Polycrystalline diamond and tool

Polycrystalline diamond with specific boron content and structural properties addresses the conductivity issue, enabling complex tool shaping through enhanced machinability and conductivity.

WO2026235132A1PCT designated stage Publication Date: 2026-11-12SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017366
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-01
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing polycrystalline diamond tools lack sufficient conductivity, making them difficult to machine into complex shapes using electrical discharge machining.

Method used

Polycrystalline diamond with a boron content of 1.0 × 10¹¹ to 6.0 × 10¹⁹ atoms/cm³, exhibiting a B-K absorption edge XAFS spectrum peak at 189 eV and a C-K absorption edge XAFS spectrum dip at 302 eV, along with grain sizes between 10 nm and 50,000 nm, and volume resistivity of 1 mΩ·cm to 1000 Ω·cm, enhancing conductivity while maintaining hardness.

Benefits of technology

The modified polycrystalline diamond exhibits improved conductivity and machinability, allowing for the formation of complex tool shapes through electrical discharge machining without compromising hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026017366_12112026_PF_FP_ABST
    Figure JP2026017366_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Polycrystalline diamond having a boron content of 1.0×1016 / cm3 to 1.0×1022 / cm3 on an atomic basis, wherein a B-K absorption edge XAFS spectrum obtained by subjecting the polycrystalline diamond to a partial fluorescence yield method and detecting fluorescent X-rays with a fluorescent X-ray energy of 183 eV has a first peak at an energy of 189 eV.
Need to check novelty before this filing date? Find Prior Art

Description

Polycrystalline diamond and tools

[0001] This disclosure relates to polycrystalline diamond and tools. This application claims priority under Japanese Patent Application No. 2025-078173, filed on 8 May 2025. All contents contained in said Japanese Patent Application are incorporated herein by reference.

[0002] Technology is being developed to impart various properties, such as conductivity, to polycrystalline diamond, which is an insulating material, by adding elements other than carbon (for example, boron).

[0003] Patent Document 1 discloses a technique for producing polycrystalline diamond in which first elements such as boron are dispersed by subjecting boron-containing graphite to high temperature and high pressure treatment, thereby converting the graphite into diamond.

[0004] Japanese Patent Publication No. 2013-28498

[0005] The polycrystalline diamond disclosed herein has a boron content of 1.0 × 10¹¹ on an atomic basis. 16 / cm 3 The above 1.0 x 10 22 / cm 3 A polycrystalline diamond, wherein in the B-K absorption edge XAFS spectrum obtained by performing a partial fluorescence yield method on the polycrystalline diamond and detecting fluorescent X-rays with a fluorescence X-ray energy of 183 eV, the first peak exists at an energy of 189 eV.

[0006] Figure 1 is an example of a B-K absorption edge XAFS spectrum obtained by performing a partial fluorescence yield method on polycrystalline diamond according to Embodiment 1 and detecting fluorescent X-rays with a fluorescence X-ray energy of 183 eV. Figure 2 is a schematic diagram illustrating the configuration of an analytical system used to measure the B-K absorption edge XAFS spectrum of polycrystalline diamond. Figure 3 is a schematic diagram illustrating the configuration of an analytical system used to measure the C-K absorption edge XAFS spectrum of polycrystalline diamond. Figure 4 is a perspective view showing an example of a state in which graphite has been formed on a substrate. Figure 5 is a perspective view showing an example of a state in which polycrystalline diamond has been produced by directly converting graphite on a substrate. Figure 6 is an example of a C-K absorption edge XAFS spectrum obtained by performing a total electron yield method on polycrystalline diamond according to Embodiment 1 and detecting the current flowing through the sample made of the polycrystalline diamond.

[0007] When using polycrystalline diamond as a tool, the tool shape is formed by electrical discharge machining (EDM) on the polycrystalline diamond. As the shapes of workpieces become more complex, the tools themselves are required to be machined into more complex shapes. Improving the conductivity of polycrystalline diamond is effective in enhancing its ease of machining. Therefore, there is a demand for polycrystalline diamond with improved conductivity.

[0008] Therefore, this disclosure aims to provide polycrystalline diamond with improved conductivity and tools.

[0009] According to this disclosure, it is possible to provide polycrystalline diamond with improved conductivity, as well as tools.

[0010] First, embodiments of the present disclosure will be listed and described. (1) The polycrystalline diamond of the present disclosure has a boron content of 1.0 × 10¹¹ on an atomic basis. 16 / cm 3 The above 1.0 x 10 22 / cm 3The following is a polycrystalline diamond, wherein in the B-K absorption edge XAFS spectrum obtained by performing a partial fluorescence yield method on the polycrystalline diamond and detecting fluorescent X-rays with an X-ray energy of 183 eV, the first peak exists at an energy of 189 eV.

[0011] According to this disclosure, it is possible to provide polycrystalline diamond with improved conductivity and tools. The reason for this is presumed to be as follows.

[0012] It is known that when the B-K absorption edge XAFS spectrum of single-crystal diamond shows a peak at energy 189 eV, the hole concentration is high (for example, Element-Selective Observation of Electronic Structure Transition between Semiconducting and Metallic States in Boron-Doped Diamond Using Soft X-ray Emission and Absorption Spectroscopy J. Iihara, Y. Muramatsu, T. Takebe, A. Sawamura, A. Namba, T. Imai, et al. Japanese Journal of Applied Physics 2005 Vol.44 Issue 9R Pages 6612).

[0013] In the B-K absorption edge XAFS spectrum obtained by detecting fluorescent X-rays with an energy of 183 eV using the partial fluorescence yield method for the polycrystalline diamond of this disclosure, a first peak exists at an energy of 189 eV. Therefore, the polycrystalline diamond of this disclosure has a high hole concentration and improved conductivity.

[0014] Furthermore, there are no reports of a peak at energy 189 eV in the B-K absorption edge XAFS spectrum of conventional boron-doped polycrystalline diamond films (for example, Fig. 5 in "Near-Edge X-ray Absorption Fine-Structure Study on Hydrogenated Boron-Doped Ultrananocrystalline Diamond / Amorphous Carbon Composite Films Prepared by Coaxial Arc Plasma Deposition," Y. Katamune, S. Takeichi, S. Ohmagari, H. Setoyama and T. Yoshitake, Transactions of the Materials Research Society of Japan 2015 Vol.40 Issue 3 Pages 243-246).

[0015] (2) In the C-K absorption edge XAFS spectrum obtained by performing the total electron yield method on the polycrystalline diamond and detecting the current flowing through the sample made of the polycrystalline diamond, a dip at energy 302 eV may be present.

[0016] The 302 eV dip in the C-K absorption edge XAFS spectrum of polycrystalline diamond indicates a characteristic of the electronic state of diamond. Polycrystalline diamond exhibiting a 302 eV dip possesses the structure of diamond. Based on this, it can be inferred that the polycrystalline diamond described in (2) above is a diamond with improved conductivity while maintaining the structure of diamond, thus improving conductivity while maintaining hardness.

[0017] Conventional boron-doped polycrystalline diamond is produced as a thin film. Such boron-doped polycrystalline diamond has a graphite-like structure, and therefore does not have the band gap of diamond. Consequently, the C-K absorption edge XAFS spectrum of conventional boron-doped polycrystalline diamond does not have a 302 eV dip.

[0018] (3) In the above (2), the polycrystalline diamond may include a plurality of diamond crystal grains, and the average grain size of the diamond crystal grains may be 10 nm or more and 50000 nm or less. The lower limit of the average grain size of the diamond crystal grains may be 10 nm or more from the viewpoint of production. When the average grain size of the diamond crystal grains is 50000 nm or less, the hardness of the polycrystalline diamond tends to increase.

[0019] (4) In any one of the above (1) to (3), the volume resistivity of the polycrystalline diamond may be 1 mΩ·cm or more and 1000 Ω·cm or less. The volume resistivity is measured at 20°C or more and 25°C or less in accordance with JIS C2141-1992.

[0020] When the volume resistivity of polycrystalline diamond is 1 mΩ·cm or more, it can have electrical conductivity while maintaining hardness. When the volume resistivity of polycrystalline diamond is 1000 Ω·cm or less, the tool is easily formed by electrical discharge machining or the like. Here, 1 mΩ·cm means 1×10 -3 Ω·cm.

[0021] (5) In any one of the above (1) to (4), the Knoop hardness of the polycrystalline diamond may be 50 GPa or more. The Knoop hardness is measured under the conditions of 18°C or more and 28°C or less and a test load of 4.9 N in accordance with JIS Z 2251:2009.

[0022] According to this, the polycrystalline diamond can have excellent hardness.

[0023] (6) In any one of the above (1) to (5), the polycrystalline diamond may consist of diamond crystal grains, the boron, and unavoidable impurities. According to this, the performance of a tool formed of the polycrystalline diamond is further improved.

[0024] (7) A tool of the present disclosure is a tool comprising the polycrystalline diamond according to any one of the above (1) to (6). The polycrystalline diamond tends to be relatively easy to subject to electrical discharge machining. Therefore, when a tool is produced by subjecting the polycrystalline diamond to electrical discharge machining, the tool can have a complicated shape.

[0025] [Details of Embodiments of the Disclosure] Specific examples of polycrystalline diamond and tools of the Disclosure are described below with reference to the drawings. In the drawings of the Disclosure, the same reference numerals indicate the same or corresponding parts. In addition, dimensional relationships such as length, width, thickness, and depth have been modified as appropriate for clarity and simplification of the drawings and do not necessarily represent actual dimensional relationships.

[0026] In this disclosure, the notation "A to B" means A or greater and B or less. If no unit is specified for A, and only a unit is specified for B, then the unit for A and the unit for B are the same.

[0027] In this disclosure, if one or more numerical values ​​are listed as the lower and upper limits of a numerical range, any combination of any one numerical value listed as the lower limit and any one numerical value listed as the upper limit shall also be disclosed.

[0028] In this disclosure, “equipment,” “includes,” “possesses,” and variations thereof are open-ended terms. Open-ended terms may or may not include additional elements in addition to the essential elements. The statement “consists of” is a closed term. However, even a configuration expressed in closed terms may include additional elements that are usually incidental or irrelevant to the subject technology.

[0029] [Embodiment 1: Polycrystalline Diamond] The polycrystalline diamond according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 1") has a boron content on an atomic basis of 1.0 × 10 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following is a polycrystalline diamond, wherein in the B-K absorption edge XAFS spectrum obtained by performing a partial fluorescence yield method on the polycrystalline diamond and detecting fluorescent X-rays with an X-ray energy of 183 eV, the first peak exists at an energy of 189 eV.

[0030] <Structure and Composition> The polycrystalline diamond of Embodiment 1 is a polycrystalline material composed of multiple diamond crystal grains. That is, the polycrystalline diamond has diamond crystal grains as its basic composition and does not contain a metallic bonding phase (binder). Therefore, the polycrystalline diamond possesses extremely high hardness and strength. Furthermore, even under high-temperature conditions, the polycrystalline diamond does not experience deterioration of mechanical properties or grain shedding due to differences in thermal expansion coefficients with the binder or catalytic action of the binder.

[0031] The polycrystalline diamond of Embodiment 1 is a polycrystalline body composed of multiple diamond crystal grains. Therefore, the polycrystalline diamond does not have the directionality (anisotropy) and cleavage of a single crystal, and has isotropic hardness and wear resistance in all directions.

[0032] The boron content of the polycrystalline diamond of Embodiment 1, based on the number of atoms, is 1.0 × 10⁻¹⁶. 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following applies: The lower limit of the boron content in polycrystalline diamond, based on the number of atoms, is 1.0 × 10¹⁶, from the viewpoint of improving oxidation resistance. 16 / cm 3 That is all, 1.0 × 10 17 / cm 3 The above is also acceptable, 1.0 × 10 18 / cm 3 The above is also acceptable, 1.0 × 10 19 / cm 3 The above is also acceptable, 5.0 x 10 19 / cm 3 The above is also acceptable, 9.0 x 10 19 / cm 3 The above is also acceptable, or 1.0 × 10 20 / cm 3 The above is also acceptable. The upper limit of the boron content in polycrystalline diamond, based on the number of atoms, is 1.0 × 10¹⁶, from the perspective of maintaining hardness. 22 / cm 3 The following is true: 1.0 × 10 21 / cm 3 The following is also acceptable: 8.0 x 10 20 / cm 3 The following is also acceptable, or 6.0 x 1020 / cm 3 The following is also acceptable: The boron content of polycrystalline diamond, based on the number of atoms, is 1.0 × 10⁻¹⁶. 17 / cm 3 The above 1.0 x 10 21 / cm 3 The following is also acceptable: 1.0 × 10 18 / cm 3 The above 1.0 x 10 21 / cm 3 The following is also acceptable: 1.0 × 10 19 / cm 3 The above 8.0 x 10 20 / cm 3 The following is also acceptable: 5.0 x 10 19 / cm 3 The above 8.0 x 10 20 / cm 3 The following is also acceptable: 9.0 x 10 19 / cm 3 The above 8.0 x 10 20 / cm 3 The following is also acceptable, or 1.0 × 10 20 / cm 3 The above 6.0 x 10 20 / cm 3 The following is also acceptable.

[0033] The oxygen content of the polycrystalline diamond of Embodiment 1, based on the number of atoms, is 1.0 × 10¹⁶, from the viewpoint of improving oxidation resistance. 18 / cm 3 The following is also acceptable, or 1.0 × 10 19 / cm 3 The following is also acceptable. The oxygen content in polycrystalline diamond, based on the number of atoms, is preferable to be as low as possible, and may be below the detection limit by secondary ion mass spectrometry. This oxygen falls under the category of unavoidable impurities, as described later.

[0034] The polycrystalline diamond of Embodiment 1 may contain unavoidable impurities, as long as the effects of the present disclosure are not impaired. Examples of unavoidable impurities include hydrogen, oxygen, nitrogen, alkali metal elements (lithium (Li), sodium (Na), potassium (K), etc.) and alkaline earth metal elements (calcium (Ca), magnesium (Mg), etc.). In the polycrystalline diamond of Embodiment 1, the content of each element that is an unavoidable impurity may be 0% by mass or more and 0.01% by mass or less. In the polycrystalline diamond of Embodiment 1, the total content of unavoidable impurities may be 0.1% by mass or less.

[0035] The boron content (based on atomic number) of polycrystalline diamond, the oxygen content (based on atomic number) of polycrystalline diamond, and the content of unavoidable impurities in polycrystalline diamond are measured by secondary ion mass spectrometry (SIMS). The SIMS conditions are, for example, using a "CAMECA IMS-7f" instrument (manufactured by AMETEK), and the primary ion species Cs + The primary acceleration voltage is 16.0 kV, and the detection area is φ30 μm.

[0036] In the polycrystalline diamond of Embodiment 1, at least a portion of the boron is doped into the crystalline structure composed of carbon. The polycrystalline diamond of Embodiment 1 may contain carbon and boron doped into the crystalline structure composed of carbon. The polycrystalline diamond of Embodiment 1 may contain carbon, boron doped into the crystalline structure composed of carbon, and unavoidable impurities. The polycrystalline diamond of Embodiment 1 may consist of carbon, boron doped into the crystalline structure composed of carbon, and unavoidable impurities.

[0037] In this disclosure, "boron doped into the crystal structure" refers to a state in which boron exists in a state in which some of the carbon atoms are replaced and dispersed within the crystal structure of diamond, which is composed of covalent bonds between carbon atoms.

[0038] The polycrystalline diamond of Embodiment 1 may be in a form that includes boron clustered within the crystal structure, as long as it does not impair the effects of the present disclosure.

[0039] "Clustered boron within the crystal structure" refers to a state in which multiple boron atoms exist within the crystal structure in an aggregated form. When polycrystalline diamond contains clustered boron within its crystal structure, the boron is unevenly distributed within the crystal structure, which reduces the homogeneity of the polycrystalline diamond and may degrade the performance of the tool material made from it. Furthermore, it can cause significant distortion in the crystal structure, potentially reducing the hardness of the polycrystalline diamond. Therefore, the less clustered boron there is within the crystal structure of the polycrystalline diamond, the better the performance of the tool material made from it. The polycrystalline diamond of Embodiment 1 does not necessarily have to contain clustered boron.

[0040] In the X-ray diffraction pattern of the polycrystalline diamond of Embodiment 1, the ratio of peak intensities originating from other crystal structures to peak intensities originating from the carbon crystal structure may be 0.0001 or less. In this case, the proportion of other crystalline phases in the polycrystalline diamond, such as the boron crystal phase, is sufficiently reduced, resulting in good performance for the tool material made of the polycrystalline diamond.

[0041] In polycrystalline diamond, whether or not boron is doped into the crystal structure can be confirmed, for example, by (1) observing whether or not a boron crystalline phase exists in the polycrystalline diamond, by (2) measuring the distribution of the boron content on an atomic basis in the polycrystalline diamond, or by appropriately combining (1) and (2) above.

[0042] Regarding (1) above, boron doped within the crystal structure does not constitute a different crystalline phase from that of diamond. Therefore, if all the boron in polycrystalline diamond is doped within the crystal structure, no boron crystalline phase is observed in the polycrystalline diamond. In contrast, clustered boron constitutes a different crystalline phase from that of diamond. Therefore, if polycrystalline diamond contains clustered boron, a boron crystalline phase is observed in the polycrystalline diamond. The presence or absence of a boron crystalline phase can be observed, for example, by X-ray diffraction. Depending on the size of the boron crystalline phase, it can also be observed visually.

[0043] Regarding (2) above, when boron is dispersed within the crystal structure, the distribution of the boron content, based on the number of atoms, is more uniform compared to when it exists in a clustered state. The distribution of the boron content, based on the number of atoms, can be measured, for example, by secondary ion mass spectrometry (SIMS). The distribution of the boron content, based on the number of atoms, can be considered uniform if the difference in the boron content measured at any two points in the crystal structure is less than or equal to a predetermined value. In other words, boron can be considered to be dispersed within the crystal structure and not in a clustered state.

[0044] The polycrystalline diamond of Embodiment 1 may consist of diamond crystal grains, boron, and unavoidable impurities. The content of diamond crystal grains in the polycrystalline diamond of Embodiment 1 may be 98% by volume or more and 100% by volume or less. The polycrystalline diamond of Embodiment 1 may consist of carbon, boron, and unavoidable impurities.

[0045] The diamond grain content (volume %) in polycrystalline diamond can be measured by combining a method using an energy-dispersive X-ray analyzer (EDX) attached to a scanning electron microscope (SEM) (e.g., JEOL's "JSM-7800F" (product name)) (e.g., Oxford's X-MAX80 EDS system) (hereinafter also referred to as "SEM-EDX") and X-ray diffraction. The specific measurement method is as follows.

[0046] First, a sample containing the cross-section of the polycrystalline diamond is prepared by cutting the diamond at an arbitrary position. A focused ion beam apparatus, a cross-section polisher, etc., can be used to prepare the cross-section. Next, the cross-section is observed using a scanning electron microscope (SEM) to obtain a backscattered electron image. In the backscattered electron image, the regions containing diamond crystal grains and non-diamond-like carbon appear as black regions, while other regions (e.g., elements derived from the binder) appear as gray or white regions. The magnification when observing the cross-section with the SEM is adjusted appropriately so that the number of diamond crystal grains observed in the measurement field of view is 100 or more. For example, the magnification when observing the cross-section with the SEM may be 10,000x.

[0047] Next, the backscattered electron image is subjected to binarization using image analysis software (such as "Win ROOF ver. 7.4.5" or "WinROOF2018" from Mitani Corporation). The image analysis software automatically sets an appropriate binarization threshold based on the image information (the measurer does not arbitrarily set the threshold). The inventors have also confirmed that there is no significant change in the measurement results even when the brightness of the image is varied. From the image after binarization, the area ratio of pixels originating from the dark field (pixels originating from diamond crystal grains and non-diamond-like carbon) to the area of ​​the measurement field of view is calculated. By considering the calculated area ratio as a volume percentage, the sum (volume percentage) of the content of diamond crystal grains and the content of non-diamond-like carbon can be determined.

[0048] By calculating the area ratio of pixels originating from the brightfield (pixels originating from other regions) to the area of ​​the measurement field of view from the binarized image, the content (volume %) of other regions can be determined.

[0049] As long as the sum (by volume) of the diamond grain content and the non-diamond-like carbon content in polycrystalline diamond is measured in the same sample, it has been confirmed that there is almost no variation in the measurement results even when the measurement field is changed and calculations are performed multiple times.

[0050] Furthermore, the fact that pixels originating from dark-field imaging are derived from diamond crystal grains and non-diamond-like carbon can be confirmed by performing elemental analysis on polycrystalline diamond using SEM-EDX.

[0051] Next, an X-ray diffractometer (Rigaku's "MiniFlex 600" (product name)) is used to obtain the X-ray spectrum of the above cross-section of polycrystalline diamond. The conditions for the X-ray diffractometer at this time are as follows: Characteristic X-ray: Cu-Kα (wavelength 1.54 Å) Tube voltage: 45 kV Tube current: 40 mA Filter: Multilayer mirror Optical system: Focusing method X-ray diffraction method: θ-2θ method.

[0052] In the obtained X-ray spectrum, the following peak intensities A and B are measured.

[0053] Peak intensity A: Peak intensity of non-diamond-like carbon, obtained by removing background noise from peak intensity at diffraction angle 2θ = 27.5° to 29.5°. Peak intensity B: Peak intensity of diamond crystal grains, obtained by removing background noise from peak intensity at diffraction angle 2θ = 43.8° to 44.0°.

[0054] The diamond grain content (volume %) is obtained by calculating the value of {peak intensity B / (peak intensity A + peak intensity B)} × {the sum of the diamond grain content and non-diamond-like carbon content obtained in the above-mentioned SEM-EDX (volume %)}. Since non-diamond-like carbon and diamond grains all have roughly the same electronic weight, the above X-ray peak intensity ratio can be considered as the volume ratio in polycrystalline diamond.

[0055] <B-K Absorption Edge XAFS Spectrum> As shown in Figure 1, in the B-K absorption edge XAFS spectrum obtained by performing the partial fluorescence yield method on the polycrystalline diamond according to Embodiment 1 and detecting fluorescent X-rays with an X-ray energy of 183 eV, a first peak exists at an energy of 189 eV. In the B-K absorption edge XAFS spectrum of Figure 1, the X axis represents energy [eV] and the Y axis represents the intensity ratio. In Figure 1, the Y axis is shown as the intensity ratio, but the same shape is observed even if the B-K absorption edge XAFS spectrum of Figure 1 is shown in a coordinate system where the X axis is energy (eV) and the Y axis is X-ray absorbance.

[0056] Figure 2 is a schematic diagram illustrating the configuration of an analytical system used to measure the B-K absorption edge XAFS spectrum of polycrystalline diamond. As shown in Figure 2, the analytical system 100 includes an X-ray generator 110, a vacuum chamber 120, and a detector 130. The detector 130 is a fluorescence X-ray detector. The X-ray generator 110, vacuum chamber 120, and detector 130 are connected in this order. The internal spaces of the X-ray generator 110 and vacuum chamber 120 are maintained at an ultra-high vacuum. The pressure in the internal spaces of the X-ray generator 110, vacuum chamber 120, and detector 130 is, for example, 4 × 10⁻¹⁰. -7 It is Pa.

[0057] The X-ray generating equipment 110 generates X-rays called synchrotron radiation. For example, beamlines "BL17" at the Saga Prefectural Kyushu Synchrotron Radiation Research Center, and beamlines "BL1N2" and "BL7U" at the Aichi Synchrotron Radiation Center can be used as the X-ray generating equipment 110.

[0058] The X-ray generating equipment 110 can generate X-rays of any energy in the range of 50 eV to 2000 eV and irradiate a polycrystalline diamond installed in a vacuum chamber 120 with X-rays. The X-ray generating equipment 110 illustrated in Figure 2 includes an X-ray source 111, slits 112 and 114, and a grating 113. The slits 112 and 114 are located upstream and downstream of the grating (spectrometer) 113, respectively. The slits 112 and 114 are, for example, four-quadrant slits.

[0059] The X-ray source 111 outputs synchrotron radiation (X-rays) that is emitted along the tangent to the direction of propagation of high-energy electrons by bending their direction of travel with a magnetic field from a bending electromagnet within the circular accelerator.

[0060] The X-rays emitted from the X-ray source 111 are high in intensity. Specifically, the number of X-ray photons emitted per second from the X-ray source 111 is 10 9 The values ​​are photos / s. However, the brightness (intensity) of the X-rays emitted from the X-ray source 111 decreases over time. For example, the brightness of the X-rays emitted 11 hours after the X-ray source 111 is started is 1 / 3 of the brightness of the X-rays emitted immediately after startup.

[0061] X-rays emitted from the X-ray source 111 are focused into the slit 112 by a mirror (not shown), and a portion of the focused X-rays are allowed to pass through. The X-rays that have passed through the slit 112 are irradiated onto the grating 113 via a mirror (not shown), and are angularly dispersed according to their energy. The slit 114 allows X-rays of a specific energy to pass through from the X-rays dispersed in the grating 113, thereby monochromatizing the X-rays.

[0062] The energy of the X-rays emitted from the X-ray generating equipment 110 is determined by the line density and angle of the grating 113. For example, by using a grating 113 with a central line density of 400 lines / mm and adjusting the emission angle of the grating, X-rays ranging from 50 eV to 1000 eV can be emitted from the X-ray generating equipment 110.

[0063] When incident X-rays with an energy of 400 eV from the X-ray generating equipment 110 are irradiated onto the outermost 1 m of the polycrystalline diamond 3 installed inside the vacuum vessel 120, fluorescent X-rays are emitted from the polycrystalline diamond 3.

[0064] The detector 130 (fluorescent X-ray detector) measures the energy distribution of fluorescent X-rays emitted from the polycrystalline diamond 3.

[0065] The angle θ1 between the direction of propagation of X-rays incident on the outermost surface 1 m of the polycrystalline diamond 3 from the X-ray generating equipment 110 and the outermost surface 1 m is variable. Furthermore, the angle between the direction of propagation of fluorescent X-rays captured by the detector 130 from the fluorescent X-rays emitted from the polycrystalline diamond 3 and the outermost surface 1 m of the polycrystalline diamond 3 (hereinafter referred to as the "extraction angle θ2") is also variable. In this disclosure, the extraction angle θ2 is set to 45°. The angle θ1 is not particularly limited, but for example, it may be set to 85°.

[0066] For example, the "XSDD50" SDD detector manufactured by Techno AP Co., Ltd. can be used as the X-ray fluorescence detector.

[0067] Using the above analysis system, a partial fluorescence yield method is performed on the outermost surface of polycrystalline diamond using X-rays with energies ranging from 170 eV to 220 eV. A fluorescent X-ray with an energy of 183 eV is detected to obtain a B-K absorption edge XAFS spectrum. The B-K absorption edge XAFS spectrum is shown in a coordinate system where the X-axis represents energy (eV) and the Y-axis represents X-ray absorbance. The B-K absorption edge XAFS spectrum obtained under the above conditions provides information about the polycrystalline diamond as a bulk material and is considered to indicate the form of boron existence in polycrystalline diamond.

[0068] In this disclosure, in a B-K absorption edge XAFS spectrum obtained by detecting fluorescent X-rays with an energy of 183 eV using a partial fluorescence yield method on polycrystalline diamond, if the X-ray absorption at 189 eV in the B-K absorption edge XAFS spectrum is greater than the X-ray absorption at 189 eV on the line connecting the X-ray absorption at 187 eV and the X-ray absorption at 191 eV, then it is determined that a first peak exists at an energy of 189 eV in the B-K absorption edge XAFS spectrum.

[0069] <C-K Absorption Edge XAFS Spectrum> In the C-K absorption edge XAFS spectrum obtained by performing the total electron yield method on the polycrystalline diamond of Embodiment 1 and detecting the current flowing through the sample made of the polycrystalline diamond, a dip may be present at energy 302 eV.

[0070] Figure 3 schematically illustrates the configuration of an analytical system used to measure the C-K absorption edge XAFS spectrum of polycrystalline diamond. The analytical system 200 in Figure 3 can have the same configuration as the analytical system used to measure the B-K absorption edge XAFS spectrum in Figure 2, except that it does not include a detector 130 and includes an ammeter 140 connected to the polycrystalline diamond 3. For the measurement of the C-K absorption edge XAFS spectrum, a grating 113 with a central line density of 400 lines / mm is used.

[0071] Using the above analysis system, the total electron yield method is performed on the outermost surface of the polycrystalline diamond using X-rays with energies from 270 eV to 340 eV to detect the current flowing through the sample made of polycrystalline diamond and obtain a C-K absorption edge XAFS spectrum. The C-K absorption edge XAFS spectrum is shown in a coordinate system where the X axis is energy (eV) and the Y axis is X-ray absorbance. The C-K absorption edge XAFS spectrum is thought to indicate the form of carbon existence in polycrystalline diamond.

[0072] In this disclosure, in a C-K absorption edge XAFS spectrum obtained by performing a total electron yield method on polycrystalline diamond and detecting the current flowing through the sample made of polycrystalline diamond, if the intensity ratio of the C-K absorption edge XAFS spectrum at 302 eV is 10% or more lower than the X-ray absorption at 302 eV on the line connecting the X-ray absorption at 298 eV and the X-ray absorption at 305 eV, it is determined that there is a dip at energy 302 eV in the C-K absorption edge XAFS spectrum.

[0073] Figure 6 is an example of a C-K absorption edge XAFS spectrum obtained by performing the total electron yield method on a polycrystalline diamond according to Embodiment 1 and detecting the current flowing through the sample made of the polycrystalline diamond. In the C-K absorption edge XAFS spectrum of Figure 6, there is a dip indicated by the arrow at an energy of 302 eV. In the C-K absorption edge XAFS spectrum of Figure 6, the X axis represents energy [eV] and the Y axis represents intensity [a.u.]. In Figure 6, the Y axis is shown as intensity [a.u.], but the same shape is observed even if the C-K absorption edge XAFS spectrum of Figure 6 is shown in a coordinate system where the X axis is energy (eV) and the Y axis is X-ray absorbance.

[0074] <Average grain size of diamond crystal grains> The polycrystalline diamond of Embodiment 1 includes a plurality of diamond crystal grains. The average grain size of the diamond crystal grains may be 10 nm to 50,000 nm, 40 nm to 1,000 nm, 50 nm to 1,000 nm, 50 nm to 500 nm, or 50 nm to 200 nm.

[0075] The average grain size of diamond crystals in polycrystalline diamond can be determined by a scanning electron microscope (SEM) sectioning method. Specifically, the polycrystalline diamond is first observed using a scanning electron microscope at a magnification of 1,000 to 100,000 times to obtain an SEM image.

[0076] Next, draw a circle on the SEM image, and draw eight straight lines radially from the center of the circle (so that the intersection angles between each line are approximately equal) to the outer circumference of the circle. In this case, it is preferable to set the observation magnification and the diameter of the circle so that the number of diamond crystal grains that lie on each of the straight lines is approximately 10 to 50.

[0077] Next, for each of the above lines, count the number of times the line crosses the grain boundaries of the diamond crystal grains, and calculate the average intercept length by dividing the length of the line by the number of crossings. Multiply this average intercept length by 1.128 to obtain the value obtained as the first average grain size. Calculate the average of the first average grain sizes for the eight lines (the second average grain size). Calculate the second average grain size for each of the five SEM images using the above procedure, and calculate the average of these second average grain sizes. This average value is the average grain size of the diamond crystal grains in the polycrystalline diamond.

[0078] Furthermore, it has been confirmed that, as long as the average grain size of diamond crystals is measured in the same sample, there is almost no variation in the measurement results even when the selection of the measurement field of view is changed and calculations are performed multiple times.

[0079] <Knoop Hardness> The Knoop hardness of the polycrystalline diamond of Embodiment 1 may be 50 GPa or higher. The Knoop hardness of the polycrystalline diamond may be 50 GPa or higher and 120 GPa or lower, 60 GPa or higher and 100 GPa or lower, or 60 GPa or higher and 90 GPa or lower.

[0080] In this disclosure, the Knoop hardness of polycrystalline diamond shall be measured by a method conforming to "JIS Z 2251:2009 Knoop hardness test - Measurement method". A general microhardness tester can be used to measure the Knoop hardness. The measurement environment may be room temperature (for example, around 23°C ± 5°C). A Knoop-type indenter (an indenter with a rhombic pyramidal shape) shall be used. The material of the indenter shall be single-crystal diamond. The test force (load) shall be 4.9 N (0.5 kgf). The holding time of the test force shall be 10 seconds. The approach speed of the indenter shall be 60 μm / s.

[0081] The Knoop hardness is measured at five locations on the polycrystalline diamond to be measured. The average value of the three measurements obtained by excluding the minimum and maximum values ​​from the five measurements is calculated. In this disclosure, this average value corresponds to the Knoop hardness of the polycrystalline diamond.

[0082] <Volume Resistivity> The volume resistivity of the polycrystalline diamond of Embodiment 1 may be 1 mΩ·cm or more and 1000 Ω·cm or less, 10 mΩ·cm or more and 1000 Ω·cm or less, 20 mΩ·cm or more and 100 Ω·cm or less, or 100 mΩ·cm or more and 10 Ω·cm or less.

[0083] In this disclosure, the volume resistivity of polycrystalline diamond is measured at a temperature of 20°C to 25°C in accordance with JIS C2141-1992.

[0084] <Method for Manufacturing Polycrystalline Diamond> The polycrystalline diamond of Embodiment 1 can be manufactured, for example, by the following method. The manufacturing method described below will be explained step by step with reference to Figures 4 and 5.

[0085] <<Preparation Process>> This process is for preparing graphite. As shown in Figure 4, in the preparation process, graphite 1 containing carbon and boron doped into the crystalline structure composed of carbon is prepared on a substrate 2. The prepared graphite 1 is converted into polycrystalline diamond by a conversion process described later. The grain size of the single crystals in graphite 1 and the boron content in graphite 1 on an atomic basis are related to polycrystalline diamond. The grain size of the single crystals constituting graphite 1 may be 100 μm or less. The boron content in graphite 1 on an atomic basis is 1 × 10⁻¹⁶ 16 / cm 3 The above 1 x 10 22 / cm 3 The following applies. Graphite 1 that satisfies the above-mentioned single crystal grain size and boron content based on the number of atoms can be formed on a substrate 2, for example, by the following chemical vapor deposition (CVD) method.

[0086] ≪CVD Method≫ A substrate 2 for vapor-phase growth of graphite is placed in a vacuum chamber on its main surface. Any metal, inorganic ceramic material, or carbon material can be used as the material for the substrate 2, as long as it can withstand temperatures of approximately 1500°C to 3000°C. However, from the viewpoint of reducing impurities mixed into the graphite that will become the raw material for polycrystalline diamond, at least the main surface of the substrate may be made of carbon material, or it may be diamond or graphite with very few impurities.

[0087] Next, the substrate 2 placed in the vacuum chamber is heated to a temperature of approximately 1500°C to 3000°C. Known heating methods can be employed, for example, by installing a heater capable of directly or indirectly heating the substrate 2 in the vacuum chamber.

[0088] Next, hydrocarbon gas and boron-containing gas are introduced into the vacuum chamber. At this time, the vacuum level (pressure) inside the vacuum chamber is set to below atmospheric pressure. This allows the hydrocarbon gas and boron-containing gas to be uniformly mixed inside the vacuum chamber.

[0089] As the hydrocarbon gas, ethane, butane, methane, etc., can be used. Methane may be used because, due to its small molecular weight, it does not easily produce by-products such as ethylene when thermally decomposed. In addition, as the boron-containing gas, gases consisting of boron hydride, hydrocarbon gases containing boron, and halogenated gases containing boron may be used. When a gas consisting of boron hydride is used, the gas can be easily decomposed at high temperatures, so boron can be efficiently supplied to the substrate. When a hydrocarbon gas containing boron is used, boron that is already bonded to carbon can be supplied to the substrate, so boron can be doped into the graphite more efficiently. When a halogenated gas containing boron is used, graphite can be synthesized while removing unintended metal impurities through the action of halogens, so the concentration of metal impurities in the graphite can be reduced more effectively. For example, boron fluoride gas can be used.

[0090] Then, by thermally decomposing the mixed gas at a temperature of 1500°C or higher, graphite containing carbon and boron doped into the carbon-based crystalline structure is formed on the main surface of the substrate. In the graphite, boron exists dispersed within the crystalline structure.

[0091] In the above CVD method, the temperature and pressure in the synthesis conditions may be set to 1600°C or higher and 13 Torr or higher, respectively, in order to reduce the grain size of the single crystals contained in graphite 1 to 100 μm or less. By reducing the grain size of the single crystals contained in graphite 1 to 100 μm or less, the grain size of the diamond crystals in polycrystalline diamond produced by direct conversion can be reduced to 50,000 nm or less. Furthermore, by adjusting the grain size of the single crystals contained in graphite 1 to 100 μm or more, the grain size of the diamond crystals in polycrystalline diamond can be reduced to 10 nm or more and 50,000 nm or less. Note that the composition of graphite 1 may include single crystals in part, with the rest being in the state of amorphous, amorphous carbon, carbon nanotubes, fullerenes, etc., or it may be a polycrystalline material composed of single crystals. To obtain polycrystalline diamond with more uniform grain size, it is preferable to form graphite 1 in which each graphite phase is formed by a single phase. Here, grain size refers to the average grain size as described above.

[0092] In the above CVD method, the boron content in graphite 1, based on the number of atoms, is 1.0 × 10⁻⁶. 16 / cm 3 The above 1.0 x 10 22 / cm 3 To achieve the following, the mixing ratio of hydrocarbon gas and boron-containing gas is adjusted. Specifically, by increasing the mixing ratio of boron-containing gas to hydrocarbon gas, the amount of boron on an atomic basis in graphite 1 can be increased. Furthermore, the amount of boron on an atomic basis can also be adjusted by changing the type of boron-containing gas. The amount of boron on an atomic basis in graphite 1 is 1.0 × 10⁻⁶. 16 / cm 3 The above 1.0 x 10 22 / cm 3By the following steps, the atomic number-based content of boron in the polycrystalline diamond can be adjusted to 1.0×10 16 / cm 3 or more and 1.0×10 22 / cm 3 or less.

[0093] In this step, by using the aforementioned CVD method, graphite 1 containing carbon and boron doped into the crystal structure constituted by carbon, with the atomic number-based content of boron being 1.0×10 16 / cm 3 or more and 1.0×10 22 / cm 3 or less is formed on the base material 2. In other words, graphite 1 in which boron is dispersedly present in the crystal structure at an atomic number-based content of 1.0×10 16 / cm 3 or more and 1.0×10 22 / cm 3 or less is vapor-phase grown on the base material 2.

[0094] Further, regarding the graphite prepared in this step, it is preferable that the distribution of the atomic number-based content of boron in the graphite is uniform in both the thickness direction and the in-plane direction. By uniformly doping boron into the graphite, the distribution of boron in the polycrystalline diamond produced by the conversion step described later can be made uniform.

[0095] In order to make the distribution of the atomic number-based content of boron uniform, it is preferable to introduce a hydrocarbon gas and a boron-containing gas into the vacuum chamber at the same time. Thereby, each gas can be easily and uniformly mixed, and graphite uniformly doped with boron can be efficiently formed on the base material. Further, each gas is supplied toward the main surface of the base material from a direction directly above the main surface of the base material.

[0096] When supplying each gas toward the main surface of the base material, the gas flow jetted toward the main surface of the base material is adjusted. As the spray nozzle, a spray nozzle having a shape in which one inflow port communicates with one first flow path, the first flow path branches into a plurality of second flow paths, and each second flow path communicates with a jet port is used. That is, the spray nozzle has a plurality of jet ports. The diameter φ of each jet port is 0.5 mm or more and 1 mm or less. All raw material gases are simultaneously introduced into the inflow port of one spray nozzle and jetted from the plurality of jet ports.

[0097] The graphite produced by jetting gas toward the main surface of the base material using the above spray nozzle is subjected to high-temperature and high-pressure treatment in the subsequent conversion step, whereby the B-K absorption edge XAFS spectrum of the obtained polycrystalline diamond has a first peak at an energy of 189 eV. This reason is presumed as follows. By using the spray nozzle having a plurality of jet ports with the above diameter φ, the gas flow reaching the surface of the base material becomes finer, and the distribution of the boron content on an atomic number basis in the graphite can be made more uniform. For this reason, boron is dispersed and grows in a non-equilibrium process, so boron has various existing forms.

[0098] Note that in the conventional manufacturing method, when jetting gas toward the main surface of the base material, a spray nozzle with one jet port is used, and a spray nozzle having a plurality of jet ports is not used.

[0099] In addition, the density of the graphite prepared in this step is 0.8 g / cm 3 or more and 2.2 g / cm 3 or less, or 1.4 g / cm 3 or more and 2.1 g / cm 3 or less. When the density of graphite is 0.8 g / cm 3 or more, in the conversion step described later, the volume change when graphite is directly converted to polycrystalline diamond can be made sufficiently small, so the probability of cracking occurring in the manufactured polycrystalline diamond can be suppressed, and changes in the environment inside the apparatus can be suppressed, and as a result, the manufacturing yield can be improved. In addition, when the density of graphite is 2.2 g / cm 3Under the following conditions, polycrystalline diamond can be synthesized with a high yield of over 80%.

[0100] The density of graphite can be adjusted, for example, by the temperature (°C) and the introduction rate (sccm) of each gas when growing graphite on the main surface of the substrate. Specifically, the density of graphite can be increased by raising the temperature and by increasing the introduction rate of hydrocarbons.

[0101] Furthermore, it is preferable that the graphite prepared in this process has a low content of unavoidable impurities. Specifically, the content of each element that is an unavoidable impurity in graphite may be 0.01 mass% or less. This is because the content of unavoidable impurities in the graphite is carried over to the polycrystalline diamond produced. In addition, by keeping the content of unavoidable impurities low, grain growth caused by the presence of unavoidable impurities can be suppressed, so that single crystals of a more uniform size can be contained in the graphite. Note that analytical instruments used for analysis that can measure the content of unavoidable impurities in graphite, such as SIMS analysis and ICP analysis, generally have a detection limit of 0.01 mass%, so elements with a content of 0.01 mass% or less will not be detected by the above analytical instruments.

[0102] The inclusion of unavoidable impurities in graphite can be suppressed by setting a relatively high vacuum level in the vacuum chamber during the thermal decomposition of the gas. Specifically, the inventors have found that by maintaining the pressure in the vacuum chamber between 20 Torr and 200 Torr, more preferably between 20 Torr and 120 Torr, the content of each element, which is an unavoidable impurity, can be controlled to 0.01 mass% or less.

[0103] In the CVD method described above, the substrate is heated before the mixed gas is introduced into the vacuum chamber. However, the substrate may also be heated after the mixed gas is introduced, or both methods may be performed simultaneously.

[0104] <<Conversion Process>> This process involves sintering the graphite produced in the preparation process to directly convert it into polycrystalline diamond. As a result, polycrystalline diamond 3 is produced on the substrate 2, as shown in Figure 5.

[0105] Specifically, first, the graphite 1 on the substrate 2 shown in Figure 4 is placed in a high-temperature, high-pressure apparatus. The high-temperature, high-pressure apparatus can be any apparatus that can accommodate graphite and control the internal conditions as described above. For example, a vacuum chamber used in the CVD method can be used.

[0106] Graphite 1 is exposed to high temperature and high pressure conditions of 2000°C or higher and 10 GPa or higher. As a result, graphite 1 is instantaneously sintered and converted into polycrystalline diamond 3, as shown in Figure 5. In this case, the shape of the polycrystalline diamond 3 will inherit the shape of graphite 1, except for a slight change in volume. Alternatively, graphite 1 may be exposed to high temperature and high pressure conditions after the substrate 2 has been removed from it, and in this case as well, the produced polycrystalline diamond will basically inherit the shape of graphite 1.

[0107] In this process, it is preferable not to use additives such as sintering aids, catalysts, and binders. According to this process, polycrystalline diamond in which single crystals are strongly bonded can be produced without the use of additives, and by not using additives, polycrystalline diamond with higher hardness can be produced compared to when additives are used.

[0108] According to the manufacturing method described in detail above, the polycrystalline diamond of Embodiment 1 can be manufactured.

[0109] Furthermore, according to the above manufacturing method, since boron is uniformly dispersed in the graphite, it is possible to effectively suppress localized abnormal growth of diamond crystal grains when directly converting graphite to diamond. As a result, the grain size of the single crystals constituting polycrystalline diamond can be made more uniform, and consequently, homogeneous polycrystalline diamond can be manufactured.

[0110] [Embodiment 2: Tools] A tool according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 2") is a tool comprising the polycrystalline diamond described in Embodiment 1. Each tool may be composed entirely of polycrystalline diamond, or only a part thereof (for example, the cutting edge portion in the case of a cutting tool) may be composed of polycrystalline diamond. Furthermore, a coating film may be formed on the surface of each tool. Examples of tools include cutting tools, wear-resistant tools, wire drawing tools, and grinding tools.

[0111] Examples of cutting tools include drills, end mills, replaceable cutting tips for drills, replaceable cutting tips for end mills, replaceable cutting tips for milling machines, replaceable cutting tips for turning machines, metal saws, gear cutting tools, reamers, taps, and cutting tools.

[0112] Examples of wear-resistant tools include scribers, scribing wheels, dressers, water and other fluid jet nozzles, and stitchels. Examples of wire drawing tools include dies. Examples of grinding tools include grinding wheels.

[0113] The tool can be manufactured by machining the polycrystalline diamond of Embodiment 1 into a desired shape, for example, by electrical discharge machining. The cutting tool manufactured by electrical discharge machining can be used, for example, for direct machining of minute shapes in molds.

[0114] This embodiment will be described in more detail by reference to examples. However, this embodiment is not limited by these examples.

[0115] [Preparation of Polycrystalline Diamonds] Polycrystalline diamonds were prepared from each sample using the following method.

[0116] ≪Preparation Process≫ Boron-containing graphite was fabricated on a substrate by the CVD method. The main surface of the substrate was diamond. After placing the substrate in a vacuum chamber, the substrate was heated to between 1500°C and 3000°C, and the vacuum (pressure) inside the vacuum chamber was reduced to below atmospheric pressure. In this state, methane gas and a gas containing boron (boron fluoride gas) were then introduced into the vacuum chamber for more than one hour. The methane gas and the gas containing boron (boron fluoride gas) were supplied to the main surface of the substrate from directly above using a spray nozzle. The number of nozzles, the diameter of each nozzle, and the number of inlets of the spray nozzle used for each sample are shown in Table 1. For example, the notation "3 / φ1mm / 1" for sample 2 means a spray nozzle with a shape in which one inlet is connected to one first channel, the first channel branches into three second channels, and each second channel is connected to a nozzle. Here, the nozzle diameter is 1 mm, and there are three nozzles. The spray nozzle used in sample 101 is a spray nozzle with one nozzle, which is commonly used in the conventional production of polycrystalline diamond.

[0117]

[0118] The mixing ratio of methane gas and boron-containing gas (boron fluoride gas) was adjusted so that the boron content in the graphite, based on the number of atoms, matched the "boron content" of "polycrystalline diamond" in Table 1. Through the above process, graphite with a thickness of more than 100 μm was produced on the main surface of the substrate by thermal decomposition of the mixed gas at a temperature of 1500°C or higher.

[0119] <<Conversion Process>> Next, the graphite on the substrate was converted into polycrystalline diamond under ultra-high temperature and pressure conditions of over 2000°C and over 10 GPa using a large press capable of generating high temperature and pressure, thereby producing polycrystalline diamond for each sample.

[0120] [Evaluation] For each polycrystalline diamond sample, the following were measured using the method described in Embodiment 1: the boron content on an atomic basis; the presence or absence of a first peak at energy 189 eV in the B-K absorption edge XAFS spectrum obtained by detecting fluorescent X-rays with an energy of 183 eV using the partial fluorescence yield method for the polycrystalline diamond; the presence or absence of a dip at energy 302 eV in the C-K absorption edge XAFS spectrum obtained by detecting the current flowing through the sample made of polycrystalline diamond using the total electron yield method for the polycrystalline diamond; the average grain size of the diamond crystals; the Knoop hardness of the polycrystalline diamond; and the volume resistivity of the polycrystalline diamond. The results are shown in Table 1.

[0121] [Discussion] The polycrystalline diamonds of Samples 1 to 8 correspond to the examples. In the B-K absorption edge XAFS spectra of the polycrystalline diamonds of Samples 1 to 8, a first peak was present at an energy of 189 eV. The polycrystalline diamond of Sample 101 corresponds to the conventional example (comparative example). In the B-K absorption edge XAFS spectrum of the polycrystalline diamond of Sample 101, there was no first peak at an energy of 189 eV. Therefore, it was confirmed that the polycrystalline diamonds of Samples 1 to 8 have improved conductivity compared to the conventional example, the polycrystalline diamond of Sample 101.

[0122] While embodiments and examples of this disclosure have been described above, it is intended from the outset that the configurations of each of the embodiments and examples described above may be combined or modified in various ways as appropriate. The embodiments and examples disclosed herein should be considered in all respects to be illustrative and not restrictive. The scope of the present invention is indicated by the claims rather than the embodiments and examples described above, and all modifications within the scope of the claims are intended to be included in the meaning of equivalences.

[0123] 1. Graphite, 2. Substrate, 3. Polycrystalline diamond, 100, 200. Analysis system, 1m. Outer surface, 110. X-ray generating equipment, 111. X-ray source, 112, 114. Slits, 113. Grating, 120. Vacuum vessel, 130. Detector, 140. Ammeter.

Claims

1. The boron content, based on the number of atoms, is 1.0 × 10⁻⁶ 16 / cm 3 The above 1.0 x 10 22 / cm 3 A polycrystalline diamond, wherein in the B-K absorption edge XAFS spectrum obtained by performing a partial fluorescence yield method on the polycrystalline diamond and detecting fluorescent X-rays with an X-ray energy of 183 eV, the first peak exists at an energy of 189 eV.

2. The polycrystalline diamond according to claim 1, wherein in the C-K absorption edge XAFS spectrum obtained by performing a total electron yield method on the polycrystalline diamond and detecting the current flowing through the sample made of the polycrystalline diamond, there is a dip at an energy of 302 eV.

3. The polycrystalline diamond according to claim 1 or claim 2, wherein the polycrystalline diamond comprises a plurality of diamond crystal grains, and the average particle size of the diamond crystal grains is 10 nm or more and 50,000 nm or less.

4. The polycrystalline diamond according to any one of claims 1 to 3, wherein the volume resistivity of the polycrystalline diamond is 1 mΩ·cm or more and 1000 Ω·cm or less, and the volume resistivity is measured at 20°C or more and 25°C or less in accordance with JIS C2141-1992.

5. The polycrystalline diamond according to any one of claims 1 to 4, wherein the Knoop hardness of the polycrystalline diamond is 50 GPa or higher, and the Knoop hardness is measured in accordance with JIS Z 2251:2009 at a temperature of 18°C ​​or higher and 28°C or lower, and with a test load of 4.9 N.

6. The polycrystalline diamond according to any one of claims 1 to 5, wherein the polycrystalline diamond comprises diamond crystal grains, boron, and unavoidable impurities.

7. A tool comprising the polycrystalline diamond described in any one of claims 1 to 6.