Fiber and method for producing same
A styrene-based thermoplastic elastomer fiber addresses recycling and environmental concerns of polyurethane fibers by improving compatibility with polyolefin resins and reducing harmful gas emissions, offering equivalent or superior properties to polyurethane fibers.
Patent Information
- Application Number
- PCT/JP2026/017567
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-12
AI Technical Summary
Polyurethane elastic fibers face challenges in recycling due to poor compatibility with polyolefin resins, leading to decreased physical properties and appearance of recycled materials, and incineration produces harmful gases like nitrogen oxides and hydrogen cyanide.
A novel elastic fiber is developed using a styrene-based thermoplastic elastomer, composed of a block copolymer with specific shear viscosity and molecular weight ratios, enabling melt-spinning and improved compatibility with polyolefin resins, reducing the risk of harmful gas generation during combustion.
The styrene-based thermoplastic elastomer fibers exhibit properties comparable to or better than conventional polyurethane fibers, with enhanced melt-spinnability, stability, and reduced environmental impact during recycling and incineration.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Fibers and methods for manufacturing the same
[0001] The present invention relates to fibers, methods for producing the same, multifilaments containing the fibers, nonwoven fabrics containing the fibers, and gathered members containing the fibers.
[0002] In recent years, polyurethane elastic fibers have been widely used as elastic fibers. On the other hand, various thermoplastic elastomers, such as styrene-based thermoplastic elastomers, are also known as elastic materials. For example, Patent Document 1 discloses a thermoplastic polymer composition with excellent elasticity, comprising (a) 100 parts by mass of an α-methylstyrene-based block copolymer and / or its hydrogenated product having a number average molecular weight in the range of 30,000 to 500,000, and a polymer block A mainly consisting of α-methylstyrene units and a polymer block B mainly consisting of conjugated diene units, and (b) 200 parts by mass or less of a non-aromatic rubber softener. Patent Document 2 discloses an elastic material comprising a polymer composition containing (a) a polymer block A mainly composed of α-methylstyrene and a polymer block B which may be hydrogenated, having a weight average molecular weight of 30,000 to 200,000, (b) an acrylic resin, and (c) a softener, in a specific blending ratio (mass ratio).
[0003] Japanese Patent Publication No. 2005-232246 Japanese Patent Publication No. 2004-196941
[0004] While polyurethane elastic fibers possess good elasticity, there is room for improvement in terms of recycling. For example, polyurethane elastic fibers are used as elastic materials for waist gathers and leak-proof gathers in disposable diapers, and in recent years, recycling of used diapers has been considered from a recycling perspective. However, polyurethane elastic fibers have the disadvantage of poor compatibility with polyolefin resins, such as polypropylene nonwoven fabric, which is the main material of disposable diapers. Therefore, it is known that mixing them with these materials for recycling can lead to a decrease in the physical properties and appearance of the resulting recycled resin, which is considered a challenge when recycling them together with polyolefin materials. Furthermore, when polyurethane elastic yarn is incinerated, there are concerns about the generation of harmful gases such as nitrogen oxides and hydrogen cyanide due to the nitrogen atoms in the polyurethane. For these reasons, there is a need for alternative materials to polyurethane elastic yarn. On the other hand, styrene-based thermoplastic elastomers have better compatibility with polyolefin resins than polyurethane, and furthermore, because they do not contain nitrogen atoms in their polymer backbone, the risk of generating nitrogen oxides during combustion can be reduced. Therefore, they have the potential to solve the aforementioned problems. However, conventionally, styrene-based thermoplastic elastomers have been difficult to melt-spin on their own, and there has been room for improvement in their melt-spinning properties.
[0005] Therefore, the present invention aims to provide a novel elastic fiber using a styrene-based thermoplastic elastomer.
[0006] As a result of diligent research, the inventors have found that the above problems can be solved by creating a fiber that satisfies specific requirements. That is, the present invention encompasses the following inventions: [1] At least a part or all of the fiber is formed from a resin comprising a block copolymer (X) comprising a polymer block (A) containing α-methylstyrene units and a polymer block (B) containing conjugated diene compound units, wherein the shear rate of the resin at 270°C is 1,500 s. -1A fiber having a shear viscosity of 250 Pa·s or less. [2] The fiber according to [1], wherein the block copolymer (X) comprises at least one selected from the group consisting of triblock copolymer (I) and diblock copolymer (II), the triblock copolymer (I) comprises a polymer block (A1) containing α-methylstyrene units and a polymer block (B1) containing conjugated diene compound units, the polymer block (A1) and the polymer block (B1) are a triblock copolymer represented as A1-B1-A1, the structures of the two polymer blocks (A1) in the triblock copolymer (I) may be the same or different from each other, and the diblock copolymer (II) comprises a polymer block (A2) containing α-methylstyrene units and a polymer block (B2) containing conjugated diene compound units, the polymer block (A2) and the polymer block (B2) are a diblock copolymer represented as A2-B2. [3] The fiber according to [2], wherein the block copolymer (X) contains the triblock copolymer (I) and the diblock copolymer (II) in a mass ratio of triblock copolymer (I):diblock copolymer (II) = 92:8 to 75:25. [4] The fiber according to [2] or [3], wherein the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 10,000 to 2,000,000, and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 5,000 to 100,000. [5] The fiber according to any one of [1] to [4], wherein the block copolymer (X) contains the polymer block (A) and the polymer block (B) in a mass ratio of polymer block (A):polymer block (B) = 5:95 to 55:45. [6] The fiber according to any one of [1] to [5], wherein the hydrogenation rate of the block copolymer (X) is 50 to 100 mol%. [7] The fiber according to any one of [1] to [6], wherein the order-to-disorder transition temperature (ODT) determined by dynamic viscoelasticity measurement of the resin is 300°C or less.[8] The fiber according to any one of [1] to [7], wherein the fiber is a core-sheath type composite fiber, and the resin is included in at least one selected from the core and the sheath. [9] A method for producing the fiber according to any one of [1] to [8], wherein the fiber is formed by melt spinning.
[10] A multifilament comprising the fiber according to any one of [1] to [8].
[11] The multifilament according to
[10] , wherein the fineness is 90 to 2,000 dtex.
[12] The multifilament according to
[10] or
[11] , wherein the 2nd hysteresis loss, determined by a tensile stretch cycle test performed in the elongation range of 0 to 200% of the multifilament, is 50% or less.
[13] A nonwoven fabric comprising the fiber according to any one of [1] to [8].
[14] A gathered member comprising the fiber according to any one of [1] to [8].
[0007] According to the present invention, a novel elastic fiber using a styrene-based thermoplastic elastomer can be provided.
[0008] This is an explanatory diagram of the measurement method for the order-to-disorder transition temperature (ODT). This is an explanatory diagram of the cycle test.
[0009] The following description is based on examples of embodiments of the present invention (hereinafter also referred to as "one aspect of the present invention"). However, the embodiments shown below are illustrative examples for realizing the technical concept of the present invention, and the present invention is not limited to the following description. Embodiments in which any of the matters described herein are arbitrarily selected or arbitrarily combined are also included in the present invention. In this specification, preferred forms of embodiments are shown, but combinations of two or more individual preferred forms are also preferred forms. Preferred provisions can be arbitrarily selected, and for example, combinations of preferred provisions can be said to be more preferred. In this specification, unless otherwise specified, the description of a numerical range as "XX to YY" means "XX or more and YY or less" (XX represents the lower limit and YY represents the upper limit). For example, when the numerical range is simply described as "10 to 90", it represents a range of 10 or more and 90 or less. In this specification, the lower and upper limits described in stages for numerical ranges (each characteristic value, each component content, each structural unit content, each manufacturing condition, and the values calculated from them, each characteristic, and each condition, etc.) can be combined independently. For example, based on the description "preferably 10 to 90, more preferably 30 to 60" for the same item, it is possible to combine the "preferred lower limit (10)" and the "more preferred upper limit (60)" to arrive at "10 to 60". Regarding the numerical range, for example, based on the description "preferably 10 to 90, more preferably 30 to 60", it is possible to specify only the lower limit as "10 or more" or "30 or more" without specifically specifying the upper limit, and similarly, it is possible to specify only the upper limit as "90 or less" or "60 or less" without specifically specifying the lower limit. The same applies when the upper limit of the numerical range is "less than", and when the lower limit is "greater than". Similarly, for example, based on the descriptions "preferably 10 or more, more preferably 30 or more" and "preferably 90 or less, more preferably 60 or less" for the same item, it is possible to combine the "preferred lower limit (10)" and the "more preferred upper limit (60)" to arrive at "10 or more and 60 or less". Furthermore, as described above, the lower limit can be specified as "10 or more" or "30 or more," and similarly, the upper limit can be specified as "90 or less" or "60 or less."The same applies when the terms "greater than or equal to" and "less than or equal to" in the above explanation are replaced with "greater than" and "less than," respectively. That is, for example, based on the statement "preferably more than 10 and less than 90, more preferably 30 or more and 60 or less," the upper and lower limits can be combined to become "more than 10 and 60 or less" and "30 or more and less than 90."
[0010] In this specification, unless otherwise specified, the following terms have the meanings described below. In this specification, unless otherwise specified, the terms "tensile properties," "stretch properties," "stress retention," "heat resistance," and "laminating properties" refer to the properties of fibers and multifilaments that are embodiments of the present invention. These properties are specifically measured and evaluated by the methods described in the examples. In this specification, unless otherwise specified, the term "melt spinnability" refers to the properties of the material forming the fiber. In this specification, "α-methylstyrene unit" means a structural unit derived from α-methylstyrene, which is the monomer before polymerization. And "conjugated diene compound unit" means a structural unit derived from a conjugated diene compound, which is the monomer before polymerization. In this specification, hydrogenation may be referred to as "hydrogenation," hydrogenated products as "hydrogenated products," and the hydrogenation rate as "hydrogenation rate." In this specification, "100% by mass of the total amount of block copolymer (X)" means that the total amount of structural units derived from polymerizable monomers such as polymer block (A) and polymer block (B), described later, is 100% by mass. The "polymerizable monomer" refers to a compound that can initiate a polymerization reaction and form a polymer through the action of a polymerization initiator or the like. For example, compounds such as polymerization initiators, polymerization inhibitors, and coupling agents may also constitute part of the molecular structure of block copolymer (X), but these components are not included in the "polymerizable monomer" because they do not repeatedly "polymerize" themselves to form a polymer skeleton. Similarly, in this specification, "100% by mass of the total of the triblock copolymer (I) and the diblock copolymer (II)" means that the total amount of structural units derived from polymerizable monomers in each copolymer is 100% by mass.
[0011] [Fiber] A fiber according to one aspect of the present invention (hereinafter also referred to as "the fiber") is formed from a resin comprising a block copolymer (X) in which at least a part or all of the fiber comprises a polymer block (A) containing α-methylstyrene units and a polymer block (B) containing conjugated diene compound units, wherein the shear rate of the resin at 270°C is 1,500 s. -1 The shear viscosity is 250 Pa·s or less. By satisfying the above-described embodiment, it becomes possible to provide a novel elastic fiber using a styrene-based thermoplastic elastomer. Furthermore, it is expected that the fiber will exhibit properties equivalent to or better than those of conventional polyurethane elastic fibers. The fiber according to one embodiment of the present invention will be described in detail below.
[0012] <Resin> The resin forming at least part or all of the fibers comprises a block copolymer (X) comprising a polymer block (A) containing α-methylstyrene units and a polymer block (B) containing conjugated diene compound units.
[0013] The shear rate of the aforementioned resin at 270°C is 1,500 s. -1The shear viscosity is 250 Pa·s or less. The resin satisfies the above shear viscosity and has excellent melt spinnability, making it possible to stably obtain novel elastic fibers using styrene-based thermoplastic elastomers. From this viewpoint, the shear viscosity of the resin is preferably 225 Pa·s or less, more preferably 200 Pa·s or less, even more preferably 175 Pa·s or less, even more preferably 150 Pa·s or less, and even more preferably 125 Pa·s or less. The lower limit of the shear viscosity of the resin is not particularly limited as long as fibers can be formed, but from the viewpoint of improving melt spinnability, the shear viscosity of the resin is preferably 30 Pa·s or more, and may be, for example, 50 Pa·s or more. As described above, these lower and upper limits described in stages can be combined independently. For example, in one embodiment of the fiber, the shear viscosity of the resin is preferably 30 to 250 Pa·s, more preferably 30 to 225 Pa·s, even more preferably 30 to 200 Pa·s, even more preferably 30 to 175 Pa·s, even more preferably 30 to 150 Pa·s, and even more preferably 30 to 125 Pa·s. In one embodiment of the fiber, the shear viscosity of the resin may be, for example, 50 to 250 Pa·s, 50 to 225 Pa·s, 50 to 200 Pa·s, 50 to 175 Pa·s, 50 to 150 Pa·s, or 50 to 125 Pa·s. The shear viscosity of the resin can be measured in accordance with ISO 11443:2005, and specifically can be measured by the method described in the examples.
[0014] From the viewpoint of improving melt spinnability, the order-to-disorder transition temperature (ODT) (hereinafter simply referred to as "ODT") of the resin, as determined by dynamic viscoelasticity measurement, is preferably 300°C or lower, more preferably 295°C or lower, even more preferably 290°C or lower, even more preferably 285°C or lower, and even more preferably 280°C or lower. On the other hand, there is no particular limit to the lower limit of the ODT of the resin, but for example, the ODT of the resin may be 0°C or higher, 50°C or higher, 100°C or higher, 150°C or higher, 200°C or higher, or 250°C or higher. As described above, these stepwise lower and upper limits can be combined independently. For example, as one embodiment of the fiber, the ODT of the resin is 0-300°C, 0-295°C, 0-290°C, 0-285°C, 0-280°C, 50-300°C, 50-295°C, 50-290°C, 50-285°C, 50-280°C, 100-300°C, 100-295°C, 100-290°C, 100-285°C, 100-280°C The temperature may be 150-300°C, 150-295°C, 150-290°C, 150-285°C, 150-280°C, 200-300°C, 200-295°C, 200-290°C, 200-285°C, 200-280°C, 250-300°C, 250-295°C, 250-290°C, 250-285°C, or 250-280°C. The ODT of the resin is measured in accordance with JIS K7244-10:2005, and can be measured specifically by the method described in the examples.
[0015] (Block copolymer (X)) The block copolymer (X) contained in the resin is a styrene-based thermoplastic elastomer and comprises a polymer block (A) containing α-methylstyrene units and a polymer block (B) containing conjugated diene compound units. From the viewpoint of increasing the heat resistance of the resulting fibers, the content of α-methylstyrene units in 100% by mass of polymer block (A) is preferably 50 to 100% by mass, more preferably 70 to 100% by mass, even more preferably 80 to 100% by mass, even more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and may also be 100% by mass.
[0016] The polymer block (A) may contain monomer units other than α-methylstyrene units, as long as it can solve the problems of the present invention. The monomers other than α-methylstyrene units are not limited as long as they are monomers that can be anionically polymerized, but for example, vinyl aromatic compounds such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 1,3-dimethylstyrene, and diphenylethylene; and conjugated diene compounds such as butadiene, isoprene, and 2,3-dimethyl-1,3-butadiene are preferred. It is more preferable that the monomers other than α-methylstyrene units are at least one selected from the group consisting of styrene, p-methylstyrene, butadiene, and isoprene. The form of the polymer block (A) when it contains monomers other than α-methylstyrene units is not particularly limited and may be random or tapered. When the block copolymer (X) contains a plurality of polymer blocks (A), the structures of the plurality of polymer blocks (A) may be the same or different.
[0017] The weight-average molecular weight (Mw) of the polymer block (A) in terms of polystyrene is preferably 500 to 300,000, more preferably 1,000 to 100,000, even more preferably 2,000 to 50,000, and even more preferably 3,000 to 20,000. When the block copolymer (X) contains a plurality of polymer blocks (A), the weight-average molecular weight (Mw) of the polymer block (A) in terms of polystyrene refers to the sum of the weight-average molecular weights (Mw) of each polymer block (A) contained in the block copolymer (X). The weight-average molecular weight (Mw) can be measured by GPC (gel permeation chromatography).
[0018] The polymer block (B) contains conjugated diene compound units. Examples of the conjugated diene compound each independently include butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, β-farnesene, and the like. One of these conjugated diene compounds may be used alone, or two or more thereof may be used. Among these conjugated diene compounds, at least one selected from the group consisting of butadiene and isoprene is preferred, and butadiene is more preferred. In one aspect of the fiber, the conjugated diene compound unit of the polymer block (B) is preferably a structural unit derived from butadiene. It is preferable that the conjugated diene compound unit is a structural unit derived from butadiene, because the stretchability tends to be easily improved.
[0019] From the viewpoint of easily obtaining favorable stretchability, the content of the conjugated diene compound unit in 100% by mass of the polymer block (B) is preferably 50 to 100% by mass, more preferably 70 to 100% by mass, still more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and may be 100% by mass.
[0020] Furthermore, the polymer block (B) may contain other anionic polymerizable monomers besides the conjugated diene compound units, as long as the object of the present invention can be solved. However, the other anionic polymerizable monomers besides the conjugated diene compound units do not include α-methylstyrene. The form in which the polymer block (B) contains other anionic polymerizable monomers besides the conjugated diene compound units is not particularly limited, and may be random or tapered. When the block copolymer (X) contains a plurality of the polymer blocks (B), the structures of the plurality of existing polymer blocks (B) may each be the same, or may each be different.
[0021] The weight-average molecular weight (Mw) of the polymer block (B) in terms of polystyrene is preferably 10,000 to 400,000, more preferably 15,000 to 200,000, even more preferably 15,000 to 150,000, and even more preferably 15,000 to 100,000. When the block copolymer (X) contains a plurality of polymer blocks (B), the weight-average molecular weight (Mw) of the polymer block (B) in terms of polystyrene refers to the sum of the weight-average molecular weights (Mw) of each polymer block (B) contained in the block copolymer (X). The weight-average molecular weight (Mw) can be measured by GPC (gel permeation chromatography).
[0022] The amount of vinyl bonding in the polymer block (B) is preferably 10 to 95 mol%, more preferably 15 to 80 mol%, even more preferably 20 to 70 mol%, even more preferably 35 to 60 mol%, and even more preferably 40 to 50 mol%. The amount of vinyl bonding in the polymer block (B) refers to the total mol% of structural units derived from the conjugated diene compound that are bonded by 1,2-bonds, 3,4-bonds (when the conjugated diene compound is not farnesene), and 3,13-bonds (when the conjugated diene compound is not farnesene) (i.e., structural units derived from the conjugated diene compound that are bonded by means other than 1,4-bonds (when the conjugated diene compound is not farnesene) and 1,13-bonds (when the conjugated diene compound is not farnesene)) relative to 100 mol% of the total structural units constituting the conjugated diene compound units in the polymer block (B). In other words, when the conjugated diene compound is anything other than farnesene, the amount of vinyl bonding in the polymer block (B) means the total mole percent of structural units derived from the conjugated diene compound that are bonded by 1,2- and 3,4-bonds, relative to 100 mol% of the total structural units constituting the conjugated diene compound unit in the polymer block (B). Furthermore, when the conjugated diene compound is anything other than farnesene, the amount of vinyl bonding in the polymer block (B) means the total mole percent of structural units derived from the conjugated diene compound that are bonded by means other than 1,4-bonds, relative to 100 mol% of the total structural units constituting the conjugated diene compound unit in the polymer block (B). On the other hand, when the conjugated diene compound is farnesene, the amount of vinyl bonding in the polymer block (B) means the total mole percent of structural units derived from farnesene that are bonded by 3,13-bonds, relative to 100 mol% of the total structural units constituting the conjugated diene compound unit in the polymer block (B). Furthermore, when the conjugated diene compound is farnesene, the amount of vinyl bonds in the polymer block (B) refers to the total mole percent of structural units derived from farnesene that are bonded by means other than 1,13-bonds, relative to 100 mole percent of the total structural units constituting the conjugated diene compound unit in the polymer block (B). The amount of vinyl bonds is 1 It can be calculated using 1H-NMR spectroscopy, and specifically, it can be calculated by the method described in the examples.
[0023] The block copolymer (X) preferably contains polymer block (A) and polymer block (B) in a mass ratio of polymer block (A):polymer block (B) = 5:95 to 55:45. The block copolymer (X) is preferable in that it contains polymer block (A) and polymer block (B) in the above ratio because it tends to have good melt spinnability and good tensile properties, stretch properties, heat resistance and stress retention of the resulting fibers. From a similar viewpoint, the content ratio of polymer block (A) and polymer block (B) in the block copolymer (X) is more preferably 10:90 to 45:55, even more preferably 15:85 to 35:65, even more preferably 20:80 to 35:65, even more preferably 22:78 to 33:67, and even more preferably 24:76 to 31:69 in mass ratio [polymer block (A):polymer block (B)]. In other words, the content of polymer block (A) in 100% by mass of the total of polymer block (A) and polymer block (B) is preferably 5 to 55% by mass, more preferably 10 to 45% by mass, even more preferably 15 to 35% by mass, even more preferably 20 to 35% by mass, even more preferably 22 to 33% by mass, and even more preferably 24 to 31% by mass. The content of polymer block (B) in 100% by mass of the total of polymer block (A) and polymer block (B) is preferably 45 to 95% by mass, more preferably 55 to 90% by mass, even more preferably 65 to 85% by mass, even more preferably 65 to 80% by mass, even more preferably 67 to 78% by mass, and even more preferably 69 to 76% by mass. Here, if the block copolymer (X) contains a plurality of polymer blocks (A), the total amount of all polymer blocks (A) contained in the block copolymer (X) is used to calculate the content ratio of polymer block (A). Similarly, if the block copolymer (X) contains multiple polymer blocks (B), the total amount of all polymer blocks (B) contained in the block copolymer (X) is used to calculate the content ratio of the polymer blocks (B). The mass ratio of the polymer blocks (A) and the polymer blocks (B) is as follows: 1It can be calculated using 1H-NMR spectrum measurement. Specifically, it can be measured and calculated by the methods described in the Examples. The content of the polymer block (A) in a total of 100 mass% of the polymer block (A) and the polymer block (B), for example, when a plurality of block copolymers are included such that the block copolymer (X) is a mixture containing both a triblock copolymer (I) and a diblock copolymer (II) as described later, can be calculated as the total content of the polymer blocks corresponding to the polymer block (A) in each copolymer contained in the block copolymer (X). The same applies to the content of the polymer block (B) in a total of 100 mass% of the polymer block (A) and the polymer block (B). Specifically, it can be measured and calculated by the methods described in the Examples.
[0024] From the viewpoint of easily achieving good melt spinnability, as well as favorable stretch properties and heat resistance of the resulting fiber, the total content of the polymer block (A) and the polymer block (B) in 100 mass% of the total amount of the block copolymer (X) is preferably 80 to 100 mass%, more preferably 90 to 100 mass%, still more preferably 95 to 100 mass%, even more preferably 98 to 100 mass%, and may be 100 mass%.
[0025] The hydrogenation rate of the block copolymer (X) is preferably 50 to 100 mol%. When the hydrogenation rate of the block copolymer (X) is 50 to 100 mol%, it is preferable from the viewpoint of easily achieving good melt spinnability and heat resistance. It is also preferable from the viewpoint of easily improving weather resistance. From the same viewpoint, the hydrogenation rate of the block copolymer (X) is more preferably 70 to 100 mol%, still more preferably 90 to 100 mol%, even more preferably 90 to 99.9 mol%, even more preferably 95 to 99.7 mol%, even more preferably 97 to 99.5 mol%. The hydrogenation rate of the block copolymer (X) is, 1 It can be calculated using 1H-NMR spectrum measurement. Specifically, it can be measured and calculated by the methods described in the Examples.
[0026] The amount of vinyl bonding in the block copolymer (X) is preferably 10 to 95 mol%, more preferably 15 to 80 mol%, even more preferably 20 to 70 mol%, even more preferably 35 to 60 mol%, and even more preferably 40 to 50 mol%. The amount of vinyl bonding in the block copolymer (X) refers to the total mol% of structural units derived from the conjugated diene compound that are bonded by 1,2-bonds, 3,4-bonds (when the conjugated diene compound is not farnesene), and 3,13-bonds (when the conjugated diene compound is not farnesene) (i.e., structural units derived from the conjugated diene compound that are bonded by means other than 1,4-bonds (when the conjugated diene compound is not farnesene) and 1,13-bonds (when the conjugated diene compound is not farnesene)) relative to 100 mol% of the total structural units constituting the conjugated diene compound units in the block copolymer (X). In other words, when the conjugated diene compound is anything other than farnesene, the amount of vinyl bonding in the block copolymer (X) represents the total mole percent of structural units derived from the conjugated diene compound that are bonded by 1,2- and 3,4-bonds, relative to 100 mol% of the total structural units constituting the conjugated diene compound units in the block copolymer (X). Furthermore, when the conjugated diene compound is anything other than farnesene, the amount of vinyl bonding in the block copolymer (X) represents the total mole percent of structural units derived from the conjugated diene compound that are bonded by means other than 1,4-bonds, relative to 100 mol% of the total structural units constituting the conjugated diene compound units in the block copolymer (X). On the other hand, when the conjugated diene compound is farnesene, the amount of vinyl bonding in the block copolymer (X) represents the total mole percent of structural units derived from farnesene that are bonded by 3,13-bonds, relative to 100 mol% of the total structural units constituting the conjugated diene compound units in the block copolymer (X). Furthermore, when the conjugated diene compound is farnesene, the amount of vinyl bonds in the block copolymer (X) refers to the total mole percent of structural units derived from farnesene that are bonded by means other than 1,13-bonds, relative to 100 mole percent of the total structural units constituting the conjugated diene compound units in the block copolymer (X). The amount of vinyl bonds is 1It can be calculated using 1H-NMR spectroscopy. Specifically, it can be measured and calculated by the method described in the examples.
[0027] In one embodiment of the fiber, the block copolymer (X) preferably comprises at least one selected from the group consisting of triblock copolymer (I) and diblock copolymer (II), wherein the triblock copolymer (I) comprises a polymer block (A1) containing α-methylstyrene units and a polymer block (B1) containing conjugated diene compound units, and the polymer block (A1) and the polymer block (B1) are a triblock copolymer represented as A1-B1-A1, and the structures of the two polymer blocks (A1) in the triblock copolymer (I) may be the same or different from each other, and the diblock copolymer (II) preferably comprises a polymer block (A2) containing α-methylstyrene units and a polymer block (B2) containing conjugated diene compound units, and the polymer block (A2) and the polymer block (B2) are a diblock copolymer represented as A2-B2.
[0028] [Triblock Copolymer (I) and Diblock Copolymer (II)] As described above, the triblock copolymer (I) comprises a polymer block (A1) containing α-methylstyrene units and a polymer block (B1) containing conjugated diene compound units, wherein the polymer block (A1) and the polymer block (B1) are a triblock copolymer represented as A1-B1-A1. However, the structures of the two polymer blocks (A1) may be identical or different. As described above, the diblock copolymer (II) comprises a polymer block (A2) containing α-methylstyrene units and a polymer block (B2) containing conjugated diene compound units, wherein the polymer block (A2) and the polymer block (B2) are a diblock copolymer represented as A2-B2.
[0029] The block copolymer (X) preferably contains the triblock copolymer (I) and the diblock copolymer (II) in a mass ratio of triblock copolymer (I):diblock copolymer (II) = 92:8 to 75:25. This is preferable because the mass ratio of the triblock copolymer (I) to the diblock copolymer (II) being within this range tends to result in good melt spinnability, stretchability, and heat resistance of the resulting fibers. From a similar viewpoint, the content ratio (mass ratio) of the triblock copolymer (I) to the diblock copolymer (II) in the block copolymer (X) is more preferably triblock copolymer (I):diblock copolymer (II) = 92:8 to 80:20, and even more preferably triblock copolymer (I):diblock copolymer (II) = 92:8 to 85:15. The content ratio (mass ratio) of the triblock copolymer (I) and the diblock copolymer (II) in the block copolymer (X) can be calculated, for example, from the area ratio of the differential refractive index (RI) in GPC (gel permeation chromatography) measurement, specifically from the ratio of the peak areas corresponding to each copolymer that appear on the GPC chromatogram obtained by measuring with RI as the detector.
[0030] {Polymer block (A1) and polymer block (A2)} The polymer block (A1) and the polymer block (A2) each independently contain α-methylstyrene units. From the viewpoint of increasing the heat resistance of the resulting fibers, the amount of α-methylstyrene units in 100% by mass of polymer block (A1) and the amount of α-methylstyrene units in 100% by mass of polymer block (A2) are preferably 50 to 100% by mass, more preferably 70 to 100% by mass, even more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and may also be 100% by mass. The content of α-methylstyrene units in the total 100% by mass of polymer block (A1) and polymer block (A2) is preferably 50 to 100% by mass, more preferably 70 to 100% by mass, even more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and may also be 100% by mass.
[0031] The polymer block (A1) and the polymer block (A2) may each independently contain monomer units other than α-methylstyrene units, as long as they can solve the problems of the present invention. The monomers other than α-methylstyrene units are not limited as long as they are generally anionically polymerizable monomers, but for example, vinyl aromatic compounds such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 1,3-dimethylstyrene, and diphenylethylene; and conjugated diene compounds such as butadiene, isoprene, and 2,3-dimethyl-1,3-butadiene are preferred. It is more preferable that the monomers other than α-methylstyrene units are at least one selected from the group consisting of styrene, p-methylstyrene, butadiene, and isoprene. The form of the polymer block (A1) and the polymer block (A2) when they contain monomers other than α-methylstyrene units is not particularly limited and may be random or tapered.
[0032] The weight-average molecular weight (Mw) of polymer block (A1) and polymer block (A2) in terms of polystyrene is preferably 500 to 300,000, more preferably 1,000 to 100,000, even more preferably 2,000 to 50,000, and even more preferably 3,000 to 10,000, respectively. The weight-average molecular weight (Mw) can be measured by GPC (gel permeation chromatography), specifically by the method described in the examples.
[0033] The two polymer blocks (A1) constituting the triblock copolymer (I) may be identical in form to each other, or they may be different in form. Each polymer block (A1) constituting the triblock copolymer (I) and the polymer block (A2) constituting the diblock copolymer (II) may be identical in form to each other, or they may be different in form to each other.
[0034] {Polymer block (B1) and polymer block (B2)} The polymer block (B1) and the polymer block (B2) each independently contain a conjugated diene compound unit. Examples of the conjugated diene compound include butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, and β-farnesene. These conjugated diene compounds may be used individually or in combination of two or more. Among the conjugated diene compounds, at least one selected from the group consisting of butadiene and isoprene is preferred, and butadiene is more preferred. In one embodiment of the fiber, it is preferable that at least one conjugated diene compound unit selected from the group consisting of the conjugated diene compound unit of polymer block (B1) and the conjugated diene compound unit of polymer block (B2) is a structural unit derived from butadiene. It is preferable that the conjugated diene compound unit is a structural unit derived from butadiene because it is easier to improve the stretchability. Both the conjugated diene compound units of the polymer block (B1) and the conjugated diene compound units of the polymer block (B2) may be structural units derived from butadiene.
[0035] The polymer block (B1) and the polymer block (B2) each independently contain conjugated diene compound units. From the viewpoint of easily achieving good stretchability, the content of conjugated diene compound units in 100% by mass of the polymer block (B1) and the content of conjugated diene compound units in 100% by mass of the polymer block (B2) are each preferably 50 to 100% by mass, more preferably 70 to 100% by mass, even more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and may also be 100% by mass.
[0036] The content of conjugated diene compound units in the total 100% by mass of the polymer block (B1) and the polymer block (B2) is preferably 50 to 100% by mass, more preferably 70 to 100% by mass, even more preferably 90 to 100% by mass, and may also be 100% by mass.
[0037] Furthermore, the polymer block (B1) and the polymer block (B2) may each independently contain other anionic polymerizable monomers other than conjugated diene compound units, as long as they can solve the problems of the present invention. However, α-methylstyrene is not included among the other anionic polymerizable monomers other than conjugated diene compound units. The form of the polymer block (B1) and the polymer block (B2) when they contain other anionic polymerizable monomers other than conjugated diene compound units is not particularly limited and may be random or tapered.
[0038] The weight-average molecular weight (Mw) of polymer block (B1) and polymer block (B2) in terms of polystyrene is preferably 10,000 to 400,000, more preferably 15,000 to 200,000, even more preferably 15,000 to 150,000, and even more preferably 15,000 to 100,000, respectively. The weight-average molecular weight (Mw) can be measured by GPC (gel permeation chromatography), specifically by the method described in the examples.
[0039] The amount of vinyl bonding in polymer block (B1) and polymer block (B2) is preferably 10 to 95 mol%, more preferably 15 to 80 mol%, even more preferably 20 to 70 mol%, even more preferably 35 to 60 mol%, and even more preferably 40 to 50 mol% respectively. Here, the "amount of vinyl bonding in polymer block (B1)" is the same as the description of the amount of vinyl bonding in polymer block (B), in which the phrase "amount of vinyl bonding in polymer block (B)" is changed to "amount of vinyl bonding in polymer block (B1)", and the phrase "for a total of 100 mol% of all structural units constituting the conjugated diene compound units in polymer block (B)" is changed to "for a total of 100 mol% of all structural units constituting the conjugated diene compound units in polymer block (B1)". Furthermore, the "amount of vinyl bonding in polymer block (B2)" is the same as the explanation in which, in the explanation of the amount of vinyl bonding in polymer block (B), the phrase "amount of vinyl bonding in polymer block (B)" is changed to "amount of vinyl bonding in polymer block (B2)", and the phrase "for a total of 100 mol% of all structural units constituting the conjugated diene compound units in polymer block (B)" is changed to "for a total of 100 mol% of all structural units constituting the conjugated diene compound units in polymer block (B2)". The amount of vinyl bonding in polymer block (B1) and polymer block (B2) is determined independently of each other. 1 It can be calculated using 1H-NMR spectroscopy. Specifically, it can be measured and calculated by the method described in the examples.
[0040] The polymer block (B1) constituting the triblock copolymer (I) and the polymer block (B2) constituting the diblock copolymer (II) may be the same or they may be different.
[0041] In the block copolymer (X), the ratio [(A1) + (A2)]:[(B1) + (B2)] of the total mass of polymer block (A1) and polymer block (A2) to the total mass of polymer block (B1) and polymer block (B2) in the block copolymer (X) is preferably 5:95 to 55:45, more preferably 10:90 to 45:55, even more preferably 15:85 to 35:65, even more preferably 20:80 to 35:65, even more preferably 22:78 to 33:67, and even more preferably 24:76 to 31:69. In other words, the total content of polymer blocks (A1) and (A2) in 100% by mass of the total polymer blocks (A1) and (A2), and polymer blocks (B1) and (B2), is preferably 5 to 55% by mass, more preferably 10 to 45% by mass, even more preferably 15 to 35% by mass, even more preferably 20 to 35% by mass, even more preferably 22 to 33% by mass, and even more preferably 24 to 31% by mass. Furthermore, the total content of polymer blocks (B1) and (B2) in 100% by mass of the total polymer blocks (A1) and (A2), and polymer blocks (B1) and (B2), is preferably 45 to 95% by mass, more preferably 55 to 90% by mass, even more preferably 65 to 85% by mass, even more preferably 65 to 80% by mass, even more preferably 67 to 78% by mass, and even more preferably 69 to 76% by mass. Here, if the block copolymer (X) contains multiple polymer blocks (A1), the total mass of all polymer blocks (A1) contained in the block copolymer (X) is used to calculate the total mass of polymer blocks (A1) and (A2), and the same applies if the block copolymer (X) contains multiple polymer blocks (A2). Furthermore, when calculating the total content of polymer blocks (A1) and (A2), the same applies as described here, except that the term "total mass" is changed to "total content".Similarly, when the block copolymer (X) contains a plurality of polymer blocks (B1), the total mass of all polymer blocks (B1) contained in the block copolymer (X) is used for calculating the total mass of the polymer blocks (B1) and (B2), and the same applies when the block copolymer (X) contains a plurality of polymer blocks (B2). When calculating the total content of the polymer blocks (B1) and (B2), the procedure is the same except that the reference to "total mass" in the description herein is changed to "total content". The total content of the polymer block (A1) and the polymer block (A2) in 100 mass% of the total of the polymer blocks (A1) and (A2) and the polymer blocks (B1) and (B2) is. 1 can be calculated using H-NMR spectrum measurement. Specifically, it can be measured and calculated by the methods described in the Examples. Therefore, the total content of the polymer block (A1) and the polymer block (A2) in 100 mass% of the total of the polymer blocks (A1) and (A2) and the polymer blocks (B1) and (B2), as well as the ratio [(A1)+(A2)]:[(B1)+(B2)], can also be 1 calculated using H-NMR spectrum measurement.
[0042] From the viewpoint of easily achieving good melt spinnability, as well as favorable stretch properties and heat resistance of the obtained fiber, the total content of the polymer blocks (A1) and (A2) and the polymer blocks (B1) and (B2) in 100 mass% of the total of the triblock copolymer (I) and the diblock copolymer (II) is preferably 80 to 100 mass%, more preferably 90 to 100 mass%, even more preferably 95 to 100 mass%, still more preferably 98 to 100 mass%, and may be 100 mass%.
[0043] The triblock copolymer (I) and the diblock copolymer (II) are each independently hydrogenated block copolymers, and their hydrogenation rates are each independently preferably 50 to 100 mol%. A hydrogenation rate of 50 to 100 mol% is preferable from the viewpoint of easily improving melt spinnability and heat resistance. It is also preferable from the viewpoint of easily improving weather resistance. From a similar viewpoint, the hydrogenation rates of the triblock copolymer (I) and the diblock copolymer (II) are each independently more preferably 70 to 100 mol%, even more preferably 90 to 100 mol%, even more preferably 90 to 99.9 mol%, even more preferably 95 to 99.7 mol%, and even more preferably 97 to 99.5 mol%. Preferably, the triblock copolymer (I) and the diblock copolymer (II) are hydrogenated, with a polymer block (B1) containing conjugated diene compound units contained in the triblock copolymer (I) and a polymer block (B2) containing conjugated diene compound units contained in the diblock copolymer (II). The hydrogenation rates of the triblock copolymer (I) and the diblock copolymer (II) are: 1 It can be calculated using H-NMR spectroscopy.
[0044] One or both of the triblock copolymer (I) and the diblock copolymer (II) may have, or may not have, a functional group such as a carboxyl group, a hydroxyl group, an acid anhydride, an amino group, or an epoxy group in at least one selected from the group consisting of the main chain, side chains, and molecular ends in the molecular chain, as long as the problems of the present invention can be solved.
[0045] The weight-average molecular weight (Mw) of the triblock copolymer (I) and the diblock copolymer (II) on a polystyrene basis can be appropriately adjusted according to the application and other factors. The weight-average molecular weight (Mw) of the triblock copolymer (I) is preferably 10,000 to 2,000,000, more preferably 10,000 to 1,000,000, even more preferably 10,000 to 500,000, even more preferably 10,000 to 250,000, even more preferably 10,000 to 150,000, and even more preferably 10,000 to 100,000, and may also be, for example, 15,000 to 100,000, 20,000 to 100,000, 25,000 to 100,000, 35,000 to 100,000, 40,000 to 100,000, or 50,000 to 100,000. The weight-average molecular weight (Mw) of the diblock copolymer (II) is preferably 5,000 to 1,000,000, more preferably 5,000 to 500,000, even more preferably 5,000 to 250,000, even more preferably 5,000 to 100,000, and even more preferably 5,000 to 50,000, and may also be, for example, 7,500 to 50,000, 10,000 to 50,000, 12,500 to 50,000, 17,500 to 50,000, 20,000 to 50,000, or 25,000 to 50,000. The weight-average molecular weight (Mw) can be measured by GPC (gel permeation chromatography), specifically by the method described in the examples.
[0046] The preferred ranges for the weight-average molecular weight (Mw) of the triblock copolymer (I) and the diblock copolymer (II) on a polystyrene basis can be combined. For example, in one embodiment of the fiber, it is preferable that the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 10,000 to 2,000,000, and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 5,000 to 100,000; more preferably, the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 10,000 to 1,000,000, and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 5,000 to 500,000; and the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 10,000 to 500,000, and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 5,000 to 250,000. It is even more preferable that the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 10,000 to 250,000 and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 5,000 to 100,000; it is even more preferable that the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 10,000 to 150,000 and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 5,000 to 50,000; and it is even more preferable that the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 10,000 to 100,000 and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 5,000 to 50,000.For example, in one embodiment of the fiber, the polystyrene-based weight-average molecular weight (Mw) of the triblock copolymer (I) may be 15,000 to 100,000, and the polystyrene-based weight-average molecular weight (Mw) of the diblock copolymer (II) may be 7,500 to 50,000; the polystyrene-based weight-average molecular weight (Mw) of the triblock copolymer (I) may be 20,000 to 100,000, and the polystyrene-based weight-average molecular weight (Mw) of the diblock copolymer (II) may be 10,000 to 50,000; the polystyrene-based weight-average molecular weight (Mw) of the triblock copolymer (I) may be 25,000 to 100,000, and the polystyrene-based weight-average molecular weight (Mw) of the diblock copolymer (II) may be 12,500 to 50,000. It may be the case that the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 35,000 to 100,000 and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 17,500 to 50,000; the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 40,000 to 100,000 and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 20,000 to 50,000; or the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 50,000 to 100,000 and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 25,000 to 50,000.
[0047] The weight-average molecular weight (Mw) of the block copolymer (X) on a polystyrene basis can be appropriately adjusted according to the application and other factors. The weight-average molecular weight (Mw) of the block copolymer (X) is preferably 10,000 to 2,000,000, more preferably 10,000 to 1,000,000, even more preferably 10,000 to 500,000, even more preferably 10,000 to 250,000, even more preferably 10,000 to 150,000, and even more preferably 10,000 to 100,000, and may also be, for example, 15,000 to 100,000, 20,000 to 100,000, 25,000 to 100,000, 35,000 to 100,000, 40,000 to 100,000, or 50,000 to 100,000. The weight-average molecular weight (Mw) can be measured by GPC (gel permeation chromatography), specifically by the method described in the examples.
[0048] The block copolymer (X), as well as the triblock copolymer (I) and diblock copolymer (II), can be synthesized by anionic polymerization. For example, for the triblock copolymer (I), specific synthesis methods such as methods (1) and (2) below are shown. Method (1): A method to obtain an A-B-A type block copolymer by polymerizing a conjugated diene compound in a tetrahydrofuran solvent using a dianionic initiator, followed by sequential polymerization of α-methylstyrene under a temperature of -78°C (Macromolecules, (1969), 2(5), 453-458). Method (2): A method to obtain an A-B-A type block copolymer by using an organolithium compound as a polymerization initiator in a nonpolar solvent, polymerizing α-methylstyrene at a specific concentration at a specific temperature in the presence of a specific concentration of a polar compound, polymerizing a conjugated diene compound on the resulting living poly-α-methylstyryllithium, and then adding a coupling agent.
[0049] Regarding the triblock copolymer (I), the method of method (2) described above is adopted as a more preferred method. Specifically, it is produced by the method described in the examples.
[0050] The polymerization initiator used during polymerization is an organolithium compound, and examples include monolithium compounds such as n-butyllithium, sec-butyllithium, and tert-butyllithium, and dilithium compounds such as tetraethylenedilithium. These compounds may be used individually or in combination of two or more.
[0051] The solvent used during polymerization is a nonpolar solvent, such as aliphatic hydrocarbons like cyclohexane, methylcyclohexane, n-hexane, and n-heptane, and aromatic hydrocarbons like benzene, toluene, and xylene. These hydrocarbons may be used individually or in combination of two or more. The polar compounds used during polymerization are compounds that do not have functional groups (such as hydroxyl groups or carbonyl groups) that react with anionic species, and that have heteroatoms such as oxygen atoms and nitrogen atoms in their molecules. Examples include diethyl ether, monoglyme, tetramethylethylenediamine, dimethoxyethane, and tetrahydrofuran. These compounds may be used individually or in combination of two or more.
[0052] The concentration of the polar compound in the reaction system is preferably 0.01 to 10% by mass, more preferably 0.05 to 5% by mass, and even more preferably 0.1 to 3% by mass, of 100% by mass of the total amount of solvent and all compounds in the reaction system, from the viewpoint of controlling the amount of vinyl bonds in polymer block (B1) and polymer block (B2). The concentration of α-methylstyrene in the reaction system is preferably 1 to 50% by mass, more preferably 3 to 30% by mass, and even more preferably 5 to 10% by mass, of 100% by mass of the total amount of solvent and all compounds in the reaction system, from the viewpoint of polymerizing α-methylstyrene with a high polymerization conversion rate and from the viewpoint of making it easier to appropriately adjust the viscosity of the reaction solution in the later stages of polymerization. The "polymerization conversion rate" refers to the percentage of unpolymerized α-methylstyrene that has been converted to living poly-α-methylstyrenelithium, and in the block copolymer (X) according to the embodiment of the present invention, from the viewpoint of ease of manufacture, this percentage is preferably 70% to 100%, and more preferably 85% to 99%.
[0053] The polymerization temperature for α-methylstyrene is preferably in the range of -30°C to 30°C, more preferably -20°C to 10°C, and even more preferably -15°C to 0°C. By setting the polymerization temperature to 30°C or lower, α-methylstyrene can be polymerized with a high polymerization conversion rate, and the proportion of the resulting living poly-α-methylstyryllithium that is deactivated is also small, suppressing the inclusion of unpolymerized α-methylstyrene in the resulting block copolymer and preventing any impairment of its physical properties, which is preferable. On the other hand, by setting the polymerization temperature to -30°C or higher, the reaction solution can be stirred without becoming highly viscous in the later stages of α-methylstyrene polymerization, and the costs required to maintain a low temperature are not increased, which is also economically preferable.
[0054] After the formation of living poly-α-methylstyryllithium, the conjugated diene compound is then polymerized. There are no particular restrictions on the method of adding the conjugated diene compound to the living poly-α-methylstyryllithium solution. The conjugated diene compound may be added directly to the living poly-α-methylstyryllithium solution, or the conjugated diene compound may be diluted with a solvent and then added to the living poly-α-methylstyryllithium solution. The method of diluting the conjugated diene compound with a solvent and then adding it to the living poly-α-methylstyryllithium solution may be one of the following: adding the conjugated diene compound and then diluting with the solvent; adding the conjugated diene compound and the solvent simultaneously; or adding the conjugated diene compound after diluting it with a solvent. Preferably, a method is recommended in which a conjugated diene compound in an amount equivalent to 1 to 100 molar equivalents, preferably 5 to 50 molar equivalents, relative to living poly-α-methylstyryllithium is added to the living poly-α-methylstyryllithium solution, the solution is diluted with a solvent, and then the remaining conjugated diene compound is added, and the polymerization reaction is carried out at a temperature preferably above 30°C, more preferably in a temperature range of 40°C to 80°C.
[0055] Examples of solvents that can be used for dilution include aliphatic hydrocarbons such as cyclohexane, methylcyclohexane, n-hexane, and n-heptane, and aromatic hydrocarbons such as benzene, toluene, and xylene. These solvents may be used individually or in combination of two or more.
[0056] A triblock copolymer (I) can be produced by reacting a coupling agent with a living polymer obtained by copolymerizing living poly-α-methylstyryllithium with a conjugated diene compound. By adjusting the amount of coupling agent used, a mixture containing triblock copolymer (I) and diblock copolymer (II) can be obtained. Examples of coupling agents include phenyl benzoate, methyl benzoate, ethyl benzoate, methyl acetate, ethyl acetate, methyl pivalate, ethyl pivalate, phenyl pivalate, α,α'-dichloro-o-xylene, α,α'-dichloro-m-xylene, α,α'-dichloro-p-xylene, bis(chloromethyl) ether, dibromomethane, diiodomethane, dimethyl phthalate, dichlorodimethylsilane, dichlorodiphenylsilane, trichloromethylsilane, tetrachlorosilane, and divinylbenzene.
[0057] When hydrogenating a triblock copolymer (I) obtained by reacting a living polymer with a coupling agent, or a mixture of triblock copolymer (I) and diblock copolymer (II), the hydrogenated block copolymer can be obtained by adding active hydrogen compounds such as alcohols, carboxylic acids, or water as needed to stop the coupling reaction, and then hydrogenating in an inert organic solvent in the presence of a hydrogenation catalyst according to a known method.
[0058] Unhydrogenated block copolymers can be subjected to hydrogenation without replacing the solvent used in their production. The hydrogenation reaction can be carried out, for example, in the presence of a hydrogenation catalyst such as a Ziegler catalyst containing an alkylaluminum compound and a transition metal such as cobalt or nickel, at a reaction temperature of 20–100°C and a hydrogen pressure of 1–100 kg / cm². 2This can be done under the following conditions.
[0059] The block copolymer (X) is preferably obtained by the method described above. The triblock copolymer (I) and diblock copolymer (II), which are preferably contained in the block copolymer (X), are also preferably obtained by the method described above. In particular, the triblock copolymer (I) and diblock copolymer (II), which can be used in one embodiment of the fiber, are preferably obtained by polymerizing α-methylstyrene at a concentration of 5 to 50% by mass at a temperature of -30 to 30°C using an organolithium compound as an initiator in a nonpolar solvent, in the presence of a polar compound at a concentration of 0.1 to 10% by mass, to form a polymer block (A1) or (A2), then polymerizing a conjugated diene compound in an amount of 1 to 100 molar equivalents relative to living poly-α-methylstyryllithium, and then polymerizing the remaining conjugated diene compound at a temperature above 30°C to form a polymer block (B1) or (B2), which is desirable from the viewpoint of stretchability and heat resistance.
[0060] {Content of triblock copolymer (I) and diblock copolymer (II) in block copolymer (X)} The total content of the triblock copolymer (I) and the diblock copolymer (II) in the block copolymer (X) is preferably 70 to 100% by mass, more preferably 80 to 100% by mass, even more preferably 90 to 100% by mass, and even more preferably 95 to 100% by mass, and may also be 100% by mass, based on 100% by mass of the total amount of each block copolymer contained in the block copolymer (X).
[0061] The block copolymer (X) may include a block copolymer (III) different from the triblock copolymer (I) and the diblock copolymer (II). The block copolymer (III) is, for example, a tetrablock copolymer represented as A-B-A-B when the polymer block (A) is represented as "A" and the polymer block (B) as "B", (A-B) mExamples include copolymers having a branched or radial (star-shaped) molecular structure represented by Z (where Z represents a coupling agent residue and m is 3 or greater). These block copolymers (III) may be used individually or in combination of two or more types.
[0062] In this specification, when polymer blocks of the same type are linearly linked via a bifunctional coupling agent or the like, the entire linked polymer block is treated as a single polymer block. Accordingly, including the above example, a polymer block that should strictly be written as A-Z-A (where Z represents a coupling agent residue) is referred to as A as a whole, unless it is necessary to distinguish it from a single polymer block A. Similarly, a polymer block that should strictly be written as B-Z-B (where Z represents a coupling agent residue) is referred to as B as a whole, unless it is necessary to distinguish it from a single polymer block B. In this specification, polymer blocks of this type containing coupling agent residues are treated as described above, so for example, a block copolymer containing coupling agent residues that should strictly be written as A-B-Z-B-A (where Z represents a coupling agent residue) is referred to as A-B-A, and in this case, it is treated as the triblock copolymer (I). Similarly, a block copolymer containing coupling agent residues, which should strictly be written as A-B-Z-B (where Z represents a coupling agent residue), is written as A-B, and in this case, it is treated as the diblock copolymer (II).
[0063] (Content of block copolymer (X) in the resin) The content of the block copolymer (X) in the resin is preferably 30 to 100% by mass, more preferably 50 to 100% by mass, even more preferably 75 to 100% by mass, even more preferably 80 to 100% by mass, even more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, even more preferably 98 to 100% by mass, and may also be 100% by mass, from the viewpoint of easily obtaining good melt spinnability and stretchability and heat resistance of the obtained fibers. In one embodiment of the present invention, the content of the block copolymer (X) may be, for example, 30 to 99.9% by mass, 50 to 99.9% by mass, 75 to 99.9% by mass, 80 to 99.9% by mass, 90 to 99.9% by mass, 95 to 99.9% by mass, or 98 to 99.9% by mass, based on 100% by mass of the total amount of the resin.
[0064] (Components other than the block copolymer (X)) The resin may or may not contain components other than the block copolymer (X). Examples of components other than the block copolymer (X) include polymers other than the block copolymer (X), oils, inorganic fillers, heat aging inhibitors, antioxidants, light stabilizers, antistatic agents, mold release agents, flame retardants, foaming agents, pigments, dyes, whitening agents, ultraviolet absorbers, and lubricants. From the viewpoint of preventing the generation of harmful gases when the resin and fibers are burned, it is preferable that the components other than the block copolymer (X) are compounds that do not contain halogens, cyanide, etc. These components may be used individually or in combination of two or more.
[0065] [Polymers other than the block copolymer (X)] The resin may or may not contain polymers other than the block copolymer (X). The resin may contain, as polymers other than the block copolymer (X), at least one selected from the group consisting of styrene resins, styrene thermoplastic elastomers other than the block copolymer (X), acrylic resins, polyolefin resins, and polyolefin elastomers. Examples of the styrene resins include poly-α-methylstyrene resin and polystyrene resin. The stereoregularity of the polystyrene resin may have at least one stereoregularity selected from the group consisting of atactic, isotactic, and syndiotactic. For example, the case in which the polystyrene resin has two types of stereoregularity, isotactic and syndiotactic, refers to the case in which both isotactic segments and syndiotactic segments are present in the polymer main chain of the polystyrene resin. In one embodiment of the present invention, if the resin includes the polystyrene resin, at least one polystyrene selected from the group consisting of atactic polystyrene, isotactic polystyrene, syndiotactic polystyrene, and polystyrene having multiple stereoregular structures in one molecule as described above may be used. Examples of styrene-based thermoplastic elastomers other than the block copolymer (X) include polystyrene-polybutadiene-polystyrene (SBS) block copolymer, hydrogenated SBS block copolymer, polystyrene-polyisoprene-polystyrene (SIS) block copolymer, hydrogenated SIS block copolymer, polystyrene-polyethylene-polybutylene-polystyrene (SEBS) block copolymer, polystyrene-polyethylene-polypropylene-polystyrene (SEEPS) block copolymer, polystyrene-polyfarnesene-polystyrene (SFS) block copolymer, and at least one polymer selected from the group consisting of polystyrene-polyethylene-polypropylene-polystyrene (SEPS) block copolymer.The polystyrene blocks in the styrene-based thermoplastic elastomer may have at least one stereoregularity selected from the group consisting of atactic, isotactic, and syndiotactic. For example, the case in which the polystyrene block has two types of stereoregularity, isotactic and syndiotactic, refers to the presence of both isotactic segments and syndiotactic segments in the main chain of the polystyrene block. In each copolymer that is a styrene-based thermoplastic elastomer, the stereoregularity, molecular weight, and other molecular structures of the multiple polystyrene blocks may be different or the same.
[0066] Examples of the acrylic resin include polymers containing structures derived from acrylic monomers such as methyl methacrylate, methyl acrylate, butyl methacrylate, ethyl methacrylate, 2-hydroxyethyl methacrylate, and acrylic acid. The acrylic resin may be a homopolymer obtained by polymerizing one of these acrylic monomers alone, or it may be a copolymer obtained by copolymerizing at least two selected from the group consisting of these acrylic monomers. Examples of the polyolefin resin include polypropylene and polyethylene. The polyolefin resin may be a modified polyolefin such as an acid-modified polyolefin, and examples of the acid-modified polyolefin include acid-modified polypropylene and acid-modified polyethylene. The polymers other than the block copolymer (X) may be used individually or in combination of two or more.
[0067] The content of polymers other than the block copolymer (X) in the resin is preferably 0 to 70% by mass, more preferably 0 to 50% by mass, even more preferably 0 to 25% by mass, even more preferably 0 to 20% by mass, even more preferably 0 to 10% by mass, even more preferably 0 to 5% by mass, and even more preferably 0 to 2% by mass, based on 100% by mass of the total amount of the resin, and may also be 0% by mass. Furthermore, the content of polymers other than the block copolymer (X) may be, for example, 10 to 70% by mass, 20 to 70% by mass, 25 to 70% by mass, or 50 to 70% by mass, based on 100% by mass of the total amount of the resin.
[0068] [Oil] From the viewpoint of facilitating recycling, the oil is preferably at least one selected from the group consisting of biomass-derived plasticizers that do not have a carboxyl group, vegetable oil, synthetic plasticizer, and recycled oil.
[0069] Examples of biomass-derived plasticizers that do not contain a carboxyl group include compounds represented by the following general formula (1) and compounds represented by the following general formula (2).
[0070] In general formula (1), n 1 ~n 3 Each of these is independently either 1 or 3. 1 ~R 6 Each of these is independently a hydrogen atom or an unsubstituted hydrocarbon group, and may or may not have a branched structure. However, R 1 and R 2 The total number of carbon atoms is 14, R 3 and R 4 The total number of carbon atoms is 14, R 5 and R 6 The total number of carbon atoms is 14.
[0071] In general formula (2), n 4 and n 5 Each of these is independently either 1 or 3. 7 ~R 10Each of these is independently a hydrogen atom or an unsubstituted hydrocarbon group, and may or may not have a branched structure. However, R 7 and R 8 The total number of carbon atoms is 14, R 9 and R 10 The total number of carbon atoms is 14.
[0072] Examples of vegetable oils include castor oil, cottonseed oil, linseed oil, safflower oil, rapeseed oil, soybean oil, Nagi oil, wood wax, pine oil, corn oil, peanut oil, olive oil, palm oil, palm olein, palm stearin, and other plant-derived oils, as well as transesterified oils, hydrogenated oils, or fractionated oils of these. Examples of synthetic plasticizers include oil-based softeners such as paraffinic, naphthenic, and aromatic process oils, mineral oil, and white oil; phthalic acid derivatives such as dioctyl phthalate and dibutyl phthalate; liquid co-oligomers of ethylene and α-olefins; liquid paraffin; polybutene; low molecular weight polyisobutylene; liquid polydienes such as liquid polybutadiene, liquid polyisoprene, liquid polyisoprene / butadiene copolymer, liquid styrene / butadiene copolymer, and liquid styrene / isoprene copolymer; and hydrogenated or modified versions thereof. The recycled oil is not particularly limited as long as it is oil that has been used and made reusable. Examples include the product names "RECOR-T 4867", "RECOR-M 1259", and "RECOR-M 1260" (all manufactured by H&R). The "liquid polydiene" that can be used as the oil refers to polydiene that is liquid at 38°C, and for example, has a melt viscosity at 38°C (hereinafter also referred to as "38°C melt viscosity") of 2,000 Pa·s or less. The 38°C melt viscosity can be measured using a Brookfield viscometer (manufactured by BROOKFIELD ENGINEERING LABS. INC.).
[0073] These oils may be used individually or in combination of two or more types.
[0074] The content of the oil in the resin is preferably 0 to 70% by mass, more preferably 0 to 50% by mass, even more preferably 0 to 25% by mass, even more preferably 0 to 20% by mass, even more preferably 0 to 10% by mass, even more preferably 0 to 5% by mass, and even more preferably 0 to 2% by mass, and may also be 0% by mass. From the viewpoint of suppressing a decrease in the stretchability and heat resistance of the resulting fibers, it is preferable that the resin is substantially free of the oil. Here, substantially free of the oil in the resin means that the oil content is 0% by mass or more and less than 2% by mass, preferably 0 to 1% by mass, more preferably 0 to 0.5% by mass, and even more preferably 0% by mass, based on 100% by mass of the total amount of the resin.
[0075] The total content of at least one component selected from the group consisting of the aforementioned inorganic fillers, heat aging inhibitors, antioxidants, light stabilizers, antistatic agents, mold release agents, flame retardants, foaming agents, pigments, dyes, whitening agents, ultraviolet absorbers, and lubricants in the resin can be appropriately determined in accordance with the balance between melt spinnability and the properties required of the resulting fiber. In one embodiment of the present invention, for example, from the viewpoint of easily improving melt spinnability and the stretchability and heat resistance of the resulting fibers, the total content of at least one component selected from the group consisting of inorganic fillers, heat aging inhibitors, antioxidants, light stabilizers, antistatic agents, mold release agents, flame retardants, foaming agents, pigments, dyes, whitening agents, ultraviolet absorbers, and lubricants in 100% by mass of the total amount of the resin is preferably 0 to 70% by mass, more preferably 0 to 50% by mass, even more preferably 0 to 25% by mass, even more preferably 0 to 20% by mass, even more preferably 0 to 10% by mass, even more preferably 0 to 5% by mass, and even more preferably 0% by mass. In one embodiment of the present invention, the total content of at least one component selected from the group consisting of inorganic fillers, heat aging inhibitors, antioxidants, light stabilizers, antistatic agents, mold release agents, flame retardants, foaming agents, pigments, dyes, whitening agents, ultraviolet absorbers, and lubricants in 100% by mass of the total amount of the resin may be, for example, 0.1 to 70% by mass, 0.1 to 50% by mass, 0.1 to 25% by mass, 0.1 to 20% by mass, 0.1 to 10% by mass, 0.1 to 5% by mass, or 0.1 to 2% by mass.
[0076] In one embodiment of the present invention, the total content of components other than the block copolymer (X) in 100% by mass of the total amount of the resin is preferably 0 to 70% by mass, more preferably 0 to 50% by mass, even more preferably 0 to 25% by mass, even more preferably 0 to 20% by mass, even more preferably 0 to 10% by mass, even more preferably 0 to 5% by mass, even more preferably 0 to 2% by mass, and may also be 0% by mass. In one embodiment of the present invention, the total content of components other than the block copolymer (X) may be, for example, 0.1 to 70% by mass, 0.1 to 50% by mass, 0.1 to 25% by mass, 0.1 to 20% by mass, 0.1 to 10% by mass, 0.1 to 5% by mass, or 0.1 to 2% by mass, in 100% by mass of the total amount of the resin.
[0077] In the resin, the respective content of each component described above can be independently determined, but when the selected content is combined, the range in which the total content of each component exceeds 100% by mass of the total amount of the resin is not included. That is, if the resin contains components other than the block copolymer (X), the total content of at least two components selected from the group consisting of the block copolymer (X) and components other than the block copolymer (X) in the total amount of the resin is 100% by mass or less, and may be 100% by mass.
[0078] <Structure of Fibers, etc.> There are no particular limitations on the aforementioned fibers, but examples include fibers having a single cross-section that is not divided, as described later (in this specification, fibers of this structure are also referred to as "single-section fibers"); and composite fibers such as core-sheath composite fibers, side-by-side composite fibers, divided composite fibers, and sea-island composite fibers (in this specification, fibers of this structure are also referred to as "composite-section fibers"). In this specification, the terms "composite fiber" and "composite-section fiber" refer to fibers in which multiple different resin components are joined to form a single fiber, and each resin component exists continuously in the length direction of the fiber. Therefore, they are distinguished from fibers in which a particular resin component forms a particulate or co-continuous phase structure in other resin components (matrix resin) by, for example, melting and mixing multiple incompatible resin components beforehand, and is dispersed in a discontinuous structure in the length direction of the fiber. Accordingly, such fiber structures are included in the sub-concepts of the single-section fibers and composite-section fibers, and may be taken in either the single-section fiber or the composite-section fiber. In one embodiment of the fiber, from the viewpoint of easily achieving good melt-spinning properties, the fiber is preferably a single-section fiber or a core-sheath composite fiber.
[0079] There are no particular restrictions on the shape of the cross-section of the fiber, but examples include circular cross-sections such as perfect circles and ellipses; polygonal cross-sections such as triangles, squares, pentagons, and hexagons; star-shaped, C-shaped, V-shaped, U-shaped, Y-shaped; and irregular cross-sections such as cross-shaped. For example, the single-section fiber and composite-section fiber described above may each have a circular cross-section, a polygonal cross-section, or an irregular cross-section. The circular cross-section, polygonal cross-section, and irregular cross-section may each have a hollow cross-section, for example, having a cavity inside the fiber (inside the cross-section). Generally, the fiber having a hollow cross-section is also called a hollow fiber. In one embodiment of the fiber, from the viewpoint of easily achieving good melt-spindle properties, the fiber is preferably a circular cross-section. Therefore, in one embodiment of the fiber, from the viewpoint of easily achieving good melt-spindle properties, the fiber is more preferably a single-section fiber having a circular cross-section or a core-sheath type composite fiber having a circular cross-section.
[0080] As described above, since at least part or all of the fiber is formed from the resin, for example, in one embodiment of the fiber, if the fiber is a core-sheath type composite fiber, the resin may be included in at least one selected from the core and the sheath, or the resin may be included in both the core and the sheath. When the fiber is a core-sheath type composite fiber, the ratio of the sheath component content to the core component content [sheath / core] may be, by mass, for example, 1 / 99 to 80 / 20, 5 / 95 to 70 / 30, 10 / 90 to 60 / 40, 12 / 88 to 55 / 45, or 15 / 85 to 50 / 50.
[0081] When the fiber is a core-sheath type composite fiber, in one embodiment, the core component may be the resin, and the sheath component may be a resin other than the resin (hereinafter also referred to as "resin for sheath component"), forming a core-sheath type composite fiber (SC1). In the embodiment of the core-sheath type composite fiber (SC1), the content of the resin in the core component is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, even more preferably 98 to 100% by mass, and may also be 100% by mass, out of 100% by mass of the total amount of the core component. On the other hand, in the embodiment of the core-sheath type composite fiber (SC1), the resin for sheath component is a resin containing polymers other than the block copolymer (X), and examples of polymers other than the block copolymer (X) include the various polymers mentioned in the "Polymers other than the block copolymer (X)" section. Among these, polyolefin resins are preferred, at least one selected from polypropylene and polyethylene is more preferred, and polyethylene is even more preferred. In the resin for the sheath component, the content of polymers other than the block copolymer (X) is preferably 50 to 100% by mass, more preferably 75 to 100% by mass, even more preferably 80 to 100% by mass, even more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and even more preferably 98 to 100% by mass, and may also be 100% by mass, based on 100% by mass of the total amount of the resin for the sheath component. In the embodiment of the core-sheath type composite fiber (SC1), the resin for the sheath component may contain, or may not contain, the various components mentioned above in the "Components other than the block copolymer (X)" section, in addition to polymers other than the block copolymer (X).
[0082] When the fiber is a core-sheath type composite fiber, in one embodiment, the resin is used as the sheath component, and a resin other than the resin (hereinafter also referred to as "core component resin") is used as the core component in a core-sheath type composite fiber (SC2). In the embodiment of the core-sheath type composite fiber (SC2), the content of the resin in the sheath component is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and even more preferably 98 to 100% by mass, and may also be 100% by mass, out of 100% by mass of the total amount of the sheath component. On the other hand, in the embodiment of the core-sheath type composite fiber (SC2), the core component resin is a polymer that includes polymers other than the block copolymer (X), and examples of polymers other than the block copolymer (X) include the various polymers mentioned in the "Polymers other than the block copolymer (X)" section. Among these, styrene-based thermoplastic elastomers other than the block copolymer (X) are preferred, at least one selected from polystyrene-polybutadiene-polystyrene (SBS) block copolymer, hydrogenated SBS block copolymer, and polystyrene-polyethylene-polybutylene-polystyrene (SEBS) block copolymer is more preferred, at least one selected from hydrogenated SBS block copolymer and SEBS block copolymer is even more preferred, and SEBS block copolymer is even more preferred. The content of polymers other than the block copolymer (X) in the core component resin is, for example, preferably 50 to 100% by mass, more preferably 55 to 100% by mass, even more preferably 60 to 100% by mass, and even more preferably 65 to 100% by mass, based on 100% by mass of the total amount of the core component resin.
[0083] In the embodiment of the core-sheath type composite fiber (SC2), the core component resin may or may not contain polymers other than the block copolymer (X) as described in the "Components other than the block copolymer (X)" section. For example, in the embodiment of the core-sheath type composite fiber (SC2), the core component resin may contain the oil described in the "Components other than the block copolymer (X)" section, in which case the content of the oil in the core component resin is preferably 1 to 50% by mass, more preferably 1 to 45% by mass, even more preferably 1 to 40% by mass, and even more preferably 1 to 35% by mass, based on 100% by mass of the total amount of the core component resin. The total content of polymers other than the block copolymer (X) and the oil in 100% by mass of the total amount of the core component resin is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, even more preferably 98 to 100% by mass, and may also be 100% by mass. In an embodiment in which the core component includes polymers and oils other than the block copolymer (X), the resin for the core component may or may not include the polymers and oils other than the block copolymer (X) and oils mentioned above in the "Components other than the block copolymer (X)" section.
[0084] <Resin Content in Fibers> As described above, at least a part or all of the fiber is formed from the resin. The resin content in the fiber may be, for example, 30-100% by mass, 35-100% by mass, 40-100% by mass, 50-100% by mass, 60-100% by mass, 70-100% by mass, 80-100% by mass, 90-100% by mass, 95-100% by mass, or 100% by mass, based on 100% by mass of the total amount of the fiber. The resin content in the fiber can also be appropriately set depending on the structure of the fiber as described above. For example, in one embodiment of the fiber, if the fiber is a single cross-sectional fiber, from the viewpoint of easily obtaining good stretchability properties of the resulting fiber, the content of the resin in the fiber is preferably 60 to 100% by mass, more preferably 70 to 100% by mass, even more preferably 80 to 100% by mass, even more preferably 90 to 100% by mass, even more preferably 95 to 100% by mass, and may also be 100% by mass, based on 100% by mass of the total amount of the fiber. In one embodiment of the fiber, if the fiber is a core-sheath type composite fiber, for example, if the block copolymer (X) is contained in only one of the core or sheath, and the other does not contain a polymer that exhibits good stretchability properties, from the viewpoint of easily obtaining good stretchability properties of the resulting fiber, the content of the resin in the fiber may be, for example, 50 to 99% by mass, 60 to 98% by mass, 70 to 95% by mass, 80 to 95% by mass, or 80 to 90% by mass, based on 100% by mass of the total amount of the fiber. In one embodiment of the fiber, if the fiber is a core-sheath type composite fiber and, for example, contains a polymer that exhibits good stretchability in both the core and the sheath, the content of the resin in the fiber may be, from the viewpoint of easily obtaining good stretchability in the resulting fiber, for example, 30 to 99% by mass, 35 to 98% by mass, 40 to 95% by mass, 30 to 90% by mass, 30 to 80% by mass, 30 to 70% by mass, 30 to 60% by mass, 30 to 50% by mass, 35 to 90% by mass, 35 to 80% by mass, 35 to 70% by mass, 35 to 60% by mass, 35 to 50% by mass, 40 to 90% by mass, 40 to 80% by mass, 40 to 70% by mass, 40 to 60% by mass, or 40 to 50% by mass, based on 100% by mass of the total amount of the fiber.
[0085] <Fiber Fineness> The fineness of the fiber (fiberness of a single fiber (monofilament)) can be appropriately determined according to the balance between melt spinnability and the properties required of the resulting fiber. For example, from the viewpoint of easily achieving good melt spinnability and heat resistance of the resulting fiber, it is preferably 5 to 500 dtex, more preferably 5 to 400 dtex, even more preferably 10 to 350 dtex, even more preferably 15 to 300 dtex, and even more preferably 25 to 200 dtex. For example, it may also be 30 to 200 dtex, 35 to 150 dtex, or 40 to 120 dtex.
[0086] For example, the fineness of the fiber is 0.1 to 2,000 dtex, 0.1 to 1,500 dtex, 0.1 to 1,000 dtex, 0.1 to 500 dtex, 0.1 to 400 dtex, 0.1 to 350 dtex, 0.1 to 300 dtex, 0.1 to 250 dtex, 0.1 to 200 dtex, 0.1 to 150 dtex, 0.1 to 125 dtex, 0.1 to 120 dtex, 0.1 to 100 dtex, 0.1 to 50 dtex, 0.1 to 25 dtex, 0.1 to 20 dtex, 0.25 to 2,000 dtex, 0.25 to 1,500 dtex. 0dtex, 0.25-1,000dtex, 0.25-500dtex, 0.25-400dtex, 0.25-350dtex, 0 .25-300dtex, 0.25-250dtex, 0.25-200dtex, 0.25-150dtex, 0.25-125dt ex, 0.25-120dtex, 0.25-100dtex, 0.25-50dtex, 0.25-25dtex, 0.25-20d tex, 0.5-2,000dtex, 0.5-1,500dtex, 0.5-1,000dtex, 0.5-500dtex, 0.5- 400dtex, 0.5-350dtex, 0.5-300dtex, 0.5-250dtex, 0.5-200dtex, 0.5-1 50dtex, 0.5~125dtex, 0.5~120dtex, 0.5~100dtex, 0.5~50dtex, 0.5~25d tex, 0.5~20dtex, 1~2,000dtex, 1~1,500dtex, 1~1,000dtex, 1~500dtex, 1~400dtex, 1~350dtex, 1~300dtex, 1~250dtex, 1~200dtex, 1~150dtex, 1~ 125dtex, 1~120dtex, 1~100dtex, 1~50dtex, 1~25dtex, 1~20dtex, 2~2,00 0dtex, 2~1,500dtex, 2~1,000dtex, 2~500dtex, 2~400dtex, 2~350dtex, 2~ 300dtex, 2~250dtex, 2~200dtex, 2~150dtex, 2~125dtex, 2~120dtex, 2~1 00dtex, 2~50dtex, 2~25dtex, 2~20dtex, 5~2,000dtex, 5~1,500dtex, 5~1,000dtex、5~500dtex、5~400dtex、5~350dtex、5~300dtex、5~250dtex、5~200dtex、5~150dtex、5~125dtex、5~120dtex、5~100dtex、5~50dtex、5~25dtex、5~20dtex、10~2,000dtex、10~1,500dtex、10~1,000dtex、10~500dtex、10~400dtex、10~350dtex、10~300dtex、10~250dtex、10~200dtex、10~150dtex、10~125dtex、10~120dtex、10~100dtex、10~50dtex、10~25dtex、10~20dtex、15~2,000dtex、15~1,500dtex、15~1,000dtex、15~500dtex、15~400dtex、15~350dtex、15~300dtex、15~250dtex、15~200dtex、15~150dtex、15~125dtex、15~120dtex、15~100dtex、25~2,000dtex、25~1,500dtex、25~1,000dtex、25~500dtex、25~400dtex、25~350dtex、25~300dtex、25~250dtex、25~200dtex、25~150dtex、25~125dtex、25~120dtex、25~100dtex、30~2,000dtex、30~1,500dtex、30~1,000dtex、30~500dtex、30~350dtex、30~300dtex、30~250dtex、30~200dtex、30~150dtex、30~125dtex、30~120dtex、30~100dtex、35~2,000dtex、35~1,500dtex、35~1,000dtex、35~500dtex、35~350dtex、35~300dtex、35~250dtex、35~200dtex、35~150dtex、35~125dtex、35~120dtex、35~100dtex、40~2,000dtex、40~1,500dtex、40~1,000 dtex, 40-500 dtex, 40-350 dtex, 40-300 dtex, 40-250 dtex, 40-200 dtex, 40-150 dtex, 40-125 dtex, 40-120 dtex, or 40-100 dtex may also be used.
[0087] In one embodiment of the fiber, when the fiber is used in sanitary products (synonymous with hygiene products), the fineness of the fiber is preferably 5 to 500 dtex, more preferably 5 to 400 dtex, even more preferably 10 to 350 dtex, even more preferably 15 to 300 dtex, and even more preferably 25 to 200 dtex. Furthermore, in one embodiment of the fiber, when the fiber is used in sanitary products (synonymous with hygiene products) described later, the fineness of the fiber may be within the ranges described above, and among them, for example, 30 to 200 dtex, 35 to 150 dtex, or 40 to 120 dtex.
[0088] In one aspect of the fiber, when the fiber is used in clothing, the fineness of the fiber may be within the ranges described above, for example, 0.1 to 2,000 dtex, 0.1 to 1,500 dtex, 0.1 to 1,000 dtex, 0.1 to 500 dtex, 0.1 to 400 dtex, 0.1 to 350 dtex, 0.1 to 300 dtex, 0.1 to 250 dtex, 0.1 to 200 dtex, 0.1 to 150 dtex, 0.1 to 125 dtex, 0.1 to 120 dtex. ex, 0.1-100dtex, 0.1-50dtex, 0.1-25dtex, 0.1-20dtex, 0.25-250dtex, 0.25-200dtex, 0.25-150dtex, 0.25-125dtex, 0.25- 120dtex, 0.25-100dtex, 0.25-50dtex, 0.25-25dtex, 0.25-20dtex, 0.5-250dtex, 0.5-200dtex, 0.5-150dtex, 0.5-125dtex, 0 .. 5-120dtex, 0.5-100dtex, 0.5-50dtex, 0.5-25dtex, 0.5-20dtex, 1-250dtex, 1-200dtex, 1-150dtex, 1-125dtex, 1-120dtex, 1~100dtex, 1~50dtex, 1~25dtex, 1~20dtex, 2~250dtex, 2~200dtex, 2~150dtex, 2~125dtex, 2~120dtex, 2~100dtex, 2~50dtex , 2-25 dtex, 2-20 dtex, 5-250 dtex, 5-200 dtex, 5-150 dtex, 5-125 dtex, 5-120 dtex, 5-100 dtex, 5-50 dtex, 5-25 dtex, 5-20 dtex, 10-250 dtex, 10-200 dtex, 10-150 dtex, 10-125 dtex, 10-120 dtex, 10-100 dtex, 10-50 dtex, 10-25 dtex, or 10-20 dtex may also be used.
[0089] [Method for Manufacturing Fibers] The fibers can be formed by employing various fiber forming methods such as melt spinning and solution spinning. Among these, it is preferable to form the fibers by melt spinning. That is, as one aspect of the present invention, a method for manufacturing the fibers by melt spinning is cited as a preferred manufacturing method. Known melt spinning methods can be used as the melt spinning method. For example, first, at least the resin is heated and melted using an extruder or the like, the flow rate is controlled by a gear pump (metering pump) or the like, and the molten resin or a composition containing the resin (hereinafter also referred to as "molten body") is discharged from a spinning nozzle equipped with one or more discharge holes. The molten body may be passed through a filter for removing foreign matter upstream of the spinning nozzle. Next, the molten body discharged from the discharge holes is usually taken up by a winding device installed below the spinning nozzle to form fibers. Here, between the time from the spinning nozzle to being wound up by the winding device, the molten body is stretched while being cooled by cooling air or the like, and becomes fibers when cooled to below the solidification temperature of the molten body. Furthermore, the process of taking up the molten material may be carried out in a closed space by installing, as necessary, an insulating cylinder to control the atmosphere directly below the spinning nozzle, a spinning cylinder for blowing cooling air to cool the material, etc., between the spinning nozzle and the winding device. Furthermore, various rolls may be installed between the spinning nozzle and the winding device, such as an oiling roll for applying an oil (e.g., silicone oil) to prevent the individual fibers (monofilaments) from sticking together during spinning and after winding, and a godet roll for adjusting the take-up speed. Furthermore, for example, multiple godet rolls may be installed, and the rotation speed of the rolls located further down the line may be increased relative to the rolls located further down the line, thereby performing a stretching process simultaneously with the take-up of the fibers during melt spinning. After obtaining the fibers by melt spinning, the fibers may be stretched separately using a stretching machine.
[0090] Here, by using a nozzle for single-section structure fibers as the spinning nozzle, the single-section structure fibers can be obtained. On the other hand, by using a nozzle for composite-section fibers as the spinning nozzle, the composite-section fibers can be obtained. When obtaining composite-section fibers, typically, for each different part of the composite-section fiber (a part formed using different forming materials), each forming material is melted using a separate extruder, and the molten forming materials merge with each other when they are simultaneously discharged from multiple discharge holes in the spinning nozzle to form the composite-section fiber.
[0091] The temperature at which the resin or other resins are melted in the extruder can be set appropriately, taking into account the melting point and decomposition temperature of each resin. For example, when using the resin, the ODT of the resin can also be used as a guideline for setting the temperature. The discharge amount from the discharge hole and the winding speed can be set appropriately by starting with a low amount or low speed and gradually increasing it while checking the discharge status of the molten material and the fiber take-up status. Here, assuming that conditions other than the winding speed, such as the discharge amount from the spinning nozzle, are constant, a resin that can be wound at a higher speed for a certain period of time will have better melt-spinning properties.
[0092] [Multifilament] A multifilament according to one aspect of the present invention includes the fibers. In one aspect of the multifilament, the fibers and preferred embodiments thereof included in the multifilament are the same as those described above in the "Fibers" section. In one aspect of the multifilament, there are no particular restrictions on the number of single fibers constituting the multifilament, but for example, it may be 2 to 64, 3 to 64, 4 to 64, 2 to 48, 3 to 48, 4 to 48, 2 to 24, 3 to 24, 4 to 24, 2 to 12, 3 to 12, or 4 to 12. The number of single fibers constituting the multifilament here is determined by the number of discharge holes provided in one spinning nozzle when using the melt spinning method described above. Therefore, when obtaining a multifilament with an increased number of fibers by bundling multiple multifilaments obtained by melt spinning from one spinning nozzle, the number of single fibers constituting the multifilament refers to the number of single fibers contained in the multifilament obtained by melt spinning from one spinning nozzle. As described above, in the manufacturing method described in the "Method for Manufacturing Fibers," the spinning nozzle is equipped with multiple discharge holes, and by converging and winding multiple molten materials discharged from this spinning nozzle using the same winding device, a multifilament can be manufactured.
[0093] In one embodiment of the multifilament, the number of fibers in the multifilament may be, for example, 25-100%, 50-100%, 75-100%, 80-100%, 90-100%, or 100% of the total number of single fibers (monofilaments) constituting the multifilament.
[0094] In one aspect of the multifilament, the fineness of the multifilament, that is, the fineness of the multifilament as a whole, which is a bundle of multiple monofilaments containing the fiber, is, for example, 0.3 to 4,000 dtex, 0.3 to 3,000 dtex, 0.3 to 2,000 dtex, 0.3 to 1,500 dtex, 0.3 to 1,000 dtex, 0.3 to 800 dtex, 0.3 to 700 dtex, 0.3 to 500 dtex, 0.5 to 4,000 dtex, 0.5 to 3,000 dtex, 0.5 to 2,000 dtex, 0.5 to 1,500 dtex. ex, 0.5-1,000dtex, 0.5-800dtex, 0.5-700dtex, 0.5-500dtex, 1-4,000dt ex, 1-3,000dtex, 1-2,000dtex, 1-1,500dtex, 1-1,000dtex, 1-800dtex, 1 ~700dtex, 1~500dtex, 5~4,000dtex, 5~3,000dtex, 5~2,000dtex, 5~1,500 dtex, 5-1,000dtex, 5-800dtex, 5-700dtex, 5-500dtex, 10-4,000dtex, 10 ~3,000dtex, 10~2,000dtex, 10~1,500dtex, 10~1,000dtex, 10~800dtex, 10-700dtex, 10-500dtex, 15-4,000dtex, 15-3,000dtex, 15-2,000dtex, 1 5-1,500dtex, 15-1,000dtex, 15-800dtex, 15-700dtex, 15-500dtex, 20-4 ,000dtex, 20~3,000dtex, 20~2,000dtex, 20~1,500dtex, 20~1,000dtex, 2 0~800dtex, 20~700dtex, 20~500dtex, 50~4,000dtex, 50~3,000dtex, 50~2 ,000dtex, 50-1,500dtex, 50-1,000dtex, 50-800dtex, 50-700dtex, 50-50 0dtex, 90-4,000dtex, 90-3,000dtex, 90-2,000dtex, 90-1,500dtex, 90-1 ,000dtex, 90-800dtex, 90-700dtex, 90-500dtex, 150-4,000dtex, 150-3,000dtex, 150-2,000dtex, 150-1,500dtex, 150-1,000dtex, 150-800dtex, 150-700dtex, 15 0~500dtex, 250~4,000dtex, 250~3,000dtex, 250~2,000dtex, 250~1,500dtex, 250~1,000dt e.g., 250-800 dtex, 250-700 dtex, 250-500 dtex, 350-4,000 dtex, 350-3,000 dtex, 350-2,000 dtex, 350-1,500 dtex, 350-1,000 dtex, 350-800 dtex, 350-700 dtex, or 250-500 dtex may also be used.
[0095] In one embodiment of the multifilament, when the fibers are used in sanitary products, the fineness of the multifilament is preferably 90 to 2,000 dtex. Furthermore, in one embodiment of the multifilament, when the fibers are used in sanitary products described later, the fineness of the multifilament may be within the ranges of the fineness of the multifilament described above, and among them, for example, it may be 90 to 1,500 dtex, 90 to 1,000 dtex, 90 to 800 dtex, or 90 to 700 dtex. When the fibers are used in sanitary products, from the viewpoint of easily improving the heat resistance of the multifilament, in one embodiment of the multifilament, the fineness of the multifilament is more preferably 150 to 1,500 dtex, even more preferably 250 to 1,500 dtex, and even more preferably 350 to 1,500 dtex.
[0096] In one aspect of the multifilament described above, when the fiber is used in clothing, the fineness of the multifilament may be within the ranges described above for the fineness of the multifilament, including, for example, 0.3 to 300 dtex, 0.3 to 250 dtex, 0.3 to 200 dtex, 0.3 to 100 dtex, 0.3 to 50 dtex, 0.5 to 300 dtex, 0.5 to 250 dtex, 0.5 to 200 dtex, 0.5 to 100 dtex, 0.5 to 50 dtex, 1 to 300 dtex, 1 to 250 dtex, and 1 to 200 dtex. , 1-100 dtex, 1-50 dtex, 5-300 dtex, 5-250 dtex, 5-200 dtex, 5-100 dtex, 5-50 dtex, 10-300 dtex, 10-250 dtex, 10-200 dtex, 10-100 dtex, 10-50 dtex, 15-300 dtex, 15-250 dtex, 15-200 dtex, 15-100 dtex, 15-50 dtex, 20-300 dtex, 20-250 dtex, 20-200 dtex, 20-100 dtex, or 20-50 dtex.
[0097] In one embodiment of the present invention, after obtaining a multifilament by spinning, the multifilament may be further divided. The method of division is, for example, to use a fiber divider to divide the obtained multifilament into one or more monofilaments, thereby obtaining a new multifilament or a single monofilament with a finer fineness than the fineness of the entire multifilament before division. For example, a multifilament consisting of 12 monofilaments obtained by spinning can be divided into four parts using a fiber divider so that each multifilament consists of three monofilaments, and then wound up to obtain four new multifilaments, each consisting of three monofilaments.
[0098] The second hysteresis loss, determined by a tensile stretch cycle test performed in the 0-200% elongation range of the multifilament, is preferably 50% or less. A second hysteresis loss of 50% or less of the multifilament tends to result in good stretch properties, which is preferable from the viewpoint of improving holding performance when used, for example, in gathered members described later. For the same reason, the second hysteresis loss is more preferably 40% or less, even more preferably 30% or less, even more preferably 20% or less, and even more preferably 15% or less. There is no particular limit to the lower limit of the second hysteresis loss, but for example, the second hysteresis loss may be 5% or more, or 10% or more. As described above, these stepwise lower and upper limits can be combined independently. For example, in one embodiment of the multifilament, the second hysteresis loss may be 5-50%, 5-40%, 5-30%, 5-20%, 5-15%, 10-50%, 10-40%, 10-30%, 10-20%, or 10-15%. The second hysteresis loss can be measured by the method described in the examples.
[0099] [Nonwoven Fabric] A nonwoven fabric according to one aspect of the present invention includes the aforementioned fibers. The method for manufacturing the nonwoven fabric is not particularly limited, and known methods can be used. Examples include the resin bonding method, the thermal bonding method, the spunlace method, the spunbond method, the meltblown method, and the nanofiber method. The manufactured nonwoven fabric can be used as a nanofiber nonwoven fabric, a resin bonded nonwoven fabric, a thermal bonded nonwoven fabric, a spunlace nonwoven fabric, a spunbond nonwoven fabric, a meltblown nonwoven fabric, or a nanofiber nonwoven fabric. For example, it may be a laminate of the various nonwoven fabrics, such as a three-phase laminate of spunbond nonwoven fabric / meltblown nonwoven fabric / spunbond nonwoven fabric (abbreviated as "SMS nonwoven fabric"). In this case, it is sufficient to include at least one layer of the aforementioned nonwoven fabric, and the nonwoven fabrics forming the other layers may be other nonwoven fabrics, such as polypropylene nonwoven fabric. In one embodiment of the nonwoven fabric, the fibers and preferred embodiments thereof included in the nonwoven fabric are the same as those described above in the "Fibers" section.
[0100] [Gathering Member] A gathering member according to one aspect of the present invention includes the fiber. Since the fiber has good elasticity, when used as a component of a body-worn member such as a disposable diaper, for example, it is expected to provide comfort and a good fit to the user while ensuring good wearability. More specifically, preferred examples include its use in gathering members such as waist gathers and side leak prevention gathers. The gathering member is preferably a form in which the fiber and a nonwoven fabric mainly made of polyolefin such as polypropylene nonwoven fabric are joined together. As one aspect of the gathering member, it may be a multilayer structure in which the fiber is sandwiched, such as nonwoven fabric / fiber / nonwoven fabric. A laminate such as SMS nonwoven fabric may be used as the nonwoven fabric. The nonwoven fabric and the fiber may be welded together, or, in the case of a multilayer structure in which the fiber is sandwiched, such as nonwoven fabric / fiber / nonwoven fabric, the fiber may be indirectly incorporated by bonding or welding the nonwoven fabrics that sandwich the fiber together. For the bonding or welding described above, for example, a method may be used in which a hot melt adhesive is applied to the fibers, the nonwoven fabric, or both, and bonded or welded to each other. For example, a method may be used in which the fibers or the nonwoven fabric, or both, are heated by ultrasound and welded to each other. The fibers used in the gathering member may be used in the form of the multifilament. That is, the fibers used in the gathering member may be used as fibers included in the multifilament, and it is preferable to use them as fibers included in the multifilament. In one embodiment of the gathering member, the fibers and preferred forms thereof included in the gathering member are the same as those described above in the "Fibers" section. Similarly, in one embodiment of the gathering member, the multifilament and preferred forms thereof that may be included in the gathering member are the same as those described above in the "Multifilament" section.
[0101] One aspect of the present invention includes sanitary products such as disposable diapers and sanitary napkins using the fiber as an elastic member; ear loops for masks; and the fiber used in these applications may also be used in the form of the multifilament. That is, the fiber used in each of these applications may also be used as a fiber included in the multifilament. The fiber that can be used in each of these applications and its preferred form are the same as those described above in the "Fiber" section. Similarly, the multifilament that can be used in each of these applications and its preferred form are the same as those described above in the "Multifilament" section. Examples of sanitary products using the fiber as an elastic member include, preferably, disposable diapers and sanitary napkins using the fiber as an elastic member, and more preferably, disposable diapers and sanitary napkins to which the gather member is applied.
[0102] [Other Uses] One aspect of the present invention is a fabric containing the fibers. Examples of the fabric include woven fabrics, knitted fabrics, lace, nets, etc. Nonwoven fabrics are also a type of fabric. The fabric is not limited to a planar form, but may be bag-shaped, tubular, etc. The fabric may be composed only of the fibers, or it may be composed of the fibers and other fibers other than the fibers (hereinafter also referred to as "other fibers"). The other fibers can be appropriately selected depending on the use of the fabric and are not particularly limited, but examples include nylon synthetic fibers; polyester synthetic fibers; acrylic fibers; polyurethane synthetic fibers; polyolefin synthetic fibers such as polypropylene fibers; acetate; regenerated fibers such as rayon; natural fibers made from cotton, hemp, bamboo, paper, wool, etc. The fibers and other fibers constituting the fabric may each be used independently, one type alone, or two or more types may be used. When using both the aforementioned fibers and the aforementioned other fibers, the fabric may be formed by combining each fiber individually, for example, in interwoven or interknitted fabrics; the fabric may also be formed from a yarn in which the aforementioned fiber, placed in the center, is used as a core yarn (bare yarn), and other fibers are wrapped around the surface of that yarn, such as in core-spun yarn or covering yarn; the fabric may also be formed using a yarn made by twisting together two or more of the aforementioned fibers, or at least two or more selected from the group consisting of the aforementioned fibers, the aforementioned other fibers, and the covered yarn, such as in ply yarn; as long as the aforementioned fibers are included, there are no particular restrictions, and the fabric may be formed by combining two or more of the yarns described herein. The fibers forming the fabric may also be used as the multifilament.
[0103] There are no particular restrictions on the uses of the aforementioned fabric, but examples include the apparel field; the sports and leisure field; the medical and healthcare field; etc. One example of the uses of the aforementioned fabric is sanitary products, clothing (including functional wear such as swimwear and sportswear), supporters, medical support bands, elastic bandages, fixing belts, straps, and car seat covers, among which it is preferable to use it as a sanitary product or clothing. In one embodiment of the present invention, a sanitary product or clothing containing the aforementioned fabric is provided. In one embodiment of the present invention, a sanitary product or clothing containing the aforementioned fibers is provided. In one embodiment of the present invention, a sanitary product or clothing containing the aforementioned multifilament is provided. Examples of the aforementioned sanitary products include disposable diapers and sanitary products. Examples of the aforementioned clothing include clothing such as tops, bottoms, outerwear, innerwear, and socks; upper components of footwear such as shoes; headwear such as hats; and accessories such as gloves, scarves, mufflers, belts, and bags.
[0104] The embodiments of this model will be described in more detail below with reference to examples and comparative examples, but the embodiments are not limited to the following examples.
[0105] [Evaluation of physical properties of block copolymers and resins containing block copolymers] The properties of the block copolymers and resins containing block copolymers used in each example and comparative example were evaluated by the following method.
[0106] <Number-average molecular weight (Mn), weight-average molecular weight (Mw), and molecular weight distribution (Mw / Mn)> The following items were measured by GPC (gel permeation chromatography). Specifically, for each block copolymer after hydrogenation, the number-average molecular weight (Mn), weight-average molecular weight (Mw), and molecular weight distribution (Mw / Mn) were determined by GPC in terms of molecular weight equivalent to standard polystyrene. ・Weight-average molecular weight (Mw) of polymer block (A) and polymer block (B) ・Weight-average molecular weight (Mw) of triblock copolymer (I) and diblock copolymer (II) ・Molecular weight distribution (Mw / Mn) of triblock copolymer (I) and diblock copolymer (II) In Production Example 1, the weight-average molecular weight (Mw) of each polymer block before hydrogenation, as well as the weight-average molecular weight (Mw) of triblock copolymer (I) and diblock copolymer (II), were also measured. The weight-average molecular weight (Mw) of each polymer block in each block copolymer was determined by measuring the sampled liquid each time polymerization of each polymer block was completed during the manufacturing process. The measurement equipment and conditions were as follows: • Equipment: Tosoh Corporation GPC instrument "HLC-8320GPC" • Separation column: Two Tosoh Corporation columns "TSKgel® SuperHZ4000" connected in series. • Eluent: Tetrahydrofuran • Eluent flow rate: 0.35 mL / min • Sample concentration: 5 mg / 10 mL • Column temperature: 40°C • Detector: RI (differential refractive index) detector
[0107] <Content of Polymer Block (A) and the Content Ratio of Polymer Block (A) and Polymer Block (B)> The content of polymer block (A) in the total 100% by mass of polymer block (A) and polymer block (B), and the content ratio of polymer block (A) and polymer block (B) in the total 100% by mass of polymer block (A) and polymer block (B) in each block copolymer [polymer block (A): polymer block (B)] (mass ratio) were calculated by the following method. However, for block copolymers CX-1 and CX-2, the content ratio of "styrene-containing polymer block" rather than "polymer block (A)" was calculated. Block copolymers CX-1 and CX-2 do not have α-methylstyrene units and therefore do not have "polymer block (A)", but for convenience, in Table 1 below, information on styrene-containing polymer block is listed in the section where information on polymer block (A) is listed. Each block copolymer was dissolved in deuterated chloroform solvent (CDCl 3 Dissolve in ) 1 ¹H-NMR measurements were performed [equipment: "AVANCE III 400 NanoBay" (manufactured by Bruker), measurement temperature: 30°C, reference substance: tetramethylsilane (hereinafter also referred to as "TMS")]. (Regarding block copolymer X-1) 1 The ratio (molar ratio) of polymer block (A) and polymer block (B) was calculated from the ratio of the peak area derived from structural units derived from α-methylstyrene and the peak area derived from structural units derived from butadiene, which appear in the 6.2–7.5 ppm range of the spectrum obtained by 1H-NMR measurement. Then, the content ratio (mass ratio) of polymer block (A) and polymer block (B) shown in Table 1 below was calculated by multiplying the calculated molar ratio of each polymer block by the molecular weight of the repeating units derived from the polymerizable monomers constituting each polymer block (molecular weight of repeating units derived from α-methylstyrene for polymer block (A) = 118, molecular weight of repeating units derived from butadiene for polymer block (B) = 54). (For block copolymers CX-1 and CX-2) 1The ratio (molar ratio) of each polymer block was calculated from the ratio of the peak area derived from styrene-derived structural units and the peak area derived from butadiene-derived structural units appearing at 6.2–7.5 ppm in the spectrum obtained by 1H-NMR measurement. Then, by multiplying the calculated molar ratio of each polymer block by the molecular weight of the repeating units derived from the polymerizable monomers constituting each polymer block (molecular weight of styrene-derived repeating units = 104 for polymer blocks containing styrene, and molecular weight of butadiene-derived repeating units = 54 for polymer block (B)), the content ratio (mass ratio) of styrene-containing polymer blocks and polymer block (B) shown in Table 1 below was calculated.
[0108] <Hydrogenation Rate> The hydrogenation rate of each block copolymer was calculated using the following method. Unhydrogenated block copolymer and hydrogenated block copolymer were each dissolved in deuterated chloroform (CDCl). 3 Dissolve in ) 1 ¹H-NMR measurements were performed [equipment: "AVANCE III 400 NanoBay" (Brker), measurement temperature: 30°C, reference material: TMS]. (For block copolymer X-1) 1 The hydrogenation rate (mol%) was calculated from the peaks derived from α-methylstyrene appearing at 6.2–7.5 ppm and the proton peaks from the carbon-carbon double bond appearing at 4.5–6.0 ppm in the spectra obtained by 1H-NMR measurement, using the following formula: Hydrogenation rate (mol%) = {1 - (Ratio of peak area derived from carbon-carbon double bond to peak area derived from α-methylstyrene in the hydrogenated block copolymer) / (Ratio of peak area derived from carbon-carbon double bond to peak area derived from α-methylstyrene in the unhydrogenated block copolymer)} × 100 (For block copolymers CX-1 and CX-2) 1The hydrogenation rate (mol%) was calculated from the peaks derived from styrene appearing at 6.2–7.5 ppm and the proton peaks from the carbon-carbon double bond appearing at 4.5–6.0 ppm in the spectrum obtained by 1H-NMR measurement, using the following formula: Hydrogenation rate (mol%) = {1 - (Ratio of peak area derived from carbon-carbon double bond to peak area derived from styrene in the hydrogenated block copolymer) / (Ratio of peak area derived from carbon-carbon double bond to peak area derived from styrene in the unhydrogenated block copolymer)} × 100
[0109] <Vinyl Bond Amount> The amount of vinyl bonds in each block copolymer was calculated using the following method: The block copolymer before hydrogenation was dissolved in deuterated chloroform (CDCl). 3 (dissolve in) 1 ¹H-NMR measurements were performed [instrument: "AVANCE III 400 NanoBay" (Brker), measurement temperature: 30°C, reference substance: TMS]. The amount of vinyl bonding was calculated from the ratio of the peak area corresponding to the 1,2-bonding unit in the butadiene structural unit to the total peak area of the structural units derived from butadiene.
[0110] <Shear viscosity of block copolymers or resins containing block copolymers> In accordance with ISO 11443:2005, using a capillary rheometer (Instron "CEAST SR20" (capillary die length (L) = 10 mm, capillary die inner diameter (D) = 1 mm)), the shear rate of the block copolymer or resin containing block copolymer was measured at a set temperature of 270°C and a preheating time of 5 minutes after sample filling, at 1,500 s. -1 The shear viscosity (apparent viscosity, as pressure loss was not measured) was determined at a shear rate of 1,500 s. -1 The shear viscosity in the block copolymer or resin containing the block copolymer is measured at a shear rate of 1,500 s at 270°C. -1 This was adopted as the shear viscosity in the given context.
[0111] <Order-to-Disorder Transition Temperature (ODT)> A sheet-like molded body (150 mm long, 150 mm wide, 1 mm thick) was obtained by compression molding a resin containing the copolymer used in the examples and comparative examples described later (including a form in which the copolymer content is 100% by mass of the total amount of resin) at 200°C and 1.0 MPa for 3 minutes. A cylindrical test piece with a diameter of 25 mm and a height of 1 mm was punched out from this sheet, and the storage modulus G' was measured using the following apparatus and conditions in accordance with JIS K7244-10:2005. From the obtained data, a chart (α) was created with the storage modulus G' on a logarithmic scale on the vertical axis and temperature (°C) on the horizontal axis. The temperature at which G' rapidly decreases in chart (α) was defined as the order-to-disorder transition temperature (ODT). The specific value of ODT was determined by finding the intersection point (point P in Figure 1) in accordance with Figure 95, which relates to the definition of number 5113 (term: intersection point) in the table of JIS B0103:2015 (spring terminology), for the obtained chart, and the temperature at point P was taken as the order-to-disorder transition temperature (ODT). • Apparatus: ARES-G2 (manufactured by TA Instruments Co., Ltd.) • Parallel plate: 25 mm diameter • Vibration mode: Torsional vibration mode • Strain amount: 0.1% • Frequency: 1 Hz • Measurement temperature: 50°C to 350°C • Heating rate: 3°C / min • Atmosphere: Nitrogen gas stream
[0112] [Production of Block Copolymers] <Production Example 1: Production of Block Copolymer X-1> 4.58 kg of α-methylstyrene, 6.47 kg of cyclohexane, and 0.13 kg of tetrahydrofuran were charged into a nitrogen-purged pressure vessel with a stirring device. 0.39 kg of sec-butyllithium (10.5% by mass cyclohexane solution) was added to this mixture, and polymerization was carried out at -10°C for 3 hours to form poly-α-methylstyrene. The weight-average molecular weight (Mw) of the obtained poly-α-methylstyrene was 6,600, and the polymerization conversion rate was 89%. Next, 0.44 kg of 1,3-butadiene (1) was added to this reaction mixture, and polymerization was carried out by stirring at -10°C for 30 minutes, after which 36.58 kg of cyclohexane was added. At this point, the polymerization conversion rate of α-methylstyrene was 89%, and the number-average molecular weight (GPC measurement, equivalent to standard polystyrene) of the formed polybutadiene block was 3,700. 1The amount of vinyl bond determined by 1H-NMR measurement was 81 mol%. Next, 11.05 kg of 1,3-butadiene(2) was added to this reaction solution, and the polymerization reaction was carried out at 50°C for 2 hours. The weight-average molecular weight (Mw) of the resulting polybutadiene block copolymer was 29,800. 1 The amount of vinyl bond determined by H-NMR measurement was 43 mol%. Next, 0.062 kg of phenyl benzoate was added to this polymerization reaction solution and stirred at 50°C for 1 hour to obtain block copolymer x-1 containing poly-α-methylstyrene-polybutadiene-poly-α-methylstyrene triblock copolymer and poly-α-methylstyrene-polybutadiene diblock copolymer. At this time, the weight ratio of poly-α-methylstyrene-polybutadiene-poly-α-methylstyrene triblock copolymer (weight-average molecular weight (Mw) = 78,500) and poly-α-methylstyrene-polybutadiene diblock copolymer (weight-average molecular weight (Mw) = 36,000) was calculated from the area ratio of RI (differential refractive index) in GPC to be 90% by mass of the triblock copolymer and 10% by mass of the diblock copolymer. 1¹H-NMR analysis revealed that the total content of poly-α-methylstyrene blocks (polymer blocks (A1) and (A2)) in the poly-α-methylstyrene-polybutadiene-poly-α-methylstyrene triblock copolymer and poly-α-methylstyrene-polybutadiene diblock copolymer was 29% by mass, and the vinyl bond content of the polybutadiene blocks (polymer blocks (B1) and (B2)) was 43 mol%. To the polymerization reaction solution obtained above, a Ziegler-type hydrogenation catalyst formed from nickel octoate and triisobutylaluminum was added under a hydrogen atmosphere, and a hydrogenation reaction was carried out at a hydrogen pressure of 1 MPa and 80°C for 5 hours to obtain block copolymer X-1 containing poly-α-methylstyrene-(polyethylene-polybutylene)-poly-α-methylstyrene triblock copolymer (αSEBαS) [hereinafter abbreviated as triblock copolymer (I)-1] and poly-α-methylstyrene-(polyethylene-polybutylene) diblock copolymer (αSEB) [hereinafter abbreviated as diblock copolymer (II)-1]. From the area ratio of RI in the GPC of block copolymer X-1, it was found that triblock copolymer (I)-1 was present at 90% by mass and diblock copolymer (II)-1 at 10% by mass, based on the total amount of each block copolymer contained in block copolymer X-1 (100% by mass). Furthermore, GPC measurements of block copolymer X-1 revealed that the number-average molecular weight (Mn) of triblock copolymer (I)-1 was 78,500, the weight-average molecular weight (Mw) was 80,200, and the molecular weight distribution (Mw / Mn) was 1.02. The number-average molecular weight (Mn) of diblock copolymer (II)-1 was 36,000, the weight-average molecular weight (Mw) was 38,400, and the molecular weight distribution (Mw / Mn) was 1.07. As shown in Table 1 below, the overall weight-average molecular weight (Mw) of block copolymer X-1 was 76,300. 1¹H-NMR measurements revealed that the hydrogenation rates of polymer block (B1) and polymer block (B2) were 98.0 mol%, respectively. That is, the hydrogenation rates of triblock copolymer (I)-1 and diblock copolymer (II)-1 were 98.0 mol%, respectively. Since the block copolymer X-1 obtained in Production Example 1 uses only α-methylstyrene and 1,3-butadiene as polymerizable monomers, the value of the content of polymer block (A) in the total 100% by mass of polymer block (A) and polymer block (B), calculated by the method described above, is also the value of the content of polymer block (A) in the total 100% by mass of the block copolymer X-1. Therefore, the statement "The total content of poly-α-methylstyrene blocks (polymer blocks (A1) and (A2)) in the poly-α-methylstyrene-polybutadiene-poly-α-methylstyrene triblock copolymer and poly-α-methylstyrene-polybutadiene diblock copolymer is 29% by mass" is also the value of the content of polymer block (A) in 100% by mass of the total amount of the block copolymer X-1. Accordingly, in Table 1 below, the value of [polymer block (A):polymer block (B)] (mass ratio) = 29:71 represents the content (mass%) of polymer block (A) and polymer block (B) in 100% by mass of the total amount, respectively, and also coincides with the values of the content (mass%) of polymer block (A) and polymer block (B) in 100% by mass of the total amount of the block copolymer X-1, respectively.
[0113] <Production Example 2: Production of Block Copolymer CX-1> In a nitrogen-purged and dried pressure vessel, 26.7 kg of cyclohexane was charged as the solvent, 0.097 kg of sec-butyllithium (10.5% by mass cyclohexane solution) as an anionic polymerization initiator, and 0.043 kg of tetrahydrofuran as a polar compound. After raising the temperature inside the pressure vessel to 50°C, 1.32 kg of styrene(1) was added and polymerization was carried out for 60 minutes, then 6.22 kg of 1,3-butadiene(1) was added and polymerization was carried out for 2 hours. Subsequently, 1.32 kg of styrene(2) was added and polymerization was carried out for 60 minutes, and methanol was added to stop the reaction, obtaining a reaction solution containing polystyrene-polybutadiene-polystyrene triblock copolymer (SBS). To the reaction solution, a Ziegler-type hydrogenation catalyst formed from nickel octyolate and triisobutylaluminum was added under a hydrogen atmosphere, and a hydrogenation reaction was carried out at a hydrogen pressure of 1 MPa and 80°C for 5 hours. After allowing the reaction solution following the hydrogenation reaction to cool and release pressure, the hydrogenation catalyst was removed by washing with water, and the mixture was vacuum-dried to obtain a hydrogenated product (SEBS) (block copolymer CX-1) in which the polymer backbone is a polystyrene-(polyethylene-polybutylene)-polystyrene triblock copolymer. The block copolymer CX-1 obtained in Production Example 2 uses only styrene and 1,3-butadiene as polymerizable monomers. Therefore, in Table 1 below, the value of [styrene-containing polymer block: polymer block (B)] (mass ratio) = 30:70 represents the content (mass%) of styrene-containing polymer block and polymer block (B) in a total of 100% by mass, respectively, and also coincides with the content (mass%) of styrene-containing polymer block and polymer block (B) in a total of 100% by mass of the block copolymer CX-1, respectively.
[0114] <Production Example 3: Production of Block Copolymer CX-2> In a nitrogen-purged and dried pressure vessel, 50.0 kg of cyclohexane (solvent) and 0.086 kg of a cyclohexane solution of sec-butyllithium at a concentration of 10.5% by mass as an anionic polymerization initiator (substantial amount of sec-butyllithium added: 9.03 g) were charged. After raising the temperature inside the pressure vessel to 50°C, 0.90 kg of styrene (1) was added and polymerization was carried out for 60 minutes, then 0.34 kg of 1,3-butadiene (1) was added and polymerization was carried out for 2 hours, then 0.11 kg of tetrahydrofuran as a polar compound was added, and 6.42 kg of 1,3-butadiene (2) was added and polymerization was carried out for 2 hours. After that, 1.35 kg of styrene (2) was added and polymerization was carried out for 60 minutes, and methanol was added to stop the reaction, obtaining a reaction solution containing a block copolymer having a polystyrene-polybutadiene-polystyrene (SBS) polymer backbone. A Ziegler-type hydrogenation catalyst formed from nickel octoate and triisobutylaluminum was added to the reaction solution under a hydrogen atmosphere, and the reaction was carried out for 5 hours under conditions of a hydrogen pressure of 1 MPa and 80°C. After the reaction solution was allowed to cool and the pressure was released, the catalyst was removed by washing with water, and the mixture was vacuum-dried to obtain block copolymer CX-2, in which the polymer backbone is polystyrene-(polyethylene-polybutylene)-polystyrene (SEBS). The block copolymer CX-2 obtained in Production Example 3 uses only styrene and 1,3-butadiene as polymerizable monomers. Therefore, in Table 1 below, the value [styrene-containing polymer block: polymer block (B)] (mass ratio) = 25:75 represents the content (mass%) of styrene-containing polymer block and polymer block (B) in a total of 100% by mass, respectively, and also coincides with the content (mass%) of styrene-containing polymer block and polymer block (B) in a total of 100% by mass of the block copolymer CX-2.
[0115]
[0116] [Evaluation of Fiber Properties] The properties of the fibers obtained in each of the examples and comparative examples described later, as well as the fiber in Reference Example 1, were evaluated by the following method.
[0117] <Melt Spinning Properties> As described in each example and comparative example, melt spinning was performed, and when winding onto a paper tube at the winding speed in each example, the melt spinning properties were evaluated based on the spinning conditions during melt spinning according to the following criteria. The results are shown in Tables 2 and 3 below. ・OK: The spun multifilament could be wound without breaking for 10 minutes from the start of winding, and was at a level that was acceptable for practical use. ・NG: The spun multifilament broke within 10 minutes from the start of winding, and winding could not be continued, and was at a level unsuitable for practical use.
[0118] <Removability> After spinning in each example and comparative example, the yarn wound onto a paper tube was stored at 30°C for one week. Then, the multifilament was manually unfurled from the paper tube. If it could be unfurled without resistance, the removal of the removability was considered "OK". If the multifilament got stuck or stuck and could not be unfurled, it was considered "NG". The results are shown in Tables 2 and 3 below.
[0119] <Fineness> The mass of each multifilament obtained in each example and comparative example was measured, and the fineness of each multifilament was calculated based on the following formula. The results are shown in Tables 2 and 3 below. Fineness (dtex) = Mass of 1 m of multifilament (g) × 10,000 (m) In Table 2 below, for example, the notation "500 / 12F" for the fineness in Example 1 indicates that the fineness of the multifilament obtained by simultaneously extruding and winding 12 single fibers (monofilaments) from the same nozzle is 500 (dtex). In other words, in Example 1, a multifilament consisting of 12 single fibers is spun, and the fineness of each single fiber constituting the multifilament is calculated as 500 (dtex) ÷ 12 (fibers) = 41.7 (dtex).
[0120] <Tensile Test> (Breaking Strength and Elongation at Breaking) The multifilaments obtained in each example and comparative example were cut to a length of 50 mm using scissors, and the number of multifilaments indicated in Table 2 or 3 below were bundled together to form the test sample. However, for Reference Example 1, the polyurethane elastic fiber "creora® Comfort 800Dtex" manufactured by HYOSUNG Corporation was cut to a length of 50 mm using scissors and used as the test sample. The test sample was then attached to the pneumatic grips of the precision universal testing machine "Autograph® AGX®-V" (manufactured by Shimadzu Corporation) equipped with a 50 N load cell (grip distance 50 mm), and the measurement started at the point where a load of 0.1 cN was applied to the test sample to remove deflection. At this time, the fluctuations between the grips were automatically corrected by the testing machine, and the displacement (strain) at the point where a load of 0.1 cN was applied to the test sample (measurement start point) was corrected to 0%. Next, a tensile test was performed by stretching the test sample at a tensile speed of 200 mm / min from the measurement start point until it broke, and the breaking strength and breaking elongation were measured. Higher values for breaking strength and breaking elongation indicate better tensile properties.
[0121] <Cycle Test> For each example and comparative example, a test sample was prepared in the same manner as the tensile test described above. The test sample was then attached to a pneumatic grip (grip distance 50 mm) on a precision universal testing machine "Autograph® AGX®-V" (manufactured by Shimadzu Corporation) equipped with a 50 N load cell. To remove deflection, the measurement started at the point where a load of 0.1 cN was applied to the test sample. At this time, the machine automatically corrected for fluctuations between the grips, and corrected the displacement (strain) at the point where a load of 0.1 cN was applied to the test sample (measurement start point) to 0%. Next, from the measurement start point, the test sample was stretched (tensile) at a tensile speed of 200 mm / min until the strain reached 200%, held at 200% strain for 30 seconds, and then returned to its original state at a speed of 200 mm / min until the strain reached 0%. The same test sample was subjected to the aforementioned procedure twice while still attached to the grip. From the chart obtained by the measurement (an example is shown in Figure 2), the stress when the strain reached 200% during the second extension ("2nd forward 200% stress") and the stress when the strain reached 50% during the second contraction ("2nd return 50% stress") were determined. Then, from the area of the region enclosed by the points 2-1 (origin), 2-2 (position corresponding to the stress when the strain reached 200% during the second extension), 2-3 (position corresponding to the stress at 200% strain when contraction begins after the second extension), 2-4 (position where the stress reaches zero during the second contraction), and 2-1 (S1), and the area connecting 2-1, 2-2, 2-5 (positions on the horizontal axis representing strain where the strain is 200%) and 2-1 (S2), the 2nd hysteresis loss was calculated using the following formula. Second hysteresis loss (%) = (S1) / (S2) × 100 The cycle characteristics obtained when the above test sample is subjected to cycle testing are preferably such that the second forward 200% stress is low from the viewpoint of reducing discomfort due to strong tightening, and that the second return 50% stress is high to improve holding performance, and furthermore, that the second hysteresis loss is small.
[0122] <Stress Retention Rate> For each example and comparative example, a test sample was prepared in the same manner as the tensile test described above. The test sample was then attached to pneumatic grips (50 mm distance between grips) in a precision universal testing machine "Autograph® AGX®-V" (manufactured by Shimadzu Corporation) equipped with a 50 N load cell and a constant temperature chamber maintained at 40°C. To remove deflection, the measurement started at the point where a load of 0.1 cN was applied to the test sample. At this time, the fluctuation between the grips was automatically corrected by the testing machine, and the displacement (strain) at the point where a load of 0.1 cN was applied to the test sample (measurement start point) was corrected to 0%. Next, from the measurement start point, the test sample was stretched at a tensile speed of 200 mm / min until the strain of the test sample reached 50%, and the test sample was held in this 50% strain state for 2 hours. The stress retention rate was then calculated using the following formula. A high stress retention rate of the fiber is preferable from the viewpoint of maintaining its holding properties for a long period of time. Stress retention rate (%) = Stress after 2 hours of 50% elongation / Stress immediately after 50% elongation × 100
[0123] <Heat Resistance> The multifilaments obtained in each example and comparative example were each cut to a length of 70 mm using scissors and used as test samples. For Reference Example 1, the polyurethane elastic fiber "creora® Comfort 800Dtex" manufactured by HYOSUNG Corporation was cut to a length of 70 mm using scissors and used as a test sample. The ends of the test sample were then fixed to the fixing part and the outer jaw part of the slider of a standard caliper with clips so that the distance between the fixing points was 50 mm. The outer jaw part of the slider of the caliper was then slid to a length where the elongation rate (strain) of the test sample was 100%, and the slider was then fixed with a set screw. In this state, the temperature at which the test sample was not cut by heat was checked when the center of the elongated test sample was in contact with a hot plate for 1 second. The temperature of the hot plate was increased in increments of 10°C from 80°C up to 140°C and checked. For example, if a test sample does not cut at 110°C but does cut at 120°C, the heat resistance is considered to be 110°C and is indicated as "110" in Tables 2 and 3 below. Furthermore, in Table 2 below, if the test sample does not cut even at 140°C, it is indicated as ">140".
[0124] <Evaluation of Laminating Properties> (Evaluation of Laminating Properties of Hot Melt Adhesive) The multifilaments (test samples) obtained in each example and comparative example were fed out from the paper tube at a speed of 100 m / min, and with the test samples stretched to 200%, a styrene-butadiene-styrene copolymer (SBS) hot melt adhesive was applied through the V-comb head of the hot melt laminating test machine at a coating rate of 0.05 g / m at a V-comb head temperature of 120°C. Then, a base weight of 20 g / m was applied from the top and bottom of the hot melt-coated multifilament. 2Gathered components were manufactured by sandwiching the material between SMS nonwoven fabrics (a laminate of spunbond / meltblown / spunbond, each layer made of polypropylene) and passing it through a pressure roll. For Reference Example 1, HYOSUNG's polyurethane elastic fiber "creora® Comfort 800Dtex" was used as a test sample. Based on the conditions during the hot melt adhesive lamination test, the lamination properties when using hot melt adhesive were evaluated according to the following criteria. For those samples that could be laminated with hot melt adhesive, the feel of the resulting gathered components was evaluated according to the following criteria. [Lamination Properties (120°C)] ・OK: The test sample was not cut by the application of the hot melt adhesive, and lamination was possible. ・NG: The test sample was cut by the application of the hot melt adhesive, and lamination was impossible. [Gathering feel] ・A: Even after repeated stretching and contraction, the nonwoven fabric and the test sample did not separate, and the gathered state was maintained. ・B: After repeated stretching and contraction, the nonwoven fabric and the test sample separated after a few times, and the gathered state could not be maintained. ・NG: The test sample was not cut, but it could not be fixed to the nonwoven fabric, or the test sample could be fixed to the nonwoven fabric, but compared to the gathered members rated "A" and "B", the gathered member was hard and had poor elasticity, making it unsuitable for practical use.
[0125] (Evaluation of ultrasonic lamination properties) The multifilaments (test samples) obtained in each example and comparative example were cut to a length of 100 mm using scissors and used as test samples. For Reference Example 1, the polyurethane elastic fiber "creora® Comfort 800Dtex" manufactured by HYOSUNG Corporation was cut to a length of 100 mm using scissors and used as a test sample. With the test sample stretched to 100-200%, a basis weight of 20 g / m was measured from the top and bottom of the multifilament test sample. 2The SMS nonwoven fabric (a laminate of spunbond / meltblown / spunbond, each layer made of polypropylene) was sandwiched between layers and placed on the anvil (receiving fixture) of an ultrasonic lamination tester. The anvil had 3.0 mm grooves drilled at 1.0 mm intervals, and grooves perpendicular to these grooves were drilled at 0.05 mm intervals from 0.15 to 0.35 mm. In this test, the 0.15 mm groove was used, and the laminate of SMS nonwoven fabric / test sample / SMS nonwoven fabric was positioned so that the test sample was placed in this groove. Then, ultrasonic waves were generated by pressing from above with an ultrasonic horn, which heated the polypropylene in the SMS nonwoven fabric, welding the SMS nonwoven fabrics together at the protruding parts that were pressed against the horn, excluding the grooves. At this time, the multifilament test sample was caught between the welded parts of the SMS nonwoven fabrics, causing the laminate to gather and thus producing a gathered member. Based on the conditions during the ultrasonic lamination test, the lamination properties using ultrasound were evaluated according to the following criteria. For materials that could be ultrasonically laminated, the feel of the resulting gathered material was evaluated according to the following criteria. [Lamination Properties (Ultrasonic)] ・OK: Lamination by ultrasound was possible. ・NG: Lamination by ultrasound was not possible. [Gathered Feel] ・A: The gathered state was maintained even after repeated stretching and contracting. ・B: After several stretching and contracting cycles, the fibers came out and the gathered state could not be maintained. ・NG: Lamination by ultrasound was possible, but a gathered state was not achieved, or a gathered state was achieved, but the stretchability was poor compared to evaluations "A" and "B" and was not suitable for practical use.
[0126] [Fiber Manufacturing] In Tables 2 and 3, the "Resin Composition (Core)" column shows the content of each component in 100% by mass of the total amount of the core component resin, and the "Resin Composition (Sheath)" column shows the content of each component in 100% by mass of the total amount of the sheath component resin. [Example 1] The block copolymer X-1 obtained in Manufacturing Example 1 was melted in a single-screw extruder and extruded from a spinning nozzle for single-section fibers at a die temperature (spinning nozzle setting temperature; the same applies hereinafter) of 275°C. Twelve threads extruded from a spinning nozzle for single-section fibers (extrusion hole shape: round hole, number of holes: 12) were cooled to room temperature (20°C ± 15°C) using a cold air device, and then silicone oil was applied as a lubricant. Next, these twelve threads were wound onto a paper tube via a roller at a winding speed of 500 m / min to obtain a multifilament containing fibers with a single-section structure. The evaluation results of the obtained multifilament are shown in Table 2 below. Although the fiber in Example 1 has a single cross-sectional structure, for convenience, information on the raw material resin, etc., is included in the column labeled "Resin Composition (Core)".
[0127] [Example 2] Block copolymer X-1 obtained in Production Example 1 was used as the core component, and polyolefin resin Z-1 (manufactured by Tosoh Corporation, polyethylene, trade name "Petrocene (registered trademark) 212", MFR = 13 g / 10 min) was used as the sheath component. The core component and the sheath component were mixed in a mass ratio of sheath / core = 15 / 85, and each was melted in separate extruders. At a die temperature of 275°C, composite fibers having a core-sheath cross-section were extruded from a composite spinning nozzle for core-sheath type composite fibers (extrusion hole shape: round hole, number of holes: 4). The four threads extruded from the spinning nozzle were cooled to room temperature (20°C ± 15°C) using a cold air device, and then silicone oil was applied as a lubricant. Next, the threads after lubrication were wound onto a paper tube via a roller at a winding speed of 500 m / min to obtain a multifilament containing core-sheath type composite fibers. The evaluation results of the obtained multifilament are shown in Table 2 below.
[0128] [Example 3] First, the block copolymer CX-2 and oil Y-1 (product name "Diana® Process Oil PW-90", paraffin oil, manufactured by Idemitsu Kosan Co., Ltd.) obtained in Production Example 3 were prepared. These materials were supplied to a hopper using a twin-screw extruder (Coperion "ZSK26Mc"; 14 cylinders) under conditions of a cylinder temperature of 200°C and a screw rotation speed of 300 rpm. The pre-mixed composition was then melt-kneaded, extruded into strands, and cut to obtain a resin composition. Next, the resin composition was used as the core component, and the block copolymer X-1 obtained in Production Example 1 was used as the sheath component. The core component and the sheath component were mixed in a mass ratio of sheath / core = 50 / 50, and each was melted in a separate extruder. At a die temperature of 260°C, composite fibers having a core-sheath cross-section were extruded from a composite spinning nozzle for core-sheath type composite fibers (extrusion hole shape: round hole, number of holes: 4). Four threads extruded from the spinning nozzle were cooled to room temperature (approximately 20°C ± 15°C) using a cooling device, and then silicone oil was applied as a lubricant. Next, the lubricated threads were wound onto a paper tube via rollers at a winding speed of 500 m / min to obtain a multifilament containing core-sheath type composite fibers. The evaluation results of the obtained multifilament are shown in Table 2 below.
[0129] [Example 4] A multifilament containing single-section structure fibers was obtained in the same manner as in Example 1, except that the winding speed was changed to 2,000 m / min. The evaluation results of the obtained multifilament are shown in Table 3 below.
[0130] [Example 5] A multifilament containing a core-sheath type composite fiber was obtained in the same manner as in Example 2, except that the winding speed was changed to 2,000 m / min. The evaluation results of the obtained multifilament are shown in Table 3 below.
[0131] [Comparative Example 1] An attempt was made to obtain a multifilament containing single cross-sectional structure fibers at a winding speed of 500 m / min, in the same manner as in Example 1, except that block copolymer CX-1 obtained in Production Example 2 was used instead of block copolymer X-1. The die temperature was started at 270°C and increased in intervals of 5 to 10°C up to a maximum of 300°C while checking the spinning condition, and the melt spinnability was checked. However, the melt spinnability was poor at all die temperatures, and it was not possible to continuously wind the multifilament for 10 minutes. The evaluation results are shown in Table 2 below. Note that in Table 2, the die temperature is indicated as 300°C.
[0132] [Comparative Example 2] An attempt was made to obtain a multifilament containing a core-sheath type composite fiber in the same manner as in Example 2, except that block copolymer CX-1 obtained in Production Example 2 was used as the core component instead of block copolymer X-1. The die temperature was started at 270°C and increased in intervals of 5 to 10°C up to a maximum of 300°C while checking the spinning condition, and the melt spinnability was checked. However, the melt spinnability was poor at all die temperatures, and it was not possible to continuously wind the multifilament for 10 minutes. The evaluation results are shown in Table 2 below. Note that in Table 2, the die temperature is indicated as 300°C.
[0133] [Comparative Example 3] An attempt was made to obtain a multifilament containing a core-sheath type composite fiber in the same manner as in Example 3, except that block copolymer CX-1 obtained in Production Example 2 was used as the sheath component instead of block copolymer X-1. Spinning properties were confirmed at a die temperature of 260°C. However, the melt spinning properties were poor, and it was not possible to continuously wind the multifilament for 10 minutes. The evaluation results are shown in Table 2 below.
[0134] [Reference Example 1] For Comparative Example 1, the polyurethane elastic fiber "creora® Comfort 800Dtex" manufactured by HYOSUNG Corporation was used. The evaluation results are shown in Table 2 below.
[0135]
[0136]
[0137] From the results in Table 2, it was confirmed that the fibers of Examples 1 to 3, which represent one aspect of the present invention, have good melt-spinning properties, as well as good tensile and stretch properties. Furthermore, it was confirmed that they also have good heat resistance and excellent lamination properties. From the results in Table 3, it was confirmed that the fibers of Examples 4 and 5 can be melt-spun even under higher speed conditions of 2,000 m / min, and that they also have good tensile properties, stretch properties, and heat resistance. Furthermore, it was confirmed that the fibers of Examples 1, 3, and 4 have significantly lower 2nd hysteresis loss compared to the fibers of Reference Example 1, and that their stretch properties are even better. In addition, since the fibers of Examples 1 to 5, which represent one aspect of the present invention, contain a block copolymer containing a polymer block (A) containing α-methylstyrene units and a polymer block (B) containing conjugated diene compound units, it is considered that, due to their molecular structure, they have high compatibility with polyolefin materials, for example, when used together with polyolefin resin, which is the main material, such as in diaper gathers. For example, if the fiber has high compatibility with polyolefin materials, it can be expected to suppress deterioration of the physical properties and appearance defects of recycled resin. Furthermore, it is expected that the work of separating the fibers from the material can be omitted. In addition, another advantage is that it can reduce or prevent the generation of harmful gases, such as those derived from nitrogen atoms contained in polyurethane, when the material is incinerated. For this reason, the fiber according to one aspect of the present invention is considered to be useful in recycling used materials, such as polyolefin materials, compared to conventional elastic fibers such as spandex.
[0138] On the other hand, the fibers of Comparative Examples 1 to 3 had poor melt-spinning properties, and melt spinning could not be continued at a winding speed of 500 m / min, making it impossible to obtain multifilaments. Therefore, tensile and stretch properties could not be evaluated.
Claims
1. The fibers are formed from a resin comprising a block copolymer (X) in which at least a portion or all of the fibers comprises a polymer block (A) containing α-methylstyrene units and a polymer block (B) containing conjugated diene compound units, wherein the shear rate of the resin at 270°C is 1,500 s. -1 A fiber having a shear viscosity of 250 Pa·s or less.
2. The fiber according to claim 1, wherein the block copolymer (X) comprises at least one selected from the group consisting of triblock copolymers (I) and diblock copolymers (II), the triblock copolymer (I) comprises a polymer block (A1) containing α-methylstyrene units and a polymer block (B1) containing conjugated diene compound units, the polymer block (A1) and the polymer block (B1) are a triblock copolymer represented as A1-B1-A1, the structures of the two polymer blocks (A1) in the triblock copolymer (I) may be identical or different from each other, and the diblock copolymer (II) comprises a polymer block (A2) containing α-methylstyrene units and a polymer block (B2) containing conjugated diene compound units, the polymer block (A2) and the polymer block (B2) are a diblock copolymer represented as A2-B2.
3. The fiber according to claim 2, wherein the block copolymer (X) contains the triblock copolymer (I) and the diblock copolymer (II) in a mass ratio of triblock copolymer (I):diblock copolymer (II) = 92:8 to 75:
25.
4. The fiber according to claim 2 or 3, wherein the weight-average molecular weight (Mw) of the triblock copolymer (I) on a polystyrene basis is 10,000 to 2,000,000, and the weight-average molecular weight (Mw) of the diblock copolymer (II) on a polystyrene basis is 5,000 to 100,000.
5. The fiber according to any one of claims 1 to 4, wherein the block copolymer (X) contains polymer block (A) and polymer block (B) in a mass ratio of polymer block (A):polymer block (B) = 5:95 to 55:
45.
6. The fiber according to any one of claims 1 to 5, wherein the hydrogenation rate of the block copolymer (X) is 50 to 100 mol%.
7. The fiber according to any one of claims 1 to 6, wherein the order-to-disorder transition temperature (ODT) of the resin, as determined by dynamic viscoelasticity measurement, is 300°C or less.
8. The fiber according to any one of claims 1 to 7, wherein the fiber is a core-sheath type composite fiber, and the resin is included in at least one of the core and the sheath.
9. A method for producing fibers according to any one of claims 1 to 8, wherein the fibers are formed by a melt spinning method.
10. A multifilament comprising the fiber described in any one of claims 1 to 8.
11. The multifilament according to claim 10, wherein the fineness is 90 to 2,000 dtex.
12. The multifilament according to claim 10 or 11, wherein the second hysteresis loss, determined by a tensile stretch cycle test performed in the range of 0 to 200% elongation of the multifilament, is 50% or less.
13. A nonwoven fabric comprising the fibers described in any one of claims 1 to 8.
14. A gathering member comprising the fiber described in any one of claims 1 to 8.