Laminated nonwoven fabric, wet wipe, package for wet wipe, and method for producing laminated nonwoven fabric
The laminated nonwoven fabric structure with heat-fusible frameworks in the core and reinforcing layers addresses the issue of low strength and sticking by enhancing dry and wet strength, ensuring easy separation and removal of wet wipes.
Patent Information
- Application Number
- PCT/JP2026/017531
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing laminated nonwoven fabrics for wet wipes have low initial strength when dry and wet, leading to issues such as sticking together and difficulty in separation, especially when used with liquid medicine, which increases the tendency for multiple wipes to be taken out at once.
A laminated nonwoven fabric structure comprising a first and second surface layer with water-retaining fibers, a core layer with pulp and heat-fusible fibers, and a reinforcing layer with heat-fusible and non-heat-fusible fibers, where the heat-fusible fibers form frameworks to enhance strength and separation, using composite fibers and heat fusion for bonding.
The laminated nonwoven fabric exhibits high initial strength when dry and wet, reducing the likelihood of wipe portions sticking together and facilitating easy separation, especially when used with liquid medicine, and maintaining ease of removal from storage containers.
Smart Images

Figure JP2026017531_12112026_PF_FP_ABST
Abstract
Description
Laminated nonwoven fabric, wet wipes, packaging for wet wipes, and method for manufacturing laminated nonwoven fabric.
[0001] This disclosure relates to laminated nonwoven fabric for wet wipes, wet wipes, packaging for wet wipes, and a method for manufacturing laminated nonwoven fabric.
[0002] Laminated nonwoven fabrics and wet wipes formed from said laminated nonwoven fabrics are known. For example, Patent Document 1 discloses a sheet-shaped wiper in which a reinforcing layer with fused fibers and a core layer containing hydrophilic fibers are interposed between a first surface layer appearing on one sheet surface and a second surface layer appearing on the other sheet surface, wherein the first and second surface layers are formed of non-fused fibers whose surface melting point is higher than that of the fused fibers or whose surface does not melt, and the surface of the non-fused fibers is not melted.
[0003] Japanese Patent Publication No. 2005-287894
[0004] Patent Document 1 does not disclose the laminated nonwoven fabric according to this disclosure. Therefore, the purpose of this disclosure is to provide a laminated nonwoven fabric that has excellent ease of removal when used as a wet wipe.
[0005] The Disclosers have found a laminated nonwoven fabric comprising a first surface layer, a second surface layer, and a core layer and a reinforcing layer disposed between the first surface layer and the second surface layer, wherein each of the first surface layer and the second surface layer contains water-retaining fibers, the core layer contains pulp fibers and heat-fusible fibers, and the reinforcing layer contains heat-fusible fibers and non-heat-fusible fibers.
[0006] The laminated nonwoven fabric relating to this disclosure exhibits excellent ease of removal when used as a wet wipe.
[0007] Figure 1 is a diagram illustrating the laminated nonwoven fabric 1 according to the first embodiment. Figure 2 is a diagram illustrating the wet wipe packaging 101 according to the second embodiment. Figure 3 is a diagram illustrating the wet wipe packaging 101 according to the second embodiment. Figure 4 is a diagram illustrating the wet wipe packaging 101 according to the second embodiment.
[0008] Specifically, this disclosure relates to the following embodiments: [Embodiment 1] A laminated nonwoven fabric comprising a first surface layer, a second surface layer, and a core layer and a reinforcing layer disposed between the first surface layer and the second surface layer, wherein each of the first surface layer and the second surface layer contains water-retaining fibers, the core layer contains pulp fibers and heat-fusible fibers, and the reinforcing layer contains heat-fusible fibers and non-heat-fusible fibers.
[0009] In the wiper described in Patent Document 1, since the core layer contains only hydrophilic fibers, not only is the initial strength of the core layer when dry (hereinafter, "initial strength when dry" is referred to as "initial strength when dry") low, but the initial strength when wet (hereinafter, "initial strength when wet" is referred to as "initial strength when wet") is also low, and consequently, the initial strength of the wiper when wet tends to be low.
[0010] In contrast, in the laminated nonwoven fabric described above, each of the heat-fusible fibers in the core layer is heat-fusible, and each of the heat-fusible fibers in the reinforcing layer is also heat-fusible. Because the heat-fusible fibers in the core layer are heat-fusible with each other, the heat-fusible fibers form a framework, making it easier to hold pulp fibers within this framework. Furthermore, because the heat-fusible fibers in the reinforcing layer are heat-fusible with each other, the reinforcing layer makes it easier to reinforce the core layer.
[0011] Therefore, compared to the wiper described in Patent Document 1, in which the core layer consists only of hydrophilic fibers, the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, and is less prone to stretching and deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0012] Consequently, when the wet wipes formed from the laminated nonwoven fabric consist of a single wet wipe folded along the fold lines, the wet wipe portions separated by the fold lines become less likely to stick together and easier to separate, making it easier to unfold them from their folded state.
[0013] Furthermore, when multiple wet wipes formed from the above-mentioned laminated nonwoven fabric are stacked and stored in a packaging sheet type, pop-up type, or other storage container, adjacent wet wipe portions in the stacking direction are less likely to stick together and are more likely to separate. This reduces the tendency for multiple wet wipes to be taken out at once when one wet wipe is removed. Note that this tendency for multiple wipes to be taken out tends to increase as the amount of liquid medicine a wet wipe holds increases.
[0014] Furthermore, when multiple wet wipes formed from the above-mentioned laminated nonwoven fabric are wound into a roll and stored in a bottle-shaped container, adjacent wet wipe portions in the thickness direction are less likely to stick together and are easier to separate. In addition, the high strength of the wet wipes themselves makes them easier to remove. Therefore, the above-mentioned laminated nonwoven fabric offers excellent ease of removal when used as wet wipes.
[0015] [Aspect 2] The laminated nonwoven fabric according to aspect 1, wherein the heat-fusible fibers in the core layer and the heat-fusible fibers in the reinforcing layer are each composite fibers.
[0016] In the above-described laminated nonwoven fabric, the heat-fusible fibers in the core layer and the heat-fusible fibers in the reinforcing layer are both composite fibers. Therefore, in the above-described laminated nonwoven fabric, the core layer and the reinforcing layer each have high initial strength when dry and high initial strength when wet, and consequently, the above-described laminated nonwoven fabric has high initial strength when dry, is resistant to stretching, and is resistant to deformation. As a result, when the above-described laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate. Consequently, when the above-described laminated nonwoven fabric is used as a wet wipe, it has excellent ease of removal.
[0017] [Aspect 3] The laminated nonwoven fabric according to aspect 2, wherein the composite fiber in the core layer is a core-sheath fiber comprising a core portion and a sheath portion, and the sheath portion is composed of a polymer containing an unsaturated carboxylic acid, an unsaturated carboxylic acid anhydride, or a mixture thereof as a monomer backbone.
[0018] In the above-described laminated nonwoven fabric, the heat-fusible fibers in the core layer are core-sheath fibers, and the sheath portion contains a predetermined monomer skeleton. Therefore, the heat-fusible fibers that are heat-fused in the core layer have a high affinity for pulp fibers and are able to hold pulp fibers more easily. As a result, the core layer has high initial strength when dry and high initial strength when wet, and consequently, the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, and is less prone to stretching and deformation. Furthermore, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate. As a result, when the laminated nonwoven fabric is used as a wet wipe, it has excellent ease of removal.
[0019] [Aspect 4] The laminated nonwoven fabric according to any one of aspects 1 to 3, wherein in the core layer, the heat-fusible fibers and the pulp fibers are bonded together by heat fusion of the heat-fusible fibers.
[0020] In the laminated nonwoven fabric described above, the heat-fusible fibers and the pulp fibers are bonded together in the core layer by heat fusion of the heat-fusible fibers. As a result, the heat-fusible fibers that are heat-fusible form a framework in the core layer, making it easier to hold the pulp fibers within this framework. Consequently, the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, is resistant to stretching and deformation, and when used as a wet wipe, adjacent wet wipe portions of the laminated nonwoven fabric are less likely to stick together and are easier to separate. As a result, when used as a wet wipe, the laminated nonwoven fabric has excellent ease of removal.
[0021] [Aspect 5] The laminated nonwoven fabric according to any one of aspects 1 to 4, wherein the heat-fusible fibers in the core layer and at least one of the water-retaining fibers in the first surface layer and the water-retaining fibers in the second surface layer are bonded together by heat fusion of the heat-fusible fibers in the core layer.
[0022] In the above-described laminated nonwoven fabric, the heat-fusible fibers in the core layer and at least one of the water-retaining fibers in the first surface layer and the water-retaining fibers in the second surface layer are bonded together by heat fusion of the heat-fusible fibers in the core layer. As a result, the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, and is resistant to stretching and deformation. Consequently, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate. As a result, when the laminated nonwoven fabric is used as a wet wipe, it has excellent ease of removal.
[0023] [Aspect 6] The laminated nonwoven fabric according to any one of aspects 1 to 5, wherein the heat-fusible fibers in the core layer and the heat-fusible fibers in the reinforcing layer are heat-fussed together.
[0024] In the above-described laminated nonwoven fabric, the heat-fusible fibers in the core layer and the heat-fusible fibers in the reinforcing layer are heat-fussed together. As a result, the reinforcing layer can easily reinforce the core layer, and the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, and is resistant to stretching and deformation. Therefore, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate. Consequently, when the laminated nonwoven fabric is used as a wet wipe, it has excellent ease of removal.
[0025] [Aspect 7] In the above laminated nonwoven fabric, in a wet tensile test, the product of the elongation at maximum strength (%) and the strength at 5% elongation (N / 25 mm) in the orthogonal direction perpendicular to the conveying direction during manufacturing is P W5% The basis weight is 50 g / m². 2 A laminated nonwoven fabric according to any one of embodiments 1 to 6, which is in the range of 25 to 100 in terms of conversion.
[0026] In the above laminated nonwoven fabric, the product is P W5% This is within a predetermined range. Therefore, the laminated nonwoven fabric has high initial strength when wet and is less prone to tearing. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0027] [Aspect 8] In the above laminated nonwoven fabric, in a wet tensile test, the product of the elongation at maximum strength (%) and the strength at 50% elongation (N / 25 mm) in the orthogonal direction perpendicular to the conveying direction during manufacturing is P W50% The basis weight is 50 g / m². 2 A laminated nonwoven fabric according to any one of embodiments 1 to 7, which is in the range of 130 to 300 in terms of conversion.
[0028] In the above laminated nonwoven fabric, the product is P W50% This is within a predetermined range. Therefore, the laminated nonwoven fabric has high initial strength when wet and is less prone to tearing. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0029] [Aspect 9] The laminated nonwoven fabric according to any one of aspects 1 to 8, wherein the heat-fusible fibers in the core layer have an average fiber length of less than 20 mm, and the heat-fusible fibers in the reinforcing layer have an average fiber length of 20 mm or more.
[0030] In the laminated nonwoven fabric described above, the heat-fusible fibers in the core layer have a predetermined average fiber length. Therefore, in the core layer, the heat-fusible fibers are more easily dispersed within the pulp fibers, and the heat-fusible fibers in the core layer form a framework, making it easier to hold the pulp fibers within that framework. Furthermore, in the nonwoven fabric described above, the heat-fusible fibers in the reinforcing layer have a predetermined average fiber length. Therefore, the reinforcing layer is more easily reinforced against the core layer, and the laminated nonwoven fabric has high initial strength when dry and when wet, is less prone to stretching, and is less prone to deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate. Consequently, when the laminated nonwoven fabric is used as a wet wipe, it has excellent ease of removal.
[0031] [Aspect 10] The laminated nonwoven fabric according to any one of aspects 1 to 9, wherein the water-retaining fibers have an average fiber length of 20 mm or more. In the above laminated nonwoven fabric, the water-retaining fibers have a predetermined average fiber length. Therefore, the water-retaining fibers are more likely to entangle with other fibers, such as other water-retaining fibers or desired synthetic fibers, resulting in a laminated nonwoven fabric with high initial strength when dry and when wet, and less prone to stretching and deformation. As a result, when the above laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate. Consequently, when the above laminated nonwoven fabric is used as a wet wipe, it has excellent ease of removal.
[0032] [Aspect 11] A laminated nonwoven fabric according to any one of aspects 1 to 10, wherein each of the first surface layer and the second surface layer contains synthetic fibers.
[0033] In the laminated nonwoven fabric described above, each of the first and second surface layers contains synthetic fibers. Therefore, the amount of liquid held by each of the first and second surface layers is reduced, and the laminated nonwoven fabric has bulkiness and resistance to deformation when wet. As a result, the laminated nonwoven fabric has excellent ease of removal when used as a wet wipe.
[0034] [Aspect 12] The laminated nonwoven fabric according to aspect 11, wherein the synthetic fibers have an average fiber length of 20 mm or more. In the laminated nonwoven fabric, the synthetic fibers have a predetermined average fiber length. Therefore, the synthetic fibers are more likely to intertwine with other fibers, such as the water-retaining fibers and other synthetic fibers, thereby increasing the initial dry strength and initial wet strength of the laminated nonwoven fabric, and consequently the initial wet strength of the wet wipes.
[0035] [Aspect 13] The laminated nonwoven fabric according to any one of aspects 1 to 12, wherein in the core layer, the average fiber length of the heat-fusible fibers is greater than the average fiber length of the pulp fibers.
[0036] In the laminated nonwoven fabric described above, the average fiber length of the heat-fusible fibers is greater than the average fiber length of the pulp fibers. Therefore, the core layer has high initial strength when dry and high initial strength when wet, and consequently, the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, making it less prone to stretching and deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate. Consequently, when the laminated nonwoven fabric is used as a wet wipe, it offers excellent ease of removal.
[0037] [Aspect 14] The laminated nonwoven fabric according to any one of aspects 1 to 13, wherein the non-heat-fusible fibers in the reinforcing layer are water-retaining fibers or synthetic fibers.
[0038] In the laminated nonwoven fabric described above, the non-heat-fusible fibers in the reinforcing layer are either water-retaining fibers or synthetic fibers. Therefore, if the non-heat-fusible fibers are water-retaining fibers, the water-retaining fibers can directly hold the chemical solution, thereby increasing the water retention capacity of the reinforcing layer. If the non-heat-fusible fibers are synthetic fibers, the volume of the reinforcing layer can be increased. As a result, the amount of chemical solution present in the first and second surface layers is reduced. Consequently, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate. As a result, when the laminated nonwoven fabric is used as a wet wipe, it offers excellent ease of removal.
[0039] [Aspect 15] The laminated nonwoven fabric is a spunlace nonwoven fabric, as described in any one of aspects 1 to 14.
[0040] The laminated nonwoven fabric described above is a spunlace nonwoven fabric. Therefore, since fibers of a certain length that make up the laminated nonwoven fabric are intertwined, the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, and is resistant to stretching and deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate. Consequently, when the laminated nonwoven fabric is used as a wet wipe, it has excellent ease of removal.
[0041] [Aspect 16] Wet wipes comprising a nonwoven fabric sheet and a chemical solution, wherein the nonwoven fabric sheet is composed of a laminated nonwoven fabric as described in any one of aspects 1 to 15. The wet wipes have the same effects as those of aspect 1.
[0042] [Aspect 17] The wet wipes according to aspect 16, wherein the above-mentioned liquid contains a fragrance, and the above-mentioned fragrance has a vapor pressure of 10.00 to 1333 Pa at 25°C.
[0043] In the above-mentioned wet wipes, the liquid contains a specified fragrance. The specified fragrance has a vapor pressure of 10.00 Pa (0.075 mmHg) or more at 25°C, which is very high. Therefore, the pulp fibers in the core layer, and the water-retaining fibers (as non-heat-fusible fibers) in the optional reinforcing layer, hold the liquid containing the fragrance, and when wiping with the wet wipes, the fragrance contained in the liquid evaporates in a short time, allowing the fragrance to be released quickly. Furthermore, when the wet wipes wipe the skin, the fragrance contained in the liquid evaporates and disappears in a short time, making it less likely to cause skin problems.
[0044] [Aspect 18] A wet wipes package comprising a plurality of wet wipes and a packaging body for storing the plurality of wet wipes, wherein each of the plurality of wet wipes is a wet wipe as described in Aspect 16 or 17, and the packaging body is a packaging sheet type, pop-up type, or bottle type packaging container.
[0045] In the packaging of wet wipes, the packaging body is a designated packaging container. Therefore, the wet wipe portions are less likely to stick together and are easier to separate, and the tendency for multiple wet wipes, including the next wet wipe, to be taken out at once when one wet wipe is removed is reduced. In addition, because the wet wipe portions are less likely to stick together and are easier to separate, and because the wet wipes themselves have high strength, the wet wipes are easier to remove. For these reasons, the above-mentioned laminated nonwoven fabric offers excellent ease of removal when used as wet wipes.
[0046] [Aspect 19] The packaging body is a packaging sheet type or pop-up type packaging container, the packaging container has a top with an opening and a bottom, and the plurality of wet wipes are stacked inside the packaging container in the direction from the bottom to the top, as described in Aspect 18.
[0047] In the above-mentioned wet wipe packaging, the multiple wet wipes are stacked within a predetermined packaging container in the direction from the bottom to the top. Therefore, in the above-mentioned wet wipe packaging, the stacked wet wipe portions are less likely to stick together and are easier to separate, and the tendency for multiple wet wipes, including the next wet wipe, to be taken out at once when one wet wipe is removed is less likely to occur.
[0048] [Aspect 20] A method for manufacturing a laminated nonwoven fabric comprising a first surface layer, a second surface layer, and a core layer and a reinforcing layer disposed between the first surface layer and the second surface layer, comprising: a first surface layer web forming step of forming a first surface layer web constituting the first surface layer, which includes water-retaining fibers, by a carding method; a core layer web forming step of forming a core layer web constituting the core layer, which includes pulp fibers and heat-fusible fibers having an average fiber length of less than 20 mm, by an airlaid method; a reinforcing layer web forming step of forming a reinforcing layer web constituting the reinforcing layer, which includes heat-fusible fibers having an average fiber length of 20 mm or more and non-heat-fusible fibers having an average fiber length of 20 mm or more, by a carding method; a second surface layer web forming step of forming a second surface layer web constituting the second surface layer, which includes water-retaining fibers, by a carding method; and a laminated web forming step of laminating the first surface layer web, the reinforcing layer web, the core layer web and the second surface layer web to form a laminated web. A method for producing a laminated nonwoven fabric, comprising: a water flow entanglement step of subjecting the laminated web to a water flow entanglement treatment to form a water flow entangled laminated web; and a heat fusion step of heating the water flow entangled laminated web to heat fuse the heat-fusible fibers in the reinforcing layer web and the heat-fusible fibers in the core layer web to form a laminated nonwoven fabric.
[0049] The above method for manufacturing the laminated nonwoven fabric can produce the laminated nonwoven fabric described in Embodiment 1.
[0050] The laminated nonwoven fabric for wet wipes (hereinafter sometimes simply referred to as "laminated nonwoven fabric"), wet wipes, packaging for wet wipes, and method for manufacturing the laminated nonwoven fabric for wet wipes (hereinafter sometimes simply referred to as "method for manufacturing the laminated nonwoven fabric") related to this disclosure will be described in detail below.
[0051] [Laminated Nonwoven Fabric] The uses of the laminated nonwoven fabric according to this disclosure are not particularly limited, but it is suitable as a laminated nonwoven fabric for wet wipes. The laminated nonwoven fabric according to this disclosure comprises a first surface layer, a second surface layer, and a core layer and a reinforcing layer disposed between them. Since the first surface layer and the second surface layer may have the same composition, the first surface layer and the second surface layer may be collectively referred to as the "surface layer." When referred to as the "surface layer," it means at least one or both of the first surface layer and the second surface layer.
[0052] <Surface Layer (First Surface Layer and Second Surface Layer)> The above surface layer contains water-retaining fibers. The water-retaining fibers are not particularly limited as long as the fibers themselves can retain moisture, and examples include cellulosic fibers. Examples of cellulosic fibers include natural cellulose fibers, regenerated cellulose fibers, refined cellulose fibers, and semi-synthetic cellulose fibers. Examples of natural cellulose fibers include plant fibers, such as seed hair fibers (e.g., cotton fibers), pulp fibers (e.g., hemp), leaf vein fibers (e.g., Manila hemp), and fruit fibers (e.g., coconut).
[0053] Examples of the cotton fibers mentioned above include cotton fibers from the cotton species *Hirstum* (e.g., Upland cotton), cotton fibers from the cotton species *Barbadense*, cotton fibers from the cotton species *Arboreum*, and cotton fibers from the cotton species *Herbacheum*. Furthermore, these cotton fibers may be organic cotton fibers or pre-organic cotton® fibers. Organic cotton fibers refer to cotton certified by GOTS (Global Organic Textile Standard).
[0054] Examples of the regenerated cellulose fibers mentioned above include rayon, such as viscose rayon obtained from viscose, polynosic and modal, and copper ammonia rayon (also called "cupro") obtained from a copper ammonia salt solution of cellulose.
[0055] Examples of the purified cellulose fibers mentioned above include lyocell, specifically, obtained by dissolving pulp in an aqueous solution of N-methylmorpholine N-oxide to make a spinning stock (dope), and then extruding it into a dilute solution of N-methylmorpholine N-oxide to produce fibers. The purified cellulose is commercially available, for example, as Tencel (trademark). Examples of the semi-synthetic fibers mentioned above include semi-synthetic cellulose, such as acetate fibers, such as triacetate and diacetate.
[0056] In the surface layer described above, the water-retaining fibers are preferably regenerated cellulose fibers, and more preferably rayon fibers. This is due to the advantages of high water retention, ease of adjusting the average fiber length, and availability.
[0057] The water-retaining fibers described above preferably have an average fiber length of 20 mm or more, more preferably 30 mm or more, and even more preferably 35 mm or more. Furthermore, the water-retaining fibers preferably have an average fiber length of 80 mm or less, more preferably 60 mm or less, and even more preferably 50 mm or less. This makes it easier for the water-retaining fibers to entangle with other fibers, such as other water-retaining fibers or synthetic fibers as desired, thereby increasing the initial dry strength and initial wet strength of the laminated nonwoven fabric, and consequently the initial wet strength of the wet wipes.
[0058] The water-retaining fibers described above preferably have a fineness of 0.6 dtex or more, more preferably 1.0 dtex or more, and even more preferably 1.2 dtex or more. Alternatively, the water-retaining fibers may have a fineness of 3.3 dtex or less, more preferably 2.5 dtex or less, and even more preferably 2.0 dtex or less. This allows for the suppression of fiber clumping in the laminated nonwoven fabric containing the water-retaining fibers while maintaining tactile properties.
[0059] In this disclosure, the average fiber length of fibers other than pulp fibers is measured according to "A7.1 Measurement of fiber length" in Annex A of JIS L 1015:2010, specifically "A7.1.1 Method A (standard method): Method for measuring the length of individual fibers on a graduated glass plate." This method corresponds to the test method specified in ISO 6989, published in 1981.
[0060] In this disclosure, the average fiber length of pulp fibers means the weight-weighted average fiber length and refers to the L(w) value measured by Kajaani Fiber Lab Fiber Properties (off-line) manufactured by Metso Automation.
[0061] The surface layer may further contain synthetic fibers. The synthetic fibers may include those containing a single component, such as single fibers. Examples of such single components include polyolefin polymers, such as polyethylene and polypropylene; polyester polymers, such as terephthalate polymers, such as polyethylene terephthalate (PET), polybutylene terephthalate, and polypentylene terephthalate; polyamide polymers, such as nylon 6 and nylon 6,6; acrylic polymers; polyacrylonitrile polymers; and modified versions thereof. Furthermore, the single component constituting the synthetic fiber may be a component constituting the core layer heat-fusible fiber, as described later in the section on core layer heat-fusible fibers, such as "the low-melting-point thermoplastic resin constituting the biodegradable heat-fusible fiber" or "the high-melting-point thermoplastic resin constituting the biodegradable heat-fusible fiber."
[0062] In this specification, the above-mentioned synthetic fiber differs from the heat-fusible fiber described later in that it is not heat-fusible. From this viewpoint, it is preferable that the above-mentioned synthetic fiber has a higher melting point than the low-melting-point thermoplastic resin that constitutes the core layer heat-fusible fiber described later, and it is also preferable that it has a higher melting point than the low-melting-point thermoplastic resin that constitutes the reinforcing layer heat-fusible fiber described later. From this viewpoint, assuming that it is not heat-fusible, the above-mentioned synthetic resin may contain multiple components described later in the section on core layer heat-fusible fiber. In other words, a heat-fusible fiber is classified as a heat-fusible fiber if it is heat-fusible itself, and as a synthetic fiber if it is not heat-fusible itself.
[0063] In the surface layer described above, the synthetic fibers are preferably polyethylene terephthalate (PET) fibers. This is due to their high melting point, ease of creating a bulky surface layer, and availability.
[0064] The above synthetic fibers preferably have an average fiber length of 20 mm or more, more preferably 30 mm or more, and even more preferably 35 mm or more. Alternatively, the above synthetic fibers may have an average fiber length of 80 mm or less, more preferably 60 mm or less, and even more preferably 50 mm or less. This makes it easier for the above synthetic fibers to intertwine with other fibers, such as the above water-retaining fibers and other synthetic fibers, thereby increasing the initial dry strength and initial wet strength of the laminated nonwoven fabric, and consequently the initial wet strength of the wet wipes.
[0065] The synthetic fibers described above preferably have a fineness of 0.6 dtex or more, more preferably 1.0 dtex or more, and even more preferably 1.2 dtex or more. Alternatively, the synthetic fibers may have a fineness of 3.3 dtex or less, more preferably 2.5 dtex or less, and even more preferably 2.0 dtex or less. As a result, the wet wipes formed from the laminated nonwoven fabric have excellent bulkiness, resistance to flattening, and other properties.
[0066] When the surface layer contains the water-retentive fibers and the synthetic fibers, the surface layer contains the water-retentive fibers and the synthetic fibers at a mass ratio of preferably 10 to 50:50 to 90, more preferably 15 to 45:55 to 85, and even more preferably 20 to 40:60 to 80, based on a total of 100 parts by mass of the water-retentive fibers and the synthetic fibers. Thereby, wet wipes formed from the laminated nonwoven fabric are excellent in wiping properties, bulkiness, resistance to deformation, and the like.
[0067] Among the above surface layers, the surface layer adjacent to the later-described reinforcing layer preferably has a basis weight of 3.0 g / m 2 or more, more preferably 4.0 g / m 2 or more, and even more preferably 5.0 g / m 2 or more. Further, among the above surface layers, the surface layer adjacent to the later-described reinforcing layer preferably has a basis weight of 11.0 g / m 2 or less, more preferably 10.0 g / m 2 or less, and even more preferably 9.0 g / m 2 or less.
[0068] Among the above surface layers, the surface layer adjacent to the later-described core layer preferably has a basis weight of 7.0 g / m 2 or more, more preferably 9.0 g / m 2 or more, and even more preferably 11.0 g / m 2 or more. Further, among the above surface layers, the surface layer adjacent to the later-described core layer preferably has a basis weight of 21.0 g / m 2 or less, more preferably 19.0 g / m 2 or less, and even more preferably 17.0 g / m 2 or less.
[0069] <Core Layer> The core layer contains pulp fibers and heat-fused heat-fusible fibers. From the viewpoint of distinguishing the heat-fusible fibers in the core layer from the heat-fusible fibers of the later-described reinforcing layer, the heat-fusible fibers in the core layer may be referred to as core layer heat-fusible fibers in some cases.
[0070] Preferably, the core layer heat-fusible fibers are heat-fusible to each other, and in addition to being heat-fusible to each other, it is preferable that the core layer heat-fusible fibers and the pulp fibers are bonded together by the heat fusion of the core layer heat-fusible fibers. As a result, the core layer heat-fusible fibers form a framework, making it easier to hold the pulp fibers within the framework, and the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, is less prone to stretching, and is less prone to deformation. Consequently, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0071] In addition to being heat-fused to each other, the core layer heat-fusible fibers are more preferably heat-fused to the reinforcing layer heat-fusible fibers described later. Because the core layer heat-fusible fibers are heat-fused to the reinforcing layer heat-fusible fibers, the reinforcing layer can more easily reinforce the core layer, resulting in a laminated nonwoven fabric with high initial strength in both dry and wet conditions, and less stretching and deformation. As a result, when used as wet wipes, the laminated nonwoven fabric makes it less likely for adjacent wet wipe portions to stick together and easier to separate.
[0072] Preferably, the core layer heat-fusible fibers and one or both of the water-retaining fibers in the first surface layer and the water-retaining fibers in the second surface layer are bonded by heat fusion of the core layer heat-fusible fibers. As a result, the laminated nonwoven fabric has high initial strength when dry and high initial strength when wet, and is less prone to stretching and deformation. Consequently, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0073] The pulp fibers mentioned above can be any pulp fibers known in the art without limitation, such as wood pulp fibers and non-wood pulp fibers. Examples of wood pulp fibers include softwood pulp fibers and hardwood pulp fibers. Examples of non-wood pulp fibers include straw pulp fibers, bagasse pulp fibers, reed pulp fibers, kenaf pulp fibers, mulberry pulp fibers, bamboo pulp fibers, hemp pulp fibers, and cotton pulp fibers (e.g., cotton linter fibers).
[0074] The core layer heat-fusible fiber described above can be any heat-fusible fiber known in the art without limitation. Specifically, the core layer heat-fusible fiber can be a composite fiber (e.g., core-sheath type, side-by-side type, etc.) containing a low-melting-point thermoplastic resin and a high-melting-point thermoplastic resin. The composite fiber is preferably one that contains a low-melting-point thermoplastic resin, such as polyethylene resin or low-melting-point polypropylene, at least on its surface in order to fuse the core layer heat-fusible fibers together. Examples of the composite fiber include a core-sheath type composite fiber in which the core is polyethylene terephthalate resin and the sheath is polyethylene resin; a core-sheath type composite fiber in which the core is polypropylene resin and the sheath is polyethylene resin; a core-sheath type composite fiber in which the core is high-melting-point polypropylene resin and the sheath is low-melting-point polypropylene resin; a side-by-side type composite fiber made of polyethylene terephthalate resin and polyethylene resin; and a side-by-side type composite fiber made of polypropylene resin and polyethylene resin.
[0075] When the composite fibers in the core layer are core-sheath fibers comprising a core portion and a sheath portion, the sheath portion is preferably composed of a polymer containing an unsaturated carboxylic acid, an unsaturated carboxylic acid anhydride, or a mixture thereof as a monomer backbone, and more preferably a copolymer of an olefin monomer and an unsaturated carboxylic acid, an unsaturated carboxylic acid anhydride, or a mixture thereof. As a result, the heat-fusible fibers that are heat-fused in the core layer have a high affinity for the pulp fibers and are able to hold the pulp fibers more easily. Consequently, the core layer has high initial strength when dry and when wet, and the laminated nonwoven fabric has high initial strength when dry and when wet, and is less prone to stretching and deformation. The polymer is disclosed, for example, in Japanese Patent Application Publication No. 2003-49360.
[0076] The core layer heat-fusible fiber described above can be a biodegradable heat-fusible fiber. This makes the laminated nonwoven fabric, and consequently the wet wipes, more biodegradable. Examples of the low-melting-point thermoplastic resins that constitute the biodegradable heat-fusible fiber include polybutylene succinate, poly(hydroxybutyrate / hydroxyhexanoate), polycaprolactone, poly(caprolactone / butylene succinate), poly(butylene succinate / adipate), poly(butylene succinate / carbonate), poly(butylene adipate / terephthalate), polyethylene succinate, or polylactic acid.
[0077] Examples of the high-melting-point thermoplastic resins that constitute the biodegradable, heat-fusible fibers mentioned above include polylactic acid, polyhydroxybutyrate, polyglycolic acid, or cellulose acetate.
[0078] Because the core layer's heat-fusible fibers are composite fibers, the core layer has high initial strength, and consequently, the laminated nonwoven fabric has high initial strength in both dry and wet conditions, is resistant to stretching, and is resistant to deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0079] The core layer heat-fusible fibers described above preferably have a shorter average fiber length than the reinforcing layer heat-fusible fibers described later, more preferably less than 20 mm, even more preferably 15 mm or less, and even more preferably 10 mm or less. Furthermore, the core layer heat-fusible fibers preferably have an average fiber length of 3 mm or more, more preferably 4 mm or more, and even more preferably 5 mm or more. As a result, in the core layer, the core layer heat-fusible fibers are more easily dispersed within the pulp fibers, and the heat-fusible core layer heat-fusible fibers form a skeleton, making it easier to hold the pulp fibers within the skeleton.
[0080] The heat-fusible fibers in the core layer preferably have a fineness of 0.6 dtex or more, more preferably 1.0 dtex or more, and even more preferably 1.4 dtex or more. Furthermore, the heat-fusible fibers preferably have a fineness of 3.3 dtex or less, more preferably 2.5 dtex or less, and even more preferably 2.0 dtex or less. This allows the heat-fusible fibers to form a framework and facilitates the retention of pulp fibers within that framework.
[0081] Preferably, the average fiber length of the heat-fusible fibers in the core layer is greater than the average fiber length of the pulp fibers. As a result, the core layer has high initial strength when dry and when wet, and consequently, the laminated nonwoven fabric has high initial strength when dry and when wet, and is less prone to stretching and deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0082] The core layer contains pulp fibers and core layer heat-fusible fibers in a mass ratio of preferably 65-99:1-35, more preferably 75-98:2-25, and even more preferably 85-95:5-15, based on 100 parts by mass of the total of the pulp fibers and the core layer heat-fusible fibers. This allows the heat-fusible core layer fibers to form a framework and makes it easier to hold the pulp fibers within the framework. Generally, heat-fusible fibers have excellent whiteness. Therefore, the inclusion of the core layer heat-fusible fibers has the effect of making irregularities in the laminated nonwoven fabric less noticeable. From the viewpoint of making irregularities in the laminated nonwoven fabric less noticeable, it is preferable that the core layer heat-fusible fibers contain a pigment such as titanium dioxide.
[0083] The core layer is preferably 8.0 g / m². 2 More preferably, 10.0 g / m 2 The above, and more preferably 12.0 g / m² 2 It has the above basis weight. Furthermore, the core layer is preferably 30.0 g / m². 2 More preferably, 26.0 g / m² 2 The following, and more preferably 21.0 g / m² 2 It has the following basis weight. As a result, when the laminated nonwoven fabric is used as a wet wipe, it has excellent liquid retention and wiping properties.
[0084] [Reinforcement Layer] The above-mentioned reinforcement layer contains heat-fusible fibers that have been heat-fused and non-heat-fusible fibers. In addition, from the viewpoint of distinguishing the heat-fusible fibers in the reinforcement layer from the heat-fusible fibers in the core layer, the heat-fusible fibers in the reinforcement layer may be referred to as reinforcement layer heat-fusible fibers.
[0085] Since the heat-fusible fibers of the reinforcing layer described above are the same as those of the heat-fusible fibers of the core layer, except for the average fiber length, the explanation for the heat-fusible fibers of the core layer described above will be applied, except for the average fiber length. The heat-fusible fibers of the reinforcing layer may or may not contain a polymer containing the above-mentioned unsaturated carboxylic acid, unsaturated carboxylic acid anhydride, or a mixture thereof as a monomer backbone.
[0086] Preferably, the heat-fusible fibers of the reinforcing layer are heat-fusible to each other, and more preferably, in addition to being heat-fusible to each other, they are heat-fusible to the heat-fusible fibers of the core layer. This makes it easier for the reinforcing layer to reinforce the core layer, and the laminated nonwoven fabric has high initial strength when dry and when wet, and is less prone to stretching and deformation. Furthermore, it is preferable that the heat-fusible fibers of the reinforcing layer are heat-fusible to one or both of the water-retaining fibers in the first surface layer and the water-retaining fibers in the second surface layer. This makes it easier for the reinforcing layer to reinforce the core layer, and the laminated nonwoven fabric has high initial strength when dry and when wet, and is less prone to stretching and deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0087] The heat-fusible fibers in the reinforcing layer preferably have an average fiber length of 20 mm or more, more preferably 30 mm or more, and even more preferably 40 mm or more. Furthermore, the heat-fusible fibers in the reinforcing layer preferably have an average fiber length of 80 mm or less, more preferably 70 mm or less, and even more preferably 60 mm or less. As a result, the reinforcing layer can easily reinforce the core layer, and the laminated nonwoven fabric has high initial strength when dry and when wet, and is less prone to stretching and deformation.
[0088] The heat-fusible fibers in the reinforcing layer preferably have a fineness of 0.6 dtex or more, more preferably 1.2 dtex or more, and even more preferably 1.8 dtex or more. Alternatively, the heat-fusible fibers may have a fineness of 3.3 dtex or less, more preferably 3.0 dtex or less, and even more preferably 2.5 dtex or less. This makes it easier for the reinforcing layer to reinforce the core layer, resulting in a laminated nonwoven fabric with high initial strength in both dry and wet conditions, and less prone to stretching and deformation.
[0089] Because the heat-fusible reinforcing layer fibers are composite fibers, the reinforcing layer has high initial strength when dry and when wet, and consequently, the laminated nonwoven fabric has high initial strength when dry and when wet, and is less prone to stretching and deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate. In addition, heat-fusible fibers generally have excellent whiteness. Therefore, the inclusion of the heat-fusible reinforcing layer fibers has the effect of making irregularities in the laminated nonwoven fabric less noticeable. From the viewpoint of making irregularities in the laminated nonwoven fabric less noticeable, it is preferable that the heat-fusible reinforcing layer fibers contain a pigment such as titanium dioxide.
[0090] The non-heat-fusible fibers mentioned above can be any fiber known in the art, without particular limitation, as long as they do not possess heat-fusible properties themselves. Preferably, the non-heat-fusible fibers are either water-retaining fibers or synthetic fibers, or both. If the non-heat-fusible fibers are water-retaining fibers, the water-retaining fibers can directly hold the chemical solution, thereby increasing the water retention of the reinforcing layer. If the non-heat-fusible fibers are synthetic fibers, the volume of the reinforcing layer can be increased. This reduces the amount of chemical solution present in the first and second surface layers. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate. Note that the non-heat-fusible fibers in the laminated nonwoven fabric refer to fibers that do not exhibit heat-fusible properties themselves, that is, fibers that are not deformed by heat and do not fuse with other fibers. Therefore, this does not exclude the possibility that the heat-fusible fibers (such as the core layer heat-fusible fibers and the reinforcing layer heat-fusible fibers) deform due to heat and heat-fuse with the non-heat-fusible fibers.
[0091] Since the water-retaining fibers described above are the same as the water-retaining fibers described in the surface layer, the explanation regarding the water-retaining fibers in the surface layer will be applied. Since the synthetic fibers described above are the same as the synthetic fibers described in the surface layer, the explanation regarding the synthetic fibers in the surface layer will be applied.
[0092] In the above-mentioned reinforcing layer, the water-retaining fibers are preferably regenerated cellulose fibers, and more preferably rayon fibers. This is from the viewpoint of high water retention, ease of adjusting the average fiber length, and availability. In the above-mentioned reinforcing layer, the synthetic fibers are preferably polyethylene terephthalate (PET) fibers. This is from the viewpoint of high melting point, ease of increasing the bulk of the reinforcing layer, and availability.
[0093] The above reinforcing layer is preferably 3.0 g / m². 2 More preferably 4.0 g / m 2 The above, and more preferably 5.0 g / m² 2 It has the above basis weight. Furthermore, the reinforcing layer is preferably 11.0 g / m². 2 More preferably, 10.0 g / m 2 The following, and more preferably 9.0 g / m² 2 The following basis weight is provided. This makes it easier for the reinforcing layer to reinforce the core layer, and the laminated nonwoven fabric has high initial strength when dry and when wet, and is resistant to stretching and deformation.
[0094] The laminated nonwoven fabric described above may, for example, be a laminated nonwoven fabric having a four-layer structure consisting of a first surface layer forming one surface, a second surface layer forming the other surface, a core layer disposed between the first surface layer and the second surface layer, and a reinforcing layer disposed between the first surface layer and the core layer. The laminated nonwoven fabric may also, for example, be a laminated nonwoven fabric having a five-layer structure consisting of a first surface layer forming one surface, a second surface layer forming the other surface, a core layer disposed between the first surface layer and the second surface layer, a reinforcing layer (first reinforcing layer) disposed between the first surface layer and the core layer, and a reinforcing layer (second reinforcing layer) disposed between the second surface layer and the core layer. In the laminated nonwoven fabric having the five-layer structure described above, since there are two reinforcing layers above and below the core layer in the thickness direction, the reinforcing layers can more easily reinforce the core layer, and the laminated nonwoven fabric has high initial strength when dry and when wet, is less prone to stretching, and is less prone to deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0095] As shown in Figure 1, the laminated nonwoven fabric 1 according to one embodiment of the present disclosure (first embodiment) comprises a first surface layer 3, a reinforcing layer 5, a core layer 7, and a second surface layer 9 in that order, and has a four-layer structure.
[0096] In the above laminated nonwoven fabric, in a tensile test during dry conditions, the product of the elongation at maximum strength (%) and the strength at 5% elongation (N / 25mm) in the orthogonal direction perpendicular to the conveying direction during manufacturing is P. D5% However, basis weight 50 g / m² 2 In terms of conversion, it is preferably 35 or more, more preferably 38 or more, and even more preferably 40 or more. Furthermore, in the laminated nonwoven fabric, the product: P D5% However, basis weight 50 g / m² 2 In terms of conversion, the value is preferably 120 or less, more preferably 110 or less, and even more preferably 100 or less. As a result, the laminated nonwoven fabric has high initial strength when dry and is less prone to tearing. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate.
[0097] Note: Product: P D5% The elongation at maximum strength of the laminated nonwoven fabric in the dry tensile test is E DMAX (%) and strength at 5% elongation: S D5% (N / 25mm) and basis weight: BW (g / m²) 2 ) From this, the following equation: P D5% = E DMAX ×S D5% It can be calculated by multiplying by (50 / BW). In this specification, the transport direction when manufacturing the laminated nonwoven fabric is sometimes referred to as the MD direction, and the direction perpendicular to the MD direction during manufacturing is sometimes referred to as the CD direction.
[0098] In the above laminated nonwoven fabric, in a dry tensile test, the product of the elongation at maximum strength (%) and the strength at 10% elongation (N / 25mm) in the CD direction is P D10% The basis weight is 50 g / m². 2 In terms of conversion, it is preferably 65 or more, more preferably 70 or more, and even more preferably 75 or more. Furthermore, in the laminated nonwoven fabric, the product: P D10% The basis weight is 50 g / m². 2 In terms of conversion, the value is preferably 160 or less, more preferably 150 or less, and even more preferably 140 or less. As a result, the laminated nonwoven fabric has high initial strength when dry and is less prone to tearing. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate.
[0099] Note: Product: P D10% The elongation at maximum strength of the laminated nonwoven fabric in the dry tensile test is E DMAX (%) and strength at 10% elongation: S D10% (N / 25mm) and basis weight: BW (g / m²) 2 ) From this, the following equation: P D10% = E DMAX ×S D10% It can be calculated by multiplying by (50 / BW).
[0100] In the above laminated nonwoven fabric, in a dry tensile test, the product of the elongation at maximum strength (%) and the strength at 50% elongation (N / 25mm) in the CD direction is P. D50%The basis weight is 50 g / m². 2 In terms of conversion, it is preferably 200 or more, more preferably 210 or more, and even more preferably 220 or more. Furthermore, in the above laminated nonwoven fabric, the product: P D50% The basis weight is 50 g / m². 2 In terms of conversion, the value is preferably 400 or less, more preferably 370 or less, and even more preferably 350 or less. As a result, the laminated nonwoven fabric has high initial strength when dry and is less prone to tearing. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate.
[0101] Note: Product: P D50% The elongation at maximum strength of the laminated nonwoven fabric in the dry tensile test is E DMAX (%) and strength at 50% elongation: S D50% (N / 25mm) and basis weight: BW (g / m²) 2 ) From this, the following equation: P D50% = E DMAX ×S D50% It can be calculated by multiplying by (50 / BW).
[0102] In this specification, the dry tensile test described above shall be carried out as follows: [Dry Tensile Test] (1) Prepare a laminated nonwoven fabric and dry it at 75°C for 180 minutes to form a sample (length: 150 mm x width: 25 mm). The sample may be obtained so that the length in the CD direction is 150 mm, or so that the length in the MD direction is 150 mm. For example, in the case of tensile strength in the CD direction, the sample shall be obtained so that the length in the CD direction is 150 mm. (2) Mount the sample on a tensile testing machine (Shimadzu Autograph AGS-1kNG) with a gripping distance of 100 mm, and apply a load (maximum point load) at a tensile speed of 100 mm / min until the sample is cut, and measure the strength at 5% elongation (N / 25 mm), the strength at 10% elongation (N / 25 mm), the strength at 50% elongation (N / 25 mm), the maximum strength (N / 25 mm), and the elongation at maximum strength (%).
[0103] (3) The strength at 5% elongation (N / 25mm), strength at 10% elongation (N / 25mm), strength at 50% elongation (N / 25mm), maximum strength (N / 25mm), and elongation at maximum strength (%) are measured on 10 different samples, and the average value is adopted. The above dry tensile test is carried out under the conditions of temperature: 23°C ± 2°C and relative humidity: 50 ± 5% RH.
[0104] For the dry tensile test described above, conditions not specified above shall be in accordance with JIS L 1913:2010, "6.3 Tensile strength and elongation (ISO method)". Note that the strength at n% elongation (N / 25mm) refers to the tensile strength (N) per 25 mm width when the sample is elongated by n%. Furthermore, the maximum strength (N / 25mm) refers to the maximum value of the tensile strength in the tensile test, and the elongation at maximum strength (%) refers to the elongation (%) at the maximum strength (N / 25mm).
[0105] In the above laminated nonwoven fabric, in a wet tensile test, the product of the elongation at maximum strength (%) and the strength at 5% elongation (N / 25mm) in the CD direction is P W5% The basis weight is 50 g / m². 2 In terms of conversion, it is preferably 25 or more, more preferably 30 or more, and even more preferably 32 or more. Furthermore, in the above laminated nonwoven fabric, the product: P W5% The basis weight is 50 g / m². 2 In terms of conversion, the value is preferably 100 or less, more preferably 90 or less, and even more preferably 80 or less. As a result, the laminated nonwoven fabric has high initial strength when wet and is less prone to tearing. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate.
[0106] Note: Product: P W5% The elongation at maximum strength of the laminated nonwoven fabric in the wet tensile test described above is E WMAX (%) and strength at 5% elongation: S W5% (N / 25mm) and basis weight: BW (g / m²) 2 ) From this, the following equation: P W5% = E WMAX ×S W5% It can be calculated by multiplying by (50 / BW).
[0107] In the above laminated nonwoven fabric, in a wet tensile test, the product of the elongation at maximum strength (%) and the strength at 10% elongation (N / 25mm) in the CD direction is P W10% The basis weight is 50 g / m². 2 In terms of conversion, it is preferably 40 or more, more preferably 45 or more, and even more preferably 50 or more. Furthermore, in the laminated nonwoven fabric described above, the product: P W10% The basis weight is 50 g / m². 2 In terms of conversion, the value is preferably 120 or less, more preferably 100 or less, and even more preferably 80 or less. As a result, the laminated nonwoven fabric has high initial strength when wet and is less prone to tearing. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate.
[0108] Note: Product: P W10% The elongation at maximum strength of the laminated nonwoven fabric in the wet tensile test described above is E WMAX (%) and strength at 10% elongation: S W10% (N / 25mm) and basis weight: BW (g / m²) 2 ) From this, the following equation: P W10% = E WMAX ×S W10% It can be calculated by multiplying by (50 / BW).
[0109] In the above laminated nonwoven fabric, in a wet tensile test, the product of the elongation at maximum strength (%) and the strength at 50% elongation (N / 25mm) in the CD direction is P W50% The basis weight is 50 g / m². 2 In terms of conversion, it is preferably 130 or more, more preferably 150 or more, and even more preferably 160 or more. Furthermore, in the above laminated nonwoven fabric, the product: P W50% The basis weight is 50 g / m². 2 In terms of conversion, the value is preferably 300 or less, more preferably 260 or less, and even more preferably 240 or less. As a result, the laminated nonwoven fabric has high initial strength when wet and is less prone to tearing. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are easier to separate.
[0110] Note that the product: P W50% is the elongation at maximum strength of the laminated nonwoven fabric in the wet tensile test described above: E WMAX (%), the strength at 50% elongation: S W50% (N / 25mm), and the basis weight: BW (g / m 2 ), and can be calculated by the following formula: P W50% =E WMAX ×S W50% ×(50 / BW).
[0111] In the present specification, the wet tensile test described above is performed as follows. [Wet Tensile Test] (1) A laminated nonwoven fabric is prepared and dried at 75°C for 180 minutes, and then a sample (length: 150 mm × width: 25 mm) is prepared. The sample may be taken such that the length in the CD direction is 150 mm, or such that the length in the MD direction is 150 mm. For example, in the case of the tensile strength in the CD direction, the sample is taken such that the length in the CD direction is 150 mm. (2) The sample is impregnated with deionized water in an amount of 240% of the sample mass, so that the impregnation ratio is 240%.
[0112] (3) The sample is mounted on a tensile tester (Autograph AGS-1kNG manufactured by Shimadzu Corporation) with a grip interval of 100 mm, and a load (maximum point load) is applied at a tensile speed of 100 mm / min until the sample is broken, to measure the strength at 5% elongation (N / 25mm), the strength at 10% elongation (N / 25mm), the strength at 50% elongation (N / 25mm), the maximum strength (N / 25mm), and the elongation at maximum strength (%). (4) For the strength at 5% elongation (N / 25mm), the strength at 10% elongation (N / 25mm), the strength at 50% elongation (N / 25mm), the maximum strength (N / 25mm), and the elongation at maximum strength (%), measurements are performed on 10 different samples, and the average value is adopted.
[0113] The wet tensile test described above is carried out under conditions of a temperature of 23°C ± 2°C and a relative humidity of 50 ± 5% RH. Regarding the wet tensile test described above, conditions not specified above conform to "6.3 Tensile Strength and Elongation (ISO Method)" of JIS L 1913:2010.
[0114] The above laminated nonwoven fabric preferably has a basis weight of 20 g / m 2 or more, more preferably 30 g / m 2 or more, and even more preferably 35 g / m 2 or more. Further, the above laminated nonwoven fabric preferably has a basis weight of 100 g / m 2 or less, more preferably 90 g / m 2 or less, even more preferably 80 g / m 2 or less, and still even more preferably 70 g / m 2 or less. This makes it easy to ensure the take-out property of wet wipes formed from the above laminated nonwoven fabric and the strength during wiping and the like.
[0115] In the present specification, the basis weight is determined by drying the laminated nonwoven fabric at 75°C for 180 minutes, then collecting 10 samples each having a size of 100 mm × 100 mm, measuring the mass of each sample, and then, for each sample, the value of mass (g) / area (m 2 ) is calculated as the respective basis weight (g / m 2 ), and the average value of the basis weights of the total 10 samples is taken as the basis weight. In addition, when it is difficult to collect a sample of the above size, a sample can be collected within a possible range.
[0116] The above laminated nonwoven fabric preferably has a dry thickness of 0.25 mm or more, more preferably 0.30 mm or more, and even more preferably 0.35 mm or more. Further, the above laminated nonwoven fabric preferably has a dry thickness of 0.90 mm or less, more preferably 0.80 mm or less, and even more preferably 0.70 mm or less. This makes it easy to ensure the take-out property of wet wipes formed from the above laminated nonwoven fabric and the strength during wiping and the like.
[0117] In the present specification, the above dry thickness is measured using THICKNESS GAUGE, UF-60 manufactured by Daiei Kagaku Seiki Seisakusho Co., Ltd. Note that in UF-60, the diameter of the measurement surface is 44 mm. Specifically, a pressure of 0.3 kPa is applied to the laminated nonwoven fabric, and the dry thickness is measured. In addition, the above dry thickness is measured after the laminated nonwoven fabric is dried at 75°C for 180 minutes.
[0118] The laminated nonwoven fabric has a wet thickness of preferably 0.15 mm or more, more preferably 0.20 mm or more, and even more preferably 0.25 mm or more. Furthermore, the laminated nonwoven fabric has a wet thickness of preferably 0.70 mm or less, more preferably 0.60 mm or less, and even more preferably 0.50 mm or less. This makes it easier to ensure both the ease of dispensing wet wipes and the strength required for wiping.
[0119] The wet thickness is measured using a THICKNESS GAUGE, UF-60, manufactured by Daiei Kagaku Seiki Seisakusho Co., Ltd., after impregnating the laminated nonwoven fabric with deionized water equivalent to 240% of its mass, resulting in an impregnation rate of 240%. The diameter of the measuring surface of the UF-60 is 44 mm. Specifically, a pressure of 0.3 kPa is applied to the laminated nonwoven fabric, and the wet thickness is measured.
[0120] The laminated nonwoven fabric described above can be any nonwoven fabric manufactured by known methods such as the dry method, wet method, water jet method (water entanglement method), spunbond method, airlaid method, needle punch method, felt method, etc. (for example, spunlace nonwoven fabric, air-through nonwoven fabric, spunbond nonwoven fabric, point bond nonwoven fabric, etc.), and spunlace nonwoven fabric is preferred. Because the laminated nonwoven fabric is a spunlace nonwoven fabric, fibers of a certain length that constitute the laminated nonwoven fabric are entangled, so the laminated nonwoven fabric has high initial strength when dry and when wet, is less prone to stretching, and is less prone to deformation. As a result, when the laminated nonwoven fabric is used as a wet wipe, adjacent wet wipe portions are less likely to stick together and are more likely to separate.
[0121] [Wet wipes and packaging for wet wipes] The wet wipes according to this disclosure include a nonwoven fabric sheet made of the laminated nonwoven fabric described above and a chemical solution. The nonwoven fabric sheet is made of the laminated nonwoven fabric described above and is formed by cutting the laminated nonwoven fabric to a desired size.
[0122] The above-mentioned chemical solution can be any chemical solution used in the art without limitation. The above-mentioned chemical solution may contain, for example, an antibacterial agent, a surfactant, water, a hydrophilic organic solvent (e.g., ethanol), a fragrance, etc.
[0123] The above fragrance can have any vapor pressure at 25°C. Preferably, at 25°C, the above fragrance has a vapor pressure of 10.00 Pa (0.075 mmHg) or more, more preferably 13.33 Pa (0.1 mmHg) or more, even more preferably 20.00 Pa (0.15 mmHg) or more, and even more preferably 26.66 Pa (0.2 mmHg) or more. Alternatively, at 25°C, the above fragrance has a vapor pressure of 1333 Pa (10 mmHg) or less, more preferably 666.5 Pa (5 mmHg) or less, and even more preferably 266.6 Pa (2 mmHg) or less. As a result, the pulp fibers in the core layer, and the water-retaining fibers (as non-heat-fusible fibers) in the optional reinforcing layer, etc., hold the chemical solution containing the fragrance, and when wiped with a wet wipe, the fragrance contained in the chemical solution volatilizes in a short time, allowing the fragrance to be released quickly. Furthermore, when the above-mentioned wet wipes are used to cleanse the skin, the fragrance contained in the above-mentioned solution evaporates and disappears in a short time, making it less likely to cause skin problems.
[0124] If the above-mentioned liquid contains a fragrance, the liquid contains the fragrance at a concentration of preferably 0.005% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.02% by mass or more, and preferably 0.5% by mass or less, more preferably 0.2% by mass or less, and even more preferably 0.1% by mass or less. If the fragrance concentration is too high, a large amount of solubilizer will be required to dissolve the fragrance (oil) transparently in the liquid, which can cause stickiness and foaming of the liquid, and tend to reduce the usability as a wet wipe. In addition, infants and guardians with a keen sense of smell may feel unwell due to the strong fragrance. If the fragrance concentration is too low, consumers may have difficulty recognizing the intended fragrance.
[0125] The above fragrance preferably includes, for example, Nature Identical as an ingredient. Nature Identical is a synthetic substance that has the exact same chemical structure as a substance found in nature. Examples of nature-identical ingredients include α-pinene, β-pinene, limonene, camphene, γ-terpinene, myrcene, citronellal, 1,8-cineole, rose oxide, linalyl acetate, hexyl acetate, amyl acetate, benzyl acetate, isobornyl acetate, terpinyl acetate, heptyl acetate, isoamyl butyrate, ethyl isobutyrate, ethyl caproate, methyl hexanoate, methyl octanoate, benzyl propionate, cis-4-hexenyl acetate, methyl benzoate, ethyl benzoate, diethyl malonate, octanal, nonanal, decanal, linalool, phenylethyl aldehyde, cis-3-hexenol, linalool, tetrahydrolinalool, dihydromyrcenolate, acetophenone, camphor, menthone, i-carbone, etc. It is preferable that the above fragrance consists solely of nature-identical ingredients. This is from a safety standpoint.
[0126] <Fragrances in the chemical solution, their ratios, and vapor pressure> The identification of fragrances in the chemical solution, their ratios, and their vapor pressures are determined as follows: (1) The individual components of the fragrance contained in the chemical solution and their ratios can be identified by placing the wet wipe sample directly into a headspace vial and performing GC-MS analysis using the SPME method. (2) The vapor pressure of each component is calculated using Raoult's Law based on the measured components and their ratios, and the vapor pressure data of each component. The vapor pressure data used is the value calculated by MPBPWIN in the EPI Suite (Estimation Programs Interface Suite) published by the U.S. Environmental Protection Agency (EPA) (Mean VP of Antonine & Grain methods). MPBPWIN is a program for estimating the melting point, boiling point, and vapor pressure of organic chemical substances. Mean VP of Antonine & Grain methods refers to the recommended average value used in MPBPWIN when estimating the vapor pressure (VP) of gaseous and liquid chemical substances.
[0127] In the above-mentioned wet wipes, the impregnation rate, which is the ratio of the chemical solution impregnated into the nonwoven fabric sheet, can be one of those commonly used in the art. The impregnation rate (mass%) [= 100 × (mass of chemical solution) / (mass of nonwoven fabric sheet)] can be, for example, 100% by mass or more, more preferably 150% by mass or more, and even more preferably 200% by mass or more. Furthermore, the impregnation rate can be preferably 700% by mass or less, more preferably 600% by mass or less, even more preferably 500% by mass or less, and even more preferably 400% by mass or less.
[0128] The wet wipe packaging described above comprises multiple wet wipes and a packaging body that houses the multiple wet wipes. Examples of the packaging body include packaging sheet type (e.g., pillow type), pop-up type, bottle type, and other packaging containers. When the packaging body is of the packaging sheet type, one or more wet wipes are housed in the packaging sheet. In this case, if the packaging contains one wet wipe, that one wet wipe is folded. In this case, if the packaging contains multiple wet wipes, the multiple wet wipes may or may not be folded.
[0129] Furthermore, if the packaging itself is a sheet-type or pop-up type packaging container, multiple wet wipes are stored in the packaging container. In this case, the wet wipes are less likely to stick together and are easier to separate, and the tendency for multiple wet wipes to be taken out at once when one wet wipe is removed is reduced. In addition, because the wet wipes are less likely to stick together and are easier to separate, and because the wet wipes themselves are strong, it becomes easier to take out the wet wipes.
[0130] The above-described packaging sheet type or pop-up type packaging container may have a top with an opening and a bottom. The plurality of wet wipes may be stacked within the packaging container in the direction from the bottom to the top. Furthermore, the plurality of wet wipes may be arranged within the packaging container such that a portion of the bottom-side wet wipes located towards the bottom and a portion of the top-side wet wipes adjacent to the top are positioned so that the portion of the bottom-side wet wipes is located towards the top than the portion of the top-side wet wipes. As a result, in the packaging of the wet wipes, the stacked wet wipe portions are less likely to stick together and are more likely to separate, and the tendency for multiple wet wipes, including the next wet wipe, to be taken out at once when one wet wipe is taken out is reduced.
[0131] Figure 2 is a perspective view of a wet wipes packaging 101 according to one embodiment of the present disclosure (hereinafter referred to as the "second embodiment"), and Figure 3 is an end view of the wet wipes packaging 101 at the III-III end face shown in Figure 2. The wet wipes packaging 101 according to the second embodiment comprises a plurality of wet wipes 109 and a packaging body 103 that houses the plurality of wet wipes 109. The packaging body 103 is a packaging sheet type (pillow type) packaging container and has a top T with an opening 105 and a bottom B. The plurality of wet wipes 109 are stored inside the packaging body 103 so that they can be sequentially removed.
[0132] The packaging body 103 has a sealing material 107 that covers the opening 105. The packaging body 103 is bag-shaped, and when the opening 105 is sealed with the sealing material 107, the wet wipes inside the packaging body 103 can be sealed, and evaporation of the medicine is suppressed. Each wet wipe can be removed through the opening 105. The sealing material 107 has an adhesive applied to the surface that comes into contact with the packaging body 103 in order to repeatedly seal the wet wipes inside the packaging body 103.
[0133] As shown in Figure 3, inside the packaging body 103, multiple wet wipes 109 are stacked in a direction from the top T to the bottom B. Each of the multiple wet wipes 109 has an outward tri-fold (approximately Z-shaped) folding structure with a first fold line and a second fold line. Furthermore, the multiple wet wipes 109 are stacked such that adjacent wet wipes 109 in the thickness direction (direction from the top T to the bottom B) face the same direction (so that the first fold lines overlap in the thickness direction, and the second fold lines overlap in the thickness direction).
[0134] Figure 4 is a diagram illustrating the multiple wet wipes 109 housed in the wet wipe packaging 101 shown in Figure 3. The wet wipes 109', 109'', and 109'''' are stacked sequentially from the top T to the bottom B. In the relationship between wet wipes 109' and 109'', the top end 109''T of the wet wipe 109'' (bottom wet wipe) located on the bottom B side and the bottom end 109'B of the wet wipe 109' (top wet wipe) adjacent to its top T side overlap each other such that the top end 109''T of the wet wipe 109'' (bottom wet wipe) is located closer to the top T than the bottom end 109'B of the wet wipe 109' (top wet wipe).
[0135] Similarly, in Figure 4, regarding the relationship between wet wipes 109'' and wet wipes 109''', the top end 109'''T of wet wipe 109''' (bottom-side wet wipe) located on the bottom B side and the bottom end 109''B of wet wipe 109'' (top-side wet wipe) adjacent to its top T side overlap each other such that the top end 109'''T of wet wipe 109''' (bottom-side wet wipe) is located closer to the top T side than the bottom end 109''B of wet wipe 109'' (top-side wet wipe).
[0136] As shown in Figures 3 and 4, when multiple wet wipes 109 are stacked, a portion of the wet wipe 109'' (mainly the top end 109''T) is pulled out when a wet wipe 109' is removed, protruding from the packaging body 103, making it easier to remove the wet wipe 109'' for the next use.
[0137] Furthermore, if the water film of the medicated solution formed between the wet wipes connects the bottom end 109'B of wet wipe 109' and the top end 109''T of wet wipe 109'', there may be a tendency for multiple wipes to be removed at once, such as when removing wet wipe 109', the entire wet wipe 109'' being removed together. In the wet wipe packaging 101 according to the second embodiment, since the wet wipe 109 is a specific wet wipe, it offers excellent single-wipe removal.
[0138] [Method for manufacturing laminated nonwoven fabric for wet wipes] The laminated nonwoven fabric for wet wipes according to this disclosure, comprising a first surface layer, a second surface layer, and a core layer and a reinforcing layer disposed between the first surface layer and the second surface layer, can be manufactured by methods known in the art.
[0139] The laminated nonwoven fabric for wet wipes according to this disclosure, comprising a first surface layer, a second surface layer, and a core layer and a reinforcing layer disposed between the first surface layer and the second surface layer, can be manufactured, for example, by a method for manufacturing a laminated nonwoven fabric that includes the following steps. - A first surface layer web forming step (hereinafter referred to as the "first surface layer web forming step") in which a first surface layer web constituting the first surface layer, which includes water-retaining fibers, is formed by the carding method. - A core layer web forming step (hereinafter referred to as the "core layer web forming step") in which a core layer web constituting the above core layer, which includes pulp fibers and heat-fusible fibers having an average fiber length of less than 20 mm, is formed by the airlaid method. - A reinforcing layer web forming step (hereinafter referred to as the "reinforcing layer web forming step") in which a reinforcing layer web constituting the above reinforcing layer, which includes heat-fusible fibers having an average fiber length of 20 mm or more and non-heat-fusible fibers having an average fiber length of 20 mm or more, is formed by the carding method. - A second surface layer web forming step (hereinafter referred to as the "second surface layer web forming step") in which a second surface layer web constituting the second surface layer, which includes water-retaining fibers, is formed by the carding method. - A laminated web forming step (hereinafter referred to as the "laminated web forming step") in which the first surface layer web, the reinforcing layer web, the core layer web, and the second surface layer web are laminated together. - A water flow entanglement treatment step (hereinafter referred to as the "water flow entanglement treatment step") in which the laminated web is subjected to a water flow entanglement treatment to form a water flow entangled laminated web. - A heat fusion step (hereinafter referred to as the "heat fusion step") in which the water flow entangled laminated web is heated to heat fuse the heat-fusible fibers in the reinforcing layer web and the heat-fusible fibers in the core layer web to form a laminated nonwoven fabric.
[0140] In the first surface layer web formation step, a first surface layer web constituting the first surface layer, which includes water-retaining fibers, is formed by a carding method. For example, in the first surface layer web formation step, a carding machine can be used to mechanically open the fibers constituting the first surface layer (water-retaining fibers, desired synthetic fibers, etc.) to form the first surface layer web. As the carding machine is well known in the art, its description is omitted. The second surface layer web formation step is the same as the first surface layer web formation step, so its description is omitted.
[0141] In the core layer web formation step described above, a core layer web constituting the core layer, which includes pulp fibers and heat-fusible fibers having an average fiber length of less than 20 mm, is formed by an airlaid method. For example, in the core layer web formation step, an airlaid apparatus can be used to uniformly disperse the fibers constituting the core layer (pulp fibers, heat-fusible fibers having an average fiber length of less than 20 mm, etc.) and laminate them on a support (e.g., a mesh) to form a core layer web. The airlaid apparatus described above is well known in the art, so its description is omitted.
[0142] In the above-described reinforced layer web formation step, a reinforced layer web constituting the reinforced layer is formed by a carding method, comprising heat-fusible fibers having an average fiber length of 20 mm or more and non-heat-fusible fibers having an average fiber length of 20 mm or more. For example, in the above-described reinforced layer web formation step, a carding machine can be used to mechanically open the fibers constituting the reinforced layer (heat-fusible fibers, non-heat-fusible fibers, etc.) to form the reinforced layer web. As the carding machine is well known in the art, its description is omitted.
[0143] In the above laminated web formation step, the first surface layer web, the reinforcing layer web, the core layer web, and the second surface layer web are laminated to form a laminated web.
[0144] In the above water flow entanglement treatment step, the laminated web is subjected to water flow entanglement treatment to form a water flow entangled laminated web. The above water flow entanglement treatment can be carried out according to methods known in the art. The above water flow entanglement treatment may be carried out, for example, with a transport speed of 5 to 20 m / min and a water flow rate of 0.05 to 0.2 m per unit time. 3 This can be carried out under conditions such as flow rate / minute, water flow pressure: 1-20 MPa, nozzle diameter: 80-120 μm, nozzle pitch: 0.5-2 mm, etc.
[0145] In the heat-sealing step described above, the laminated web that has been subjected to the water-entanglement treatment is heated to heat-seal the heat-sealable fibers in the reinforcing layer web and the heat-sealable fibers in the core layer web, thereby forming the laminated nonwoven fabric. The heat-sealing step can be carried out, for example, by placing the laminated web on a support (e.g., a mesh) and applying hot air to the laminated web in a direction intersecting or parallel to the laminated web.
[0146] The above heat-sealing step can be carried out at a temperature of, for example, 120 to 160°C. Preferably, the above temperature is above the higher of the melting point of the heat-sealable fibers in the core layer and the melting point of the heat-sealable fibers in the reinforcing layer. This is from the viewpoint of heat-sealing the heat-sealable fibers in both the core layer and the reinforcing layer. The melting point of the heat-sealable fibers refers to the melting point of the thermoplastic resin constituting the single fiber if the heat-sealable fiber is a single fiber, and the melting point of the relatively low-melting-point thermoplastic resin if the heat-sealable fiber is a composite fiber (including a thermoplastic resin with a relatively high melting point and a thermoplastic resin with a relatively low melting point). For example, if both the core layer and the reinforcing layer are composite fibers (including a thermoplastic resin with a relatively high melting point and a thermoplastic resin with a relatively low melting point), preferably, the above temperature is above the higher of the melting point of the relatively low-melting-point thermoplastic resin constituting the core layer and the melting point of the relatively low-melting-point thermoplastic resin constituting the reinforcing layer. Furthermore, if at least one of the core layer and the reinforcing layer is a composite fiber (including a thermoplastic resin with a relatively high melting point and a thermoplastic resin with a relatively low melting point), the vapor temperature is preferably lower than the melting point of the thermoplastic resin with a relatively high melting point. In the laminated nonwoven fabric described above, if at least one of the first surface layer, the second surface layer, and the reinforcing layer contains synthetic fibers, the above temperature is preferably lower than the melting point of the synthetic fibers.
[0147] The above method for manufacturing the laminated nonwoven fabric may include a drying step between the water entanglement treatment step and the heat fusion step, in which the water entanglement treated laminated web is dried. The drying step can be carried out at a temperature of, for example, 80°C or higher and less than 120°C.
[0148] The present disclosure will be explained below with examples, but the present disclosure is not limited to these examples. [Manufacturing Example 1] Laminated web No. 1 with the following composition was prepared. In laminated web No. 1, the following first surface layer web, the following reinforcing layer web, the following core layer web, and the following second surface layer web were laminated in that order. [First Surface Layer Web] Using a carding machine, first surface layer web No. 1 (basis weight: 7.0 g / m²) containing 30% by mass of rayon fibers as water-retaining fibers (average fiber length: 44 mm, fineness: 1.40 dtex) and 70% by mass of polyethylene terephthalate (PET) fibers as synthetic fibers (single fiber, average fiber length: 38 mm, fineness: 1.45 dtex) was produced. 2 I prepared (this).
[0149] [Reinforcement Layer Web] Using a carding machine, reinforcement layer web No. 1 (basis weight: 7.0 g / m²) containing 60% by mass of composite fibers as heat-fusible fibers (core-sheath fibers with a polypropylene (PP) core and polyethylene (PE) sheath, average fiber length: 51 mm, fineness: 2.20 dtex) and 40% by mass of PET fibers as non-heat-fusible fibers (synthetic fibers) (single fiber, average fiber length: 38 mm, fineness: 1.45 dtex) is produced (basis weight: 7.0 g / m²). 2 I prepared (this).
[0150] [Core Web] Core web No. 1 (basis weight: 17.0 g / m²) is produced using an airlaid apparatus, containing 90% by mass of softwood pulp fibers as pulp fibers and 10% by mass of composite fibers (core-sheath fibers, core: 40% by volume of PP, sheath: 60% by volume of PE, average fiber length: 6 mm, fineness: 1.70 dtex) as heat-fusible fibers. 2 A composite fiber was prepared. In the above composite fiber, the PE in the sheath contained an unsaturated carboxylic acid, an unsaturated carboxylic acid anhydride, or a mixture thereof as a monomer backbone (hereinafter referred to as "acid modified"). [Second surface layer web] Using a carding machine, a second surface layer web No. 1 (basis weight: 14.0 g / m²) containing 30% by mass of rayon fibers as water-retaining fibers (average fiber length: 44 mm, fineness: 1.40 dtex) and 70% by mass of polyethylene terephthalate (PET) fibers as synthetic fibers (single fiber, average fiber length: 38 mm, fineness: 1.45 dtex) was prepared. 2 I prepared (this).
[0151] Laminated nonwoven fabric No. 1 was formed by performing a water jet entanglement step, a drying step, and a heat fusion step on laminated web No. 1 under the conditions described below. In the water jet entanglement step, while conveying laminated web No. 1, water jet treatment was performed from the first surface layer web No. 1 side of laminated web No. 1, and then from the second surface layer web No. 1 side.
[0152] [Water flow entanglement step] - Nozzle pressure on the first surface layer: 3 MPa - Nozzle pressure on the second surface layer: 6 MPa - Nozzle diameter: 92 μm - Nozzle pitch: 0.5 mm - Conveying speed: 5 m / min [Drying step] - Temperature: 100°C - Time: 40 seconds [Heat fusion step] - Temperature: 140°C - Time: 40 seconds
[0153] [Manufacturing Example 2] Using a carding machine, a reinforcing web No. 2 (basis weight: 7 g / m²) was produced containing 60% by mass of composite fibers as heat-fusible fibers (core-sheath fibers with a PP core and a PE sheath, average fiber length: 51 mm, fineness: 2.20 dtex) and 40% by mass of rayon fibers as non-heat-fusible fibers (water-retaining fibers) (average fiber length: 44 mm, fineness: 1.40 dtex). 2 A lamination web No. 2 and lamination nonwoven fabric No. 2 were manufactured in the same manner as in Manufacturing Example 1, except that reinforcement web No. 1 was changed to reinforcement web No. 2.
[0154] [Comparative Manufacturing Example 1] Using an airlaid apparatus, core layer web No. 3 containing 100% by mass of softwood pulp fiber as pulp fiber (basis weight: 17 g / m²) was produced. 2 A laminated web No. 3 and laminated nonwoven fabric No. 3 were manufactured in the same manner as in Manufacturing Example 1, except that core layer web No. 1 was changed to core layer web No. 3. Laminated nonwoven fabric No. 3 is modeled after the wiper described in Patent Document 1.
[0155] [Comparative Manufacturing Examples 2-7] Six commercially available wet wipe packaging products were purchased, and the nonwoven fabric sheets contained within them were dried at 75°C for 180 minutes to produce laminated nonwoven fabrics No. 4-9.
[0156] [Examples 1 and 2, and Comparative Examples 1 to 7] For laminated nonwoven fabrics No. 1 to No. 9, the basis weight, dry thickness, wet thickness, maximum strength in the CD direction, elongation at maximum strength, strength at 5% elongation, strength at 10% elongation, and strength at 50% elongation (dry tensile test and wet tensile test), and maximum strength in the MD direction, elongation at maximum strength, strength at 5% elongation, strength at 10% elongation, and strength at 50% elongation (dry tensile test and wet tensile test) were measured. The results are shown in Tables 1 and 2.
[0157] Regarding wet thickness and wet tensile tests, laminated nonwoven fabrics No. 1 to No. 3 were measured after impregnation with deionized water to a density of 240% by mass, while laminated nonwoven fabrics No. 4 to No. 9 were measured using commercially available wet wipes. The impregnation percentages for laminated nonwoven fabrics No. 4 to No. 9 are shown in Table 2. Also, product: P D5% , P D10% , Product: P D50% , Product: P W5% , Product: P W10% , and product: P W50% The following was calculated. The results are shown in Tables 1 and 2.
[0158]
[0159]
[0160] [Manufacturing Example 3] Laminated nonwoven fabric No. 1 was cut into nonwoven fabric sheet No. 1 with dimensions of 200 x 140 mm (dispensing direction x width direction). Nonwoven fabric sheet No. 1 was cut so that the dispensing direction was the CD direction. As shown in the second embodiment, 60 sheets of nonwoven fabric sheet No. 1 were laminated, the 60 laminates were packaged in a packaging body, and then the packaging body was filled with 265% by mass of the liquid medicine from the 60 laminates to form wet wipe packaging No. 1. [Manufacturing Example 4] Wet wipe packaging No. 2 was formed in the same manner as in Manufacturing Example 3, except that laminated nonwoven fabric No. 1 was changed to laminated nonwoven fabric No. 2.
[0161] [Comparative Manufacturing Example 8] Laminated nonwoven fabric No. 3 was cut into nonwoven fabric sheet No. 3 with dimensions of 200 x 140 mm (dispensing direction x width direction). The nonwoven fabric sheet No. 3 was cut so that the dispensing direction was the CD direction. As shown in the second embodiment, 60 sheets of nonwoven fabric sheet No. 3 were laminated, the 60 laminates were packaged in a packaging body, and then the packaging body was filled with a liquid solution equivalent to 240% by mass of the 60 laminates to form a wet wipe packaging No. 3.
[0162] [Examples 3 and 4, and Comparative Example 8] For each of the wet wipe packaging No. 1 to No. 3, the ability to dispense multiple wipes and the dispensing height were evaluated as defined below. The results are shown in Table 3.
[0163] [Multiple Wipes Dispensing] When one wet wipe is taken out of the packaging at a time, and the nth wet wipe (1, 2, ..., n, ..., 60 from the top) is taken out, the number of wet wipes that are pulled out together with the nth wet wipe (the wet wipe that is taken out directly) (the wet wipes that are taken out indirectly as a whole) is counted.
[0164] For example, when you take out the nth wet wipe, if the (n+1)th wet wipe that is one wipe below it is pulled out along with the nth wet wipe, the wet wipe that was indirectly pulled out as one wipe.
[0165] Furthermore, when the nth wet wipe is removed, if the (n+1)th wet wipe one sheet below it is pulled out together with the nth wet wipe, and the (n+2)th wet wipe two sheets below it is also pulled out together with the (n+1)th wet wipe, then the wet wipes that were indirectly removed in their entirety are counted as two. The experiment continues until all 60 wet wipes have been removed, and the total number of wet wipes that were indirectly removed in their entirety (m) is counted and defined as the multiple-wipe removal rate (sheets). The above multiple-wipe removal rate is determined by conducting a total of three tests with different packaging, and the average value is adopted.
[0166] [Pickup Height] One wet wipe is removed from the packaging at a time. When the nth wet wipe (2, ..., n, ..., 60 from the top) is removed, the length of the wet wipe that is pulled out along with the nth wet wipe (the wet wipe that is pulled out indirectly, in part) (the wet wipe that is pulled out indirectly, in part) is measured (the length from the edge of the wet wipe to the opening). The average value of the total is taken as the pickup height. When measuring the pickup height, cases where the entire wet wipe is pulled out indirectly and cases where the next wet wipe does not come out are ignored. The above pickup height is measured by conducting a total of three tests with different packaging and using the average value.
[0167]
[0168] [Manufacturing Example 5] Laminated nonwoven fabric No. 1 was cut into nonwoven fabric sheet No. 1 with dimensions of 200 x 140 mm (dispensing direction x width direction). The nonwoven fabric sheet No. 1 was cut so that the dispensing direction was the CD direction. As shown in the second embodiment, 30 sheets of nonwoven fabric sheet No. 1 were laminated, the 30 laminates were packaged in a packaging body, and then the packaging body was filled with a liquid solution equivalent to 240% by mass of the 30 laminates to form wet wipe packaging No. 4.
[0169] [Manufacturing Example 6] Core layer web No. 4 and laminated nonwoven fabric No. 10 were formed in the same manner as in Manufacturing Example 1, except that the composite fiber used as a heat-fusible fiber in the core layer web was changed to 10% by mass of composite fiber (core-sheath fiber, core: PP 50% by volume, sheath: PE 50% by volume, average fiber length: 6 mm, fineness: 2.20 dtex). In the above composite fiber, the PE in the sheath portion did not contain unsaturated carboxylic acid, unsaturated carboxylic acid anhydride, or a mixture thereof as a monomer backbone (hereinafter referred to as "without acid modification").
[0170] [Manufacturing Example 7] Wet wipe packaging No. 5 was formed in the same manner as in Manufacturing Example 5, except that laminated nonwoven fabric No. 1 was changed to laminated nonwoven fabric No. 10. [Comparative Manufacturing Example 9] Wet wipe packaging No. 6 was formed in the same manner as in Manufacturing Example 5, except that laminated nonwoven fabric No. 1 was changed to laminated nonwoven fabric No. 3.
[0171] [Examples 5 and 6, and Comparative Example 9] For each of the wet wipe packaging No. 4 to No. 6, the ability to dispense multiple wipes and the dispensing height as defined in this example (however, the number of wet wipes was changed from "60" to "30") were evaluated. The results are shown in Table 4.
[0172]
[0173] 1 Laminated nonwoven fabric 3 First surface layer 5 Reinforcement layer 7 Core layer 9 Second surface layer 101 Wet wipe packaging 103 Packaging body 105 Opening 107 Sealing material 109 Wet wipes
Claims
1. A laminated nonwoven fabric comprising a first surface layer, a second surface layer, and a core layer and a reinforcing layer disposed between the first surface layer and the second surface layer, wherein each of the first surface layer and the second surface layer contains water-retaining fibers, the core layer contains pulp fibers and heat-fusible fibers, and the reinforcing layer contains heat-fusible fibers and non-heat-fusible fibers.
2. The laminated nonwoven fabric according to claim 1, wherein each of the heat-fusible fibers in the core layer and the heat-fusible fibers in the reinforcing layer are composite fibers.
3. The laminated nonwoven fabric according to claim 2, wherein the composite fiber in the core layer is a core-sheath fiber comprising a core portion and a sheath portion, and the sheath portion is composed of a polymer containing an unsaturated carboxylic acid, an unsaturated carboxylic acid anhydride, or a mixture thereof as a monomer backbone.
4. The laminated nonwoven fabric according to any one of claims 1 to 3, wherein in the core layer, the heat-fusible fibers and the pulp fibers are bonded together by heat fusion of the heat-fusible fibers.
5. The laminated nonwoven fabric according to any one of claims 1 to 4, wherein the heat-fusible fibers in the core layer and at least one of the water-retaining fibers in the first surface layer and the water-retaining fibers in the second surface layer are bonded together by heat fusion of the heat-fusible fibers in the core layer.
6. The laminated nonwoven fabric according to any one of claims 1 to 5, wherein the heat-fusible fibers in the core layer and the heat-fusible fibers in the reinforcing layer are heat-fussed together.
7. In the laminated nonwoven fabric, in a wet tensile test, the product of the elongation at maximum strength (%) and the strength at 5% elongation (N / 25 mm) in the orthogonal direction perpendicular to the conveying direction during manufacturing is P W5% The basis weight is 50 g / m². 2 A laminated nonwoven fabric according to any one of claims 1 to 6, wherein the converted value is in the range of 25 to 100.
8. In the laminated nonwoven fabric, in a wet tensile test, the product of the elongation at maximum strength (%) and the strength at 50% elongation (N / 25mm) in the orthogonal direction perpendicular to the conveying direction during manufacturing is P. W50% The basis weight is 50 g / m². 2 A laminated nonwoven fabric according to any one of claims 1 to 7, wherein the converted value is in the range of 130 to 300.
9. The laminated nonwoven fabric according to any one of claims 1 to 8, wherein the heat-fusible fibers in the core layer have an average fiber length of less than 20 mm, and the heat-fusible fibers in the reinforcing layer have an average fiber length of 20 mm or more.
10. The laminated nonwoven fabric according to any one of claims 1 to 9, wherein the water-retaining fibers have an average fiber length of 20 mm or more.
11. The laminated nonwoven fabric according to any one of claims 1 to 10, wherein each of the first surface layer and the second surface layer contains synthetic fibers.
12. The laminated nonwoven fabric according to claim 11, wherein the synthetic fibers have an average fiber length of 20 mm or more.
13. The laminated nonwoven fabric according to any one of claims 1 to 12, wherein in the core layer, the average fiber length of the heat-fusible fibers is greater than the average fiber length of the pulp fibers.
14. The laminated nonwoven fabric according to any one of claims 1 to 13, wherein the non-heat-fusible fibers in the reinforcing layer are water-retaining fibers or synthetic fibers.
15. The laminated nonwoven fabric according to any one of claims 1 to 14, wherein the laminated nonwoven fabric is a spunlace nonwoven fabric.
16. Wet wipes comprising a nonwoven fabric sheet and a chemical solution, wherein the nonwoven fabric sheet is composed of a laminated nonwoven fabric as described in any one of claims 1 to 15.
17. The wet wipes according to claim 16, wherein the liquid contains a fragrance, and the fragrance has a vapor pressure of 10.00 to 1333 Pa at 25°C.
18. A wet wipes package comprising a plurality of wet wipes and a packaging body for storing the plurality of wet wipes, wherein each of the plurality of wet wipes is a wet wipe according to claim 16 or 17, and the packaging body is a packaging sheet type, pop-up type, or bottle type packaging container.
19. The packaging body is a packaging sheet type or pop-up type packaging container, the packaging container has a top with an opening and a bottom, and the plurality of wet wipes are stacked inside the packaging container in the direction from the bottom to the top, as described in claim 18.
20. A method for manufacturing a laminated nonwoven fabric comprising a first surface layer, a second surface layer, and a core layer and a reinforcing layer disposed between the first surface layer and the second surface layer, comprising: a first surface layer web forming step of forming a first surface layer web constituting the first surface layer, which includes water-retaining fibers, by a carding method; a core layer web forming step of forming a core layer web constituting the core layer, which includes pulp fibers and heat-fusible fibers having an average fiber length of less than 20 mm, by an airlaid method; a reinforcing layer web forming step of forming a reinforcing layer web constituting the reinforcing layer, which includes heat-fusible fibers having an average fiber length of 20 mm or more and non-heat-fusible fibers having an average fiber length of 20 mm or more, by a carding method; a second surface layer web forming step of forming a second surface layer web constituting the second surface layer, which includes water-retaining fibers, by a carding method; and a laminated web forming step of laminating the first surface layer web, the reinforcing layer web, the core layer web and the second surface layer web to form a laminated web. A method for manufacturing a laminated nonwoven fabric, comprising: a water flow entanglement step of subjecting the laminated web to a water flow entanglement treatment to form a water flow entangled laminated web; and a heat fusion step of heating the water flow entangled laminated web to heat fuse the heat-fusible fibers in the reinforcing layer web and the heat-fusible fibers in the core layer web to form the laminated nonwoven fabric.