Cylinder liner and preparation method thereof

By designing recessed portions and convex rib structures on the outer surface of the cylinder liner, and using paint spraying technology during the casting process, the problem of poor bonding tightness between the cylinder liner and the aluminum alloy has been solved, the bonding rate and metallographic quality have been improved, and it is suitable for many applications. casting conditions.

CN111659867BActive Publication Date: 2024-10-01ZYNP CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910176596.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-03-08
Publication Date
2024-10-01
Estimated Expiration
2039-03-08

AI Technical Summary

Technical Problem

The existing cylinder liner has poor bonding tightness with the aluminum alloy, resulting in dissatisfaction with the aluminum alloy liquid filling and low bonding rate.

Method used

Design a cylinder liner with recessed parts and convex ribs dividing adjacent recessed parts distributed on its outer circumferential surface. The convex ribs enclose the recessed parts. The mesh diameter is 0.5-4.0mm and the mesh depth is 0.1-0.6mm. , and form a coating layer by spraying paint on the inner wall of the mold at least twice, optimizing the casting process to increase the bonding rate.

Benefits of technology

The combination rate of cylinder liner and aluminum alloy liquid has been achieved to reach more than 90%, reducing the cylinder liner wall thickness, improving the metallographic quality and oil storage and lubrication performance of the outer wall, and adapting to a variety of casting conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111659867B_ABST
    Figure CN111659867B_ABST
Patent Text Reader

Abstract

The invention discloses a cylinder sleeve and a preparation method thereof. The outer circular surface of the cylinder sleeve is randomly distributed with recessed parts and convex edges that divide adjacent recessed parts, and the convex edges enclose the recessed parts, and the mesh diameter of the recessed parts is controlled to be 0.5-4.0mm, and the mesh depth is 0.1-0.6mm. The mesh structure of the specific mesh diameter and mesh depth distributed on the outer circular surface does not have gaps. During the pouring process of aluminum alloy liquid, the aluminum alloy liquid is easy to fill the mold and fill its surface. After testing, the combination rate of the cylinder sleeve of the present invention and the aluminum alloy liquid reaches more than 90%, while the combination rate of the outer circular burr-shaped cylinder sleeve and the aluminum alloy liquid is less than 50%. The preparation method adopts at least two coating sprayings to ensure that the coating layer is completely isolated from the inner wall of the mold. During the subsequent iron liquid pouring process, the iron liquid will not contact the inner wall of the mold, thereby reducing the supercooling of the iron liquid and improving the metallographic phase of the outer wall of the casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of cylinder liner manufacturing, and particularly relates to a cylinder liner and a preparation method thereof. Background Art

[0002] The cylinder liner is a cylindrical part, placed in the cylinder barrel of the engine cylinder block, and fixed by the cylinder head. The cylinder liner, piston and cylinder head together form a combustion chamber, and the piston reciprocates in the inner hole of the cylinder liner. At present, the car engine generally uses aluminum alloy embedded gray cast iron cylinder liners. The cylinder liners used are of the threaded type with outer circle processing, and the other is the burr-shaped outer circle of the cast state.

[0003] The surface of the external cylindrical threaded cylinder liner is too smooth and the bonding with the aluminum alloy is not tight; while the external cylindrical burred cylinder liner has too high requirements for the press, because the pressure is too low and the root of the burr is not easy to fill the mold, which results in poor bonding between the aluminum alloy and the cylinder liner. Summary of the invention

[0004] To this end, the present invention aims to solve the defect that the existing cylinder liner and the aluminum alloy have poor tightness, and further provides a cylinder liner with good tightness to the aluminum alloy and a preparation method thereof.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0006] A cylinder liner has an outer circumferential surface on which recessed portions and convex edges that divide adjacent recessed portions are randomly distributed, the recessed portions are enclosed by the convex edges, the mesh diameter of the recessed portions is 0.5-4.0 mm, and the mesh depth is 0.1-0.6 mm.

[0007] In the present invention, the method for measuring the mesh diameter is to use computer-aided design software, such as solidworks drawing software or UG drawing software, to measure the mesh diameter using Solidworks drawing software or UG drawing software, to trace the inner edge of the recessed portion (i.e., the edge of the mesh), to connect the inner edges end to end to form a closed figure, and to calculate the area of ​​the closed figure using Solidworks drawing software or UG drawing software, and to convert the area of ​​the closed figure into a circle of equal area, thereby obtaining the diameter of the circle, i.e., the mesh diameter.

[0008] In the present invention, the method for measuring the mesh depth is: clamp the cylinder sleeve and turn the outer circle on a lathe, and half of the difference between the diameter of the outer circle before turning and the diameter of the outer circle after the raised edge is turned off is the mesh depth. The surface of the outer circle of the cylinder sleeve after turning off is the base bottom surface of the recessed part. A more accurate measurement method is: take the line connecting the lowest points of the recessed parts on the left and right sides of the detected raised edge as the reference plane, and measure the distance between the reference plane and the top plane of the raised edge as the height of the raised edge, that is, the mesh depth.

[0009] In the present invention, the definition of a raised ridge is: taking the basic bottom surface of the recessed portion to be enclosed as a reference, any continuous protrusions that are higher than the basic bottom surface of the recessed portion are considered as raised ridges; more preferably, any continuous protrusions with a height of not less than 0.1 mm relative to the basic bottom surface of the recessed portion are considered as raised ridges.

[0010] Furthermore, the outer circumferential surface of the cylinder liner has closed meshes accounting for at least 10% of the total number of meshes, and the remaining meshes are discontinuous meshes.

[0011] In the present invention, a closed mesh refers to a recessed portion surrounded by raised edges, with no gaps in the mesh; a discontinuous mesh refers to a recessed portion surrounded by raised edges, with gaps in the mesh, and no raised edges at the gaps.

[0012] Furthermore, the number of meshes with a mesh diameter of 0.5-2 mm accounts for no less than 50% of the total number of meshes in the field of view; or,

[0013] The number of meshes with a mesh diameter of 2-4 mm accounts for no less than 50% of the total number of meshes in the field of view.

[0014] In the present invention, the field of view refers to the field of view displayed by the ultra-depth-of-field microscope after randomly selecting a number of observation points on the outer circumferential surface of the cylinder liner using an ultra-depth-of-field microscope and magnifying the outer circumferential surface of the cylinder liner by a certain multiple. Specifically, the magnification can be 20 times and the number of observation points can be 5.

[0015] Preferably, the mesh depth is 0.2-0.4 mm.

[0016] The outer circular surface of the cylinder sleeve has closed meshes accounting for 20-50% of the total mesh number, and the remaining meshes are discontinuous meshes.

[0017] Preferably, the recessed portions and raised edges are distributed throughout the outer circumferential surface of the cylinder liner.

[0018] In addition, the present invention also provides a method for preparing the above-mentioned cylinder liner, which includes spraying paint on the inner wall of the mold at least twice and forming a paint layer on the inner wall of the mold before pouring molten iron into the inner cavity of the mold.

[0019] Furthermore, when the coating is sprayed, the temperature of the mold is 250-450°C, for example, 250-380°C, 390°C-450°C, and the coating spraying pressure is 0.2-0.4Mpa;

[0020] The rotation speed of the paint spraying is 400-1000 rpm, for example, 500-1000 rpm, 400-480 rpm.

[0021] Furthermore, the paint spraying is carried out using a nozzle with a diameter of 1.5-2.5 mm as a nozzle;

[0022] The spraying direction of the coating spraying has an axial angle of 25-60° with respect to the mold. In addition, the opening angle of the coating spraying is twice the angle, which is 50-120°.

[0023] The spraying speed is 30-50 mm / s. The spraying speed here refers to the speed at which the nozzle moves along the axial direction of the mold in its inner cavity.

[0024] Furthermore, the paint spraying consists of a first paint spraying and a second paint spraying, and the spraying interval time between the first paint spraying and the second paint spraying is 3-10s.

[0025] Preferably, the parameter values ​​of the first paint spraying and the second paint spraying are the same.

[0026] Further, the pouring temperature of the pouring is 1400-1600°C, for example, 1400-1500°C, 1550-1600°C;

[0027] During the pouring process, centrifugal casting is performed, and the rotation speed of the mold is 1400-1700 rpm, for example, 1400-1600 rpm, 1620-1700 rpm.

[0028] Furthermore, the coating used for coating spraying comprises the following raw materials in parts by weight: 70-73 parts of water, 20-22 parts of diatomaceous earth and 5-10 parts of bentonite.

[0029] Furthermore, the specific gravity of the coating is 1.1-1.2 g / cm 3 , viscosity is 50-70s.

[0030] Furthermore, before using the coating, the method further comprises adding a foaming agent accounting for 0.9-1.5% of the total weight of the coating into the coating.

[0031] Furthermore, before pouring the molten iron into the inner cavity of the mold, the method further includes adding 0.4-0.8% of the total weight of an inoculant to the molten iron, and inoculating the molten iron at 1380-1500°C.

[0032] Further, the molten iron is composed of the following raw materials: 3.0-3.5wt% carbon, 2.0-2.7wt% silicon, 0.5-1.0wt% manganese, 0.1-0.4wt% chromium, 0.2-1.5wt% copper, <0.1wt% sulfur, ≤0.4wt% phosphorus, and the balance is iron;

[0033] The inoculant is silicon strontium zirconium.

[0034] Furthermore, the air permeable plugs are evenly distributed on the side wall of the mold, and the roughness of the inner wall of the mold is less than 3.2 μm;

[0035] The method also includes cooling the mold after pouring molten iron to 700-800°C, taking the casting out of the mold, air cooling it to obtain a blank, and shot blasting the blank.

[0036] Furthermore, the shot blasting diameter of the shot blasting treatment is 0.2-0.4 mm, preferably 0.3 mm.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The cylinder liner provided by the present invention has concave parts and convex edges that divide adjacent concave parts randomly distributed on the outer surface of the cylinder liner, and the convex edges enclose the concave parts. At the same time, the mesh diameter of the concave parts is controlled to be 0.5-4.0mm, and the mesh depth is 0.1-0.6mm, which overcomes the defect that the existing outer burr cylinder liner has gaps between the mushroom-shaped or conical burrs on the surface, which hinders the flow of aluminum alloy liquid during the gravity aluminum alloy casting process, causing the aluminum alloy liquid to not fill the mold completely. On the other hand, the cylinder liner of the present invention has a mesh structure with a specific mesh diameter and mesh depth distributed on its outer surface, and there are no gaps. During the pouring process of aluminum alloy liquid, the aluminum alloy liquid can easily fill its surface. According to tests, the combination rate of the cylinder liner of the present invention and the aluminum alloy liquid reaches more than 90%, while the combination rate of the outer burr cylinder liner and the aluminum alloy liquid is less than 50%.

[0039] (2) The cylinder liner provided by the present invention helps to improve the bonding rate between the cylinder liner and the aluminum alloy liquid by optimizing the closed meshes on the outer circumferential surface of the cylinder liner to account for no less than 50% of the total number of meshes, the number of meshes with a mesh diameter of 0.5-2 mm to account for the total number of meshes in the field of view, or the number of meshes with a mesh diameter of 2-4 mm to account for no less than 50% of the total number of meshes in the field of view.

[0040] (3) The cylinder liner provided by the present invention has a low mesh depth, so that the height of the raised edge is low relative to the burrs on the surface of the existing outer cylindrical burr-shaped cylinder liner, and the outer wall metallography is good. Under the same conditions, the cylinder liner of the present invention can achieve A-type graphite accounting for more than 70% and a length of 5-6 levels at 1mm from the outer wall, while the outer cylindrical burr-shaped cylinder liner is basically D+E type graphite at 1mm from the outer wall, with a length of more than 7 levels. To achieve the metallographic state of the cylinder liner of the present invention, the wall thickness must be increased, and the requirement can only be barely met at 2mm from the outer wall, and it is very unstable. Therefore, under the same metallographic conditions, the cylinder liner of the present invention has a thinner wall thickness, and under the same conditions, the effective wall thickness of the cylinder liner can be reduced, and the same oil storage and lubrication performance can be achieved after honing in the later stage, thereby reducing the weight of the engine and improving fuel consumption.

[0041] (4) The cylinder liner provided by the present invention has a convex edge on its outer cylindrical surface that forms a convexity similar to a reinforcing rib. When the wall thickness of the cylinder liner is reduced, its strength can remain unchanged, fully ensuring the rigidity of the entire cylinder liner and reducing its deformation, thereby reducing the fuel consumption of the engine. At the same time, the concave portion on its outer surface has a better filling capacity and is more adaptable to a wider range of die-casting plants, from gravity casting, low-pressure casting to high-pressure casting, while the existing outer cylindrical burr-shaped cylinder liner (such as a mushroom-shaped cylinder liner) can only be adapted to high-pressure casting.

[0042] (5) The preparation method of the cylinder liner provided by the present invention is to spray the inner wall of the mold with paint at least twice before pouring molten iron into the inner cavity of the mold, and form a coating layer on the inner wall of the mold. Through the above process, it can be ensured that the coating layer completely isolates the inner wall of the mold. In the subsequent molten iron pouring process, the molten iron will not contact the inner wall of the mold, thereby reducing the supercooling of the molten iron and improving the metallographic structure of the outer wall of the casting. Therefore, the metallographic structure of the outer wall is much better than that of mushroom head burrs, and the outer wall can basically achieve 5-6 grade graphite. The evenly distributed graphite can improve the processing performance.

[0043] (6) The preparation method of the cylinder liner provided by the present invention comprises a first coating spraying and a second coating spraying, wherein the spraying interval between the first coating spraying and the second coating spraying is 3-10s, and the interval between the two coating sprayings is optimized so that the water and the foaming agent in the coating layer formed after the first coating spraying are rapidly vaporized and exploded during the continuous heating process, thereby forming many tiny voids in the coating layer, and then the second coating spraying is performed before the coating is completely dried to cover the pits formed by the previous coating, thereby optimizing the structure of the outer cylindrical surface of the cylinder liner, forming a honeycomb or hilly structure on its surface, thereby increasing the bonding rate between the cylinder liner and the aluminum alloy liquid, and improving the metallographic structure of the outer wall of the casting. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0045] Figure 1 This is an appearance diagram of a cylinder liner in Embodiment 1 of the present invention;

[0046] Figure 2 for Figure 1 A microscopic enlarged image of point A in the middle, where the magnification is 20 times;

[0047] Figure 3 for Figure 1 The magnified microscope image of the cross section along the A1-A2 section line at A in the middle, where the magnification is 100 times;

[0048] Figure 4 for Figure 1 The microscope magnified image at B in the middle, where the magnification is 20 times;

[0049] Figure 5 for Figure 1 The magnified microscope image of the cross section along the B1-B2 section line at B in the middle, where the magnification is 100 times;

[0050] Figure 6 for Figure 1 The microscope magnification at C in the middle shows a magnification of 20 times;

[0051] Figure 7 for Figure 1 The magnified microscope image of the cross section along the C1-C2 section line at center C, where the magnification is 100 times;

[0052] Description of reference numerals:

[0053] 1-depression; 1-1-closed mesh; 1-2-intermittent mesh; 2-raised ridge. DETAILED DESCRIPTION

[0054] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0055] Example 1

[0056] This embodiment provides a cylinder liner, such as Figure 1As shown, the outer surface of the cylinder liner is randomly distributed with recessed portions 1 and raised edges 2 that divide adjacent recessed portions 1. The raised edges 2 enclose the recessed portions 1. The mesh diameter of the recessed portions 1 is 0.5-4.0 mm, and the mesh depth is 0.1-0.6 mm. Preferably, as Figure 2-7 As shown, the mesh depth is 0.2-0.4 mm. More specifically, as Figure 3 As shown, the mesh depth is 428 μm; Figure 5 As shown, the mesh depth is 328 μm; Figure 7 As shown, the mesh depth is 353 μm.

[0057] In the above cylinder sleeve, the above arrangement overcomes the defect that the existing cylinder sleeve with outer burr has gaps between mushroom-shaped or pointed cone-shaped burrs on the surface, which hinders the flow of aluminum alloy liquid during gravity aluminum alloy casting and causes the aluminum alloy liquid to not fill the mold completely. In contrast, the cylinder sleeve of the present invention has a mesh structure with a specific mesh diameter and mesh depth distributed on its outer circumferential surface, and there are no gaps. During the pouring of aluminum alloy liquid, the aluminum alloy liquid can easily fill its surface. According to tests, the combination rate of the cylinder sleeve of the present invention and the aluminum alloy liquid reaches more than 90%, while the combination rate of the cylinder sleeve with outer burr and the aluminum alloy liquid is less than 50%.

[0058] Furthermore, the outer circumferential surface of the cylinder liner has closed meshes 1-1 accounting for at least 10% of the total number of meshes, and the remaining meshes are discontinuous meshes 1-2.

[0059] Furthermore, the number of meshes with a mesh diameter of 0.5-2 mm accounts for no less than 50% of the total number of meshes in the field of view; or,

[0060] The number of meshes with a mesh diameter of 2-4 mm accounts for no less than 50% of the total number of meshes in the field of view.

[0061] By optimizing the closed meshes on the outer circumferential surface of the cylinder liner to account for the total number of meshes, the number of meshes with a mesh diameter of 0.5-2mm to account for the total number of meshes in the field of view, or the number of meshes with a mesh diameter of 2-4mm to account for no less than 50% of the total number of meshes in the field of view, it helps to improve the bonding rate between the cylinder liner and the aluminum alloy liquid.

[0062] Example 2

[0063] This embodiment provides a cylinder liner and a preparation method thereof. The preparation method of the low outer cylindrical cast honeycomb-like or hilly-like cylinder liner adopts a centrifugal casting process and specifically includes the following steps:

[0064] (1) Smelting raw materials: adjusting the chemical composition of molten iron, specifically: weighing the specified raw materials in proportion, smelting them in a medium frequency induction furnace at 1500° C., and adjusting the raw materials according to the following weight requirements: carbon: 3.0%; sulfur: <0.1%; silicon: 2.7%; phosphorus: ≤0.4%; manganese: 0.5%; chromium: 0.4%; copper: 0.2%, and the balance is iron, to obtain molten iron;

[0065] (2) tapping and inoculation: tapping the above molten iron for inoculation, the tapping temperature is 1450°C, the inoculation is carried out by downstream inoculation, the inoculation amount is 0.6wt%, and the inoculant is silicon strontium zirconium;

[0066] (3) Coating preparation: Mix 75g of water, 20g of diatomaceous earth and 5g of bentonite and stir for more than 8h. The specific gravity is 1.1g / cm 3 , viscosity 50s, before using the paint, add 1.0% of the total weight of the paint into the foaming agent liquid, stir evenly for 5 minutes and then start using;

[0067] (4) Casting: A metal mold equipped with a vent plug was used, the roughness of the inner wall of the metal mold was less than 3.2 μm, and a nozzle with a diameter of 2 mm was used as a nozzle for spraying. Before spraying, the metal mold temperature was controlled at 390°C, the spraying speed was 480 rpm, the spraying pressure was 0.33 MPa, and the spraying opening angle was 110°. The nozzle first entered the inner cavity of the metal mold, and then started spraying. The spraying speed was 45 mm / s, and the first coating was sprayed;

[0068] Then, after staying for 8 seconds, the second coating spraying is carried out. At this time, the temperature of the metal mold is controlled at 400°C, the spraying speed is 450rpm, the spraying pressure is 0.35Mpa, the spraying opening angle is 90°, the nozzle first enters the inner cavity of the metal mold, and then starts spraying. The spraying speed is 35mm / s. After the spraying is completed, the inner hole of the metal mold cavity is blown with compressed air through the air plug for 8s to ensure that the coating is dry. Finally, the above-mentioned molten iron is poured at a pouring temperature of 1550°C. During the pouring process, centrifugal casting is carried out, the speed of the metal mold is 1700rpm, and the casting temperature is cooled by water to 790°C. After leaving the cylinder, it is air-cooled to obtain a blank.

[0069] (5) Shot blasting: The cooled blank is subjected to shot blasting treatment, with a shot blasting diameter of 0.4 mm, to obtain a low outer cylindrical cast-like honeycomb-like or hilly-like cylinder liner, wherein the outer cylindrical surface of the cylinder liner is randomly distributed with recessed portions and convex ridges that divide adjacent recessed portions, and the convex ridges enclose the recessed portions, and the mesh diameter of the recessed portions is 0.8-1.4 mm, and the mesh depth is 0.38-0.44 mm. The outer cylindrical surface of the cylinder liner has continuous closed irregular closed meshes that account for 8-8.5% of the total number of meshes, and the remaining meshes are intermittent irregular intermittent meshes, and the number of meshes with a mesh diameter of 0.5-2 mm accounts for no less than 50% of the total number of meshes in the field of view;

[0070] According to tests, the bonding rate between the cylinder liner of the present invention and the aluminum alloy liquid reaches more than 90%. At the same time, the cylinder liner of the present invention can achieve a proportion of more than 70% of type A graphite and a length of 5-6 levels at a distance of 1 mm from the outer wall.

[0071] Example 3

[0072] This embodiment provides a cylinder liner and a preparation method thereof. The preparation method of the low outer cylindrical cast honeycomb-like or hilly-like cylinder liner adopts a centrifugal casting process and specifically includes the following steps:

[0073] (1) Smelting raw materials: adjusting the chemical composition of molten iron, specifically: weighing the specified raw materials in proportion, smelting them in a medium frequency induction furnace at 1500° C., and adjusting the raw materials according to the following weight requirements: carbon: 3.0%; sulfur: <0.1%; silicon: 2.7%; phosphorus: ≤0.4%; manganese: 0.5%; chromium: 0.4%; copper: 0.2%, and the balance is iron, to obtain molten iron;

[0074] (2) tapping and inoculation: tapping the above molten iron for inoculation, the tapping temperature is 1500° C., the inoculation is carried out by downstream inoculation, the inoculation amount is 0.6 wt%, and the inoculant is silicon strontium zirconium;

[0075] (3) Coating preparation: Mix 75g of water, 20g of diatomaceous earth and 5g of bentonite and stir for more than 8h. The specific gravity is 1.1g / cm 3 , viscosity 50s, before using the paint, add 1.0% of the total weight of the paint into the foaming agent liquid, stir evenly for 5 minutes and then start using;

[0076] (4) Casting: A metal mold equipped with a vent plug was used, the roughness of the inner wall of the metal mold was less than 3.2 μm, and a nozzle with a diameter of 2 mm was used as a nozzle for spraying. Before spraying, the temperature of the metal mold was controlled at 300°C, the spraying speed was 1000 rpm, the spraying pressure was 0.2 MPa, and the spraying opening angle was 50°. The nozzle first entered the inner cavity of the metal mold, and then started spraying. The spraying speed was 50 mm / s, and the first coating was sprayed;

[0077] Then, after staying for 5 seconds, the second coating spraying is carried out according to the parameters of the first coating spraying. After the spraying is completed, the inner hole of the metal mold cavity is blown with compressed air through the vent plug for 5 seconds to ensure that the coating is dry. Finally, the above-mentioned molten iron is poured at a pouring temperature of 1500°C. During the pouring process, centrifugal casting is carried out, the speed of the metal mold is 1500rpm, and the casting temperature is cooled by water to 750°C. After leaving the cylinder, it is air-cooled to obtain a blank;

[0078] (5) Shot blasting: The cooled blank is subjected to shot blasting treatment, with a shot blasting diameter of 0.3 mm, to obtain a low outer cylindrical cast-like honeycomb-like or hilly-like cylinder liner, wherein the outer cylindrical surface of the cylinder liner is randomly distributed with recessed portions and convex ridges that divide adjacent recessed portions, and the convex ridges enclose the recessed portions, and the mesh diameter of the recessed portions is 0.5-1.0 mm, and the mesh depth is 0.22-0.28 mm. The outer cylindrical surface of the cylinder liner has continuous closed irregular closed meshes that account for 19-21% of the total number of meshes, and the remaining meshes are intermittent irregular intermittent meshes, and the number of meshes with a mesh diameter of 0.5-2 mm accounts for no less than 50% of the total number of meshes in the field of view;

[0079] According to tests, the bonding rate between the cylinder liner of the present invention and the aluminum alloy liquid reaches more than 93%. At the same time, the cylinder liner of the present invention can achieve a proportion of more than 75% of type A graphite and a length of 4-5 levels at a distance of 1 mm from the outer wall.

[0080] Example 4

[0081] This embodiment provides a cylinder liner and a preparation method thereof. The preparation method of the low outer cylindrical cast honeycomb-like or hilly-like cylinder liner adopts a centrifugal casting process and specifically includes the following steps:

[0082] (1) Smelting raw materials: adjusting the chemical composition of the molten iron, specifically: weighing the specified raw materials in proportion, smelting them in a medium frequency induction furnace at 1500° C., and adjusting the raw materials according to the following weight requirements: carbon: 3.4%; sulfur: <0.1%; silicon: 2.2%; phosphorus: ≤0.4%; manganese: 0.9%; chromium: 0.2%; copper: 1.2%, and the balance is iron, to obtain molten iron;

[0083] (2) tapping and inoculation: tapping the above molten iron for inoculation, the tapping temperature is 1525°C, the inoculation is carried out by downstream inoculation, the inoculation amount is 0.4wt%, and the inoculant is silicon strontium zirconium;

[0084] (3) Coating preparation: Mix 71g of water, 24g of diatomaceous earth and 5g of bentonite and stir for more than 8h. The specific gravity is 1.11g / cm 3 , viscosity 52s, before using the paint, add 1.5% of the total weight of the paint into the foaming agent liquid, stir evenly for 5 minutes and then start using;

[0085] (4) Casting: A metal mold equipped with a vent plug was used, the roughness of the inner wall of the metal mold was less than 3.2 μm, and a nozzle with a diameter of 1.8 mm was used as a nozzle for spraying. Before spraying, the metal mold temperature was controlled at 450°C, the spraying speed was 400 rpm, the spraying pressure was 0.4 MPa, and the spraying opening angle was 120°. The nozzle first entered the inner cavity of the metal mold, and then started spraying. The spraying speed was 45 mm / s, and the first coating was sprayed;

[0086] Then, after staying for 8 seconds, the second coating spraying is carried out. At this time, the temperature of the metal mold is controlled at 420°C, the spraying speed is 470rpm, the spraying pressure is 0.31Mpa, the spraying opening angle is 100°, the nozzle first enters the inner cavity of the metal mold, and then starts spraying. The spraying speed is 42mm / s. After the spraying is completed, the inner hole of the metal mold cavity is blown with compressed air through the air plug for 8s to ensure that the coating is dry. Finally, the above-mentioned molten iron is poured at a pouring temperature of 1600°C. During the pouring process, centrifugal casting is carried out, the speed of the metal mold is 1620rpm, and the casting temperature is cooled by water to 730°C. After leaving the cylinder, it is air-cooled to obtain a blank.

[0087] (5) Shot blasting: The cooled blank is subjected to shot blasting treatment, with a shot blasting diameter of 0.2 mm, to obtain a low outer cylindrical cast-like honeycomb-like or hilly-like cylinder liner, wherein the outer cylindrical surface of the cylinder liner is randomly distributed with recessed portions and convex ridges that divide adjacent recessed portions, the convex ridges enclose the recessed portions, the mesh diameter of the recessed portions is 0.7-1.2 mm, the mesh depth is 0.39-0.43 mm, the outer cylindrical surface of the cylinder liner has continuous closed irregular closed meshes accounting for 7-7.6% of the total number of meshes, and the remaining meshes are intermittent irregular discontinuous meshes, and the number of meshes with a mesh diameter of 0.5-2 mm accounts for no less than 50% of the total number of meshes in the field of view;

[0088] According to tests, the bonding rate between the cylinder liner of the present invention and the aluminum alloy liquid reaches more than 90%. At the same time, the cylinder liner of the present invention can achieve a proportion of more than 70% of type A graphite and a length of 5-6 levels at a distance of 1 mm from the outer wall.

[0089] Example 5

[0090] This embodiment provides a cylinder liner and a preparation method thereof. The preparation method of the low outer cylindrical cast honeycomb-like or hilly-like cylinder liner adopts a centrifugal casting process and specifically includes the following steps:

[0091] (1) Smelting raw materials: adjusting the chemical composition of molten iron, specifically: weighing the specified raw materials in proportion, smelting them in a medium frequency induction furnace at 1550° C., and adjusting the raw materials according to the following weight requirements: carbon: 3.3%; sulfur: <0.1%; silicon: 2.4%; phosphorus: ≤0.4%; manganese: 0.8%; chromium: 0.25%; copper: 1%, and the balance is iron, to obtain molten iron;

[0092] (2) tapping and inoculation: tapping the above molten iron for inoculation, the tapping temperature is 1500° C., the inoculation is carried out by downstream inoculation, the inoculation amount is 0.5 wt%, and the inoculant is silicon strontium zirconium;

[0093] (3) Coating preparation: Mix 73g of water, 22g of diatomaceous earth and 5g of bentonite and stir for more than 8h. The specific gravity is 1.15g / cm 3, viscosity 58s, before using the paint, add 1.3% of the total weight of the paint into the foaming agent liquid, stir evenly for 5 minutes and then start using;

[0094] (4) Casting: A metal mold equipped with a vent plug was used, the roughness of the inner wall of the metal mold was less than 3.2 μm, and a nozzle with a diameter of 2.5 mm was used as a nozzle for spraying. Before spraying, the temperature of the metal mold was controlled at 250°C, the spraying speed was 700 rpm, the spraying pressure was 0.3 MPa, and the spraying opening angle was 50°. The nozzle first entered the inner cavity of the metal mold, and then started spraying. The spraying speed was 40 mm / s, and the first coating was sprayed;

[0095] Then, after staying for 3 seconds, the second coating spraying is carried out according to the parameters of the first coating spraying. After the spraying is completed, the inner hole of the metal mold cavity is blown with compressed air through the vent plug for 5 seconds to ensure that the coating is dry. Finally, the above-mentioned molten iron is poured at a pouring temperature of 1450°C. During the pouring process, centrifugal casting is carried out, the speed of the metal mold is 1400rpm, and the casting temperature is cooled by water to 700°C. After leaving the cylinder, it is air-cooled to obtain a blank;

[0096] (5) Shot blasting: The cooled blank is subjected to shot blasting treatment, with a shot blasting diameter of 0.3 mm, to obtain a low outer cylindrical cast-like honeycomb-like or hilly-like cylinder liner, wherein the outer cylindrical surface of the cylinder liner is randomly distributed with recessed portions and convex ridges that divide adjacent recessed portions, the convex ridges enclose the recessed portions, the mesh diameter of the recessed portions is 1.0-2.0 mm, the mesh depth is 0.51-0.57 mm, the outer cylindrical surface of the cylinder liner has continuous closed irregular closed meshes accounting for 20-22% of the total number of meshes, and the remaining meshes are intermittent irregular discontinuous meshes, and the number of meshes with a mesh diameter of 0.5-2 mm accounts for no less than 50% of the total number of meshes in the field of view;

[0097] According to tests, the bonding rate between the cylinder liner of the present invention and the aluminum alloy liquid reaches more than 93%. At the same time, the cylinder liner of the present invention can achieve a proportion of more than 75% of type A graphite and a length of 4-5 levels at a distance of 1 mm from the outer wall.

[0098] Example 6

[0099] This embodiment provides a cylinder liner and a preparation method thereof. The preparation method of the low outer cylindrical cast honeycomb-like or hilly-like cylinder liner adopts a centrifugal casting process and specifically includes the following steps:

[0100] (1) Smelting raw materials: adjusting the chemical composition of molten iron, specifically: weighing the specified raw materials in proportion, smelting them in a medium frequency induction furnace at 1480° C., and adjusting the raw materials according to the following weight requirements: carbon: 3.5%; sulfur: <0.1%; silicon: 2.0%; phosphorus: ≤0.4%; manganese: 1.0%; chromium: 0.1%; copper: 1.5%, and the balance is iron, to obtain molten iron;

[0101] (2) tapping and inoculation: tapping the above molten iron for inoculation, the tapping temperature is 1480°C, the inoculation is carried out by downstream inoculation, the inoculation amount is 0.7wt%, and the inoculant is silicon strontium zirconium;

[0102] (3) Coating preparation: Mix 70g of water, 25g of diatomaceous earth and 5g of bentonite and stir for more than 8h. The specific gravity is 1.2g / cm 3 , viscosity 60s, before using the paint, add 1.3% of the total weight of the paint into the foaming agent liquid, stir evenly for 5 minutes and then start using;

[0103] (4) Casting: A metal mold equipped with a vent plug was used, the roughness of the inner wall of the metal mold was less than 3.2 μm, and a nozzle with a diameter of 1.5 mm was used as a nozzle for spraying. Before spraying, the temperature of the metal mold was controlled at 380°C, the spraying speed was 500 rpm, the spraying pressure was 0.4 MPa, and the spraying opening angle was 50°. The nozzle first entered the inner cavity of the metal mold, and then started spraying. The spraying speed was 30 mm / s, and the first coating was sprayed;

[0104] Then, after staying for 10 seconds, the second coating spraying is carried out according to the parameters of the first coating spraying. After the spraying is completed, the inner hole of the metal mold cavity is blown with compressed air through the vent plug for 5 seconds to ensure that the coating is dry. Finally, the above-mentioned molten iron is poured at a pouring temperature of 1400°C. During the pouring process, centrifugal casting is carried out, the speed of the metal mold is 1500rpm, and the casting temperature is cooled by water to 800°C. After leaving the cylinder, it is air-cooled to obtain a blank;

[0105] (5) Shot blasting: The cooled blank is subjected to shot blasting treatment, with a shot blasting diameter of 0.3 mm, to obtain a low outer cylindrical cast-like honeycomb-like or hilly-like cylinder liner, wherein the outer cylindrical surface of the cylinder liner is randomly distributed with recessed portions and convex ridges that divide adjacent recessed portions, and the convex ridges enclose the recessed portions, and the mesh diameter of the recessed portions is 2.0-3.0 mm, and the mesh depth is 0.58-0.63 mm. The outer cylindrical surface of the cylinder liner has continuous closed irregular closed meshes that account for 19-20% of the total number of meshes, and the remaining meshes are intermittent irregular intermittent meshes, and the number of meshes with a mesh diameter of 2-4 mm accounts for no less than 50% of the total number of meshes in the field of view;

[0106] According to tests, the bonding rate between the cylinder liner of the present invention and the aluminum alloy liquid reaches more than 93%. At the same time, the cylinder liner of the present invention can achieve a proportion of more than 75% of type A graphite and a length of 4-5 levels at a distance of 1 mm from the outer wall.

[0107] Example 7

[0108] This embodiment provides a cylinder liner and a preparation method thereof. The preparation method of the low outer cylindrical cast honeycomb-like or hilly-like cylinder liner adopts a centrifugal casting process and specifically includes the following steps:

[0109] (1) Smelting raw materials: adjusting the chemical composition of molten iron, specifically: weighing the specified raw materials in proportion, smelting them in a medium frequency induction furnace at 1500° C., and adjusting the raw materials according to the following weight requirements: carbon: 3.0%; sulfur: <0.1%; silicon: 2.7%; phosphorus: ≤0.4%; manganese: 0.5%; chromium: 0.4%; copper: 0.2%, and the balance is iron, to obtain molten iron;

[0110] (2) tapping and inoculation: tapping the above molten iron for inoculation, the tapping temperature is 1450°C, the inoculation is carried out by downstream inoculation, the inoculation amount is 0.6wt%, and the inoculant is silicon strontium zirconium;

[0111] (3) Coating preparation: Mix 75g of water, 20g of diatomaceous earth and 5g of bentonite and stir for more than 8h. The specific gravity is 1.1g / cm 3 , viscosity 50s, before using the paint, add 1.0% of the total weight of the paint into the foaming agent liquid, stir evenly for 5 minutes and then start using;

[0112] (4) Casting: A metal mold equipped with a vent plug was used, the roughness of the inner wall of the metal mold was less than 3.2 μm, and a nozzle with a diameter of 2 mm was used as a nozzle for spraying. Before spraying, the temperature of the metal mold was controlled at 360°C, the spraying speed was 900 rpm, the spraying pressure was 0.35 MPa, the spraying opening angle was 100°, the nozzle first entered the inner cavity of the metal mold, and then started spraying. The spraying speed was 45 mm / s, and the first coating was sprayed;

[0113] Then, after staying for 8 seconds, the second coating spraying is carried out according to the parameters of the first coating spraying. After the spraying is completed, the inner hole of the metal mold cavity is blown with compressed air through the vent plug for 8 seconds to ensure that the coating is dry. Finally, the above-mentioned molten iron is poured at a pouring temperature of 1450°C. During the pouring process, centrifugal casting is carried out, the speed of the metal mold is 1450rpm, and the casting temperature is cooled by water to 790°C. After leaving the cylinder, it is air-cooled to obtain a blank.

[0114] (5) Shot blasting: The cooled blank is subjected to shot blasting treatment, with a shot blasting diameter of 0.4 mm, to obtain a low outer cylindrical cast-like honeycomb-like or hilly-like cylinder liner, wherein the outer cylindrical surface of the cylinder liner is randomly distributed with recessed portions and convex ridges that divide adjacent recessed portions, the convex ridges enclose the recessed portions, the mesh diameter of the recessed portions is 0.5-1.0 mm, the mesh depth is 0.36-0.41 mm, the outer cylindrical surface of the cylinder liner has continuous closed irregular closed meshes accounting for 48-50% of the total number of meshes, and the remaining meshes are intermittent irregular intermittent meshes, and the number of meshes with a mesh diameter of 0.5-2 mm accounts for no less than 50% of the total number of meshes in the field of view;

[0115] According to tests, the bonding rate between the cylinder liner of the present invention and the aluminum alloy liquid reaches more than 93%. At the same time, the cylinder liner of the present invention can achieve a proportion of more than 75% of type A graphite and a length of 4-5 levels at a distance of 1 mm from the outer wall.

[0116] Example 8

[0117] This embodiment provides a cylinder liner and a preparation method thereof. The preparation method of the low outer cylindrical cast honeycomb-like or hilly-like cylinder liner adopts a centrifugal casting process and specifically includes the following steps:

[0118] (1) Smelting raw materials: adjusting the chemical composition of the molten iron, specifically: weighing the specified raw materials in proportion, smelting them in a medium frequency induction furnace at 1500° C., and adjusting the raw materials according to the following weight requirements: carbon: 3.4%; sulfur: <0.1%; silicon: 2.2%; phosphorus: ≤0.4%; manganese: 0.9%; chromium: 0.2%; copper: 1.2%, and the balance is iron, to obtain molten iron;

[0119] (2) tapping and inoculation: tapping the above molten iron for inoculation, the tapping temperature is 1525°C, the inoculation is carried out by downstream inoculation, the inoculation amount is 0.4wt%, and the inoculant is silicon strontium zirconium;

[0120] (3) Coating preparation: Mix 71g of water, 24g of diatomaceous earth and 5g of bentonite and stir for more than 8h. The specific gravity is 1.11g / cm 3 , viscosity 52s, before using the paint, add 1.5% of the total weight of the paint into the foaming agent liquid, stir evenly for 5 minutes and then start using;

[0121] (4) Casting: A metal mold equipped with a vent plug was used, the roughness of the inner wall of the metal mold was less than 3.2 μm, and a nozzle with a diameter of 1.8 mm was used as a nozzle for spraying. Before spraying, the metal mold temperature was controlled at 320°C, the spraying speed was 800 rpm, the spraying pressure was 0.4 MPa, the spraying opening angle was 120°, the nozzle first entered the inner cavity of the metal mold, and then started spraying. The spraying speed was 45 mm / s, and the first coating was sprayed;

[0122] Then, after staying for 8 seconds, the second coating spraying is carried out according to the parameters of the first coating spraying. After the spraying is completed, the inner hole of the metal mold cavity is blown with compressed air through the vent plug for 8 seconds to ensure that the coating is dry. Finally, the above-mentioned molten iron is poured at a pouring temperature of 1425°C. During the pouring process, centrifugal casting is carried out, the speed of the metal mold is 1600rpm, and the casting temperature is cooled by water to 730°C. After leaving the cylinder, it is air-cooled to obtain a blank;

[0123] (5) Shot blasting: The cooled blank is subjected to shot blasting treatment, with a shot blasting diameter of 0.2 mm, to obtain a low outer cylindrical cast-like honeycomb-like or hilly-like cylinder liner, wherein the outer cylindrical surface of the cylinder liner is randomly distributed with recessed portions and convex ridges that divide adjacent recessed portions, the convex ridges enclose the recessed portions, the mesh diameter of the recessed portions is 0.5-1.0 mm, the mesh depth is 0.43-0.46 mm, the outer cylindrical surface of the cylinder liner has continuous closed irregular closed meshes accounting for 38-42% of the total number of meshes, and the remaining meshes are intermittent irregular discontinuous meshes, and the number of meshes with a mesh diameter of 0.5-2 mm accounts for no less than 50% of the total number of meshes in the field of view;

[0124] According to tests, the bonding rate between the cylinder liner of the present invention and the aluminum alloy liquid reaches more than 93%. At the same time, the cylinder liner of the present invention can achieve a proportion of more than 75% of type A graphite and a length of 4-5 levels at a distance of 1 mm from the outer wall.

[0125] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a cylinder liner, characterized in that: Before pouring molten iron into the inner cavity of the mold, the method further includes the steps of spraying a coating on the inner wall of the mold at least twice and forming a coating layer on the inner wall of the mold; after pouring molten iron into the inner cavity of the mold, taking the casting out of the mold, air-cooling it to obtain a blank, and performing a shot blasting treatment on the blank; The paint spraying consists of a first paint spraying and a second paint spraying; after the first paint spraying, the second paint spraying is performed before the paint is completely dried, and the spraying interval between the first paint spraying and the second paint spraying is 3-10s; When spraying the coating, the temperature of the mold is 250-450°C, and the spraying pressure of the coating is 0.2-0.4Mpa; The coating used for coating spraying comprises the following raw materials by weight: 70-73 parts of water, 20-22 parts of diatomaceous earth and 5-10 parts of bentonite; before using the coating, a foaming agent accounting for 0.9-1.5% of the total weight of the coating is added to the coating; The outer circumferential surface of the cylinder sleeve is randomly distributed with recessed parts and convex edges that divide adjacent recessed parts, the recessed parts are enclosed by the convex edges, the mesh diameter of the recessed parts is 0.5-4.0 mm, and the mesh depth is 0.1-0.6 mm; The specific gravity of the coating is 1.1-1.2 g / cm³ and the viscosity is 50-70s; The rotation speed of the paint spraying is 400-1000rpm.

2. The preparation method according to claim 1, characterized in that: The paint spraying is carried out using a nozzle with a diameter of 1.5-2.5 mm as a nozzle; The angle between the spraying direction of the coating and the axial direction of the mold is 25-60°.

3. The preparation method according to claim 1, characterized in that: The pouring temperature of the pouring is 1400-1600°C; During the pouring process, centrifugal casting is performed, and the rotation speed of the mold is 1400-1700 rpm.

4. The preparation method according to claim 1, characterized in that: Before pouring the molten iron into the inner cavity of the mold, the method further includes adding an inoculant accounting for 0.4-0.8% of the total weight of the molten iron and inoculating the molten iron at 1380-1500°C.

5. The preparation method according to claim 4, characterized in that: The molten iron is composed of the following raw materials: 3.0-3.5wt% carbon, 2.0-2.7wt% silicon, 0.5-1.0wt% manganese, 0.1-0.4wt% chromium, 0.2-1.5wt% copper, <0.1wt% sulfur, ≤0.4wt% phosphorus, and the balance is iron; The inoculant is silicon strontium zirconium.

6. The preparation method according to claim 1, characterized in that: The vent plugs are evenly distributed on the side wall of the mold, and the roughness of the inner wall of the mold is less than 3.2 μm; The method also includes cooling the mold after pouring the molten iron to 700-800° C. and then taking the casting out of the mold.

7. The preparation method according to claim 1, characterized in that: The shot diameter of the shot blasting process is 0.2-0.4 mm.

8. A cylinder liner, characterized in that: The cylinder liner is prepared by the preparation method of any one of claims 1 to 7.

9. The cylinder liner according to claim 8, characterized in that: The mesh depth is 0.2-0.4 mm.