Solar power generation window based on colloidal silicon quantum dot nanoparticles selectively absorbing ultraviolet light

By using colloidal silicon quantum dot nanoparticles in solar power generation windows, the ultraviolet absorption efficiency and long-term stability problems in the prior art are solved, and efficient energy conversion and high transmittance are achieved. Spectral mass.

CN111987180BActive Publication Date: 2024-11-15ZHEJIANG ZHENENG TECHN RES INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010867042.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-26
Publication Date
2024-11-15
Estimated Expiration
2040-08-26

AI Technical Summary

Technical Problem

While existing solar power generation windows achieve high conversion efficiency and visible light transmittance, it is difficult to maintain long-term stability and efficiently absorb ultraviolet rays, resulting in limited energy efficiency and spectral quality.

Method used

Solar power generation windows based on colloidal silicon quantum dot nanoparticles (SiQDNPs) as fluorescent substances are used to form a luminescent solar concentrator (LSC) through a thin layer of liquid SiQDNPs suspension sandwiched between glass plates. Combined with a mirror structure, silicon-based photovoltaic The battery is front-coupled to achieve selective absorption and efficient conversion of ultraviolet rays.

Benefits of technology

It improves the power conversion efficiency and spectral quality of solar power generation windows, maintains high visible light transmittance, reduces fluorescence reabsorption loss, and enhances the overall electric energy generation ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111987180B_ABST
    Figure CN111987180B_ABST
Patent Text Reader

Abstract

The present invention relates to a solar power generation window based on colloidal silicon quantum dot nanoparticles selectively absorbing ultraviolet rays, comprising: SiQDNPs-LSC (silicon quantum dot nanoparticle solar concentrator), a power generation window and a reflector; a silicon-based photovoltaic cell strip (Si PV strip) is arranged in the power generation window, and the upper surface of the silicon-based photovoltaic cell strip adheres to the lower surface of SiQDNPs-LSC. The beneficial effects of the present invention are: under simulated sunlight, since SiQDNPs mainly absorb only ultraviolet rays, the propagated red fluorescence is hardly reabsorbed, and the sunlight passing through the window glass retains extremely high AVT and CRI; SiQDNPs-LSC can produce a higher power conversion efficiency, in which SiQDNPs fluorescence contribution accounts for a large proportion, and SiQDNPs-LSC retains a higher spectral quality, which is beneficial to window applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building integrated photovoltaic (BIPV), and in particular relates to a solar power generation window based on colloidal silicon quantum dot nanoparticles selectively absorbing ultraviolet rays. Background Art

[0002] Solar windows turn ordinary skylights or facade windows into small generators to extend the power grid, playing an indispensable role in building integrated photovoltaics (BIPV). BIPV is an emerging renewable energy technology that can replace or retrofit traditional building components with photovoltaic modules. Especially for high-rise buildings in highly urbanized areas, the space for installing ground or rooftop solar panels is far from enough to compensate for the energy consumption of the building itself. Therefore, in order to achieve the ultimate goal of near-zero energy buildings that many countries are actively pursuing, utilizing the huge window area of ​​high-rise buildings for energy collection is an effective method.

[0003] Although solar windows are not as efficient as traditional solar panels, they can still generate enough electricity when connected to a large power grid. At the same time, solar windows must meet certain safety requirements and remain translucent so that building residents can enjoy natural light. Ideally, solar windows will only absorb and collect the ultraviolet (UV) and near-infrared (NIR) parts of the solar spectrum, and change the incident spectrum through the visible light part (similar to the low-e coating on the window) to improve the energy efficiency of the building.

[0004] Several transparent photovoltaic technologies have emerged in solar window applications, some of which have been commercialized by companies (such as Onyx Solar, Ubiquitous Energy, SolarWindow Technologies, and UbiQD) and installed on famous buildings around the world. Among them, spatially segmented or intermediate-color silicon thin film technology has gained the most attention in the solar window market. In addition, semi-transparent films based on organic and organic-inorganic hybrid materials (such as perovskites) (dye-based and dye-sensitized photovoltaic cells) have recently attracted much attention, but the long-term stability of semi-transparent films must be improved before they can be widely deployed. Although these thin-film devices are able to achieve high power conversion efficiencies (PCEs) of up to 14%, they have a wide absorption capacity for the solar spectrum, including the visible light range, resulting in relatively low average visible light transmittance (AVT).

[0005] On the other hand, visibly transparent luminescent solar concentrators (LSCs) with selective absorption of UV and / or NIR wavelengths can easily achieve AVTs higher than 50%, a crucial feature for applications with visible light transmittance. In addition, LSCs with simple structures (usually waveguide plastic or glass flat panels coated or embedded with fluorophores) can seamlessly replace or retrofit existing windows without compromising their original aesthetic quality. Under sunlight, the fluorophores emit fluorescence, which is then guided by the LSCs and directed to the edges through total reflection, where conventional photovoltaic cells convert the fluorescence into electrical energy. The LSC sidewall area is much smaller than that of photovoltaic cells. On the front surface, the fluorescence photon flux received by the photovoltaic cell is concentrated, and the photovoltaic material cost is reduced.

[0006] LSC performance is evaluated from two important aspects, namely conversion efficiency (e.g., PCE and optical efficiency) and spectral quality (e.g., AVT and color rendering index CRI), which are usually inversely proportional to each other. In order to achieve high conversion efficiency without sacrificing spectral quality, the fluorophores used in LSCs need to have not only high photoluminescence quantum efficiency (PLQY), but also selective absorption outside the visible light and large Stokes shift to mitigate the reabsorption effect, which is usually the main loss of fluorescence conduction on LSCs. For single-junction, UV- and NIR-selective LSCs with 100% AVT, the thermodynamic limit of PCE can be as high as 21%. Recently, various fluorophores with the above optical properties have been explored to realize efficient and visible LSCs for solar power window applications, including organic dyes, phosphorescent nanocrystals, sustainable natural organic molecules, carbon nanodots, perovskite quantum dots, and other heavy metal-free quantum dots.

[0007] In summary, a solar power generation window based on colloidal silicon quantum dot nanoparticles that selectively absorbs ultraviolet rays is proposed. Summary of the invention

[0008] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a solar power generation window based on colloidal silicon quantum dot nanoparticles that selectively absorbs ultraviolet rays.

[0009] The solar power generation window based on colloidal silicon quantum dot nanoparticles selectively absorbing ultraviolet rays comprises: SiQDNPs-LSC (silicon quantum dot nanoparticle solar concentrator), a power generation window and a reflector; a silicon-based photovoltaic cell strip (Si PV strip) is arranged in the power generation window, the upper surface of the silicon-based photovoltaic cell strip is adhered to the lower surface of the SiQDNPs-LSC, and the four outer sides of the SiQDNPs-LSC are connected to the reflector through epoxy resin;

[0010] The SiQDNPs-LSC comprises a front glass plate, a PMMA ring, a rear glass plate and a thin layer of liquid SiQDNPs suspension (window glass); the lower surface of the front glass plate is bonded to the upper surface of the PMMA ring, the upper surface of the rear glass plate is bonded to the lower surface of the PMMA ring, and a gap structure is formed between the front glass plate, the PMMA ring and the rear glass plate; the thin layer of liquid SiQDNPs suspension is a gap structure filled with SiQDNPs suspension in 1-octadecene; the rear glass plate is the lower surface of the SiQDNPs-LSC.

[0011] Preferably, the inclination angle of the reflector in the horizontal direction of the SiQDNPs-LSC is 45°.

[0012] Preferably, the inclination angle of the reflector in the horizontal direction of the SiQDNPs-LSC is 0°.

[0013] Preferably, the thickness of the front glass plate is 0.1 mm to 100 mm.

[0014] Preferably, the thickness of the PMMA ring is 0.1 mm to 100 mm.

[0015] Preferably, the width of the silicon-based photovoltaic cell strip is 1 cm to 10 cm.

[0016] The beneficial effects of the present invention are:

[0017] (1) The present invention designs a solar power generation window using colloidal silicon quantum dot nanoparticles (SiQDNPs) as a fluorescent material for a luminescent solar concentrator (LSC), a silicon-based photovoltaic cell with a front-coupled solar power generation window; the luminescent solar concentrator (LSC) is composed of a thin layer of a liquid SiQDNPs suspension sandwiched between two thin glass plates, and the power generation window is made by adhering the front surface of the silicon-based photovoltaic cell to the rear surface of the LSC; in order to prevent fluorescence from leaking out from the edges, reflectors are attached to the four outer sides of the LSC;

[0018] (2) SiQDNPs dispersed in 1-octadecene can selectively absorb the ultraviolet part of the solar spectrum and convert it into red fluorescence with high quantum efficiency; through the inherent waveguide structure of the LSC and the reflectors around the edge of the LSC, the fluorescence generated by the SiQDNPs is ultimately directed to the forward silicon-based solar cell strip, thereby enhancing the overall PCE; since the overlap between the absorption spectrum and the photoluminescence spectrum of the SiQDNPs is negligible, the loss due to reabsorption is not significant; the forward peripheral silicon photovoltaic strip can not only collect the red fluorescence generated by the SiQDNPs to generate electricity, but also obtain direct solar radiation to generate electricity through the forward design;

[0019] (3) Under simulated sunlight, since SiQDNPs mainly absorb only ultraviolet rays, the transmitted red fluorescence is almost not reabsorbed. At the same time, the sunlight passing through the window glass retains extremely high AVT and CRI. SiQDNPs-LSC can produce higher power conversion efficiency, in which the SiQDNPs fluorescence contribution accounts for a large proportion. At the same time, SiQDNPs-LSC retains a higher spectral quality, which is beneficial for window applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 3D magnified image of SiQDNPs-LSC (mirror not shown);

[0021] Figure 2 is the cross-sectional view of the edge of SiQDNPs-LSC;

[0022] Figure 3 is the back view of SiQDNPs-LSC;

[0023] Figure 4 PCE gain diagram of SiQDNPs-LSCs of different sizes when the reflector is tilted 45° and 0° respectively under ultraviolet irradiation;

[0024] Figure 5 (A) is a schematic diagram of the experimental setup. Figure 5 (B) is the measured PL spectra at two slit positions;

[0025] Figure 6 (A) and Figure 6 (B) SiQDNPs-LSC with the mirror tilted 45° and 0° (W LSC =10cm) with the change trend of the PCE gain of illumination wavelength (365nm, 465nm, 525nm and 625nm); Figure 6 (C) Figure 6 (D) shows SiQDNPs-LSC with the mirror tilted at 45° and 0° (W LSC =10cm) of the overall PCE versus illumination wavelength;

[0026] Figure 7 (A) is the relationship between the PCE gain of SiQDNPs-LSC and the SiQDNPs concentration under simulated sunlight; Figure 7 (B) is the overall PCE and AVT of the window glass or the overall AVT diagram corresponding to (A); Figure 7 (C) is 2.7 mg*mL -1 SiQDNPs-LSC(W LSC =10cm) state diagram in outdoor environment; Figure 7(D) CRI and CCT diagrams of SiQDNPs-LSC with different SiQDNPs concentrations;

[0027] Figure 8 (A) Schematic diagram of SiQDNPs-LSC installation; Figure 8 (B) Photos of SiQDNPs-LSCs of different sizes with the mirror tilted 45° (upper row) and 0° (lower row)

[0028] Fig. 9 (A) Transmission spectra of SiQDNPs-LSC window glass with and without SiQDNPs; Fig. 9 (B) is the transmission spectrum of SiQDNPs-LSC power generation window; Fig. 9 (C) is the transmission spectrum of 5mm glass / 2mm 1-octadecene / 5mm glass.

[0029] Fig.10 Optical path diagram for critical light cone analysis of the window glass area of ​​SiQDNPs-LSC;

[0030] Fig.11 (A) is the transmission spectrum through the window glass area of ​​SiQDNPs-LSC. Fig.11 (B) is the curve of AM 1.5G photon flux; Fig.11 (C) is the AM 1.5G spectral irradiance diagram.

[0031] Explanation of the reference numerals: front glass plate 1, PMMA ring 2, rear glass plate 3, silicon-based photovoltaic cell strip 4, thin layer of liquid SiQDNPs suspension 5, epoxy resin 6, reflector 7, SiQDNPs suspension in 1-octadecene 8, fiber 9, photomultiplier tube 10, black board paper 11. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with embodiments. The description of the following embodiments is only used to help understand the present invention. It should be noted that for ordinary persons in the art, without departing from the principle of the present invention, the present invention can also be modified in some ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0033] Embodiment 1:

[0034] like Figure 1As shown, the solar power generation window based on colloidal silicon quantum dot nanoparticles selectively absorbing ultraviolet rays includes: SiQDNPs-LSC, a power generation window and a reflector; SiQDNPs-LSC includes a front glass plate 1 (thickness of 1 mm), a PMMA ring 2 (thickness of 2 mm) and a rear glass plate 3 (thickness of 1 mm); the gap structure formed by the two glass plates (front glass plate 1 and rear glass plate 3) and the PMMA ring 2 is filled with SiQDNPs suspension; the central square area containing the SiQDNPs suspension (area = W LSC ×W LSC ) is defined as a thin layer of liquid SiQDNPs suspension 5, while the silicon photovoltaic strip (Si PV strip) (width = 1 cm) adhered to the back of the SiQDNPs-LSC forms the power generation window;

[0035] like Figure 2 As shown, the edge of SiQDNPs-LSC is provided with a reflector 7 with a bottom tilted upward at 45° or a reflector 7 with a bottom tilted upward at 0°, and the reflector 7 with a bottom tilted upward at 45° is connected to the front glass plate 1, the PMMA ring 2 and the rear glass plate 3 through the epoxy resin 6; under 365nm ultraviolet irradiation, the SiQDNPs-LSC with the reflector 7 tilted at 45° shows more red fluorescence reflected along the power generation window, while the SiQDNPs-LSC with the reflector 7 tilted at 0° shows more red fluorescence escaping from the window glass.

[0036] Under illumination, the front silicon-based solar cell (Si PV) can generate electricity by collecting the light incident on the power generation window. At the same time, the fluorescence generated by the silicon quantum dots in the window glass can also be transmitted to the silicon-based photovoltaic cell strip 4 and improve its efficiency. The efficiency enhancement can be quantified by the PCE gain, which is defined as the PCE of the silicon-based photovoltaic cell strip 4 measured with the SiQDNPs suspension contained in the thin layer of liquid SiQDNPs suspension 5 divided by the PCE measured with pure 1-octadecene in the window glass. In order to avoid the complexity of wiring, for each SiQDNPs-LSC, we only placed a silicon-based photovoltaic cell strip 4 cut into small pieces from a conventional single-crystalline silicon solar cell wafer (PCE = 20.8%) along one edge of the SiQDNPs-LSC. The total light absorption area for calculating the total PCE is equal to (W LSC +2cm)×(W LSC +2cm), and the total electrical energy generated is equal to the total electrical energy generated by a silicon-based photovoltaic cell strip 4 multiplied by four.

[0037] Embodiment 2:

[0038] In order to understand how window glass size affects the enhancement effect, the window glass with different W LSC PCE gain under size ( Figure 4and Table 1). Figure 4 The intensity of medium ultraviolet light is equal to 0.97mW*cm -2 , wavelength is 365nm, the concentration of SiQDNPs suspension is about 0.7mg*mL -1 Table 1 shows the SiQDNPs-LSCs (W LSC =2cm, 4cm, 6cm, 8cm and 10cm) short-circuit current (I SC ), open circuit voltage (V OC ), fill factor (FF) and maximum power values.

[0039] Table 1 Parameters of SiQDNPs-LSCs of different sizes under UV illumination

[0040]

[0041] Since the light intensity incident on the SiQDNPs-LSC surface is constant (0.97 mW*cm -2 ), so the SiQDNPs suspension loaded in the window glass (about 0.7 mg*mL -1 ) and the result obtained with pure 1-octadecene in window glass (i.e. without SiQDNPs) corresponds to Figure 4 The PCE gain is shown in Figure 1. The I is highlighted when the mirror is tilted 45° and 0° respectively. SC The difference between them is ΔI SC , used to calculate W LSC =10 cm and the mirror is tilted 45° for SiQDNPs-LSC opt . Two groups I SC The difference between them is ΔI SC , used to calculate W LSC =10 cm and the mirror tilted 0° for SiQDNPs-LSC opt .

[0042] Fig. 9 (A) Curve #1 represents the light path through 1mm glass / 2mm 1-octadecene / 1mm glass; Curve #2 represents the light path through 1mm glass / 2mm SiQDNPs suspension (about 0.7mg*mL-1) / 1mm glass; Curve #3 is curve #1 minus curve #2, representing the absorption of SiQDNPs dispersed in 1-octadecene; at 365nm, the absorption is 50%; Fig. 9 The curve in (B) represents the optical path of 1mm glass / 2mm PMMA / 1mm glass. Fig. 9 Curve #1 in (A) is almost identical. Fig.10Path (A) shows critical cone loss, while path (C) shows total internal reflection; path (B) shows the incident angle of the fluorescent beam at the glass-air interface is equal to θ C (critical angle) and the incident angle at the 1-octadecene-glass interface is equal to θ1; at this time, according to Snell's law, 1.44×sinθ1=1.46×sinθ C =1×sin 90°=1; therefore, the percentage of fluorescent photons in the window glass that can propagate to the edge of the LSC via total internal reflection is η opt The maximum theoretical value is equal to (1-1 / 1.44 2 ) 1 / 2 =72%.

[0043] During the experiment, for each W LSC The PCE with and without SiQDNPs was measured using the same SiQDNPs-LSC but with different contents in the window glass. In general, a larger light absorption area leads to more fluorescence inside the window glass, thus improving the PCE of Si-based photovoltaic cells with 4. In particular, in W LSC = 10 cm, the PCE gain can be as high as 2.24 and 1.28 when the mirror is tilted 45° and 0° respectively. LSC When the PCE drops below 2 cm, it approaches unity. In addition, the optical efficiency (η opt ), defined here as the percentage of fluorescent photons generated inside the window glass that are able to propagate to and be received by the Si PV, can be calculated using the following formula: Where ΔI SC represents the short-circuit current difference of a silicon photovoltaic strip measured with and without SiQDNPs (Table 1), I light is the incident light intensity at 365 nm (=0.97 mW cm -2 ), A SiQDNPs is the absorbance of the SiQDNPs layer at 365 nm (=50%, Fig. 9 (A)), hν 365nm is the photon energy of 365nm (=5.44×10 - 19 J), is the PLQY of the SiQDNPs layer at 365 nm (about 0.35) and Quantum efficiency of Si PV at 650nm (about 0.95).

[0044] For W LSC =10 cm and the SiQDNPs-LSC with the mirror tilted at 45°, η optis estimated to be 49%, while η defined by Snell's law opt The maximum theoretical value of is 72%. In other words, in addition to the 28% escape cone loss, about 32% of the propagated fluorescence photons are lost when propagating through the waveguide by total internal reflection and are finally absorbed by the Si PV. The reasons for the loss of propagated fluorescence photons may include: (1) reabsorption by SiQDNPs, (2) absorption by the glass plate, (3) scattering due to imperfect waveguide structure and (4) non-ideal reflectivity of the mirror. For comparison, for the waveguide with the same W LSC size (=10 cm) but with a mirror tilted at 0°, η opt The estimated value is 28%, which is much lower than that of using W LSC The obtained η opt (=49%). The reflector is tilted 45° because most of the fluorescence photons propagating perpendicular to the edge will be reflected back into the waveguide by the perpendicular reflector, resulting in a higher probability that the above loss mechanism will be exhausted. Figure 3 As shown, the stronger red fluorescence escaping from the window glass is a manifestation.

[0045] To identify the key factors for the loss of fluorescent photons when propagating in the window glass region, we characterized the fluorescence (PL) collected from the edge of the SiQDNPs-LSC when only a slit of the window glass was exposed to 365 nm UV irradiation ( Figure 5 ), SiQDNPs-LSC (without reflector), and a device with only a slit in the window glass exposed to 365nm UV light. Figure 5 (A) shows the optical setup for measuring the edge fluorescence spectra of SiQDNPs-LSC at two different slit positions. Figure 5 In (A), both the #1 device and the #2 device use a fiber 9 and a photomultiplier tube 10, the fiber 9 is connected to a spectrometer, and the spectrometer is connected to the photomultiplier tube 10; Figure 5 (B) shows that compared with the slit configuration #1 curve, the PL spectrum measured with the slit configuration #1 curve shows that the PL peak has a 6nm blue shift and the integrated area is reduced by about 30%. The 365nm UV intensity incident on the SiQDNPs-LSC surface is 4mW*cm -2 , the concentration of SiQDNPs is about 0.7mg*mL -1. PL spectra were obtained using a multimode quartz fiber (numerical aperture = 0.22), one end of which was fixed to the SiQDNPs-LSC edge and the other end was connected to a fluorescence spectrophotometer consisting of a monochromator and a photomultiplier tube (PMT). The relative position between the multimode quartz fiber and the SiQDNPs-LSC edge was always kept constant, and the small gap between the two parts was filled with immersion lens oil (refractive index = 1.52) to facilitate the entry of fluorescence into the fiber. The slit was placed 9 cm away from the silicon-based photovoltaic cell strip ( Figure 5 Compared with the slits next to the silicon-based photovoltaic cell strip ( Figure 5 The fluorescence spectrum shows a 6nm blue shift in the PL peak. This blue shift is attributed to the absorption of soda-lime glass, which has a stronger absorption in the red spectral range ( Fig. 9 (C)). Although the front and rear glass plates are very thin (1 mm), the cumulative thickness of the glass that the red fluorescent beam passes through can be significant, given the fact that multiple total internal reflections may be required for the beam to reach the edge of the LSC. Unlike most other LSCs, the reabsorption due to the fluorophore is not significant relative to the glass absorption, because based on the absorption spectrum, SiQDNPs reabsorption should result in a red-shift rather than a blue-shift in the PL. ( Figure 5 (B) In addition, since the overlap between the absorbance and PL spectra of the SiQDNPs suspension is negligible and has a small molar extinction coefficient at wavelengths greater than 500 nm, the fluorescence reabsorption effect is insignificant. Finally, the integrated area of ​​the PL spectrum measured at slit #2 is 30% smaller than that measured at slit #1, indicating that approximately 30% of the fluorescence photons are lost when propagating within a distance of 9 cm. window glass. In fact, in a 10 cm × 10 cm window glass, the average propagation distance of the fluorescence photons should be less than 9 cm. Considering other potential losses at the edge of the LSC, the window glass loss analysis here is consistent with the previously estimated optical efficiency (η opt =49%, i.e., about 32% of the propagating fluorescent photons are lost before being received by the Si PV) LSC =10cm and SiQDNPs-LSC with the mirror tilted at 45°.

[0046] Next, SiQDNPs-LSCs (W LSC =10cm) and the overall PCE (Table 2). Figure 6 (A) Figure 6 (B) The single wavelength light sources used are high-power light-emitting diodes with wavelengths of 365 nm, 465 nm, 525 nm, and 625 nm, and the light intensities incident on the SiQDNPs-LSC surface are equal to 0.97 mW*cm -2、0.93mW*cm -2 、1.00mW*cm -2 and 0.84mW*cm -2 The concentration of SiQDNPs is about 0.7 mg*mL -1 The curve in the figure represents the absorption of SiQDNPs in window glass. Figure 6 (C) Figure 6 (D) The illumination wavelengths include 365nm, 465nm, 525nm and 625nm, Figure 6 (C) and Figure 6 The upper curve in (D) represents the overall PCE measured by LSC filled with SiQDNPs, and the lower curve represents the overall PCE measured by LSC not filled with SiQDNPs. Table 2 below shows the PCE of SiQDNPs-LSC (W) under irradiation of single wavelength light sources at 365nm, 465nm, 525nm and 625nm. LSC =10cm) short-circuit current (I SC ), open circuit voltage (V OC ), fill factor (FF) and PCE values; the single wavelength light source here is generated by 365nm, 465nm, 525nm and 625nm high-power light-emitting diodes, and the light intensity incident on the SiQDNPs-LSC surface is equal to 0.97mW*cm -2 、0.93mW*cm -2 、1.00mW*cm -2 and 0.84mW*cm -2 The concentration of SiQDNPs is about 0.7 mg*mL -1 The total PCE was calculated using a total light absorption area equal to 12 cm x 12 cm and a total electrical energy generated equal to the total electrical energy generated by one silicon photovoltaic strip as shown in the table multiplied by four.

[0047] Table 2 Parameters of SiQDNPs-LSC under different wavelengths of light source irradiation

[0048]

[0049] Generally, SiQDNPs-LSCs with a mirror tilted at 45° have higher optical efficiency (η opt =49% vs. 28%), thus showing a higher PCE gain, but an overall relatively low PCE, because the SiPV is partially shaded by the 45° tilted mirror ( Figure 2 In addition, the trend of PCE gain is almost consistent with that of SiQDNPs absorption ( Figure 1 , Figure 2 and Fig. 9The gain is shown in Figure 3 (curve #3 in Figure 4), indicating that the gain should be attributed to the fluorescence generated by SiQDNPs. Under 365nm illumination, SiQDNPs-LSCs with mirrors tilted 45° and 0° have high PCE gains of 2.24 and 1.28, respectively. However, since the absorption of SiQDNPs at wavelengths >500nm is negligible, the PCE gain values ​​in the green and red spectral ranges are almost equal and tend to be consistent. On the other hand, the overall PCE trend of LSCs without SiQDNPs added to window glass (respectively Figure 6 (C) and the lower curve in 6(D)) is related to the transmission spectrum through the band region of silicon-based photovoltaic cells ( Fig. 9 (B) The overall PCE measured using SiQDNPs in window glass due to fluorescence enhancement under 365 and 465 nm illumination (respectively Figure 6 (C) and 6(D) above) are higher than the PCE measured without SiQDNPs. Under 525nm illumination, for SiQDNPs-LSC with mirrors tilted 45° and 0°, the PCE gain is negligible and the overall PCE reaches a maximum of 1.3% and 2%, respectively. The overall PCE decreases at 625nm, which may be due to the stronger absorption of the soda-lime glass plate in the red spectral range.

[0050] In addition to the wavelength-resolved analysis, we also performed a quantitative analysis of the SiQDNPs suspension at different concentrations ( Figure 7 (A) and Figure 7 (B) and Table 3) of SiQDNPs-LSC (W LSC =10cm) under simulated sunlight were characterized. Figure 7 (A) Middle W LSC =10cm, SiQDNPs concentration is 0.9mg*mL -1 、1.8mg*mL -1 , 2.7mg*mL -1 and 3.6mg*mL -1 These four values; the simulated sunlight is generated by a conventional xenon lamp, and the light intensity incident on the SiQDNPs-LSC surface is 6.51 mW*cm -2 . Figure 7 In (B), for Figure 7 (A) SiQDNPs-LSC, the overall PCE and the AVT of the window glass or the overall AVT (= (window glass AVT) × 10 2 / 12 2 ), for each data point, the corresponding SiQDNPs concentration is marked. Table 3 below shows the SiQDNPs-LSC (WLSC =10cm) short-circuit current (I SC ), open circuit voltage (V OC ), fill factor (FF), and PCE values. Here, the simulated sunlight was generated by a conventional xenon lamp, and the light intensity incident on the SiQDNPs-LSC surface was 6.51 mW*cm -2 Note that the total PCE is calculated using a total light absorption area equal to 12 cm × 12 cm, and the total power produced is equal to the total power produced by one silicon photovoltaic strip as shown in the table, multiplied by four.

[0051] Table 3 Parameter values ​​of SiQDNPs-LSC with different SiQDNPs concentrations under simulated sunlight

[0052]

[0053] Figure 8 (A) The size of the strip silicon photovoltaic panel 4 is 13 cm × 1 cm, and the silicon photovoltaic panel 4 just covers a quarter of the entire power generation window area; Figure 8 (B) Each SiQDNPs-LSC is coupled to a silicon photovoltaic panel with four strips. The width of the power generation window (1 cm) remains unchanged, while the window glass area (W LSC ×W LSC A small hole was opened on the PMMA ring for injecting or removing SiQDNPs suspension or pure 1-octadecene.

[0054] Similar to the single-wavelength experiments described above, the SiQDNPs-LSC tilted at 45° shows higher PCE gain than the mirror tilted at 0°, but the overall PCE is relatively low. In addition, since more fluorescence is generated inside the window glass, the PCE gain and overall PCE will increase with increasing SiQDNPs concentration. However, when the SiQDNPs concentration becomes too high, the SiQDNPs absorption (especially in the UV range) will saturate ( Fig.11 (A)), i.e., further increase in SiQDNPs concentration does not lead to more fluorescence. On the other hand, the reabsorption loss increases due to high SiQDNPs concentration. Therefore, the PCE gain and total PCE values ​​of SiQDNPs-LSCs with mirror tilts of 45° and 0° increase at high concentrations of 3.6 mg mL -1 The concentration was lower than 2.7 mg mL -1 . Fig.11 (A) Transmission spectra T(λ) through the window glass region of SiQDNPs-LSC filled with pure 1-octadecene (curve a), 0.9 mg*mL -1 (b curve), 1.8 mg*mL -1(Curve c) and 3.6 mg*mL -1 (d) SiQDNPs suspension. As the SiQDNPs concentration increases, the absorption of SiQDNPs, especially in the UV range, tends to be saturated. In addition, it is compared with the photopic brightness function P(λ) (black dashed line). Fig.11 (B) AM 1.5G photon flux is set to S flux (λ). Fig.11 (C) AM 1.5G spectral irradiance is set to S irradiance (λ). AVT is calculated as follows: ∫T(λ)P(λ)S flux (λ)dλ / ∫P(λ)S flux (λ)dλ. CRI and CCT values ​​are estimated based on: T(λ)S irradiance (λ).

[0055] In terms of spectral properties, since the main absorption of SiQDNPs suspension is in the UV range and there is almost no absorption in the visible range, the AVT and CRI measured in the window glass area are over 80% and 90%, respectively, and the correlated color temperature (CCT) is generally above 4000K ( Figure 7 (B) and 7 (C)). In addition, since the silicon-based photovoltaic cell strip composed of strip Si PV (width = 1 cm) is completely opaque, it can be obtained by multiplying the window glass AVT by 10 2 / 12 2 To calculate the total AVT. In summary, when the SiQDNPs concentration is equal to 2.7 mg mL -1 The PCE is the highest when the reflector is tilted 45° and 0°, and the PCE gains of SiQDNPs-LSC are 1.06 and 1.02, respectively, and the overall PCE is 2.47% and 4.37%, respectively. The AVT of the window glass is 86%, the overall AVT is 60%, the CRI is 94, and the CCT is 4612K. Compared with other solar power generation window technologies, such as large-capacity heterojunction organic photovoltaic cells (PCE=4%, AVT=64.4%, CRI=94.5), near-infrared selective exciton semiconductor photovoltaic cells based on organic salt derivatives (PCE=5.1%, AVT=51.5% and CRI=65.3) and based on NIR selective LSCs (PCE=0.4%, AVT=88.3% and CRI=94.3), SiQDNPs-LSC obtained similar PCE in this work, while obtaining excellent spectral characteristics due to the UV selective absorption of SiQDNPs. By adopting a larger W LSC , while keeping the width of the Si PV strip the same, the PCE gain (following Figure 4 The trend shown in Figure 2) and the overall AVT (i.e. the window glass AVT multiplied by the factor W LSC2 / (W LSC +2) 2 , can be further improved.

[0056] in conclusion:

[0057] The present invention proposes a novel solar power generation window structure, which combines the concepts of spatially segmented PV and LSC; the window glass is composed of a SiQDNP suspended thin layer sandwiched between two thin glass plates, and the Si PV strips placed forward along the periphery of the LSC form a power generation window; in sunlight, the forward-placed silicon photovoltaic panel (Si PV) not only directly collects solar radiation, but also utilizes the fluorescence generated by the SiQDNP transmitted from the window glass.

[0058] SiQDNPs (<10 nm) were chemically grafted with 1-octene by hydrosilylation to form a uniform and stable suspension in 1-octene. The molar extinction coefficient of the SiQDNP suspension for selective absorption of 350 nm UV light was equal to 2.68 × 10 5 M -1 cm -1 The SiQDNP-LSCs re-emit red fluorescence (peak at about 650nm) with a PLQY value of 42%. LSC ) and SiQDNP absorption. Under 365nm ultraviolet irradiation, the PCE gain (W LSC =10cm, SiQDNP concentration = 0.7mg*mL -1 , the mirror is tilted 45°) can be as high as 2.24, which corresponds to the optical efficiency (η opt ) is equal to 49%. In contrast, the maximum theoretical η defined by Snell's law is opt Here, the main optical loss is due to the absorption of the soda-lime glass plate rather than the reabsorption of SiQDNP. Finally, under simulated sunlight, SiQDNP-LSC (W LSC =10cm, SiQDNP concentration = 2.7mg*mL -1 , mirror tilted 45°) with overall PCE = 2.47%, PCE gain = 1.06, window glass AVT = 86%, overall AVT = 60%, CRI = 94, CCT = 4612K.

[0059] Compared with other solar window technologies, the SiQDNP-LSCs in this work achieved similar PCEs while achieving excellent spectral properties due to the ultraviolet-selective absorption of SiQDNPs.

Claims

1. A solar power generation window based on colloidal silicon quantum dot nanoparticles selectively absorbing ultraviolet light, characterized in that: include: A silicon quantum dot nanoparticle solar concentrator, a power generation window and a reflector; the power generation window is provided with a silicon-based photovoltaic cell strip (4), the upper surface of the silicon-based photovoltaic cell strip (4) is adhered to the lower surface of the silicon quantum dot nanoparticle solar concentrator, and the four outer sides of the silicon quantum dot nanoparticle solar concentrator are connected to the reflector (7) via epoxy resin (6); The silicon quantum dot nanoparticle solar energy concentrator comprises a front glass plate (1), a PMMA ring (2), a rear glass plate (3) and a thin layer (5) of a liquid silicon quantum dot nanoparticle suspension; the lower surface of the front glass plate (1) is bonded to the upper surface of the PMMA ring (2), the upper surface of the rear glass plate (3) is bonded to the lower surface of the PMMA ring (2), and a gap structure is formed between the front glass plate (1), the PMMA ring (2) and the rear glass plate (3); the thin layer (5) of the liquid silicon quantum dot nanoparticle suspension is a gap structure filled with a silicon quantum dot nanoparticle suspension (8) in 1-octadecene; the rear glass plate (3) is the lower surface of the silicon quantum dot nanoparticle solar energy concentrator; The inclination angle of the reflector (7) in the horizontal direction of the silicon quantum dot nanoparticle solar energy concentrator is 45°; the thickness of the front glass plate (1) is 0.1 mm to 100 mm.

2. The solar power generation window based on colloidal silicon quantum dot nanoparticles selectively absorbing ultraviolet rays according to claim 1, characterized in that: The thickness of the PMMA ring (2) is 0.1 mm to 100 mm.

3. The solar power generation window based on colloidal silicon quantum dot nanoparticles selectively absorbing ultraviolet rays according to claim 1, characterized in that: The width of the silicon-based photovoltaic cell strip (4) is 1 cm to 10 cm.