Photosensitive resin composition, method for producing cured relief pattern, cured relief pattern, and semiconductor device

A negative-type photosensitive resin composition with a low-boiling-point solvent enhances sensitivity, resolution, and adhesion to metal wiring layers, addressing the challenges of low-temperature curing in semiconductor manufacturing.

WO2026235078A1PCT designated stage Publication Date: 2026-11-12ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016977
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-28
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions used in semiconductor manufacturing face challenges in achieving high sensitivity, high resolution, and high adhesion to metal wiring layers while being cured at low temperatures, which is essential for efficient semiconductor packaging methods like Fan-Out packaging, and there is a need for compositions that can reduce stepper exposure time and improve yield.

Method used

A negative-type photosensitive resin composition comprising a polyimide precursor or polyimide, a photoradical initiator, and a solvent with a specific compound represented by general formula (I) that has a low boiling point, allowing for high sensitivity, resolution, and adhesion to metal wiring layers even at low temperatures.

Benefits of technology

The composition achieves high sensitivity, high resolution, and high adhesion to metal wiring layers during low-temperature curing, improving the efficiency and yield of semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026016977_12112026_PF_FP_ABST
    Figure JP2026016977_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present disclosure is to provide: a negative photosensitive resin composition (hereinafter simply referred to as a photosensitive resin composition) capable of achieving high sensitivity, high resolution, and high adhesion to a metal wiring layer even when cured at low temperatures; a cured relief pattern produced using the photosensitive resin composition; a method for producing the cured relief pattern; and a semiconductor device. A negative photosensitive resin composition according to the present disclosure contains (A) a polyimide precursor or a polyimide, (B) a photoradical initiator, and (C) a solvent, wherein the solvent (C) contains a compound represented by general formula (I). (In the formula, R1, R2, and R3 are each independently an organic group having three or less carbon atoms, and at least one of R1, R2, and R3 is an alkyl group having two or more carbon atoms.)
Need to check novelty before this filing date? Find Prior Art

Description

Photosensitive resin composition, method for producing cured relief pattern, cured relief pattern, and semiconductor device

[0001] The present disclosure relates to a photosensitive resin composition containing a polyimide precursor or polyimide, a cured relief pattern obtained by curing the photosensitive resin composition and a method for producing the same, and a semiconductor device having the cured relief pattern.

[0002] Conventionally, polyimide resins having excellent heat resistance, electrical properties and mechanical properties in combination have been used for insulating materials of electronic components, passivation films, surface protective films, interlayer insulating films and the like of semiconductor devices. There are various semiconductor packaging methods for semiconductor devices. Examples of the semiconductor packaging method include a packaging method in which a semiconductor chip is covered with a sealing material (mold resin) to form an element sealing material, and a rewiring layer electrically connected to the semiconductor chip is further formed. Among semiconductor packaging methods, in recent years, a Fan-Out semiconductor packaging method has become mainstream.

[0003] In a fan-out type semiconductor package, a semiconductor chip sealing body larger than the chip size of the semiconductor chip is formed by covering the semiconductor chip with a sealing material. Further, a rewiring layer extending to the regions of the semiconductor chip and the sealing material is formed. The rewiring layer is formed with a thin film thickness. In addition, since the rewiring layer can be formed up to the region of the sealing material, the number of external connection terminals can be increased. For example, as a fan-out type semiconductor device, the device described in Patent Document 1 below is known.

[0004] Furthermore, in recent semiconductor manufacturing processes, the stepper exposure time has increased due to the larger wafer size. Consequently, from the viewpoint of shortening the exposure process time and improving yield, there is a demand for highly sensitive photosensitive resin compositions. Additionally, from the viewpoint of semiconductor package manufacturing processes and the heat resistance of encapsulants, there is a demand for photosensitive resin compositions that can be cured at low temperatures, such as 230°C or below. Moreover, in the redistribution process, the film formed from the photosensitive resin composition is required to adhere well to the wiring layer made of metal such as copper. For example, Patent Document 2 describes the study of combinations of specific compounds containing a specific polyimide precursor with polymerizable groups, with the aim of providing a photosensitive resin composition with excellent sensitivity, and also describes the case of curing at low temperatures.

[0005] Japanese Patent Publication No. 2005-167191, International Publication No. 2020 / 031976, International Publication No. 2017 / 038598, Japanese Patent Publication No. 2012-194520

[0006] The present disclosure aims to provide a negative-type photosensitive resin composition (hereinafter also simply referred to as a photosensitive resin composition) capable of achieving high sensitivity, high resolution, and high adhesion to a metal wiring layer even with low-temperature curing, a cured relief pattern manufactured using the above-mentioned photosensitive resin composition, a method for manufacturing the same, and a semiconductor device.

[0007] One aspect of the present disclosure is listed below: [1] A negative-type photosensitive resin composition comprising (A) a polyimide precursor or polyimide, (B) a photoradical initiator, and (C) a solvent, wherein the (C) solvent contains a compound represented by the following general formula (I). {In the formula, R 1 , R 2 , and R 3 Each of these is an organic group with 3 or fewer carbon atoms, and R 1 , R 2 , and R 3[2] The negative-type photosensitive resin composition according to item 1, wherein the compound represented by the general formula (I) is contained in an amount of more than 50% by mass based on the total mass of the solvent (C). [3] The negative-type photosensitive resin composition according to item 1 or 2, wherein the compound represented by the general formula (I) is contained in an amount of 10 to 90% by mass based on the total mass of the negative-type photosensitive resin composition. [4] The negative-type photosensitive resin composition according to any one of items 1 to 3, wherein the boiling point of the compound represented by the general formula (I) is less than 215°C at atmospheric pressure. [5] The negative-type photosensitive resin composition according to any one of items 1 to 4, wherein the solvent (C) contains at least one compound selected from the group consisting of N,N-diethylacetamide, N,N-diethylacrylamide, and N,N-dimethylpropionamide. [6] The solvent further comprises other solvents other than the compound represented by the general formula (I), the negative-type photosensitive resin composition according to any one of items 1 to 5. [7] The other solvents are N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, dimethyl sulfoxide, tetramethylurea, tetraethylurea, 1,3-dimethyl-2-imidazolidinone, N,N'-dimethylpropyleneurea, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl acetate, ethyl acetate, butyl acetate, diethyl oxalate, ethyl lactate, methyl lactate, butyl lactate, γ-butyrolactone A negative-type photosensitive resin composition according to item 6, comprising propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, benzyl alcohol, phenyl glycol, tetrahydrofurfuryl alcohol, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, morpholin, dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, chlorobenzene, o-dichlorobenzene, anisole, hexane, heptane, benzene, toluene, xylene, or mesitylene.[8] The negative photosensitive resin composition according to item 6 or 7, wherein the other solvent contains γ-butyrolactone or ethyl lactate. [9] The negative photosensitive resin composition according to any one of items 6 to 8, wherein the other solvent does not contain N-methyl-2-pyrrolidone or N-ethyl-2-pyrrolidone.

[10] The negative photosensitive resin composition according to any one of items 6 to 9, wherein the other solvent contains a solvent (C') having a boiling point of less than 215°C at atmospheric pressure.

[11] The negative photosensitive resin composition according to item 10, wherein the solvent (C') contains γ-butyrolactone, dimethyl sulfoxide, ethyl lactate, or N,N-diethylformamide.

[12] The negative photosensitive resin composition according to any one of items 1 to 11, further comprising a radical polymerizable monomer other than the (C) solvent.

[13] The negative photosensitive resin composition according to any one of items 1 to 12, further comprising a polymerization inhibitor.

[14] The negative photosensitive resin composition according to any one of items 1 to 13, further comprising a thermal base generator.

[15] The negative photosensitive resin composition according to any one of items 1 to 14, further comprising a rust inhibitor.

[16] The negative photosensitive resin composition according to item 15, wherein the rust inhibitor is at least one compound selected from the group consisting of purine, purine derivatives, and azole derivatives.

[17] The following general formula (1):. A polyimide precursor comprising a repeating structure represented by, and / or the following general formula (9): {In formula (1) and formula (9), X 1 and X 2 are each independently a tetravalent organic group, Y 1 and Y 2 are each independently a divalent organic group, m and n are each an integer of 2 to 100, R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group.} The negative photosensitive resin composition according to any one of items 1 to 16, comprising a polyimide represented by.

[18] In the general formula (1) and the general formula (9), X 1 and / or X 2 has at least one of the structures represented by the following formulas (2) to (4), and Y1 The negative-type photosensitive resin composition according to item 17, wherein the structure is represented by at least one of the following formulas (5) to (7). (In the formula, R 6 (This is a hydrogen atom, an alkyl group, or a phenyl group.) (In the formula, R 7 and R 8 Each of these is independently either a hydrogen atom or a methyl group. (In the formula, R 9 and R 10 (Each is independently a hydrogen atom or a methyl group.)

[19] A negative-type photosensitive resin composition according to any one of items 1 to 18, used for forming a buffer coat layer or redistribution layer of a semiconductor package.

[20] A method for producing a cured relief pattern, comprising: (1) forming a photosensitive resin layer on a substrate by coating the negative-type photosensitive resin composition according to any one of items 1 to 19 onto the substrate; (2) exposing the photosensitive resin layer; (3) developing the photosensitive resin layer after exposure to form a relief pattern; and (4) forming a cured relief pattern by heat-treating the relief pattern.

[21] A cured relief pattern comprising a cured product of the negative-type photosensitive resin composition according to any one of items 1 to 19.

[22] A semiconductor device comprising the cured relief pattern according to item 21.

[0008] According to this disclosure, it is possible to provide a photosensitive resin composition that can achieve high sensitivity, high resolution, and high adhesion to a metal wiring layer even when cured at low temperatures, a cured relief pattern manufactured using the above photosensitive resin composition, a method for manufacturing the same, and a semiconductor device.

[0009] The following describes in detail the forms for implementing this disclosure. However, this disclosure is not limited to the embodiments described below, and can be implemented in various modified forms within the scope of its essence.

[0010] Throughout this specification, structures represented by the same symbols in a general formula may be identical or different from each other if multiple such structures exist in a molecule.

[0011] 《Negative-type photosensitive resin composition》 The negative-type photosensitive resin composition of this disclosure comprises the following components: (A) a polyimide precursor or polyimide, (B) a photoradical initiator, and (C) a solvent, wherein the (C) solvent contains a compound represented by the following general formula (I). {In the formula, R 1 , R 2 , and R 3 Each of these is an organic group with 3 or fewer carbon atoms, and R 1 , R 2 , and R 3 At least one of them is an alkyl group having two or more carbon atoms.

[0012] In this specification, these components are referred to as "component (A)," etc. Optionally, the photosensitive resin composition of this disclosure may further contain (D) other components as components other than components (A) to (C).

[0013] In the above general formula (I), the organic group is preferably a hydrocarbon group. 1 , R 2 , and R 3When is a hydrocarbon group having 3 or fewer carbon atoms, the boiling point of the compound represented by the above general formula (I) is low, making it possible to achieve high sensitivity, high resolution, and high adhesion in the above photosensitive resin composition even with low-temperature curing. The reason why the effects of this disclosure are achieved by using the compound represented by the above general formula (I) is not clear, but the inventors assume the following. That is, the compound represented by the above general formula (I) tends to have a lower boiling point compared to compounds conventionally used as solvents, due to its lower polarity and weaker intermolecular forces. Because the boiling point of the solvent is low, the amount of residual solvent in the coating film obtained by applying the liquid photosensitive resin composition is reduced, and as a result, the mobility of the additives in the coating film is appropriately restricted. The restriction of the mobility of the photoinitiator and radical polymerizable monomer improves the resolution of the photosensitive resin composition, and the restriction of the mobility of the inhibitor leads to an improvement in the sensitivity of the photosensitive resin composition. Furthermore, when the above photosensitive resin composition contains an adhesion aid, the adhesion aid remains at the interface between the resin and the metal due to its restricted mobility, contributing to an improvement in the adhesion of the polyimide resin. Conventional photosensitive resin compositions may suffer performance degradation due to a large amount of residual solvent during low-temperature curing. Therefore, the photosensitive resin composition disclosed herein, which can exhibit high sensitivity, resolution, and adhesion even at low temperatures, can provide remarkable results.

[0014] From the viewpoint of further improving the sensitivity, resolution, and adhesion of the above photosensitive resin composition, the content of the compound represented by the above general formula (I) is preferably 20% to 80% by mass, more preferably 30 to 70% by mass, and even more preferably 50 to 65% by mass, based on the total mass of the above photosensitive resin composition.

[0015] Each component of the photosensitive resin composition of this disclosure is described below.

[0016] (A) Polyimide precursor or polyimide Component (A) of this disclosure contains (A-1) polyimide precursor or (A-2) polyimide. The embodiments of component (A-1) and component (A-2) are described below.

[0017] (A-1) Polyimide precursor The (A-1) polyimide precursor is a resin component included in the negative-type photosensitive resin composition, and any resin that forms polyimide by heat cyclization treatment can be used without particular limitations, however, the (A-1) component preferably has a polyamic acid ester structure represented by the following general formula (1). (In the formula, X 1 Y is a tetravalent organic group. 1 R is a divalent organic group. 4 and R 5 Each of these is independently a hydrogen atom or a monovalent organic group, and m is an integer between 2 and 100.

[0018] In the above general formula (1), X 1 The tetravalent organic group represented by is preferably an organic group having 6 to 40 carbon atoms, and more preferably -COOR, in that it can achieve both heat resistance and photosensitive properties. 4 Base and -COOR 5 It is an aromatic group or alicyclic aliphatic group in which the group and the -CONH- group are in the ortho position relative to each other. 1 Examples of tetravalent organic groups represented by the following general formula (X 1 Examples of groups having the structure represented by -1) include, but are not limited to, these.

[0019] Groups having the structure represented by {In the formula, R6 is a monovalent group selected from the group consisting of a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 10 carbon atoms, and a fluorine-containing hydrocarbon group having 1 to 10 carbon atoms; l is an integer selected from 0 to 2; m is an integer selected from 0 to 3; and n is an integer selected from 0 to 4.} are examples, but are not limited to these. Also, X 1 The structure may be one type or a combination of two or more types. The above formula (X 1 X having the structure represented by -1) 1 The base material is preferable from the viewpoint of achieving both heat resistance and photosensitive properties.

[0020] (X 1 Among the structures represented in -1), X 1Preferably, the base contains at least one of the structures represented by the following formulas (2) to (4).

[0021] In the above general formula (1), Y 1 The divalent organic group represented by the following formula (Y) is preferably an aromatic group having 6 to 40 carbon atoms, in terms of achieving both heat resistance and photosensitive properties, for example, the following formula (Y 1 -1): In the formula, R6 is a monovalent group selected from the group consisting of a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 10 carbon atoms, and a fluorine-containing hydrocarbon group having 1 to 10 carbon atoms, and n is an integer selected from 0 to 4. Also, Y 1 The structure can be one type or a combination of two or more types.

[0022] Y 1 As above, (Y 1 -1) Of these, from the viewpoint of Young's modulus and chemical resistance, it is preferable that it be a divalent organic group containing an aromatic group. More preferably, Y 1 Y has at least one of the structures represented by the following formulas (5) to (7). 1 The structure represented by the following formula (5) is expected to reduce the absorbance of the photosensitive resin composition and improve the elongation of the polyimide coating. 1 The structure represented by the following formula (6) and / or formula (7) is expected to improve the mechanical properties. (In the formula, R 6 (This is a hydrogen atom, an alkyl group, or a phenyl group.) (In the formula, R 7 and R 8 Each of these is independently either a hydrogen atom or a methyl group. (In the formula, R 9 and R 10 Each of these is independently either a hydrogen atom or a methyl group.

[0023] In the above general formula (1), R 4 and R 5At least one of the groups is preferably a monovalent organic group. The monovalent organic group preferably has 1 to 40 carbon atoms, and more preferably 1 to 30 carbon atoms. The monovalent organic group is preferably a group containing a radical polymerizable group, and is preferably a group represented by the following general formula (8). {In the formula, R 11 , R 12 and R 13 Each is independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and m 1 R in the above general formula (1) is an integer from 1 to 10, preferably an integer from 1 to 5, or an integer from 1 to 3. 4 and R 5 At least one of the groups is preferably a group containing a radical polymerizable group, more preferably a monovalent organic group having 1 to 40 carbon atoms, and more preferably a group represented by the general formula (8) above.

[0024] [(A-1) Method for preparing a polyimide precursor] The polyimide precursor represented by the above general formula (1) in this disclosure is, for example, a tetravalent organic group X having 6 to 40 carbon atoms as described above. 1 A tetracarboxylic dianhydride containing (a) is reacted with alcohols to prepare a partially esterified tetracarboxylic acid (hereinafter also called an acid / ester), and then a divalent organic group Y represented by the general formula (5) or general formula (6) is reacted with (a) alcohols, and then a divalent organic group Y represented by the general formula (5) or general formula (6) is reacted with (a) alcohols. 1 It is obtained by polycondensation with diamines containing [the specified compound]. The polyimide precursor may have a partially imidized structure. The upper limit of the imidization rate, based on the total number of polyimide precursors, is preferably less than 20%, less than 10%, or less than 5%. The lower limit of the imidization rate is preferably 0 or more. The above upper and lower limits can be selected as appropriate.

[0025] (Preparation of acid / ester compounds) In this disclosure, a tetravalent organic group X having 6 to 40 carbon atoms 1Examples of tetracarboxylic dianhydrides containing the above include 4,4'-oxydiphthalic acid dianhydride (ODPA), pyromellitic acid anhydride (PMDA), benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride (BPDA), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)1,4-phenylene, diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane. Furthermore, these can be used individually or in combination of two or more types.

[0026] By dissolving and mixing the above-mentioned tetracarboxylic dianhydride and (a) alcohols in a reaction solvent in the presence of a basic catalyst such as pyridine, the half-esterification reaction of the acid dianhydride proceeds, and the desired acid / ester product can be obtained. The reaction conditions are preferably stirred for 4 to 30 hours at a reaction temperature of 20 to 50°C.

[0027] The alcohols (a) used in the esterification reaction of the tetracarboxylic dianhydride described above are alcohols having an olefinic double bond. Specifically, these include 2-hydroxyethyl methacrylate (HEMA), 2-methacryloyloxyethyl alcohol, glycerin diacrylate, glycerin dimethacrylate, 2-acryloyloxyethyl alcohol, 1-acryloyloxy-3-propyl alcohol, 2-acrylamidoethyl alcohol, methylol vinyl ketone, 2-hydroxyethyl vinyl ketone, 2-hydroxy-3-methoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, and 2-hydroxy-3-t-butoxypropyl acrylate. Examples of alcohols that can be used include, but are not limited to, relate, 2-hydroxy-3-cyclohexyloxypropyl acrylate, 2-methacryloyloxyethyl alcohol, 1-methacryloyloxy-3-propyl alcohol, 2-methacrylamidoethyl alcohol, 2-hydroxy-3-methoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-phenoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-t-butoxypropyl methacrylate, and 2-hydroxy-3-cyclohexyloxypropyl methacrylate. These alcohols can be used individually or in combination of two or more.

[0028] The reaction solvent is preferably one that dissolves the acid / ester compound and the polyimide precursor, which is a polycondensation product of the acid / ester compound and diamines. Examples of reaction solvents include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, tetramethylurea, gamma-butyrolactone, ketones, esters, lactones, ethers, halogenated hydrocarbons, hydrocarbons, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methyl acetate, ethyl acetate, butyl acetate, diethyl oxalate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, chlorobenzene, o-dichlorobenzene, hexane, heptane, benzene, toluene, and xylene. These may be used individually or in combination of two or more as needed.

[0029] Examples of dehydration condensing agents include dicyclohexylcarbodiimide (DCC), diethylcarbodiimide, diisopropylcarbodiimide, ethylcyclohexylcarbodiimide, diphenylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, and 1-cyclohexyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride.

[0030] A divalent organic group Y that is preferably used in this disclosure 1Examples of diamines containing the above include 2,2'-dimethyl-4,4-diaminobiphenyl (m-TB), 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 2,2'-dimethyl-4,4'-diaminodiphenylmethane, 2,2'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dimethitoxy-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl, p-phenylenediamine, 2,5-dimethyl-1,4-phenylenediamine, and 4,4'-oxydianiline (ODA). These may be used individually or in combination of two or more. Furthermore, among these, it is preferable to use 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethoxy-4,4'-diaminobiphenyl, and p-phenylenediamine, and it is even more preferable to use 2,2'-dimethyl-4,4'-diaminobiphenyl and p-phenylenediamine.

[0031] After the reaction is complete, any water-absorbing by-products of the dehydrating condensation agent present in the reaction solution are filtered off as needed. Then, a poor solvent such as water, an aliphatic lower alcohol, or a mixture thereof is added to the obtained polymer component to precipitate it. Further purification of the polymer is carried out by repeating the redissolution and reprecipitation operations, and the polymer is then vacuum-dried to isolate the target polyimide precursor. To improve the degree of purification, the solution of this polymer may be passed through a column packed with anion exchange resin and / or cation exchange resin swollen with a suitable organic solvent to remove ionic impurities.

[0032] (A-2) Polyimide (A-2) Polyimide is a resin component included in the negative-type photosensitive resin composition, and preferably has a structure represented by the following general formula (9). (In the formula, X 2 Y is a tetravalent organic group. 2 (where n represents a divalent organic group, and n is an integer between 2 and 100.)

[0033] Since the negative-type photosensitive resin composition of this disclosure can be developed with an organic solvent, it is preferable that the above component (A-2) does not have an acidic group, and in general formula (9), X 2 , and Y 2 It is more preferable that the compound does not have an acidic group. Examples of acidic groups include carboxyl groups, phenolic hydroxyl groups, mercapto groups, and sulfo groups.

[0034] In general formula (9), X 2 Examples of tetravalent organic groups represented by the following general formula (X 2 Examples of groups having the structure represented by -1) include, but are not limited to, these.

[0035] In the above general formula (9), Y 2 The divalent organic group represented by the following formula (Y) is preferably an aromatic group having 6 to 40 carbon atoms, in that it can achieve both heat resistance and photosensitive properties, for example, the following formula (Y 2 Examples of structures include, but are not limited to, those represented in -1).

[0036] (A-2) Polyimides are preferably provided with radical polymerizable groups at the ends of the main chain from the viewpoint of mechanical strength (elongation). Although the theory is not limited to this, it is believed that the mechanical strength is improved by providing (meth)acryloyl groups at the ends of the main chain of polyimides. Examples of radical polymerizable groups include functional groups having (meth)acryloyl groups and (meth)acrylamide groups. (A-2) The structure of the radical polymerizable group that may be provided at the ends of the main chain of polyimides is not particularly limited, but for example, the structure shown in the general formula (M-1) below can be provided.

[0037] [(A-2) Method for preparing polyimide] (A-2) A method for preparing polyimide is, for example, the aforementioned tetravalent organic group X 1 A tetracarboxylic dianhydride containing the aforementioned divalent organic group Y 1It is obtained by reacting a diamine containing with a polyamic acid and then dehydrating and cyclizing the resulting polyamic acid by heat treatment. When obtaining a polyimide having a (meth)acryloyl group at the end of the main chain, the process includes reacting the end of the main chain (amino group or carboxyl group) of the polyimide obtained in the above step with a compound having a (meth)acryloyl group that can react with the functional group at the end.

[0038] The temperature at which the above polyamic acid is dehydrated and ring-closed by heat treatment is not particularly limited, but since the ring-closing reaction will not be completed at low temperatures, the lower limit is preferably 150°C or higher, and more preferably 160°C or higher. On the other hand, since side reactions will proceed at high temperatures, the upper limit is preferably 200°C or lower, and more preferably 180°C or lower.

[0039] In the photosensitive resin composition of this disclosure, the (A-2) polyimide may have a structure that is not partially imidized. The imidization rate of the (A-2) polyimide may be 80% or more, 90% or more, or 95% or more. Particularly preferably, the polyimide is fully imidized.

[0040] (A-2) There are no particular limitations on the tetracarboxylic dianhydrides that are suitably used to prepare polyimides, but specific examples include oxydiphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidene diphenoxy)diphthalic anhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 4,4'-(hexafluoroisopropylidene)diphthalic anhydride. These can be used individually, or two or more may be used in combination.

[0041] A divalent organic group Y that is preferably used in this disclosure 1The diamines containing these compounds are not particularly limited, but specific examples include 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(3-aminophenoxy)benzene, 6-(4-aminophenoxy)[1,1'-biphenyl]-3-amine, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]sulfone, 9,9-bis(4-aminophenyl)fluorene, 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine, and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane.

[0042] Specific examples of compounds having a (meth)acryloyl group that can react with the functional group at the end of the main chain of polyimide include isocyanate compounds such as 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate; chloride compounds such as acryloyl chloride and metachloroyl chloride; and alcohol compounds such as 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 4-hydroxyethyl methacrylate, and 4-hydroxyethyl acrylate.

[0043] The above isocyanate compounds react with the amino groups of the dehydrated, cyclized polyimide to form urea bonds, the above chloride compounds react with the amino groups of the dehydrated, cyclized polyimide to form amide bonds, and the above alcohol compounds react with the carboxyl groups of the dehydrated, cyclized polyimide to form ester bonds.

[0044] The method for reacting the above-mentioned isocyanate compounds is not particularly limited, but they can be reacted with the amino groups of dehydrated, ring-closed polyimides by stirring at room temperature.

[0045] The method for reacting the above-mentioned chloride compounds is not particularly limited, but it can be carried out by cooling a dehydrated, ring-closed polyimide solution on ice and adding the chloride compound dropwise.

[0046] The method for reacting the above alcohol-based compounds is not particularly limited, but they can be reacted with the carboxyl groups of dehydrated and cyclized polyimides using a condensing agent such as N,N'-dicyclohexylcarbodiimide or an esterification catalyst such as p-toluenesulfonic acid.

[0047] In the production of the polyimide described above (A-2), a reaction solvent may be used to efficiently carry out the reaction in a homogeneous system. The reaction solvent is not particularly limited as long as it can uniformly dissolve or suspend the tetracarboxylic dianhydride and the diamine, but examples include γ-butyrolactone, dimethyl sulfoxide, N,N-dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.

[0048] The (A-2) polyimide described above may be purified by known methods such as those described in Japanese Patent Publication No. 2012-194520. For example, methods include removing unreacted substances by dropping the (A-2) polyimide solution into water and reprecipitation, removing condensing agents and other substances insoluble in the reaction solvent by filtration, and removing the catalyst with an ion exchange resin. After these purification methods, the (A-2) polyimide may be dried by known methods and isolated in powder form.

[0049] (B) Photoradical initiators (B) Any compound that generates radicals upon irradiation with light can be used without particular limitations, and any compound conventionally used as a photoradical initiator for UV curing can be arbitrarily selected. For example, benzophenone derivatives such as benzophenone, o-benzoylmethyl benzoate, 4-benzoyl-4'-methyldiphenyl ketone, dibenzyl ketone, and fluorenone; acetophenone derivatives such as 2,2'-diethoxyacetophenone, 2-hydroxy-2-methylpropiophenone, and 1-hydroxycyclohexylphenyl ketone; thioxanthone derivatives such as thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, and diethylthioxanthone; benzyl derivatives such as benzyl, benzyldimethyl ketal, and benzyl-β-methoxyethyl acetal; benzoin derivatives such as benzoin and benzoin methyl ether; Preferred oximes include 1-phenyl-1,2-butanedione-2-(O-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(O-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(O-benzoyl)oxime, 1,3-diphenylpropanetrione-2-(O-ethoxycarbonyl)oxime, and 1-phenyl-3-ethoxypropanetrione-2-(O-benzoyl)oxime; N-arylglycines such as N-phenylglycine; peroxides such as benzoyl perchloride; and aromatic biimidazoles, but are not limited to these. These can be used individually or in combination of two or more. Among the above (B) photoradical initiators, oximes are particularly preferred in terms of photosensitivity.

[0050] (B) The content of the photoradical initiator is preferably 0.1 to 20 parts by mass, and more preferably 1 to 15 parts by mass, per 100 parts by mass of component (A).

[0051] (C) Solvent Component (C) of the present disclosure is used as a solvent in the photosensitive resin composition of the present disclosure, and as described above, by including the compound represented by the above general formula (I), it is possible to achieve high sensitivity, high resolution, and high adhesion even with low-temperature curing.

[0052] (C) The ratio of the compound represented by the above general formula (I) is not particularly limited, but from the viewpoint of the solubility of the additive in the composition and the reduction of foreign matter in the coating film, it is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60 to 100% by mass, and particularly preferably 70 to 100% by mass. If the content is above the lower limit of the above, the adhesion and sensitivity of the negative-type photosensitive resin composition can be further improved.

[0053] Furthermore, residual solvent in the polyimide coating formed by heat curing may impair the performance of the polyimide. Therefore, it is preferable to use a solvent with a lower boiling point as the heat curing temperature decreases. Preferably, the solvent of the compound represented by the above general formula (I) has a boiling point of less than 230°C at atmospheric pressure, more preferably less than 215°C, even more preferably less than 204°C, and particularly preferably less than 200°C. The lower limit is not particularly limited, but may be 160°C or higher, 165°C or higher, 170°C or higher, or 175°C or higher.

[0054] In the compound represented by the above general formula (I), R 1 , R 2 and R 3 At least one of them is an alkyl group having 2 or more carbon atoms. The organic group having 3 or fewer carbon atoms is preferably a hydrocarbon group having 3 or fewer carbon atoms, and may have an ethylenically unsaturated bond, but may not have an ethylenically unsaturated bond. Also, R 1 , R 2 and R 3 It is preferable that none of them have a ring-shaped structure.

[0055] A specific example of a compound represented by the above general formula (I) is, for example, the following formula (C-1): Examples of compounds represented by [the formula] are, but are not limited to, those shown. These may be used individually or in combination of two or more types.

[0056] The above-mentioned component (C) contains, from the viewpoint of sensitivity and resolution of the photosensitive resin composition, at least one compound selected from the group consisting of N,N-diethylacetamide, N,N-diethylacrylamide, and N,N-dimethylpropionamide, and from the viewpoint of adhesion, it more preferably contains N,N-diethylacetamide and / or N,N-dimethylpropionamide.

[0057] If desired, component (C) above can be used as a solvent for the photosensitive resin composition of this disclosure by mixing the compound represented by the above general formula (I) with other solvents other than the compound represented by the above general formula (I). Examples of other solvents include amides, sulfoxides, ureas, ketones, esters, lactones, ethers, halogenated hydrocarbons, hydrocarbons, and alcohols other than the above compound. More specifically, for example, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, dimethyl sulfoxide, tetramethylurea, tetraethylurea, 1,3-dimethyl-2-imidazolidinone, N,N'-dimethylpropyleneurea, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl acetate, ethyl acetate, butyl acetate, diethyl oxalate, ethyl lactate, methyl lactate, butyl lactate, γ- Butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, benzyl alcohol, phenyl glycol, tetrahydrofurfuryl alcohol, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, morpholine, dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, chlorobenzene, o-dichlorobenzene, anisole, hexane, heptane, benzene, toluene, xylene, mesitylene, etc. can be used. From the viewpoint of the sensitivity of the photosensitive resin composition, storage stability, and copper adhesion, it is preferable that the above other solvents include γ-butyrolactone or ethyl lactate.

[0058] The above component (C) does not necessarily have to contain sulfoxides, such as dimethyl sulfoxide, or cyclic amides, such as N-methyl-2-pyrrolidone or N-ethyl-2-pyrrolidone, as the other solvents.

[0059] The above-mentioned other solvents, when used in combination with the compound represented by the above-mentioned general formula (I), preferably contain a solvent (C') having a boiling point of less than 230°C at atmospheric pressure, for the same reasons as described above, in order to suitably exhibit the effects of this disclosure. The boiling point of solvent (C') is preferably less than 215°C, more preferably less than 210°C, even more preferably less than 205°C, and particularly preferably less than 200°C. The lower limit is not particularly limited, but may be 140°C or higher, 145°C or higher, 150°C or higher, 155°C or higher, 160°C or higher, 165°C or higher, 170°C or higher, or 175°C or higher.

[0060] As the solvent (C') above, γ-butyrolactone, dimethyl sulfoxide, ethyl lactate, or N,N-diethylformamide can be used. Of the other solvents mentioned above, it is preferable that they contain γ-butyrolactone or ethyl lactate from the viewpoint of the sensitivity of the photosensitive resin composition, storage stability, and copper adhesion.

[0061] The above-mentioned other solvents are preferably 36% by mass or less, more preferably 30% by mass or less, and even more preferably 24% by mass or less, based on the total mass of the photosensitive resin composition of this disclosure, from the viewpoint of suitably exhibiting the effects of the compound represented by the above-mentioned general formula (I). The lower limit is not particularly limited, but may be 0 or greater.

[0062] When the compound represented by the general formula (I) and the other solvents are mixed and used in component (C) above, the content of the compound represented by the general formula (I) is preferably 67 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 150 parts by mass or more, based on 100 parts by mass of the total amount of the other solvents. The upper limit is not particularly limited, but may be, for example, 2000 parts by mass or less, 1500 parts by mass or less, or 1000 parts by mass or less.

[0063] The above-mentioned component (C) is preferably present in an amount of 10 to 90% by mass, and more preferably 20 to 60% by mass, relative to the total mass of the photosensitive resin composition of this disclosure, in order to exhibit suitable fluidity as a solvent. The same applies when component (C) contains only the compound represented by the above-mentioned general formula (I).

[0064] Furthermore, the disclosure is not limited to a preferred mass ratio of component (C) to the total mass of the photosensitive resin composition, and the content of component (C) can be determined according to the desired coating film thickness and viscosity of the photosensitive resin composition. For example, it can be used in the range of 30 to 1500 parts by mass, and more preferably 100 to 1000 parts by mass, per 100 parts by mass of component (A).

[0065] (D) Other Components In this disclosure, the photosensitive resin composition may further contain (D) other components as components other than the components (A) to (C) above. Examples of components (D) include other resin components other than the polyimide precursors (A), radical polymerizable monomers, sensitizers, polymerization inhibitors, rust inhibitors, thermal base generators, hindered phenol compounds, thermal crosslinking agents, organotitanium compounds, silane coupling agents, and the like.

[0066] (Other resin components) The photosensitive resin composition of this disclosure may further contain resin components other than component (A). Examples of resin components that can be contained in the photosensitive resin composition of this disclosure include polyoxazole, polyoxazole precursor, phenolic resin, polyamide, epoxy resin, siloxane resin, acrylic resin, etc. The content of these resin components is preferably in the range of 0.01 parts by mass to 20 parts by mass per 100 parts by mass of component (A).

[0067] (Radical Polymerizable Monomers) To improve the resolution of the cured relief pattern, radical polymerizable monomers other than component (C) above may be optionally included in the photosensitive resin composition of this disclosure. The radical polymerizable monomer is not particularly limited as long as it is a compound that undergoes a radical polymerization reaction with a photopolymerization initiator, but it is preferably a (meth)acrylic compound.

[0068] Radical polymerizable monomers are not limited to the following examples, but include mono- or diacrylates and methacrylates of ethylene glycol or polyethylene glycol, such as diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate; mono- or diacrylates and methacrylates of propylene glycol or polypropylene glycol; mono-, di- or triacrylates and methacrylates of glycerol; cyclohexane diacrylate and dimethacrylate; diacrylate and dimethacrylate of 1,4-butanediol; diacrylate and dimethacrylate of 1,6-hexanediol; diacrylate and dimethacrylate of neopentyl glycol. Examples of compounds include methylates, mono- or diacrylates of bisphenol A and mono- or dimethacrylates of bisphenol A, benzene trimethacrylate, isobornyl acrylate and methacrylate, acrylamide and its derivatives, methacrylamide and its derivatives, trimethylolpropane triacrylate and methacrylate, di- or triacrylate and methacrylate of glycerol, di-, tri- or tetraacrylate and methacrylate of pentaerythritol, tricyclodecanedimethanol diacrylate, tris-(2-acryloxyethyl) isocyanurate, and ethylene oxide or propylene oxide adducts of these compounds. These can be used individually or in combination of two or more.

[0069] The content of the radical polymerizable monomer is preferably 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, and even more preferably 10 to 30 parts by mass, per 100 parts by mass of component (A). The above content further improves the resolution of the resulting cured relief pattern.

[0070] (Sensitizers) The photosensitive resin compositions of this disclosure may optionally contain sensitizers to improve photosensitivity. Examples of sensitizers of this disclosure include Michla's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, and p-dimethylaminocinnamyridene. Danonone, p-dimethylaminobenzylideneindanone, 2-(p-dimethylaminophenylbiphenylene)-benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3- Examples include cetyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin, N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, N-p-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzthiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, and 2-(p-dimethylaminobenzoyl)styrene. These can be used individually or in combinations of several types (for example, two to five types).

[0071] The amount of sensitizer is preferably 0.1 to 25 parts by mass per 100 parts by mass of component (A).

[0072] (Polymerization Inhibitors) The photosensitive resin compositions of this disclosure may optionally contain polymerization inhibitors to improve storage stability or resolution. Examples of polymerization inhibitors include hydroquinone, N-nitrosamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol etherdiaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 4-methoxyphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt, etc.

[0073] The polymerization inhibitor content is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.5 to 1.0 parts by mass, per 100 parts by mass of component (A). Photosensitive resin compositions in which the polymerization inhibitor is contained within the above range have further improved storage stability and resolution.

[0074] (Rust Inhibitor) In order to improve the adhesion between the film formed using the photosensitive resin composition of this disclosure and the substrate, a rust inhibitor may be optionally included in the photosensitive resin composition. The rust inhibitor only needs to be able to prevent metal rust, and examples include nitrogen-containing heterocyclic compounds. Examples of nitrogen-containing heterocyclic compounds include purines, purine derivatives, and azole derivatives. Preferably, the rust inhibitor is at least one compound selected from the group consisting of purines, purine derivatives, and azole derivatives.

[0075] Examples of purine derivatives include adenine, guanine, hypoxanthine, xanthine, theobromine, caffeine, uric acid, isoguanine, 2,6-diaminopurine, 2-acetamido-6-hydroxypurine, 9-methyladenine, 2-hydroxyadenine, 2-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, and N-(2-hydroxyethyl)adenine. Examples include 8-aminoadenine, 6-amino-8-phenyl-9H-purine, 1-ethyladenine, 6-ethylaminopurine, 1-benzyladenine, N-methylguanine, 7-(2-hydroxyethyl)guanine, N-(3-chlorophenyl)guanine, N-(3-ethylphenyl)guanine, 2-azaadenine, 5-azaadenine, 8-azaadenine, 8-azaguanine, 8-azapurine, 8-azaxanthine, and 8-azahypoxanthine, as well as derivatives thereof. These compounds may be used individually or in combination of two or more.

[0076] Examples of azole derivatives include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-t-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, and 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-benzo Examples include triazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, and 1-methyl-1H-tetrazole. These compounds may be used individually or in combination of two or more.

[0077] The amount of rust inhibitor is preferably 0.1 parts by mass to 5 parts by mass, more preferably 0.2 parts by mass to 2 parts by mass, even more preferably 0.4 parts by mass to 1 part by mass, and particularly preferably 0.5 parts by mass, per 100 parts by mass of component (A). The above blending ratio further improves the adhesion between the film formed using the photosensitive resin composition and the substrate.

[0078] (Thermobase Generating Agent) The negative-type photosensitive resin composition of this disclosure may contain a thermobase generating agent. A thermobase generating agent is a compound that generates a base when heated. The inclusion of a thermobase generating agent can further promote the imidization of the photosensitive resin composition. The type of thermobase generating agent is not particularly limited, but examples include amine compounds protected by a tert-butoxycarbonyl group, or thermobase generating agents disclosed in International Publication No. 2017 / 038598. However, it is not limited to these, and other known thermobase generating agents can be used.

[0079] Examples of amine compounds protected by the tert-butoxycarbonyl group include ethanolamine, 3-amino-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 4-amino-1-butanol, 2-amino-1-butanol, 1-amino-2-butanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-2-methyl-1-butanol, valinol, 3-amino-1,2-propanediol, and 2-amino-1,3-propane Diol, tyramine, norephedrine, 2-amino-1-phenyl-1,3-propanediol, 2-aminocyclohexanol, 4-aminocyclohexanol, 4-aminocyclohexaneethanol, 4-(2-aminoethyl)cyclohexanol, N-methylethanolamine, 3-(methylamino)-1-propanol, 3-(isopropylamino)propanol, N-cyclohexylethanolamine, α-[2-(methylamino)ethyl]benzyl alcohol, diethanol Luamine, diisopropanolamine, 3-pyrrolidinol, 2-pyrrolidinemethanol, 4-hydroxypiperidine, 3-hydroxypiperidine, 4-hydroxy-4-phenylpiperidine, 4-(3-hydroxyphenyl)piperidine, 4-piperidinemethanol, 3-piperidinemethanol, 2-piperidinemethanol, 4-piperidineethanol, 2-piperidineethanol, 2-(4-piperidyl)-2-propanol, 1,4-butanol bis(3-aminopropyl)A Examples include, but are not limited to, ter, 1,2-bis(2-aminoethoxy)ethane, 2,2'-oxybis(ethylamine), 1,14-diamino-3,6,9,12-tetraoxatetradecane, 1-aza-15-crown 5-ether, diethylene glycol bis(3-aminopropyl) ether, 1,11-diamino-3,6,9-trioxaundecane, or compounds in which the amino group of an amino acid or its derivative is protected by a tert-butoxycarbonyl group.

[0080] The amount of the thermal base generator is preferably 0.1 parts by mass or more and 30 parts by mass or less, and more preferably 1 part by mass or more and 20 parts by mass or less, per 100 parts by mass of component (A). The above blending amount is preferably 0.1 parts by mass or more from the viewpoint of the imidization promoting effect, and preferably 30 parts by mass or less from the viewpoint of the physical properties of the photosensitive resin layer after curing of the negative-type photosensitive resin composition.

[0081] (Hindered phenol compounds) To suppress discoloration on the copper surface, the negative-type photosensitive resin composition may optionally contain hindered phenol compounds. Examples of hindered phenol compounds include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), and 4,4'-butylidene-bis(3-methyl-6 3,6-Hexamethylenebis(3,5-di-t-butyl-4-hydroxyphenyl)propionate), 2,2-Thi-diethylenebis(3,5-di-t-butyl-4-hydroxyphenyl)propionate), 2,2-Thi-diethylenebis(3,5-di-t-butyl-4-hydroxyphenyl)propionate), N,N'-Hexamethylenebis(3,5-di-t-butyl-4-hydroxyphenyl)propionate), 2,2'-Methylenebis(4-methyl 6-t-butylphenol), 2,2'-methylene-bis(4-ethyl-6-t-butylphenol), pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)- 1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxyl C-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione,1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione,1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)- Trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3 Examples include, but are not limited to, 5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione. Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione is particularly preferred.

[0082] When the negative-type photosensitive resin composition contains a hindered phenol compound, the amount of the compound is preferably 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of component (A). The lower limit is more preferably 0.5 parts by mass or more, as this prevents discoloration and corrosion of the copper or copper alloy when the negative-type photosensitive resin composition is formed on copper or a copper alloy. The upper limit is more preferably 10 parts by mass or less, from the viewpoint of photosensitivity.

[0083] (Thermal Crosslinking Agent) The negative-type photosensitive resin composition of this disclosure may optionally contain a thermal crosslinking agent to improve heat resistance.

[0084] A thermal crosslinking agent refers to a compound that undergoes an addition reaction or condensation polymerization reaction upon exposure to heat. These reactions occur in combinations of component (A) and the thermal crosslinking agent, between thermal crosslinking agents, and between the thermal crosslinking agent and other components, and the reaction temperature is preferably 150°C or higher.

[0085] Examples of thermal crosslinking agents include alkoxymethyl compounds, epoxy compounds, oxetane compounds, bismaleimide compounds, allyl compounds, and blocked isocyanate compounds. From the viewpoint of suppressing curing shrinkage, it is preferable that the thermal crosslinking agent contains nitrogen atoms.

[0086] Examples of alkoxymethyl compounds include, but are not limited to, the following compounds.

[0087]

[0088] Examples of epoxy compounds include 4-hydroxybutyl acrylate glycidyl ether, epoxy compounds containing a bisphenol A group, and hydrogenated bisphenol A diglycidyl ether (e.g., Epolite 4000 manufactured by Kyoeisha Chemical Co., Ltd.). Examples of oxetane compounds include 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, bis[1-ethyl(3-oxetanyl)]methyl ether, 4,4'-bis[(3-ethyl-3-oxetanyl)methyl]biphenyl, 4,4'-bis(3-ethyl-3-oxetanylmethoxy)biphenyl, ethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, diethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, and bis(3-ethyl-3-oxetanylmethyl) Examples include diphenoates, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl) ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl) ether, poly[[3-[(3-ethyl-3-oxetanyl)methoxy]propyl]silasesquioxane] derivatives, oxetanyl silicates, phenol novolac type oxetanes, 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, OXT121 (manufactured by Toagosei, trade name), OXT221 (manufactured by Toagosei, trade name), etc.

[0089] Examples of bismaleimide compounds include 1,2-bis(maleimide)ethane, 1,3-bis(maleimide)propane, 1,4-bis(maleimide)butane, 1,5-bis(maleimide)pentane, 1,6-bis(maleimide)hexane, 2,2,4-trimethyl-1,6-bis(maleimide)hexane, N,N'-1,3-phenylenebis(maleimide), 4-methyl-N,N'-1,3-phenylenebis(maleimide), N,N'-1,4-phenylenebis(maleimide), 3-methyl-N,N'-1,4-phenylenebis(maleimide), 4,4'-bis(maleimide)diphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-bis(maleimide)diphenylmethane, or 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane.

[0090] Examples of allyl compounds include allyl alcohol, allylanisole, allyl benzoate, allyl cinnamate, N-alyloxyphthalimide, allylphenol, allylphenylsulfone, allylurea, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl maleate, diallyl isocyanurate, triallylamine, triallyl isocyanurate, triallyl cyanurate, triallylamine, 1,3,5-benzenetricarboxylic acid triallyl, trimellitate triallyl, triallyl phosphate, triallyl phosphite, and triallyl citrate.

[0091] Examples of blocked isocyanate compounds include hexamethylene diisocyanate-based blocked isocyanates (e.g., Duranate SBN-70D, SBB-70P, SBF-70E, TPA-B80E, 17B-60P, MF-B60B, E402-B80B, MF-K60B, and WM44-L70G from Asahi Kasei Corporation, Takenate B-882N from Mitsui Chemicals, Inc., and 7960, 7961, 7982, 7991, and 7992 from Baxenden, etc.), tolylene diisocyanate-based blocked isocyanates (e.g., Takenate B-830 from Mitsui Chemicals, Inc.), 4 Examples include 4'-diphenylmethane diisocyanate-based blocked isocyanates (e.g., Takenate B-815N manufactured by Mitsui Chemicals, Inc., Bronate PMD-OA01 and PMD-MA01 manufactured by Daiei Sangyo Co., Ltd.), 1,3-bis(isocyanatemethyl)cyclohexane-based blocked isocyanates (e.g., Takenate B-846N manufactured by Mitsui Chemicals, Inc., Coronate BI-301, 2507 and 2554 manufactured by Tosoh Corporation), and isophorone diisocyanate-based blocked isocyanates (e.g., 7950, 7951 and 7990 manufactured by Baxenden).

[0092] Among these, alkoxymethyl compounds and bismaleimide compounds are preferred from the viewpoint of storage stability. The thermal crosslinking agent may be used alone or in combination of two or more types.

[0093] (Organotitanium Compounds) The photosensitive resin composition of this disclosure may contain organotitanium compounds for the purpose of improving elongation after a humid heat endurance test. There are no particular limitations on the organotitanium compounds that can be used, as long as an organic chemical substance is bonded to a titanium atom via covalent or ionic bonds.

[0094] Specific examples of organotitanium compounds are shown below in I) to VII): I) Titanium chelate compounds: Titanium chelate compounds having two or more alkoxy groups are preferred because they provide good storage stability and a good pattern for the photosensitive resin composition of this disclosure. Specific examples include titanium bis(triethanolamine)diisopropoxide, titanium di(n-butoxide)bis(2,4-pentanedione), titanium diisopropoxidebis(2,4-pentanedione), titanium diisopropoxidebis(tetramethylheptanedione), and titanium diisopropoxidebis(ethylacetoacetate).

[0095] II) Tetraalkoxy titanium compounds: For example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearaloxide, and titanium tetrakis[bis{2,2-(alyloxymethyl)butoxide}].

[0096] III) Titanocene compounds: For example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, and bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrole-1-yl)phenyl)titanium.

[0097] IV) Monoalkoxy titanium compounds: For example, titanium tris(dioctyl phosphate) isopropoxide and titanium tris(dodecylbenzenesulfonate) isopropoxide.

[0098] V) Titanium oxide compounds: For example, titanium oxide bis(pentanedione) and titanium oxide bis(tetramethylheptanedione), phthalocyanine titanium oxide, etc.

[0099] VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate, etc.

[0100] VII) Titanate coupling agents: For example, isopropyltridodecylbenzenesulfonyl titanate.

[0101] Among the above I) to VII), it is preferable from the viewpoint of achieving better chemical resistance that the organotitanium compound is at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds. In particular, titanium diisopropoxide bis(ethyl acetoacetate), titanium tetra(n-butoxide), and bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrole-1-yl)phenyl)titanium are preferred.

[0102] The content of these organotitanium compounds is preferably 0.01 to 10 parts by weight, and more preferably 0.1 to 2 parts by weight, per 100 parts by weight of component (A). If the content is less than 0.01 parts by weight, the desired adhesion will not be achieved, and if it exceeds 10 parts by weight, the storage stability may be poor.

[0103] (Silane Coupling Agent) The negative-type photosensitive resin composition of the present disclosure may further contain a silane coupling agent. Examples of silane coupling agents include γ-aminopropyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, dimethoxymethyl-3-piperidinopropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-diethoxymethylsilylpropyl)succinimide, and N-[3-(triethoxysilyl) Examples of silane coupling agents include propyl phthalamide, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamide)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride, N-phenylaminopropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, and 3-(trialkoxysilyl)propylsuccinic anhydride.

[0104] More specifically, as silane coupling agents, there are 3-mercaptopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: product name KBM803, manufactured by Chisso Corporation: product name Cyra Ace S810), 3-mercaptopropyltriethoxysilane (manufactured by Azmax Co., Ltd.: product name SIM6475.0), 3-mercaptopropylmethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: product name LS1375, manufactured by Azmax Co., Ltd.: product name SIM6474.0), mercaptomethyltrimethoxysilane (manufactured by Azmax Co., Ltd.: product name SIM6473.5C), and mercaptomethylmethyldimethoxysilane (manufactured by Azmax Co., Ltd.: product name SIM6473.0), 3-mercaptopropyldiethoxymethoxysilane, 3-mercaptopropylethoxydimethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropyldiethoxypropoxysilane, 3-mercaptopropylethoxydipropoxysilane, 3-mercaptopropyldimethoxypropoxysilane, 3-mercaptopropylmethoxydipropoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyldiethoxymethoxysilane, 2-mercapto Toethylethoxydimethoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethylethoxydipropoxysilane, 2-mercaptoethyldimethoxypropoxysilane, 2-mercaptoethylmethoxydipropoxysilane, 4-mercaptobutyltrimethoxysilane, 4-mercaptobutyltriethoxysilane, 4-mercaptobutyltripropoxysilane, N-(3-triethoxysilylpropyl)urea (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name) LS3610, manufactured by Azmax Co., Ltd.: product name SIU9055.0), N-(3-trimethoxysilylpropyl)urea (manufactured by Azmax Co., Ltd.: product name SIU9058.0), N-(3-diethoxymethoxysilylpropyl)urea, N-(3-ethoxydimethoxysilylpropyl)urea, N-(3-tripropoxysilylpropyl)urea, N-(3-diethoxypropoxysilylpropyl)urea, N-(3-ethoxydipropoxysilylpropyl)urea, N-(3-dimethoxypropoxysilylpropyl)urea,N-(3-methoxydipropoxysilylpropyl)urea, N-(3-trimethoxysilylethyl)urea, N-(3-ethoxydimethoxysilylethyl)urea, N-(3-tripropoxysilylethyl)urea, N-(3-tripropoxysilylethyl)urea, N-(3-ethoxydipropoxysilylethyl)urea, N-(3-dimethoxypropoxysilylethyl)urea, N-(3-methoxydipropoxysilylethyl)urea, N-(3-trimethoxysilylbutyl)urea, N-(3-triethoxysilylbutyl)urea, N-(3-tripropoxysilylbutyl)urea, 3-(m-aminophenoxy)propyltrimethoxysilane (manufactured by Azmax Co., Ltd.: product name SLA0598.0), m-aminophenyltrimethoxysilane (manufactured by Azmax Co., Ltd.: product name) SLA0599.0), p-aminophenyltrimethoxysilane (manufactured by Azmax Co., Ltd.: product name SLA0599.1), aminophenyltrimethoxysilane (manufactured by Azmax Co., Ltd.: product name SLA0599.2), 2-(trimethoxysilylethyl)pyridine (manufactured by Azmax Co., Ltd.: product name SIT8396.0), 2-(triethoxysilylethyl)pyridine, 2-(dimethoxysilylmethylethyl)pyridine, 2-(diethoxysilylmethylethyl)pyridine, (3-triethoxysilylpropyl)-t-butylcarbamate, (3-glycidoxypropyl)triethoxysilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-i-propoxysilane, tetra-n-butoxysilane, tetra-i-butoxysilane, tetra-t-butoxysilane, tetrakis(methoxyethoxysilane), te Trakis(methoxy-n-propoxysilane), tetrakis(ethoxyethoxysilane), tetrakis(methoxyethoxyethoxysilane), bis(trimethoxysilyl)ethane, bis(trimethoxysilyl)hexane, bis(triethoxysilyl)methane, bis(triethoxysilyl)ethane, bis(triethoxysilyl)ethylene, bis(triethoxysilyl)octane, bis(triethoxysilyl)octadiene, bis[3-(triethoxysilyl)propyl]disulfide, bis[3-(triethoxysilyl)propyl]tetrasulfide,Di-t-butoxydiacetoxysilane, di-i-butoxyaluminoxytriethoxysilane, phenylsilanetriol, methylphenylsilanediol, ethylphenylsilanediol, n-propylphenylsilanediol, isopropylphenylsilanediol, n-butylsiphenylsilanediol, isobutylphenylsilanediol, tert-butylphenylsilanediol, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, ethylmethylphenylsilanol, n-propylmethylphenylsilanol, isopropylmethylphenylsilanol, n-butyl Examples include, but are not limited to, methylphenylsilanol, isobutylmethylphenylsilanol, tert-butylmethylphenylsilanol, ethyl n-propylphenylsilanol, ethyl isopropylphenylsilanol, n-butylethylphenylsilanol, isobutylethylphenylsilanol, tert-butylethylphenylsilanol, methyldiphenylsilanol, ethyldiphenylsilanol, n-propyldiphenylsilanol, isopropyldiphenylsilanol, n-butyldiphenylsilanol, isobutyldiphenylsilanol, tert-butyldiphenylsilanol, and triphenylsilanol. These may be used individually or in combination.

[0105] The negative-type photosensitive resin composition of this disclosure is suitably used for forming a buffer coat layer or redistribution layer of a semiconductor package.

[0106] A method for manufacturing a cured relief pattern is provided, comprising the following steps (1) to (4) in one embodiment of the present disclosure: (1) applying the photosensitive resin composition of the above-described embodiment onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the photosensitive resin layer after exposure to form a relief pattern; and (4) heat-treating the relief pattern to form a cured relief pattern.

[0107] The following describes each step. (1) Step of applying the photosensitive resin composition of the present disclosure onto a substrate to form a photosensitive resin layer on the substrate In this step, the photosensitive resin composition of the above-described embodiment is applied onto a substrate (in one embodiment, a base material), and if necessary, is then dried to form a photosensitive resin layer. As for the application method, methods that have been conventionally used for applying photosensitive resin compositions, such as application using a spin coater, bar coater, blade coater, curtain coater, screen printing machine, etc., or spray application using a spray coater, etc., can be used.

[0108] If necessary, the coating film made of the photosensitive resin composition of this disclosure can be dried, and drying methods such as air drying, heating with an oven or hot plate, or vacuum drying can be used. Furthermore, it is desirable to dry the coating film under conditions that do not promote the imidization of component (A) in the photosensitive resin composition of this disclosure. Specifically, when air drying or heating drying is performed, drying can be carried out at 20°C to 140°C for 1 minute to 1 hour. Heating at 90°C to 140°C for 120 seconds to 500 seconds is preferable, and heating at 100°C to 120°C for 180 seconds to 480 seconds is more preferable. A photosensitive resin layer can be formed on the substrate by the above steps.

[0109] (2) Exposure process for the photosensitive resin layer In this process, the photosensitive resin layer formed in step (1) above is exposed to ultraviolet light or the like using an exposure device such as a contact aligner, mirror projection, or stepper, either through a photomask or reticle having a pattern, or directly.

[0110] Subsequently, if necessary, post-exposure baking (PEB) and / or pre-development baking may be performed using any combination of temperature and time to improve photosensitivity, etc. The baking conditions are preferably in the range of 40°C to 120°C and 10 seconds to 240 seconds, but are not limited to this range as long as they do not impair the properties of the photosensitive resin composition of this disclosure.

[0111] (3) Process of developing the photosensitive resin layer after exposure to form a relief pattern In this process, the unexposed portion of the photosensitive resin layer after exposure is developed and removed. As a development method for developing the photosensitive resin layer after exposure (irradiation), any method can be selected and used from conventionally known photoresist development methods, such as the rotary spray method, the paddle method, and the immersion method with ultrasonic treatment. In addition, after development, if necessary, a post-development bake may be performed using any combination of temperature and time for purposes such as adjusting the shape of the relief pattern.

[0112] As the developer used for development, for example, a good solvent for the photosensitive resin composition of this disclosure, or a combination of the good solvent and a poor solvent is preferred. Preferred good solvents include, for example, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, and α-acetyl-γ-butyrolactone. Preferred poor solvents include, for example, toluene, xylene, methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol monomethyl ether acetate, and water. When using a mixture of the good solvent and the poor solvent, it is preferable to adjust the ratio of the poor solvent to the good solvent according to the solubility of the polymer in the photosensitive resin composition of this disclosure. Furthermore, two or more types of each solvent can be used in combination, for example, several types.

[0113] After development, post-development baking (PDB) may be performed using any combination of temperature and time as needed for purposes such as adjusting the pattern shape. The baking conditions are preferably in the range of 40°C to 160°C and 10 seconds to 300 seconds, but are not limited to this range as long as they do not impair the properties of the photosensitive resin composition of this disclosure.

[0114] (4) Process of heating the relief pattern to form a cured relief pattern In this process, the relief pattern obtained by the above development is heated to dilute the photosensitive component and promote the imidization reaction of component (A), thereby converting it into a cured relief pattern made of a polyimide resin film. Various methods can be selected for heat curing, such as using a hot plate, using an oven, or using a heating oven with a temperature program that can be set. Heating can be carried out, for example, at 170°C to 400°C for 30 minutes to 5 hours, preferably 250°C or lower, and more preferably 230°C or lower. Air may be used as the atmospheric gas during heat curing, or an inert gas such as nitrogen or argon may be used.

[0115] Cured Relief Pattern The cured relief pattern of this disclosure includes a cured product of the photosensitive resin composition described above. Furthermore, the cured relief pattern includes a cured relief pattern obtained by the method for producing the cured relief pattern described above.

[0116] 《Semiconductor Devices》 In this disclosure, a semiconductor device is also provided that includes a cured relief pattern obtained by the cured relief pattern manufacturing method described above. Therefore, a semiconductor device is provided having a substrate which is a semiconductor element and a polyimide cured relief pattern formed on the substrate by the cured relief pattern manufacturing method described above. Furthermore, this disclosure can also be applied to a method for manufacturing a semiconductor device that uses a semiconductor element as a substrate and includes the cured relief pattern manufacturing method described above as part of the process. The semiconductor device of this disclosure can be manufactured by forming the cured relief pattern formed by the cured relief pattern manufacturing method as a surface protective film, an interlayer insulating film, a redistribution insulating film, a protective film for a flip-chip device, or a protective film for a semiconductor device having a bump structure, and combining it with a known method for manufacturing a semiconductor device.

[0117] <Display Device> This disclosure provides a display device comprising a display element and a cured film provided on the upper part of the display element, wherein the cured film is the cured relief pattern described above. Here, the cured relief pattern may be laminated in direct contact with the display element, or it may be laminated with another layer in between. For example, the cured film can be a surface protective film, insulating film, and planarization film for TFT liquid crystal display elements and color filter elements, a projection for an MVA type liquid crystal display device, and a partition wall for the cathode of an organic EL element.

[0118] In addition to applications in semiconductor devices as described above, the photosensitive resin composition of this disclosure is also useful for applications such as interlayer insulation of multilayer circuits, cover coatings for flexible copper-clad sheets, solder resist films, and liquid crystal alignment films.

[0119] The following describes examples taken to clarify the effects of this disclosure, but this disclosure is not limited to these examples. The following materials and measurement methods were used in the examples.

[0120] <Measurement and Evaluation Method> - Sensitivity Evaluation A 6-inch silicon wafer, on which a vapor-deposited layer of 200 nm Ti and 400 nm Cu was deposited on the surface using a sputtering apparatus (L-440S-FHL type, manufactured by Canon Anelva Corporation), was spin-coated with the photosensitive resin composition prepared as described below using a spin coater (product name: D-SPIN60A, manufactured by SOKUDO Corporation) to a film thickness of 7.5 μm, and pre-baked at 110°C for 4 minutes. The resulting coating film was then exposed to an exposure dose of 150 mJ / cm using a stepper FP-3030iWa (manufactured by Canon Corporation) with an exposure wavelength of i-line (365 nm) through a reticle with a test pattern. 2 ~750 mJ / cm 2 i-ray light at 50 mJ / cm 2The material was exposed by irradiating it in small increments. Next, using a D-SPIN60A developer (manufactured by SOKUDO), a rotary spray development was performed at 23°C with cyclopentanone as the developer for a time equal to 1.4 times the time until the unexposed areas completely dissolved and disappeared. Subsequently, a rotary spray rinse was performed for 10 seconds using propylene glycol monomethyl ether acetate to obtain a relief pattern made of resin film. The exposure amount at which the film thickness of the obtained pattern became 85% of the coated film thickness was evaluated as the sensitivity of the resin composition.

[0121] - Evaluation of foreign matter The pattern films obtained above were observed in dark-field mode using an optical microscope (Nikon ECLIPSE LV150). Patterns in which no bright spots were observed were marked with ○, and those in which foreign matter was observed as bright spots were marked with ×.

[0122] - Resolution Evaluation The pattern films obtained above were cured in a vertical curing furnace VF200B (manufactured by Koyo Thermo Systems Co., Ltd.) under a nitrogen atmosphere at 230°C for 2 hours to obtain cured relief patterns with a film thickness of 5 μm. The shape of each pattern was observed using a scanning electron microscope (Hitachi High-Technogies S-4800) with a reticle size of 5 μm tilted at 30° and at a magnification of 10 k. Patterns with no residue at the bottom, smooth side walls, and no abnormal protrusions were evaluated as "acceptable," while patterns with residue at the bottom or abnormal side walls were evaluated as "unacceptable."

[0123] - Copper adhesion evaluation (peel strength test) A 6-inch silicon wafer, on which a vapor-deposited layer of 200 nm Ti followed by a 400 nm Cu layer was prepared using a sputtering apparatus (L-440S-FHL type, manufactured by Canon Anelva Corporation), was spin-coated with the photosensitive resin compositions prepared in the examples and comparative examples to a thickness of 10 μm, and pre-baked at 110°C for 4 minutes. Then, a stepper FP-3030iWa (manufactured by Canon Corporation) was used to measure 500 mJ / cm². 2A wafer with a polyimide resin film was fabricated by exposing it to i-ray light and then heat-curing it in a vertical curing furnace (Koyo Lindbergh, model VF-2000B) under a nitrogen atmosphere at 230°C for 2 hours. The peel strength may be the peel strength between aluminum and polyimide film measured according to the 180-degree peel method of JIS K6854-1 using a sample with a polyimide film formed on a substrate. The peel strength was measured under the following conditions: Equipment name: RTG-1210 (A&D Company, Limited) Measurement temperature: Room temperature Peeling rate: 50 mm / min Atmosphere: Air Sample width: 5 mm

[0124] Furthermore, the copper adhesion of the photosensitive resin composition was evaluated according to the following criteria: A: Peel strength of 0.30 N / mm or more B: Peel strength of 0.10 N / mm or more and less than 0.30 N / mm C: Peel strength less than 0.10 N / mm If the evaluation is A or B, it can be suitably used as the photosensitive resin composition of this disclosure.

[0125] <Synthesis Example 1> (Polymer A1: Synthesis of Polyimide Precursor) 62.0 g (0.2 mol) of 4,4'-oxydiphthalic acid dianhydride (ODPA) was placed in a 2 L separable flask, and 52.1 g (0.40 mol) of 2-hydroxyethyl methacrylate (HEMA) and 400 mL of γ-butyrolactone were added. While stirring at room temperature, 31.6 g (0.40 mol) of pyridine was added to obtain a reaction mixture. After the exothermic reaction was complete, the reaction mixture was allowed to cool to room temperature and stirred for 16 hours. Next, under ice cooling, a solution of 81.3 g of dicyclohexylcarbodiimide (DCC) dissolved in 80.00 g of γ-butyrolactone was added to the reaction mixture over 30 minutes while stirring. Subsequently, 19.7 g of p-phenylenediamine (p-PD) suspended in 100 mL of γ-butyrolactone was added over 60 minutes while stirring. After stirring at room temperature for 4 hours, 30 mL of ethyl alcohol was added and the mixture was stirred for 30 minutes, followed by the addition of 400 mL of γ-butyrolactone. The precipitate formed in the reaction mixture was removed by filtration to obtain the reaction solution.

[0126] To the resulting reaction solution, 3 L of ethanol was added to produce a precipitate consisting of crude polymer. The crude polymer was filtered off and dissolved in 600 g of γ-butyrolactone to obtain a crude polymer solution. The obtained crude polymer solution was added dropwise to 6 L of water to precipitate the polymer, and the resulting precipitate was filtered off and then vacuum-dried at 40°C for 72 hours to obtain a powdered polymer (polymer I).

[0127] <Synthesis Example 2> (Polymer A2: Synthesis of Polyimide Precursor) 24.8 g (0.08 mol) of 4,4'-oxydiphthalic acid dianhydride (ODPA) and 26.2 g (0.12 mol) of pyromellitic acid dianhydride (PMDA) were placed in a 2 L separable flask and 74.9 g of γ-butyrolactone was added. Next, 52.1 g (0.40 mol) of 2-hydroxyethyl methacrylate (HEMA) was added, and while stirring, 31.6 g (0.40 mol) of pyridine was added, and the mixture was then stirred at room temperature for 16 hours.

[0128] Next, the reaction mixture was cooled to below 0°C, and a solution of 81.3 g of dicyclohexylcarbodiimide (DCC) dissolved in 80.00 g of γ-butyrolactone was added over 20 minutes while stirring. Subsequently, while maintaining the reaction temperature below 2°C, a solution of 38.2 g (0.18 mol) of 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB) dissolved in 80.00 g of γ-butyrolactone was added dropwise over 30 minutes. The reaction mixture was then raised to room temperature and stirred for 4 hours at room temperature. Finally, 13.66 g of ethanol was added as a terminal sealant and stirred for 30 minutes. The precipitate formed in the reaction mixture was removed by filtration to obtain the reaction solution.

[0129] To the resulting reaction solution, 3 L of ethanol was added to produce a precipitate consisting of crude polymer. The crude polymer was filtered off and dissolved in 600 g of γ-butyrolactone to obtain a crude polymer solution. The obtained crude polymer solution was added dropwise to 6 L of water to precipitate the polymer, and the resulting precipitate was filtered off and then vacuum-dried at 40°C for 72 hours to obtain powdered polymer (polymer II).

[0130] <Synthesis Example 3> (Polymer A3: Synthesis of Polyimide) A Dean-Stark extractor was attached, and 100.0 g of N-methylpyrrolidone (hereinafter NMP) and 27.7 g (0.10 mol) of 6-(4-aminophenoxy)[1,1'-biphenyl]-3-amine were added to a nitrogen-purged three-necked flask and dissolved. To this, 15.6 g (0.05 mol) of 4,4'-oxydiphthalic acid dianhydride (ODPA) and 25.0 g of toluene were added and heated to 180°C. After confirming that the theoretical amount of water (1.80 g) and the added toluene (25.0 g) had been extracted into the Dean-Stark extractor, heating was stopped and the mixture was cooled to room temperature.

[0131] To the resulting reaction solution, 15.5 g (0.1 mol) of 2-methacryloyloxyethyl isocyanate (Kalenz MOI, trade name: Resonaq Corporation) was added and stirred to obtain a polymer solution. The obtained polymer solution was added dropwise to 3 kg of water to precipitate the polymer, and after filtering off the precipitate, it was vacuum-dried at 40°C for 72 hours to obtain a powdered polymer (polymer III).

[0132] The components used in the examples and comparative examples are as follows:

[0133] (A) Polyimide precursors or polymers A1-A3 obtained in polyimide production examples (B) Photoradical initiators (B1) 1-phenyl-2-[(benzoyloxy)imino]-1-propanone (B2) Irgacure OXE-01 (C) Solvents (C1) N,N-diethylacetamide (boiling point: 185°C) (C2) N,N-dimethylpropionamide (boiling point: 176°C) (C3) N,N-diethylacrylamide (boiling point: 190°C) (C4) 3-methoxy-N,N-dimethylpropanamide (boiling point at 98.3 kPa: 215°C) (C5) N,N'-dimethylpropylene urea (boiling point: 246°C) (C6) γ-butyrolactone (boiling point: 204°C) (C7) ethyl lactate (boiling point: 154°C) (D) Other components (radical polymerizable monomers) (D1) Tetraethylene glycol dimethacrylate (D2) Tris-(2-acryloxyethyl) isocyanurate (sensitizer) (E1) N-phenyldiethanolamine (inhibitor) (F1) 4-methoxyphenol (rust inhibitor) (G1) 8-azaadenine

[0134] <Examples 1-12, Comparative Examples 1-4> The photosensitive resin compositions of Examples 1-12 and Comparative Examples 1-4 were prepared by mixing the polymer and additives shown in Table 1, stirring at 23°C for 24 hours, and then filtering through a PTFE filter with a pore size of 1 μm. The obtained photosensitive resin compositions were evaluated for sensitivity, foreign matter, resolution, and copper adhesion using the method described above. The evaluation results are summarized in Table 1.

[0135]

[0136]

[0137]

[0138] As shown in Table 1, the polyimides obtained from the photosensitive resin compositions of the examples showed higher sensitivity, higher resolution, and better adhesion compared to the photosensitive resin compositions of the comparative examples. Furthermore, when the content of compounds containing specific amide structures is high as a solvent, the solubility of each component of the photosensitive resin composition is improved, and the generation of foreign matter can be suppressed.

[0139] By using the photosensitive resin composition according to this disclosure, it is possible to form an insulating layer that exhibits excellent film properties and good adhesion to metal electrodes when cured, and to stably open via patterns. This makes it suitably applicable in the field of photosensitive materials useful for the manufacture of electrical and electronic materials such as semiconductor devices and multilayer wiring boards.

Claims

(A) Polyimide precursor or polyimide, (B) Photoradical initiator, and (C) Solvent A negative-type photosensitive resin composition containing, wherein the (C) solvent contains a compound represented by the following general formula (I). {In the formula, R 1 , R 2 , and R 3 Each of these is an organic group with 3 or fewer carbon atoms, and R 1 , R 2 , and R 3 Of these, at least one is an alkyl group having two or more carbon atoms.   The negative-type photosensitive resin composition according to claim 1, comprising more than 50% by mass of the compound represented by the general formula (I) based on the total mass of the solvent (C).   The negative-type photosensitive resin composition according to claim 1 or 2, comprising 10 to 90% by mass of the compound represented by the general formula (I) based on the total mass of the negative-type photosensitive resin composition.   The negative-type photosensitive resin composition according to claim 1 or 2, wherein the boiling point of the compound represented by the general formula (I) is less than 215°C under atmospheric pressure.   The negative-type photosensitive resin composition according to claim 1 or 2, wherein the solvent (C) contains at least one compound selected from the group consisting of N,N-diethylacetamide, N,N-diethylacrylamide, and N,N-dimethylpropionamide.   The negative-type photosensitive resin composition according to claim 1 or 2, wherein the solvent further comprises other solvents other than the compound represented by the general formula (I).   The other solvents mentioned above include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, dimethyl sulfoxide, tetramethylurea, tetraethylurea, 1,3-dimethyl-2-imidazolidinone, N,N'-dimethylpropyleneurea, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl acetate, ethyl acetate, butyl acetate, diethyl oxalate, ethyl lactate, methyl lactate, butyl lactate, and γ-butyrolactone. The negative-type photosensitive resin composition according to claim 6, comprising propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, benzyl alcohol, phenyl glycol, tetrahydrofurfuryl alcohol, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, morpholin, dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, chlorobenzene, o-dichlorobenzene, anisole, hexane, heptane, benzene, toluene, xylene, or mesitylene.   The negative-type photosensitive resin composition according to claim 6, wherein the other solvent comprises γ-butyrolactone or ethyl lactate.   The negative-type photosensitive resin composition according to claim 6, wherein the other solvent does not contain N-methyl-2-pyrrolidone.   The negative-type photosensitive resin composition according to claim 6, wherein the other solvent includes a solvent (C') having a boiling point of less than 215°C at atmospheric pressure.   The negative-type photosensitive resin composition according to claim 10, wherein the solvent (C') comprises γ-butyrolactone, dimethyl sulfoxide, ethyl lactate, or N,N-diethylformamide.   Furthermore, the negative-type photosensitive resin composition according to claim 1 or 2, comprising a radical polymerizable monomer other than the solvent (C) mentioned above.   Furthermore, the negative-type photosensitive resin composition according to claim 1 or 2, comprising a polymerization inhibitor.   Furthermore, the negative-type photosensitive resin composition according to claim 1 or 2, comprising a thermobase generating agent.   Furthermore, the negative-type photosensitive resin composition according to claim 1 or 2, comprising a rust inhibitor.   The negative-type photosensitive resin composition according to claim 15, wherein the rust inhibitor is at least one compound selected from the group consisting of purines, purine derivatives, and azole derivatives.   The following general formula (1): A polyimide precursor comprising a repeating structure represented by the following general formula (9): In formula (1) and formula (9), X 1 and X 2 are each independently a tetravalent organic group, Y 1 and Y 2 are each independently a divalent organic group, m and n are each an integer of 2 to 100, R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group.} A negative-type photosensitive resin composition according to claim 1 or 2, comprising a polyimide represented by [the specified formula].   In the above general formula (1) and the above general formula (9), X 1 and / or X 2 Y has at least one of the structures represented by the following formulas (2) to (4), 1 The negative-type photosensitive resin composition according to claim 17, wherein the structure is represented by at least one of the following formulas (5) to (7). (In the formula, R 6 (This is a hydrogen atom, an alkyl group, or a phenyl group.) (In the formula, R 7 and R 8 Each of these is independently either a hydrogen atom or a methyl group. (In the formula, R 9 and R 10 Each of these is independently either a hydrogen atom or a methyl group. A negative-type photosensitive resin composition according to claim 1 or 2, used for forming a buffer coat layer or redistribution layer of a semiconductor package.   (1) Forming a photosensitive resin layer on a substrate by applying the negative-type photosensitive resin composition described in claim 1 or 2 to the substrate, (2) Exposing the photosensitive resin layer, (3) Developing the photosensitive resin layer after exposure to form a relief pattern, (4) Forming a hardened relief pattern by heat treatment of the relief pattern, A method for manufacturing a hardened relief pattern, including [the specified element].   A cured relief pattern comprising a cured product of the negative-type photosensitive resin composition according to claim 1 or 2.   A semiconductor device comprising the cured relief pattern described in claim 21.