or copolymers, propylene homopolymers (polypropylene) or copolymers, and olefin homopolymers or copolymers having four or more carbon atoms. One embodiment of an ethylene copolymer or propylene copolymer is ethylene-propylene copolymer, ethylene-1-butene copolymer, propylene-4-methyl-1-pentene copolymer, and propylene-ethylene-1-butene copolymer.

[0038] Examples of homopolymers of olefins having four or more carbon atoms include poly(1-butene), poly(3-methyl-1-butene), poly(3-methyl-1-pentene), poly(4-methyl-1-pentene), and polyvinylcyclohexane. Examples of copolymers of olefins having four or more carbon atoms include copolymers of an olefin having four or more carbon atoms (hereinafter also referred to as "(m1-1) component") and an α,β-unsaturated carboxylic acid (hereinafter also referred to as "(m1-2) component") (hereinafter also referred to as "polymer (P1)"). That is, copolymer (P1) has constituent units derived from the (m1-1) component and constituent units derived from the (m1-2) component.

[0039] The copolymer (P1) may, in addition to the constituent units derived from component (m1-1) and component (m1-2), further optionally have constituent units derived from an α,β-unsaturated monocarboxylate alkyl ester (hereinafter also referred to as "component (m1-3)") and constituent units derived from another polymerizable monomer (hereinafter also referred to as "component (m1-4)"). That is, the copolymer (P1) may be a copolymer of component (m1-1), component (m1-2), and at least one of component (m1-3) and component (m1-4).

[0040] The content of constituent units derived from component (m1-1) is preferably 20 to 70% by mass, and more preferably 30 to 60% by mass, relative to the total mass of all units constituting the copolymer (P1). Similarly, the content of constituent units derived from component (m1-2) is preferably 10 to 50% by mass, and more preferably 20 to 40% by mass. The content of constituent units derived from component (m1-3) is preferably 20% by mass or less, and more preferably 1 to 10% by mass. The content of constituent units derived from component (m1-4) is preferably 10% by mass or less, and more preferably 5% by mass or less.

[0041] The weight-average molecular weight of the olefin resin is preferably 1,000 to 500,000, and more preferably 5,000 to 50,000. The weight-average molecular weight of the olefin resin is a polystyrene equivalent value measured by gel permeation chromatography (GPC).

[0042] Olefin resins are obtained by reacting the monomer components constituting the resin in a solvent in the presence of a polymerization initiator. Examples of solvents include aromatic hydrocarbons such as benzene, toluene, ethylbenzene, n-propylbenzene, t-butylbenzene, o-xylene, m-xylene, p-xylene, tetralin, decalin, and aromatic naphtha; esters such as ethyl acetate, n-butyl acetate, n-amyl acetate, 2-hydroxyethyl acetate, 2-butoxyethyl acetate, 3-methoxybutyl acetate, and methyl benzoate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, isophorone, cyclohexanone, and methylcyclohexanone; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, s-butanol, and t-butanol; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; and water such as deionized water, purified water, tap water, soft water, hard water, and industrial water. The solvent may be used alone, or two or more solvents may be used in combination.

[0043] These solvents may be added during the reaction. Furthermore, if a solvent other than water is used, it is preferable to remove the solvent from the reaction system by vacuum distillation or the like at the end of the reaction. The amount of solvent used should preferably be adjusted so that the concentration of the reaction solution is 10 to 80% by mass.

[0044] Examples of polymerization initiators include persulfates such as ammonium persulfate, potassium persulfate, and sodium persulfate; azo compounds such as 2,2'-azobis(2-amidinopropane) hydrochloride, 2,2'-azobis[2(2-imidazolin-2-yl)propane] hydrochloride, 2,2'-azobisisobutyronitrile, and dimethyl-2,2'-azobisisobutyrate; organic peroxides such as benzoyl peroxide, dicumyl peroxide, and lauryl peroxide; and hydrogen peroxide. In addition, reducing agents such as sodium sulfite and sodium thiosulfate may be used in combination with the polymerization initiators, and the reaction system may be redox. The polymerization initiator may be used alone or in combination of two or more.

[0045] The amount of polymerization initiator used is preferably 0.01 to 5 parts by mass, and more preferably 0.05 to 3 parts by mass, per 100 parts by mass of the total monomer components.

[0046] A chain transfer agent may be used in the above reaction. Examples of chain transfer agents include alkyl mercaptans such as n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, n-hexadecyl mercaptan, and n-octadecyl mercaptan; and 2-mercaptobenzothiazole, bromotrichloromethane, and α-methylstyrene dimer. The chain transfer agent may be used alone or in combination of two or more.

[0047] The amount of chain transfer agent used is preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, per 100 parts by mass of the total monomer components.

[0048] The reaction conditions are not particularly limited, but for example, the reaction temperature is preferably 40 to 150°C, and more preferably 60 to 120°C. The reaction time is preferably 1 to 10 hours, and more preferably 1 to 3 hours.

[0049] In the above reaction, inorganic acids such as sulfuric acid and phosphoric acid; alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; inorganic amines such as ammonia and ammonium carbonate; alkylamines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, and n-butylamine; cycloalkylamines such as cyclohexylamine; and aromatic amines such as aniline may be added before, during, or after the reaction, as needed. Furthermore, it is preferable to carry out the reaction under a nitrogen atmosphere.

[0050] The olefin resin content in the paper substrate 11 is preferably 0.1 to 8% by mass, more preferably 0.3 to 6% by mass, and even more preferably 0.5 to 4% by mass, based on the total mass of the paper substrate 11. If the olefin resin content is above the lower limit mentioned above, the oil resistance will be further improved.

[0051] (Urethane Resin) Urethane resin is a polymer compound having urethane bonds in its molecule, and is typically obtained by the reaction of a polyol (hereinafter also referred to as "(m2-1) component") and a polyisocyanate (hereinafter also referred to as "(m2-2) component"). When reacting component (m2-1) and component (m2-2), it is preferable to use a chain extender (hereinafter also referred to as "(m2-3) component"). Furthermore, when reacting component (m2-1) and component (m2-2), one or more selected from (meth)acrylate hydroxyalkyl ester (hereinafter also referred to as "(m2-4) component"), (meth)acrylate monoalkyl ester without a hydroxyl group (hereinafter also referred to as "(m2-5) component"), and chain extension inhibitor (hereinafter also referred to as "(m2-6) component") may be used in combination. In other words, the urethane resin is typically a polymer obtained by reacting component (m2-1) and component (m2-2), and a polymer obtained by reacting component (m2-1), component (m2-2), component (m2-3), and optionally one or more components selected from component (m2-4), component (m2-5), and component (m2-6) is preferred.

[0052] The polyol component (m2-1) is a compound having two or more hydroxyl groups in one molecule. Examples of components (m2-1) include polyether polyols, poly(meth)acrylic polyols, polycaprolactone polyols, and polycarbonate polyols. Among these, polyether polyols are preferred. Component (m2-1) may be used alone or in combination of two or more.

[0053] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polybutylene glycol, polytetramethylene glycol, polyhexamethylene glycol, polyheptamethylene glycol, polydecamethylene glycol, polyoxyethylene-polyoxypropylene glycol, polyoxytetramethylene-polyoxyethylene glycol, and polyoxytetramethylene-polyoxypropylene glycol. The structure of the polyether polyol may be random or blocky. The polyether polyol may be used alone or in combination of two or more types.

[0054] As the polyether polyol, synthetic products or commercially available products may be used. Examples of commercially available polyether polyols include: "ADEKA Polyether P-400", "ADEKA Polyether G-400", "ADEKA Polyether T-400", "ADEKA Polyether AM-302", "ADEKA Polyether P1000", and "ADEKA Polyether P2000" from ADEKA Corporation; "Polyethylene Glycol #1,540" from Nakalai Tesque Co., Ltd.; "Dipropylene Glycol" and "Polypropylene Glycol 400" from Junsei Chemical Co., Ltd.; and "PEG #200", "PEG #300", "PEG #400", "PEG #600", and "PEG #10" from NOF Corporation. Examples include "00", "PEG#1500", "PEG#2000", "PEG#4000", "Uniol D-200", "Uniol D-700", "Uniol D-1000", "Uniol D-1200", "Uniol D-2000", "Uniol D-4000", "Uniol PB-500", "Uniol PB-700", "Uniol PB-1000", "Uniol PB-2000", "Polycerin DC-1100", "Polycerin DC-1800E", "Polycerin DC-3000E", "Polycerin DCB-1000", "Polycerin DCB-2000", and "Polycerin DCB-4000".

[0055] The content of constituent units derived from component (m2-1) is preferably 30 to 70% by mass, and more preferably 40 to 65% by mass, relative to the total mass of the urethane resin.

[0056] (m2-2) The polyisocyanates include, for example, aliphatic diisocyanates such as methylene diisocyanate, isopropyl diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and dimer diisocyanates in which the carboxyl group of the dimer acid is replaced with an isocyanate group; and cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-di(isocyanate methyl)cyclohexane, and methylcyclohexane diisocyanate. Alicyclic diisocyanates; aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-diphenyltetramethylmethane diisocyanate, 1,4-phenylenediisocyanate, tolylene diisocyanate, xylylene diisocyanate, m-tetramethylxylylene diisocyanate, 1,5-naphthylene diisocyanate, 4,4'-dibenzylendiisocyanate, and 1,3-phenylenediisocyanate; amino acid diisocyanates such as lysine diisocyanate; and their nurates (isocyanurates, trimers), adducts (trimers), or biuretes (trimers). Component (m2-2) may be used alone or in combination of two or more.

[0057] The content of constituent units derived from component (m2-2) is preferably 10 to 40% by mass, and more preferably 15 to 35% by mass, relative to the total mass of the urethane resin.

[0058] The ratio of components (m2-1) and (m2-2) used is not particularly limited, but it is preferable that the ratio (NCO / OH) of the number of moles of isocyanate groups (NCO) of component (m2-2) to the number of moles of hydroxyl groups (OH) of component (m2-1) be about 1.1 / 1 to 8 / 1. The molar ratio expressed as [constituent units derived from component (m2-2)] / [constituent units derived from component (m2-1)] is preferably 1.1 to 8, and more preferably 2 to 4. If the molar ratio is above the lower limit, the adhesion of the urethane resin to the paper substrate will be improved. If the molar ratio is below the upper limit, the flexibility of the urethane resin will be improved.

[0059] (m2-3) Examples of chain extenders include diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, triethylenetetramine, diethylenetriamine, isophoronediamine, dimeramine, dicyclohexylmethane-4,4'-diamine, 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine; triamines such as diethylenetriamine, dipropylenetriamine, dibutylenetriamine; tetramines such as triethylenetetramine, tripylenetetramine; N-methyldiethanolamine, N-ethyldiethanolamine, N-propyldiethanolamine, N-isopropyl Examples include N-alkyldialkanolamines such as didiethanolamine, N-butyldiethanolamine, N-isobutyldiethanolamine, N-oleyldiethanolamine, N-stearyldiethanolamine, N-methyldiisopropanolamine, N-ethyldiisopropanolamine, N-propyldiisopropanolamine, and N-butyldiisopropanolamine; hydrazine or its hydrazine derivatives (such as adipic acid hydrazide); dialkanolalkanoic acids such as glyceric acid, dioxymaleic acid, dioxyfumaric acid, dimethylolacetic acid, dimethylolpropionic acid, dimethylolbutanoic acid, dimethylolpentanoic acid, and dimethylolhexanoic acid; and aromatic hydroxycarboxylic acids such as 4,4-di(hydroxyphenyl)butanoic acid, 4,4-di(hydroxyphenyl)pentanoic acid, and 2,6-dioxybenzoic acid. Among these, dialkanolalkanoic acids are preferred. The (m2-3) component may be used alone or in combination of two or more types.

[0060] The N-alkyldialkanolamine may also be used in the form of its quaternized salt. The quaternized salt refers to the N-alkyldialkanolamine that has reacted with a quaternizing agent. Examples of quaternizing agents include inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid; organic acids such as dimethyl sulfuric acid, acetic acid, and propionic acid; and organic halogens such as methyl chloride, benzyl chloride, and epichlorohydrin.

[0061] The aforementioned dialkanolalkanoic acid and aromatic hydroxycarboxylic acid may each have their carboxyl groups neutralized with a neutralizing agent. Examples of neutralizing agents include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; ammonia; and organic amines such as trimethylamine, triethylamine, triethanolamine, triisopropanolamine, N,N-dimethylethanolamine, and N,N-diethylethanolamine. The neutralizing agent may be used alone or in combination of two or more.

[0062] The amount of component (m2-3) used is preferably 1 to 30% by mass, and more preferably 3 to 20% by mass, relative to the total mass of all components constituting the urethane resin. The content of constituent units derived from component (m2-3) is preferably 1 to 30% by mass, and more preferably 3 to 20% by mass, relative to the total mass of the urethane resin.

[0063] The molar ratio expressed as [constituent units derived from component (m2-2)] / [constituent units derived from component (m2-3)] is preferably 0.5 to 5, and more preferably 1 to 3. If the molar ratio is above the lower limit, the adhesion of the urethane resin to the paper substrate is improved. If the molar ratio is below the upper limit, the flexibility of the urethane resin is improved.

[0064] Examples of the (m2-4) component, a hydroxyalkyl (meth)acrylate, include 2-hydroxyethyl (meth)acrylate, 2-hydroxyn-propyl (meth)acrylate, 3-hydroxyn-propyl (meth)acrylate, 3-hydroxyn-butyl (meth)acrylate, 4-hydroxyn-butyl (meth)acrylate, and 6-hydroxyn-hexyl (meth)acrylate. The (m2-4) component may be used alone or in combination of two or more.

[0065] The amount of component (m2-4) used is preferably 10% by mass or less, and more preferably 5% by mass or less, relative to the total mass of all components constituting the urethane resin.

[0066] Examples of monoalkyl (meth)acrylate esters that do not have a hydroxyl group and are component (m2-5) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, myristyl (meth)acrylate, isomyristyl (meth)acrylate, palmityl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate. Component (m2-5) may be used alone or in combination of two or more.

[0067] The amount of component (m2-5) used is preferably 50% by mass or less, and more preferably 30% by mass or less, relative to the total mass of all components constituting the urethane resin.

[0068] Examples of chain elongation inhibitors that constitute component (m2-6) include monoalcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, and isobutyl alcohol; monoamines such as ethylamine, n-propylamine, diethylamine, di-n-propylamine, and di-n-butylamine; and alkanol monoamines such as monoethanolamine and diethanolamine. Component (m2-6) may be used alone or in combination of two or more.

[0069] The amount of component (m2-6) used is preferably 5% by mass or less, and more preferably 3% by mass or less, relative to the total mass of all components constituting the urethane resin. The constituent units derived from component (m2-6) are preferably 5% by mass or less, and more preferably 3% by mass or less, relative to the total mass of the urethane resin.

[0070] The weight-average molecular weight of the urethane resin is preferably 5,000 to 50,000. The weight-average molecular weight of the urethane resin is a polystyrene equivalent value measured by gel permeation chromatography (GPC).

[0071] The urethane resin can be obtained, for example, by reacting component (a2-1) and component (a2-2) to produce a urethane prepolymer, and then reacting the urethane prepolymer and component (a2-3) with one or more components selected from components (m2-4), (m2-5), and (m2-6) as needed.

[0072] The reaction conditions for obtaining the urethane prepolymer are not particularly limited, but for example, the reaction temperature is preferably 40 to 150°C, and more preferably 60 to 100°C. The reaction time is preferably 1 to 20 hours, and more preferably 1 to 10 hours. The conditions for reacting the urethane prepolymer with components (a2-3), etc., are not particularly limited, but for example, the reaction temperature is preferably 20 to 100°C, and more preferably 30 to 80°C. The reaction time is preferably 1 to 10 hours, and more preferably 1 to 5 hours. The mixing method and mixing order of each component are not particularly limited.

[0073] The production of urethane resin may be carried out in a solvent-free environment or in a solvent. Examples of solvents include aromatic hydrocarbons such as benzene, toluene, ethylbenzene, n-propylbenzene, t-butylbenzene, o-xylene, m-xylene, p-xylene, tetralin, decalin, and aromatic naphtha; aliphatic hydrocarbons such as n-hexane, n-heptane, n-octane, isooctane, and n-decane; alicyclic hydrocarbons such as cyclohexane; esters such as ethyl acetate, n-butyl acetate, n-amyl acetate, 2-hydroxyethyl acetate, 2-butoxyethyl acetate, 3-methoxybutyl acetate, and methyl benzoate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, isophorone, cyclohexanone, and methylcyclohexanone; and ethyl Examples of solvents include glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, s-butanol, and t-butanol; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; amines such as N-methylpyrrolidone; water such as deionized water, purified water, tap water, soft water, hard water, and industrial water; and dimethyl sulfoxide. The solvent may be used alone or in combination of two or more. After the reaction is complete, the solvent may be removed by distillation under reduced pressure. It is preferable to adjust the amount of solvent used so that the concentration of the reaction solution is 10% by mass or more.

[0074] The urethane resin content in the paper substrate 11 is preferably 0.1 to 8% by mass, more preferably 0.3 to 6% by mass, and even more preferably 0.5 to 4% by mass, based on the total mass of the paper substrate 11. If the urethane resin content is above the lower limit mentioned above, the oil resistance will be further improved.

[0075] Furthermore, the total content of olefin resin and urethane resin in the paper substrate 11 is preferably 0.1 to 8% by mass, more preferably 0.3 to 6% by mass, and even more preferably 0.5 to 4% by mass, relative to the total mass of the paper substrate 11. If the total content of olefin resin and urethane resin is above the above lower limit, the oil resistance will be further improved.

[0076] (Poly(meth)acrylamide) Poly(meth)acrylamide is a polymer having (meth)acrylamide units. The inclusion of poly(meth)acrylamide improves the oil resistance of the cross-section. Examples of poly(meth)acrylamide include anionic poly(meth)acrylamide, cationic poly(meth)acrylamide, and amphoteric poly(meth)acrylamide. Poly(meth)acrylamide may be used alone or in combination of two or more types.

[0077] Examples of anionic poly(meth)acrylamides include water-soluble copolymers composed of (meth)acrylamide and anionic monomers, and hydrolyzed poly(meth)acrylamides. Anionic poly(meth)acrylamides may be used alone or in combination of two or more types.

[0078] Examples of anionic monomers that can be used as components of water-soluble copolymers include anionic vinyl monomers such as monocarboxylic acids having unsaturated bonds, dicarboxylic acids having unsaturated bonds, tricarboxylic acids having unsaturated bonds, tetracarboxylic acids having unsaturated bonds, sulfonic acids having unsaturated bonds, phosphonic acids having unsaturated bonds, and their salts. Among these, monomers of (meth)acrylic acid and its salts are preferred. Anionic monomers may be used alone or in combination of two or more. In polymerization of anionic water-soluble copolymers, additives such as chain transfer agents commonly used in polymerization may be added.

[0079] Hydrolyzed poly(meth)acrylamide is a decomposition product obtained by decomposing poly(meth)acrylamide through a conventionally known hydrolysis reaction. Hydrolyzed poly(meth)acrylamide can be obtained, for example, by partially hydrolyzing at least one of a (meth)acrylamide copolymer and a (meth)acrylamide homopolymer by reacting an alkaline substance such as sodium hydroxide with the copolymer, thereby converting the amide groups to carboxyl groups.

[0080] Examples of cationic poly(meth)acrylamides include water-soluble copolymers composed of (meth)acrylamide and cationic monomers, Mannich-modified poly(meth)acrylamides, and Hoffmann-degraded poly(meth)acrylamides. Cationic poly(meth)acrylamides may be used alone or in combination of two or more types.

[0081] Cationic monomers that can be used as components of water-soluble copolymers include, for example, cationic vinyl monomers such as vinyl monomers having a tertiary amino group or a quaternary ammonia group. Cationic monomers may be used alone or in combination of two or more. In polymerization of cationic water-soluble copolymers, additives such as chain transfer agents commonly used in polymerization may be added.

[0082] Mannich-modified poly(meth)acrylamide is a reaction product obtained by modifying poly(meth)acrylamide using the conventionally known Mannich reaction. Mannich-modified poly(meth)acrylamide can be obtained, for example, by reacting at least one of a (meth)acrylamide copolymer and a (meth)acrylamide homopolymer with formaldehyde and a secondary amine, thereby cationizing some of the amide groups. Examples of formaldehyde include aqueous solutions (formalin) and paraformaldehyde. Examples of secondary amines include dimethylamine, diethylamine, dipropylamine, dibutylamine, diethanolamine, and dipropanolamine. The secondary amine may be used alone or in combination of two or more.

[0083] Hoffmann-decomposed poly(meth)acrylamide is a decomposition product obtained by decomposing poly(meth)acrylamide using the conventionally known Hoffmann reaction. Hoffmann-decomposed poly(meth)acrylamide can be obtained, for example, by reacting at least one of a (meth)acrylamide copolymer and a (meth)acrylamide homopolymer with a hypohalite salt such as sodium hypochlorite (NaOCl) in the presence of an alkaline substance such as sodium hydroxide (NaOH), thereby converting the amide group (-C=ONH-) to an amino group (-NH). 2 It can be obtained by converting it to ).

[0084] Examples of amphoteric poly(meth)acrylamides include water-soluble copolymers composed of (meth)acrylamide, anionic monomers, and cationic monomers. Amphoteric poly(meth)acrylamides may be used alone or in combination of two or more types.

[0085] Examples of anionic monomers used as components of amphoteric water-soluble copolymers include those used as components of anionic poly(meth)acrylamide. Examples of cationic monomers used as components of amphoteric water-soluble copolymers include those used as components of cationic poly(meth)acrylamide. In polymerization of amphoteric water-soluble copolymers, additives such as chain transfer agents commonly used in polymerization may be added.

[0086] Among the poly(meth)acrylamides mentioned above, amphoteric poly(meth)acrylamides are preferred, and more preferably, they are water-soluble copolymers composed of (meth)acrylamide, anionic monomers, and cationic monomers.

[0087] The weight-average molecular weight of poly(meth)acrylamide is preferably 300,000 to 4,000,000, and more preferably 1,000,000 to 3,000,000. The weight-average molecular weight of poly(meth)acrylamide is a polystyrene equivalent value measured by gel permeation chromatography (GPC).

[0088] The poly(meth)acrylamide content in the paper substrate 11 is preferably 0.1 to 2.0% by mass, and more preferably 0.2 to 1.5% by mass, relative to the total mass of the paper substrate 11. If the poly(meth)acrylamide content is above the lower limit, the wax will remain in the paper substrate 11 more easily, and the oil resistance will be further improved. In particular, the oil resistance of the cross-section will be further improved. If the poly(meth)acrylamide content is below the upper limit, deterioration of the base due to excessive aggregation can be suppressed.

[0089] The mass ratio expressed as [olefin resin content] / [poly(meth)acrylamide content] is preferably 0.5 to 10, and more preferably 1 to 5. If the mass ratio is above the lower limit, oil resistance is improved. If the mass ratio is below the upper limit, dispersibility and fixability are improved.

[0090] The mass ratio expressed as [urethane resin content] / [poly(meth)acrylamide content] is preferably 0.1 to 5, and more preferably 0.3 to 3. If the mass ratio is above the lower limit, the adhesion to the paper substrate is improved. If the mass ratio is below the upper limit, the dispersion stability is improved.

[0091] (Optional components) Optional components, as will be explained in more detail later, include internal additives added to the papermaking raw materials used in the manufacture of oil-resistant sheets, and external additives added to the papermaking products (hereinafter also referred to as "papermaking products") obtained by papermaking using the papermaking raw materials. External additives will be explained later.

[0092] Examples of internal additives include wet strength enhancers, paper strength enhancers, sizing agents, fixing agents, viscosities, fillers, yield enhancers, pH adjusters, water drainage enhancers, water resistance enhancers, softeners, antistatic agents, defoamers, slime control agents, dyes, pigments, and fibers other than pulp fibers (e.g., synthetic fibers such as rayon fibers and nylon fibers). Internal additives may be used individually or in combination of two or more types.

[0093] The paper substrate 11 preferably contains a wet strength enhancer. By including a wet strength enhancer in the paper substrate 11, the pulp fibers are crosslinked, and the wet strength of the paper substrate 11 can be increased. If the wet strength of the paper substrate 11 is low, the oil-resistant sheet 10 may tear when tension is applied to it during the manufacture or processing of the oil-resistant sheet 10. Known wet strength enhancers can be used, such as polyamide epichlorohydrin resin, polyamine-polyamide epichlorohydrin resin, epichlorohydrin-based wet strength enhancers, polyvinylamine resin, polyethyleneimine resin, melamine resin, and citric acid. Among these, epichlorohydrin-based wet strength enhancers are preferred, and polyamide epichlorohydrin resin and polyamine-polyamide epichlorohydrin resin are more preferred. The wet strength enhancer may be used alone or two or more may be used in combination. The content of the wet strength enhancer in the paper substrate 11 is preferably 0.01 to 1.0% by mass, and more preferably 0.1 to 0.4% by mass, relative to the total mass of the paper substrate 11.

[0094] The paper substrate 11 preferably contains a paper strength enhancer (excluding poly(meth)acrylamide). By including a paper strength enhancer in the paper substrate 11, the hydrogen bonds between the pulps are reinforced, and the paper strength of the paper substrate 11 can be increased. If the paper strength of the paper substrate is low, the oil-resistant sheet 10 may tear when tension is applied to it during the manufacture or processing of the oil-resistant sheet 10. Known paper strength enhancers can be used, such as cationized starch, carboxymethylcellulose, and graft polymerized starch. One type of paper strength enhancer may be used alone, or two or more types may be used in combination. The content of the paper strength enhancer in the paper substrate 11 is preferably 0.01 to 1.0% by mass, and more preferably 0.1 to 0.6% by mass, based on the total mass of the paper substrate 11.

[0095] The paper substrate 11 preferably contains a fixative (excluding poly(meth)acrylamide). Including a fixative in the paper substrate 11 promotes the fixation of chemicals to the pulp, improving the chemical yield. Known fixatives can be used, such as aluminum sulfate and sodium aluminate. The fixative may be used alone or in combination of two or more. The fixative content in the paper substrate 11 is preferably 0.01 to 1.0% by mass, and more preferably 0.1 to 1.0% by mass, relative to the total mass of the paper substrate 11.

[0096] The paper substrate 11 preferably contains a sizing agent. By including a sizing agent in the paper substrate 11, water resistance can be improved and water seepage from the edges of the paper substrate 11 can be suppressed. Examples of sizing agents include rosin-based sizing agents, alkyl ketene dimer-based sizing agents, alkenyl succinic anhydride-based sizing agents, and fatty acid sizing agents. Among these, alkyl ketene dimer-based sizing agents are preferred from the viewpoint of water resistance. The sizing agent may be used alone or two or more types may be used in combination. The content of the sizing agent in the paper substrate 11 is preferably 0.01 to 1.0% by mass, and more preferably 0.1 to 0.4% by mass, based on the total mass of the paper substrate 11.

[0097] The paper substrate 11 preferably contains a filler. By including a filler in the paper substrate 11, the opacity is increased, making it difficult to see the contents from the outside when food or other items are placed in a container made using the oil-resistant sheet 10. Examples of fillers include titanium dioxide, kaolin, calcium carbonate, talc, and silica. Among these, titanium dioxide is preferred in terms of opacity. The filler may be used alone or two or more may be used in combination. The amount of filler in the paper substrate 11 varies depending on the desired opacity, but for example, 0.1 to 30% by mass and more preferably 0.5 to 10% by mass relative to the total mass of the paper substrate 11.

[0098] <Method for Manufacturing Oil-Resistant Sheets> The oil-resistant sheet 10 according to this embodiment is obtained by manufacturing the paper substrate 11 described above. The paper substrate 11 is obtained, for example, by forming wet paper from papermaking raw materials including pulp slurry using various papermaking machines, and then drying the obtained wet paper. The paper produced in this way may be used as the paper substrate 11, i.e., the oil-resistant sheet 10, or an oil-resistant agent may be applied to the surface of the paper product as needed, and the paper product coated with the oil-resistant agent may be used as the paper substrate 11, i.e., the oil-resistant sheet 10. The oil-resistant agent may be applied to the wet paper. In addition, a smoothing treatment may be performed as needed, and the paper product after the smoothing treatment may be used as the paper substrate 11, i.e., the oil-resistant sheet 10.

[0099] The papermaking raw material is obtained by mixing a pulp slurry, wax, at least one of an olefin resin and a urethane resin, and an internal additive as needed. For the preparation of the pulp slurry, it is preferable to disintegrate pulp containing hardwood pulp and beat it using a refiner and beater to give the pulp appropriate flexibility and fluffiness. However, the pulp beating method is not particularly limited. The preferred range of disintegration-freeness, which is an indicator of the degree of pulp beating, is as described above. The pulp slurry obtained by beating the pulp, wax, at least one of an olefin resin and a urethane resin, and an internal additive as needed are mixed and dispersed in water to obtain a papermaking raw material of a concentration suitable for papermaking.

[0100] The papermaking machine used for papermaking raw materials is not particularly limited, but examples include long-wire papermaking machines, gap former type papermaking machines, cylinder papermaking machines, and short-wire papermaking machines. Among these, a papermaking machine equipped with an on-machine coating machine is preferred in terms of economic efficiency.

[0101] The wet paper obtained from the paper machine is preferably dried using a multi-stage cylinder dryer, an air dryer, or a Yankee dryer.

[0102] Oil-resistant agents are equivalent to external additives. Applying an oil-resistant agent to wet paper or papermaking material further improves oil resistance and strength. In addition, as will be described in more detail later, it becomes easier to laminate polyethylene or the like onto the surface of the oil-resistant sheet 10. Examples of oil-resistant agents include polyvinyl alcohol, starch, styrene-butadiene latex, acrylic resin, polyvinylidene chloride resin, olefin resin, polylactic acid resin, wax, and fatty acids. Among these, polyvinyl alcohol and starch are preferred. The amount of oil-resistant agent to be applied is 1 to 20 g / m². 2 Preferably, 1.5 to 10 g / m 2 This is preferable.

[0103] The oil-resistant agent may be diluted with a solvent as needed before application. The application method is not particularly limited, and various commonly available application machines can be used. Examples of application machines include blade coaters, air knife coaters, roll coaters, reverse roll coaters, bar coaters, curtain coaters, slot die coaters, gravure coaters, champlex coaters, brush coaters, slide bead coaters, two-roll size press coaters, pound size press coaters, rod metering size press coaters, blade metering size press coaters, short dwell coaters, gate roll coaters, and nip coaters using a calender. Among these, on-machine application machines are preferred in terms of productivity. Examples of on-machine application machines include blade coaters, bar coaters, gate roll coaters, rod metering size press coaters, blade metering size press coaters, and pound size press coaters. The application rate is 0.5 to 20 g / m² in terms of solid content. 2 Preferably, 1 to 10 g / m 2 This is more preferable. The oil-resistant agent may be applied to one side of the paper substrate or to both sides.

[0104] The smoothing process can be performed on-machine or off-machine using a standard smoothing device such as a supercalender, gross calender, or soft calender.

[0105] The oil-resistant sheet 10 composed of the paper base material 11 thus obtained is wound into a roll. Thereafter, in order to match the width of the oil-resistant sheet 10 to the width of the processing machine in the subsequent step, both end portions of the wound roll may be removed by a slitter.

[0106] <Properties of Oil-Resistant Sheet> The basis weight of the paper base material 11 is 150 to 1000 g / m 2 , preferably 160 to 700 g / m 2 , more preferably 170 to 500 g / m 2 , still more preferably 180 to 300 g / m 2 . When the basis weight of the paper base material 11 is at least the above lower limit value, the wax tends to remain in the paper base material 11, and the oil resistance is improved. In particular, the cross-sectional oil resistance is improved. In addition, the oil-resistant sheet 10 has sufficient strength as a container such as a food cup. When the basis weight of the paper base material 11 is at most the above upper limit value, the moldability into a cup shape or the like is excellent. The basis weight of the paper base material 11 is a value measured in accordance with JIS P 8124:2011.

[0107] The density of the paper base material 11 is 0.6 to 1.0 g / cm 3 , preferably 0.65 to 0.95 g / m 3 , more preferably 0.7 to 0.9 g / m 3 , still more preferably 0.8 to 0.9 g / m 3 . When the density of the paper base material 11 is at least the above lower limit value, when the oil-resistant agent is applied, the oil-resistant agent is easily fixed, and the oil resistance is more easily exhibited. When the density of the paper base material 11 is at most the above upper limit value, the moldability into a cup shape or the like is excellent. The density of the paper base material 11 is a value measured in accordance with JIS P 8118:2014.

[0108] The thickness of the paper base material 11 is preferably 150 to 1000 μm, more preferably 200 to 700 μm, still more preferably 250 to 400 μm. When the thickness of the paper base material 11 is at least the above lower limit value, good strength is easily obtained. When the thickness of the paper base material 11 is at most the above upper limit value, the moldability into a cup shape or the like is excellent. The thickness of the paper base material 11 is a value measured in accordance with JIS P 8118:2014.

[0109] <Effects> The oil-resistant sheet of this embodiment described above consists of a paper substrate comprising the pulp mentioned above, a specific amount of wax, and at least one of an olefin resin and a urethane resin, and having a specific basis weight and density. The ratio (α / β) of the wax content (β) in the region from the surface of the paper substrate up to 20 μm to the total mass of the paper substrate to the wax content (α) is 0.5 or more, and the wax is uniformly dispersed in the paper substrate. In other words, the wax is present not only on the surface of the paper substrate (first surface and second surface), but also on the sides and inside of the paper substrate.

[0110] For example, when an oil-resistant agent is applied to the surface of a conventional paper substrate to impart oil resistance, the oil-resistant agent is mainly present on the surface of the paper substrate. As a result, while the oil resistance of the surface of the paper substrate is excellent, the oil resistance of the sides of the paper substrate is poor. However, with the oil-resistant sheet of this embodiment, the wax is present even on the sides of the paper substrate. Therefore, in addition to the oil resistance of the surface of the paper substrate (first and second surfaces), the oil resistance of the sides is also excellent. Consequently, when the oil-resistant sheet is processed into a cup shape, for example, as shown in Figure 3, it exhibits excellent cross-sectional oil resistance, making it difficult for oils from food to seep into the edges.

[0111] <Other Embodiments> The oil-resistant sheet of the present invention is not limited to those described above. For example, the oil-resistant sheet 10 shown in Figure 1 is a sheet made of a single-layer paper substrate 11, but the oil-resistant sheet may be made of a multi-layer paper substrate of two or more layers, as shown in Figure 2, for example. The paper substrate is preferably made of three or more layers, but may be made of four or more layers, or five or more layers. There is no particular upper limit, but for example it may be 20 layers or less, 10 layers or less, or 8 layers or less.

[0112] The oil-resistant sheet 20 shown in Figure 2 consists of three layers of paper substrate 21. The paper substrate 21 is composed of a first layer 211, a second layer 212, and a third layer 213 located between the first layer 211 and the second layer 212. In this specification, the surface 21a of the paper substrate 21 on the first layer 211 side is also referred to as the "first surface," and the surface 21b on the second layer 212 side is also referred to as the "second surface." Furthermore, the surface 21c of the paper substrate 21 perpendicular to the first surface 21a and the second surface 21b is also referred to as the "side surface."

[0113] The paper substrate 21 comprises the pulp described above, wax, and at least one of an olefin resin and a urethane resin, and may further contain the internal additives described above as needed. The wax content in the paper substrate 21 is 0.5 to 10% by mass of the total mass of the paper substrate 21, preferably 0.6 to 5% by mass, more preferably 0.8 to 3% by mass, and even more preferably 1 to 2% by mass. Furthermore, when the wax content in the paper substrate 21 is denoted as "content (α)" and the wax content in the region from the surface of the paper substrate 21 up to 20 μm is denoted as "content (β)", the ratio of content (α) to content (β) (α / β) is 0.5 or more. Specifically, as shown in Figure 2, when the content of wax in region (S21) relative to the total mass of region (S21) from the first surface 21a to 20 μm of the paper substrate 21 is defined as "content (β21)", the ratio of content (α) to content (β21) (α / β21) is 0.5 or more, preferably 0.5 to 5, more preferably 0.7 to 3, and even more preferably 0.9 to 1.1. Furthermore, when the content of wax in region (S22) relative to the total mass of region (S22) from the second surface 21b to 20 μm of the paper substrate 21 is defined as "content (β22)", the ratio of content (α) to content (β22) (α / β22) is 0.5 or more, preferably 0.5 to 5, more preferably 0.7 to 3, and even more preferably 0.9 to 1.1.

[0114] The overall basis weight of the paper substrate 21 is 150 to 1000 g / m². 2 Therefore, 160-700 g / m 2 Preferably, 170-500 g / m 2 More preferably, 180-300 g / m2 This is even more preferable. The overall density of the paper substrate 21 is 0.6 to 1.0 g / cm³. 3 Therefore, 0.65 to 0.95 g / m 3 Preferably, 0.7 to 0.9 g / m 3 More preferably, 0.8 to 0.9 g / m 3 This is even more preferable. The overall thickness of the paper substrate 21 is preferably 150 to 1000 μm, more preferably 200 to 700 μm, and even more preferably 250 to 400 μm.

[0115] The first layer 211, the second layer 212, and the third layer 213 each contain the pulp and wax described above. One or more layers selected from the first layer 211, the second layer 212, and the third layer 213 contain at least one of an olefin resin and a urethane resin. It is preferable that each layer contains at least one of an olefin resin and a urethane resin. The first layer 211, the second layer 212, and the third layer 213 may each further contain the internal additives described above, as necessary. At least one of the first layer 211 and the third layer 213 may further contain the external additives described above. The components contained in the first layer 211, the second layer 212, and the third layer 213 may be of the same type or of different types.

[0116] The wax content in the first layer 211 is preferably 0.5 to 10% by mass, more preferably 0.6 to 5% by mass, even more preferably 0.8 to 3% by mass, and particularly preferably 1 to 2% by mass, relative to the total mass of the first layer 211. The wax content in the second layer 212 is preferably 0.5 to 10% by mass, more preferably 0.6 to 5% by mass, even more preferably 0.8 to 3% by mass, and particularly preferably 1 to 2% by mass, relative to the total mass of the first layer 211. The wax content in the third layer 213 is preferably 0.5 to 10% by mass, more preferably 0.6 to 5% by mass, even more preferably 0.8 to 3% by mass, and particularly preferably 1 to 2% by mass, relative to the total mass of the first layer 211.

[0117] The basis weight of the first layer 211 is 50-340 g / m². 2 Preferably, 50 to 240 g / m 2More preferably, 50 to 170 g / m 2 More preferably, 50-100 g / m 2 This is particularly preferable. The density of the first layer 211 is 0.6 to 1.0 g / cm³. 3 Preferably, 0.65 to 0.95 g / cm³ 3 Preferably, 0.7 to 0.9 g / cm³ 3 More preferably, 0.8 to 0.9 g / cm³ 3 The above is particularly preferred. The thickness of the first layer 211 is preferably 50 to 340 μm, more preferably 50 to 240 μm, and even more preferably 50 to 100 μm.

[0118] The basis weight of the second layer 212 is 50-340 g / m². 2 Preferably, 50 to 240 g / m 2 More preferably, 50 to 170 g / m 2 More preferably, 50-100 g / m 2 This is particularly preferable. The density of the second layer 212 is 0.6 to 1.0 g / cm³. 3 Preferably, 0.65 to 0.95 g / cm³ 3 Preferably, 0.7 to 0.9 g / cm³ 3 More preferably, 0.8 to 0.9 g / cm³ 3 This is particularly preferable. The thickness of the second layer 212 is preferably 50 to 340 μm, more preferably 50 to 240 μm, and even more preferably 50 to 100 μm.

[0119] The basis weight of the third layer, 213, is 50-340 g / m². 2 Preferably, 50 to 240 g / m 2 More preferably, 50 to 170 g / m 2 More preferably, 50-100 g / m 2 This is particularly preferable. The density of the third layer 213 is 0.6 to 1.0 g / cm³. 3 Preferably, 0.65 to 0.95 g / cm³ 3 Preferably, 0.7 to 0.9 g / cm³ 3 More preferably, 0.8 to 0.9 g / cm³ 3 This is particularly preferable. The thickness of the third layer 213 is preferably 50 to 340 μm, more preferably 50 to 240 μm, and even more preferably 50 to 100 μm.

[0120] The oil-resistant sheet 20 is obtained by sequentially forming wet paper from the papermaking raw materials of each layer constituting the paper substrate 21, and then drying the resulting wet paper. The paper produced in this way may be used as the paper substrate 21, i.e., the oil-resistant sheet 20, or an oil-resistant agent may be applied to the surface of the paper product as needed, and the paper product coated with the oil-resistant agent may be used as the paper substrate 21, i.e., the oil-resistant sheet 20. The oil-resistant agent may be applied to the wet paper. In addition, a smoothing treatment may be performed as needed, and the paper product after the smoothing treatment may be used as the paper substrate 21, i.e., the oil-resistant sheet 20.

[0121] When the oil-resistant sheet consists of two layers of paper substrate, an example of the oil-resistant sheet is one made of a paper substrate composed of the first layer and the second layer described above. When the oil-resistant sheet consists of four or more layers of paper substrate, an example of the oil-resistant sheet is one made of a paper substrate composed of the first layer and the second layer described above, and two or more third layers.

[0122] <Applications> The applications of the oil-resistant sheet of this embodiment are not particularly limited, but include containers, packaging materials, lining paper, etc. Among these, the oil-resistant sheet of this embodiment is suitable for containers, especially food containers (hereinafter also referred to as "food cups" or "food cups"). An example of a food cup using the oil-resistant sheet of this embodiment will be described below.

[0123] Figure 3 shows an example of a food cup using the oil-resistant sheet of the present invention. The food cup 30 of this embodiment comprises a hollow cylindrical body 31 and a substantially circular bottom 32. The height and opening shape of the body 31 and the size and shape of the bottom 32 are not particularly limited and are appropriately determined depending on the type of food to be contained in the food cup 30.

[0124] Food cup 30 is manufactured, for example, as follows. First, a heat seal layer is formed on the first or second surface of the oil-resistant sheet of the present invention. The heat seal layer is a layer made of a heat-sealable resin. Examples of heat-sealable resins include ethylene homopolymers (polyethylene) or copolymers. Examples of ethylene copolymers include ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer, ethylene-vinyl acetate copolymer, etc. Among these, polyethylene is preferred. The heat seal layer can be formed, for example, by laminating a heat-sealable resin onto the first or second surface of the oil-resistant sheet. The melting point of the heat seal layer is preferably 90 to 160°C, and more preferably 105 to 145°C. If the melting point of the heat seal layer is above the lower limit, a food cup with excellent heat resistance can be provided. If the melting point of the heat seal layer is below the upper limit, excellent heat seal properties are provided. The thickness of the heat seal layer is preferably 10 to 60 μm, and more preferably 15 to 40 μm. If the thickness of the heat-seal layer is greater than or equal to the lower limit above, a food cup without leaks such as pinholes can be provided. If the thickness of the heat-seal layer is less than or equal to the upper limit above, excellent heat-seal properties are achieved.

[0125] Next, the oil-resistant sheet with a heat-seal layer formed on it (hereinafter also referred to as the "laminated sheet") is punched out into a desired shape (for example, a fan shape) as needed, the laminated sheet is made into a cylinder with the heat-seal layer on the inside, and the overlapping portion H of the laminated sheet is heat-sealed to create the body portion 31. Separately, the laminated sheet is punched out into a desired shape (for example, a circle) to create the bottom portion 32. Next, one end of the body portion 31 and the bottom portion 32 are attached so that the heat-seal layers are in contact with each other, and joined by heat sealing. If necessary, the edge of the other end of the body portion 31 is curled outwards to obtain a food cup 30 as shown in Figure 3.

[0126] The food cup 30 of this embodiment is made using the oil-resistant sheet of the present invention, and therefore has excellent oil resistance. The end face 31c of the overlapping portion (seal portion) H of the laminated sheet constituting the body portion 31 corresponds to the side surface of the oil-resistant sheet. As described above, since the oil-resistant sheet of the present invention has wax even on the side surface, it also has excellent oil resistance (cross-sectional oil resistance) at the end face 31c. Thus, because the food cup 30 of this embodiment has excellent cross-sectional oil resistance, when food is placed inside, oil and other substances from the food are less likely to seep in, and the appearance of the product is less likely to be affected.

[0127] There are no particular restrictions on the food that can be contained in the food cup 30, but examples include pasta, curry, fried rice, doria, lasagna, gratin, mapo tofu, soup, ramen, and fried foods.

[0128] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Embodiments of the present invention can be modified in various ways without changing the essence of the invention.

[0129] [Measurement and Evaluation] <Measurement of Wax Content> The wax content (α) in the paper substrate was measured by heating an oil-resistant sheet to decompose it and analyzing the generated gas using a gas chromatograph-mass spectrometer.

[0130] Separately, a region from the first surface of the paper substrate up to 20 μm was cut out from the paper substrate. The cut-out piece was heated and thermally decomposed, and the resulting gas was analyzed using a gas chromatograph-mass spectrometer to determine the wax content (β1) in the cut-out piece and calculate the ratio (α / β1). Similarly, a region from the second surface of the paper substrate up to 20 μm was cut out from the paper substrate. The cut-out piece was heated and thermally decomposed, and the resulting gas was analyzed using a gas chromatograph-mass spectrometer to determine the wax content (β2) in the cut-out piece and calculate the ratio (α / β2).

[0131] <Measurement of Disintegration Freeness> Paper substrates were disintegrated in accordance with JIS P 8220-1, and the freeness (Canadian standard filtration rate) of the obtained pulp was measured in accordance with JIS P 8121-2:2012, and this value was defined as the disintegration freeness.

[0132] <Measurement of basis weight> The basis weight (grammage) of the paper substrate was measured in accordance with JIS P 8124:2011. <Measurement of density> The density of the paper substrate was measured in accordance with JIS P 8118:2014.

[0133] <Measurement of Thickness> The thickness of the paper substrate was measured in accordance with JIS P 8118:2014.

[0134] <Evaluation of Oil Resistance (Kit)> The oil resistance (kit) of the oil-resistant sheet was evaluated in accordance with "Paper and cardboard - Oil repellency test method - Kit method" as specified in J. TAPPI No. 41:2000. A higher numerical value indicates better oil resistance.

[0135] <Evaluation of Edgewick (water, 15hr)> Using MS pouches manufactured by Meiko Shokai Co., Ltd. (resin type: base material PET / adhesive layer EVA), MS pouch-specific films were laminated to the first and second surfaces of a paper substrate to prevent water from penetrating into the paper substrate from the first and second surfaces. Then, test specimens were prepared by cutting the paper substrate into a 60mm x 90mm rectangle so that the cross-section was exposed. The obtained test specimens were immersed in water for 15 hours, then removed from the water, the water adhering to the film surface of the test specimen was wiped off, and the water penetration distance from the cross-section of the paper substrate was measured.

[0136] <Evaluation of Edgewick (Salad Oil, 15hr)> Using MS pouches manufactured by Meiko Shokai Co., Ltd., MS pouch-specific films were laminated to the first and second surfaces of a paper substrate to prevent salad oil from penetrating into the paper substrate from the first and second surfaces. Then, test specimens were prepared by cutting the paper substrate into a 60mm x 90mm rectangle so that the cross-section was exposed. The obtained test specimens were immersed in salad oil (manufactured by Nisshin Oillio Group Ltd., product name "Canola Oil") for 15 hours. After removing them from the salad oil, the salad oil adhering to the film surface of the test specimens was wiped off, and the penetration distance of the salad oil from the cross-section of the paper substrate was measured.

[0137] [Production Example 1] Nitrogen was introduced into a reaction vessel equipped with a stirrer, thermometer, reflux condenser, nitrogen gas inlet tube, and two dropping funnels. 98 parts by mass of maleic anhydride and 75.2 parts by mass of toluene were charged, and the reaction system was heated to 110°C while stirring under a nitrogen stream. Next, 73.7 parts by mass of diisobutylene (containing 76% by mass of 2,2,4-trimethyl-1-pentene), 112 parts by mass of 1-hexadecene, and 12 parts by mass of n-butyl acrylate were charged into dropping funnel (1). Separately, 6.6 parts by mass of t-butyl peroxybenzoate and 35 parts by mass of toluene were charged into dropping funnel (2), and each was added dropwise to the vessel over 1.5 hours. After maintaining the temperature under reflux for 2 hours, 2.6 parts by mass of t-butyl peroxybenzoate and 15 parts by mass of toluene were added dropwise over 30 minutes, and the temperature was maintained at the same temperature for another hour. Sixteen parts by mass of sodium hydroxide, eighty-five parts by mass of 28% by mass aqueous ammonia, and a predetermined amount of water were added and stirred. Toluene was removed by distillation under reduced pressure to obtain an olefin resin with a non-volatile content of 20% by mass, a viscosity of 80 mPa·s, and a pH of 9.0.

[0138] [Production Example 1'] Nitrogen was introduced into a reaction vessel equipped with a stirrer, thermometer, reflux condenser, nitrogen gas inlet tube, and two dropping funnels. 98 parts by mass of maleic anhydride and 75.2 parts by mass of toluene were charged, and the reaction system was heated to 110°C while stirring under a nitrogen stream. Next, 85.0 parts by mass of diisobutylene (2,2,4-trimethyl-1-pentene content 76% by mass), 95.0 parts by mass of 1-hexadecene, and 18.0 parts by mass of n-butyl acrylate were charged into dropping funnel (1). Separately, 6.6 parts by mass of t-butyl peroxybenzoate and 35 parts by mass of toluene were charged into dropping funnel (2), and each was added dropwise to the reaction vessel over 1.5 hours. After maintaining the temperature under reflux for 2 hours, 2.6 parts by mass of t-butyl peroxybenzoate and 15 parts by mass of toluene were added dropwise over 30 minutes, and the temperature was maintained at the same temperature for another hour. Subsequently, 16 parts by mass of sodium hydroxide, 85 parts by mass of 28% by mass aqueous ammonia, and a predetermined amount of water were added and the mixture was stirred, and toluene was removed by distillation under reduced pressure. As a result, an olefin resin with a non-volatile content of 20% by mass, a viscosity of 120 mPa·s, and a pH of 9.0 was obtained.

[0139] [Production Example 2] In a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, 59.4 parts by mass of dimethylolbutanoic acid, 489.9 parts by mass of polyoxytetramethylene-polyoxypropylene glycol (manufactured by NOF Corporation, trade name "Polycerin DCB-2000"), and 200.8 parts by mass of isophorone diisocyanate were charged, and the reaction was carried out at 85°C under a nitrogen stream for 5 hours to obtain 750 parts by mass of urethane prepolymer. Next, the urethane prepolymer was added and dispersed under stirring in an aqueous solution consisting of 1208 parts by mass of water, 225 parts by mass of isopropyl alcohol, 40.5 parts by mass of triethylamine, and 43.3 parts by mass of adipic acid dihydrazide. The reaction was carried out at 50°C for 3 hours, and then a predetermined amount of water was added to obtain a urethane resin with a non-volatile content of 35% by mass, a viscosity of 800 mPa·s / 25°C, and a pH of 8.0.

[0140] [Production Example 2'] In a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, 72.0 parts by mass of dimethylolbutanoic acid, 460.0 parts by mass of polyoxytetramethylene-polyoxypropylene glycol ("Polycerin DCB-2000" manufactured by NOF Corporation) and 215.0 parts by mass of isophorone diisocyanate were charged, and the reaction was carried out at 85°C under a nitrogen stream for 5 hours to obtain 747 parts by mass of urethane prepolymer. Next, the urethane prepolymer was added and dispersed under stirring in an aqueous solution consisting of 1210 parts by mass of water, 225 parts by mass of isopropyl alcohol, 48.0 parts by mass of triethylamine and 43.3 parts by mass of adipic acid dihydrazide. The reaction was carried out at 50°C for 3 hours, and then a predetermined amount of water was added to obtain a urethane resin with a non-volatile content of 35% by mass, a viscosity of 1100 mPa·s / 25°C, and a pH of 8.5.

[0141] [Manufacturing Example 3] In a reaction vessel equipped with a stirrer, thermometer, reflux condenser, nitrogen gas inlet tube, and dropping funnel, 100 parts by mass of paraffin wax (melting point: 69°C) and 10 parts by mass of polyoxyethylene alkyl ether (manufactured by Nippon Emulsifier Co., Ltd., trade name "Newcol 2305") were charged and melted at 90°C or higher, and then 250 parts by mass of ion-exchanged water was added. Next, the mixture was emulsified using a high-pressure emulsifier to obtain paraffin wax (aqueous emulsion) with a non-volatile content of 30% by mass.

[0142] [Example 1] To obtain a pulp slurry, 70% by mass of bleached hardwood kraft pulp (LBKP) and 30% by mass of bleached softwood kraft pulp (NBKP) were beaten in a double disc refiner (DDR) to obtain a pulp slurry. To the obtained pulp slurry, the paraffin wax obtained in Production Example 3, the olefin resin obtained in Production Example 1, amphoteric poly(meth)acrylamide (manufactured by Arakawa Chemical Industries, Ltd., trade name "TS-1"), cationic poly(meth)acrylamide (manufactured by Arakawa Chemical Industries, Ltd., trade name "AW-308"), sodium bicarbonate as a pH adjuster, and alkyl ketene dimer (manufactured by Arakawa Chemical Industries, Ltd., trade name "Sizing Pine K-287") as a sizing agent were added and mixed to obtain a papermaking raw material. The obtained papermaking raw material was used in a papermaking machine to form wet paper a total of six times, so that the basis weight and density of the paper substrate would be as shown in Table 1. The resulting wet paper was then dried. Polyvinyl alcohol (PVA) was applied to both sides of the resulting paper using a gravure coater, with a dry coating amount of 4 g / m². 2 The paper substrate was coated and dried to obtain an oil-resistant sheet. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 1.

[0143] [Example 2] A pulp slurry was prepared in the same manner as in Example 1. To the obtained pulp slurry, the paraffin wax obtained in Production Example 3, the olefin resin obtained in Production Example 1, poly(meth)acrylamide (manufactured by Arakawa Chemical Industries, Ltd., trade names "TS-1" and "AW-308"), sodium bicarbonate as a pH adjuster, polyamine-polyamide epichlorohydrin resin (manufactured by Seikoh PMC Co., Ltd., trade name "WS4024") as a wet paper strength enhancer, and alkyl ketene dimer (manufactured by Arakawa Chemical Industries, Ltd., trade name "Sizing Pine K-287") as a sizing agent were added and mixed to obtain a papermaking raw material. The obtained papermaking raw material was used in a papermaking machine to form wet paper once, so that the basis weight and density of the paper substrate were the values ​​shown in Table 1, and the obtained wet paper was dried. Polyvinyl alcohol was applied to both sides of the obtained papermaking material using a gravure coater, with a coating amount of 4 g / m² after drying. 2 The paper substrate was coated and dried to obtain an oil-resistant sheet. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 1.

[0144] [Example 3] Papermaking raw materials were prepared in the same manner as in Example 1, except that the content of paraffin wax obtained in Production Example 3 and olefin resin obtained in Production Example 1 relative to the total mass of the paper substrate was changed to the values ​​shown in Table 1, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 1.

[0145] [Example 4] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that the basis weight and thickness of the paper substrate were changed to the values ​​shown in Table 1. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 1.

[0146] [Example 5] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that the basis weight and thickness of the paper substrate were changed to the values ​​shown in Table 1. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 1.

[0147] [Example 6] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that the density and thickness of the paper substrate were changed to the values ​​shown in Table 1. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 1.

[0148] [Example 7] Papermaking raw materials were prepared in the same manner as in Example 1, except that the urethane resin obtained in Production Example 2 was used instead of the olefin resin. Using the obtained papermaking raw materials, an oil-resistant sheet was manufactured in the same manner as in Example 1, except that the basis weight, density, and thickness of the paper substrate were changed to the values ​​shown in Table 2. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 2.

[0149] [Example 8] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that starch (Ingredion Co., Ltd., product name "Bondstar T800") was coated on both sides of the papermaking material instead of PVA. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 2.

[0150] [Example 9] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that acrylic resin (manufactured by Daikin Industries, Ltd., product name "Unidyne XP8001") was coated on both sides of the paper material instead of PVA. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 2.

[0151] [Example 10] Papermaking raw materials were prepared in the same manner as in Example 1, except that hydrogenated castor oil (manufactured by Ito Oil Co., Ltd., trade name "Hydrogenated Castor Oil A") was used instead of paraffin wax, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 2.

[0152] [Example 11] Papermaking raw materials were prepared in the same manner as in Example 1, except that rice wax (manufactured by Boso Oil & Fat Co., Ltd., product name "Rice Wax SS-2") was used instead of paraffin wax, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 2.

[0153] [Example 12] Papermaking raw materials were prepared in the same manner as in Example 1, except that poly(meth)acrylamide was not added, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 3.

[0154] [Example 13] Papermaking raw materials were prepared in the same manner as in Example 1, except that the content of paraffin wax obtained in Production Example 3 relative to the total mass of the paper substrate was changed to the value shown in Table 3, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 3.

[0155] [Example 14] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that the disintegration-freeness was changed to 450 mL. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 3.

[0156] [Example 15] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that the wax content (β1) and (β2) were changed to the values ​​shown in Table 3. Specifically, the paraffin wax obtained in Manufacturing Example 3 and the olefin resin obtained in Manufacturing Example 1 were added in such a high amount to the outermost wet paper layer and in such a low amount to the middle wet paper layer to manufacture the oil-resistant sheet. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 3.

[0157] [Example 16] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that the wax content (β1) and (β2) were changed to the values ​​shown in Table 3. Specifically, the paraffin wax obtained in Manufacturing Example 3 and the olefin resin obtained in Manufacturing Example 1 were added in such a way that the amount was reduced in the outermost wet paper layer and increased in the middle wet paper layer to manufacture an oil-resistant sheet. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 3.

[0158] [Example 17] Papermaking raw materials were prepared in the same manner as in Example 1, except that the content of paraffin wax obtained in Production Example 3 and olefin resin obtained in Production Example 1 was changed to the values ​​shown in Table 3, relative to the total mass of the paper substrate, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 3.

[0159] [Example 18] Papermaking raw materials were prepared in the same manner as in Example 1, except that the olefin resin obtained in Production Example 1' was used instead of the olefin resin obtained in Production Example 1, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 4.

[0160] [Example 19] Papermaking raw materials were prepared in the same manner as in Example 7, except that the urethane resin obtained in Production Example 2' was used instead of the urethane resin obtained in Production Example 2, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 4.

[0161] [Comparative Example 1] An oil-resistant sheet was manufactured in the same manner as in Example 1, except that the basis weight and thickness of the paper substrate were changed to the values ​​shown in Table 4. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 4.

[0162] [Comparative Example 2] Papermaking raw materials were prepared in the same manner as in Example 1, except that paraffin wax was not added, and an oil-resistant sheet was manufactured. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 4.

[0163] [Comparative Example 3] Papermaking raw materials were prepared in the same manner as in Example 1, except that the disintegration-freeness was changed to 500 mL. Using the obtained papermaking raw materials, an oil-resistant sheet was manufactured in the same manner as in Example 1, except that the density and thickness of the paper substrate were changed to the values ​​shown in Table 4. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 4.

[0164] [Comparative Example 4] Papermaking raw materials were prepared in the same manner as in Example 1, except that paraffin wax and olefin resin were not included. An oil-resistant sheet was manufactured in the same manner as in Example 1, except that paraffin wax was applied to both sides of the papermaking material using the obtained papermaking raw materials, and PVA was replaced with paraffin wax. Various measurements and evaluations were performed on the obtained oil-resistant sheet. The results are shown in Table 4.

[0165]

[0166]

[0167]

[0168]

[0169] The abbreviations in Tables 1-4 are as follows. Blank spaces in Tables 1-4 indicate that the ingredient is not included. • PAE: Polyamine-polyamide epichlorohydrin resin • AKD: Alkyl ketene dimer • PVA: Polyvinyl alcohol • WAX: Paraffin wax

[0170] As is clear from the results in Tables 1 to 4, the oil-resistant sheets obtained in each example exhibited excellent oil resistance on the surface and sides, as well as water resistance on the sides. However, the oil-resistant sheet obtained in Example 17 was more prone to paper slippage than the oil-resistant sheets obtained in Examples 1 to 16. On the other hand, the oil-resistant sheets obtained in each comparative example were inferior in oil resistance on the surface and sides, as well as water resistance on the sides.

[0171] According to the present invention, it is possible to provide an oil-resistant sheet that has excellent oil resistance on the surface and sides, as well as excellent water resistance on the sides.

[0172] 10 Oil-resistant sheet 11 Paper substrate 11a First surface 11b Second surface 11c Side 20 Oil-resistant sheet 21 Paper substrate 211 First layer 212 Second layer 213 Third layer 21a First surface 21b Second surface 30 Food cup 31 Body 31c End face 32 Bottom S11 Region from the first surface up to 20 μm S12 Region from the second surface up to 20 μm S21 Region from the first surface up to 20 μm S22 Region from the second surface up to 20 μm H Overlapping portion (seal portion)

Claims

1. An oil-resistant sheet made of a paper substrate containing pulp, wax, and at least one of olefin resin and urethane resin, wherein the pulp contains hardwood pulp, and the basis weight of the paper substrate is 150 to 1000 g / m². 2 The density of the paper substrate is 0.6 to 1.0 g / cm³. 3 An oil-resistant sheet wherein the wax content (α) relative to the total mass of the paper substrate is 0.5 to 10% by mass, and the ratio (α / β) of the wax content (α) to the wax content (β) in the region from the surface of the paper substrate up to 20 μm is 0.5 or more.

2. The oil-resistant sheet according to claim 1, wherein the wax comprises paraffin wax.

3. The oil-resistant sheet according to claim 1 or 2, wherein the disintegration-freeness of the pulp is 450 mL or less.

4. The oil-resistant sheet according to claim 1 or 2, wherein the paper substrate further comprises poly(meth)acrylamide.

5. The oil-resistant sheet according to claim 1 or 2, wherein the paper substrate is made of three or more layers.

6. An oil-resistant sheet according to claim 1 or 2, for use in food cups.