A kind of low carbon concrete and preparation method thereof

By using a combination of composite admixtures and polycarboxylic acid water reducing agents in fly ash, the activity of fly ash and blast furnace slag is stimulated, and the problem of low early strength of fly ash is solved, achieving the improvement of early strength of concrete and cement Reduced dosage.

CN117024074BActive Publication Date: 2024-11-12XINJIANG CONSTR RES INST (CO LTD) +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202311008759.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-11
Publication Date
2024-11-12
Estimated Expiration
2043-08-11

AI Technical Summary

Technical Problem

Fly ash has low early strength in concrete and requires activation pretreatment to improve its utilization, but this process is complex and time-consuming, affecting the early performance of concrete.

Method used

Compound admixtures, including dopamine, resorcinol, small molecule alcohol amine compounds and amino silicone oil, use wet grinding to refine the surface layer of fly ash to stimulate its activity, combine with polycarboxylic acid water reducing agent to improve fly ash The doping effect of blast furnace slag reduces the amount of cement and enhances the early strength of concrete.

Benefits of technology

It significantly improves the doping effect of fly ash and blast furnace slag, reduces the amount of cement, improves the early strength of concrete, and enhances the dispersion ability of cement particles through the coordination effect of phenols and alcohols, and promotes the Early hydration of cement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117024074B_ABST
    Figure CN117024074B_ABST
Patent Text Reader

Abstract

The invention discloses a low-carbon concrete and a preparation method thereof, comprising the following components: 180-200 parts of silicate cement, 50-80 parts of blast furnace slag powder, 70-100 parts of fly ash, 600-900 parts of sand, 1000-1100 parts of stone, 240-380 parts of stone powder, 120-200 parts of water, 5-20 parts of composite admixture, and 5-10 parts of polycarboxylic acid water reducer; the composite admixture comprises: 5-10% dopamine, 1-3% resorcinol, 1-3% small molecule alcohol amine compound, 0.5-1.5% amino silicone oil, 0.1-0.5% hexadecyl trimethyl ammonium hydroxide, and the balance is water. The admixture plays the role of reducing glue and water, while improving the early doping efficiency of fly ash and improving the early strength of concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of concrete materials, and in particular relates to low-carbon concrete and a preparation method thereof. Background Art

[0002] Fly ash can replace cement and be added to concrete, which can not only improve the resource utilization rate of solid waste, but also reduce the heat release of cement hydration, improve the mechanical and durability of concrete, and have both technical and economic benefits. Fly ash mainly contains stable substances such as aluminum silicate glass, tricalcium aluminate, mullite, calcite, sodalite and spinel ferrite. Since the polymerization degree of these substances is very high, it takes a long activation process after adding cement to react with calcium hydroxide released during the cement maturation process to achieve the effect of strengthening concrete. Therefore, in the early stage of hydration, fly ash only plays a role of physical filling, resulting in low early strength of cement. To improve the utilization rate of fly ash and realize the efficient application of fly ash, it is necessary to activate it beforehand, destroy the dense Si-Al structure on the surface of fly ash, and improve the activity of fly ash. Only after activation can useful substances such as aluminum and iron in fly ash be extracted and utilized. Summary of the invention

[0003] Aiming at how to improve the early strength of concrete mixed with fly ash, the present invention provides a composite admixture, which plays the role of reducing glue and water, and at the same time improves the early mixing efficiency of fly ash and improves the early strength of concrete.

[0004] The object of the present invention is to provide a low-carbon concrete, which comprises the following components calculated by weight:

[0005] 180-200 parts of silicate cement, 50-80 parts of blast furnace slag powder, 70-100 parts of fly ash, 600-900 parts of sand, 1000-1100 parts of stone, 240-380 parts of stone powder, 120-200 parts of water, 5-20 parts of composite admixture, and 5-10 parts of polycarboxylate water reducer.

[0006] The composite admixture comprises: 5-10% dopamine, 1-3% resorcinol, 1-3% small molecule alcohol amine compound, 0.5-1.5% amino silicone oil, 0.1-0.5% hexadecyl trimethyl ammonium hydroxide, and the balance is water.

[0007] The small molecule alcohol amine compound is selected from one or a combination of triethanolamine, triisopropanolamine, butylethanolamine, methyldiethanolamine, N-(3-aminopropyl)diethanolamine, N-phenylethanolamine, N-benzylethanolamine, and tert-butylethanolamine.

[0008] Furthermore, the water-to-binder ratio ranges from 0.3 to 0.5.

[0009] Furthermore, the stone powder is obtained by crushing and grinding rocks, and has a specific surface area of ​​≥400m 2 / g, MB value ≤1, wherein the parent rock of the stone powder includes one or more of limestone, basalt, granite, quartzite, dolomite, and tuff.

[0010] Furthermore, the sand is machine-made sand, with a fineness modulus of 2.3 to 3.2, a content of particles below 0.075 mm of ≥3%, and an MB value of ≤1.

[0011] Furthermore, the maximum particle size of the stone is 25 mm.

[0012] Another object of the present invention is to provide a method for preparing low-carbon concrete, comprising the following steps:

[0013] (3) Add the water reducer and the composite admixture into water, mix well, and add them into a grinding jar together with the fly ash and blast furnace slag powder. Seal the grinding jar, grind at a speed of 400 to 600 rpm for 20 to 40 minutes, filter the obtained slurry, and obtain the ultra-high activity admixture.

[0014] (4) Add sand and gravel aggregates into a concrete mixer and stir for 30 seconds; then add the ultra-high activity admixture and continue stirring for 60 seconds; finally add cement and continue stirring for 90 seconds; after stirring evenly, pour out until the iron plate is moist and free of visible water and set aside.

[0015] Beneficial effects:

[0016] The present invention provides a low-carbon concrete, wherein the composite admixture contained in the concrete has a good coordination effect with a polycarboxylate water-reducing agent, improves the doping effect of fly ash and blast furnace slag, further reduces the amount of cement used, and improves the early strength of concrete. Specifically, the present invention mixes fly ash, blast furnace slag powder with a water-reducing agent and a composite admixture for wet grinding and refining, destroys the surface glass of the fly ash, improves the leaching of valuable elements, and the phenolic substances and alcohol substances in the composite admixture can coordinate with the leached iron ions and aluminum ions, dissolve the surface structure of the fly ash particles, and make the fly ash or blast furnace slag powder release active SiO2 and active Al2O3 faster, thereby stimulating the activity of the fly ash. Compared with alcohol substances, phenolic substances cooperate with water-reducing agents, and due to the steric hindrance, the dispersibility of cement particles is greatly improved, thereby reducing the amount of water and cement. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is the hydration rate of cement paste.

[0018] Figure 2 The heat released by cement paste hydration.

[0019] Figure 3This is the SEM of fly ash admixture. DETAILED DESCRIPTION

[0020] The present invention is further described in detail below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0021] The sources and specifications of some raw materials are as follows

[0022]

[0023] Example 1

[0024] A low-carbon concrete comprises the following ingredients in parts by weight: 200 parts of P.O42.5 silicate cement, 90 parts of fly ash, 60 parts of S95 slag powder, 325 parts of stone powder, 120 parts of water, 800 parts of sand, 1000 parts of small stones, 8 parts of polycarboxylic acid water reducer, and 5 parts of composite admixture.

[0025] The components of the composite admixture are as follows: 8% dopamine, 2% resorcinol, 1% triisopropanolamine, 1% amino silicone oil, 0.3% hexadecyltrimethylammonium hydroxide, and the balance is water.

[0026] The preparation method is as follows:

[0027] (1) Add polycarboxylic acid water reducer and composite admixture into water, mix well, add fly ash and blast furnace slag powder into a grinding jar, seal the grinding jar, grind at a speed of 400 rpm for 30 minutes, filter the obtained slurry, and obtain the ultra-high activity admixture.

[0028] (2) Add sand and gravel aggregates into a concrete mixer and stir for 30 seconds; then add ultra-high activity admixtures and continue stirring for 60 seconds; finally add cement and continue stirring for 90 seconds; after stirring evenly, pour out until the iron plate is moist and free of visible water and set aside.

[0029] Example 2

[0030] A low-carbon concrete comprises the following ingredients in parts by weight: 200 parts of P.O42.5 silicate cement, 90 parts of fly ash, 60 parts of S95 slag powder, 325 parts of stone powder, 120 parts of water, 800 parts of sand, 1000 parts of small stones, 8 parts of polycarboxylic acid water reducer, and 10 parts of composite admixture.

[0031] The components of the composite admixture are as follows: 8% dopamine, 2% resorcinol, 1% triisopropanolamine, 1% amino silicone oil, 0.3% hexadecyltrimethylammonium hydroxide, and the balance is water.

[0032] Example 3

[0033] A low-carbon concrete comprises the following ingredients in parts by weight: 200 parts of P.O42.5 silicate cement, 90 parts of fly ash, 60 parts of S95 slag powder, 325 parts of stone powder, 120 parts of water, 800 parts of sand, 1000 parts of small stones, 8 parts of polycarboxylic acid water reducer, and 20 parts of composite admixture.

[0034] The components of the composite admixture are as follows: 8% dopamine, 2% resorcinol, 1% triisopropanolamine, 1% amino silicone oil, 0.3% hexadecyltrimethylammonium hydroxide, and the balance is water.

[0035] Example 4

[0036] A low-carbon concrete comprises the following ingredients in parts by weight: 180 parts of P.O42.5 silicate cement, 100 parts of fly ash, 80 parts of S95 slag powder, 325 parts of stone powder, 125 parts of water, 800 parts of sand, 1000 parts of small stones, 8 parts of polycarboxylic acid water reducer, and 20 parts of composite admixture.

[0037] The components of the composite admixture are as follows: 8% dopamine, 2% resorcinol, 1% triisopropanolamine, 1% amino silicone oil, 0.3% hexadecyltrimethylammonium hydroxide, and the balance is water.

[0038] Example 5

[0039] A low-carbon concrete comprises the following ingredients in parts by weight: 200 parts of P.O42.5 silicate cement, 90 parts of fly ash, 60 parts of S95 slag powder, 325 parts of stone powder, 155 parts of water, 800 parts of sand, 1000 parts of small stones, 8 parts of polycarboxylic acid water reducer, and 10 parts of composite admixture.

[0040] The components of the composite admixture are as follows: 8% dopamine, 2% resorcinol, 1% triisopropanolamine, 1% amino silicone oil, 0.3% hexadecyltrimethylammonium hydroxide, and the balance is water.

[0041] Example 6

[0042] A low-carbon concrete comprises the following ingredients in parts by weight: 200 parts of P.O42.5 silicate cement, 90 parts of fly ash, 60 parts of S95 slag powder, 325 parts of stone powder, 180 parts of water, 800 parts of sand, 1000 parts of small stones, 8 parts of polycarboxylic acid water reducer, and 10 parts of composite admixture.

[0043] The components of the composite admixture are as follows: 8% dopamine, 2% resorcinol, 1% triisopropanolamine, 1% amino silicone oil, 0.3% hexadecyltrimethylammonium hydroxide, and the balance is water.

[0044] In order to better illustrate the advantages of the present invention, the present invention further provides the following comparative examples.

[0045] Comparative Example 1

[0046] A concrete comprises the following ingredients in parts by weight: 200 parts of P.O42.5 silicate cement, 90 parts of fly ash, 60 parts of S95 slag powder, 325 parts of stone powder, 120 parts of water, 800 parts of sand, 1000 parts of small stones, and 8 parts of polycarboxylic acid water reducer.

[0047] Comparative Example 2

[0048] A concrete comprises the following ingredients in parts by weight: 200 parts of P.O42.5 silicate cement, 90 parts of fly ash, 60 parts of S95 slag powder, 325 parts of stone powder, 120 parts of water, 800 parts of sand, 1000 parts of small stones, and 10 parts of composite admixture.

[0049] The components of the composite admixture are as follows: 8% dopamine, 2% resorcinol, 1% triisopropanolamine, 1% amino silicone oil, 0.3% hexadecyltrimethylammonium hydroxide, and the balance is water.

[0050] Comparative Example 3

[0051] A concrete comprises the following ingredients in parts by weight: 200 parts of P.O42.5 silicate cement, 90 parts of fly ash, 60 parts of S95 slag powder, 325 parts of stone powder, 120 parts of water, 800 parts of sand, and 1000 parts of small stones.

[0052] Comparative Example 4

[0053] A concrete comprising the following ingredients in parts by weight: 350 parts of P.O42.5 silicate cement, 325 parts of stone powder, 120 parts of water, 800 parts of sand, and 1000 parts of small stones.

[0054] Strength test: referring to GB / T 17671-1999 "Test method for strength of cement mortar (ISO method)", the test specimens were cast in a molding room with a temperature of 20±5℃ and RH≥50%. The molded specimens were placed in a curing room with a temperature of 20±2℃ and RH≥90%. After curing for 24 hours, the molds were demoulded. Then the specimens were placed in the curing room for curing until the set age and taken out for compressive strength test.

[0055] The mechanical property test results of Examples 1 to 6 and Comparative Examples 1 to 4 are listed in Table 1.

[0056] Table 1

[0057]

[0058]

[0059] In order to study the effect of composite admixtures on the physical and chemical properties of concrete, the cement paste (water-binder ratio of 0.3) shown in Table 2 was prepared and the following experiments were carried out:

[0060] Setting time test: refer to GB / T1346-2001 "Test method for water consumption, setting time and stability of cement standard consistency", the standard consistency and setting time of cement slurry are listed in Table 3.

[0061] Hydration heat test: TAM air eight-channel hydration calorimeter was used, and the results are shown in the attached Figure 1 and 2 .

[0062] The microstructure of fly ash admixture was analyzed using a JSM-IT300 field emission environmental scanning electron microscope produced by JEOL Ltd. The results are shown in the attached Figure 3 .

[0063] Table 2 (Unit: mass fraction)

[0064]

[0065]

[0066] The composite admixture 1 specifically comprises: 8% dopamine, 2% resorcinol, 1% triisopropanolamine, 1% amino silicone oil, and 0.3% hexadecyltrimethylammonium hydroxide;

[0067] The alcoholamine admixture specifically includes: 1% triisopropanolamine, 1% amino silicone oil, and 0.3% hexadecyltrimethylammonium hydroxide.

[0068] The pure slurries 1 to 4 all adopt wet grinding to first obtain fly ash admixture, and then mix it with cement.

[0069] Table 3

[0070] Sample Standard consistency, % Initial setting time, min Final setting time, min Pure pulp 1 27.9 240 297 Pure pulp 2 27.4 232 280 Pure pulp 3 27.2 230 277 Pure pulp 4 28.2 244 300 Pure pulp 5 28.6 252 312

[0071] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A low-carbon concrete, characterized in that: Calculated by weight, it includes the following components: 180-200 parts of silicate cement, 50-80 parts of blast furnace slag powder, 70-100 parts of fly ash, 600-900 parts of sand, 1000-1100 parts of stone, 240-380 parts of stone powder, 120-200 parts of water, 5-20 parts of composite admixture, and 5-10 parts of polycarboxylate water reducer; The composite admixture comprises: 5-10% dopamine, 1-3% resorcinol, 1-3% small molecule alcohol amine compound, 0.5-1.5% amino silicone oil, 0.1-0.5% hexadecyl trimethyl ammonium hydroxide, and the balance is water; The preparation method comprises the following steps: (1) Add polycarboxylate water reducer and composite admixture into water, mix well, add into grinding jar together with fly ash and blast furnace slag powder, seal the grinding jar, grind at 400-600 rpm for 20-40 min, filter the obtained slurry, and obtain ultra-high activity admixture; (2) Add sand and gravel aggregates into a concrete mixer and stir for 30 seconds; then add ultra-high activity admixtures and continue stirring for 60 seconds; finally add cement and continue stirring for 90 seconds; after stirring evenly, pour out until the iron plate is moist and free of visible water and set aside.

2. A low-carbon concrete according to claim 1, characterized in that: The small molecule alcohol amine compound is selected from one or a combination of triethanolamine, triisopropanolamine, butylethanolamine, methyldiethanolamine, N-(3-aminopropyl)diethanolamine, N-phenylethanolamine, N-benzylethanolamine, and tert-butylethanolamine.

3. A low-carbon concrete according to claim 1, characterized in that: The water-cement ratio of the concrete is in the range of 0.3 to 0.

5.

4. The low-carbon concrete according to claim 1, characterized in that: The stone powder is obtained by crushing and grinding rocks, with a specific surface area of ​​≥400m 2 / g, MB value ≤1, wherein the parent rock of the stone powder includes one or more of limestone, basalt, granite, quartzite, dolomite, and tuff.

5. The low-carbon concrete according to claim 1, characterized in that: The sand is machine-made sand with a fineness modulus of 2.3 to 3.2, a content of particles below 0.075 mm of ≥3%, and an MB value of ≤1.

6. The low-carbon concrete according to claim 1, characterized in that: The maximum particle size of the stone is 25 mm.

Citation Information

Patent Citations

  • Functional protecting surface material with good adhesive performance and preparation method for function protecting surface material

    CN105418821A

  • High-performance concrete with large mixing amount of mineral powder and manufacturing method of high-performance concrete

    CN105645894A

  • Concrete admixture and preparation method thereof as well as concrete containing concrete admixture

    CN106746818A

  • Waste concrete blended type regenerated concrete

    CN108341642A

  • Early strength quick-setting concrete and preparation method thereof

    CN109020373A