Single and multimetallic composite catalysts for biogas conversion to syngas, chemicals, and fuels
A core-shell-shell structured catalyst with non-noble transition, alkaline earth, and inert metal oxide components addresses sintering and coking issues, ensuring stable biogas-to-syngas conversion and scalable chemical production.
Patent Information
- Application Number
- PCT/SG2026/050292
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing catalysts for biogas steam reforming face challenges such as sintering, hydrothermal instability, and coking under high-temperature and high-pressure conditions, leading to performance degradation, and the presence of CO2 affects catalyst robustness, with traditional processes being less favorable at elevated pressures.
A catalyst comprising a core-shell-shell configuration with a non-noble transition metal core, surrounded by an alkaline earth and/or rare earth metal shell, and an inert metal oxide outer shell, providing structural stability and resistance to sintering and coking, while maintaining catalytic activity under harsh conditions.
The catalyst achieves sustained catalytic activity and stability for over 400 hours, enabling efficient conversion of biogas to syngas with a desirable H2/CO ratio, suitable for downstream chemical synthesis, and supports scalable and cost-effective industrial applications.
Smart Images

Figure SG2026050292_12112026_PF_FP_ABST
Abstract
Description
SINGLE AND MULTIMETALLIC COMPOSITE CATALYSTS FOR BIOGAS CONVERSION TO SYNGAS, CHEMICALS, AND FUELSCross-Reference to Related Application
[0001] This application claims the benefit of priority of Singapore Patent Application No. 10202501178R, filed 7 May 2025, the content of it being hereby incorporated by reference in its entirety for all purposes.Technical Field
[0002] The present disclosure relates to a catalyst and a method for making the catalyst. The present disclosure also relates to a process involving the catalyst for producing chemicals from biogas.Background
[0003] Given the global climate change challenge due to increasing greenhouse gases in the environment, there may be tremendous pressure to shift away from fossil feedstocks and find alternative sustainable feedstock for chemical and fuel manufacturers. One such feedstock may be biogas produced from anaerobic digestions of various wastes (e.g., food waste, biomass, manure, wastewater). Generally, a composition of biogas may be about 60% methane and 40%> CO2. However, an efficient and effective technology for converting biogas to chemicals may be desired. Steam reforming (Equation 1) of biogas may be known to convert it into syngas (a mixture of CO and H2), which may be then used for producing chemicals, such as methanol. However, a catalyst that may withstand the conditions of steam reforming (temperature above 700°C) generally is required. Key challenges for catalysts include (1) sintering -a physical and / or thermal phenomenon that leads to agglomeration, a reduction in the surface-to-volume ratio of catalyst, (2) hydrothermal stability - stability of catalyst in the presence of water vapour and heat, and (3) coking - clogging of pores or active sites by coke produced at the time of condensation or cracking of products and reactants.
[0004] 3CH4+ CO2+ 2H2O → 4CO + 8H2(Equation 1)
[0005] Besides catalyst issues, the presence of CO2 in the feed also may induce additional issues for a catalyst’s robustness. Also, from a process economic viewpoint,it may be beneficial to conduct a reaction at elevated pressure, however, with equilibrium constraint, the forward reaction is less favored at elevated pressures.
[0006] There is thus a need to provide for a solution that addresses one or more of the limitations mentioned above. The solution should at least provide for a catalyst capable of withstanding harsh reaction conditions of steam reforming of various compositions of biogas at elevated pressures and temperatures.Summary
[0007] In a first aspect, there is a catalyst comprising:more than one metal denoted by:AxByCzwherein:A comprises at least one non-noble transition metal,B comprises at least one alkaline earth metal,C comprises at least one rare earth metal, andwherein x represents a range of 2 to 30 wt%, y represents a range of 0 to 20 wt%, and / or z represents a range of 0 to 20 wt%;andwherein the catalyst comprises a core, a first shell configured around the core, and a second shell configured outer to the first shell;wherein the core comprises A;wherein the first shell comprises B and / or C; andwherein the second shell comprises an inert metal oxide.
[0008] In another aspect, there is a method for making the catalyst described in various embodiments of the first aspect, the method comprising:forming a mixture comprising a precursor of A with an organic linker in water; andmixing the mixture with a precursor of B and / or a precursor of C.
[0009] In another aspect, there is a process for producing chemicals from biogas, the process comprising:providing a biogas; andcontacting the biogas with the catalyst described in various embodiments of the first aspect in the presence of steam.Brief Description of the Drawings
[0010] The drawings are not necessarily to scale, emphasis instead generally being placed upon illustrating the principles of the present disclosure. In the following description, various embodiments of the present disclosure are described with reference to the following drawings, in which:
[0011] FIG. 1 A is a XRD analysis plot of catalysts in its fresh form (before use in the reaction). dSin FIG. 1 denotes domain size determined by Scherrer equation.
[0012] FIG. IB is a XRD analysis plot of the same catalysts of FIG. 1A but after reaction (spent form) - used for 426 hours.
[0013] FIG. 2A shows a scanning electron microscopy (SEM) image of a sample catalyst (Ni20) with big agglomerates of no particular shape.
[0014] FIG. 2B shows the same SEM image of the catalyst of FIG. 2A, but with an energy dispersive x-ray (EDX) mapping for Si (Kai).
[0015] FIG. 2C shows the same SEM image of the catalyst of FIG. 2A, but with an energy dispersive x-ray (EDX) mapping for Ni (Lai, 2).
[0016] FIG. 2D shows a scanning electron microscopy (SEM) image of a sample catalyst (Nil3Ce6) with big agglomerates of no particular shape.
[0017] FIG. 2E shows the same SEM image of the catalyst of FIG. 2D, but with an energy dispersive x-ray (EDX) mapping for Si (Kai).
[0018] FIG. 2F shows the same SEM image of the catalyst of FIG. 2D, but with an energy dispersive x-ray (EDX) mapping for Ni (Lai, 2).
[0019] FIG. 2G shows the same SEM image of the catalyst of FIG. 2D, but with an energy dispersive x-ray (EDX) mapping for Cc (Ma).
[0020] FIG. 2H shows a scanning electron microscopy (SEM) image of a sample catalyst (Ni8Mgl2) with big agglomerates of no particular shape.
[0021] FIG. 21 shows the same SEM image of the catalyst of FIG. 2H, but with an energy dispersive x-ray (EDX) mapping for Si (Kai).
[0022] FIG. 2J shows the same SEM image of the catalyst of FIG. 2H, but with an energy dispersive x-ray (EDX) mapping for Ni (Lai, 2).
[0023] FIG. 2K shows the same SEM image of the catalyst of FIG. 2H, but with an energy dispersive x-ray (EDX) mapping for Mg (Kai, 2).
[0024] FIG. 3A is a TEM image for Ni8Mgl2 catalyst. Scale bar denotes 20 nm.
[0025] FIG. 3B is another TEM image (but at higher resolution) of the same catalyst of FIG. 3A. Scale bar denotes 2 nm.
[0026] FIG. 3C is a TEM image for the same catalyst of FIG. 3A, but with energy dispersive X-ray spectroscopy (EDS) elemental mapping, wherein SiO2, MgO and NiO were identified. Small NiO nanoparticles with domain size of about 8 nm were observed. NiO is surrounded and / or supported by MgO. Porous metal oxide matrix (SiO2) surrounds NiO and MgO. Scale bar denotes 300 nm.
[0027] FIG.4 is a table indicating properties of the various catalysts. " Determined from N2 sorption analysis.bDetermined from X-ray fluorescence analysis. " Determined from total weight loss in thermogravimetric analysis (TGA) and dividing it by total reaction time of 426 hrs.
[0028] FIG. 5 A is a plot of the catalytic performance of Ni20, Ni8Mgl 2, and Ni 13Ce6 catalysts in biogas conversion to syngas. Conditions: Space velocity = 14 (low) and 28 (high) L h-1gc t-1, temperature = 690°C, and pressure = 5 bar. Specifically, FIG. 5 A shows a plot of conversion of CH₄ and CO₂ as a function of time-on-stream under low and high space velocity conditions. At low space velocity, higher CH₄ conversion (about 50–55%) and moderate CO₂ conversion (about 8–13%) were observed. At high space velocity, both CH₄ and CO₂ conversions may decrease due to reduced residence time, but remain relatively stable over time, indicating steady catalytic performance..
[0029] FIG. 5B is a plot of the catalytic performance of Ni20, Ni8Mgl2, and Nil3Ce6 catalysts in biogas conversion to syngas. Conditions: Space velocity = 14 (low) and 28 (high) L h-1gcat-1, temperature = 690°C, and pressure = 5 bar-. Specifically, FIG. 5B shows a plot of methane conversion rate (mol CH₄ h−1gNi−1) over time under low and high space velocity conditions. The conversion rate increases significantly at higher space velocity, reflecting increased throughput. Ni8Mgl2 shows the highest activity, followed by Nil3Ce6 and Ni20, demonstrating that addition of metals further renders synergistic effect of enhancing catalytic activity. The relatively constant values over time indicate good catalyst stability.
[0030] FIG. 5C is a plot of the catalytic performance of Ni20, Ni8Mg12, and Ni13Ce6 catalysts in biogas conversion to syngas. Conditions: Space velocity = 14 (low) and 28 (high) L h-1gcat-1, temperature = 690°C, and pressure = 5 bar. Specifically, FIG. 5C shows a plot of the H₂ / CO molar ratio of the produced syngas as a function of time-onstream. The ratio remains consistently in the range of approximately 2.7-3.1 across all catalysts and conditions, indicating stable syngas composition. This range is suitable for downstream chemical synthesis.
[0031] FIG. 6 is a plot of catalytic performance of Ni20, Ni8Mgl2, and Nil3Ce6 catalysts in biogas conversion to syngas. Conditions: CH₄ / CO₂ / steam = 2:1:2, GHSV = 28 L h−1gcat−1, temperature = 690°C, and pressure = 10 bar. GHSV denotes gas hourly space velocity.
[0032] FIG. 7 is a comparison table of the present catalysts (denoted this work under the “Ref’ column) with reported catalysts (denoted “others” under the “Ref’ column). “CHVCCh / HjO ratios.bCatalytic performance in biogas steam reforming, in which catalytic CH4 conversions are normalized by corresponding thermodynamic equilibrium values at the same conditions. ' References to whether the catalysts are of the present disclosure (this work) or are reported catalysts (others). GHSV denotes gas hourly space velocity (L gcat-1h-1), T denotes temperature (°C), P denotes pressure in bar.
[0033] FIG. 8A is a plot of CH4 conversion for Nil3Ce6 and Ni20 catalysts in biogas conversion to syngas. Conditions: CH4 / CO2 / steam = 2:1.33:2, GHSV = 28 L h-1gcat−1, T = 600–690°C, and P = 10 and 30 bar.
[0034] FIG. 8B is a plot of CH₄ conversion for Ni13Ce6 catalysts (different amounts and synthesized from methods of present disclosure, wherein there is a Nil3Ce6 catalyst sample denoted “one pot”; see example 2A for a more detailed explanation of the “one pot” method) and for NilOSrlO and Nil0Mg5Cc5 catalysts in biogas conversion to syngas. Conditions: CH4 / CO2 = 2:1.33, CH4 / steam as per specified in FIG. 8B, GHSV = 28 L h-1gcat-1(56 and 168 L h-1gcat-1for Nil3Ce6 with catalyst mass of 0.15 g and 0.05 g, respectively), T = 690°C, and P = 10 and 30 bar. GHSV denotes gas hourly space velocity. All the catalysts are catalysts of the present disclosure. The catalyst denoted with “one pot” is from a method of the present disclosure, wherein its synthesis can be more straightforward than the method for theother Nil3Ce6 samples. The two differ in whether there is a separation of precipitate by filtration before adding precusor of B and / or precursor C. In the method of “one pot”, NtUOH was used as precipitating agent while in the method with separation NaOH was used as precipitating agent. So all the catalyst samples in relation to FIG.8B are of the present disclosure.
[0035] FIG. 8C is a plot of CH₄ conversion for Ni13Ce6, Ni10Ca10, Ni15Ce5-one pot-Al₂O₃ and Ni15-one pot-Al₂O₃ catalysts in biogas conversion to syngas. Conditions: CH4 / CO2 = 2:1.33, CH4 / steam as per specified in FIG. 8C, GHSV = 28 L h−1gcat−1(56 L h−1gcat−1for Ni13Ce6-one pot), T = 690°C, and P = 10 and 30 bar. GHSV denotes gas hourly space velocity.
[0036] FIG. 9A is a plot of CH4 conversion for Nil3Ce6-one pot catalyst (scaled-up synthesis) in biogas conversion to syngas. Conditions: CH4 / CO2 / stcam = 2:1.33:2, 0.5 g (sieved 0.4-0.8 mm), dry gas = 127.2 ml / min, 0.06 ml / min H2O liquid flow, T = 740°C-790°C, and P = 1 bar.
[0037] FIG. 9B is a plot of CO2 conversion for Ni13Ce6-one pot catalyst (scaled-up synthesis) in biogas conversion to syngas. Conditions: CH4 / CO2 / steani = 2:1.33:2, 0.5 g (sieved O.4-O.8 mm), dry gas = 127.2 ml / min, 0.06 ml / min H2O liquid flow, T = 740°C-790°C, and P = 1 bar.
[0038] FIG. 9C is a plot of H₂:CO molar ratio for Ni13Ce6-one pot catalyst (scaled-up synthesis) in biogas conversion to syngas. Conditions: CH₄ / CO₂ / steam = 2:1.33:2, 0.5 g (sieved 0.4-0.8 mm), dry gas = 127.2 ml / min, 0.06 ml / min H2O liquid flow, T = 740°C-790°C, and P = 1 bar.
[0039] FIG. 9D is a plot of the carbon recovery for Ni13Ce6-one pot catalyst (scaled-up synthesis) in biogas conversion to syngas. Conditions: CH₄ / CO₂ / steam = 2:1.33:2, 0.5 g (sieved 0.4-0.8 mm), dry gas = 127.2 ml / min, 0.06 ml / min H2O liquid flow, T = 740°C-790°C, and P = 1 bar.
[0040] FIG. 10A illustrates a traditional process flow for converting biogas into methanol and related products. In step 1, raw biogas (approximately 60% CH4 and 40% CO2) undergoes biogas upgrading to produce bio-CH4 while separating biogenic CO2. In step 2, the bio-CH is subjected to steam methane reforming to generate syngas with an H2: CO ratio of about 3 to 5. In step 3, the syngas is conditioned to adjust its composition, producing “metgas” with an H2: CO ratio of approximately 2, which issuitable for downstream synthesis. In step 4, the metgas is converted via methanol synthesis to produce bio-methanol (Bio-CHsOH).
[0041] FIG. 10B illustrates an integrated two-step process involving catalysts of the present disclosure for converting biogas into methanol. In step 1, biogas (approximately 60% CH4 and 40% CO2) is subjected to steam / bi-reforming in the presence of steam to produce syngas, particularly metgas with an H2: CO ratio of about 2, wherein the present catalysts are involved. In step 2, the metgas is directly fed into a methanol synthesis unit to produce bio-methanol (Bio-CH₃OH), enabling a more streamlined and integrated process.Detailed Description
[0042] The following detailed description refers to the accompanying drawings that show, by way of illustration, specific details and embodiments in which the present disclosure may be practised.
[0043] Features that are described in the context of an embodiment may correspondingly be applicable to the same or similar features in the other embodiments. Features that are described in the context of an embodiment may correspondingly be applicable to the other embodiments, even if not explicitly described in these other embodiments. Furthermore, additions and / or combinations and / or alternatives as described for a feature in the context of an embodiment may correspondingly be applicable to the same or similar feature in the other embodiments.
[0044] The present disclosure relates to a catalyst. The catalyst may include at least one metal, e.g., more than one metal. The catalyst is able to circumvent one or more challenges mentioned above associated with catalytic reforming processes. In particular, traditional catalysts for biogas reforming may be often limited by sintering, coking, and hydrothermal instability under high-temperature and high-pressure conditions, leading to performance degradation over time. The catalyst of the present disclosure can overcome these limitations due to its developed composition, enabling sustained catalytic activity, improved durability, and enhanced process efficiency. In various examples, the catalysts of the present disclosure can demonstrate stability for over 400 hrs on stream. For brevity, catalyst(s) of the present disclosure may be referred to herein as the present catalyst(s).
[0045] The present catalyst may include at least one non-noble transition metal, optionally in combination with at least one alkaline earth metal and / or at least one rare earth metal, arranged in a “core-shell-shell” configuration, providing a synergistic effect between activity and stability. The non-noble transition metal (“core”) may be configured in a matrix of the catalyst to render high catalytic activity for methane activation, while the surrounding shell(s) may help modulate electronic properties and provide structural stabilization to the core (and the catalyst as a whole). The outermost shell (i.e., a second shell), which may comprise an inert metal oxide and may be mesoporous, protects the active phase from sintering and coking while maintaining accessibility to reactants. Advantageously, the catalyst can exhibit high resistance to deactivation by the sintering and coking, prolonged operational lifetime, and stable performance across a wide range of reaction conditions, including elevated temperatures and pressures.
[0046] In the present disclosure, and in one or more statements mentioned above, the term "mesoporous" refers to a material that has pores with diameters in the range of 2 nanometers (nm) to 50 nm, 10 nm to 50 nm, 20 nm to 50 nm, 30 nm to 50 nm, 40 nm to 50 nm, etc.
[0047] The present disclosure also provides for a method for making the catalyst. Understandably, the advantages of the catalyst arc applicable to the method, and vice versa. The method for making the catalyst contributes to the overall advantages conferred by the catalyst. In particular, the present method can be a one-pot synthesis approach, which enables efficient and scalable production of the catalyst, ensuring homogeneous distribution of the active and stabilizing components. The method renders the catalyst manufacturing process straightforward, reduces processing steps, and facilitates cost-effective scale-up for industrial applications, while maintaining control over, for example, particle size and particle dispersion, which may have an impact on catalytic performance.
[0048] The present disclosure also provides for a process for producing chemicals from biogas, wherein the process involves the present catalyst. As such, it follows that the advantages of the catalyst and method for forming the catalyst are applicable to such a process, and vice versa. The present catalyst is advantageous for converting a biogas mixture (e.g., in the presence of steam) into a syngas mixture, i.e., enabling efficienttransformation of methane and carbon dioxide into syngas with a desirable H2 / CO ratio. Advantageously, the catalyst is operable under elevated pressures and high temperatures that allow for improved reaction rates, and this facilitates direct integration with downstream chemical synthesis processes, such as methanol or fuel production. This eliminates the need for intermediate processing steps and enhances overall process intensification. Furthermore, the process supports the utilization of renewable feedstocks such as biogas, thereby contributing to carbon utilization, waste valorization, and sustainable chemical production.
[0049] In the context of the present disclosure, the term “biogas” refers to a gaseous feedstock that may contain methane and carbon dioxide, wherein such feedstock may be generated from renewable or waste-derived sources such as anaerobic digestion of biomass, food waste, manure, wastewater, etc. The composition of biogas may vary, but is generally characterised by a significant proportion of methane and carbon dioxide, which may form the reactant stream supplied to the catalyst in aforesaid process.
[0050] Through the present process, which may involve catalytic conversion in the presence of steam and the catalyst, the biogas may be transformed into syngas. The term “syngas” refers to a gaseous mixture that may contain hydrogen and carbon monoxide. The process, advantageously, is able to render syngas with a controllable H2 / CO ratio (c.g., about 1.5 to 6, or about 2 for metgas), making it particularly suitable as an intermediate for downstream synthesis of chemicals and fuels, such as methanol, light olefins, and hydrocarbons. The term “metgas” refers to a specific syngas having a composition suitable as a direct feedstock for methanol production (e.g., the H2 / CO ratio may be about 2).
[0051] Holistically, the catalyst, method for making the catalyst, and process described herein provide a robust, scalable, and economically viable solution for converting biogas into valuable products, while addressing technical challenges associated with traditional approaches in catalytic reforming processes.
[0052] Details of various embodiments of the catalyst, the method for making the catalyst, the process, and the advantages associated with the various embodiments are now described below. Where the embodiments and / or advantages are already described in the examples section herein, further below, they shall not be reiterated for brevity.
[0053] In the present disclosure, there is provided a catalyst comprising more than one metal denoted by AxByCzwherein A may comprise at least one non-noble transition metal, B may comprise at least one alkaline earth metal, C may comprise at least one rare earth metal, and wherein x may represent a range of 2 to 30 wt%, 2 to 20 wt%, 2 to 10 wt%, etc., y may represent a range of 0 to 20 wt%, more than 0 to 20 wt%, 5 to 20 wt%, 10 to 20 wt%, etc., and / or z may represent a range of 0 to 20 wt%, more than 0 to 20 wt%, 5 to 20 wt%, 10 to 20 wt%, etc., and wherein the catalyst may comprise a core, a first shell configured around the core, and a second shell configured outer to the first shell, wherein the core may comprise A, wherein the first shell may comprise B and / or C, and wherein the second shell may comprise an inert metal oxide.
[0054] In the present disclosure and in various embodiments mentioned herein, the representation “AxByCz” is understood to mean that the more than one metal present in the catalyst (i.e., a composite) may be represented by metal A, metal B, and metal C. wherein metal A, metal B, and metal C, may be present in the weight percentages (wt%) mentioned above. Said differently, the representation “AxByCz” is not a chemical formula representing the catalyst, but just a representation of the metal(s) in the catalyst and its compositional configuration (e.g., wt% based on the catalyst). In various examples, y and / or z may be more than 0 wt%, for example, y and / or z may be more than 0 wt% and up to 20 wt%.
[0055] In the context of the present disclosure, the term “non-noble transition metal” refers to a transition metal that is not classified as noble metals (e.g., platinum, palladium, rhodium, ruthenium, iridium, silver, and gold, which are examples of noble metals). In other words, the non-noble transition metal constituting A is absent of platinum, palladium, rhodium, ruthenium, iridium, silver, and gold.
[0056] In the present catalyst, the matrix may be defined by a continuous porous metal oxide framework, e.g., comprising or formed from an inert oxide, such as silica, alumina, or zirconia, which constitutes the second (outermost) shell, within which the at least one non-noble transition metal (active phase) may be dispersed and / or embedded. This matrix may be generated during the method via hydrolysis and condensation of an oxide precursor (e.g., TEOS), followed by calcination, resulting in a mesoporous network that envelops the internal components of the catalyst. The matrix therefore serves not merely as a passive support, but as a structurally integratedoutermost shell that embeds and stabilises the catalytically active phase within a unified architecture.
[0057] Structurally, the catalyst exhibits a hierarchical arrangement in which the at least one non-noble transition metal (A), which may be present as nanoparticles, forms the core, which may be directly surrounded by the first shell comprising the at least one alkaline earth and / or the at least one rare earth metal species (B and / or C, respectively). The first shell may be present as a continuous or semi-continuous layer, or as a distribution of nanoparticles in intimate contact with the core, forming a core-shell interface that may provide catalytic activity and metal-support interactions. Surrounding this inner configuration is the second shell, which constitutes the inert metal oxide forming the matrix, encapsulating both the core and first shell. The first shell may partially integrate into or interface with the matrix. The second shell may fully or partially enclose the underlying structure, including any exposed regions of the core not covered by the first shell, forming a core-first shell-matrix (second shell) configuration.
[0058] Such structural relationship ensures that the active non-noble transition metal is spatially confined within the matrix via the intermediate first shell, which acts as both a chemical and physical stabiliser. The first shell may modulate the electronic and catalytic properties of the core while anchoring it within the matrix, and the second shell may provide a porous yet protective enclosure that maintains accessibility of reactants to the active sites. The resultant catalyst achieves a synergistic balance between accessibility, dispersion, and structural integrity, enabling high catalytic performance under demanding reaction conditions.
[0059] Advantageously, the catalyst, which may have a single metallic (or multimetallic) composition and hierarchical core-shell-shell architecture, can advantageously offer control over the chemical reactivity and structural stability of the active phase of the catalyst under reforming conditions. In particular, the non-noble transition metal component (e.g., Ni) can provide highly active sites for C-H bond activation in methane, and can be combined with the incorporation of alkaline earth and / or rare earth metals (e.g., Mg, Ce), to render the electronic environment and dispersion of the active phase for aforesaid advantages. Such active metal phase can be present as finely dispersed nanoparticles (e.g., on the order of ~6–8 nm) embeddedwithin a chemically stable matrix under reforming conditions, which maximizes accessible active surface area while minimizing the likelihood of particle agglomeration during high-temperature reforming operation.
[0060] The first shell, comprising the alkaline earth and / or the rare earth metal, may help stabilize the active phase (the at least one non-noble transition metal) and suppress deactivation pathways. For example, the Mg or Ce (or their oxides) surrounding the active Ni phase may enhance metal-support interactions, anchoring nanoparticles and reducing mobility that may otherwise lead to sintering. In addition, these metals introduce basic and redox functionalities, which facilitate adsorption and activation of CO2 and promote gasification of carbonaceous intermediates. This may mitigate coke formation, as evidenced by the significantly lower coking rates.
[0061] The outermost (second) shell, formed from an inert metal oxide, may provide a physical confinement effect and thermal barrier that helps protect the internal active phases from harsh reaction environments. The second shell may be mesoporous, allowing diffusion of reactants (e.g., CH₄, CO₂, steam) and products (e.g., H₂, CO) to and from the active sites, while still preventing coalescence of the encapsulated nanoparticles. This combination of confinement and permeability aids the catalyst in maintaining high activity without sacrificing stability. Furthermore, the encapsulation structure distributes thermal and mechanical stresses more evenly, contributing to the observed long-term stability (e.g., 400 hours or more on stream under industrially relevant conditions).
[0062] Collectively, the synergistic interaction between the at least one non-noble transition metal in the core, the first shell, and the protective porous second shell enables a catalytic environment in which methane activation, CO₂ reforming, and coke suppression occur concurrently and efficiently. The enhanced dispersion and stabilization of the active phase help in sustained catalytic turnover, while promoting desirable reaction pathways over deactivation routes. As a result, the catalyst achieves high conversion efficiency, stable performance under elevated temperature and pressure, and resistance to sintering and coking.
[0063] In various embodiments, the first shell may be configured around the core. In various embodiments, the first shell may be formed as a layered shell around the core. In various embodiments, the first shell may surround the core entirely or partially. Invarious embodiments, the first shell may be in contact with (i.e., configured adjacent to) the core.
[0064] In various embodiments, the first shell may comprise nanoparticles. In various embodiments, the nanoparticles may be configured around the core. In various embodiments, the nanoparticles may form a layer surrounding the core entirely or partially. In various embodiments, the nanoparticles may be in contact with (i.e., configured adjacent to) the core.
[0065] In various embodiments, the second shell may be configured outer to the first shell and may cover any portion of the core that is not enclosed by the first shell (e.g., any part of the core not covered by the first shell).
[0066] In various embodiments, the at least one non-noble transition metal may comprise nickel, copper, cobalt, manganese, iron, and / or zinc. Such non-noble transition metals may help in C-H bond activation, allowing efficient CH₄ conversion to syngas.
[0067] In various embodiments, the at least one alkaline earth metal or an oxide thereof may comprise barium, calcium, magnesium, and / or strontium. Incorporation of such alkaline earth metals may help enhance structural stabilization and coke resistance. These metals may form basic oxides that promote CO₂ activation and suppress carbon deposition, rendering the catalyst to exhibit significantly lower coking rates and improved stability.
[0068] In various embodiments, the at least one rare earth metal may comprise lanthanum, cerium, praseodymium, neodymium, samarium, europium, or gadolinium. Such rare earth metals may provide oxygen storage and redox properties, which may improve catalyst regeneration and resistance to deactivation.
[0069] In various embodiments, A may be a non-noble transition metal or an oxide thereof. The non-noble transition metal (or the oxide thereof) is already described above. Advantageously, the non-noble transition metal and its oxides may enable flexibility in catalyst activation and reaction pathways. Also, oxides of such non-noble transition metal may be reduced in situ to active metal species, facilitating controlled activation and improved dispersion, which contribute to higher catalytic efficiency and durability.
[0070] In various embodiments, B may be an alkaline earth metal or an oxide thereof. The alkaline earth metal is already described above. The presence of B as such alkaline earth metal or its oxide may allow tuning of basicity and interaction with CO₂, enhancing reforming reactions. This may improve CO₂ conversion and syngas composition control, which is helpful for downstream applications such as methanol synthesis
[0071] In various embodiments, the second shell may be mesoporous, which offers high surface area and improved mass transport, in turn helping reactants (e.g., CH₄, CO₂, steam) to diffuse efficiently to active sites while maintaining protection against sintering, resulting in high activity and long-term stability.
[0072] In various embodiments, the inert metal oxide may comprise silica, zirconia, or alumina. Such inert metal oxides may provide thermal stability and structural integrity to the catalyst, as these materials can form robust matrices that protect active sites under harsh conditions (e.g., 600-900°C), enabling operation without degradation of the catalyst.
[0073] In various embodiments, A may comprise nickel, B may comprise magnesium, x may be 5 to 30 wt%, y may be 5 to 20 wt%, and z may be 0 wt%. In various embodiments, A may comprise nickel, B may comprise magnesium, x may be 5 to 30 wt%, y may be 5 to 20 wt%, and z may be 0 wt%, and the catalyst may have a peak at a diffraction angle 2θ in a range of 35° to 45°, in a range of 50° to 55°, and in a range of 60° to 65°. In such non-limiting embodiments, the catalyst may be denoted NixMgy, where x and y are weight percentages of Ni and Mg (e.g., as defined above). A nonlimiting example may be x is 8.23 wt%, y is 12 wt%, and z is 0 wt%. Advantageously, in such non-limiting embodiments, the catalyst may offer a balanced combination of activity and stability. In various embodiments. Mg may enhance dispersion of Ni and reduce sintering, while maintaining strong catalytic activity, in turn improving methane conversion and reducing coking.
[0074] In various embodiments, A may comprise nickel, C may comprise cerium, x may be in a range of 5 to 30 wt%, y may be 0 wt%, and z may be in a range of 5 to 20 wt%. In various embodiments, A may comprise nickel, C may comprise cerium, x may be in a range of 5 to 30 wt%, y may be 0 wt%, and z may be in a range of 5 to 20 wt%, and the catalyst may have a peak at a diffraction angle 2θ in a range of 60° to 65° andone or more weak peaks at a diffraction angle 2θ in a range of 35° to 45°. In such embodiments, the catalyst may be denoted NixCez, where x and z are weight percentages of Ni and Ce (e.g., as defined above). A non-limiting example may be x is 13.22 wt%, y is 0 wt%, and z is 5.98 wt%. Advantageously, Ni and / or Ce may offer benefits of oxygen mobility and redox buffering, leading to improved catalyst longevity and stable catalyst performance under varying conditions even for long operation durations.
[0075] In various embodiments, A may comprise nickel, x may be 10-30 wt%, and y and z may be 0 wt%. In various embodiments, A may comprise nickel, x may be 5 to 30 wt%, and y and z may be 0 wt%, and the catalyst may have a peak at a diffraction angle 2θ in a range of 60° to 65° and one or more weak peaks at a diffraction angle 20 in a range of 35° to 45°. In such embodiments, the catalyst may be denoted Nix, where x is weight percentage of Ni. A non-limiting example may be x is 20.43 wt%, y and z are 0 wt%.
[0076] In various embodiments, A may comprise nickel, B may comprise magnesium, C may comprise Ce, x may be 5-30 wt%, y may be 5-20 wt%, and z may be 5-20 wt%. In various embodiments, A may comprise nickel, B may comprise magnesium, C may comprise Ce, x may be 10 wt%, y may be 5 wt%, and z may be 5 wt%.
[0077] The present disclosure also provides for a method for making the catalyst described in various embodiments of the first aspect. Embodiments and advantages described for various embodiments of the first aspect can be analogously valid for the present method subsequently described herein, and vice versa. Where the various embodiments and advantages have already been described above and in the examples section herein, they shall not be iterated for brevity.
[0078] The method may comprise forming a mixture comprising a precursor of A with an organic linker in water, and mixing the mixture with a precursor of B and / or a precursor of C. Advantageously, the method enables controlled synthesis of the catalyst, even with incorporation of multiple metals in a one-pot synthesis approach.
[0079] In various embodiments, the method may further comprise adding a precursor of an inert metal oxide to the mixture containing the precursor of B and / or precursor of C.
[0080] In various embodiments, forming the mixture comprising the precursor of A with the organic linker in water, may further comprise: forming a first mixture comprising the precursor of A, and the organic linker, in water, forming a precipitate from the first mixture, forming a dispersion comprising the precipitate, adjusting the dispersion to a pH of 12 or higher, and mixing the mixture with the precursor of B and / or the precursor of C comprises mixing the dispersion with an aqueous solution containing the precursor of B and / or the precursor of C. The high-pH precipitation step promotes uniform nucleation and controlled particle size formation. Advantageously, the high pH precipitation renders highly dispersed active phases, which helps in maximizing catalytic surface area and activity.
[0081] In various embodiments, mixing the mixture with the precursor of B and / or the precursor of C comprises mixing the mixture with a base prior to mixing the mixture with an aqueous solution containing the precursor of B and / or an aqueous solution containing the precursor of C. Advantageously, the order of base addition may allow tailored precipitation kinetics. This may help improve metal distribution and interaction, improving catalyst performance.
[0082] In various embodiments, mixing the mixture with the precursor of B and / or the precursor of C may comprise mixing the precursor of B and / or the precursor of C with a base prior to adding the mixture to the precursor of B and / or the precursor of C. This may provide flexibility in synthesis, allowing fine-tuning of catalyst structure. Such flexibility may be advantageous for scaling and adapting the process to different compositions.
[0083] In various embodiments, the method may further comprise: mixing the mixture with an alcoholic solution of a sol of an inert metal oxide (as the precursor of the inert metal oxide), or mixing the mixture with a sol of an inert metal oxide (as the precursor of the inert metal oxide), after mixing the mixture with the precursor of B and / or the precursor of C, then centrifuging the mixture to render a solid, and calcining the solid. The addition of an inert metal oxide sol followed by calcination may help to create a robust encapsulating shell so as to render the catalyst having better thermal stability, resistance to sintering, and protection of active sites under high-temperature operation.
[0084] In various embodiments, forming the mixture may comprise dissolving the precursor of A and the organic linker in water. In various embodiments, the organiclinker may comprise, for example, n-dodecylammonium bromide, n-dodecylammonium chloride, cetrimonium bromide, cetrimonium chloride, or behentrimonium chloride. Such organic linkers may provide multiple advantages during catalyst synthesis by acting as a structure-directing agent that enables the formation of small, well-dispersed metal nanoparticles, thereby enhancing catalytic activity, while also serving as a sacrificial template that decomposes during calcination to generate mesoporous channels for improved mass transport. In addition, such organic linkers may promote uniform integration of the catalyst components, facilitating close interaction between the active metal core and the shell materials, which contributes to improved structural stability, resistance to sintering and coking, and overall catalytic durability.
[0085] In various embodiments, the precursor of A may comprise a carbonate or a nitrate comprising the at least one non-noble transition metal, and / or wherein the precursor of B may comprise a nitrate comprising the at least one alkaline earth metal; and / or wherein the precursor of C may comprise a nitrate comprising the at least one rare earth metal. Such nitrates and carbonates may aid in formation of active phases.
[0086] The present disclosure further provides for a process for producing chemicals from biogas. Embodiments and advantages described for the catalyst and its method of making can be analogously valid for the present process subsequently described herein, and vice versa. Where the various embodiments and advantages have already been described above and in the examples section herein, they shall not be iterated for brevity.
[0087] Advantageously, the process offers a direct conversion of biogas (CH₄ + CO₂) into syngas, providing a sustainable route to chemicals and fuels. This eliminates the need for CO₂ separation and supports carbon utilization and waste valorization. In various embodiments, the chemicals generated from the process may include a syngas. The syngas may consist of hydrogen and carbon monoxide.
[0088] The process involves the catalyst described in various embodiments of the first aspect. The process may comprise providing a biogas, and contacting the biogas with the catalyst described in various embodiments of first aspect in the presence of steam. Said differently, in various embodiments, the process may comprise providing a biogas, and contacting the biogas with the catalyst described in various embodiments of thepresent disclosure in the presence of steam to convert the biogas to a mixture of hydrogen and carbon monoxide, wherein the hydrogen to the carbon monoxide may be present in a ratio of 1.5 to 6. In various embodiments, the biogas may include a mixture of methane and carbon dioxide, and the biogas may contain nitrogen gas, and the biogas may have some sulfur impurities in less than 10 ppm.
[0089] In various embodiments, the process may further comprise treating the catalyst with a reducing agent, optionally in the presence of an inert gas, prior to contacting the biogas and steam with the catalyst. Pre-treatment with a reducing agent may help to reduce (better activate) the catalyst. Advantageously, reducing the catalyst may help to render the catalyst in its active phase. The reducing agent may comprise hydrogen gas. In non-limiting examples, reducing the catalyst with hydrogen gas may involve converting nickel in nickel oxide form (Ni oxidation state +2) to metallic nickel (Ni oxidation state 0). This step renders metallic nickel, which is nickel in its active phase, i.e., the reduction step helps form active phase nickel state. The inert gas may comprise nitrogen gas. This step may be carried out at ambient pressure (e.g., 1 bar). This step may be carried out in a temperature ranging from 650°C to 850°C, 700°C to 800°C, 650°C to 750°C, etc.
[0090] In various embodiments, contacting the biogas with the catalyst in the presence of steam may be carried out at a temperature range of 600°C to 900°C, 700°C to 850°C, 600°C to 800°C, etc. These temperature ranges may help to improve reaction rates and render equilibrium (or near-equilibrium) conversions.
[0091] In various embodiments, contacting the biogas with the catalyst in the presence of steam may be carried out at a pressure range of 1 bar to 40 bar, 10 bar to 40 bar, 20 bar to 40 bar, 30 bar to 40 bar, etc. Such pressures may aid in process intensification and integration with downstream synthesis (e.g., methanol production). Unlike traditional systems limited to ambient pressure, this allows direct coupling to subsequent reactors, improving overall process efficiency. For instance, in various examples, the process can be performed at an ambient pressure (e.g., 1 bar) and / or at a high pressure in the range of 5 bar to 40 bar - this is advantageous - as the process can be configured to include further steps for generating higher value chemicals from the hydrogen and / or carbon monoxide, e.g., more valuable chemicals, such as methanol, long-chain hydrocarbons, aromatics, etc. As one non-limiting example, the reactor (e.g.,the tubular reactor or tubular microreactor), also referred to herein as “first reactor”, that produces the syngas from the biogas can be integrated with another reactor (i.e., second reactor) that converts the syngas to one or more of aforesaid higher value chemicals. In other words, the process may further comprise a step of converting the syngas into another chemical following directly from the step of generating the syngas from the biogas. As a non-limiting example, the second reactor can be operated (i) at the same pressure as the first reactor, (ii) at a temperature lower than the first reactor, and / or (iii) involve a catalyst system suitable for converting the syngas to one or more of the desired higher value chemicals.
[0092] In various embodiments, contacting the biogas with the catalyst in the presence of steam may include introducing the biogas (e.g., contains methane and carbon dioxide) to the catalyst with methane, carbon dioxide, and steam, present in a ratio of 2:1:1 to 2:2:10, e.g., 2:1:2.
[0093] In various embodiments, the process may involve a catalyst diluent. The catalyst diluent may comprise silicon carbide (SiC). In various embodiments, the method may further comprise mixing the catalyst and the diluent, which may be carried out separately from and before the step of treating the catalyst with the reducing agent in the presence of an inert gas.
[0094] In summary, the present catalysts (and its method of making and use) arc economical and scalable, enabled by a straightforward synthesis approach that simplifies preparation while ensuring uniform distribution of active and stabilising components. Notably, the present catalysts exhibit high catalytic activity despite the absence of noble metals, significantly reducing materials needed and costs without compromising performance. In addition, the present catalysts demonstrate stable performance under reforming and harsh reaction conditions, with high resistance to coking and sintering, w'hich arc factors contributing to catalyst deactivation in traditional catalysts. Furthermore, the ability of the present catalysts to operate effectively at elevated pressures allows the produced syngas to be directly fed into a downstream reactor for further conversion into chemicals and fuels, thereby facilitating process integration and improving overall process efficiency.
[0095] The term “one pot” and “one-pot” are used interchangeably in the present disclosure.
[0096] The word “substantially” does not exclude “completely” e.g. a composition which is “substantially free” from Y may be completely free from Y. Where necessary, the word “substantially” may be omitted from the definition of the present disclosure.
[0097] In the context of various embodiments, the articles “a”, “an” and “the” as used with regard to a feature or element include a reference to one or more of the features or elements.
[0098] In the context of various embodiments, the symbol and the term “about” or “approximately” as applied to a numeric value encompasses the exact value and a reasonable variance.
[0099] As used herein, the expressions “h” and “hr” may be used interchangeably to refer to hour.
[0100] As used herein, the term “and / or” includes any and all combinations of one or more of the associated listed items.
[0101] Unless specified otherwise, the terms "comprising" and "comprise", and grammatical variants thereof, are intended to represent "open" or "inclusive" language such that they include recited elements but also permit inclusion of additional, unrecited elements.Examples
[0102] The present disclosure provides examples for the catalyst as described above. The present disclosure provides examples for the method for making the catalyst as described above. The present disclosure provides examples for a process, and the catalyst systems involved, for efficient conversion of biogas to syngas under process conditions (e.g., reforming), which enable direct linking of the product stream to a subsequent step of upgrading so as to produce chemicals and fuels from the syngas. In various examples, and described above in various embodiments, a formula for the catalyst, includings its active component, may be denoted by AxByCz, where x can be 2-30 wt% (e.g., 2-20 wt%), y can be 0-20 wt% (e.g., more than 0 and up to 20 wt%), z can be 0-20 wt% (e.g., more than 0 and up to 20 wt%), and wherein A can be, for example, Ni, Mn, Zn, Co; B can be at least one alkaline earth metal, and C can be at least one rare earth metal.
[0103] The present catalyst, method, and process are described in further detail, by way of non-limiting examples, as set forth below. For brevity and for purpose of illustration, and to facilitate understanding and not to limit the examples, the catalyst, method, and process are demonstrated using nine example catalysts. The example catalysts include metals for which x, y, and z are greater than zero, and the example catalysts also include single metal catalysts. When the composite and / or outer shell forming inert material is silica, silica is not mentioned in the catalyst name abbreviation. However, when the composite and / or outer shell forming material is other than silica (e.g., if it is alumina or zirconia), it is mentioned in the catalyst name abbreviation. Thus, a catalyst with 20 wt% Ni and 80 wt% SiO2 is abbreviated as Ni20; a catalyst with 13 wt% Ni, 6 wt% Ce, and 81 wt% SiO2 is abbreviated as Ni13Ce6; and a catalyst with 15 wt% Ni, 5 wt% Cc, and 80 wt% AI2O3 is abbreviated as Ni15Ce5-Al2O3. The examples include Ni20 (active component is Ni with 20 wt%), Nil3Ce6 (active component may be Ni with 13 wt% and Ce with 6 wt%), Ni8Mgl2 (active component may be Ni with 8 wt% and Mg with 12 wt%), NilOSrlO (active component may be Ni with 10 wt% and Sr with 10 wt%), Nil0Mg5Ce5 (active component may be Ni with 10 wt%, Mg with 5 wt%, and Ce with 5 wt%), Nil3Ce6-one pot (active component may be Ni with 13 wt% and Ce with 6 wt%, see example 2A for “one pot”), NilOCalO (active component may be Ni with 10 wt% and Ca with 10 wt%), Ni15Ce5-one pot-Al2O3 (active component may be Ni with 15 wt% and Ce with 5 wt%, and alumina as second shell material instead of silica), and Ni15-one pot-Al2O3 (active component may be Ni with 15 wt% and alumina as second shell material instead of silica).
[0104] Example 1: Overview of the catalyst, method for making the catalyst, and process for producing chemicals from biogas
[0105] Various examples of the present disclosure relate to (1) an economical and scalable method for the synthesis of the catalyst, (2) a “catalyst system” suitable for stable conversion of biogas (mixtures of methane and carbon dioxide gases in different compositions) to syngas (a mixture of carbon monoxide and hydrogen) and other chemicals as well as fuels, and (3) efficient process for the use of the catalyst for converting biogas to syngas.
[0106] Various examples of the present disclosure also relate to the process configuration for the use of syngas produced in this process to produce chemicals suchas methanol, light olefins, and fuels. The syngas produced from the process can be tuned to metgas composition (i.e., H2 / CO = 2) directly useful for methanol synthesis or H2-rich syngas for the production of other chemicals and fuels (e.g., light olefins and fuels). The Ha-rich syngas is also useful for utilizing unreacted CO2 in biogas, circumventing the need for separation of unreacted CO2. The active components in the catalysts include at least one non-noble transition metal (denoted A, which can be Ni, Mn, Zn, and / or Co) and one or more metals (or their oxides) from at least one alkaline earth metal (denoted B) and / or at least one rare earth metal (denoted C). Thus, the formula of the catalyst, including the active component / phase, may be denoted as AxByCz, where x, y and z are already described above in various embodiments and examples. The at least one non-noble transition metal-based active component (A) is protected by a metal oxide shell (second shell) made of inert materials, such as silica, alumina, or zirconia. The second active component / phase, B and / or C, may also be present as the first shell on the at least one non-noble transition metal. The first shell is further shelled by the second shell (the inert metal oxide). The inert metal oxide shell is synthesized in a way that it has mesopore channels. The synthesis method for the catalysts involves an efficient precipitation-hydrolysis chemistry described in various embodiments above and in examples hereinbelow.
[0107] The process involving the catalyst may be in a continuous-flow fixed-bed reactor process, where different compositions of biogas are reacted with steam on the catalyst at temperatures, for example, in the range of 600°C to 900°C (e.g,. 600°C to 800°C, 650°C to 850°C, 650°C to 750°C) and pressure in the range of 1 bar to 30 bar (and even elevated pressure in the range of 5 bar to 30 bar), which can be above the normal testing range of such reactions. The process configuration for the utilization of the syngas in the product stream with any unreacted CO2 involves feeding the stream, after removing unreacted steam, at reaction pressure to a second reactor operated at a lower temperature in the range of, for example, 200°C to 400°C and containing catalysts capable of converting the product stream of the first reactor to various products, such as methanol, light olefins, and fuels (C5+ hydrocarbons). The catalysts can achieve CH4 conversion above 50% (which is -95% of the equilibrium value) and CO2 conversion of -10% at 690°C, 5 bars, and a space velocity of 28000 mL h-1g-1. Even at an elevated pressure of 10 bar, significant activity of about 40% CH4 conversion was still obtained.The catalyst of the present disclosure can achieve CH4 covnersion of above 90% and CO2 conversion of above 40% at 790°C, 1 bar, and space velocity of 28000 mL h-1g-1. The catalysts of the present disclosure were used under various conditions during the first 330 hrs on stream and then at 10 bar and 690°C for another 100 hrs, where the catalysts demonstrated stable performance. Besides, various compositions were found to have outstanding resistance to coking (carbon deposition (< 0.3 mg g^r1h-1)). The syngas was produced with desirably high H2 / CO ratios (2 to 3.5).
[0108] Example 2A: Catalyst synthesis
[0109] The method for making the catalysts involves consecutive precipitation and hydrolysis chemistry. Generally, in the method, a precursor of A (e.g., nitrate or carbonate of the metal A) and an organic linker (e.g., n-dodecylammonium bromide, n-dodecylammonium chloride, cetrimonium bromide, cetrimonium chloride, behentrimonium chloride, etc.) are dissolved in water in a ratio, followed by the addition of a base such as sodium hydroxide or ammonium hydroxide. The mixture is stirred for 2 hrs at room temperature (e.g,. 20°C to 30°C) and then a desired amount of the aqueous precursor solution of B or C (or a mixture thereof) is added dropwise at room temperature. The precursor (e.g., solution form) of metal B may include a nitrate comprising the at least one alkaline earth metal. The precursor (e.g., solution form) of C may include a nitrate comprising the at least one rare earth metal. Before adding precursors for B and / or C, the precipitate can be separated to remove halide salts and the precipitate (wet) may then dissolved in water again and pH of the mixture was adjusted to above 12 and maintained with stirring for another 2 hr after complete addition. The temperature of the oil bath may then be increased to 80°C and the inert metal oxide sol (alumina, silica, or zirconia), optionally in the form of an alcoholic solution (e.g., ethanol), is then added dropwise at 80°C. In various examples, silica sol (tetraethyl orthosilicate) and / or alumina sol (aluminium isopropoxide) can be employed as the inert metal oxide sol. The mixture is then stirred for up to 6 hrs to 24 hrs at 80°C. The solid is then separated by centrifugation, followed by drying at 80°C and calcination at 800°C. It may be noted that when NaOH is used as the base, the precipitate of A may be separated before addition of the precursor of B and / or the precusor of C. The catalyst obtained with this approach may be deemed as a “default” method of the present disclosure. When NH4OH is used as the base, the precipitate ofA may not be separated and the precursor of B and / or the precursor of C can be directly added as described above. The latter approach, which involves NH4OH and without the separation of the precipitate of A, is denoted “one -pot” (or “one pot”) and the corresponding catalyst samples are generally denoted herein as “A BlC--one pot”, wherein AxByCzare as described in various embodiments mentioned above and in the examples of the present disclosure.
[0110] Example 2B: Characterisations / Properties of catalyst
[0111] Properties of the catalysts were determined by various characterisation methods. Powder X-ray diffraction (XRD) analysis showed that all catalyst samples led to the formation of nickel oxide in nanoparticulate form with domain size (dS) – derived by the application of Scherrer equation to nickel oxide reflections - in the range of about 6 nm to about 8 nm (FIG. 1A).
[0112] Scanning electron microscopy (SEM) analysis showed that sample form big agglomerates of no particular shape (FIG. 2A, FIG. 2D, FIG. 2H). SEM with energy dispersive X-ray (EDX) elemental mapping analysis showed that all metals are uniformly distributed in all samples (FIG. 2B to FIG. 2C, FIG. 2E to FIG. 2G, FIG. 21 to FIG. 2K).
[0113] High resolution transmission electron microscopy analysis (HR-TEM) showed that active phase is well distributed within the matrix (FIG. 3A to FIG. 3C). Hexagonal to rounded particles (darker spots) in bright field image point to heavier component in the specimen. In this case, it should be nickel, and, the lighter surrounding matrix should be made of magnesium and silica. To confirm this, TEM-energy dispersive X-ray spectroscopy (EDS) was performed. The obtained elemental map (FIG. 3C) showed that nickel-based phase is surrounded by magnesium oxide, which itself is surrounded by silica shell. Thus, one type of catalysts of the present disclosure are dual shelled nickel catalyst. The immediate shell to nickel can also be a component of the active phase of the catalyst.
[0114] Additional properties of the catalysts are indicated in FIG. 4. The specific surface area of the catalysts ranged between 80 and 160 m2g-1with highest being Ni20 and lowest being Ni8Mgl2. Actual metal content determined from X-ray fluorescence (XRF) analysis is also given in FIG. 4.
[0115] Example 2C: Catalytic results on selected catalysts
[0116] Catalyst testing for biogas steam reforming was carried out in a continuous flow, fixed-bed, custom-built automated high-throughput reactor system from hte GmbH. A mixture of 300 mg sieved catalyst particles (0.25-0.4 mm) and SiC (0.5 mm, topped up to a total volume of 1.8 mL) was loaded into a tubular microreactor with an internal diameter of 6.3 mm. 300 mg was the default mass of catalysts used in all catalyst testing. If lower or higher catalyst mass is used, it is shown in the catalyst code. For instance, if Nil3Ce6 is tested using 0.15 g of catalyst mass, the catalyst name in the drawing is shown as Nil3Ce6-0.15 g. Prior to the reaction, the catalyst was reduced in situ using 50% H2 in N2 at 690°C for 3 hours under ambient pressure with a flow rate of 30 mL min-1. Biogas steam reforming reaction was performed by feeding 70 to 140 mL min-1of reaction gas containing CH4 / CO2 / steam = 2:1:2 and 5% to 7% argon (Ar) as internal standard. The screening was done at 5 bar to 10 bar and 600°C to 690°C at a gas hourly space velocity of 14 to 28 L hr-1gcat-1. The reaction products were analyzed using an online Agilent GC 8890 equipped with multiple FID and TCD detectors (i.e., flame ionisation detector and thermal conductivity detectors, respectively). The first FID detector detects Ci to C4 hydrocarbon products, whereas the second detects C5 and longer hydrocarbon products. On the other hand, the first TCD detector was used to quantify Ar, which is used as the internal standard throughout the reaction. The second TCD detector detects H2. The catalysts at each condition were tested for more than 10 hours or for the duration to collect at least 4 GC analysis data points. The CH4 and CO2 conversions, and H2 / CO ratio were calculated using the following equations:
[0117] CH4conversion (%), X(CH4) = [CH4(in, mmol / h) - CH4(out, mmol / h)] / CH4(in, mmol / h) x 100
[0118] CO2 conversion (%), X(CO2) = [CO2(in, mmol / h) - CO2 (out, mmol / h)] / CO2 (in, mmol / h) X 100
[0119] CH4conversion rate (mol(CH4) h’1gw’1), R(CH4) = [CH4(in, mmol / h) - CH4(out, mmol / h)] / 1000 / [catalyst mass (g)*wt% of Ni]
[0120] H2 / CO = H2 (out, mmol / h) / CO (out, mmol / h)
[0121] Carbon balance was determined using the equation below. Carbon balance for the reported results was within 100 + 3.5%.Carbon balance = [CH4 (out, mmol / h) + CO2 (out, mmol / h) + CO (out, mmol / h)] / [CH4(in, mmol / h) + CO2 (in, mmol / h)] x 100
[0122] The catalytic performance of catalysts is summarized in FIG. 5 A to FIG. 5C. Overall, the catalysts exhibited remarkable conversion levels at 690°C and 5 bars, which was above 45% for CH4 and 5% for CO2. Slightly lower conversions were observed at high space velocity, which may be suitable for applications that have such requirements. In both cases, the conversion levels were close to equilibrium conversion of 95%. Comparing the conversion rate, addition of second metal to the composition can improve the conversion significantly, with Ni8Mgl2 as one of the non-limiting examples reaching 2 mol(CH4) h-1gNi-1. H2 / CO ratio achieved was 2.5 to 3.3.
[0123] The durability of catalysts was evaluated at 690°C and 10 bar pressure. The tests were conducted on the same load of catalysts after conducting a series of tests under variable conditions for 330 hrs on stream. The runs were continued for about another 100 hr on stream. The catalysts with Ce and Mg showed a stable performance throughout the run, with slight increase in both CH4 and CO2 conversions. However, Ni20 showed signs for deactivation after 50 hr on stream. CO2 conversion was fully depleted for this catalyst at about 85 hr on stream. The results highlight the effectiveness of multimetallic catalysts of the present disclosure.
[0124] The spent catalysts after 426 hr on stream were characterised by XRD analysis (FIG. IB). As expected, nickel was present in metallic form. How'ever, Ni20 indicated noticeable sintering of nickel particles with a domain size of 26 nm and much sharper reflection for metallic nickel compared to those with magnesium or cerium in their composition (domain size was about 20 nm). Thus, the sintering in the multimetallic catalysts was lower and excessive sintering for Ni20 might be a result of some deactivation observed over this catalyst. Besides, the extent of coking was determined by weight loss in TGA (FIG. 7). Ni20 showed severe coking compared to NiMg-based or NiCe-based catalysts. The coking resistance on the latter systems was compared with the literature (FIG. 7). Even with no noble metals, the catalysts of the present study showed a significantly lower coking rate.
[0125] Most of the traditional works conducted the biogas steam reforming at ambient pressure. In the present process, the reaction conditions applied (with high pressure and low temperatures) favor and aids in downstream processing, such as formed syngas processing to convert to other chemicals (e.g., methanol). The present catalysts still exhibited superior activity in the biogas steam reforming reaction, particularlyregarding CH4 conversion performance and coking resistance. Indeed, while the highly endothermic nature of biogas steam reforming may challenge the catalytic performance at low temperatures, the present catalysts still showed a conversion that is very close the equilibrium at the range of 600°C to 690°C, which is relatively lower than that from most traditional reactions. Besides, the coking resistance was demonstrated over a considerably long time on stream with remarkably minimal carbon deposition, even when compared with noble metal-based catalysts. The Hz / CO was exceptionally higher than 2, which is potentially advantageous for the downstream CO and CO2 conversions.
[0126] Example 3: Further Catalytic testing
[0127] Further catalytic tests on Nil3Ce6 and Ni20 catalysts under different conditions were carried out. Results are presented in FIG. 8A, showing stable performance under different conditions. FIG. 8A shows the methane (CH4) conversion (X(CH4), %) as a function of time-on-stream (TOS) for Nil3Ce6 and Ni20 catalysts under varying reaction conditions during biogas conversion to syngas. At the initial stage (about 50-110 h), both catalysts exhibit stable CH4 conversion of about 35-38% at 690°C and 10 bar, indicating comparable activity and stability under baseline conditions. Upon switching to 30 bar (about 110-200 h) while maintaining high temperature conditions (around 690°C, with variations to 650°C and 600°C), the CH4 conversion decreases to about 22-25%, due to equilibrium limitation of methane reforming at elevated pressure. Despite this reduction, both catalysts maintain stable and consistent performance over extended operation, demonstrating resistance to deactivation. A temporary interruption in CH4 supply (indicated by “N2 only”) did not affect the activity, as the same activity level was achieved after switching to reactant feed stream. At lower temperatures toward the end of the high-pressure segment (around 600°C), conversion further decreases to approximately 10-17%, consistent with reduced reaction kinetics at lower temperatures. In the subsequent segment (about 220-300 h), an N2 flow period is introduced, during which no methane conversion occurs. Upon reintroduction of reactants at 10 bar, the catalysts again show recovery of activity, with CH4 conversion returning to approximately 20-25% at lower temperatures and increasing to -35-45% at 690°C toward the final stage (about 300- 320 h). Overall, FIG. 8A demonstrates that both Nil3Ce6 and Ni20 catalysts exhibit stable catalytic performance over prolonged time-on-stream (>300 h), with consistentresponse to changes in pressure and temperature, and the ability to recover activity after interruption, highlighting their robustness under varying reaction conditions.
[0128] Catalytic testing on Nil3Ce6 using different amounts (i.e., higher GHSV), different second metal (Sr) and combination of Mg and Ce, and one-pot synthesis of Nil3Ce6, were carried out. Results are presented in FIG. 8B, showing stable performance for the catalysts of the present disclosure. FIG. 8B shows the methane conversion (X(CH4), %) as a function of time-on-stream (TOS) for Nil3Ce6-based catalysts under varying catalyst loadings, demonstrating the effect of GHSV, second metal addition, and synthesis method on catalytic performance. In the initial stage (about 0-25 h), conducted at 10 bar and 690°C with steam / CH4 = 1, relatively high CH4 conversion is observed. The Nil3Ce6 (0.15 g) sample exhibits stable conversion of approximately 32-34%, while the lower loading Ni13Ce6 (0.05 g) shows reduced conversion (~24–26%), reflecting the effect of higher GHSV (lower catalyst amount) leading to shorter residence time and lower conversion. Other catalysts, including NilOSrlO, Ni10Mg5Ce5, and Nil3Ce6 (one-pot), show comparable or slightly higher conversion (-36-38%), indicating that incorporation of a second metal and optimized synthesis can enhance catalytic performance. In the second stage (about 25-115 h), conditions are changed to 30 bar and 690°C with steam / CH4 = 1. Under these higher pressure conditions, CH4 conversion decreases to approximately 23-25% for most catalysts, consistent with thermodynamic limitations at elevated pressure. Despite this, the multimetallic catalysts (NilOSrlO, Nil0Mg5Ce5, and Nil3Ce6 one-pot) maintain stable and consistent performance over extended operation, whereas the low-loading Nil3Ce6 (0.05 g) shows a lower in conversion to around 15-18%, but still maintaining stable performance. A lower conversion at a lower catalyst amount may be expected due to possibility of lower active sites available for the reaction. In the final stage (about 115-145 h), the steam / CH4 ratio is increased to 1.5 at 30 bar and 690°C, resulting in an increase in CH4 conversion to approximately 27-30% for the higher-performing catalysts. This improvement highlights the beneficial effect of increased steam content in promoting reforming reactions and mitigating carbon formation. The multimetallic and one -pot synthesized catalysts continue to show stable and superior performance, while the low-loading sample remains less active. Overall, FIG. 8B demonstrates that catalyst composition (e.g., addition of Sr or Mg / Ce), synthesis method (one-pot), andoperating conditions (GHSV and steam ratio) can be used to tune catalytic performance. The results highlight that catalysts of the present disclosure can exhibit enhanced activity and stability.
[0129] Other alkali metals, such as Ca, and different oxides, e.g., AI2O3 (alumina) replacing SiO2 (silica), were tested. Results are shown in FIG. 8C. FIG. 8C shows the methane conversion (X(CH4), %) as a function of time-on-stream (TOS) for Ni-based catalysts incorporating different alkaline earth metal (Ca) and different oxide supports (SiO2 and AI2O3), under varying reaction conditions, thereby illustrating the effect of metal composition and support material on catalytic performance. In the initial stage (about 0-45 h), conducted at 10 bar and 690°C with steam / CH4 = 1, most catalysts, including Ni10Ca10, Ni15Ce5-one pot-Al2O3, and Ni15-one pot-Al2O3. exhibit relatively high and stable CFU conversion in the range of -37-39%, comparable to the one-pot Nil3Ce6 reference sample (-35-36%). In the second stage (about 45-160 h), the pressure is increased to 30 bar at 690°C with sleam / CH i = 1. Under these conditions, CH4 conversion decreases for all catalysts to approximately 24-26%, consistent with limitations at higher pressure. Despite this, most catalysts (Ni10Ca10, Ni15Ce5-one pot-Al2O3, and Ni15-one pot-Al2O3) maintain stable performance over extended time-on-stream, indicating good resistance to deactivation. The Ni13Ce6-one-pot catalyst (tested with halve catalyst mass compared to other catalysts in FIG. 8C, i.e., with twice the GHSV) shows only slightly lower conversion (-21-23%) but remains stable. This result shows that Nil3Ce6-one-pot is highly active for biogas conversion to syngas. The NilOCalO and AI2O3- supported catalysts (Ni15Ce5-one pot-Al2O3 and Ni15-one pot-Al2O3) show improved conversion to approximately 29-32%, highlighting the beneficial effect of increased steam in enhancing reforming reactions and suppressing carbon formation. Nil3Ce6 one-pot catalyst shows modest improvement (-24-25%). Overall, FIG. 8C demonstrates that catalyst composition and support material significantly influence catalytic activity and stability. Calcium-containing and Al2O3-supported catalysts exhibit superior performance and stability. The results also confirm that increasing pressure reduces conversion, while increasing steam ratio enhances conversion, and that catalysts maintain stable operation over extended time-on-stream, indicating good durability under varying conditions.
[0130] Scaling up the catalyst by 5 times using a one-pot synthesis described in example 2A was tested. The samples were tested at 1 bar and high temperatures up to 790°C to maximize CH4 and CO2 conversion. FIG. 9A to FIG. 9D summarize the results, which show stable performance for more than 430 hr on stream with CH4 conversion reaching above 90% at 790°C. FIG. 9A to FIG. 9D present the long-term catalytic performance of a scaled-up Nil3Ce6-one pot catalyst (5x scale) during biogas conversion to syngas, evaluated over more than 430 hours on stream at 1 bar and temperatures ranging from 740°C to 790°C, demonstrating the effect of temperature and durability under extended operation. In FIG. 9A, the CH4 conversion is shown as a function of time -on-stream. At 740°C (about 0-220 h), the catalyst exhibits relatively stable CH4 conversion in the range of -65-75%, with a slight decline over time, partly associated with a temporary disturbance (c.g., gas bottle change). Upon increasing the temperature to 790°C (about 220-430 h), the CH4 conversion increases significantly to approximately 85-92%, and remains stable for the remainder of the run. This indicates that higher temperature enhances reaction kinetics while the catalyst maintains excellent stability over prolonged operation. In FIG. 9B, the CO2 conversion follows a similar trend. At 740°C, CO2 conversion is around -25-35%, with some fluctuation and a slight decrease over time. When the temperature is increased to 790°C, CO2 conversion improves to approximately -35-45%, and remains relatively stable throughout the extended time-on-stream. This reflects improved reforming efficiency at higher temperature while maintaining durability. In FIG. 9C, the H2 / CO molar ratio is shown to remain relatively stable throughout the experiment, generally in the range of -2.3-2.7, with a slight decrease at higher temperature. This indicates consistent syngas composition over long-term operation, which is important for downstream processing. In FIG. 9D, the carbon balance (C%) remains close to -100% throughout the entire duration, confirming reliable measurement accuracy and minimal carbon loss. This also suggests limited coke formation or carbon deposition, consistent with the catalyst’s high resistance to coking. Overall, FIG. 9A to FIG. 9D demonstrate that the scaled-up catalyst maintains high activity, improved conversion at elevated temperature, stable syngas composition, and excellent durability over more than 430 hours, thereby confirming the scalability and robustness of the catalyst system under industrially relevant conditions.
[0131] In addition, the method for making the catalyst has been tested to increase solid concentrations of the catalysts during the synthesis. This helps in scalability. In particular, 10 times less water were used and a silica source (tetraethyl orthosilicate, TEOS) was directly added to the precipitated-composite solution at 80°C, instead of an ethanolic solution of TEOS.
[0132] Example 4: Commercial and Potential Applications
[0133] The present disclosure describes a one-pot synthesis for the catalysts of the present disclosure, which makes the overall synthesis economical and scalable. The catalyst may be a dual shell catalysts that offer protection from sintering and coking. The catalysts can be used in an intensified process environment that enables direct upgrading of biogas to chemicals and fuels.
[0134] The catalysts can be applied for biogas conversion via steam reforming, methane conversion via steam reforming, and methane conversion via dry reforming. All this leads to syngas production which can be used as building block feedstock for the preparation of various chemicals and fuels. The purity of biogas feed is largely dependent on its source.
[0135] The presence of excessive amounts of catalyst surface poisoning substances (e.g., sulfur compounds) may lead to catalyst deactivation. Traditionally, upstream purification should be applied in such cases to remove such catalyst-poisoning compounds. However, the present catalyts may have increased sulfur tolerance. In addition, the present catalysts can undergo in situ catalyst regeneration (such as oxidative treatment).
[0136] The present catalysts can offer extended operation durability and feedstock flexibility. Synthesis of the present catalysts can be scaled-up to several 10s gram scale. The catalysts are compatible in a process configuration involving dual reactor bed system for further converting any formed syngas to other chemicals (such as methanol).
[0137] While the present disclosure has been particularly shown and described with reference to specific embodiments, it should be understood by those skilled in the art that various changes in form and detail may be made therein without departing from the spirit and scope of the present disclosure as defined by the appended claims. The scope of the present disclosure is thus indicated by the appended claims and all changeswhich come within the meaning and range of equivalency of the claims are therefore intended to be embraced.
Claims
CLAIMS1. A catalyst comprising:more than one metal denoted by:AxByCzwherein:A comprises at least one non-noble transition metal,B comprises at least one alkaline earth metal,C comprises at least one rare earth metal, andwherein x represents a range of 2 to 30 wt%, y represents a range of 0 to 20 wt%, and / or z represents a range of 0 to 20 wt%;andwherein the catalyst comprises a core, a first shell configured around the core, and a second shell configured outer to the first shell;wherein the core comprises A;wherein the first shell comprises B and / or C; andwherein the second shell comprises an inert metal oxide.
2. The catalyst of claim 1, wherein the at least one non-noble transition metal comprises nickel, copper, cobalt, manganese, iron, or zinc.
3. The catalyst of claim 1 or 2, wherein the at least one alkaline earth metal or an oxide thereof comprises barium, calcium, magnesium, or strontium.
4. The catalyst of any one of claims 1 to 3, wherein the at least one rare earth metal comprises lanthanum, cerium, praseodymium, neodymium, samarium, europium, or gadolinium.
5. The catalyst of any one of claims 1 to 4, wherein A is a non-noble transition metal or an oxide thereof.
6. The catalyst of any one of claims 1 to 5, wherein B is an alkaline earth metal or an oxide thereof.
7. The catalyst of any one of claims 1 to 6, wherein the second shell is mesoporous.
8. The catalyst of any one of claims 1 to 7, wherein the inert metal oxide comprises silicon, zirconia, or alumina.
9. The catalyst of claim 1, wherein A comprises nickel, B comprises magnesium, x is 5-30 wt%, y is 5-20 wt%, and z is 0 wt%.
10. The catalyst of claim 1, wherein A comprises nickel, C comprises cerium, x is in a range of 5 to 30 wt%, y is 0 wt%, and z is in a range of 5 to 20 wt%.
11. The catalyst of claim 1, wherein A comprises nickel, x is 10-30 wt%, and y and z are 0 wt%.
12. The catalyst of claim 1, wherein A comprises nickel, B comprises magnesium, C comprises Ce, x is 5-30 wt%, y is 5-20 wt%, and z is 5-20 wt%.
13. A method of making the catalyst of any one of claims 1 to 12, the method comprising:forming a mixture comprising a precursor of A with an organic linker in water; mixing the mixture with a precursor of B and / or a precursor of C.
14. The method of claim 13, further comprising:adding a precursor of an inert metal oxide to the mixture containing the precursor of B and / or precursor of C.
15. The method of claim 13, wherein forming the mixture comprising the precursor of A with the organic linker in water, further comprises:forming a first mixture comprising the precursor of A, and the organic linker, in water;forming a precipitate from the first mixture;forming a dispersion comprising the precipitate;adjusting the dispersion to a pH of 12 or higher; andmixing the mixture with the precursor of B and / or the precursor of C comprises mixing the dispersion with an aqueous solution containing the precursor of B and / or the precursor of C.
16. The method of claim 13, wherein mixing the mixture with the precursor of B and / or the precursor of C comprises mixing the mixture with a base prior to mixing the mixture with an aqueous solution containing the precursor of B and / or an aqueous solution containing the precursor of C.
17. The method of claim 13, wherein mixing the mixture with the precursor of B and / or the precursor of C comprises:mixing the precursor of B and / or the precursor of C with a base prior to adding the mixture to the precursor of B and / or the precursor of C.
18. The method of claim 14, further comprising:mixing the mixture with an alcoholic solution of a sol of the inert metal oxide as the precursor of the inert metal oxide, or mixing the mixture with a sol of the inert metal oxide as the precursor of the inert metal oxide, after mixing the mixture with the precursor of B and / or the precursor of C, then centrifuging the mixture to render a solid; andcalcining the solid.
19. The method of any one of claims 13 to 18, wherein forming the mixture comprises dissolving the precursor of A and the organic linker in water.
20. The method of any one of claims 13 to 19,wherein the precursor of A comprises a carbonate or a nitrate comprising the at least one non-noble transition metal; and / orwherein the precursor of B comprises a nitrate comprising the at least one alkaline earth metal; and / orwherein the precursor of C comprises a nitrate comprising the at least one rare earth metal.
21. A process for producing chemicals from biogas, the process comprising: providing a biogas; andcontacting the biogas with the catalyst of any one of claims 1 to 12 in the presence of steam.
22. The process of claim 21, further comprising:treating the catalyst with a reducing agent prior to contacting the biogas and steam with the catalyst.
23. The process of claim 21 or 22, wherein contacting the biogas with the catalyst in the presence of steam is carried out at a temperature range of 600°C to 800°C.
24. The process of any one of claims 21 to 23, wherein contacting the biogas with the catalyst in the presence of steam is carried out at a pressure range of 1 bar to 40 bar.