Ternary positive electrode material and preparation method, lithium ion battery

The metal element doping and coating layer preparation in high-nickel ternary cathode materials is carried out through a one-step pure solid phase method, which solves the problem of material cycle stability and safety, and forms a dense coating layer to block electrolyte contact, which significantly Improved cycle stability and safety.

CN115385394BActive Publication Date: 2024-10-15ZHEJIANG HUAYOU COBALT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211020730.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-24
Publication Date
2024-10-15
Estimated Expiration
2042-08-24

AI Technical Summary

Technical Problem

High-nickel ternary cathode materials have problems in terms of cycle stability and safety, mainly due to insufficient Ni-O chemical bond strength, material structure changes and electrolyte contact caused by side reactions, and conventional water washing methods will destroy the surface chemical structure, affecting cycle life.

Method used

A one-step pure solid phase method is used to mix and sinter the ternary cathode material precursor, lithium salt and doping metal source. Doping metal elements are used to form a dense coating layer, which enhances the binding force between transition metal ions and oxygen atoms, and neutralizes the and residual alkali on the surface to prevent contact with the electrolyte.

Benefits of technology

It significantly improves the cycle stability and safety of the ternary cathode material, reduces the risk of side reactions, extends the cycle life of the battery, and improves the application prospects of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115385394B_ABST
    Figure CN115385394B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of lithium-ion battery materials, and in particular to a ternary positive electrode material and a preparation method, and a lithium-ion battery. The preparation method of the ternary positive electrode material of the present application comprises the following steps: mixing a ternary positive electrode material precursor, a lithium salt and a doping metal source to obtain a mixed material; wherein the doping metal source is selected from oxides and / or hydroxides of doping metals, and the doping metal source contains at least two doping metals, and the total amount of doping metals is calculated based on the remaining amount after being doped in the ternary positive electrode material precursor; sintering the mixed material to obtain a ternary positive electrode material. The preparation method provided in the present application adopts a one-step pure solid-phase method to simultaneously realize the metal element doping and coating layer preparation of the ternary positive electrode material. The prepared ternary positive electrode material has a good doping effect, can significantly improve the cycle stability, and has a good application prospect in lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lithium-ion battery materials, and in particular, relates to a ternary positive electrode material and a preparation method, and a lithium-ion battery. Background Art

[0002] High nickel ternary cathode materials have the advantages of ultra-high specific capacity, high working voltage and compaction density, and have become the first choice for high-end lithium-ion power batteries for use in new energy vehicles with long driving range. However, high nickel ternary cathode materials face two industry pain points: poor cycle stability and safety, which hinder their further promotion. The main reason is that the Ni-O chemical bond is weak, which makes it easy to release oxygen and the material structure changes from α-NaFeO 2 The layered structure is transformed into an electrochemically inactive NiO rock salt structure. The stress caused by the volume anisotropy change during the charge and discharge process will also cause the positive electrode material to be easily crushed. In addition, the high-nickel ternary positive electrode material is in a charged state due to the presence of a large amount of highly oxidizing Ni 4+ Ions are prone to strong side reactions with the electrolyte, affecting cycle stability. In addition, there is residual alkali on the surface of general high-nickel ternary precursors, which comes from residual lithium compounds after sintering. The residual alkali will react with moisture and carbon dioxide in the air, not only easily causing the positive electrode slurry to gel "jelly", but also high moisture content will easily cause battery bloating, thereby deteriorating cycle stability and safety.

[0003] At present, the conventional solution is water washing, but water washing will destroy the surface chemical structure of the ternary positive electrode material and seriously deteriorate the cycle life. Therefore, the industry is moving towards the direction of "no water washing", such as pure coating, single element or multi-element co-doping, coating combined with doping, etc. The coating method is to coat other inorganic or organic compounds using a dry or wet method. The coating wraps the surface of the ternary positive electrode material or even the grain boundary to prevent the side reaction between the electrolyte and the ternary positive electrode material; element doping generally uses a wet method or solid phase sintering method to dope the element into the ternary positive electrode material lattice; however, a single element doping or a single coating is not enough to completely solve the problem of attenuation and safety of the ternary positive electrode material.

[0004] In order to exert the synergistic effect, the ternary cathode material can be coated and doped with elements at the same time. Generally, element doping is performed first and then coating is performed. However, this method has a relatively long process, which not only results in high cost and uncontrollable product quality, but also the non-in-situ coating will cause the electronic resistance and ion transport resistance of the ternary cathode material to increase. It has been reported that element doping and coating can be performed simultaneously in a one-step method, but the one-step method realizes element doping and coating under liquid or semi-liquid phase conditions. Such a process is relatively complicated and costly, and it is mainly surface doping, not bulk doping, and the effect is limited. Summary of the invention

[0005] The purpose of the present application is to provide a ternary positive electrode material and a preparation method, and a lithium-ion battery, aiming to solve the technical problem of how to achieve bulk doping of metal elements or reduce surface alkalinity while coating the ternary positive electrode material.

[0006] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0007] In a first aspect, the present application provides a method for preparing a ternary positive electrode material, comprising:

[0008] The ternary cathode material precursor, lithium salt and doping metal source are mixed to obtain a mixed material; wherein the doping metal source is selected from oxides and / or hydroxides of doping metals, the doping metal source contains at least two doping metals, and the total amount of doping metals is calculated based on the remaining amount after being doped in the ternary cathode material precursor;

[0009] The mixed material is sintered to obtain a ternary positive electrode material.

[0010] In one embodiment, the general formula of the ternary cathode material precursor is Ni x Co y Mn 1-x-y (OH) z ; Among them, 0.85≤x≤0.90, 0≤y≤0.15, x+y≤1.0, 1.8≤z≤2.2;

[0011] The ratio of the total molar amount of nickel, cobalt and manganese to the total molar amount of the doped metal element in the obtained ternary positive electrode material is n:m, and 0<1-n<m<0.05.

[0012] In one embodiment, the molar ratio of the total molar amount of nickel, cobalt and manganese in the ternary positive electrode material precursor to the lithium element in the lithium salt is (1:1.01) to (1:1.05).

[0013] In one embodiment, the doping metal in the doping metal source is selected from at least two of aluminum, niobium and tantalum.

[0014] In one embodiment, when the doping metal includes aluminum, the doping metal source corresponding to the aluminum is selected from at least one of aluminum oxide and aluminum hydroxide;

[0015] When the doping metal includes niobium, the doping metal source corresponding to the niobium element is selected from at least one of niobium oxide and niobium hydroxide;

[0016] When the doping metal includes tantalum, the doping metal source corresponding to the tantalum is selected from at least one of tantalum oxide and tantalum hydroxide.

[0017] In one embodiment, the lithium salt is selected from at least one of lithium hydroxide and lithium carbonate.

[0018] In one embodiment, the step of sintering the mixed material comprises: placing the mixed material in a sintering furnace, first keeping the temperature at 490-600° C. for 3-5 hours, then heating to 700-800° C. for 8-20 hours; and / or,

[0019] The mixing treatment of the ternary positive electrode material precursor, the lithium salt and the doped metal source includes: mechanically mixing the ternary positive electrode material precursor, the lithium salt and the doped metal source.

[0020] In one embodiment, the mixed material is placed in a sintering furnace, and oxygen atmosphere is introduced into the sintering furnace for sintering; and / or,

[0021] The heating rate to 700-800°C is 2-5°C / min.

[0022] In a second aspect, the present application provides a ternary positive electrode material, which is prepared by the preparation method of the ternary positive electrode material of the present application.

[0023] In a third aspect, the present application provides a lithium-ion battery, wherein the positive electrode of the lithium-ion battery uses a ternary positive electrode material prepared by the preparation method of the present application.

[0024] The preparation method of the ternary positive electrode material provided in the first aspect of the present application adopts a one-step pure solid phase method to simultaneously realize the metal element doping and coating preparation of the ternary positive electrode material. Specifically, the ternary positive electrode material precursor, lithium salt and doping metal source (selected from metal-doped oxides and / or hydroxides, containing at least two doping metals, and the total amount of doping metal is calculated by the remaining amount after being doped in the ternary positive electrode material precursor) are mixed and sintered to obtain the ternary positive electrode material. No solvent is present in the process, and multiple metal elements can be doped into the ternary positive electrode material precursor body and surface at the same time, thereby greatly strengthening the binding force between transition metal ions and oxygen atoms to improve the cycle stability. In addition, the excess doping metal elements react with the residual alkali on the surface to form a dense coating layer, so that not only the residual lithium salt on the surface can be converted to reduce the alkalinity, but also the coating layer can effectively prevent the electrolyte from contacting the ternary positive electrode material to reduce the side reaction. Therefore, the ternary positive electrode material obtained by the preparation method of the present application has a good doping effect, can significantly improve the cycle stability, and has a good application prospect in lithium-ion batteries.

[0025] The ternary positive electrode material provided in the second aspect of the present application is prepared by a preparation method of a ternary positive electrode material unique to the present application. Based on the preparation method, the metal element doping and coating layer preparation of the ternary positive electrode material can be simultaneously realized in a pure solid phase in one step. Therefore, the ternary positive electrode material provided by the present application has a good doping effect, can significantly improve the cycle stability, and has a good application prospect in lithium-ion batteries.

[0026] The positive electrode of the lithium-ion battery provided in the third aspect of the present application uses a ternary positive electrode material prepared by the preparation method of the ternary positive electrode material unique to the present application. Based on this preparation method, the metal element doping and coating layer preparation of the ternary positive electrode material can be simultaneously achieved in a pure solid phase in one step. Therefore, the ternary positive electrode material used in the lithium-ion battery provided by the present application has a good doping effect, and such a lithium-ion battery can significantly improve the cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 is the X-ray diffraction pattern of the ternary cathode material prepared in Example 1 of the present application;

[0029] Figure 2 This is the aluminum element mapping diagram of the scanning electron microscope EDX test after ion milling and slicing of the ternary positive electrode material prepared in Example 1 of the present application;

[0030] Figure 3 1 is a performance diagram of a button-type battery assembled with a ternary positive electrode material prepared in Example 1 of the present application, a is a charge-discharge curve of the 2nd, 40th and 210th cycles at 0.5C, and b is a discharge curve corresponding to each cycle;

[0031] Figure 4 1 is a performance diagram of a button-type battery assembled with a ternary positive electrode material prepared in Example 2 of the present application, a is a charge-discharge curve of the 2nd, 74th and 200th cycles at 0.5C, and b is a discharge curve corresponding to each cycle;

[0032] Figure 5 3 is a performance diagram of a button-type battery assembled with a ternary positive electrode material prepared in Example 3 of the present application, a is a charge-discharge curve of the 2nd, 100th and 180th cycles at 0.5C, and b is a discharge curve corresponding to each cycle;

[0033] Figure 6The discharge curve corresponding to each cycle of the button-type battery assembled with the ternary positive electrode material prepared in Example 4 of the present application at 0.5C;

[0034] Figure 7 The discharge curve corresponding to each cycle of the button-type battery assembled with the ternary positive electrode material prepared in Example 5 of the present application at 0.5C;

[0035] Figure 8 The discharge curve corresponding to each cycle of the button-type battery assembled with the ternary positive electrode material prepared in Example 6 of the present application at 0.5C;

[0036] Fig. 9 The performance diagram of button-type batteries assembled with ternary positive electrode materials prepared in Comparative Example 1 of the present application, a is the charge-discharge curves of the 2nd, 100th and 180th cycles at 0.5C, and b is the discharge curve corresponding to each cycle;

[0037] Fig.10 The performance diagram of button-type batteries assembled with ternary positive electrode materials prepared in comparative example 2 of the present application, a is the charge-discharge curves of the 2nd, 100th and 180th cycles at 0.5C, and b is the discharge curve corresponding to each cycle;

[0038] Fig.11 The discharge curve corresponding to each cycle of the button-type battery assembled with the ternary positive electrode material prepared in Comparative Example 3 of the present application at 0.5C;

[0039] Fig.12 This is a performance diagram of a button-type battery assembled with the ternary positive electrode material prepared in comparative example 4 of the present application, wherein a is the charge and discharge curve of the 2nd, 100th and 180th cycles at 0.5C, and b is the discharge curve corresponding to each cycle. DETAILED DESCRIPTION

[0040] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0041] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0042] In the present application, "at least one" means one or more, "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items.

[0043] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0044] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0045] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0046] The first aspect of the present application provides a method for preparing a ternary positive electrode material, comprising the following steps:

[0047] S01: mixing a ternary cathode material precursor, a lithium salt and a doping metal source to obtain a mixed material; wherein the doping metal source is selected from oxides and / or hydroxides of doping metals, the doping metal source contains at least two doping metals, and the total amount of the doping metal is calculated based on the remaining amount after being doped in the ternary cathode material precursor;

[0048] S02: Sintering the mixed material to obtain a ternary positive electrode material.

[0049] The embodiment of the present application adopts a one-step pure solid phase method to simultaneously realize the metal element doping and coating preparation of the ternary positive electrode material. Specifically, the preparation method of the ternary positive electrode material provided in the embodiment of the present application is to mix the ternary positive electrode material precursor, the lithium salt and the above-mentioned specially selected doping metal source and then sinter to obtain the ternary positive electrode material. No solvent is present in the process, and multiple metal elements can be doped into the ternary positive electrode material precursor body and surface at the same time, thereby greatly strengthening the binding force between the transition metal ions and the oxygen atoms to improve the cycle stability. In addition, the excess doped metal elements react with the residual alkali on the surface to form a dense coating layer, which can not only convert the residual lithium salt on the surface to reduce the alkalinity, but also the coating layer can effectively block the electrolyte from contacting the ternary positive electrode material to reduce side reactions. Therefore, the ternary positive electrode material obtained by the preparation method of the present application has a good doping effect, can significantly improve the cycle stability, and has a good application prospect in lithium-ion batteries.

[0050] In one embodiment, the ternary positive electrode material precursor is a nickel-cobalt-manganese ternary positive electrode material precursor, and the prepared ternary positive electrode material is a nickel-cobalt-manganese ternary positive electrode material.

[0051] Specifically, the general formula of the nickel-cobalt-manganese ternary cathode material precursor is Ni x Co y Mn 1-x-y (OH) z ; Wherein, 0.85≤x≤0.90, 0≤y≤0.15, x+y≤1.0, 1.8≤z≤2.2; Wherein, x can be 0.86, 0.87, 0.89, etc., x can be 0.1, 0.12, 0.13, 0.14, etc., and z can be 1.9, 2.0, 2.1, 2.2, etc. The embodiment of the present application uses such a ternary cathode material precursor as a raw material to prepare a high-nickel ternary cathode material. Therefore, the high-nickel ternary cathode material with high specific capacity, high working voltage and compaction density can further improve its cycle stability and safety. The ratio of the total molar amount of nickel (Ni), cobalt (Co), and manganese (Mn) in the obtained ternary positive electrode material to the total molar amount of the doped metal element is n:m, and 0<1-n<m<0.05. Under such a ratio range, the doped metal element is not only doped in the body and surface of the ternary positive electrode material, but also has a residual amount and a residual alkali (OH - , CO 3 2-) reaction, thereby having the effect of reducing the residual alkali content. For example, taking the ratio of the total molar amount of nickel, cobalt, and manganese in the ternary positive electrode material to the total molar amount of the doped metal element as 0.96:0.043, the doped metal is doped in a molar amount of 0.04 parts in the body and surface of the ternary positive electrode material with a total molar amount of 0.96 parts of nickel, cobalt, and manganese, and the remaining 0.003 parts (0.043-0.04=0.003) of the doped metal element and the residual alkali (OH) on the surface of the ternary positive electrode material - , CO 3 2- )reaction.

[0052] In one embodiment, the total molar ratio of nickel, cobalt and manganese in the ternary cathode material precursor to the lithium element in the lithium salt is (1:1.01) to (1:1.05), such as 1:1.02, 1:1.03, 1:1.04, etc. Under the above ratio conditions, a nickel-cobalt-manganese oxide ternary cathode material can be prepared and used in a lithium ion battery. Furthermore, the above lithium salt can be selected from at least one of lithium hydroxide and lithium carbonate.

[0053] In one embodiment, the doping metal in the doping metal source is selected from at least two of aluminum (Al), niobium (Nb) and tantalum (Ta). Specifically, when the doping metal includes aluminum, the doping metal source corresponding to the aluminum is selected from at least one of aluminum oxide and aluminum hydroxide; when the doping metal includes niobium, the doping metal source corresponding to the niobium is selected from at least one of niobium oxide and niobium hydroxide; when the doping metal includes tantalum, the doping metal source corresponding to the tantalum is selected from at least one of tantalum oxide and tantalum hydroxide. By selecting two or more of the above doping metal sources, two or more of the metal doping among aluminum, niobium and tantalum can be achieved.

[0054] The embodiment of the present application uses Al, Nb, and Ta elements for doping, which can better stabilize the binding force between the transition metal layer and the O layer, reduce the phase change during the cycle, and thus reduce the fragmentation and oxygen evolution. Calculations can prove that the change in the formation energy of the ternary positive electrode material molecules after doping with 10000ppm of metal elements is as follows: 0.89 Co 0.04 Mn 0.07 O 2 For example, the change of molecular formation energy of ternary cathode materials, after Al, Ta, Nb, W, Mg are doped with 10000ppm of metal elements, the LiNi 0.89 Co 0.04 Mn 0.07 O 2The changes in the formation energy of the ternary cathode material molecules are shown in Table 1. According to the principles of thermodynamics, the more the formation energy is reduced, the more stable the structure is after element doping. Therefore, the formation energy of aluminum, tantalum, and niobium elements is reduced more than that of magnesium and tungsten elements, and the structure is more stable.

[0055] Table 1 LiNi 0.89 Co 0.04 Mn 0.07 O 2 Changes in the formation energy of molecules after doping with metal elements

[0056] Doping elements Doping amount (ppm) Change in formation energy (eV) Aluminum (Al) 10000 -3.01 Tantalum (Ta) 10000 -4.52 Niobium (Nb) 10000 -3.32 Tungsten (W) 10000 0.02 Magnesium (Mg) 10000 -0.30

[0057] Furthermore, the doping metal sources of Al, Nb and Ta are selected from oxides and / or hydroxides of doping metals. The ternary positive electrode material at full charge contains a large amount of Ni 4+ , which has extremely strong oxidizing properties and will cause side reactions when in direct contact with the electrolyte. In the embodiment of the present application, a coating layer is formed by reacting the metal-doped oxide with the residual lithium salt on the surface under high-temperature sintering conditions, and the coating prevents the electrolyte from directly contacting the ternary positive electrode material, thereby reducing side reactions; and the metal-doped metal oxide can reduce the residual alkali after reacting with the residual lithium salt on the surface. The reduction of the residual alkali can not only improve the processability of the material, but also improve the cycle life and safety of the subsequent battery.

[0058] In one embodiment, the step of sintering the mixed material includes: placing the mixed material in a sintering furnace, first keeping it at 490-600°C for 3-5 hours, and then heating it to 700-800°C for 8-20 hours. Specifically, such as keeping it at 500°C, 520°C, 540°C, 550°C, 580°C or 600°C for 3 hours, 3.5 hours, 4 hours or 5 hours, and then heating it to 700°C, 750°C, 760°C, 780°C or 800°C for 8 hours, 9 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours or 20 hours. The above sintering process can better perform pre-lithiation and crystal growth, and after sintering, crushing and refining, a ternary positive electrode material product is obtained.

[0059] Furthermore, an oxygen atmosphere is introduced into the sintering furnace, the oxygen flow rate may be 200-400 sccm, and the heating rate to 700-800°C is 2-5°C / min. For example, the heating rate is 2°C / min, 3°C / min, 4°C / min, 5°C / min, etc. Under the above conditions, oxidation sintering can be performed more stably.

[0060] In one embodiment, the step of mixing the ternary cathode material precursor, the lithium salt and the doping metal source includes: mechanically mixing the ternary cathode material precursor, the lithium salt and the doping metal source, for example, first mechanically mixing the ternary cathode material precursor and the lithium salt, and then adding the doping metal source for second mechanical mixing. The first mechanical mixing can be mixing by a blender or a ball mill, and the precursor aggregate structure is not broken during the mixing process; the second mechanical mixing can be mixing by a blender or a ball mill, and the precursor aggregate structure is not broken during the mixing process.

[0061] In one embodiment, a method for preparing a ternary positive electrode material includes the following steps:

[0062] Step 1: The ternary cathode material precursor and lithium hydroxide monohydrate are mechanically mixed uniformly, including but not limited to a high-speed mixer and a ball mill, and the precursor agglomerate structure is not broken during the mechanical mixing process. The total molar amount of nickel, cobalt and manganese in the ternary cathode material precursor and the molar ratio of lithium element in lithium hydroxide monohydrate are between (1:1.01) and (1:1.05).

[0063] A certain amount of doping metal source (metal oxide and / or metal hydroxide) is added to the mixture obtained above, and then mechanically mixed evenly, including but not limited to a high-speed stirrer and a ball mill, and the precursor agglomerate structure is not destroyed during the mechanical mixing process. The doping metal elements are two or three of Al, Nb, and Ta, and the total molar amount of Ni, Co, and Mn in the final ternary positive electrode material is n:m with a total molar amount of Al / Nb / Ta doped metal elements, and 0<1-n<m<0.05.

[0064] Step 2: The mixture obtained in step 1 is sintered at high temperature in steps, and an oxygen atmosphere is passed through the sintering furnace, which includes a tube furnace and a box furnace. The high temperature sintering specifically includes: keeping the temperature at 490-600°C for 3-5 hours to pre-lithiate and remove crystal water, and then keeping the temperature at 700-800°C for 8-20 hours to grow crystals. The heating rate is 2-5°C / min, and the cooling rate is 2-5°C / min.

[0065] A second aspect of an embodiment of the present application provides a ternary positive electrode material, which is prepared by the preparation method of the ternary positive electrode material of the embodiment of the present application.

[0066] The ternary positive electrode material provided in the embodiment of the present application is prepared by the preparation method of the ternary positive electrode material unique to the embodiment of the present application. Based on the preparation method, the metal element doping and coating layer preparation of the ternary positive electrode material can be simultaneously realized in one step in a pure solid phase. Therefore, the ternary positive electrode material provided in the embodiment of the present application has a good doping effect, can significantly improve the cycle stability, and has a good application prospect in lithium-ion batteries.

[0067] A third aspect of an embodiment of the present application further provides a lithium-ion battery, wherein the positive electrode of the lithium-ion battery uses a ternary positive electrode material prepared by the above-mentioned preparation method of an embodiment of the present application.

[0068] The positive electrode of the lithium-ion battery provided in the embodiment of the present application uses a ternary positive electrode material prepared by the preparation method of the ternary positive electrode material unique to the present application. Based on this preparation method, the metal element doping and coating layer preparation of the ternary positive electrode material can be simultaneously achieved in a pure solid phase in one step. Therefore, in the lithium-ion battery provided in the embodiment of the present application, the ternary positive electrode material used has a good doping effect, and such a lithium-ion battery can significantly improve the cycle stability.

[0069] The following describes the invention in conjunction with specific embodiments.

[0070] Example 1

[0071] A method for preparing a ternary positive electrode material comprises the following steps:

[0072] S11: 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high-nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first evenly mixed, wherein the total molar amount of nickel, cobalt and manganese in the ternary positive electrode material precursor and the molar ratio of lithium in the lithium salt are 1:1.04. The above mixed powder is evenly mixed with niobium oxide and aluminum hydroxide weighed in proportion to obtain a mixed material, according to the total molar ratio of Ni, Co, Mn to Al, Nb of 0.965:0.0316:0.0062, and the excess doped metal cations react with residual alkali to construct an oxide coating layer.

[0073] S12: The mixed material prepared above was placed in a tube furnace for sintering. The first sintering temperature was 500°C, pure oxygen atmosphere was passed, the oxygen flow rate was 400sccm, and the sintering time was 4 hours, pre-lithiation and removal of crystal water. The second sintering temperature was 730°C, pure oxygen atmosphere was passed, the oxygen flow rate was 500sccm, and the sintering time was 12 hours, which promoted the completion of lithiation and crystal growth. The heating and cooling rates were both 5°C / min.

[0074] The sintered sample is crushed and refined without destroying the structure of the agglomerates, and finally a ternary positive electrode material is prepared.

[0075] The X-ray diffraction pattern of the ternary positive electrode material prepared in this example (scanning speed is 5° / min) is as follows: Figure 1 As shown in PDF card LiNiO 2 (PDF#85-1966) characteristic peak phase composite. FIB-SEM characterization test, Figure 2 This is the mapping diagram of the Al element in the EDX test after slicing, where the white spots represent the Al element. From the figure, it can be seen that the doped metal elements form a dense coating layer on the surface, and the Al ions are evenly distributed inside the material. Combined with the solid nuclear magnetic resonance test, it shows that the aluminum ions have entered the material body after high-temperature sintering. The ternary positive electrode material prepared above is prepared into a positive electrode, where the mass ratio of the ternary positive electrode material: conductive agent: binder is 92:5:3, and assembled into a button battery. Figure 3 The electrochemical performance test results show that the maximum capacity reaches 195.2 mAh g at 0.5C charge and discharge cycle at room temperature (25-27°C). -1 After 210 cycles, the discharge capacity is 174.3 mAhg -1 , the capacity retention rate is 89.3%, and the cycle is very stable.

[0076] Example 2

[0077] A method for preparing a ternary positive electrode material comprises the following steps:

[0078] S21: 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first uniformly mixed, wherein the molar ratio of lithium hydroxide to the ternary precursor nickel, cobalt and manganese is 1.05: 1. Then the mixed powder is uniformly mixed with niobium oxide and aluminum hydroxide weighed in proportion to obtain a mixed material, according to the total molar ratio of Ni, Co, Mn to Al, Nb being 0.955: 0.043: 0.0052, and the excess doped metal cations react with the residual alkali to construct the oxide coating layer.

[0079] S22:The mixed material prepared above was placed in a tube furnace for sintering. The first sintering temperature was 500°C, pure oxygen atmosphere was passed, the oxygen flow rate was 200 sccm, and the sintering time was 4 hours, pre-lithiation and removal of crystal water. The second sintering temperature was 750°C, pure oxygen atmosphere was passed, the oxygen flow rate was 500 sccm, and the sintering time was 12 hours, which promoted the completion of lithiation and crystal growth. The heating and cooling rates were both 5°C / min.

[0080] The sintered sample is crushed and refined without destroying the structure of the agglomerate, and finally a ternary positive electrode material is prepared.

[0081] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Figure 4 The electrochemical performance test results show that the maximum capacity reaches 191.6 mAh g at 0.5C charge and discharge cycle at room temperature. -1 After 200 cycles, the discharge capacity is 185.1 mAh g -1 , the capacity retention rate is 96.6%, and the cycle is very stable.

[0082] Example 3

[0083] A method for preparing a ternary positive electrode material comprises the following steps:

[0084] S31: 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first uniformly mixed, wherein the molar ratio of lithium hydroxide to the ternary precursor nickel, cobalt and manganese is 1.04: 1. The above mixed powder is uniformly mixed with niobium oxide and aluminum hydroxide weighed in proportion to obtain a mixed material, according to the total molar ratio of Ni, Co, Mn to Al, Nb of 0.96: 0.032: 0.011, and the excess doped metal cations react with residual alkali to construct an oxide coating layer.

[0085] S32: The mixed material prepared above was placed in a tube furnace for sintering. The first sintering temperature was 500°C, pure oxygen atmosphere was passed, the oxygen flow rate was 200 sccm, and the sintering time was 4 hours, pre-lithiation and removal of crystal water. The second sintering temperature was 750°C, pure oxygen atmosphere was passed, the oxygen flow rate was 500 sccm, and the sintering time was 12 hours, which promoted the completion of lithiation and crystal growth. The heating and cooling rates were both 5°C / min.

[0086] The sintered sample is crushed and refined without destroying the structure of the agglomerates, and finally a ternary positive electrode material is prepared.

[0087] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Figure 5 The electrochemical performance test results show that the maximum capacity reaches 182.0 mAh g at 0.5C charge and discharge cycle at room temperature. -1 About 200 cycles, the discharge capacity is 171.1 mAhg -1 , the capacity retention rate is 94.0%, and the cycle is very stable.

[0088] Example 4

[0089] A method for preparing a ternary positive electrode material comprises the following steps:

[0090] S41: 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first uniformly mixed, wherein the molar ratio of lithium hydroxide to the ternary precursor nickel, cobalt and manganese is 1.05: 1. Then the mixed powder is uniformly mixed with weighed niobium oxide and tantalum oxide to obtain a mixed material, according to the total molar ratio of Ni, Co, Mn to Ta, Nb is 0.99: 0.0053: 0.0053, and the excess doped metal cations react with the residual base to construct the oxide coating layer.

[0091] S41: The mixed material prepared above was placed in a tube furnace for sintering. The first sintering temperature was 500°C, pure oxygen atmosphere was passed, the oxygen flow rate was 200 sccm, and the sintering time was 4 hours to remove crystal water and pre-lithiation. The second sintering temperature was 750°C, pure oxygen atmosphere was passed, the oxygen flow rate was 500 sccm, and the sintering time was 12 hours to promote the completion of lithiation and crystal growth. The heating and cooling rates were both 5°C / min.

[0092] The sintered sample is crushed and refined without destroying the structure of the agglomerates, and finally a ternary positive electrode material is prepared.

[0093] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Figure 6 The electrochemical performance test results show that the maximum capacity reaches 185.3 mAh g at 0.5C charge and discharge cycle at room temperature. -1 After 180 cycles, the discharge capacity is 169.4 mAhg -1 , the capacity retention rate is 91.4%, and the cycle is stable.

[0094] Example 5

[0095] A method for preparing a ternary positive electrode material comprises the following steps:

[0096] S51: 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first uniformly mixed, wherein the molar ratio of lithium hydroxide to the ternary precursor nickel, cobalt and manganese is 1.04: 1. Then the mixed powder is uniformly mixed with weighed niobium oxide and tantalum oxide to obtain a mixed material, according to the total molar ratio of Ni, Co, Mn to Ta, Nb is 0.98: 0.013: 0.013, and the excess doped metal cations react with the residual base to construct the oxide coating layer.

[0097] S52: The mixed material prepared above was placed in a tube furnace for sintering. The first sintering temperature was 500°C, pure oxygen atmosphere was passed, the oxygen flow rate was 200 sccm, and the sintering time was 4 hours to remove crystal water and pre-lithiation. The second sintering temperature was 750°C, pure oxygen atmosphere was passed, the oxygen flow rate was 500 sccm, and the sintering time was 12 hours to promote the completion of lithiation and crystal growth. The heating and cooling rates were both 5°C / min.

[0098] The sintered sample is crushed and refined without destroying the structure of the agglomerates, and finally a ternary positive electrode material is prepared.

[0099] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Figure 7 The electrochemical performance test results show that the maximum capacity reaches 190.1 mAh g at 0.5C charge and discharge cycle at room temperature. -1 After 200 cycles, the discharge capacity is 174.4 mAhg -1 , the capacity retention rate is 91.7%, and the cycle is very stable.

[0100] Example 6

[0101] A method for preparing a ternary positive electrode material comprises the following steps:

[0102] S61: 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2The high nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first uniformly mixed, wherein the molar ratio of lithium hydroxide to the ternary precursor nickel, cobalt and manganese is 1.04: 1. Then the mixed powder is further uniformly mixed with two of the weighed tantalum oxide and aluminum hydroxide, according to the total molar ratio of Ni, Co, Mn to Al, Ta of 0.985: 0.015: 0.008, and the excess doped metal cations react with the residual base to construct the oxide coating layer.

[0103] S62: The mixed material prepared above was placed in a tube furnace for sintering. The first sintering temperature was 500°C, pure oxygen atmosphere was passed, the oxygen flow rate was 200 sccm, and the sintering time was 4 hours to remove crystal water and pre-lithiation. The second sintering temperature was 750°C, pure oxygen atmosphere was passed, the oxygen flow rate was 500 sccm, and the sintering time was 12 hours to promote the completion of lithiation and crystal growth. The heating and cooling rates were both 5°C / min.

[0104] The sintered sample is crushed and refined without destroying the structure of the agglomerates, and finally a ternary positive electrode material is prepared.

[0105] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Figure 8 The electrochemical performance test results show that the maximum capacity reaches 192.5 mAh g at 0.5 C charge and discharge cycle at room temperature. -1 About 200 cycles, the discharge capacity is 175.0 mAhg -1 , the capacity retention rate is 90.9%, and the cycle is very stable.

[0106] Comparative Example 1

[0107] A method for preparing a ternary positive electrode material comprises the following steps:

[0108] 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high-nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first evenly mixed, wherein the molar ratio of lithium hydroxide to the ternary precursor nickel, cobalt and manganese is 1.04:1. The above-prepared mixture is sintered in a tubular furnace: the first sintering temperature is 500°C, a pure oxygen atmosphere is passed, the oxygen flow rate is 200sccm, and the sintering time is 4 hours to remove crystal water and pre-lithiation. The second sintering temperature is 750°C, a pure oxygen atmosphere is passed, the oxygen flow rate is 500sccm, and the sintering time is 12 hours to promote the completion of lithiation and crystal growth. The heating and cooling rates are both 5°C / min. The sintered sample is crushed and refined, but the structure of the agglomerate is not destroyed, and LiNi is finally prepared.0.89 Co 0.04 Mn 0.07 O 2 Ternary positive electrode material.

[0109] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Fig. 9 The electrochemical performance test results show that the maximum capacity reaches 198.2 mAh g at 0.5C charge and discharge cycle at room temperature. -1 After 180 cycles, the discharge capacity is 117.8 mAhg -1 , the capacity retention rate is only 59.7%. Without multi-element doping or coating, the capacity retention rate is very low.

[0110] Comparative Example 2

[0111] A method for preparing a ternary positive electrode material comprises the following steps:

[0112] 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high-nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first evenly mixed, wherein the molar ratio of lithium hydroxide to the ternary precursor nickel, cobalt and manganese is 1.05:1. Then the above mixed powder is evenly mixed with the weighed aluminum hydroxide to obtain a mixed material, wherein the total molar ratio of Ni, Co, and Mn to Al in the ternary precursor is 0.96:0.04. The mixed material is sintered in a tubular furnace: the first sintering temperature is 500°C, pure oxygen atmosphere is passed, the oxygen flow rate is 200sccm, and the sintering time is 4 hours to remove crystal water and pre-lithiation. The second sintering temperature is 750°C, pure oxygen atmosphere is passed, the oxygen flow rate is 500sccm, and the sintering time is 12 hours to promote the completion of lithiation and crystal growth. The heating and cooling rates are both 5°C / min.

[0113] The sintered sample was crushed and refined without destroying the structure of the agglomerate, and finally Li a (Ni 0.89 Co 0.04 Mn 0.07 ) 0.96 Al 0.04 O 2 Ternary positive electrode material.

[0114] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Fig.10The electrochemical performance test results show that the maximum capacity reaches 184.5 mAh g at 0.5 C charge and discharge cycle at room temperature. -1 After 180 cycles, the discharge capacity is 150.9 mAhg -1 The capacity retention rate is 81.8%, and the cycle stability is average.

[0115] Comparative Example 3

[0116] A method for preparing a ternary positive electrode material comprises the following steps:

[0117] 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high-nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first evenly mixed, wherein the molar ratio of lithium hydroxide to the ternary precursor nickel, cobalt and manganese is 1.05:1. Then the mixed powder is evenly mixed with the weighed niobium oxide to obtain a mixed material, wherein the total molar ratio of Ni, Co, and Mn to Nb in the ternary precursor is 0.99:0.01. The mixed material is sintered in a tubular furnace: the first sintering temperature is 500°C, pure oxygen atmosphere is passed, the oxygen flow rate is 200sccm, and the sintering time is 4 hours to remove crystal water and pre-lithiation. The second sintering temperature is 750°C, pure oxygen atmosphere is passed, the oxygen flow rate is 500sccm, and the sintering time is 12 hours to promote the completion of lithiation and crystal growth. The heating and cooling rates are both 5°C / min.

[0118] The sintered sample was crushed and refined without destroying the structure of the agglomerate, and finally Li a (Ni 0.89 Co 0.04 Mn 0.07 ) 0.99 Nb 0.01 O 2 Ternary positive electrode material.

[0119] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Fig.11 The electrochemical performance test results show that the maximum capacity reaches 184.5 mAh g at 0.5 C charge and discharge cycle at room temperature. -1 After 180 cycles, the discharge capacity is 150.9 mAhg -1 The capacity retention rate is 81.8%, and the cycle stability is average.

[0120] Comparative Example 4

[0121] In contrast, a method for preparing a ternary positive electrode material by wet synthesis includes the following steps:

[0122] S71: 9.165 g (Ni 0.89 Co 0.04 Mn 0.07 )(OH) 2 The high-nickel ternary precursor and 4.402 grams of lithium hydroxide monohydrate are first evenly mixed, wherein the total molar ratio of nickel, cobalt and manganese in the ternary positive electrode material precursor to the lithium element in the lithium salt is 1:1.04, and it is placed in 100ml of deionized water and continuously stirred magnetically. Then aluminum sulfate and ammonium niobate oxalate are added, wherein the total molar ratio of Ni, Co, and Mn in the ternary precursor to Al and Nb is 0.965:0.0316:0.0062, and the excess doped metal cations react with the residual alkali to construct the oxide coating layer. Heat while stirring magnetically until drying.

[0123] S72: The mixed material prepared above was placed in a tube furnace for sintering. The first sintering temperature was 500°C, pure oxygen atmosphere was passed, the oxygen flow rate was 400sccm, and the sintering time was 4 hours, pre-lithiation and removal of crystal water. The second sintering temperature was 730°C, pure oxygen atmosphere was passed, the oxygen flow rate was 500sccm, and the sintering time was 12 hours, which promoted the completion of lithiation and crystal growth. The heating and cooling rates were both 5°C / min.

[0124] Finally, a ternary positive electrode material is prepared.

[0125] The ternary positive electrode material prepared above is prepared into a positive electrode, wherein the mass ratio of the ternary positive electrode material: the conductive agent: the binder is 92:5:3, and assembled into a button cell, Fig.12 The electrochemical performance test results show that the maximum capacity reaches 180.5 mAh g at 0.5 C charge and discharge cycle at room temperature. -1 After 180 cycles, the discharge capacity is 140.0 mAhg -1 , the capacity retention rate is 77.5%, which is very low.

[0126] Residual alkali test

[0127] In addition, the residual alkali of the embodiment and the comparative example was tested, and the results are shown in Table 2. The residual alkali content of the ternary positive electrode material prepared in the embodiment of the present application (tested by Swiss Metrohm 916Ti-Touch automatic point titrator) is significantly lower than that of the comparative example. In the comparative example, no extra metal elements are used for doping, and the residual alkali content is high.

[0128] Table 2 Residual alkali content of ternary positive electrode materials

[0129]

[0130]

[0131] It can be seen from the above examples and comparative examples that the preparation method of the pure solid phase multi-element doping and alkali removal and coating ternary positive electrode material of the present invention can improve the cycle stability of the ternary positive electrode material; it can significantly reduce the residual alkali (OH - , CO 3 2- )content.

[0132] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a ternary positive electrode material, characterized in that: include: The ternary cathode material precursor, lithium salt and doping metal source are mixed to obtain a mixed material; wherein the doping metal source is selected from oxides and / or hydroxides of doping metals, the doping metal source contains at least two doping metals, and the total amount of the doping metals is calculated based on the remaining amount after being doped in the ternary cathode material precursor; The mixed material is sintered to obtain a ternary positive electrode material; the mixed material is sintered including: placing the mixed material in a sintering furnace, first keeping the temperature at 490-600° C. for 3-5 hours, then heating to 700-800° C. for 8-20 hours; The doping metal in the doping metal source is selected from aluminum and niobium, and the ternary positive electrode material precursor is Ni 0.89 Co 0.04 Mn 0.07 (OH)2; the molar ratio of the total molar amount of nickel, cobalt and manganese in the obtained ternary positive electrode material to the aluminum element and the niobium element is 0.955:0.043:0.0052; the molar ratio of the total molar amount of nickel, cobalt and manganese in the ternary positive electrode material precursor to the lithium element in the lithium salt is 1:1.

05.

2. The preparation method according to claim 1, characterized in that The doping metal source corresponding to the aluminum element is selected from at least one of aluminum oxide and aluminum hydroxide; The doping metal source corresponding to the niobium element is selected from at least one of niobium oxide and niobium hydroxide.

3. The preparation method according to claim 1, characterized in that: The lithium salt is selected from at least one of lithium hydroxide and lithium carbonate.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The mixing treatment of the ternary positive electrode material precursor, the lithium salt and the doping metal source includes: mechanically mixing the ternary positive electrode material precursor, the lithium salt and the doping metal source.

5. The preparation method according to claim 4, characterized in that: placing the mixed material in a sintering furnace, introducing an oxygen atmosphere into the sintering furnace for sintering; and / or, The heating rate to 700-800° C. is 2-5° C. / min.

6. A ternary positive electrode material, characterized in that: The ternary positive electrode material is prepared by the preparation method described in any one of claims 1-5.

7. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery uses a ternary positive electrode material prepared by the preparation method according to any one of claims 1 to 5.