Ligand leaving promoting additives for organotin photoresist compositions and patterning

Organyl ligand leaving promoting additives in organotin precursor solutions enhance radiation-induced thermal condensation and dissolution contrast, addressing the challenge of high radiation doses in organometallic photoresist materials by improving patterning performance and efficiency.

WO2026236365A1PCT designated stage Publication Date: 2026-11-12INPRIA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/026905
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Current organometallic photoresist materials face challenges in achieving high-resolution, high-etch resistance, and high-fidelity patterns while requiring high radiation doses, which can compromise patterning performance and efficiency.

Method used

Incorporation of organyl ligand leaving promoting additives into organotin precursor solutions to enhance radiation-induced thermal condensation and dissolution contrast, allowing for improved patterning performance with reduced radiation doses.

Benefits of technology

The additives facilitate lower radiation doses without compromising patterning quality, enhancing etch selectivity and dissolution contrast, thereby improving throughput and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026026905_12112026_PF_FP_ABST
    Figure US2026026905_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Solutions comprise a blend of an organic solvent, an organotin composition and an additive composition, which are useful for the coating of high resolution photolithography coatings. The additive composition can be represented by the formula Q+ nAn- wherein 1≤n≤5 An- is Cl-, Br-, OH-, or an oxyanion comprising at least 1 and up to 10 oxygen atoms bonded to one or more core atoms selected from B, Si, C or group 15-17 elements, Q+ is H+, onium cation [ERc m]+, or a combination thereof wherein E is a group 15 to group 17 element, each Rc is independently selected from H, 1 to 11 carbon alkyl, alkenyl, or aryl groups, and a 1 to 11 carbon hydroxyl substituted group, and are attached to E via an E-C bond, and 2≤m≤4 with the proviso that Q+ is not H+ when An- is OH- or phosphite. Corresponding coatings and methods of patterning are presented.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Attorney Docket No. 5063.67W001 LIGAND LEAVING PROMOTING ADDITIVES FOR ORGANOTIN PHOTORESIST COMPOSITIONS AND PATTERNING

[0002] CROSS REFERENCE TO RELATED APPLICATIONS:

[0003] This application claims priority to co-pending provisional US Patent Application No.

[0004] 63 / 803,127 to Cardineau, et al. filed on May 9th, 2025 and titled “LIGAND LEAVING PROMOTING ADDITIVES FOR ORGANOTIN PHOTORESIST COMPOSITIONS AND PATTERNING”, which is hereby incorporated by reference in its entirety.

[0005] FIELD OF THE INVENTION:

[0006] The invention pertains to tin based organometallic photoresist materials having organyl ligands as well as additives for improving the performance of said materials. The invention further relates to precursor solutions comprising organotin precursors and the additives for coating the photoresist materials on a substrate, radiation patternable coatings formed therefrom, and lithographic methods for patterning the coatings.

[0007] BACKGROUND OF THE INVENTION:

[0008] Semiconductor lithography is a complex and critical technology used to fabricate myriad and diverse devices that have dominated and transformed the modern world beginning in the 20thcentury. The semiconductor lithographic process is generally an iterative process involving repeated steps of deposition, patterning, and etching of many layers and materials to form the desired devices. As technology advances and new, increasing demands and requirements are placed upon each generation of devices, the need to develop processes and materials that are able to meet these requirements increases. One of the critical materials used in the semiconductor lithographic process is the photoresist in which an initial pattern is formed by exposure to radiation and is then subsequently transferred into the underlying substrate.

[0009] Organometallic photoresists have been shown to be promising materials for use in current and next-generation semiconductor lithography processing due to their ability to form high-resolution, high etch resistance, and high-fidelity patterns. These organometallic systems generally operate through radiation exposure-mediated formation of condensed oxide networks that drive contrast between exposed and unexposed regions of the material. A development process can then be used that can selectively remove either of the exposed or the unexposedAttorney Docket No. 5063.67W001 material to realize a physical pattern of material based on a latent image formed by the pattern of radiation.

[0010] BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Fig. 1 is a cartoon depicting radiation-induced thermal condensation of a non-additive enhanced organotin material.

[0012] Fig. 2 is a cartoon depicting radiation-induced thermal condensation of an additive-enhanced organotin material. In this depiction, the additive does not coordinate with Sn.

[0013] Fig. 3 is a cartoon depicting radiation-induced thermal condensation of an additive-enhanced organotin material. In this depiction, the additive can coordinate with Sn.

[0014] Fig. 4 is a cartoon depicting mechanisms for positive tone patterning of organotin coatings deposited from ligand leaving promoting additive enhanced and unenhanced solutions through a range of PEB temperatures.

[0015] Fig. 5 is a set of six CD-SEM images of organotin films patterned via EUV lithography to form 14 nm lines on a 28-nm pitch with the three SEM images in each column corresponding to an organotin resist film prepared with a comparative precursor solution having no additive (PRZ) or a precursor solution having an ammonium chloride additive (PRZ-H1). Both precursor solutions were prepared with a blend of precursors having primary organyl ligands and precursors having tertiary organyl ligands.

[0016] Fig. 6 is a set of six CD-SEM images of organotin films patterned via EUV lithography to form 14 nm lines on a 28-nm pitch with the three SEM images in each column corresponding to an organotin resist film prepared with a comparative precursor solution having no additive (PRQ) or a precursor solution having an ammonium chloride additive (PRQ-H1). Both precursor solutions were prepared with precursors having secondary organyl ligands.

[0017] Fig. 7 is a plot of organyl ligand fraction remaining, as determined by FTIR, through exposure dose for a triethylammonium nitrate enhanced precursor solution (PRY-CI) and a comparative unenhanced precursor solution (PRY).

[0018] SUMMARY OF THE INVENTION

[0019] In a first aspect, the invention relates to a solution comprising a blend of:

[0020] an organic solvent, an organotin composition, and an additive composition. The organotin composition can be represented by the formula RSnLi, wherein R is an organyl ligand havingAttorney Docket No. 5063.67W001 from 1 to 31 carbon atoms and optionally substituted with a heteroatom or unsaturated bond at any position and L is a hydrolysable ligand. The additive composition can be represented by the formula Q+nAn’ wherein l<n<5 A11’ is CT, Br , OH’, or an oxyanion comprising at least 1 and up to 10 oxygen atoms bonded to one or more core atoms selected from B, Si, C or group 15-17 elements, Q+is H+, onium cation [ERcm]+, or a combination thereof wherein E is a group 15 to group 17 element, each Rcis independently selected from H, 1 to 11 carbon alkyl, alkenyl, or aryl groups, and a 1 to 11 carbon hydroxyl substituted group, and are attached to E via an E-C bond, and 2<m<4 with the proviso that Q+is not H+when A11’ is OH’ or phosphite.

[0021] In a further aspect, the invention pertains to a radiation patternable organometallic coating comprising a tin oxo-hydroxo network with organo ligands bonded to the tin via Sn-C bonds and incorporated additive, wherein the organo ligands comprise group with 1-31 carbon atoms with optional unsaturated carbon bonds wherein one or more carbon atoms are optionally substituted with heteroatoms. Generally, the incorporated additive is provided in a formulation represented by the formula Q+nAn’ wherein l<n<5 A is O’, Br’, OH’, or an oxyanion comprising at least 1 and up to 10 oxygen atoms bonded to one or more core atoms selected from B, Si, C or group 15-17 elements, Q+is H+, onium cation [ERcm]+, or a combination thereof wherein each Rcis independently selected from H, 1 to 11 carbon alkyl, aryl, and 1 to 11 carbon hydroxyl substituted groups, and are attached to E via an E-C bond, and 2<m<4, with the proviso that Q+is not H+when A11’ is OH’ or phosphite.

[0022] In another aspect, the invention pertains to a method for patterning an organometallic coating comprising a tin oxo-hydroxo network with organo ligands bonded to the tin via Sn-C bonds and an additive incorporated into the coating as provided in a precursor represented by the formula Q+nAn’ wherein l<n<5 A is O’, Br’, OH’, or an oxyanion comprising at least 1 and up to 6 oxygen atoms bonded to a core atom selected from B, Si, C or group 15-17 elements, Q is H+, onium cation [ERcm]+, or a combination thereof wherein each Rcis independently selected from H, 1 to 11 carbon alkyl, aryl, and 1 to 11 carbon hydroxyl substituted groups, and are attached to E via an E-C bond, and 2<m<4, with the proviso that Q+is not H+when A11’ is an OH’ or phosphite, wherein the organo ligands comprise 1-31 carbon atoms with optional unsaturated carbon bonds wherein one or more carbon atoms are optionally substituted with heteroatoms, the method comprising:

[0023] exposing a pattern of radiation of the coating to form a latent image comprising exposed and unexposed regions andAttorney Docket No. 5063.67W001 developing the coating with a developer composition to selectively remove either the exposed material or the unexposed material.

[0024] DETAILED DESCRIPTION OF THE INVENTION

[0025] Stable organotin precursor solutions enhanced with organyl ligand leaving promoting additives have been formulated and offer advantages for lithographic processing of coatings formed therefrom. Generally, the organyl ligand leaving promoting additives can be added to organotin precursor solutions to introduce ions, for example hydroxyl, halogens, and oxyanions, or oxidizing agents to organotin films. The oxidizing agents are generally characterized as compounds having atoms in high oxidation states. Atoms in high oxidation states can possess a high electron affinity to achieve a more stable lower oxidation state. Similarly, and owing to their electron configuration, halogens in high oxidation states generally possess high electron affinities. The high electron affinity of ligand leaving promoting additives can produce interactions with organotin oxo-hydroxo networks wherein Sn-C bond cleavage (sometimes referred to as dealkylation or organyl ligand displacement) is promoted and Sn-O-Sn linkages may occur more readily when ligand leaving promoting compounds are active. The additives can enhance dissolution contrast or etch selectivity contrast to enable improved positive or negative tone patterning of organometallic photoresist materials upon development of the irradiated material. In some embodiments, organotin films comprising an organyl ligand leaving promoting additive can exhibit a dose reduction without significantly compromising patterning performance. In other embodiments, patterning performance improvements are observed sometimes in conjunction with dose increases or roughly equivalent doses. In some embodiments, radiation induced thermal Sn-C bond cleavage can occur to an increased extent at selected process temperatures for organotin coatings enhanced with one or more ligand leaving promoting additives. This last effect can amplify dose reduction to obtain target patterning performance. Thus, in some embodiments, the additives described herein provide a promising path to effectively lower dose requirements without sacrificing patterning performance.

[0026] Organotin compounds, particularly those based on mono-organotin trialkoxide (RSn(OR')3) and mono-organotin triamide (RSn(NR'2)s) precursor compounds, are useful compositions for extreme ultraviolet (EUV) lithography. Organotin compounds can also be referred to as alkyltin compounds, and the terms are used interchangeably herein as well asAttorney Docket No. 5063.67W001 generally in the art. The use of organotin compounds in high performance radiation-based patterning compositions is described, for example, in U.S. patent 9,310,684 to Meyers et al., entitled "Organometallic Solution Based High Resolution Patterning Compositions," incorporated herein by reference. Refinements of these organometallic compositions for patterning are described in U.S. patents 10,642,153 to Meyers et al., entitled "Organometallic Solution Based High Resolution Patterning Compositions and Corresponding Methods," and 10,228,618 to Meyers et al. (hereinafter the '618 patent), entitled "Organotin Oxide Hydroxide Patterning Compositions, Precursors, and Patterning," both of which are incorporated herein by reference.

[0027] The alkyltin (organotin) precursor compositions generally comprise a ligand that can be hydrolyzed with water or other suitable reagent under appropriate conditions to form mono-organo tin oxo-hydroxo patterning compositions, generally as solid coatings, which, when fully hydrolyzed in terms of removing hydrolysable ligands, can be represented by the formula RSnO(i.5-(x / 2))(OH)xwhere 0 < x < 3. It can be convenient to perform the hydrolysis to form the oxo-hydroxo compositions in situ, such as during deposition and / or following initial coating formation. Mono-organo tin precursor compositions can generally be represented by the formula RSnLi, where R is an organyl group bonded to the tin atom via a radiation-sensitive Sn-C bond and L is a hydrolysable ligand. For processing to form radiation patternable coatings, L is generally hydrolyzed before or during (e.g., in-situ) deposition to result in a coating comprising a polymeric organotin oxo-hydroxo composition on a substrate wherein the Sn-C bonds remain substantially intact. As a result, a radiation patternable coating having radiationsensitive Sn-C bonds can be realized. R generally can comprise 1 to 31 carbon atoms, optional heteroatoms, optional unsaturated or aromatic groups, and a large variety of such R groups have been exemplified since Applicant originally developed this class of organotin patterning compositions.

[0028] The R group, alternatively referred to as the organyl ligand, that forms a C-Sn bond generally has from 1 to 31 carbon atoms with 3 to 31 carbon atoms for the secondary-bonded carbon atom and 4 to 31 carbon atoms for the tertiary-bonded carbon atom embodiments, for example, methyl, ethyl, propyl, butyl, propenyl, butenyl, pentenyl, isomers thereof, and branched alkyl. In particular, branched alkyl ligands represented by R1R2R3C where R1and R2are independently an alkyl group with 1-10 carbon atoms, and R3is hydrogen or an alkyl group with 1-10 carbon atoms. In some embodiments R1and R2can form a cyclicAttorney Docket No. 5063.67W001 alkyl moiety, and R3 may also join the other groups in a cyclic moiety. Suitable branched alkyl ligands can be, for example, isopropyl (R1and R2are methyl and R3is hydrogen), tert-butyl (R1, R2and R3are methyl), tert-amyl (R1and R2are methyl and R3is — CHCH3), sec-butyl (R1is methyl, R2is — CHCH3, and R3is hydrogen), n-pentyl, sec -pentyl, isopentyl, neopentyl. Examples of suitable cyclic groups include, for example, cyclohexyl, cyclopentyl, cyclobutyl, and cyclopropyl, 1-adamantyl ( — C(CH2)3(CH)3(CH2)3 or tricyclo(3.3.1.13,7) decane bonded to the metal at a tertiary carbon) and 2-adamantyl ( — CH(CH)2(CH2)4(CH)2(CH2) or tri cyclo(3.3.1.13, 7) decane bonded to the metal at a secondary carbon). In other embodiments organyl groups may comprise unsaturated groups, including aryl, or alkenyl groups, for example benzyl, allyl, or alkynyl groups. In other embodiments the organyl ligand R may include any group consisting solely of C and H, and comprising 1-31 carbon atoms. For example: linear or branched alkyl t'Pr, ‘ Bu, Me,nBu), cyclo-alkyl (cyclo -propyl, cyclo-butyl, cyclo-pentyl), olefinic (alkenyl, aryl, allylic), or alkynyl groups, or combinations thereof. In further embodiments suitable R-groups may include organyl groups substituted with hetero-atom functional groups selected from cyano, thio, silyl, ether, keto, ester, acetal, ketal, or halogenated groups or combinations thereof. In some embodiments, R can be a ligand with one or more carbon atoms optionally substituted with one of more heteroatoms selected from the group consisting of O, S, N, Se, Te, Si, Ge, Sn, F, and I. As generally used in the art, organo, organyl, alkyl and hydrocarbyl can be used interchangeably in reference to ligands without restricting incorporation of unsaturated bonds or heteroatoms.

[0029] In some embodiments, R can be an organic ligand comprising an acetal group represented by the formula (OR4)(OR3)R2CR1, wherein R1is a substituted or unsubstituted hydrocarbyl group having from 1 to 15 carbon atoms and a Sn — C bond, R2is hydrogen or a substituted or unsubstituted hydrocarbyl group having from 1 to carbon atoms, wherein R3and R4are independently substituted or unsubstituted hydrocarbyl groups having 1 to 4 carbon atoms or wherein R3and R4collectively form a bridging structure — OR5O — (R5=R3+R4) where R5is a hydrocarbyl group having 1 to 10 carbon atoms and forms a cyclic linkage between the acetal O atoms. As used presently in the art, acetal refers to either a traditional acetal group or a ketal group. Organotin compositions comprising acetal ligands have previously been disclosed by Applicant in published U.S. Patent Application No. 2025 / 0074930 to Marwitz, et al. entitled ‘Organotin Compositions Having Eigands WithAttorney Docket No. 5063.67W001 Acetal Functional Groups, Patterning Compositions With Organotin Blends And Positive Tone Patterning’, which is hereby incorporated by reference. The previous results with the acetal group ligands demonstrated desirable positive-tone patterning.

[0030] Each R group individually and generally can have from 1 to 31 carbon atoms with 3 to 31 carbon atoms for the group with a secondary-bonded carbon atom and 4 to 31 carbon atoms for the group with a tertiary-bonded carbon atom, optionally with unsaturated or aromatic carbon bonds and with optional heteroatoms. Groups with unsaturated carbon bonds and no hetero atoms can be described as a branched or linear alkyl group with an overall stoichiometry of CnH2(n-i)+3, n=l to 31. In particular, branched or cyclo alkyl (unsaturated) ligands can be desirable for some patterning compositions. The formation of the oxo-hydroxo coating material can comprise deposition of one or more tin composition(s) with hydrolysable bonds, such as RSnLi, where L is a hydrolysable ligand, such as an alkoxide (OR'), a dialkyl amine (NR'2), an acetylide (C=CR'), or other suitable hydrolysable ligand. Suitable L ligands can include alkylamido or dialkylamido ( — NR1R2, where R1and R2arc independently hydrocarbon groups with 1-10 carbon atoms or hydrogen), siloxo ( — OSiR^R3, where R1, R2, and R3are independently hydrocarbon groups with 1-10 carbon atoms), silylamido ( — N(Si R ) (R2), where R’ and R2are independently hydrocarbon groups with 1-10 carbon atoms), disilylamido ( — N(SiR1s) (SiR23) where R’ and R2are independently hydrocarbon groups with 1-10 carbon atoms), alkoxo or aryloxo ( — OR, where R is an alkyl or aryl group with 1-11 carbon atoms), azido ( — N3), alkynido ( — C=CR, where R is a hydrocarbon group with 1-9 carbon atoms), amidato ( — NR1(COR2) where R’ and R2are independently hydrocarbon groups with 1-7 carbon atoms or hydrogen), amidinato ( — NR ’C (NR2) R3) where R’.R2, and R3are independently hydrocarbon groups with 1-8 carbon atoms or hydrogen), imido ( — NiCOR1) (COR2), where R1and R2are independently hydrocarbon groups with 1-8 carbon atoms or hydrogen), or fluorinated analogues thereof. The hydrolysable ligands can be hydrolyzed to form the oxo-hydroxo network during deposition of the coating and / or in the coating following deposition, i.e., completing the hydrolysis after deposition. Applicant has developed methodologies to efficiently and effectively form a wide range of patterning compositions with different R groups, optionally with various hetero atoms, with C-Sn bonds, as described further in published U.S. patent application 2022 / 00064192 to Edson et al. (herein the ‘192 application), entitled "Methods to Produce Organotin Compositions With Convenient Ligand Providing Reactants," incorporated herein by reference.Attorney Docket No. 5063.67W001 Processing of the organotin precursor compositions to afford organotin oxo-hydroxo coatings generally involves hydrolysis of the RSnLt composition(s) to form the related organotin oxo-hydroxo composition(s). Hydrolysis can be performed prior to the deposition process to yield soluble organotin oxo-hydroxo species (i.e., clusters, oligomeric species, etc.). These soluble organotin oxo-hydroxo species can then be dissolved and / or dispersed into a suitable solvent to form an organotin photoresist solution that can then be deposited to form radiation-patternable organotin oxo-hydroxo coatings. Alternatively and desirably, the RSnLt compositions can be directly dissolved in a suitable solvent to form a photoresist precursor solution that can then be used to deposit radiation-patternable organotin oxo-hydroxo coatings. Thus, the organotin precursor compositions can also be hydrolyzed in-situ with water or any suitable water forming reagent during the substrate coating process, such as during vapor deposition. Various processing options are described further in the ‘684 and ‘618 patents referenced above.

[0031] For organotin photoresist compositions wherein the organotin precursor(s) are dissolved into a solvent for spin-coating or similar solution-based deposition methods, organotin trialkoxides (triorganooxides) RSnLi, L = OR', where R' is an organyl group with at least one C atom, optional heteroatoms and optional unsaturated groups) can be desirable for use. Some advantages to organotin trialkoxide compositions are, for example, the high thermal and hydrolytic stability relative to organotin triamide compositions. While organotin triamides can be useful as precursors in vapor-based deposition methods (such as described in the ‘618 patent), organotin trialkoxides also possess appreciable vapor pressures and low melting points which also makes them attractive compounds for use in vapor deposition methods to prepare radiation-patternable coatings. In any case, the choice of organotin precursors used to produce radiation-patternable organotin oxide hydroxide films can be largely driven by processing considerations and / or limitations.

[0032] For deposition of organotin oxide hydroxide films via spin-coating, the hydrolysis of RSnLt compounds is generally achieved during the spin-coating process (i.e., in-situ hydrolysis) due to the presence of moisture in the ambient environment. In the spin-coating process, an aliquot of an organotin photoresist solution is deposited onto the surface of a substrate (e.g., a silicon wafer) which is then rotated rapidly. The rapid rotation causes the photoresist solution to spread evenly across the surface of the wafer which dramatically increases the surface area to volume ratio of the photoresist solution. Solvent evaporation asAttorney Docket No. 5063.67W001 well as hydrolysis and / or condensation reactions during spin coating and further thermal processing can drive the transition from organotin precursor species to an organotin oxo-hydroxo based coating. In some embodiments, the humidity or composition of the ambient spin coating environment can be controlled to influence film formation mechanisms and resulting coating morphologies. Applicant has described suitable apparatuses and methods for spin coating organotin precursor solutions in controlled environments in U.S. Provisional Application No. 63 / 995,537 to De Schepper, et al. entitled “Improved Deposition and Processing Methods for Organometallic Photoresists”, which is hereby incorporated by reference in its entirety.

[0033] As used herein, the term contrast refers to the dissolution (solubility) difference or etch rate difference between the exposed and unexposed regions of the organotin based coating. Contrast is generally measured by plotting post- development thickness remaining as a function of irradiation dose. In some embodiments, the contrast values may not exactly mirror the realized physical contrast between removed and remaining regions upon development. Various factors including but not limited to developer composition and development time can contribute to further mechanistic complexity and discrepancies between the exposed latent image and the physical photoresist pattern extracted during development. As used herein, dose reduction refers to a decrease in the dose necessitated to achieve a target critical dimension (CD), such as the width of patterned line space features or diameter of pillar or contact hole features using positive or negative tone development. The dose to achieve a target critical dimension can be referred to as dose-to-size. As used herein, the term critical dimension can refer to the target size dimension of a selection from wide variety of features, for example line width, space width, hole diameter, pillar diameter, or more broadly any other feature dimension, depending on the patterned structures. Ligand leaving promoting additives can generally increase contrast by amplifying changes in etch or dissolution resistance of the exposed regions. More efficient organic ligand cleavage in the exposed region is exemplified herein for an organotin based coating with a ligand leaving promoting additive. While increased contrast from more efficient organic ligand cleavage can generally improve patterning performance as indicated, for example, by metrics such as reduced patterning dose, line width roughness (LWR) and detectivity, the exacerbation of stochastic effects resulting from dose reductions can simultaneously increase roughness metrics to some extent. However, with appropriately selected additives, the contrast improvements can function to enable dose reductions withoutAttorney Docket No. 5063.67W001 significantly compromising patterning performance. With no additive present, dose reductions can generally be realized through processing changes, such as higher PEB temperatures, which can cause significant performance degradations in LER and / or resolution.

[0034] The formation of coating materials with performance improving additives is performed through the deposition of a precursor solution, and the precise structure of species, which may be transient in solution, may not be known. Nevertheless, gelling is controlled to help maintain processability of the precursor solution, avoid instability and provide a reasonable shelflife for commercial patterning compositions. In particular, gelling can result in precipitation resulting in undesirable changes over time of the composition and reduction of shelf life. It has been found that controlling the amount of water in the precursor solution can be desirable for process uniformity without excessively sacrificing shelflife, as described further below. In some cases, organotin photoresist precursor solutions can be formulated to comprise cluster compositions where multiple RSn moieties are linked through Sn-O-Sn, Sn-OH-Sn, or Sn-COO-Sn bonds, that can amass into structures such as, for example, in the dodecameric “football” clusters [(RSn)i2Oi4(OH)e]2+and the hexameric “drum” clusters [RSnOOCR' . Control of the amount of water can limit clustering in solution and without being limited by theory, suppressing clustering to retain the precursor species as monomeric or low-order clusters (ie. less than dodecamer) can be desirable for forming more amorphous coatings, which can be desirable for patterning coatings with small features and low roughness. The use of tin dodecamer clusters for patterning is described in U.S. patent 11,392,028 to Cardineau et al., entitled "Tin Dodecamers and Radiation Patternable Coatings With Strong EUV Absorption," incorporated herein by reference. Some of the additive anions described herein having oxidative properties have been described in the context of dodecamer ligands for making a patterning coating, in which these anions are exchanged within preformed dodecamers, See. published U.S. patent application 2025 / 0147416 to Kim et al., entitled "Photoresist Composition," incorporated herein by reference. In contrast, the present invention is directed towards solutions formed primarily from monomeric precursor species, which may form various transient clusters in solution, as contrasted with solutions formed by combining pre-formed tin dodecamers in a solution. The solutions described herein are generally formulated under conditions that do not facilitate complete dodecamer formation, for example, with a water concentration of > 10,000 ppm, whereas water concentrations over 10,000 ppm can generate complete transformation of monomers into dodecamers. When some water is present, some transient cluster formation isAttorney Docket No. 5063.67W001 expected, and in resulting films formed from coating the precursor composition, clusters can influence the film properties while still forming an oxo-hydroxo network through the film. Control of processing conditions may influence the degree of cluster formation in solution as well as in the deposited material in the context of an oxo-hydroxo network in the deposited film, and further processing for pattern formation may or may not be influenced by the degree of clustering within the oxo-hydroxo network. In general, the patterning compositions described herein are formulated to have low clustering in solution and correspondingly low order in resulting coatings to provide desirable patterning performance.

[0035] Generally, organotin coatings can be patterned via irradiation, wherein a radiation source, for example extreme ultraviolet (EUV), ultraviolet (UV), far ultraviolet (FUV), deep ultraviolet (DUV), or electron-beam (EB) is directed through a mask on to the coating to form a latent image comprising exposed and unexposed regions. The exposed regions generally undergo organic cleavage to some extent, owing to the radiation-sensitive nature of the Sn-C bonds. The organic cleavage in tin species in the exposed regions can directly or indirectly generate contrast between the nominally unexposed regions and the contrast can be extracted as a physical pattern upon development. This mechanism is depicted in Fig. 1. Unexposed organotin material 101 is depicted as an oxo-hydroxo network with tin oxo-hydroxo cores 103 bonded to organyl ligands 105 via Sn-C bonds 107 with Sn-OH bonds 109 and Sn-O-Sn linkages 111 and with some potential clustering within the network vaguely suggested. After exposure and an optional post exposure bake (PEB) step 102, the exposed material is transformed into condensed organotin material 113 having additional Sn-O-Sn linkages and / or additional Sn-OH bonds which are associated with some further crosslinking 115 and / or condensation of the oxo-hydroxo network. As compared to the corresponding unexposed organotin material, condensed organotin material 113 has a higher oxide character and fewer organyl ligands and generally exhibits a distinct difference in etch rate or dissolution rate from unexposed which can be leveraged to form negative or positive tone physical patterns during development.

[0036] The efficiency of this mechanism can be improved with the addition of an organyl ligand leaving promoting additive. The design of the compositions can be with regard to improving patterning performance metrics such as detectivity or line edge roughness (LER) and / or decreasing the dose-to-size. An improved mechanism is depicted in Fig. 2, which illustrates a mechanism of patterning an additive enhanced organotin material wherein theAttorney Docket No. 5063.67W001 organyl ligand leaving promoter additive creates a localized environment wherein organic ligand cleavage allows for organic ligand removal and the subsequent condensation, and formation of Sn-O-Sn bonds occurs more readily. The process in Fig. 2 can be contrasted with the process depicted in Fig. 1. Referring to Fig. 2, unexposed organotin material 201 is depicted as an oxo-hydroxo network with tin oxo hydroxo cores 203 bonded to organyl ligands 205 via Sn-C bonds 207 with Sn-OH bonds 209 and Sn-O-Sn linkages 211 and with some potential clustering within the network vaguely suggested. The organotin material further comprises ligand leaving promoting additive 213 After exposure and an optional post exposure bake (PEB) step 202, the unexposed material is transformed into condensed organotin material 215 having additional Sn-O-Sn linkages, Sn-OH bonds and further crosslinking 217 and / or condensation the oxo-hydroxo network. As compared to the condensed organotin material 113 of Fig. 1, condensed organotin material 215 has more crosslinking sites, less organyl ligands remaining and with appropriate processing, a distinctly different etch rate or dissolution rate contrast with respect to the corresponding unexposed materials. Thus, at lower exposure doses the additive enhanced material can undergo sufficient organic cleavage and / or condensation to generate contrast relative to the unenhanced material.

[0037] While not wanting to be limited by theory, it is believed that in some embodiments the ligand leaving promoting additive can coordinate with a tin atom. In addition to the four ligands in the precursor composition, Sn+4can take one or two additional ligands, and the hydrolysable ligands can be replaced through nucleophilic substitution. Fig. 3 depicts a mechanism of patterning an additive enhanced organotin material wherein a ligand leaving promoting additive can promote organic cleavage by creating a localized environment and / or by coordinating with tin atoms, thereby creating an environment at the tin ion promoting the organic cleavage. Unexposed organotin material 301 is depicted as an oxo-hydroxo network with a tin oxo hydroxo cores 303 bonded to organyl ligands 305 via Sn-C bonds 307 with Sn-OH bonds 309 and additional Sn-O-Sn linkages 311. The material further comprises ligand leaving promoting additive 315 and 317. Notably and in contrast to the mechanism depicted in Fig. 2, organotin material 301 has a mixture of ligand leaving promoting compounds coordinated to tin atoms 315 and ligand leaving promoting compound 317 as an un-coordinated additive. Without wanting to be limited by theory, this depiction illustrates the theory that the inclusion of ligand leaving promoting compound in the deposited photoresist coating can promote loss of organyl ligands (dealkylation) via different mechanisms that may involveAttorney Docket No. 5063.67W001 transient species and / or ligand exchange. After exposure and optionally a post exposure bake (PEB) step 302, condensed organotin material 319 has a significantly increased number of Sn-O-Sn linkages, Sn-OH bonds, and / or crosslinking sites 321 in comparison to the non-additive enhanced condensed organotin material 115 of Fig. 1. Thus, at lower exposure doses the additive enhanced material can undergo sufficient organic cleavage and / or condensation to generate contrast relative to the unenhanced material. Applicant does not propose any specific mechanism at this time and potentially a plurality of mechanisms can play some role.

[0038] Ligand leaving promoting additives generally are salts with selected anions and cations, although in some embodiments the cation can be a proton such that the additive becomes a neutral acid, or a combination of cations and protons to form a partially protonated salt. Suitable additive anions can be organized into different groups, which may involve different characteristics within the radiation sensitive films. The bonds formed between the additive anion and tin atom and / or of the additive anion integrated into the oxo-hydroxo network can be highly polar which can increase the hydrophilicity of the film as a whole. In some embodiments, the anion is an oxygen-rich oxyanion which can increase the hydrophilicity of the film due to the presence of highly polar oxo bonds. In other embodiments, the anion can be a chloride or bromide ion. Due to changes in the structure upon irradiation, the coordination and resulting hydrophilic properties may be accentuated in the irradiated region, and in a sense, the coordination and resulting polarity may provide an additional route of contrast generation for wet development processes, thereby alleviating the reliance on organic cleavage to generate contrast. The various effects of the additive can reduce the required dose to generate a suitable contrast for development. The additional route of contrast generation may also improve the overall contrast generated between the irradiated and non-irradiated regions.

[0039] Furthermore, increased polarity of the film can be particularly beneficial in positive tone imaging applications. Organotin films such as those described in this disclosure can generally be hydrophobic in nature and suffer from poor development quality with aqueous base developer solutions, for example aqueous solutions of 2.38% tetramethyl ammonium hydroxide (TMAH). Poor development quality can result in residual photoresist material on the substrate, which is commonly referred to in the art as scumming. Film hydrophilicity can generally be measured by its contact angle with a water droplet. Improved hydrophilicity can be desirable for aqueous development processes, such as positive-tone development with aqueous bases, such that better wetting, coverage, and interaction between the film and theAttorney Docket No. 5063.67W001 developer solution is achieved. Organotin coatings formed from ligand leaving promoting additive-enhanced organotin precursor solutions can exhibit lower water droplet contact angles and therefore increased hydrophilicity, as exemplified herein.

[0040] Without being limited by theory, it is believed that two concurrent mechanisms can occur during irradiative exposure and subsequent thermal processing of the organotin-based coatings. The first is a dealkylation mechanism wherein Sn-C bonds are cleaved, thereby eliminating some organic ligands from the tin oxo-hydroxo matrix and generally increasing the material’s solubility in a positive tone developer composition, for example an aqueous base, , and generally decreasing the material’s solubility in a negative tone developer composition, for example, organic solvents. The second is a condensation mechanism wherein Sn-O-Sn bridges are formed, particularly during post-irradiation heating of the material, thereby increasing the metal oxide character of the coating and can lead to denser and less soluble irradiated material. A goal of positive tone patterning can be to modulate the exposure dose and PEB temperatures and durations to achieve organic cleavage and removal sufficient to render the exposed region soluble in the positive tone developer composition without causing excessive condensation which can render the entire coating less soluble to the positive developer composition. Although the organic cleavage and condensation mechanisms can proceed concurrently and can even exhibit kinetic coupling in some instances, the respective extents of organic removal and condensation can be each modulated somewhat independently to affect patterning performance through the incorporation of oxyanions or halide ions into the material, such as through inclusion of ligand leaving promoting additives.

[0041] To the extent that the incorporation of oxyanions or halide ions into the material, such as through adding a ligand leaving promoting additive, can decrease the radiation induced thermolysis temperature of the Sn-C bonds within the organotin based coating, thorough and sufficient organic cleavage can be achieved at lower PEB temperatures. The use of a lower PEB temperature can limit the extent of non-radiation induced thermolysis driven condensation, which can improve the solubility contrast between exposed and unexposed regions with either a positive tone developer or a negative tone developer. The inclusion of oxyanions and / or halide ions, such as using the ligand leaving promoting additives described herein, can provide a method of achieving sufficient organic removal in irradiated material at a lower dose and / or PEB temperature without sacrificing pattern quality.Attorney Docket No. 5063.67W001 While not wanting to be limited by theory, Fig. 4 illustrates proposed structures of radiation exposed tin-based films at varying PEB temperatures. A ligand leaving promotor enhanced organotin-based material 401 comprises alkylated organotin species 403 and ligand leaving promoter additive 405. A comparative non-enhanced organotin-based material 411 comprises alkylated organotin species 403. While not wanting to be limited by theory, the additive can decrease the radiation induced thermolysis temperature of the organic ligands. The additive enhanced material is subjected to a relatively low PEB temperature and undergoes significant organic removal to yield an additive enhanced lower temperature baked material 407 comprising sufficiently organic cleaved organotin species 409. The additive enhanced lower temperature baked material has high solubility to a positive tone developer composition. Contrastingly, the non-enhanced material is subjected to the same relatively low PEB temperature and undergoes less organic removal to yield a nonenhanced lower temperature baked material 413 comprising insufficiently organic cleaved organotin species 415. The non-enhanced lower temperature baked material retains a low solubility to a positive tone developer composition. At the same lower PEB temperature, the additive enhanced material generates higher contrast between the exposed and unexposed regions than the non-enhanced material. The non-enhanced material is subjected to a higher temperature PEB to induce sufficient organic cleavage and yield a non-enhanced high temperature baked material 417. Although the non-enhanced higher temperature baked material undergoes significant organic cleavage to comprise sufficiently organic cleaved organotin material 409, significant crosslinking 419 forms at the high PEB temperature. The non-enhanced higher temperature baked material is crosslinked and denser and thus retains low solubility to a positive tone developer composition and reduced contrast between the exposed and unexposed region is generated. The additive may or may not be removed by processing, including the PEB, as described further below. The structures schematically depicted in Fig. 4 are intended to be illustrative and may not correspond to the actual chemical structures of the tin-based films. While not wanting to be limited by theory, the figures are intended to convey proposed mechanistic distinctions between additive enhanced and non-enhanced organotin materials.

[0042] In some embodiments, the interaction of anions with the tin oxo-hydroxo network can generally reduce the radiation dose necessary to produce patterned features of a target characteristic dimension at certain temperatures, as exemplified herein. Appropriate selectionAttorney Docket No. 5063.67W001 of the cations may also provide beneficial effects, as described further below. By providing an additive as an alternate means of increasing the organotin material’s contrast, i.e., resistance of appropriate portion of material to removal by a developer solution, gas, or plasma, the interaction of anions with the tin oxo-hydroxo film can alleviate, to some degree, the dependence on increasing dose for cleaving organic ligands attached by Sn-C bonds to generate contrast. The patterning of additive enhanced organotin compositions described herein can necessitate a lower radiation dose to achieve a target critical dimension (CD) than a nonadditive enhanced equivalent photoresist. In some embodiments, the patterning can be performed by irradiating an additive enhanced organotin material with patterned EUV radiation at a dose at least about 1% lower, in other embodiments at least about 5% lower, and in further embodiments at least about 20% lower, and in even further embodiments at least about 50% lower, and in some embodiments from about 10% lower to about 75% lower than a corresponding dose needed to produce equivalent pattern dimensions for an otherwise equivalent non-additive enhanced organotin coating without the additive at the same coating thickness, the same PAB and PEB conditions, and using the same selected developer. The exposure dose-to-size can vary between processing for comparable samples although statistical variation is generally within ±10%. In some embodiments, when the exposure dose is reduced by a percentage due to the presence of an additive, a corresponding stochastic increase in line width roughness (LWR) can be less than or equal to the dose reduction percentage within a tolerance of ±10%. The dose decreases can translate into reduced irradiation times and a correspondingly increased throughput and reduced costs.

[0043] While irradiative exposure serves to develop some initial solubility contrast, the material may thereafter be subjected to a post exposure bake (PEB) to induce further organic removal in the irradiated regions through a phenomenon termed radiation induced thermolysis. Sn-C bonds can decompose at certain temperatures through a thermolysis driven mechanism during baking, although irradiation induces enhanced thermolysis. To achieve desired contrast, it is desirable for unexposed material to have a low level of thermolysis compared to the exposed material. The contrast can be improved by the presence of the ligand leaving promoting additive by enabling the exposed material to undergo radiation induced thermolysis at lower temperatures. The removal of organyl ligands through irradiative exposure locally decreases the thermal stability of adjacent remaining organyl substituents by lowering the bond dissociation energy (BDE) of the Sn-C bonds. Data suggests that the addition of a ligandAttorney Docket No. 5063.67W001 leaving promoting additive can decrease the thermolysis temperature of the organyl ligands of the exposed material to induce greater organic removal during a PEB step. PEB temperatures can be carefully selected and optimized by leveraging this phenomenon to selectively promote organic removal in irradiated regions while maintaining the chemical structure of the unexposed region. More thorough organic removal can be realized by increasing the efficacy of radiolysis induced thermolysis through the addition of a ligand leaving promoting additive. While not wanting to be limited by theory, it is believed that ligand leaving promoting additives can influence the chemical environment within the irradiated regions to render the remaining Sn- C bonds more susceptible to cleavage through thermolysis during PEB processing.

[0044] Specifically, a unique behavior can be observed for coatings comprising organyl ligand leaving promoter additives when dry development methods are utilized as a developing means. Additive-enhanced coatings can generally exhibit larger dose increases or decreases at higher PEB temperatures for particular additives, while the effect can be unsubstantial or even opposite at lower PEB temperatures, suggesting that the additive may influence the radiation induced thermolysis mechanism. This effect can be realized for both alkylammonium salts having hydroxide, halogen, or oxyanion components as well as conjugate acid forms of oxyanions or halogens. This effect is exemplified herein for some non-limiting embodiments of ligand leaving promoting additives. While not wanting to be limited by theory, this suggests that while the ligand leaving promoter additives can reduce the dose for both wet and dry development techniques, the mechanism for generating dissolution and etch resistance contrast may differ and / or have different degrees of thermal dependence. In any case, the ligand leaving promoting additives can be effective for realizing dose reductions with both wet a dry development approaches.

[0045] As noted above, the ligand leaving promoter additive is generally a salt. In some embodiments, the cation is a proton while the anion would be a conjugate base of an acid, and for these embodiments, the additive becomes a neutral molecule. Applicant has previously recognized usefulness of phosphonate additives, which include phosphonic acids and their esters. See published U.S. patent application 2026 / 0036901 to Voss et al., entitled "Organometallic Compositions With Phosphonate Additives for EUV Patterning," incorporated herein by reference. The present additives avoid this earlier work. With respect to the presently introduced additives, additive compositions are represented by the formula Q+nAn" wherein l<n<5, where the anion A11’ is Cl’, Br’, OH’, or an oxyanion comprising at leastAttorney Docket No. 5063.67W001 1 and up to 10 oxygen atoms bonded to one or more core atoms selected from B, Si, C or group 15-17 elements, and cation Q+is H+, onium cation [ERcm]+, or a combination thereof wherein E is a group 15 to group 17 element , each Rcis independently selected from H, 1 to 11 C alkyl, aryl, and a 1 to 11 C alcohol attached to E via an E-C bond and 2<m<4 with the proviso that Q+is not H+when A11’ is OH’ or phosphite. The following discussion elaborates on the additive compositions.

[0046] As noted below, Applicant's previous work has identified fluoride ions and iodine species as being useful constituents in organotin patterning compositions. This earlier work relied upon identified aspects of these species in providing reasons to introduce these species. In the further developments herein, other desirable anions are identified as useful in additives including, chloride ions and bromide ions.

[0047] In some embodiments, the anion can be an oxyanion comprising at least one core atom selected from B, C, Si or group 15, 16, or 17 elements and at least one and up to ten oxygen atoms. In some embodiments, the oxyanion can comprise one, two, three, four, five, or six oxygen atoms bonded to one or more core atoms selected from B, C, Si or group 15, 16, or 17 elements. Oxyanions are generally known to be strong oxidizing agents, owing to the high oxidation state of the non-oxygen core atoms therein. Electron withdrawing properties of oxygen atoms give rise to high oxidation states of the non-oxygen core atoms. In some embodiments, the oxidation state of the core atom can be +1, +2, +3, +4, +5, +6, or +7. In some embodiments, the oxyanions have from about 1 to about 8 oxygen atoms, while in other embodiments the oxyanions have from about 2 to about 5 oxygen atoms, and from about 2 to about 3 oxygen atoms in further embodiments. A person of ordinary skill in the art will realize that oxyanions having oxidation states and a number of oxygen atoms contained within the explicit ranges above are contemplated and are within the present disclosure.

[0048] In some embodiments, useful oxyanions for ligand leaving promoters can be one of or any combination of oxyanions selected from the group consisting of borate (BO33), orthosilicate (SiCh4), metasilicate (SiOs2), carbonate (CO32) nitrate (NO3 ), nitrite (NO2 ), sulfate (SO42), sulfite (SO32), thiosulfate (S2O32), phosphite (HPO33), phosphate (PO43), iodate (IO3 ), ortho periodate (ICE5), meta periodate (IO4 ), chlorate (CIO3 ), and perchlorate (CIO4 ), hypochlorite (CIO ), arsenate (ASO43), arsenite (ASO33), selenate (SeO42), antimonate (SbO43), tellurite (TeO32), and tellurate (TeO42). In some embodiments, the oxyanions can be partially protonated, such as HPO42, H2PO4-, or HSO4-, and the like. In some embodiments,Attorney Docket No. 5063.67W001 the oxyanion can comprise two or more core atoms selected from B, C, Si, or group 15, 16, or 17 elements and from one to ten oxygen atoms. Suitable oxyanions comprising multiple core atoms include, for example, pyrophosphate (P2O74), tripolyphosphate (P3O105), tetraborate (B4O72), oxalate (C2O42), thiosulfate (S2O32), dithionate (S2O62), pyrosulfate (S2O72), and hyponitrite (N2O22). The anions generally do not comprise peroxo (O-O) bonds which can have unique photochemistry and this class of additives has been described by Applicant in published U.S. Patent Application No. 20250334877 to Boutilier, et al. entitled “Peroxidestabilized organotin photoresist compositions and patterning”, which is hereby incorporated by reference.

[0049] While not wanting to be limited by theory, an oxyanion’s ability to promote dealkylation, as exemplified herein, may in some embodiments involve a radical species generated from the oxyanion. Radical compounds are defined as having at least one unpaired electron. In some embodiments, the formation of a radical can be associated with further function as an oxidizing agent or as a hydrogen atom abstractor. Additionally or alternatively, the additive may be effective with respect to reactions with radiation generated species involving the organyl ligands that facilitate ultimate removal of the resulting organic reaction products. While the precise mechanism involving radical species is unknown, the addition of oxyanions, for example nitrate, which can produce radical species, for example nitric oxide (• NO) and nitrogen dioxide (• NO2), can effectively enhance the EUV sensitivity of the radiation patternable organotin coating. See, for example, Wu, et al., "Mini review on the roles of nitrate / nitrite in advanced oxidation processes: Radicals transformation and products formation," Journal of Cleaner Production, 273:123065 (November 10, 2020), incorporated herein by reference. Some oxyanions, such as nitrate, are also known to be powerful oxidizing agents under appropriate conditions. The oxidizing abilities of these anions may facilitate the organic ligand leaving process. Furthermore, and also not wanting to be limited by theory, it is believed that the decomposition of oxyanions into oxygen-containing radical species can be at least somewhat driven by radiolysis, possibly due to secondary processes such as electron quenching or absorption of scattered photons or due to EUV absorption for strong absorbers, thereby at least somewhat concentrating the formation of radical species to the irradiated regions which can enhance contrast generation. The localized formation of radical species within the irradiated region can increase the extent of Sn-C bond cleavage and the formationAttorney Docket No. 5063.67W001 of Sn-O-Sn linkages therein, to correspondingly increase the contrast between the exposed and unexposed regions.

[0050] The influence of radicals can be beneficial or detrimental depending on the circumstances. To the extent that radical generation is not localized to irradiated regions, radicals can decrease contrast through the non-radiation induced organyl ligand cleavage. Similarly, radical formation in precursor solutions can be detrimental to precursor stability. Thus, radical scavengers can be added to precursor solutions to provide desired stability. To decrease deleterious effects from radicals, further additives can be included in the precursor solutions to scavenge radicals. Such additives have been shown to be beneficial, as described in published U.S. patent Application No. 2025 / 0251662 to Eberle et al. (hereinafter the '662 application), entitled "Radical Scavenger Additives for Metal Oxide Based Resists and Precursor Solutions," incorporated herein by reference. Some radical scavengers can be volatile, so that they are removed following deposition of the precursor solution and prior to irradiation to avoid interference of desired irradiation induced processes. To the extent that radiation induced radical formation is localized, it can be desirable to offset the formation of such radicals that may occur undesirably in non-irradiated regions of the film. From this perspective, in some embodiments, appropriate radical scavenging additives can be combined with the organyl ligand leaving promoting additives, although these additives should be selected to not directly react with each other under the conditions experienced in the processing.

[0051] In addition to the nitrate compounds, other oxyanions comprising group 15, 16, or 17 core atoms can form radical oxides and / or provide useful oxidizing capabilities that provide such a functionality during the patterning process. For example, iodine based oxyanions such as iodate or periodate can involve iodine in a +7 oxidation state that is a strong oxidizing agent, and sulfur based oxyanions such as sulfate, sulfite, or persulfate can react to form sulfur monoxide (• SO) and sulfur trioxide (• SO3) radicals and include sulfur in its +6 oxidation state. Phosphorous based oxyanions can react to form phosphorous monoxide (• PO) and phosphorous dioxide (• PO2) radicals, and chlorine-based oxyanions (hypochlorite, chlorite, chlorate, and perchlorate) can react to form chlorine monoxide (• CIO), chlorine trioxide (• CIO3), and chlorine tetroxide (• CIO4) radicals and hypochlorite and chlorate are particularly strong oxidizing agents. It can be possible for the oxyanions to form additional radical species which are not explicitly listed above.Attorney Docket No. 5063.67W001 Some anions may further contribute to the condensation process by forming ligands to the tin and / or by integration into the oxy-hydroxo network. In some embodiments, the anion can be hydroxide, which can then be available to ligate to tin. In some embodiments, the anion can be a halide, such as F, Cl’, Br’, or I’. Halides can also be introduced to the film as conjugate acids of the anions, such as HF, HC1, HBr, or HI. While these hydrogen halides are gases, they can be dissolved in the solvent and may ligate during the coating process. Applicant has previously described some embodiments recognizing potential desirability of fluorine or iodine as constituents in organotin material, including such additive-enhanced organotin precursor compositions and coatings formed therefrom in US Application No. 2025 / 0085627 to Cardineau, et al. entitled Organotin photoresist compositions having fluoride generator compounds, fluorinated organotin coatings and patterning and US Patent Application No.

[0052] 19 / 404,631 to Jilek, et al. Entitled “Organotin Compositions with Iodo Species and Radiation Sensitive Films”, both of which are hereby incorporated by reference. While Applicant’s previous work has described ammonium-based iodides and fluorides, the present disclosure further encompasses chlorides, bromides, conjugate acids of halogens, oxyanions of halogens, and additional ammonium-based cations not previously described. The previous work with iodo species provided identification of species that indicated ligand exchange in precursor solutions involving hydrolysable ligands, including the halide ligands. Halide ligands may be hydrolysable so the ligand structure in the precursor solutions may or may not carry over into the deposited patternable materials with available atmospheric moisture or other hydrolyzing agents available. The use of fluoride species was found to result in a decrease of the dose requirements without resulting in an increase in line edge roughness. However, as exemplified herein, the fluoride additives can be less effective for dose reduction in some embodiments while the chloride additives are highly effective, suggesting that the chloride additives can be employed to address the shortcomings of fluoride additives in certain applications, especially with low bake temperatures.

[0053] A unique behavior can be observed for some ligand leaving promoting additives wherein a dose reduction to obtain a target feature size is realized for organotin films comprising a blend of primary and tertiary organyl ligands while a dose increase is realized for organotin films comprising secondary organyl ligands. This is not observed for embodiments wherein the anion is F, rather the addition of fluoride containing compounds has been shown to produce dose reductions for organotin coatings formed from precursor solutions comprisingAttorney Docket No. 5063.67W001 primary, secondary, and tertiary organyl ligands. In some embodiments, a dose increase resulting from the addition of an organyl ligand leaving promoting additive to an organotin precursor solution comprising secondary organyl ligands can be accompanied by a decrease in line edge roughness. Decreased line edge roughness is desirable for improved pattern fidelity and decreased occurrence of defects.

[0054] As noted above, the additives can match the anions with cations that are onium ions or, in some embodiments, H+. In particular, H+has been described above in the context of halide anions. If H+is combined with oxyanions, a conjugate acid of the oxyanion is generally formed. In some embodiments, the cation is an onium ion formed using a group 15 to group 17 core elements, such as iodonium, sulfonium, ammonium, phosphonium, and the like, which can have functional groups for UV absorption. Onium ions can be components of photoacid generators (PAGs) with absorption in the UV. Onium ions can also be effective as radical scavengers or absorbers of scattered light to reduce shot noise. To provide UV absorption and increase electron scavenging function, the onium ions can have aromatic substituents or derivatives thereof, such as aromatic onium ions. Onium ions with iodine central atoms can also provide increased EUV absorption.

[0055] The onium ions in general have a structure [ERcm]+, where Rcare independently H or organyl ligands with 1-15 carbon atoms, optional unsaturated bonds, such as aromatic groups and / or optional substitutions, such as with O, N, S, halide, or combinations thereof, and E is a group 15 to group 17 core element. If at least one of the Rcis a hydrogen, the cation generally is somewhat acidic and may deprotonate under appropriate conditions to form a neutral compound. Formation of a neutral compound may result in a volatile compound, and the protonated cation is generally not volatile. The onion ions are generally selected to form salts with solubility in appropriate solvents.

[0056] Ammonium salts have been identified as particularly useful ligand leaving promoting additives, as they provide an effective means of introducing the described anions into organotin films. The ammonium cation can be ammonium (NH4+), monoalkylammonium, dialkyl ammonium, trialkyl ammonium or tetraalkyl (quaternary) ammonium cations. Since ammonium can refer to the specific species of NH4+as well as the genus of 0-4 alkyl substituted ammonium cations, the discussion herein generally refers to the genus unless specifically noted otherwise. The ammonium salts generally comprise an anion, which can be either hydroxide,Attorney Docket No. 5063.67W001 a halogen, or an oxyanion, ionically coordinated to an ammonium cation [NR1R2R3R4]+represented by the structure:

[0057] R4

[0058] R22- N I^-R 33

[0059]

[0060] R I®1

[0061] wherein R1-R4are independently either hydrogen, a hydrocarbyl group having from about 1 to about 11 carbons, which can be alkyl, aryl, or unsaturated, for example methyl, ethyl, butyl, phenyl, or butenyl or an alcohol having from about 1 to about 11 carbons and forming a C-N bond, for example methanol, ethanol, or butanol. In some embodiments, the ammonium cation is ammonium (NH4+). In some embodiments the ammonium cation is a trialkyl ammonium cation, wherein R1is H and R2-R4are independently an alkyl or aryl group having from about 1 to about 11 carbons, for example methyl, ethyl, or butyl. In other embodiments, the ammonium cation is a tetraalkylammonium cation wherein each of R ’-R4are independently selected from an alkyl or aryl group having from about 1 to about 11 carbons, for example methyl, ethyl, or butyl. In other embodiments, the ammonium cation is a hydroxy-substituted ammonium cation, wherein at least one of R1, R2, R3, or R4is an alcohol ligand, for example choline wherein R1, R2, and R3are methyl and R4is ethanol attached via a C-N bond and a free OH group.

[0062] For ammonium cations with at least one hydrogen bound to the nitrogen, deprotonation can result in a volatile amine, while providing a proton that can be available for bonding, such as with a cleaved organyl group from the organotin. Thus, ammonium cations with a labile proton are generally volatilized during spin coating to a greater extent than quaternary ammonium cations. In embodiments wherein the ammonium based cation has at least one labile proton, for example an ammonium cation (NHC), a monoalkyl ammonium cation NR'H C), a dialkyl ammonium cation (NR'2H2+), a trialkyl ammonium cation (NR'sH4), a labile proton is generally removed from the ammonium based cation to form water (HOH) and a volatile amine byproduct. While not wanting to be limited by theory, it is believed that in some embodiments in which the cations do deprotonate and volatilize prior to irradiation, the anions can be more available to coordinate with tin atoms to form highly polar ligands which are believed to contribute to the improved dose sensitivity of the photoresist coatings. This is consistent with the examples wherein trialkylammonium salts produce higher dose reductions per mole relativeAttorney Docket No. 5063.67W001 to tetraalkyl ammonium salts. In other embodiments, in which the cations do not deprotonate prior to irradiation, at least some of the anion can remain uncoordinated to tin atoms and the additive can electrostatically interact with the tin network to result in enhanced film properties, for example increased polarity, without coordinating with a tin atom. While the precise reaction mechanisms and nature of the interaction between the additive and organotin oxo-hydroxo networks are not known, the same ultimate effect from the addition of the additive to a precursor solution is achieved and additive enhanced coatings can exhibit improved sensitivity Additive salts, such as ammonium cations with additive anions, can be introduced to the organotin coating in a variety of ways. Generally, additive salts are solids at room temperature, and in some embodiments, it can be convenient to dissolve the salt in an organotin precursor solution to form an additive-enhanced organotin precursor solution comprising organic solvent, organotin composition, and additive salt present at a desired concentration. In other embodiments, the additive salt can be independently dissolved in an organic solvent and subsequently combined with a non-additive enhanced organotin precursor solution to afford an additive-enhanced organotin precursor solution with an additive salt present at a desired concentration. In some embodiments, coatings deposited from said additive-enhanced precursor solutions can incorporate the additive salt. In some embodiments, the coatings can incorporate the additive anions while deprotonated cation byproducts are volatilized such that the coating does not comprise the cation byproduct, such as an amine.

[0063] While not wanting to be limited by theory, it is believed that an onium cation with at least one proton, such as an ammonium cation, can deprotonate to form a neutral compound, such as an amine, for example ammonia, methylamine, trimethylamine, or triethylamine. Amine compounds that can form can be relatively volatile in comparison to organotin species and generally in some embodiments have boiling points under 250 °C, in some embodiments under 150 °C, and under 100 °C in further embodiments.

[0064] In some embodiments, the described oxyanions or halogens can be introduced to the organotin precursor solution or organotin coated substrate as a conjugate acid, such as an oxyacid. These embodiments correspond in the sense of the general additive salt as the cation being a proton. The conjugate acid form of the oxyanion or halogen comprises the oxyanion or halogen in addition to as many hydrogen atoms as are needed to form a net neutrally charged compound. The number of protons of the conjugate acids can vary between embodiments depending on the identity of the conjugate oxyanion or halogen and the conjugate acids can beAttorney Docket No. 5063.67W001 monoprotic, polyprotic, diprotic, triprotic, tetraprotic, or pentaprotic. For example, the conjugate acid form of nitrate, NOV, is nitric acid, HNO3, the conjugate acid form of sulfate, SO42’, is sulfuric acid, H2SO4, and the conjugate acid form of phosphate, PO43’, is phosphoric acid, H3PO4, and the conjugate acid form of ortho periodate, lOe5-, is ortho periodic acid, lOeHs, which contains five hydrogen atoms. The conjugate acid form of meta periodate IO4-is monoprotic meta periodic acid HIO4. In some embodiments, the oxyanions can be introduced to the organotin precursor solution as a partially protonated form with the remaining charge being compensated by onium cation(s) as described above. For example, PCh3-, can be partially protonated in the form of HPO42or FFPCh" and can be provided as (NR'4)2(HPO4) or (NR 4XH2PO4), respectively, where R' is defined above with respect to the ammonium cation or more generally as ER'4, where E is a group 15 to group 17 core element. Similarly, other oxyanions capable of partial protonation, such as SCh2-and lOe v can be provided as the corresponding onium salt (ER'4)n(HmA) such that n + m is equal to the charge of the bare anion, A(n+m)’, for example, (NR4XHSO4), (NRhb FEICX), and the like. Conjugate acid forms of described halogens comprise a singular hydrogen atom, for example HF, HC1, HBr, or HI.

[0065] Suitable ammonium salt based additive compositions include, for example, ammonium chloride, ammonium bromide, tetramethyl ammonium chloride, tetramethyl ammonium bromide, tetraethylammonium chloride, tetraethyl ammonium bromide, choline chloride, choline bromide, choline hydroxide, ammonium nitrate, tetramethylammonium nitrate, tetraethylammonium nitrate, ammonium sulfate, tetramethylammonium sulfate, ammonium sulfite, ammonium thiosulfate, ammonium phosphite, ammonium phosphate, tetrabutylammonium phosphate, ammonium iodate, tetraethylammonium (metajperiodate, ammonium perchlorate, tetraethylammonium perchlorate, tetramethylammonium perchlorate, tetrabutylammonium perchlorate, ammonium dihydrogen arsenate, ammonium selenate, and ammonium tellurate. Corresponding additive salts can be formed using other onium cations substituting for the ammonium cations, such as iodonium, sulfonium, phosphonium, and the like, with suitable substituents. Suitable acid based additive compositions include, for example, nitric acid, hydrochloric acid, hydrobromic acid, sulfuric acid, phosphoric acid, telluric acid, hypochlorous acid, chloric acid, perchloric acid, iodic acid, periodic acid, and selenic acid. These exemplary additive compounds are available from commercial suppliers such as Millipore Sigma (MA, US), Fisher Scientific (PA, US), or TCI Chemical (OR, US). Conjugate acids of oxyanions can be introduced to the organotin coating in a variety of ways. In someAttorney Docket No. 5063.67W001 embodiments, the conjugate acids are solids at room temperature, for example orthoperiodic acid, it can be convenient to dissolve the acid in an organotin precursor solution to form an additive-enhanced organotin precursor solution comprising organic solvent, organotin composition, and oxyanion conjugate acid present at a desired concentration. In some embodiments, the conjugate acids of oxyanions are liquids at room temperature and can be combined to form an additive enhanced organotin precursor solution in like fashion. In other embodiments, the oxyanion conjugate acid can be independently dissolved in a solvent and subsequently combined with a non-additive enhanced organotin precursor solution to afford an additive-enhanced organotin precursor solution with an oxyanion conjugate acid present at a desired concentration. Conjugate acids of described oxyanions and halogens, for example hydrochloric acid, nitric acid and sulfuric acid, and others of the like are commercially available for purchase in a various selection of solvents from suppliers such as Lab Alley, Sigma- Aldrich, and Grainger. Coatings deposited from additive-enhanced precursor solutions can incorporate the conjugate acids.

[0066] Organotin precursor solutions enhanced with ligand leaving promoting additives can be deposited to form enhanced organotin coatings comprising incorporated additive species which can be the additive, a derivative of the additive, a fragment of the additive, or a combination thereof. As described in some embodiments, some additive compositions can undergo deprotonation and outgassing of volatile products of the additive. Accordingly, in some embodiments an additive Q+nAn’ is provided in the organotin solution and the corresponding organotin coating can comprise the additive, a derivative of the additive, a fragment of the additive, or a combination thereof. In some embodiments, the enhanced organotin coating comprises the anion A11-, whether or not the cation remains in the coating. The enhanced organotin coatings generally comprise a tin oxo-hydroxo network having radiation sensitive organyl ligands bound to the tin via Sn-C bonds and incorporated additive. The incorporated additive species can be coordinated to tin atoms within the oxo-hydroxo network, uncoordinated, or present in a combination of coordinated and uncoordinated forms. In some embodiments, the enhanced organotin coating can comprise the additive or additive anion at a molar ratio from about 0.001 to about 0.5 relative to tin, and from about 0.01 to about 0.25 relative to tin in other embodiments. A person of ordinary skill in the art will realize that additional molar ratios within the explicit ranges stated above are contemplated and within the scope of the present disclosure.Attorney Docket No. 5063.67W001 The enhanced coatings can generally be represented by the formula RSnO3 / 2-x / 2(OH)x: Q+nAn", wherein 0 < x <3, wherein R is an alkyl, aryl, alkenyl, or cycloalkyl group with 1 to 31 carbon atoms wherein one or more carbon atoms are optionally substituted with heteroatoms and Q+nAn" is integrated into the oxo-hydroxo network with potential ligand bonding to tin and possible degassing of volatile byproducts of the additive. In some embodiments the organotin coating comprises a blend of two different organyl ligands R and R’ , where R’ is an alkyl, aryl, alkenyl, or cycloalkyl group with 1 to 31 carbon atoms wherein one or more carbon atoms are optionally substituted with heteroatoms and different from R. For the blended coating, the organotin moiety RSn in the above formula can be replaced by the formula (R1a,R2b)Sn, wherein in (R^R2!,), R1is present at a mole fraction a and R2is present at a mole fraction b wherein a+b=l and wherein each of a and b is greater than about 0.05 (5 mol%). In some embodiments, the blended coating can further comprise additional organyl ligands, and the organotin moiety can be represented by the formula (RaR’b- • -Ryn)Sn where each organyl ligand (R, R’, •••, Ry) is represented by a mole fraction a, b, •••, n, which collectively sum to 1 and wherein each mole fraction is greater than about 0.05 (5 mol %).

[0067] It can be desirable for the organyl ligand leaving promoting additive to be soluble in the organic solvent comprising an organotin precursor solution. Suitable ligand leaving promoting additives are generally soluble in the organic solvent or solvent mixture comprising an organotin precursor solution. This can generally allow for the more uniform distribution of organyl ligand leaving promoting additives within deposited coatings formed therefrom. Solid precipitates within organotin precursor solutions are generally undesirable and can negatively impact the lithographic process for multiple reasons including but not limited to poor repeatability, clogging of process lines, and increased defectivity. Furthermore, it can be desirable for the organyl ligand leaving promoting additives to form stable organotin precursor solutions wherein solid precipitates are not observed after the precursor solution has been allowed to rest for a specific amount of time. Organyl ligand leaving promoting additives that exhibit observable precipitates when added to otherwise stable organotin precursor solutions can be less desirable, as solid precipitates within the organotin precursor solution are generally undesirable. However, organyl ligand leaving promoting additives that generate observable precipitates in one organotin precursor solution composition can be useful for other organotin precursor solution compositions. In some embodiments, the additive-enhanced organotin precursor solutions can be stable and free of observable precipitates from about 1 day to aboutAttorney Docket No. 5063.67W001 4 months, while in other embodiments the additive-enhanced organotin precursor solution is free of observable precipitates from about 3 days to about 2 months, and the additive-enhanced organotin precursor solution is free of observable precipitates from about 7 days to about 1 month. Applicant has synthesized stable additive-enhanced organotin precursor solutions, as exemplified herein.

[0068] In some embodiments, the oxidizing nature of the ligand leaving promoting additives can reduce the storage stability of additive-enhanced precursor solutions. An additive codeposition approach can be employed for nonvolatile additives to obtain the beneficial effect of the additive in the coating while mitigating degradation of the precursor solution during storage or handling. In an additive co-deposition approach, an organotin precursor solution and a separate solution comprising an additive composition are dispensed simultaneously during the spin-coating process. In some embodiments, the additive solution and the organotin precursor solution are maintained in separate containments prior to dispensing (i.e. reservoirs, bottles, tanks or the like) and combined only shortly before dispensing. The combining of the two fluids can be performed within a dispensing nozzle before exiting the nozzle or can be dispensed separately but concurrently such that mixing occurs during dispensing and / or during the spin coating. Suitable solvents for the additive solution can generally be the same solvents used for photoresist precursor solutions described herein. Suitable methods and apparatuses for liquid co-deposition of semiconductor materials are described in published U.S. Patent Application No. 20100209852 to Yeh, et al. entitled “Track nozzle system for semiconductor fabrication”, which is hereby incorporated by reference.

[0069] Organyl ligand leaving promoting additives can be present in additive-enhanced organotin precursor solutions at varying concentrations. While not wanting to be limited by theory it is believed that the concentration of ligand leaving promoting additives can correlate to the degree of enhanced organotin photoresist properties over significant ranges, such that a higher concentration of additive can produce, for example, larger dose reductions or greater increases in contrast. Ligand leaving promoting additives need not be present in high concentrations to produce substantial enhancements in patterning performance and relatively low concentrations of ligand leaving promoting additives can produce substantial dose reductions and chemical contrast improvements. Generally, the concentration of the additive in the additive enhanced organotin precursor solution can be measured as a ratio relative to the molar concentration of tin atoms. In some embodiments, the additives are present at a molarAttorney Docket No. 5063.67W001 ratio from about 0.001 to about 2 relative to tin, while in other embodiments the additives are present at a molar ratio of 0.01 to about 1.25, at a molar ratio of about 0.05 to about 1 relative to tin, or present at a molar ratio of 0.1 to 0.5 relative to tin. The additive concentration can be purposely selected to produce a radiation patternable coating with properties that have been enhanced to a desired degree to balance appropriate design considerations. A person of ordinary skill in the art will recognize that additional ranges of additive relative concentrations within the explicit ranges above are contemplated and are within the present disclosure.

[0070] In some embodiments, the organotin composition comprises a mixture of organotin compounds having different hydrocarbyl R groups with the same and / or different L groups bound accordingly. In some embodiments, the organotin photoresist composition has R ligands comprising a blend of a linear alkyl ligand and a non-linear alkyl ligand or an alternative second organyl ligand. In some embodiments, a blend of a linear alkyl ligand and a second organyl ligand comprises 1) a ligand with a branched alkyl group or a cyclo-alkyl group, 2) an unsaturated group, such as a dialkylene group, or 3) an aryl group. In additional embodiments, the organo tin composition can comprise organotin species having three or more than three distinct organyl ligands, such as those just described. In some embodiments, the organotin composition is a mixture of distinct organotin compounds having methyl ligands and tert-butyl ligands, respectively. In some embodiments, the precursor compositions comprise a blend of organotin compounds having the same and / or different L groups.

[0071] In some embodiments, the organotin composition comprises distinct organotin compounds with L ligands comprising a dialkylamide, an alkylsilylamide, an alkyloxide, an alkylacetylide, or a combination thereof. In other embodiments, the organotin composition comprises distinct organotin compounds with L ligands comprising methoxide, ethoxide, propoxide, iso-propoxide, butoxide, iso-butoxide, tert-butoxide, tert-amyloxide, pentoxide, iso-pentoxide, dimethyl amide, diethyl amide, diiso-propyl amide, trimethylsilyl amide, other isomers thereof, or combinations thereof. In embodiments wherein a blend of different organotin compounds, whether different with respect to organyl ligand R, hydrolysable ligand L or both, are used, any one of the distinct organotin compounds can comprise from about 1 mol. % to about 99 mol. % of the total organotin moles in some embodiments, from about 5 mol. % to about 95 mol. % of the total organotin moles in other embodiments, from about 10 mol. % to about 90 mol. % of the total organotin moles in other embodiments, and from about 15 mol. % to about 85 mol. % of the total organotin moles in further embodiments. In someAttorney Docket No. 5063.67W001 embodiments, blends can comprise 50 mol% of a first organotin compound and 50 mol% of a second organotin compound. In the Examples below, organotin precursor solutions comprising a mixture of two distinct organotin tri-tert-amyl alkoxide compounds are demonstrated. As is conventional in this art, the hydrocarbyl group can be referred to as an alkyl group even though the group can have unsaturated bonds, aryl groups, heteroatoms, and so forth. A person of ordinary skill in the art will recognize that additional ranges within the explicit ranges of organotin compound ratios above are contemplated and are within the present disclosure.

[0072] At an appropriate point in the preparation of the desired organotin precursor, the precursor and organyl ligand leaving promoting additive can be combined in an appropriate solvent to prepare a precursor solution, such as an organic solvent, e.g., alcohols, aromatic and aliphatic hydrocarbons, esters or combinations thereof. As noted above, in some embodiments, the organotin precursor compositions and the organyl ligand leaving promoting additive can be separately delivered. In particular, suitable solvents for the solutions include, for example, aromatic compounds (e.g., xylenes, toluene), ethers (anisole, tetrahydrofuran, propylene glycol methyl ether), esters (propylene glycol monomethyl ether acetate, ethyl acetate, ethyl lactate), alcohols (e.g., 4-methyl-2-pentanol, 1-pentanol, 1-butanol, methanol, isopropyl alcohol, 1-propanol), ketones (e.g., methyl ethyl ketone), mixtures thereof, and the like. In general, organic solvent selection can be influenced by solubility parameters, volatility, flammability, toxicity, viscosity and potential chemical interactions with other processing materials, such as the additives. The organotin precursor(s) can also generally be dissolved in mixtures of solvents to prepare precursor solutions. Some solvent mixtures useful for forming organotin photoresist solutions have been described in published U.S. Patent Application 2023 / 0143592 to Jiang et al., entitled “Stability-Enhanced Organotin Photoresist Compositions”, incorporated herein by reference. It can be desirable for the organotin precursor(s) to be dissolved in a solvent mixture comprising a primary alcohol. In some embodiments, the solvent can comprise a primary alcohol, such as methanol, ethanol, 1-propanol, 1-butanol, 1-pentanol, 1-hexanol, and the like. In some embodiments, the solvent can comprise a mixture of two alcohols. In other embodiments the solvent can comprise a mixture of an alcohol and an ester.

[0073] An additive-enhanced organotin photoresist solutions generally comprise one or more organotin precursor compositions, a ligand leaving promoting additive, and an organic solvent. The concentration of resist precursor composition can be conveniently specified based on tin atom molar concentration. In general, the resist precursor solution generally comprises fromAttorney Docket No. 5063.67W001 about 0.0025 M to about 1 M tin atoms, in some embodiments from about 0.004 M to about 0.9 M, in further embodiments from about 0.005 M to about 0.75 M, in some embodiments from about 0.01 M to about 1 M, and in additional embodiments from about 0.01 M to about 0.5 M tin atoms. If an additive solution is separately applied or blended at the time of dispensing, these same ranges of tin concentrations are suitable for the organotin precursor solution initially without the ligand leaving promoting additive. Other Sn concentrations not directly disclosed but within the above ranges are contemplated are within the scope of the present disclosure. A person of ordinary skill in the art will recognize that additional ranges of additive amounts in organotin photoresist precursor solutions within the explicit ranges above are contemplated and are within the present disclosure.

[0074] As described herein, water can react with the organotin species to form hydrolysis / condensation products. Organotin photoresist solutions comprising different amounts of water can result in different degrees of hydrolysis / condensation occurring and thus different distributions of hydrolysis / condensation products within the different solutions which may impact resist performance. Therefore, to improve batch to batch reproducibility of organotin photoresist precursor solutions it is desirable to controllably target specific concentrations of water formulated into the photoresist precursor solutions. Desirable amounts of water can generally be expressed as either absolute concentrations, such as parts-per-million (ppm) by weight or molarity, or the desirable amounts of water can be expressed as molar ratios with respect to the Sn concentration. In some embodiments, the additive-enhanced organotin photoresist precursor solutions can comprise a selected concentration of water from about 200 ppm to about 10,000 ppm water, from about 250 ppm to about 8,000 ppm in further embodiments, from about 275 ppm to about 5,000 ppm in other embodiments, and from about 300 ppm to about 2,000 ppm in further embodiments. In some embodiments, the additive-enhanced organotin photoresist solutions can comprise a selected molar ratio of water to Sn from about 0.1 to about 20, from about 0.2 to about 15 in some embodiments, and from about 0.25 to about 10. A person of ordinary skill in the art will recognize that additional ranges of water in organotin photoresist precursor solutions within the explicit ranges above are contemplated and are within the present disclosure.

[0075] In some embodiments, the additive enhanced organotin precursor solutions can further comprise a radical scavenging additive. The addition of a radical scavenging compound can reduce undesirable effects of radical contaminants which can increase wafer to waferAttorney Docket No. 5063.67W001 consistency amidst changes to the processing environment. To decrease deleterious effects from radicals, further additives can be included in the precursor solutions to scavenge radicals. Such additives have been shown to be beneficial, as described in the ‘662 application. A suitable concentration of radical scavenger can depend significantly on the agent used, but generally the concentration of radical scavenger in the precursor solution can be from about 0.000025M to about 0.4M. A person of ordinary skill in the art will realize that any subrange or intermediate value within the explicit concentration ranges above is contemplated and within the scope of the present disclosure.

[0076] Radical scavenger compounds can include, for example, H-donor radical scavengers, such as phenolic compounds and hindered amines. The phenolic compounds can be characterized by the presence of a substituted aromatic ring which can improve their ability to form relatively stable radicals after hydrogen atom transfer. In some embodiments, the H-donor radical scavenger is a hindered phenol compound having an aromatic ring substituted with an electron-donating group. In some embodiments, the H-donor radical scavenger is butylated hydroxytoluene (BHT) or butylated hydroxyanisole (BHA), and more general embodiments are described in the '662 application. In some embodiments, the H-donor radical scavenger is an aromatic diol. In some embodiments, the H-donor radical scavenger is an alkoxyphenol, hindered aromatic amine, or derivative thereof. In some embodiments, the radical scavenging additive is a hindered amine compound. The hindered amine compound can react with oxygen or reactive oxygen species to form a stable and sterically hindered aminoxyl (-NO-) radical which can preferentially react with other radical species instead of the non-radical components of the photoresist. In some embodiments, the radical scavenger additive is TEMPO ((2, 2,6,6-tetramethylpiperidin-l-yl)oxyl) or TEMPOL ((4- Hydroxy-2, 2,6, 6-Tetramethylpiperidin- 1-yl)oxyl). In some embodiments, the radical scavenger additive is 2 -phenyl -4 ,4,5 ,5-tetramethylimidazoline-l-oxyl 3 -oxide (PTIO).

[0077] The additive-enhanced organotin photoresist precursor solutions can be used to form radiation-patternable additive-enhanced organotin oxide hydroxide materials, and such coatings can be formed using any suitable method known in the art. Spin coating can be particularly desirable for forming coatings using the additive-enhanced organotin photoresist compositions. In a typical spin coating process, a volume of a photoresist solution is introduced onto the surface of a substrate, and the substrate is rotated at high speeds to drive rapid evaporation and hydrolysis processes to enable the formation of a radiation patternable coating.Attorney Docket No. 5063.67W001 In some embodiments, the substrate can be spun at rates (i.e., spin speeds) from about 500 rpm to about 10,000 rpm, in further embodiments from about 1000 rpm to about 7500 rpm, and in additional embodiments from about 2000 rpm to about 6000 rpm. The spin speed can be adjusted to obtain a desired coating thickness. The spin coating can be performed from about 5 seconds to about 5 minutes and in further embodiments from about 15 seconds to about 2 minutes. An initial low speed spin, e.g., at 50 rpm to 250 rpm, can be used to perform an initial bulk spreading of the composition across the substrate. A back side rinse, edge bead removal step, or the like can be performed with water or other suitable solvent to remove any edge bead. A person or ordinary skill in the art will recognize that additional ranges of spin coating parameters within the explicit ranges above are contemplated and are within the present disclosure.

[0078] A substrate generally presents a surface onto which the coating material can be deposited, and the substrate may comprise a plurality of layers in which the surface relates to an upper most layer. The substrate surface can be treated to prepare the surface for adhesion of the coating material. Prior to preparation of the surface, the surface can be cleaned and / or smoothed as appropriate. Suitable substrate surfaces can comprise any reasonable material. For semiconductor applications, a suitable substrate generally comprises a semiconductor wafer. Some substrates of interest include, for example, silicon wafers, silica substrates, other inorganic materials, polymer substrates, such as organic polymers, composites thereof and combinations thereof and / or in layers of the substrate. In some embodiments, the substrate can comprise apatterned structure such as described by Stowers et al. in U.S. Patent No. 10,649,328, entitled “Pre-Patterned Lithography Templates, Process Based on Radiation Patterning Using The Templates And Processes To Form The Templates”, incorporated herein by reference.

[0079] The thickness of the coating generally can be a function of the precursor solution concentration, viscosity, and the spin speed for spin coating. For other coating processes, the thickness can generally also be adjusted through the selection of the coating parameters. In some embodiments, it can be desirable to use a thin coating to facilitate formation of small and highly resolved features in the subsequent patterning process. For example, the coating materials after drying can have an average thickness of no more than about 250 nanometers (nm), in additional embodiments from about 1 nm to about 50 nm, in other embodiments from about 2 nm to about 40 nm and in further embodiments from about 3 nm to about 25 nm. A person of ordinary skill in the art will recognize that additional ranges of thicknesses within theAttorney Docket No. 5063.67W001 explicit ranges above are contemplated and are within the present disclosure. The thickness can be evaluated using non-contact methods, such as x-ray reflectivity and / or ellipsometry, based on the optical properties of the film. In general, the coatings are relatively uniform to facilitate processing. In some embodiments, such as high uniformity coatings on reasonably sized substrates, the evaluation of coating uniformity or flatness may be evaluated with, for example, a 1 -centimeter edge exclusion, i.e., the coating uniformity is not evaluated for portions of the coating within 1 centimeter of the edge, although other suitable edge exclusions can be selected.

[0080] While heating may not be needed for successful application of the deposition process, it can be desirable to heat the coated substrate to densify the coating material, to remove solvent, to speed the processing, to increase the reproducibility of the process, and / or to facilitate vaporization of the hydrolysis by-products, such as alcohols and / or amines. Selection of the post application bake conditions can be influenced by the desire to remove, partially remove, or not significantly remove an additive, such as the ligand leaving promoting additive or a radical scavenger additive, which in turn can depend on the properties of the additive. In embodiments in which heating of the coated substrate is performed prior to irradiation, the coated substrate can be heated to temperatures from about 45 °C to about 250 °C, and in further embodiments from about 55 °C to about 225 °C. The heating can generally be performed for at least about 0.1 minute, in further embodiments for about 0.5 minutes to about 30 minutes, and in additional embodiments from about 0.75 minutes to about 10 minutes. Heating can be performed over facility ambient atmosphere, an inert atmosphere, such as nitrogen, argon or another substantially inert gas, a reactive atmosphere, such as with enhanced carbon dioxide, and at facility pressure or a reduced pressure. Post coating, pre-irradiation processing can further comprise rest periods, which can divide distinct heating steps. A person of ordinary skill in the art will recognize that additional ranges of heating temperatures and times within the explicit ranges above are contemplated and are within the present disclosure.

[0081] Generally, photoresist coatings can be patterned using radiation. Suitable radiation sources include extreme ultraviolet (EUV), ultraviolet (UV), or electron beam (EB) radiation. For fabrication of semiconductor devices, EUV radiation can be desirable due to its higher resolution compared to UV radiation, and its higher throughput compared to electron beam (EB)-based processing. Radiation can generally be directed to the substrate material through a mask or a radiation beam can be controllably scanned across the substrate to form a latentAttorney Docket No. 5063.67W001 image within the resist coating. For EUV "masking", the patterns are generally formed using mirrors to reflect and direct light from a plasma source.

[0082] The amount of electromagnetic radiation can be characterized by a fluence or dose which is obtained by the integrated radiative flux over the exposure time. For embodiments in which EUV radiation is used, suitable radiation doses can be from about 1 mJ / cm2to about 150 mJ / cm2, in further embodiments from about 2 mJ / cm2to about 100 mJ / cm2and in further embodiments from about 3 mJ / cm2to about 50 mJ / cm2. A person of ordinary skill in the art will recognize that additional ranges of radiation doses within the explicit ranges above are contemplated and are within the present disclosure.

[0083] Following exposure to radiation and the formation of a latent image, a subsequent postexposure bake (PEB) is typically performed. In some embodiments, the PEB can be performed at temperatures from about 45 °C to about 250 °C, in additional embodiments from about 50 °C to about 190 °C and in further embodiments from about 90 °C to about 185 °C. The post exposure heating can generally be performed for at least about 0.1 minute, in further embodiments from about 0.5 minutes to about 30 minutes and in additional embodiments from about 0.75 minutes to about 10 minutes. A PEB step can be performed in air, inert gas or a specific gas environment, such as enriched on O2, CO2 and / or other oxygen-containing species, and / or in low humidity atmospheres, and similarly, the pressure during post irradiation process steps can be set to low pressures, to ambient pressure, to higher than ambient pressures or various combinations thereof. Also, the processing between irradiation and development can also include rest steps and / or multiple PEB steps, each of which can be performed similarly under selected atmospheres. See U.S. Patent No. 11,947,262 to Telecky et al., entitled "Process Environment for Inorganic Resist Patterning," incorporated herein by reference. A person of ordinary skill in the art will recognize that additional ranges of PEB temperatures and times within the explicit ranges above are contemplated and are within the present disclosure.

[0084] Following performing a PEB, development of the image involves the contact of the patterned coating material including the latent image to a developer composition to remove either the un-irradiated coating material to form the negative image or the irradiated coating to form the positive image. Irradiated regions of organotin oxide hydroxide coatings are generally hydrophilic and are thus soluble in aqueous bases and insoluble in organic solvents; conversely, non-irradiated regions are generally hydrophobic and are thus soluble in organic solvents andAttorney Docket No. 5063.67W001 insoluble in aqueous bases. For negative tone imaging, the developer can be an organic solvent, such as the solvents used to form the precursor solutions.

[0085] For positive tone imaging, suitable developers can generally be aqueous bases. To reduce contamination from the developer, it can be desirable to use a developer that does not have metal atoms. Thus, quaternary ammonium hydroxide compositions, such as tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide or combinations thereof, are desirable positive tone developers. In general, the quaternary ammonium hydroxides of particular interest can be represented with the formula R4NOH, where R = a methyl group, an ethyl group, a propyl group, a butyl group, or combinations thereof. The coating materials described herein generally can be developed with the same developer commonly used presently for polymer resists, specifically tetramethyl ammonium hydroxide (TMAH). Commercial TMAH is available at 2.38 weight percent. Furthermore, mixed quaternary tetra alkyl ammonium hydroxides can be used. In some embodiments, the developer can comprise from about 0.5 to about 30 weight percent tetra alkyl ammonium hydroxides, in further embodiments from about 1 to about 25 weight percent tetra alkyl ammonium hydroxides and in other embodiments from about 1.25 to about 20 weight percent tetraalkylammonium hydroxides. A person of ordinary skill in the art will recognize that additional ranges of developer concentrations within the explicit ranges above are contemplated and are within the present disclosure.

[0086] For the negative tone imaging, the developer can be an organic solvent, such as the solvents used to form the precursor solutions. In general, developer selection can be influenced by solubility parameters with respect to the coating material, both irradiated and non-irradiated, as well as developer volatility, flammability, toxicity, viscosity, and potential chemical interactions with other process material. In particular, suitable developers include, for example, aromatic compounds (e.g., benzene, xylenes, toluene), esters (e.g., propylene glycol monomethyl ester acetate (PGMEA), ethyl acetate, ethyl lactate, n-butyl acetate, butyrolactone), alcohols (e.g., 4-methyl-2-pentanol, 1-butanol, isopropanol, 1-propanol, methanol), ketones (e.g., methyl ethyl ketone, acetone, cyclohexanone, 2-heptanone, 2-octanone), ethers (e.g., tetrahydrofuran, dioxane, anisole) and the like. Improved developer compositions have been described in U.S. Patent No. 12,416,861 to Jiang et al., entitled “Organometallic Photoresist Developer Compositions and Processing Methods,” incorporated herein by reference. Improved developer solutions generally comprise a reference organicAttorney Docket No. 5063.67W001 solvent composition and an additive composition having a higher polarity and / or hydrogenbonding character than the reference solvent composition. In one example, an improved developer composition can comprise PGMEA and acetic acid. The development can be performed for about 5 seconds to about 30 minutes, in further embodiments from about 8 seconds to about 15 minutes and in addition embodiments from about 10 seconds to about 10 minutes. A person of ordinary skill in the art will recognize that additional ranges within the explicit ranges above are contemplated and are within the present disclosure.

[0087] For negative tone development, developer selection can be effectively influenced by solubility parameters with respect to the coating material, both irradiated and non-irradiated, as well as developer volatility, flammability, toxicity, viscosity, and potential chemical interactions with other process material. In particular, developers can have differing amounts of more polar or less polar components, which can be specified more specifically with solubility parameters. In some embodiments, the solvent blend can comprise at least two solvents with at least 55 volume % of one or more solvents each independently having a sum of Hansen solubility parameter 5H + 5P of no more than about 16 (J / cm3)1 / 2, and with from about 0.25 volume % to about 45 volume% of one or more solvents each independently having a sum of Hansen solubility parameter 5H + 5P of at least about 16 (J / cm3)1 / 2. A double bakedouble develop processing can be performed in which the second development can involve a developed for a negative tone pattern comprising all or a larger percentage of a solvent having a sum of Hansen solubility parameter 5H + 5P of at least about 16 (J / cm3)1 / 2, or a positive tone developer can be used in the second step of a negative tone patterning process.

[0088] It has also been discovered that solventless development, also referred to as dry development, can be employed with organotin materials for negative tone patterning wherein selective removal of the non-irradiated regions of the photoresist is achieved by exposing the material to an appropriate plasma or appropriate flowing gas. Dry development of organotin resists has been described in PCT Publication No. 2020 / 132281A1 by Volosskiy et al., entitled "Dry Development of Resists", in published U.S. Patent Application No. 2023 / 0100995 to Cardineau et al., entitled “High Resolution Latent Image Processing and Thermal Development”, and in published U.S. Patent Application No.

[0089] 2023 / 0408916 to de Schepper et al. entitled "Gas-Based Development of Organometallic Resist in an Oxidizing Halogen-Donating Environment," all three of which are incorporated herein by reference. In such dry development processes, development can be achieved by exposing theAttorney Docket No. 5063.67W001 irradiated substrate to a plasma or a thermal process while flowing a gas comprising a small molecule reactant (reactive gas) that facilitates removal of non-irradiated regions. In some embodiments, the developer can be HBr or HBr plasma. In other embodiments, the reactive developer gas can be a compound QxZyor where Q is B, Al, Si, C, S, or SO with x >0 and Z is Cl, H, Br, or F with y>0. In further embodiments, the reactive developer gas can be an amine, a silyl halide, an alcohol, an amide, a sulfonic acid, a carboxylic acid, a thiol, tin halide, germanium halide, and mixtures thereof. The reactive gas species can be introduced in a gaseous form or activated into a plasma state to enhance reactivity. Following development, a rinse step can be conducted using water, a positive tone developer solution or the like, if desired to further remove undesired residual material from the pattern, and such methods have been described in U.S. Patent 11,480,874 to Kocsis et al., entitled "Patterned Organometallic Photoresists and Methods of Patterning," incorporated herein by reference.

[0090] Solventless development can be performed at various process conditions and the process conditions can be selected to achieve the desired development for certain developer species and organometallic coatings. The temperature of the developer gas or etch chamber can influence the efficacy of the solventless development, as can the duration of the development, and the pressure of the etch chamber during development. In some embodiments, the solventless development can be performed at a temperature from about 10 °C to about 100 °C, from about 20 °C to about 80 °C, or from about 30 °C to about 60 °C. In other embodiments, the solventless development can be performed at a temperature from about 100 °C to about 250 °C, from about 120 °C to about 230 °C, or from about 150 °C to about 200 °C. In some embodiments, the solventless development process can be performed for about 10 seconds, about 20 seconds, or about 40 seconds, each about ±5 seconds. In other embodiments, the solventless development process can be performed for more than about 3 seconds and less than about 5 minutes, from about 10 seconds to about 2 minutes in further embodiments, and from about 20 seconds to about 60 seconds in yet further embodiments. In some embodiments, the solventless development process can be performed at reduced pressures in other embodiments the solventless development process can be performed at near atmospheric pressures, and in other embodiments the solvent development process can be performed at higher than atmospheric pressures. In other embodiments pressure can be from about 0.1 mTorr(mT) to about 800 mT, in other embodiments the pressure can be from about 1 mT to about 500 mT, and from about lOmTto about 300 mT in further embodiments. In embodiments whereinAttorney Docket No. 5063.67W001 the solventless development process is conducted at pressures near or above atmospheric pressure, the solventless development process can be performed at pressures from about 100 Torr to about 1000 Torr, from about 100 Torr to about 800 Torr in further embodiments, and from about 200 Torr to about 800 Torr in other embodiments. In some embodiments, the solventless development can be performed at the ambient pressure of the fabrication facility. A person of ordinary skill in the art will realize that additional values of temperatures, durations, and pressures within the explicitly recited ranges above are contemplated and part of the present disclosure.

[0091] After completion of the development step and any optional rinses, the patterned wafers can be treated to further condense the patterned material and to further dehydrate, densify, or remove residual developer from the material. The treatment can involve heat, exposure to a suitable plasma, and / or exposure to radiation. A heat treatment can be particularly desirable for embodiments in which the oxide coating material is incorporated into the ultimate device, although it may be desirable to perform the heat treatment for some embodiments in which the coating material is used as a resist and ultimately removed if the stabilization of the coating material is desirable to facilitate further patterning. In particular, the baking of the patterned coating material can be performed under conditions in which the patterned coating material exhibits desired levels of etch selectivity. In some embodiments, the patterned coating material can be heated to a temperature from about 100° C. to about 600° C., in further embodiments from about 175° C. to about 500° C. and in additional embodiments from about 200° C. to about 400° C. The heating can be performed for at least about 1 minute, in other embodiments for about 2 minutes to about 1 hour, in further embodiments from about 2.5 minutes to about 25 minutes. The heating may be performed in air, vacuum, or an inert gas ambient, such as Ar or N2. A person of ordinary skill in the art will recognize that additional ranges of temperatures and time for the heat treatment within the explicit ranges above are contemplated and are within the present disclosure. Likewise, nonthermal treatments, including blanket UV exposure, or exposure to an oxidizing plasma such as O2 may also be employed for similar purposes.

[0092] EXAMPLES

[0093] Example 1: Formulation and spin coating deposition of stable ligand leaving promoting additive-enhanced organotin precursor solutions.Attorney Docket No. 5063.67W001 In this example, organotin photoresist solutions comprising ligand leaving promoting additives are formulated and coatings deposited therefrom are identified to have desirable characteristics.

[0094] Formulation of Additive Enhanced Organotin Precursor Solutions:

[0095] A bulk organotin precursor solution was prepared by dissolving an appropriate amount of isopropyl tin tris(sec-butoxide) in a solution comprising 62% 1 -pentanol by weight and 38% 1-propanol by weight such that the final solution had a Sn concentration of 0.07 M. Prior to formulation, the solvent was adjusted to comprise water at a concentration of 300 ppm by weight. The bulk solution was divided into smaller aliquots, one of which was reserved as a comparative non-additive enhanced solution (PRX). To the other aliquots, selected ligand leaving promoting additives were dissolved at varying concentrations to form 8 additive-enhanced precursor solutions. The compounds used to synthesize the solutions are shown in Table 1 and the formulation details for each precursor solution is presented in Table 2.

[0096]

[0097] Attorney Docket No. 5063.67W001

[0098] H3C Tetramethyl ammonium \ / CH3A Additive H3c- Nf chloride

[0099] CH3C!

[0100] B Additive Ortho Periodic Acid

[0101] CH2CH3

[0102] C Additive Triethyl ammonium nitrate H ~N~CH2CH3NO3~

[0103] CH2CH3

[0104] CH3

[0105] D Additive Choline chloride HQ ^-^N”CH3

[0106] CH3

[0107]

[0108] TABLE 2:

[0109] Organotin Additive: Sn Precursor Sn Water

[0110] Solvent Composition (Molar Solution Concentration Concentration

[0111] (mol %) Ratio) PRX S-l P-1 (100%) 0.07 M 300 ppm ** PRX-A1 S-l P-1 (100%) 0.07 M 300 ppm A (0.1) PRX-A2 S-l P-1 (100%) 0.07 M 300 ppm A (0.5) PRX-B1 S-l P-1 (100%) 0.07 M 300 ppm B (0.1) PRX-B2 S-l P-1 (100%) 0.07 M 300 ppm B (0.5) PRX-C1 S-l P-1 (100%) 0.07 M 300 ppm C (0.1) PRX-C2 S-l P-1 (100%) 0.07 M 300 ppm C (0.5) PRX-D1 S-l P-1 (100%) 0.07 M 300 ppm D (0.05) PRX-D2 S-l P-1 (100%) 0.07 M 300 ppm D (0.7)

[0112]

[0113] The organotin precursor solutions were then deposited on 300 mm Si wafers with a spin-on-glass underlayer via spin coating to form coated wafers. The wafers were then exposed to a 60 second, 100 °C post application bake (PAB). The thickness of the coatings was measured using ellipsometry and presented in Table 3. An analysis was performed to determine the contact angle between the organotin coating and a water droplet. Measured contact anglesAttorney Docket No. 5063.67W001 for each sample are presented in Table 3. The data suggests that additive-enhanced precursor solutions can be successfully deposited to form organotin films with desirable properties for patterning. Notably, that addition of additives decreased the contact angle for all samples in comparison to the comparative non-additive enhanced sample PRX, indicating that additive-enhanced films have an increased hydrophilicity. The decrease in contact angle varied for each sample from about 0.7 degrees to about 66.8 degrees, indicating that the magnitude of contact angle decrease can vary with the identity and concentration of the ligand leaving promoting additive. Triethylammonium nitrate, ortho periodic acid, and choline chloride enhanced samples exhibited a correlation between additive concentration and contact angle decrease, such that high additive concentrations increased the magnitude of the contact angle decrease. The increase in hydrophilicity may improve the wettability and surface interaction with a developer solvent and lead to better cross wafer uniformity during the development process, in particular during positive tone development with aqueous base solutions.

[0114] TABLE 3:

[0115] Sample Film Thickness (nm) Contact Angle (°) Stability Duration PRX 26.08 + 0.11 78.3 + 0.3 4 months + PRX-A1 24.53 + 0.05 72.4 + 0.9 4 months + PRX-A2 28.72 + 0.17 72.4 + 0.04 4 months + PRX-B1 27.39 + 0.03 77.6 + 0.6 7 days

[0116] PRX-B2 36.47 + 0.03 73.2 + 0.25 daYs

[0117] PRX-C1 23.34 + 0.03 75.5 + 0.6 4 months + PRX-C2 28.04 + 0.14 33.3 + 1.1 4 months + PRX-D1 26.35 + 0.08 22.6 + 1.34months + PRX-D2 29.83 + 0.13 21.9 + 0.6 4 months +

[0118]

[0119] All of the additive enhanced precursor solutions were observed to be shelf stable for at least 4 months, with the exception of solutions PRX-B1 and PRX-B2 enhanced with periodic acid which precipitated within a week from formulation. These results indicate that many of the ligand leaving promoting additives can improve coating contact angle without sacrificing the shelflife of the precursor solutions.Attorney Docket No. 5063.67W001 Example 2: EUV Patterning of ligand leaving promoting additive enhanced organotin films.

[0120] In this example, ligand leaving promoting additives are added to organotin precursor solutions, and coatings deposited therefrom are patterned with EUV radiation and dry development techniques.

[0121] In an inert environment, a bulk solution of organotin photoresist precursor was prepared by combining an organotin composition comprising 60% isopropyl tin tris(sec-butoxide) by mole and 40% tert-butyl tin tris(3-pentoxide) by mole with a solvent mixture comprising 62% 1-pentanol by weight and 38% 1-propanol by weight to form a solution having an Sn concentration of 0.065 M. Prior to formulation the solvent was adjusted to comprise water at a concentration of 300 parts per million (ppm) by weight. The solution was then divided into aliquots, one of which was reserved as comparative sample PRY, and to the remainder a ligand leaving promoting additives were added at a molar ratio of 0.05 relative to Sn. The compounds used to formulate the precursor solutions are shown in Tables 1 and 4 and the formulation details for the precursor solutions are presented in Table 5.

[0122]

[0123] Attorney Docket No. 5063.67W001 CH

[0124] Tetramethyl ammonium3

[0125] Additive H3C-N-CH3 F fluoride CH3

[0126]

[0127] TABLE 5:

[0128] Precursor Solvent ^r"anot'nComposition Sn Water Additive Solution (mol %) Concentration Concentration ( Ratio :Sn) PRY S-l 0.065 M 300 ppm **

[0129] PRY-CI S-l P 0.065 M 300 ppm C (0.05)

[0130] PRY-E1 S-l p ? Sw ) 0.065 M 300 ppm E (0.05)

[0131] PRY-D1 S-l P ? SW ) 0.065 M 300 ppm D (0.05)

[0132] PRY-A1 S-l p ? 2nS 0.065 M 300 ppm A (0.05)

[0133] PRY-F1 S-l P ? SW ) 0.065 M 300 ppm Y (0.05)

[0134] PRY-G1 S-l P 15 ~ ? £ S 1 W / O)) 0.065 M 300 ppm G (0.05)

[0135]

[0136] Each of the prepared precursor solutions were used to independently coat 300mm diameter silicon wafers with a spin-on-glass underlayer via spin coating to form an about 30 nm thick coating, confirmed by ellipsometry. The coated wafers were subsequently subjected to a 60 second post-application bake (PAB) at a temperature of 130 °C. Then, line-space patterns having a target critical dimension (CD) of 14 nm on a 28 nm pitch (14p28) were produced on each coated wafer by exposing the coated wafers to 13.5 nm EUV radiation between about 0 mJ / cm2and about 100 mJ / cm2using an ASML NXE3400B exposure tool to form irradiated wafers having an array of patterns within fields, wherein each field corresponds to the mask pattern printed at a specified dose. As is customary in the art, this type of exposure is often referred to as a dose meander exposure. By exposing the same 14p28 pattern at different doses across each coated wafer, the dose required for printing the desired 14p28 for a given organotin composition (i.e. the dose-to-size for printing 14 nm lines on a 28 nm pitch) can beAttorney Docket No. 5063.67W001 determined through inspection of each field of the patterned, coated wafer after processing is complete. The irradiated wafers were then subjected to a 60 second post-exposure bake (PEB) at a temperature of either 200 °C, 210 °C, or 220 °C to form baked, irradiated wafers.

[0137] The baked, irradiated wafers were then developed using HBr plasma in a semiconductor etch tool in a negative tone development process to form developed wafers. The developed wafers were inspected using a Hitachi CS-SEM to determine the critical dimension of linespace pattern in each field of the developed wafer using metrology software. The dose-to-size corresponds to the exposure dose that produced a critical dimension nearest to the target critical dimension of 14 nm. The exposure dose and critical dimension for the line space patterns are presented in Table 6.

[0138] TABLE 6:

[0139] P nEeBo ' TT'emp P r>r..ecursor S Co 1lution Exp ,osTu / re D vose Critical ,

[0140] (mJ / cm ) Dimension (nm) PRY 64.25 14.00

[0141] 200 °C PRY-CI 49.25 13.88

[0142] PRY-E1 66.5 13.84

[0143] PRY 50.25 14.19

[0144] PRY-CI 13.75 14.10

[0145] PRY-D1 49.00 14.01

[0146] 210 °C PRY-A1 45.25 14.04

[0147] PRY-E1 34.75 13.92

[0148] PRY-F1 57.25 14.19

[0149] PRY-G1 51.25 14.06

[0150] PRY 36.75 14.00

[0151] 220 °C PRY-D1 30 13.87

[0152] PRY-A1 30 14.53

[0153] PRY-F1 34.5 13.83

[0154]

[0155] PRY-G1 30.75 14.24

[0156] Decreases in dose-to-size were observed at one or more PEB temperatures for each of the ligand leaving promoting additives tested. Generally, larger dose reductions were observed for higher PEB temperatures, suggesting that the ligand leaving promoting additives can influence the thermal stability of organyl ligands and sensitivity of the coating to provide sufficient contrast at lower exposure doses. Notably, the solution enhanced with tetramethyl ammonium chloride PRY-A1 produced dose reductions of 5.00 and 6.75 mJ / cm2at PEB temperatures of 210 °C and 220 °C, respectively, whereas the solution enhanced withAttorney Docket No. 5063.67W001 tetramethyl ammonium fluoride PRY-G1 increased the dose at a PEB temperature of 210 °C and produced a dose reduction of only 6 mJ / cm2at a PEB temperature of 220 °C. Since additives A and G are otherwise identical and the solutions comprised additive at the same concentration, this indicates that the addition of chloride is more effective for reducing the exposure dose than fluoride. The opposite effects of the chloride and fluoride based additives at a PEB temperature of 210 °C further indicates that chloride based additives can be employed to reduce the exposure dose for low temperature processing where fluoride would be less effective or even produce a dose increase in some cases.

[0157] The coating formed from tri ethylammonium nitrate enhanced solution PRY-CI exhibited a greater magnitude of dose reduction than an otherwise identical solution PRY- Al enhanced with tetraethylammonium nitrate at the same concentration. This suggests that trialkyl ammonium salts are more effective at producing dose reductions per mole of additive than tetra-alkyl ammonium salts, which correspondingly indicates that the cations can also influence the dose-to-size. Additionally, the nitrate containing additives samples PRY-CI and PRY- Al exhibited significantly large dose reductions in comparison to samples comprising halogen and hydroxide anions, suggesting that nitrate ions are particularly effective at producing dose reductions per mole of additive than F, Cl, and OH. The dose reductions resulting from the addition of choline chloride PRY-D1 increased more with PEB temperature than that of tetramethylammonium chloride PRY -Al, suggesting that the dose reduction effects realized from choline-based additives can have a greater thermal dependance than those realized by tetramethylammonium based additives. This example showed that the addition of ligand leaving promoting additives can generally reduce the dost-to-size for organometallic photoresist patterning at some PEB temperatures. The magnitude of the effect can vary with additive species, as can the thermal dependence of the effect.

[0158] Example 3: Deposition and patterning of coatings deposited from chloride enhanced precursor solutions.

[0159] In this example, the addition of ammonium chloride to organotin precursor solutions is determined to increase the radiation sensitivity of films having primary and tertiary organyl ligands and decrease the sensitivity of films having secondary organyl ligands.Attorney Docket No. 5063.67W001 Four samples of organotin precursor solutions were prepared by combining an organotin composition, an organic solvent blend, and optionally ammonium chloride (the structures of which are shown in Tables 1 (Pl), 4 (P2), and 7) according to specification in Table 8. The comparable precursor solutions PRZ and PRZ-H1 both comprised a blend of tertiary and primary organyl ligands except PRZ-H1 was enhanced with ammonium chloride. It is worth noting that while the exact compositions of samples PRZ and PRZ-H1 may differ aside from the additive based on their hydrolysable ligands, the patterning properties of organotin photoresists are known to be primarily influenced by the organyl ligand identity which is identical for the two samples (20% CHs / 80% tBu). The comparable precursor solutions PRQ and PRQ-H1 comprised secondary organyl ligands and were otherwise identical, except PRQ-H1 was enhanced with ammonium chloride additive at a molar ratio of 0.05 relative to Sn.

[0160]

[0161] Attorney Docket No. 5063.67W001

[0162] H Additive Ammonium Chloride

[0163]

[0164] TABLE 8:

[0165] Precursor Organotin Composition Sn Water Additive Solvent

[0166] Solution (mol %) Concentration Concentration (Ratio: Sn)

[0167] P-3 (20%)

[0168] PRZ S-2 0.050 M 300 ppm ** P-4 (80%)

[0169] P-3 (20%)

[0170] PRZ-H1 S-l 0.062 M 300 ppm H (0.05)

[0171] P-2 (80%)

[0172] PRQ S-l P-1 (100%) 0.062 M 300 ppm ** PRQ-H1 S-l P-1 (100%) 0.062 M 300 ppm H (0.05)

[0173]

[0174] The four samples were deposited onto 300 mm Si wafers with a spin-on-glass underlayer via spin coating to form coated wafers having coating thicknesses of 26 nm, as determined by ellipsometry. The wafers were then subjected to a 100 °C post application bake (PAB) for 60 seconds. Then, line-space patterns having a target critical dimension (CD) of 14 nm on a 28 nm pitch (14p28) were produced on each coated wafer by exposing the coated wafers to 13.5 nm EUV radiation between about 10 mJ / cm2and about 100 mJ / cm2using an ASML NXE3400B exposure tool to form irradiated wafers having an array of patterns within fields, wherein each field corresponds to the mask pattern printed at a specified dose. As is customary in the art, this type of exposure is often referred to as a dose meander exposure. By exposing the same 14p28 pattern at different doses across each coated wafer, the dose required for printing the desired 14p28 for a given organotin composition (i.e. the dose-to-size for printing 14 nm lines on a 28 nm pitch) can be determined through inspection of each field of the patterned, coated wafer after processing is complete. The irradiated wafers formed from samples PRZ and PRZ-H1 were subjected to post exposure bakes (PEB) for 60 seconds at either 140°C, 160°C, or 180°C. The irradiated wafers formed from samples PRQ and PRQ-H1 were subjected to PEBs for 60 seconds at either 180°C, 200°C, or 220°C. The PEB temperatures differ as they were selected to align with the different thermal decomposition temperatures of the secondary vs. primary / tertiary ligand blends. The wafers were thenAttorney Docket No. 5063.67W001 developed in a negative tone development process using a solution of 5% wt acetic acid in PGMEA. The wafers were then subjected to a hard bake (HB) for 60 seconds at a temperature of 250 °C.

[0175] Table 9 shows the nearest to 14nm critical dimension (CD) for each sample, the dose required to achieve this CD, and the corresponding line edge roughness (LER), all determined through inspection using CD-SEM and metrology software. The CD-SEM images are presented in Figs. 5 and 6.

[0176] TABLE 9:

[0177] Sample PEB (°C) Dose (mJ / cm2) CD (nm) LER (nm)

[0178] 140 83.75 13.95 2.9 PRZ 160 62.25 14.07 3.1

[0179] 180 42.50 14.09 3.0 140 79.00 13.83 2.9 PRZ-H1 160 58.50 13.88 3.0

[0180] 180 37.25 14.11 3.5 180 64.00 13.93 3.1 PRQ 200 53.00 14.26 3.4

[0181] 220 40.50 14.15 3.3 180 73.25 13.63 3.0 PRQ-H1 200 62.25 14.02 3.2

[0182] 220 48.50 14.17 3.5

[0183]

[0184] Reductions in the dose necessary to achieve 14p28 line space patterns were observed at 140 °C, 160 °C, and 180 °C for the ammonium chloride enhanced sample PRZ-H1 in comparison to the comparative non-additive enhanced sample PRZ. This indicates that the addition of ammonium chloride additive can improve the EUV sensitivity of organotin films formed from precursor solutions comprising a blend of primary and tertiary organyl ligands. Notably, the line edge roughness stayed the same or slightly improved for PEB temperatures 140 °C and 160 °C and increased by 0.5 for a 180 °C PEB for the ammonium chloride enhanced film. This suggests that a dose reduction can be achieved with the addition of ammonium chloride for organotin coatings comprising primary and tertiary organyl ligands withoutAttorney Docket No. 5063.67W001 significantly compromising patterning performance and may even be achieved while improving patterning performance in some embodiments.

[0185] The dose necessary to achieve 14p28 line space patterns was observed to increase at 180 °C, 200 °C, and 220 °C for additive-enhanced sample PRQ-H1 in comparison to nonadditive enhanced sample PRQ. This indicates that the addition of ammonium chloride additive can decrease the EUV sensitivity of organotin films formed from precursor solutions comprising secondary organyl ligands. Decreases in line edge roughness were observed at PEB temperatures of 180 °C and 200 °C. This indicates that the addition of an ammonium chloride additive can increase the quality of line space patterns formed from organotin precursor solutions comprising secondary organyl ligands, suggesting increased contrast and potential decreases in the occurrence of defects.

[0186] Example 4: Improved organyl ligand cleavage efficiency with ligand leaving promoting additives.

[0187] In this example, FTIR is used to determine the amount of organyl ligands through exposure dose of coatings deposited from an organotin photoresist comprising a ligand leaving promoting additive in comparison to a comparative sample absent an additive.

[0188] A photoresist precursor stock solution was prepared by combining a mixture comprising 40 mol% tert-butyl tin tris(3-pentoxide) and 60 mol% isopropyl tin tris (sec-butoxide) in a solvent comprising 62% 1 -pentanol and 38% 1 -propanol by weight such that the final solution had a Sn concentration of 0.065 M. Prior to formulation the solvent was adjusted to have a water concentration of about 300 ppm by weight. An aliquot of the stock solution was reserved as a comparative example absent of an additive and to a separate aliquot of stock solution triethylammonium nitrate was added at a molar ratio of 0.05 relative to Sn. The compounds used to formulate the solutions are presented in Tables 1 and 4 and the formulation details for each precursor solution are presented in Table 10.

[0189] TABLE 10:

[0190] Precursor Organotin Sn Water Additive Solvent

[0191] Solution Composition (mol %) Concentration Concentration (Ratio : Sn)

[0192]

[0193] Attorney Docket No. 5063.67W001

[0194] Pl (60%)

[0195] PRY S-l 0.065 M 300 ppm ** P2 (40%)

[0196] Pl (60%)

[0197] PRY-CI S-l 0.065 M 300 ppm C (0.05)

[0198] P2 (40%)

[0199]

[0200] Both photoresist precursor solutions were deposited onto FTIR grade Si wafers via spin coating to form coatings having an approximate thickness of about 30 nm, as determined by ellipsometry. The wafers were then subjected to a 100 °C post apply bake (PAB) before a pattern of 13.5 nm EUV radiation was exposed onto each wafer using an ASML NXE3400B scanner tool. The pattern consisted of an array of regions, with each region corresponding to a unique exposure dose ranging from about 0 mJ / cm2(unexposed) to about 90 mJ / cm2. Following the exposure step, the wafers were subjected to a 60 second post exposure bake at a temperature of 200 °C. The wafers were then analyzed using Fourier Transform Infrared Spectroscopy (FTIR) to determine the amount of organyl ligands remaining in each exposure region. The determination was made by integrating FTIR peak area from a C-H alkyl stretching frequency range from 2,800 cm'1to 3,016 cm1, which are consistent with the presence of the isopropyl and tert-butyl organyl ligands. The normalized fraction of organyl ligands was plotted as a function of exposure dose and shown in Fig. 7.

[0201] The results indicate that the coating deposited from the additive enhanced solution PRY-CI lost a greater fraction of its initial organyl ligands than the coating deposited from the comparative solution PRY absent of additive. These results further indicate that inclusion of ligand loss promoting additive triethylammonium nitrate can produce greater organyl ligand loss at lower exposure doses. Without being limited by theory, it is believed that organyl ligand cleavage is primarily responsible for generating image contrast, suggesting that a lower dose can be sufficient to produce patterns for ligand leaving promoter additive enhanced materials. This lower patterning dose is consistent with the data reported for resist solution PRY-CI in Example 2. To the extent that more ligands can be cleaved per radiation dose unit, the efficiency of patterning can be improved which can correspond to reduced costs and improved throughputs. This dose dependent difference in organyl ligand loss was not observed for otherwise identical coatings that were not subjected to a post-exposure bake, indicating that triethylammonium nitrate can influence the thermal stability of the organyl ligands afterAttorney Docket No. 5063.67W001 exposure. Accordingly, the post-exposure bake conditions can be selected to provide a desired extent of organyl ligand removal at a certain dose.

[0202] The embodiments above are intended to be illustrative and not limiting. Additional embodiments are within the claims. In addition, although the present invention has been described with reference to particular embodiments, those skilled in the art will recognize that changes can be made in form and detail without departing from the spirit and scope of the invention. Any incorporation by reference of documents above is limited such that no subject matter is incorporated that is contrary to the explicit disclosure herein. To the extent that specific structures, compositions and / or processes are described herein with components, elements, ingredients or other partitions, it is to be understand that the disclosure herein covers the specific embodiments, embodiments comprising the specific components, elements, ingredients, other partitions or combinations thereof as well as embodiments consisting essentially of such specific components, ingredients or other partitions or combinations thereof that can include additional features that do not change the fundamental nature of the subject matter, as suggested in the discussion, unless otherwise specifically indicated. The use of the term "about" herein refers to expected uncertainties in the associated values as would be understood in the particular context by a person of ordinary skill in the art. A person of ordinary skill in the art is notified that the assertions above regarding the contemplation of subranges within explicit ranges are sincerely intended to provide explicit written description for the subranges, as clearly suggested, even though not explicitly written and that the subranges are not believed to change the character of the associated invention, although of course the specific values of parameters will certainly quantitatively change corresponding results obtained, which could influence patentability even though the basic character of the invention may not be changing, in view of the potential nature of the state of the art known or unknown at filing given that the inventiveness may follow from the factual details. A person of ordinary skill in the art is further notified that upper and lower values of explicit ranges and values within explicit ranges are intended to provide explicit written description for endpoints of subranges, furthermore explicit disclosure of upper and / and lower values of explicit ranges of a certain feature are intended to be disclosed as upper and / or lower values for additional ranges, including subranges.

Claims

Attorney Docket No. 5063.67W001 What is claimed is:

1. A solution comprising a blend of:an organic solvent,an organotin composition represented by the formula RSnLt, wherein R is an organyl ligand having from 1 to 31 carbon atoms and optionally substituted with a heteroatom or unsaturated bond at any position and L is a hydrolysable ligand, andan additive composition represented by the formula Q+nAn’ wherein l<n<5 A11’ is Ch, Br’, OH’, or an oxyanion comprising at least 1 and up to 10 oxygen atoms bonded to one or more core atoms selected from B, Si, C or group 15-17 elements, Q+is H+, onium cation [ERcm]+, or a combination thereof wherein E is a group 15 to group 17 element, each Rcis independently selected from H, 1 to 11 carbon alkyl, alkenyl, or aryl groups, and a 1 to 11 carbon hydroxyl substituted group, and are attached to E via an E-C bond, and 2<m<4 with the proviso that Q+is not H+when A11’ is OH’ or phosphite.

2. The solution of claim 1 wherein A11’ comprises O’, Br’ or a combination thereof.

3. The soludon of claim 1 wherein the oxyanion is selected from the group consisting of borate, carbonate, silicate, nitrate, nitrite, sulfate, sulfite, thiosulfate, chlorate, perchlorate, chlorite, iodate, periodate, phosphate, phosphite, arsenate, arsenite, antimonate, selenate, tellurite, tellurate, pyrophosphate, tripolyphosphate, tetraborate, oxalate, dithionate, pyrosulfate, hyponitrite, and a mixture thereof.

4. The solution of any one of claims 1-3 wherein Q+is [NRn4]+.

5. The solution of any one of claims 1-3 wherein Q+is choline, ammonium (NH4+), tetramethyl ammonium, tetraethyl ammonium, tetrabutyl ammonium, trimethyl ammonium, triethyl ammonium, tributyl ammonium or a combination thereof.

6. The solution of any one of claims 1-3 wherein at least one Rcis a hydrogen.

7. The solution of any one of claims 1-6 wherein the additive composition is present at a molar ratio relative to Sn from 0.001 to 2.Attorney Docket No. 5063.67W0018. The solution of any one of claims 1-6 wherein the additive composition is present at a molar ratio relative to Sn from 0.01 to 0.5.

9. The solution of claim 1 wherein the additive composition is triethyl ammonium nitrate or tetraethyl ammonium nitrate.

10. The solution of claim 1 wherein the additive composition is ammonium chloride, tetramethyl ammonium chloride, or choline chloride.

11. The solution of any one of claims 1-10 wherein R is branched alkyl represented by R1R2R3C where R1and R2are independently an alkyl group with 1-10 carbon atoms, and R3is hydrogen or an alkyl group with 1-10 carbon atoms.

12. The solution of any one of claims 1-10 wherein R is methyl, ethyl, isopropyl, propyl, butyl, sec -butyl, tert-butyl, n-pentyl, sec-pentyl, isopentyl, or neopentyl.

13. The solution of any one of claims 1-10 wherein R is an organyl ligand with a tertiary carbon bonded to Sn, a primary carbon bonded to Sn, or a mixture thereof.

14. The solution of any one of claims 1-10 wherein R is substituted with one of more heteroatoms selected from the group consisting of O, S, N, Se, Te, Si, Ge, Sn, F, and I.

15. The solution of any one of claims 1-14 wherein L is selected from the group consisting of alkylamido, dialkylamido, disilylamido, alkoxo, aryloxo, azido, amidinato, imido, and fluorinated analogues thereof.

16. The solution of any one of claims 1-14 wherein L is OR', NR'2, CCR', or a combination thereof wherein R' is an alkyl group having from 1 to 11 carbon atoms.

17. The solution of any one of claims 1-14 wherein L is tert-butoxide, sec-butoxide, tertamyloxide, 3-pentoxide, diethyl amide, or dimethyl amide, or a combination thereof.Attorney Docket No. 5063.67W00118. The solution of any one of claims 1-17 having a Sn concentration from 0.0025 M to 1 M.

19. The solution of any one of claims 1-18 further comprising a second organotin composition represented by the formula RxSnL'3, wherein Rxis an organyl ligand having from 1 to 31 carbon atoms and different from R and L' is a hydrolysable ligand and the same of different from L.

20. The solution of any one of claims 1-19 further comprising a radical scavenger additive.

21. The solution of claim 19 wherein the radical scavenger additive is TEMPO, TEMPOL, BHT, PTIO, or BHA or a combination thereof.

22. The solution of any one of claims 1-21 further comprising water at a concentration from 200 ppm to 10,000 ppm by weight.

23. The solution of any one of claims 1-22 wherein the solvent is an aromatic hydrocarbon, an ether, an alcohol, a ketone, or a mixture thereof.

24. A radiation patternable organometallic coating comprising a tin oxo-hydroxo network with organo ligands bonded to the tin via Sn-C bonds and an incorporated additive, wherein the organo ligands comprise group with 1-31 carbon atoms with optional unsaturated carbon bonds wherein one or more carbon atoms are optionally substituted with heteroatoms, wherein the incorporated additive is provided in a formulation represented by the formula Q+nAn’ wherein l<n<5 A is CT, Br , OH’, or an oxyanion comprising at least 1 and up to 10 oxygen atoms bonded to one or more core atoms selected from B, Si, C or group 15-17 elements, Q+is H+, onium cation [ERcm]+, or a combination thereof wherein, 2<m<4, E is a group 15-17 element and each Rcis independently selected from H, 1 to 11 carbon alkyl, aryl, and 1 to 11 carbon hydroxyl substituted groups, and are attached to E via an E-C bond, and 2<m<4, with the proviso that Q+is not H+when A11’ is OH’ or phosphite.Attorney Docket No. 5063.67W001 25. The coating of claim 24 wherein the coating comprises additive at a molar ratio from about 0.001 to about 0.5 relative to tin.

26. The coating of claim 24 wherein the coating comprises additive at a molar ratio from about 0.01 to about 0.25 relative to tin.

27. The coating of any one of claims 24-26 wherein Q+is an onium ion with at least one proton and deprotonation of the onium ion forms a volatile compound.

28. The coating of any one of claims 24-26 wherein Q+is an ammonium ion.

29. The coating of any one of claims 24-28 wherein A11-comprises CT, Br or a mixture thereof.

30. The coating of any one of claims 24-28 wherein A11-comprises a nitrate ion.

31. The coating of any one of claims 24-30 wherein the organo ligands comprise methyl, ethyl, propyl, isopropyl, n-butyl, sec -butyl, isobutyl, or tert-butyl, or combinations thereof.

32. The coating of any one of claims 24-31 comprising a blend of two or more different organo ligands.

33. The coating of inventive concept Al wherein the coating can be represented by (R, R’)SnO3 / 2-x / 2 (OH)X: Q+nAn’ wherein 0 < x < 3, wherein R and R’ independently comprise an alkyl, an aryl, an alkenyl, an alkynyl, or a cycloalkyl group with 1-31 carbon atoms wherein one or more carbon atoms are optionally substituted with heteroatoms, wherein Q+nAn’ is integrated into the oxo-hydroxo network with potential ligand bonding to the tin ion and possible degassing of volatile products of the additive.

34. The coating of claim 33 wherein (R,R’) = RaRb, a+b=l and a,b > 0.05 = 5 mol%.

35. The coating of any one of claims 24-34 wherein the coating has a thickness from about 1 nm to about 100 nm.Attorney Docket No. 5063.67W00136. The coating of any one of claims 24-34 wherein the coating has a thickness from about 2 nm to about 50 nm.

37. An article comprising a substrate and the radiation patternable coating of any one of claims 24-36.

38. The article of claim 37 wherein the substrate comprises Si.

39. The article of claim 37 or claim 38 wherein the radiation patternable coating comprises a physical pattern.

40. The coating of any one of claims 24-36 wherein the coating is deposited from a precursor solution comprising an organotin composition represented by the formula RSnLt and the incorporated additive, wherein R comprises an alkyl, an aryl, an alkenyl, an alkynyl, or a cycloalkyl group with 1-31 carbon atoms wherein one or more carbon atoms are optionally substituted with heteroatoms, L is a hydrolysable ligand, and wherein the solution has a tin concentration from about 0.00025 M to about 1.0 M and the additive is present at a molar ratio from about 0.001 to about 0.5 relative to the total concentration of tin.

41. The coating of claim 40 wherein E is nitrogen.

42. The coating of claim 40 or claim 41 wherein Q+is an onium ion with at least one proton and deprotonation of the onium ion forms a volatile compound.

43. The coating of any one of claims 40-42 wherein A11’ comprises Cl’, Br’ or a mixture thereof.

44. The coating of any one of claims 40-42 wherein A11’ comprises a nitrate ion.

45. A method for patterning an organometallic coating comprising a tin oxo-hydroxo network with organo ligands bonded to the tin via Sn-C bonds and an additive incorporated into the coating as provided in a precursor represented by the formula Q+nAn’ wherein l<n<5 A is Cl’,Attorney Docket No. 5063.67W001 Br’, OH’, or an oxyanion comprising at least 1 and up to 6 oxygen atoms bonded to a core atom selected from B, Si, C or group 15-17 elements, Q+is H+, onium cation [ERcnm]+, or a combination thereof wherein E is a group 15-17 elements and each Rcis independently selected from H, 1 to 11 carbon alkyl, aryl, and 1 to 11 carbon hydroxyl substituted groups, and are attached to E via an E-C bond, with the proviso that Q+is not H+when A11’ is OH’ or phosphite, wherein the organo ligands comprise 1-31 carbon atoms with optional unsaturated carbon bonds wherein one or more carbon atoms are optionally substituted with heteroatoms, the method comprising:exposing a pattern of radiation of the coating to form a latent image comprising exposed and unexposed regions anddeveloping the coating with a developer composition to selectively remove either the exposed material or the unexposed material.

46. The method of claim 45 wherein the radiation source is EUV radiation.

47. The method of claim 45 wherein the radiation source has a wavelength of 13.5 nm.

48. The method of any one of claims 45-47 wherein the pattern of radiation is exposed at a dose from about 1 mJ / cm2to about 150 mJ / cm2.

49. The method of any one of claims 45-48 further comprising baking the coating at a temperature from about 45 °C to about 225 °C before developing the coating and after exposing a pattern of radiation.

50. The method of claim 49 wherein the baking is performed for at least about 0.1 minutes to about 30 minutes.

51. The method of any one of claims 45-50 wherein the developing comprises a negative tone development process.

52. The method of claim 51 wherein the developer composition comprises an organic solvent.Attorney Docket No. 5063.67W001 53. The method of claim 51 wherein the developing comprises a solventless development process.

54. The method of claim 53 wherein the developer composition comprises a plasma or a reactive developer gas.

55. The method of any one of claims 45-50 wherein the developing comprises a positive tone development process.

56. The method of claim 55 wherein the developer composition comprises an aqueous base.

57. The method of any one of claims 45-56 wherein the organic ligands comprise a blend of different ligands.

58. The method of any one of claims 45-57 wherein E is nitrogen.

59. The method of any one of claims 45-57 wherein Q+is an onium ion with at least one proton and deprotonation of the onium ion forms a volatile compound.

60. The method of any one of claims 45-59 wherein A11-comprises CT, Br or a mixture thereof.

61. The coating of any one of claims 45-59 wherein A11-comprises a nitrate ion.

62. The method of any one of claims 45-61 wherein the organometallic coating comprises a radical scavenger additive at a concentration from about 0.000025 M to about 0.4 M.

63. The method of claim 62 wherein the radical scavenger additive comprises a hindered amine, a hindered phenol, TEMPO, BHT, BHA, TEMPOL, PTIO, or a combination thereof.

64. The method of any one of claims 45-63 wherein Q+is an aromatic onium ion.Attorney Docket No. 5063.67W001 65. The method of any one of claims 45-64 further comprising forming the coating by spin coating a solution of any one of claims 1-23.