Adhesive with thermochromic indicator

Hindered benzyl compounds in adhesive compositions offer visual cues for monitoring cure and debonding, addressing the uncertainty in substrate separation by providing clear indicators for safe and controlled separation.

WO2026239307A1PCT designated stage Publication Date: 2026-11-193M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054765
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing structural adhesives lack effective indicators for monitoring the degree of cure or debonding, which can lead to uncertainty in the separation of bonded substrates.

Method used

Incorporation of hindered benzyl compounds in adhesive compositions that provide a visual color change at cure or debonding temperatures, acting as thermochromic indicators to signal the appropriate time for substrate separation.

Benefits of technology

Enables precise monitoring of adhesive cure and debonding through visible color changes, ensuring safe and controlled separation of bonded substrates without damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026054765_19112026_PF_FP_ABST
    Figure IB2026054765_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Aspects of the present disclosure relate to an adhesive composition, a system, and a method of use thereof. The adhesive composition can be a hindered benzyl having the formula (I), wherein X is an oxo or a hydroxy group, and R is a hydrogen, alkyl, an alkylbenzyl, or an aminoalkyl. The alkyl, the alkylbenzyl or aminoalkyl optionally includes an oxygen linkage to the hindered benzyl. In at least one embodiment, the hindered benzyl is present in an effective amount that indicates a degree of cure or debonding by providing a visual color change as the degree of cure or debonding occurs.
Need to check novelty before this filing date? Find Prior Art

Description

PA103894W002ADHESIVE WITH THERMOCHROMIC INDICATORField of the Invention

[0001] Provided are adhesive compositions containing thermochromic indicators that can be useful in structural adhesive applications.Background

[0002] Adhesives have been used in many structural applications. Such structural applications have included vehicles, computer cases, buildings, and appliances. For example, structural adhesives have been used in vehicle assembly (e.g., automobile and aircraft assembly) to replace or augment conventional joining techniques such as welds, nuts and bolts, and rivets. Epoxy compositions are known and have been used for structural adhesive applications. Tougheners have been included in epoxy adhesive compositions to improve the impact resistance of the adhesive.

[0003] Various hindered benzyls have been used in lubricants, automatic transmission fluids, differential fluids, and turbine oils, and have been used in applications over 150 degrees Celsius.Summary

[0004] Aspects of the present disclosure relate to an adhesive composition. The adhesive composition can be a hindered benzyl having the formula:, wherein X is an oxo or a hydroxy group, and R is a hydrogen, alkyl, an alkylbenzyl, or an aminoalkyl, wherein the alkyl, the alkylbenzyl or aminoalkyl optionally includes an oxygen linkage to the hindered benzyl. In at least one embodiment, the hindered benzyl is present in an effective amount that indicates a degree of cure or debonding by providing a visual color change as the degree of cure or debonding occurs.

[0005] In at least one embodiment, the hindered benzyl is present in an effective amount that indicates mixing of a first component and a second component of a two-component (2K) adhesive composition.

[0006] In at least one embodiment, the hindered benzyl can act as an indicator for reversible and / or non-reversible heating color change.

[0007] The alkylbenzyl is independently substituted with alkyl groups on an ortho position to a phenol group, the alkyl groups have more than one carbon atom.

[0008] In at least one embodiment, the alkylbenzyl has the formula:, wherein Ri is an alkyl group or an alkoxy group having between 1 and 4 carbon atoms, and each Rz is, independently a Cl to CIO alkyl, and R3 is an oxygen or a hydroxy group. In one example, Ri is a methyl group. In one example, Rj is a tert-butyl group or a methyl group. In one example, the hindered benzyl is 4,4'-methylenebis(2,6-di-t-butylphenol) (MTBP) or a galvinoxyl free radical.

[0009] In at least one embodiment, the hindered benzyl has the formula:

[0010] In at least one embodiment, the aminoalkyl has the formulaCH2-N(R)2, wherein each R is, independently, a hydrogen, or a Cl to CIO alkyl.

[0011] In at least one embodiment, the hindered benzyl has the formula:OH, wherein each R is, independently, a Cl to CIO alkyl.

[0012] In at least one embodiment, the hindered benzyl has a concentration no greater than 5 wt.% in the first component or the second component.

[0013] In at least one embodiment, the hindered benzyl excludes phenolphthalein. The visual color change can be silver to purple. The hindered benzyl can be non-staining. The hindered benzyl is configured to provide the visual color change of the adhesive composition at a debonding temperature. The hindered benzyl can also be configured to produce a visual color change as part of a mix indicator.

[0014] The adhesive composition can include a first component and a second component that chemically reacts with the first component. The hindered benzyl can be present in the first component, the second component, or combinations thereof.

[0015] The adhesive composition can include a secondary curative. In at least one embodiment, the secondary curative includes thiol as a curative for the epoxy. In at least one embodiment, at least one of the first component or the second component comprises an amine or thiol curing agent, at least one of the first component or the second component comprises a curable epoxy resin, at least one of the first component or the second component comprises a toughening agent.

[0016] In at least one embodiment, the curable epoxy resin has two or more epoxy groups and the amine curing agent has two or more amine hydrogens and the molar ratio of epoxy groups on the curable epoxy resin to amine hydrogens on the amine curing agent ranges from about 0.5: 1 to about 3: 1.

[0017] In at least one embodiment, the amine curing agent comprises at least one of an aliphatic diamine, aromatic diamine, an arylalkylene diamine, a polyether diamine, or a combination thereof. In at least one embodiment, the curable epoxy resin comprises a bisphenol epoxy resin, a novolac epoxy resin, or a combination thereof. In at least one embodiment, the first component or second component further comprise at least one of a corrosion inhibitor, a plasticizer, a silane coupling agent, a thixotropic agent, a pigment, a reinforcing agent, clay, or a filler. In at least one embodiment, the adhesive composition is curable at room temperature and can also be a 1 component adhesive composition.

[0018] Additional aspects of the present disclosure relate to a system that includes an applicator and a container containing the adhesive composition. In at least one embodiment, the container includes a first chamber configured to contain the first component of the adhesive composition. The system includes an applicator tip coupled to the first chamber. The second chamber contains the second component, and the applicator tip is coupled to the second chamber. The first component and second component are combined at the applicator tip.

[0019] Additional aspects of the present disclosure relate to a method for forming a bond between two substrates. The method can include applying the adhesive composition to a first substrate and / or a second substrate by admixing the first component with the second component.

[0020] The method can include contacting the first substrate or the second substrate to the adhesive composition such that the adhesive composition is disposed between the first substrate and the second substrate. In at least one embodiment, contacting the first substrate or the second substrate to the adhesive composition optionally includes leaving an exposed area of the adhesive composition to observe a visual color change of the cured adhesive composition.

[0021] The method can include curing, using a curing process, the adhesive composition to form a cured adhesive composition. The adhesive composition is a first color, and the cured adhesive composition is a second color.

[0022] In at least one embodiment, the first substrate and second substrate are components of an automobile.

[0023] In at least one embodiment, the method can also include heating the cured adhesive composition to a debonding temperature, and allowing the cured adhesive composition to perform a visual color change from the second color to the first color. In at least one embodiment, the visual color change indicates that at a temperature that the cured adhesive composition can be separated from the first or second substrate or split during debonding and is associated with the debonding temperature.

[0024] The method can also include removing the first substrate from the second substrate at the temperature responsive to the visual color change. In at least one embodiment, the second color is purple, the first color is silver.Brief Description of the Drawings

[0025] To easily identify the discussion of any particular element or act, the most significant digit or digits in a reference number refer to the figure number in which that element is first introduced.

[0026] FIG. 1 illustrates a flowchart of bonding two substrates using an adhesive composition in accordance with one embodiment.

[0027] FIG. 2A illustrates a side cross-sectional view of two bonded substrates in accordance with one embodiment.

[0028] FIG. 2B illustrates a top view of two bonded substrates in accordance with one embodiment.

[0029] FIG. 3 illustrates a system for joining two substrates together in accordance with one embodiment.

[0030] FIG. 4A illustrates a mechanical fastener in accordance with one embodiment.

[0031] FIG. 4B illustrates a mechanical fastener in accordance with one embodiment.

[0032] FIG. 4C illustrates a mechanical fastener in accordance with one embodiment.

[0033] FIG. 5 illustrates an aspect of the subject matter in accordance with one embodiment.Detailed Description

[0034] Adhesive compositions in the present disclosure can include a hindered benzyl such that adhesive composition produces a visual color change at a debonding temperature and / or a cure temperature of the adhesive composition. Advantageously, the hindered benzyl can act as a thermochromic indicator. Additional methods can include using a hindered benzyl as a thermochromic indicator for an adhesive composition.

[0035] In at least one embodiment, the adhesive composition is a one-component (IK) adhesive composition that is heat initiated. The adhesive composition can also be a two-component adhesive composition that uses a first component (e.g., amine curing agent) and a second component (e.g., a curable epoxy resin) that is mixed together to form the adhesive composition at sub-ambient temperatures or greater (e.g., at least 15 degrees Celsius).

[0036] The hindered benzyl can be present with the first component, the second component, or both the first component and the second component. The first component may be referred to as the "accelerator component" and can comprise the amine curing agent and any catalysts. The second part may be referred to as the "base resin component" and can comprise any curable resins. The other components of the curable adhesive composition, described in further detail below, can be included in one or both the first and second components.

[0037] The present disclosure further provides an adhesive dispenser comprising a first chamber and a second chamber. The first chamber comprises the first part, and the second chamber comprises the second part. The two components can be combined through the adhesive dispenser. Such adhesive dispensers can include nozzles that can be integral to or detachable from the container. Examples of the adhesive dispensers are commercially available from 3M (St. Paul, MN).

[0038] For example, the first component can be the part A component. The first component can include an amine curing agent capable of crosslinking an epoxy resin at room temperature. Theamine curing agent can include one or more of aliphatic amines, modified cycloaliphatic amines, polyetheramines, polyamides, amidoamines, aromatic amines, and / or mixtures thereof. The amine curing agent can include at least two amino groups. The amino groups in the amine curing agent are each independently primary or secondary amino groups. Typically, at least one of the amino groups is a primary amino group so that a crosslinked network may form.

[0039] In some embodiments, the amine curing agent includes at least two primary amino groups. Useful amine curing agents may be aliphatic amines including at least two amino groups. In some embodiments, an alkylene polyamine, for example, a linear or branched alkylene polyamine is included in the curable composition.

[0040] Useful alkylene polyamines include ethylene amines (e.g., ethylenediamine, diethylenetriamine, triethylenetetramine, etc.), propylamines (e.g., dimethylaminopropyl amine, diethylaminopropylamine, and cyclohexylaminopropylamine), higher alkylenediamines (e.g., hexamethylenediamine, methylpentamethylenediamine, and trimethylhexanediamine), polyetheramines (e.g., polyoxyalkylene diamines such as polyoxypropylene diamines of various molecular weights and 4,7, 10-trioxa-l, 13-tridecane diamine).

[0041] In at least one embodiment, catalytically active tertiary acryl- or alkyl-amines, such as benzyldimethylamine, tris(dimethylamino)phenol, piperidine or piperidine derivatives, may also be used. Various imidazole derivatives, preferably solid imidazole derivatives, may also be used as catalytically-active accelerators. Examples which may be mentioned are 2-ethyl-2-methylimidazole, N-butylimidazole, benzimidazole and N-Cl to C12-alkylimidazoles or N-arylimidazoles.

[0042] An amine curing agent useful in the curable compositions disclosed herein can comprise at least two amino groups and at least one aromatic ring. The amine curing agent may be an aromatic polyamine, in which the amino groups are bonded directly to the aromatic ring, or an arylalkylenyl polyamine, in which the amino groups are bonded to alkylene groups that are in turn bonded to the aromatic ring. An amine curing agent may also contain two or more aromatic rings and at least two amino groups. In any of these embodiments, the aromatic ring can be unsubstituted or substituted by one or more halogens (e.g., fluoro, chloro, bromo, iodo), alkyl groups having 1 to 4 carbon atoms (e.g., methyl or ethyl), or hydroxyalkyl groups having 1 to 4 carbon atoms (e.g., hydroxymethyl). For amines containing two or more aromatic rings, the rings may be directly connected or connected, for example, by a branched or straight-chain alkylene group having 1 to 4 carbon atoms that may optionally be substituted by one or more halogens (e.g., fluoro, chloro, bromo, iodo), an oxygen, a sulfur, or a sulfone group. Examples of suitable amine curing agents that comprise at least two amino groups and at least one aromatic ring include phenylenediamine (e.g., meta-phenylenediamine or para-phenylenediamine), diethyl toluene diamine (e.g., in any of its isomeric forms), diamino toluene (e.g., 2, 3 -diaminotoluene and 3,4- diaminotoluene, and methyl-m-phenylenediamine), l,2-diamino-3,5-dimethylbenzene, 4,5-dimethyl-l,2- phenylenediamine, 2,4,6-trimethyl-m-phenylenediamine, 2,3,5,6-tetramethyl-p-phenylenediamine, aminobenzylamines (e.g., 2-aminobenzylamine and 4-aminobenzylamine), ethylenedianiline, 2,2'- biphenyldiamine, diaminodiphenylmethane, diaminodiphenylsulfone, halogenated substituted pheneylene diamines (e.g., 4-chloro-l,3-diaminobenzene, 4-chloro-l,2-diaminobenzene, and 4-bromo-l,2-diaminobenzene), a xylylenediamine (e.g., ortho-xylylenediamine or meta- xylylenediamine), and 4-(2- aminoethyl)aniline .

[0043] An amine curing agent useful in the curable compositions disclosed herein can comprise at least two amino groups and at least one cycloaliphatic ring. The amino groups may be bonded directly to the cycloaliphatic ring, or the amino groups may be bonded to straight-chain or branched alkylene groups that are in turn bonded to the cycloaliphatic ring. An amine curing agent may also contain two or more cycloaliphatic rings and at least two amino groups. In any of these embodiments, the cycloaliphatic ring can be unsubstituted or substituted by one or more halogens (e.g., fluoro, chloro, bromo, iodo), straight- chain or branched alkyl groups having 1 to 4 carbon atoms (e.g., methyl or ethyl), or hydroxyalkyl groups having 1 to 4 carbon atoms (e.g., hydroxymethyl). In any of these embodiments, the cycloaliphatic ring may be a carbocyclic ring, for example, including no heteroatoms such as sulfur or nitrogen. For amines containing two or more cycloaliphatic rings, the rings may be directly connected or connected, for example, by a branched or straight-chain alkylene group having 1 to 4 carbon atoms that may optionally be substituted by one or more halogens (e.g., fluoro, chloro, bromo, iodo), an oxygen, a sulfur, or a sulfone group. Examples of suitable amine curing agents that comprise at least two amino groups and at least one cycloaliphatic group are the fully or partially hydrogenated products of any of the amine curing agents that comprise at least two amino groups and at least one aromatic ring described above. For example, suitable amine curing agents include diaminocyclohexanes (e.g., 1,2-diaminocyclohexane or 1,4-diaminocyclohexane in their cis- or trans- forms) and 3-aminomethyl-3, 5, 5 -trimethylcyclohexylamine (also called isophorone diamine).

[0044] Several amine curing agents including at least two amino groups and at least one of an aromatic ring or a cycloaliphatic ring are available, for example, from Lonza, Basel, Switzerland, and Amberlite Corporation, Baton Rouge, LA. Other amine curing agents that may be useful include polyetheramines available, for example, from Huntsman Chemical, The Woodlands, Tex., under the trade designation "JEFF AMINE".

[0045] In some embodiments, the molar ratio of epoxy groups on the curable epoxy resin to amine hydrogens on the amine curing agent ranges from about 0.5: 1 to about 3: 1, in some embodiments, in a range from about 0.5 : 1 to about 2 : 1 , or about 1 : 1.

[0046] In at least one embodiment, the second component can include the curable epoxy resin. The curable epoxy resin can include epoxy compounds useful for adhesive composition.

[0047] For example, the curable epoxy resin can include aromatic polyepoxide resins (e.g., a chain-extended diepoxide or novolac epoxy resin having at least two epoxide groups) and aromatic monomeric diepoxides. A crosslinkable epoxy resin typically will have at least two epoxy end groups. The aromatic polyepoxide or aromatic monomeric diepoxide typically contains at least one (in some embodiments, at least 2, in some embodiments, in a range from 1 to 4) aromatic ring that is optionally substituted by a halogen (e.g., fluoro, chloro, bromo, iodo), alkyl having 1 to 4 carbon atoms (e.g., methyl or ethyl), or hydroxyalkyl having 1 to 4 carbon atoms (e.g., hydroxymethyl). For epoxy resins containing two or more aromatic rings, the rings may be connected, for example, by a branched or straight-chain alkylene group having 1 to 4 carbon atoms that may optionally be substituted by halogen (e.g., fluoro, chloro, bromo, iodo).

[0048] Examples of aromatic epoxy resins useful in the curable compositions disclosed herein include novolac epoxy resins (e.g., phenol novolacs, ortho-, meta-, or para-cresol novolacs or combinations thereof), bisphenol epoxy resins (e.g., bisphenol A, bisphenol F, halogenated bisphenol epoxies, and combinations thereof), resorcinol epoxy resins, tetrakis phenylolethane epoxy resins and combinations of any of these. Useful epoxy compounds include diglycidyl ethers of difunctional phenolic compounds (e.g., p,p'-dihydroxydibenzyl, p,p'-dihydroxydiphenyl, p,p'-dihydroxyphenyl sulfone, p,p'- dihydroxybenzophenone, 2,2'-dihydroxy-l,l-dinaphthylmethane, and the 2,2', 2,3', 2,4', 3,3', 3,4', and 4,4' isomers of dihydroxydiphenylmethane, dihydroxydiphenyl dimethylmethane, dihydroxydiphenylethylmethylmethane, dihydroxydiphenylmethylpropylmethane, dihydroxydiphenylethylphenylmethane, dihydroxydiphenylpropylphenylmethane, dihydroxydiphenylbutylphenylmethane, dihydroxydiphenyl tolylethane, dihydroxydiphenyltolylmethylmethane,dihydroxydiphenyl dicyclohexylmethane, and dihydroxydiphenylcyclohexane. )

[0049] In some embodiments, the adhesive includes a bisphenol diglycidyl ether, wherein the bisphenol (i.e., -O-CeHs-CFh-CeHs-O-) may be unsubstituted (e.g., bisphenol F), or either of the phenyl rings or the methylene group may be substituted by one or more halogens (e.g., fluoro, chloro, bromo, iodo), methyl groups, trifluoromethyl groups, or hydroxymethyl groups.

[0050] Examples of aromatic monomelic diepoxides useful in the curable compositions according to the present disclosure include the diglycidyl ethers of bisphenol A and bisphenol F and mixtures thereof. Bisphenol epoxy resins, for example, may be chain extended to have any desirable epoxy equivalent weight. Chain extending epoxy resins can be carried out by reacting a monomelic diepoxide, for example, with a bisphenol in the presence of a catalyst to make a linear polymer.

[0051] In some embodiments, the aromatic epoxy resin (e.g., either a bisphenol epoxy resin or a novolac epoxy resin) may have an epoxy equivalent weight of at least 150, 170, 200, or 225 grams per equivalent. In some embodiments, the aromatic epoxy resin may have an epoxy equivalent weight of up to 2000, 1500, or 1000 grams per equivalent. In some embodiments, the aromaticepoxy resin may have an epoxy equivalent weight in a range from 150 to 2000, 150 to 1000, or 170 to 900 grams per equivalent. In some embodiments, the first epoxy resin has an epoxy equivalent weight in a range from 150 to 450, 150 to 350, or 150 to 300 grams per equivalent. Epoxy equivalent weights may be selected, for example, so that the epoxy resin may be used as a liquid or solid, as desired.

[0052] For some applications, it may be useful to incorporate a flexible, non-aromatic chain into the crosslinked epoxy network. In some cases, non-aromatic epoxy resins can be useful as reactive diluents that may help control the flow characteristics of the adhesive composition. A non-aromatic epoxy useful in the curable compositions according to the present disclosure can include a branched or straight-chain alkylene group having 1 to 20 carbon atoms optionally interrupted with at least one -O- and optionally substituted by hydroxyl. In some embodiments, the non-aromatic epoxy can include a poly(oxyalkylene) group having a plurality (x) of oxyalkylene groups, OR1, wherein each R1is independently C2 to C5 alkylene, in some embodiments, C2 to C3 alkylene, x is 2 to about 6, 2 to 5, 2 to 4, or 2 to 3. To become crosslinked into a network, useful non-aromatic epoxy resins will typically have at least two epoxy end groups. Examples of useful non-aromatic epoxy resins include glycidyl epoxy resins such as those based on diglycidyl ether compounds comprising one or more oxyalkylene units. Examples of these include resins made from ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, propanediol diglycidyl ether, butanediol diglycidyl ether, and hexanediol diglycidyl ether. Other useful non-aromatic epoxy resins include a diglycidyl ether of cyclohexane dimethanol, a diglycidyl ether of neopentyl glycol, a triglycidyl ether of trimethylolpropane, and a diglycidyl ether of 1,4-butanediol. In some embodiments, the non- aromatic epoxy is present at up to 20 (in some embodiments, 15, 10, 9, 8, 7, 6, or 5) percent by weight, based on the total weight of epoxy resin in the curable adhesive composition. In some embodiments, non-aromatic epoxies can be present in higher concentrations. For example, cycloaliphatic epoxy resins can form a majority of the curable epoxy resin (e.g., at least 50 percent, at least 60 percent, or at least 70 percent by weight based on the total weight of epoxy resin).

[0053] Crosslinked aromatic epoxies (that is, epoxy polymers) as described herein will be understood to be preparable by crosslinking aromatic epoxy resins. The crosslinked aromatic epoxy typically contains a repeating unit with at least one (in some embodiments, at least 2, in some embodiments, in a range from 1 to 4) aromatic ring (e.g., phenyl group) that is optionally substituted by one or more halogens (e.g., fluoro, chloro, bromo, iodo), alkyl groups having 1 to 4 carbon atoms (e.g., methyl or ethyl), or hydroxyalkyl groups having 1 to 4 carbon atoms (e.g., hydroxymethyl). For repeating units containing two or more aromatic rings, the rings may beconnected, for example, by a branched or straight-chain alkylene group having 1 to 4 carbon atoms that may optionally be substituted by halogen (e.g., fluoro, chloro, bromo, iodo).

[0054] Several curable epoxy resins useful in the curable composition according to the present disclosure are commercially available. For example, several epoxy resins of various classes and epoxy equivalent weights are available from Dow Chemical Company, Midland, Mich.; Momentive Specialty Chemicals, Inc., Columbus, OH; Huntsman Advanced Materials, The Woodlands, Tex.; CVC Specialty Chemicals Inc. Akron, OH (acquired by Emerald Performance Materials); and Nan Ya Plastics Corporation, Taipei City, Taiwan. Examples of commercially available glycidyl ethers include diglycidylethers of bisphenol A (e.g. those available under the trade designations "EPON 828", "EPON 1001", "EPON 1310" and "EPON 1510" from Hexion Specialty Chemicals GmbH, Rosbach, Germany, those available under the trade designation "D.E.R." from Dow Chemical Co. (e.g., D.E.R. 331, 332, and 334), those available under the trade designation "EPICLON" from Dainippon Ink and Chemicals, Inc. (e.g., EPICLON 840 and 850) and those available under the trade designation " YL-980" from Japan Epoxy Resins Co., Ltd.); diglycidyl ethers of bisphenol F (e.g. those available under the trade designation "EPICLON" from Dainippon Ink and Chemicals, Inc. (e.g., "EPICLON 830")); polyglycidyl ethers of novolac resins (e.g., novolac epoxy resins, such as those available under the trade designation "D.E.N." from Dow Chemical Co. (e.g., D.E.N. 425, 431, and 438)); and flame retardant epoxy resins (e.g., "D.E.R. 580", a brominated bisphenol type epoxy resin available from Dow Chemical Co.). Examples of commercially available non- aromatic epoxy resins include the glycidyl ether of cyclohexane dimethanol, available from Hexion Specialty Chemicals GmbH, under the trade designation "HELOXY MODIFIER 107".

[0055] An epoxy cured with an amine curing agent will typically have crosslinked units represented by formula,, wherein R is an aryl, arylalkylene, alkylene-aryl-alkylene, a branched alkylene, straight-chain alkylene, or cycloalkylene group as described above, optionally including ether linkages, and wherein the asterisk (*) indicates that the O is bonded to the epoxide backbone, usually to an aromatic ring, although in some embodiments, to a cycloaliphatic ring or a branched or straight-chain alkylene group having 1 to 20 carbon atoms optionally interrupted with at least one -O- and optionally substituted by hydroxyl as described above.

[0056] In at least one embodiment, the curable adhesive composition can include the hindered benzyl. The hindered benzyl can be used to provide a visual color change in the adhesive composition in response to debonding or curing. In at least one embodiment, the hindered benzyl can be used to provide a visual color change in the adhesive composition in response to mixing a first component with a second component. The hindered benzyl can be present in an effective amount to act as a thermochromic indicator or a mix indicator in the adhesive composition in either the first component, the second component, or combinations thereof. The effective amount can be the amount that allows the adhesive composition to undergo a visual color change in response to debonding or curing. The effective amount can be based on a concentration of the hindered benzyl in the first component, second component, or the adhesive composition as a whole. In at least one embodiment, the hindered benzyl has a concentration no greater than 10 wt%, 8 wt%, 6 wt%, 5 wt%, 4 wt%, 3 wt%, or 2 wt% in the first component, the second component, or the adhesive composition. The hindered benzyl can also have a concentration of at least 0.5 wt%, or 1 wt % in the first component, the second component, or the adhesive composition (when first component and second component are combined). Thus, the range of concentrations of hindered benzyl can be from 0.5 wt% to 6 wt% (inclusive), 1 wt% to 5 wt% (inclusive), or 1 wt% to 4 wt% (inclusive).

[0057] The hindered benzyl can have the formula:t Bi .dyl ,x„..AX, wherein X is an oxo or a hydroxy group, R is a hydrogen, alkyl (e.g., a Cl to CIO alkyl), an alkylbenzyl, or an aminoalkyl.

[0058] For example, the hindered benzyl can have the formula:

[0059] The alkylbenzyl can be independently substituted with alkyl groups on an ortho position to a phenol group, the alkyl groups each have more than one carbon atom.

[0060] The alkylbenzyl can have the formula:R3R,xA ... K.2Ri, wherein Ri is an alkyl group or an alkoxy group having between 1 and 4 carbon atoms, Ri can optionally form a double bond with the benzyl group, and each Rj is, independently a Cl to CIO alkyl, and R3 is an oxygen or a hydroxy group. For example, Rj can be a tert-butyl group. Ri can be a methyl group or a methoxy group with the oxygen bonded to the R and the R is attached to the aryl ring. Some examples, like 4,4'-methylene bis(2,6-di-tert-butylphenol) (MTBP), are commercially available under the trade designation IONOL 220. The hindered benzyl can exclude non-antioxidants such as phenolphthalein.

[0061] In at least one embodiment, the hindered benzyl can be a galvinoxyl, free radical and have the formula:CH2■■■■ N(B)3

[0062] In at least one embodiment, the aminoalkyl can have the formulawherein each R is, independently, a hydrogen, or a Cl to CIO alkyl. Thus, the hindered benzyl can have the formula:OHt-Butyl, wherein each R is, independently, a hydrogen, or Cl to CIO alkyl. A specific example is 2,6-di-tert-butyl-N,N-dimethylamino-p-cresol, commercially available under the trade designation IONOL 103.

[0063] In at least one embodiment, the hindered benzyl can be a substituted bisphenol antioxidant and have the formula:, wherein each R is, independently, a Cl to CIO alkyl. In at least one embodiment, each R is (independently) a Cl to C4 alkyl. In one example, the alkyl group can be a tert-butyl group, isobutyl group, n-butyl group, sec-butyl, ethyl group, propyl group, methylethyl group, cyclopropyl group, or a methyl group.

[0064] In at least one embodiment, the hindered benzyl also be selected from among 2,2'-ethylidenebis[4,6-di-tert-butylphenol] , 2,2'-ethylidenebis [6-tert-butyl-4-isobutylphenol] , 2,2'-isobutylidenebis[4,6-dimethylphenol], 2,2'-methylenebis[4,6-di-tert-butylphenol], 2,2'-methylenebis[4-methyl-6-(a-methylcyclohexyl)phenol], 2,2'-methylenebis[6-cyclohexyl-4-methylphenol] , 2,2'-methylenebis[6-(a,a'-dimethylbenzyl)-4-nonylphenol], 2,2'-methylenebis[6-(a-methylbenzyl)-4-nonylphenol], 2,2'-methylenebis[4-methyl-6-nonylphenol], 2,2'-methylenebis[6-tert-butyl-4-ethylphenol], 2,2'-methylenebis[6-tert-butyl-4-methylphenol], 2,2'-thiobis[6-tert-butyl-4-methylphenol] , 4,4 '-butylidenebis [2-tert-butyl-5 -methylphenol] , 4,4'-methylenebis [2,6-di-tert-butylphenol], 4,4'-methylenebis[6-tert-butyl-2-methylphenol], 4,4'-thiobis[2-tert-butyl-5-methylphenol] and / or 4,4 '-isoprop ylidenediphenol.

[0065] Curable adhesive compositions according to the present disclosure comprise a toughening agent. Toughening agents may be useful, for example, for improving the properties (e.g., peel strength) of some cured epoxies, for example, so that they do not undergo brittle failure in a fracture. The toughening agent (e.g., an elastomeric resin or elastomeric filler) may or may not be covalently bonded to the curable epoxy and ultimately the crosslinked network. In some embodiments, the toughening agent includes an epoxy- terminated compound, which can be incorporated into the polymer backbone. Examples of useful toughening agents, which may also be referred to as elastomeric modifiers, include polymeric compounds having both a rubbery phase and a thermoplastic phase such as graft copolymers having a polymerized diene rubbery core and a polyacrylate or polymethacrylate shell; graft copolymers having a rubbery core with a polyacrylate or polymethacrylate shell; elastomeric particles polymerized in situ in the epoxide from free-radical polymerizable monomers and a copolymeric stabilizer; elastomer molecules such as polyurethanes and thermoplastic elastomers; separate elastomer precursor molecules; combination molecules that include epoxy-resin segments and elastomeric segments; and, mixtures of such separate and combination molecules. The combination molecules may be prepared by reacting epoxy resin materials with elastomeric segments; the reaction leaving reactive functional groups, such as unreacted epoxy groups, on the reaction product.

[0066] The use of tougheners in epoxy resins is described in the Advances in Chemistry Series No. 208 entitled "Rubbery -Modified Thermoset Resins", edited by C. K. Riew and J. K. Gillham, American Chemical Society, Washington, 1984. The amount of toughening agent to be used depends in part upon the final physical characteristics of the cured resin desired, and is generally determined empirically.

[0067] FIG. 1 illustrates a method 110 of using the adhesive composition to join two substrates. For example, the method 110 can begin with admixing the first component with the second component in block 102. The admixing can be performed through an adhesive dispenser for combining 2K adhesive systems.

[0068] When the first component is admixed with the second component, an adhesive composition with the hindered benzyl is formed. The adhesive composition can be applied to the first substrate or the second substrate in block 104, or both. In at least one embodiment, the first component and second component can also be applied to a substrate itself and mixed thereon. The substrate is formed of a heat-resistant material. The heat-resistant material is configured to not deform at temperatures between 200 and 250 degrees Celsius. For example, metals (steel, aluminum, and alloys thereof), ceramics, silicone, glass, or heat-resistant plastics (e.g., polytetrafluoroethylene). The substrate can have a planar or non-planar (e.g., curvy or jagged)surface. In at least one embodiment, the substrates are components of an automobile (e.g., a frame member, a body panel, body kit, etc.).

[0069] The adhesive composition can then contact the first substrate or the second substrate in block 106 (depending on which substrate the adhesive composition was applied to). For example, if the adhesive composition is first applied to the first substrate, then the adhesive composition can be brought to contact the second substrate such that the first substrate and second substrate are adhered together. In at least one embodiment, a technician can apply the adhesive composition using an edge fillet (e.g., with an exposed area and a bonding area, where the adhesive composition is bonded to one substrate and the other substrate at the bonding area but is not bonded to the other substrate at the exposed area). For example, FIG. 3 illustrates a system 300 that includes a first substrate 302 and second substrate 304 joined together using adhesive composition 306. As shown, an edge fillet 308 can be visible on the surface of the first substrate 302. Thus, the exposed area can be an area of visible adhesive composition so that the technician can visually confirm the visual color change.

[0070] In block 108, the adhesive composition can cure to form a cured adhesive composition. In at least one embodiment, the adhesive composition is capable of curing at no greater than 150 degrees Celsius, no greater than 100 degrees Celsius, or at room temperature. As a result of the cure, the cured adhesive composition can adhesively bond the first substrate to the second substrate. Additional mechanical fasteners can be used between the two substrates to further reinforce the adhesive bond. For example, FIG. 4A, FIG. 4B, and FIG. 4C illustrate the first substrate 402 and second substrate 404 joined using the adhesive composition 406 and a mechanical fastener. As shown, examples of the mechanical fastener can include bolt 408, rivet 410, and weld 412.

[0071] The curing process can produce a visual color change from the adhesive composition to the cured adhesive composition. The visual color change can be any suitable color change that is perceivable by a human eye under natural light (e.g., silver to purple, pink to purple, yellow to green, pale green to pink, dark burgundy to dark violet, etc.). The visual color change can refer to polychromic color changes and generally excludes monochromic color changes (e.g., grey to black). In at least one embodiment, multiple visual color changes can occur. For example, a first visual color change can be observed when the first component is admixed with the second component at a cure temperature. In at least one embodiment, the cure temperature may be at room temperature. In at least one embodiment, the visual color change can also be the result of mixing two different colored components. After the adhesive composition is formed, then a second visual color change can occur once cured.

[0072] FIG. 2A and FIG. 2B illustrate two bonded substrates. The second substrate 202 can be bonded with the first substrate 204 using both mechanical fasteners 206 and the cured adhesivecomposition 208. The cured adhesive composition 208 can have an area sufficient to bond a first substrate 204 with second substrate 202.

[0073] As shown in FIG. 2B, the cured adhesive composition 208 can have a bonding area 214 that is less than the total area of the cured adhesive composition 208. The cured adhesive composition 208 can have the bonding area 214 that bonds the first substrate 204 with the second substrate 202 and an exposed area 210 that only bonds with one of the substrates (e.g., the second substrate 202). When applied in method 110, the technician can deliberately create an exposed area 210 in order to view the visual color change related to the curing process, as well as related to the heating of the adhesive at the time of debonding.

[0074] The mechanical fasteners 206 can be removed from the second substrate 202 and / or first substrate 204.

[0075] Heat 212 can be applied to the cured adhesive composition 208 to debond the first substrate 204 and the second substrate 202 using a heat gun or other heating tool. The heat 212 can vary with the adhesive composition used, but generally the cured adhesive composition 208 can be heated to the debonding temperature of the cured adhesive composition. In at least one embodiment, the debonding temperature is where substrates can be easily separated with applied force (including gravity), but would not separate spontaneously. For example, the debonding temperature can be at least 80 degrees Celsius, at least 175 degrees Celsius, at least 180 degrees Celsius, at least 185 degrees Celsius, at least 190 degrees Celsius, at least 195 degrees Celsius, at least 200 degrees Celsius, at least 204 degrees Celsius, or at least 210 degrees Celsius.

[0076] In at least one embodiment, a technician or other user can use a heat gun to heat a panel to 250-425F to soften the adhesive bond making it easier to separate without damaging the host panel. Hand separation by the technician can allow for heating the area as the panels are being separated. Many aluminum substrates avoid heating beyond 425 F to prevent annealing of the aluminum.

[0077] In at least one embodiment, to dissemble metal panels previously bonded a flameless heat source can be used to heat the bonded flange, observing the OEM recommended maximum temperature limit of the metal to avoid damaging the host panel. In at least one embodiment, the adhesive can soften at 300° F / 150°C but will separate easier as the temperature approaches 400°F / 200°C. While the bond-line is at the desired temperature, the technician can carefully separate the panels with a panel separator, putty knife or chisel using the least aggressive method that is successful without causing damage to the panel.

[0078] The hindered benzyl can produce a visual color change to the debonding temperature (which further indicates debonding). For example, the color change can be from purple to silver, or vice versa. Once the cured adhesive composition 208 has debonded from at least one of the second substrate 202 or first substrate 204, and in response to the visual color change, the technician can remove the first substrate 204 and the second substrate 202 from each other. By using the hinderedbenzyl as a debonding indicator as described, the technician no longer has to guess when two substrates are safe to remove from each other.

[0079] FIG. 5 illustrates a system 500 for dispensing the adhesive composition. The system 500 can include an applicator 512 configured to dispense a 2K adhesive composition. The applicator 512 can be configured to couple to a container 514. The container 514 can couple to the applicator tip 506. The container 514 can include a first chamber 502 and second chamber 504. For example, the first chamber 502 can be configured to contain the first component 508 and the second chamber 504 can be configured to contain the second component 510. The first component 508 and second component 510 are fluidically isolated from each other. When dispensed, the first component 508 and second component 510 are pushed through the applicator tip 506. The applicator tip 506 can ensure the mixing of first component 508 and second component 510 before application on a substrate. Examples of applicators 512 and containers 514 are commercially available from 3M (Saint Paul, MN).

[0080] "Alkyl group" or the prefix “alk-” refers to both straight chain and branched chain groups and of cyclic groups. The alkyl group can refer to a linear or branched alkyl having the number of carbon atoms specifically indicated, e.g. C1-C10. Examples of alkyl groups include methyl, ethyl, n-propyl-, isopropyl, n-butyl, tert-butyl, pentyl, isopentyl, hexyl, 2-methylbutyl, 1 -methylbutyl, 1-ethylpropyl, 1 ,2-dimethylpropyl, neo-pentyl, 1,1 -dimethylpropyl, 4-methylpentyl, 3 -methylpentyl, 2-methylpentyl, 1 -methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3 -dimethylbutyl, 2,2-dimethylbutyl, 1,1 -dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl, or 1,2-dimethylbutyl groups.

[0081] "Aryl" refers to carbocyclic aromatic rings or ring systems, for example, having 1, 2, or 3 rings and optionally containing at least one heteroatom (e.g., O, S, or N) in the ring optionally substituted by up to five substituents including one or more alkyl groups having up to 4 carbon atoms (e.g., methyl or ethyl), alkoxy having up to 4 carbon atoms, halo (i.e., fluoro, chloro, bromo or iodo), hydroxy, or nitro groups. Examples of aryl groups include phenyl, naphthyl, biphenyl, fluorenyl as well as furyl, thienyl, pyridyl, quinolinyl, isoquinolinyl, indolyl, isoindolyl, triazolyl, pyrrolyl, tetrazolyl, imidazolyl, pyrazolyl, oxazolyl, and thiazolyl.

[0082] "Cure" refers to joining polymer chains together by covalent chemical bonds, usually via crosslinking molecules or groups, to form a network polymer. Therefore, in this disclosure the terms "cured" and "crosslinked" may be used interchangeably. A cured or crosslinked polymer is generally characterized by insolubility, but may be swellable in the presence of an appropriate solvent.

[0083] "Debonding" or “debonded” refers to freeing two materials from each other with a human-applied force. A human-applied force can be less than 400 Newtons.

[0084] "Mechanical fastener" refers to a device that is used to mechanically join two or more objects together which include may include non-permanent fasteners. Examples of mechanicalfasteners include screws, bolts and nuts, locking tabs, hooks, pins, rivets, and latches. Other examples of mechanical fasteners can include welds.

[0085] "Polymer" refers to polymers, copolymers (e.g., polymers formed using two or more different monomers), oligomers or monomers that can form polymers, and combinations thereof, as well as polymers, oligomers, monomers, or copolymers that can be blended.

[0086] "Room temperature" refers to a temperature range suitable for human occupancy from 15 to 25 degrees Celsius, inclusive.

[0087] "Substituted bisphenol antioxidant" refers to a bisphenol molecule having one or more substituted groups. The substituted groups can be on the ortho, or meta positions.

[0088] "Visual color change" refers to a color change that occurs at a visible light spectrum (i.e., wavelengths from 380 to 700 nanometers). The color change can be related to the minimum perceptible color difference to a human. In an example, the color change can have a Delta E (CIEDE2000) of at least 2, or at least 4.EXAMPLES

[0089] Objects and advantages of this disclosure are further illustrated by the following nonlimiting examples. Particular materials and amounts thereof recited in these examples, however, as well as other conditions and details, should not be construed to unduly limit this disclosure. Weight percent (wt%) quantities are based on the total weight of the composition.

[0090] Materials:Trade Description Supplier Designation / AbbreviationExemplary AntioxidantsTrade Description Supplier Designation / AbbreviationMTBP 4,4'-methylenebis(2,6-di-tert-butylphenol) Sigma-Aldrich,St. Louis, MO, USADtBP 2,6-di-tert-butylphenol Alfa Aesar,Haverhill, MA EBtBP 2,2'-ethylidene-bis(4,6-di-tert-butylphenol) Pflatz & Bauer,Waterbury, CT GFR Galvinoxyl free radical TCI America,Portland, OR DtBDC 2,6-di-tert-butyl-N,N-dimethylamino-p-cresol TCI America,Portland, ORIRGANOX 2,2-Bis({ [3-(3,5-di-tert-butyl-4- BASF, Germany 1010 hydroxyphenyl)propanoyl] oxy } methyl)propane- 1,3- diyl bis[3-(3,5-di-tert-butyl-4- hydroxyphenyl)propanoate]MDMP 4,4'-Methylenebis(2,6-dimethylphenol) Sigma- Aldrich,St. Louis, MO, USAComparative AntioxidantsTrade Description Supplier Designation / Abbreviation4-nitrophenol Alfa Aesar, Haverhill, MA Other ComponentsTrade Description Supplier Designation / Abbreviation7333A Part A component of 3M Impact Resistant 3M Company, St.Structural Adhesive, P / N 07333 Paul, MN 7333B Part B component of 3M Impact Resistant 3M Company, St.Structural Adhesive, P / N 07333 Paul, MN Trade Description Supplier Designation / Abbreviation167-Al 1 95:5 (w:w) mixture of 7333A and DtBDC 3M Company, St.Paul, MN;Sigma-Aldrich, St. Louis, MO, USA167 -B 11 98:2 (w:w) mixture of 7333B and MTBP 3M Company, St.Paul, MN;Sigma-Aldrich, St. Louis, MO, USA TTD 4,7,10-trioxa 1,13 -tridecane diamine Tokyo Chemical Industry Co. Ltd; Tokyo, Japan EPON 828 Difunctional bisphenol A / epichlorohydrin derived Hexion,liquid epoxy resin Columbus, OH KANE ACE 40% core shell rubber in unmodified, liquid epoxy Kaneka Texas MX-154 resin based on bisphenol-A Corporation, Pasadena, Tex. EH-30 Amine curing agent Gabriel Performance Products, Akron, OH GABEPRO Mercaptan-terminated polymer Gabriel GPM-800 Performance Products, Akron,OHTS-720 Fumed silica which has a surface modification of Cabot poly dimethylsiloxane Corporation,Billerica, MA BALLOTINI Amorphous microspherical glass beads with 250- Potters Industries BEADS micron diameter LLC, Valley Forge, PATEDA Triethyl diamine Alfa Aesar,Haverhill, MA MX-257 37% concentration of 200 nm core shell rubber Kaneka North particles dispersed in thermosetting resins for America LLC, toughening Pasadena, TX HELOXY 107 Diglycidyl ether of cyclohexane dimethanol; used Hexion,as a diluent or viscosity modifier Columbus, OH Trade Description Supplier Designation / AbbreviationZ-6040 Glycidoxypropyltrimethoxysilane as an epoxy Dow Corning,functional coupling agent to improve adhesion Midland, MI

[0091] Antioxidant Preparations:

[0092] MTBPNa: A solution of MTBP in xylene was prepared by dissolving 10 grams of MTBP in 20 grams of xylene. A solution of NaOH in methanol was prepared by dissolving 21.7 grams NaOH pellets in 79.9 grams of methanol. 10 grams of the MTBP / xylene solution was mixed with 2.94 grams of the NaOH / methanol solution. Additional IPA was added until the solution became homogenous. The material was placed in a 65°C oven overnight. Anhydrous sodium sulfate was added to the solution and then several grams of liquid were decanted into an aluminum weight boat and the liquid was evaporated under dry nitrogen. The resulting solid, MTPBNa was reddish yellow.

[0093] DtBPNa: A solution of DtBP and sodium hydroxide in IPA xylene was prepared mixing 6.0 grams of DtBP with 1.18 grams of NaOH pellets and diluted with IPA until all solids dissolved. The material was placed in a 65°C oven overnight. Several grams of liquid were decanted and the liquid was evaporated under dry nitrogen. The resulting solid, DtPBNa, was orange.

[0094] Curative Preparations:

[0095] The curative component adduct was prepared as described in U.S. Patent No. 10683441, “ADDUCT”, the disclosure of which is incorporated herein by reference in its entirety.

[0096] Curative Preparations 1-6: Curative Preparations 1-6 were prepared by combining the ingredients listed in Table 1, below.

[0097] Table 1. Curative Preparations 1-6TTD EH GPM- DtBP Na Curative Adduct TS- Beads TEDA MTBPNa720 AminePreparation - 30 800 (g) (g) (g) (g) (g)(g) (g) (g) (g)CurativePreparation 132.50 12.20 44.00 5.00 6.60 0 0 0 0 1CurativePreparation 132.50 12.20 44.00 5.00 0 0 0 0 0 2Curative0 Preparation 4.54 0.52 13.68 1.26 0 0.20 0 03Curative0 Preparation 0 0 0 0 0 0 50 04Curative0 Preparation 0 0 0 0 0.10 0 5.00 05Curative0 Preparation 0.67 2.42 0.4 7.29 0.28 0.36 0 06Amine0.2 Preparation 6.62 0.61 2.20 .025 .33 0 0 07

[0098] Epoxy Preparations:

[0099] Epoxy Preparations 1-3 were prepared by combining the ingredients listed on Table 2, below.

[0100] Table 2. Epoxy Preparations 1-3EPON HELOEpoxy MX- DtBPN MTBP MTBP TS-720 Z-6040 XY 107 828 Preparation 257 (g) Na (g) a (g) (g) (g) (g) (g) (g)Epoxy180 0 9.00 4.50 3.00 0 0 0 Preparation 1Epoxy5.86 0 0.29 0.15 0.10 0 0.06 0 Preparation 2Epoxy9.16 0 0.46 0.23 0.15 0 0 0.1 Preparation 3

[0101] Examples 1-4 and Comparative Example A

[0102] Examples 1 - 4 and Comparative Example A were prepared as described below.

[0103] An antioxidant was added to one of a first component comprising EPON 828 or to a second component comprising a curative such as an amine. The curative component was prepared as described in U.S. Patent No. 10683441, “ADDUCT”, the disclosure of which is incorporated herein by reference in its entirety.

[0104] The first and second components were then mixed until a homogeneous mixture was obtained. The weight ratio of the epoxy component / curative component was 3:2. Color at mixing was noted.

[0105] The mixture was cured at 80°C or 110°C with 2% EH-30 for 30 minutes. The catalyst was added to the ADDUCT and EPON 828 for mixing color. Color after curing was noted.

[0106] To simulate a debonding operation, the cured composition was heated to 400°F (204°C) using a heat gun or oven and color of the heated composition noted. The composition was then allowed to cool to room temperature and color after cooling was noted.

[0107] Colors noted at different stages in the process are summarized in Table 3, below.

[0108] Table 3. Composition of Examples 1-4 and Comparative Example AAntioxidant Color at Color after Color of(component / mixing cure (curing Color after Examples heatedamount temperature cooling composition(wt%)) (°C))PinkMTBP Dark bright Colorless / Example 1 Reddish purple (epoxy / 1.5) purple (80) off-whiteDtBP (epoxyExample 2 Yellow Green (80) Yellow Green / 1.5)GVR (epoxy Dark Dark violet LightExample 3 / 1.5) burgundy Purple(80) yellowPale green Colorless / PinkExample 4 DtBDCPink (110)(amine / 1.5) off whiteMDMP Clear, Colorless / Example 4-1(epoxy / 1.5) colorless Pink Pinkoff whiteComparative 4-nitrophenol Yellow No change No change Example A Yellow (80)(epoxy / 3) (yellow) (yellow)

[0109] Examples 5-13

[0110] Examples 5 -13 were prepared by mixing epoxy and curative components prepared as described above, as shown in Table 4, below. Color of the homogenized mixture was noted.

[0111] Examples 5-7 contained MTBP, MTBPNa and DtBPNa. Examples 8-9 contained two types of tertiary amines in their curative preparations. Examples 10-13 were thiol-cured two-component adhesives including MTBPNa as catalyst / accelerator.pyp Eox Pre.

[0112] Table 4. Compositions of Examples 5-13g() 3 pyp Eox Pre.g() 2pyp Eox Pre.Example 0 0 0 0 0 1 g() 1 1.28 0 0 5 CurativeExample 0 0 0 0 0 0 pg () Pre.7 1 1.28 0 0 5-1Example 0 1 0 0 0 0 Curative 0 1.28 0 6pg () 6 Pre.Example 1 0 0 0 0 0 0 0 1.28 7Example 0 0 0.5 0 0 Curative 0 0 0 0.64 8 pg () 5 Pre.Example 0 0 0.5 0 0 0 0 0.64 0 9 CurativeExample 0 0 0 pg () Pre.4 0.5 0 0 0 0 0.55 10Example 0 0 0 Curative 0.5 0 0 0 0.55 0 11 pg () 3 Pre.Example 0 0 0 0 0.5 0 0 0 0.55 12Example 0 0 Curative 0 0 0.5 0 0 0.55 0 pg () Pre.213Curative

[0113] The mpg () Pre.1ixtures were then cured at room temperature (about 23°C) for 24 hours. Color of the cured samples was noted. The cured samples were subsequently heated to 300-400°F, at which p Examlepoint, color of the heated sample was noted. The samples were allowed to cool to room temperature and color upon cooling was noted. This heating / cooling cycle was repeated to determine if color changes were still observed — see Table 5, below.

[0114] Table 5. Color of Examples 5-13Color when Color Color when Color after heated Color on changes in Example mixed curing (temperature) cooling cycle 2Off-whiteExample 5 Light pink Dark pink Pink / purple yes (350°F)Example 5-1 GreenBrown yellow yeG Yellow green s yellow reen (230°F)ColorlessExample 6 Fuchsia Fuchsia Fuchsia yes (300°F)ColorlessExample 7 White White Reddish pink yes(400°F)ColorlessExample 8 Light pink Purple Pink / purple yes (350°F)ColorlessExample 9 Fuchsia Purple Pink / purple yes (350°F)ColorlessExample 10 White Light pink Light pink yes (176°F)Off-whiteExample 11 Light orange Wine red Brick red yes (300°F)Off-whiteExample 12 White Purple Wine red yes (400°F)Off-whiteExample 13 Light orange Wine red Brick red yes(400°F)

[0115] Comparative Example B and C and Examples 14-15:

[0116] A commercially available two-component structural adhesive obtained under the trade designation “3M IMPACT RESISTANT STRUCTURAL ADHESIVE (IRSA)” from 3M Company (Minnesota, USA) is hereinafter referred to as Comparative Example B. The adhesive comprised a light-yellow epoxy component and a silver color curative component in a, respectively, 2: 1 volume ratio. When mixed, the adhesive had a silver color which changed to purple after being heat-cured (65°C for 15-20 minutes).

[0117] The commercially available two-component adhesive of Comparative Example B was obtained and modified as follows: to the epoxy component, 2 wt% of an antioxidant was added. The epoxy component was blended until a homogeneous mixture was obtained.

[0118] The epoxy component was then mixed with the curative component as described for Comparative Example B. Colors of the mixture, after cure (65°C for 15-20 minutes), upon heating to 400°F (204°C) and after cooling were noted.

[0119] Table 6. Comparative Example B and C and Examples 14-15Example Antioxidant Color 65°C cure, Color at Color on Mixture 15 or 20 min 204°C cooling back to RTComparative Example B None Silver Purple Silver SilverExample 14 MTBP Silver Purple Silver Purple Example 15 DtBDC Silver Purple Silver Purple Comparative Example C IRGANOX 1010 Silver Silver Silver Silver

[0120] Comparative Example D and Examples 17-18:

[0121] A commercially available one-component structural adhesive obtained under the trade designation “3M™ Scotch-Weld™ One-Part Epoxy Adhesive 6101” from 3M Company (Minnesota, USA) is hereinafter referred to as Comparative Example D.

[0122] The commercially available one-component adhesive of Comparative Example D was obtained and modified as follows: an antioxidant was mixed with the adhesive prior to curing.

[0123] Colors of the mixture, after cure (65°C for 15-20 minutes), upon heating to 400°F (204°C) and after cooling were noted. See Table 7, below.

[0124] Table 7. Comparative Example D and Examples 17-18Antioxidant Color 65°C cure, 15 Color at Color on Mixture or 20 min cooling Example 204°Cback to RTComparative Example D - White White White White Example 17 MTBP White Pink White White Purple / redWhite White WhiteExample 18 DtBDC specks

[0125] In Table 8 below, debonding data is provided, along with insight from observed thermal temperature transitions. The antioxidant is present in 167-Al 1 (2,6-di-tert-butyl-a-dimethylamino-p-cresol added to 7333A) and 167-B11 (4,4'-methylenebis-2,6-di-tert-butylphenol added to 7333B). This demonstrates the ability to add to either Part A or B as well as the mix ratio being tolerant to being off ratio, as shown in Examples 19-21.

[0126] The initial strength of the adhesives after curing at 60°C for 30 minutes on standard G70 hot-dipped galvanized steel substrate (2.54 cm x 10 cm x 0.08 cm laps from ACT with a 10 mm bond overlap and nominal bond line thickness of 250 microns) was in the range of about 20 to 22 MPa, typical for a structural adhesive on a thin metal substrate. Heating the overlap shear samples to 190°C for 3 minutes caused the purple color to fade.

[0127] Table 8. Examples 19-23Lap ShearStrength Colorafter afterInitial heating to heatingColor Lap 190°C (3 to Initial T- after Shear Lap Shear min.) and 190°C Peel T-Peel Vol. curing strength Strength cooling, (3 min.) strength Strength ratio Part Part B 60°C for @ 23°C @ 190°C @ 23°C and @ 23°C @ 190°C Example (A:B) Part A A (g) Part B (g) 30 min. (MPa) (MPa) (MPa) cooling (N / m) (N / m) Example 19 1.0:1.8 167-Al 1 2.2 7333B 3.8 Purple 21.9 0.10 NT Purple NT NT Example 20 1.0:2.0 167-Al 1 2.2 7333B 4.2 Purple 20.8 0.11 NT Purple NT NT Example 21 1.0:2.2 167-Al 1 2.2 7333B 4.6 Purple 20.9 0.09 NT Purple 9230 478 Example 22 1.0:2.0 7333A 2.2 167 -B 11 4.2 Purple 20.1 0.07 18.4 Purple NT NT Comparative1.0:2.0 7333A 2.2 7333B 4.2 Purple 19.8 0.10 17.7 Grey NT NTExample ENT = not tested

[0128] When the adhesives were heated to 190°C in an environmental chamber enclosing the tensile tester, color change occurred as the temperature of the chamber approached 190°C, at which point the sample was tested. Observed lap shear strength was less than 1% of the original lap shear strength.

[0129] When the above conditions were repeated and these samples were allowed to cool, the purple color returned for Example 22 containing the antioxidant 4,4'-methylenebis(2,6-di-tert-butylphenol), but remained grey in color for Comparative Example E, which did not contain the antioxidant. Thus, while tests on the cooled specimens showed little change in strength, the adhesive performance of the latter specimen (Comparative Example E) could no longer be visually verified as a function of temperature.

[0130] Similarly, a T-peel test was run for initial peel strength at 23°C and at 190°C showing a drop in average peel force from 9230 N / m to 478 N / m, or approximately 5% of the original peel force needed to debond, once the color of the adhesive changed near 190°C.

[0131] All cited references, patents, and patent applications in the above application for letters patent, are herein incorporated by reference in their entirety in a consistent manner. In the event of inconsistencies or contradictions between portions of the incorporated references and this application, the information in the preceding description shall control. The preceding description, given in order to enable one of ordinary skill in the art to practice the claimed disclosure, is not to be construed as limiting the scope of the disclosure, which is defined by the claims and all equivalents thereto.

Claims

CLAIMS:What is claimed is:

1. An adhesive composition, comprising:a hindered benzyl having the formula:x.....A'yA, wherein X is an oxo or a hydroxy group;wherein R is a hydrogen, alkyl, an alkylbenzyl, or an aminoalkyl, wherein the alkyl, the alkylbenzyl or aminoalkyl optionally includes an oxygen linkage to the hindered benzyl;wherein the hindered benzyl is present in an effective amount that indicates a degree of cure or debonding by providing a visual color change as the degree of cure or debonding occurs.

2. The adhesive composition of claim 1, wherein the alkylbenzyl is independently substituted with alkyl groups on an ortho position to a phenol group, the alkyl groups having more than one carbon atom.

3. The adhesive composition of claim 1 or 2, wherein the alkylbenzyl has the formula:, wherein Ri is an alkyl group or an alkoxy group having between 1 and 4 carbon atoms, and each Rj is, independently a Cl to CIO alkyl, and R3 is an oxygen or a hydroxy group.

4. The adhesive composition of claim 3, wherein Ri is a methyl group.

5. The adhesive composition of claim 3 or 4, wherein Rj is a tert-butyl group or a methyl group.

6. The adhesive composition of any one of claims 1-5, wherein the hindered benzyl is 4,4'-methylenebis(2,6-di-t-butylphenol) (MTBP).

7. The adhesive composition of any one of claims 1-5, wherein the hindered benzyl is a galvinoxyl free radical.

8. The adhesive composition of claim 1, wherein the hindered benzyl has the formula:

9. The adhesive composition of claim 1, wherein the aminoalkyl has the formula:.CB> - N(R)2, wherein each R is, independently, a hydrogen, or a Cl to CIO alkyl.

10. The adhesive composition of claim 1, wherein the hindered benzyl has the formula:OHt-Butyl t-ButylR, wherein each R is, independently, a Cl to CIO alkyl.

11. The adhesive composition of any one of claims 1-10, wherein the hindered benzyl has a concentration no greater than 5 wt.% in the first component or the second component.

12. The adhesive composition of any one of claims 1-11, wherein the hindered benzyl excludes phenolphthalein.

13. The adhesive composition of any one of claims 1-12, further comprising:a first component; anda second component that chemically reacts with the first component;wherein the hindered benzyl is present in the first component, the second component, or combinations thereof.

14. The adhesive composition of claim 13, wherein at least one of the first component or the second component comprises an amine or thiol curing agent, at least one of the first component or the second component comprises a curable epoxy resin, and at least one of the first component or the second component comprises a toughening agent.

15. A system, comprising:a first substrate;a second substrate; andthe adhesive composition of any one of claims 1-14, wherein the adhesive composition forms an edge fillet that is visible with respect to the first substrate or the second substrate.

16. A method for forming a bond between two substrates comprising:applying the adhesive composition of claim 13 or 14 to a first substrate and / or a second substrate by admixing the first component with the second component;contacting the first substrate or the second substrate to the adhesive composition such that the adhesive composition is disposed between the first substrate and the second substrate; andcuring, using a curing process, the adhesive composition to form a cured adhesive composition, wherein the adhesive composition is a first color, and the cured adhesive composition is a second color.

17. The method of claim 16, wherein contacting the first substrate or the second substrate to the adhesive composition includes leaving an exposed area of the adhesive composition to observe a visual color change of the cured adhesive composition.

18. The method of claim 16 or 17, further comprising:heating the cured adhesive composition to a debonding temperature; and allowing the cured adhesive composition to perform a visual color change from the second color to the first color,wherein the visual color change indicates that at a temperature that the cured adhesive composition can be separated from the first or second substrate or split during debonding and is associated with the debonding temperature.

19. The method of claim 18, further comprising removing the first substrate from the second substrate at the temperature responsive to the visual color change.