A kind of ablation-resistant structure of expansion section outlet
By using a step structure combination of tungsten copper permeable, carbon/carbon back wall and heat insulation in the nozzle outlet area of solid rocket engine, the ablation and fixability problems in high temperature and high pressure environment are solved, and the flame resistance of the nozzle outlet is achieved Corrosiveness and structural stability reduce material requirements and costs.
Patent Information
- Application Number
- CN202211332446.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-10-28
AI Technical Summary
The nozzle outlet area of the existing solid rocket engine is prone to ablation under high temperature and high pressure environment, and the material is poor, resulting in thrust loss and spoiler damage, making it difficult to achieve ablation resistance and structural stability matching.
The step structure combination of tungsten copper permeable, carbon/carbon back wall and heat insulation parts is fixed in the metal shell through bonding, and the high strength and carbonization characteristics of carbon/carbon back wall are used to support tungsten copper permeable, heat insulation parts The step structure limits material displacement and provides a gap between the expansion section liner and tungsten copper to relieve thermal expansion and extrusion.
Effectively prevent ablation of the nozzle outlet, ensure reliable material fixation, reduce material requirements, save costs, avoid thrust loss and spoiler damage, and achieve ablation resistance and structural stability of the nozzle outlet.
Smart Images

Figure CN115573829B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid rocket engines, and more specifically, relates to a thermal protection structure for matching a nozzle outlet area of a solid rocket engine with a gas rudder. Background Art
[0002] Gas rudder technology is a common method for thrust vector control of small and medium-sized solid rocket engines, enabling aircraft to achieve large maneuverable flight. For aircraft that have thrust direction adjustment requirements throughout the entire working section, the gas rudder must ensure that the structure is intact throughout the entire process. Therefore, they are all high-temperature and erosion-resistant non-ablative rudders. Due to their good ablation resistance, the engine nozzle outlet thermal protection structure needs to match the gas rudder ablation to prevent the nozzle structure from burning through. Especially for the spoiler structure (a type of gas rudder) close to the outlet, not only is the nozzle outlet required to have good ablation resistance, but also the thermal protection materials must be reliably positioned to ensure that the material does not move and contact the spoiler to cause motion jamming, and the spoiler must not be damaged due to material blowing out.
[0003] In the early days, a spoiler-type thrust vector structure was adopted. The engine propellant had low performance and was usually aluminum-free or low-aluminum propellant. The combustion temperature was below 3000K, there was little oxidizing atmosphere, and the combustion time was mostly less than 10s. Therefore, no additional thermal protection measures were required at the nozzle outlet. Generally, carbon-based molded and cloth-wrap materials were integrally formed and fixed in the nozzle shell to solve the ablation problem. The fixation was usually at the front end of the nozzle, and there was no risk of fixation at the outlet.
[0004] As the engine performance improves, the propellant performance improves, the oxidizing atmosphere is significantly enhanced, the gas temperature is as high as 3600K, and the aluminum powder content is usually greater than 15%. When the spoiler is working, a high-temperature and high-pressure spoiler zone is formed within a certain range of the nozzle outlet, and the stagnation temperature basically reaches the high temperature of 3600K of the gas. Conventional thermal protection materials, even carbon / carbon materials, cannot achieve the ability to resist ablation. Therefore, only tungsten copper-infiltrated materials with excellent ablation resistance can be used to embed them in the nozzle outlet. At the same time, due to the reduction of the dead weight of the engine structure, the layout of the nozzle outlet and the spoiler is more compact, with only a 1mm gap between the two, which further improves the reliability requirements of the nozzle outlet material fixation.
[0005] At present, most of the solid hair that can be found use tungsten copper as the ablation-resistant material. In addition to being used in gas rudders, it is mainly used in throat structures. Its thermal structure layout from the inside to the outside is tungsten copper, graphite or C / C back wall, and thermal insulation. Three-layer layout (see Figure 1 ), which relies on non-carbonizable carbon-carbon materials as the support of tungsten copper infiltration materials, is a reference for this structure. The tungsten copper infiltration throat liner adopts a "trumpet-shaped" cone structure facing the flow direction. Due to the space allowed by the throat structure, the large drop design of the large and small openings effectively prevents the throat liner from being blown out by the airflow, but it cannot be set in the nozzle outlet area:
[0006] 1) The nozzle outlet is usually less than a quarter of the throat thickness relative to the throat structure, so it is impossible to lay out a large drop cone structure to ensure reliable fixation of the tungsten copper infiltration material, which can easily cause the tungsten copper infiltration to move or fly out;
[0007] 2) Since the expansion area belongs to the high-velocity scouring area, the increase of ablation-resistant materials in the outlet area of the expansion section will inevitably cause abnormal ablation of the upstream materials connected to it, resulting in thrust loss. Summary of the invention
[0008] In order to overcome the deficiencies of the prior art, the present invention provides an ablation-resistant structure for an expansion section outlet, which can solve the problems of nozzle outlet ablation, structural fixation, heat insulation and ablation dimension within a limited space and under economical material application conditions.
[0009] The technical solution adopted by the present invention to solve the technical problem is: an ablation-resistant structure at the outlet of the expansion section, including a tungsten copper infiltration structure, a carbon / carbon back wall, a heat insulation component and an expansion section lining.
[0010] The thermal insulation member is a step column structure with an axial step hole inside, the outer diameter toward the rear end of the engine is smaller than the outer diameter at the other end, the inner diameter toward the rear end of the engine is smaller than the inner diameter at the other end, the outer wall step surface cooperates with the inner wall step surface at the rear end of the engine metal shell to limit the axial displacement of the thermal insulation member; the carbon / carbon back wall is a columnar structure with an axial step hole inside, coaxially fixedly connected to the large end of the step hole of the thermal insulation member, the rear end of the carbon / carbon back wall cooperates with the inner wall step surface of the thermal insulation member to limit the axial displacement of the carbon / carbon back wall; The tungsten copper infiltrated structure is a step column structure with an axial tapered hole inside, which is coaxially fixed to the thermal insulation and the carbon / carbon back wall, and the step surface of the outer wall cooperates with the step surface of the carbon / carbon back wall to limit the axial displacement of the tungsten copper infiltrated structure; the expansion section lining is a column structure with an axial tapered hole inside, the outer wall is fixed to the metal shell, the inner wall and the inner wall of the tungsten copper infiltrated structure together constitute the inner wall profile of the expansion section outlet, and the rear end cooperates with the thermal insulation and the carbon / carbon back wall to limit the axial displacement of the expansion section lining; the gap between the expansion section lining and the tungsten copper infiltrated structure is butted.
[0011] The tungsten copper infiltration, carbon / carbon back wall, heat insulation component and expansion section lining are all fixed by bonding and finally fixed in the metal shell.
[0012] The carbon / carbon back wall is made of needle-punched carbon-carbon material or punctured carbon-carbon material.
[0013] The axial thickness of the carbon-carbon back wall is not less than 6 mm.
[0014] The coverage length of the tungsten-copper-infiltrated structure is the length of the velocity stagnation influence zone caused when the spoiler completely enters the nozzle outlet plus no less than 5 mm.
[0015] The restraining step between the tungsten copper infiltrated structure and the carbon-carbon back wall has a drop of 3.5 mm and is provided with an R2 arc chamfer.
[0016] At the joint surface between the expansion section liner and the tungsten copper infiltrated structure, the inner diameter of the tungsten copper infiltrated structure is larger than the inner diameter of the expansion section liner, forming an airflow step in the direction facing the incoming flow.
[0017] A gap of not less than 0.3 mm is set between the expansion section lining and the tungsten-copper-infiltrated structure; when the working time exceeds 40 seconds, the gap is not less than 0.5 mm.
[0018] The inner diameter of the expansion section lining is 1.2 mm smaller than the inner diameter of the tungsten copper infiltrated structure.
[0019] The expansion section lining is made of a carbon cloth / high silica cloth / phenolic composite winding material, with an inner layer of carbon cloth / phenolic and an outer layer of high silica cloth / phenolic.
[0020] The beneficial effects of the present invention are:
[0021] 1) Tungsten-infiltrated copper 1 uses the same material as the spoiler and has the same ablation rate, which effectively avoids abnormal ablation at the nozzle outlet, solves the difficulty of ablation reliability at the expansion section outlet, and achieves reasonable matching with the ablation of the spoiler structure;
[0022] 2) Drawing on the engine tungsten copper infiltration throat liner structure, the carbon-carbon back wall constrains the tungsten copper infiltration material, and its high strength and non-carburization characteristics form an effective support for the tungsten copper infiltration 1;
[0023] 3) The 90° step structure with mutual restraint between tungsten copper infiltration 1 and carbon / carbon back wall 2 is more reliable in positioning and occupies less structural space than the fixed inclined cone surface, which is beneficial to the structural layout of the nozzle outlet with small wall thickness;
[0024] 4) The truncated carbon / carbon back wall 2 and the "Z"-shaped thermal insulation member 3 ensure the axial strength of the carbon / carbon back wall to the tungsten copper infiltration 1, and also ensure the effect of the high thermal conductivity of the tungsten copper infiltration on the high silicon oxygen thermal insulation member 3;
[0025] 5) The above features 2), 3) and 4) effectively solve the problem of reliable fixation of the tungsten copper infiltrated 1 at the nozzle outlet;
[0026] 6) The structural material selection can maximize the material advantages and functions, using the ablation resistance of tungsten copper infiltration 1, the high strength and low thermal conductivity of carbon / carbon back wall 2, and the thermal insulation performance of thermal insulation 3, and the partitioned combination application, which reduces the material requirements and saves costs;
[0027] 7) The large gap between the expansion section lining 5 and the tungsten copper infiltration 1 reserves space for the volume expansion of the tungsten copper infiltration, effectively alleviates the extrusion between the materials, alleviates its backward movement, and reasonably avoids interference with the 1mm assembly gap spoiler;
[0028] 8) Compared with the increase in the inner diameter of the expansion section liner 5, although the initial expansion profile is discontinuous, the common ablation step effect is effectively suppressed, and the continuity of the expansion profile after ablation is achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the structure of the tungsten-infiltrated copper throat liner in the prior art;
[0030] Figure 2 It is a schematic diagram of an ablation-resistant structure of an expansion section outlet of the present invention;
[0031] In the figure, 1-tungsten infiltrated copper, 2-carbon / carbon back wall, 3-thermal insulation, 4-metal shell, 5-expansion section lining. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with the accompanying drawings and embodiments. The present invention includes but is not limited to the following embodiments.
[0033] like Figure 2 As shown, the present invention provides an ablation-resistant structure for an expansion section outlet, which includes, from the inside to the outside, a tungsten copper infiltrated 1, a carbon / carbon back wall 2, a heat insulating member 3, a metal shell 4 of the outer wall, and a carbon cloth-wrapped expansion section lining 5 adjacent to the tungsten copper infiltrated 1, and each part is a rotating body, which is fixed by bonding and finally fixed in the metal shell.
[0034] The nozzle outlet uses the same tungsten copper-infiltrated 1 material as the spoiler to resist ultra-high temperature ablation. The selection of the same material effectively avoids abnormal ablation on the low ablation rate material side caused by the difference in ablation rates.
[0035] The outer surface of the tungsten copper infiltration 1 adopts a simple step structure at 90 degrees to the horizontal, which cooperates with the carbon-carbon back wall 2 to avoid Figure 1 The fixation of the middle oblique cone takes up a lot of space and is unreliable;
[0036] The carbon / carbon back wall 2 has a 90-degree reverse step structure, which is combined with the tungsten-infiltrated copper 1 to form a "Z"-shaped structure, constraining each other;
[0037] The carbon / carbon back wall 2 material is a carbon-carbon material with a small axial linear expansion, such as a needle-piercing or puncturing carbon-carbon material, to avoid squeezing the thermal insulation 3 and causing the tungsten copper infiltration 1 to move backward;
[0038] In order to ensure that the carbon-carbon back wall 2 serves as the axial support for the tungsten-infiltrated copper 1, its axial thickness should be able to ensure its own structural strength, and the axial thickness should not be less than 6mm;
[0039] The outer wall heat insulation member 3 adopts a "Z"-shaped structure, which relies on the metal shell 4 to fix itself while restricting the displacement of the carbon-carbon back wall 2 and the tungsten-infiltrated copper 1;
[0040] In order to avoid complete axial carbonization of the thermal insulation member 3 (generally not less than 6 m (10 s)), the carbon / carbon back wall 2 is shortened to ensure the axial thickness of the thermal insulation member 3.
[0041] The nozzle outlet structure is the weakest area, and the heat insulation 3 is in direct contact with the tungsten copper infiltrated 1 to ensure the heat insulation of the shell;
[0042] The expansion section liner 5 is connected to the tungsten copper infiltrated surface 1. The inner diameter of the tungsten copper infiltrated surface 1 is larger than the inner diameter of the expansion section liner 5. A flow-oriented step is formed in the direction of the incoming flow to alleviate the ablation of the expansion section liner and avoid local abnormal ablation of the expansion surface, which causes thrust loss.
[0043] The expansion section lining 5 and the tungsten-infiltrated copper 1 are butt-jointed with a gap, leaving space for the tungsten-infiltrated copper 1 to expand forward to avoid damage to the tungsten-infiltrated copper by heat pressure, and at the same time avoiding the tungsten-infiltrated copper from unidirectionally expanding toward the nozzle outlet, causing structural interference with the spoiler.
[0044] The expansion section lining is made of a carbon cloth / high silica cloth / phenolic composite winding material, with an inner layer of carbon cloth / phenolic and an outer layer of high silica cloth / phenolic.
[0045] Take an engine as an example. The engine has an operating pressure of 12 MPa, a working time of 12 seconds, and four Wu-7Cu spoilers are set at the nozzle outlet. To ensure that the nozzle outlet matches the spoiler structure, the following design is made: Figure 2 The structure shown:
[0046] After the three parts of tungsten copper infiltration 1, carbon-carbon back wall 2, and heat insulation 3 are bonded together, the matching surface with the expansion section lining 5 is processed, and then they are bonded and fixed in the metal shell together;
[0047] The tungsten copper infiltrated 1 adopts the same Wu-7Cu material as the spoiler, the carbon-carbon back wall 2 adopts the low-cost needle-punched carbon-carbon material, and the heat insulation 3 adopts the commonly used high-silicon-oxygen molded material;
[0048] The coverage length of tungsten copper infiltration 1 is set according to the length of the velocity stagnation influence zone caused when the spoiler completely enters the nozzle outlet, and should be appropriately lengthened to not less than 5mm;
[0049] When the solid rocket engine is working normally, the carbon-carbon back wall 2 uses its high strength and non-carbonized characteristics and adopts a 90° step structure to effectively restrict the axial displacement of the tungsten-infiltrated copper 1
[0050] The constraint step between the tungsten copper infiltration 1 and the carbon-carbon back wall 2 adopts a 3.5mm drop and an R2 arc chamfer, which not only achieves reliable constraint but also avoids the stress concentration of the sharp corners of the tungsten copper infiltration material;
[0051] The heat insulating element 3 , by virtue of its good heat insulating properties, on the one hand, insulates the nozzle housing, and on the other hand, fixes the carbon-carbon back wall 2 , that is, indirectly fixes the tungsten-infiltrated copper 1 , via the step.
[0052] The axial thickness of the carbon / carbon back wall 2 and the axial thickness of the heat insulation member are 8mm and 7mm respectively to ensure the strength of the carbon / carbon back wall and the insulation thickness of the heat insulation member;
[0053] The gap between the expansion section lining 5 and the tungsten copper infiltration 1 is set to be no less than 0.3mm to alleviate the thermal expansion of the tungsten copper infiltration itself during the test, and avoid thermal structural damage caused by extrusion or spoiler jamming caused by extrusion backward movement. When the time is extended to more than 40s, the gap should be further increased and should be no less than 0.5mm; the gap between the two is naturally formed by the dimensional tolerance and the nozzle shell limiting the two respectively;
[0054] The inner diameter of the expansion section lining 5 is about 1.2 mm smaller than the inner diameter of the tungsten copper infiltrated 1. The diameter difference is set for the purpose of allowing the low ablation rate product to be ablated in advance through thickness balance ablation, and after a certain period of time, it will participate in the ablation together with the ablation-resistant tungsten copper infiltrated 1, thereby shortening the exposure time of the ablation-resistant material and avoiding the discontinuity of the expansion surface caused by excessive ablation of the low ablation rate product due to the difference in ablation rate.
[0055] Through the above measures, the nozzle outlet structure is ablated and matched, and the structure is fixed reliably. The experimental results show that:
[0056] Since there are gaps in front and behind the tungsten-infiltrated copper 1, it expands axially in two directions, which alleviates the extrusion displacement caused by the unidirectional thermal expansion toward the nozzle outlet;
[0057] The uncarbonized amount of the heat insulation member 3 is greater than 2 mm, and the carbon / carbon back wall does not form an indentation on the heat insulation member 3, indicating that the carbon / carbon back wall does not move toward the nozzle outlet and is reliably fixed;
[0058] The inner profile of the expansion section liner 5 is continuous, and there is no abnormal ablation area at the joint with the tungsten-infiltrated copper 1, thereby eliminating the thrust loss factor.
Claims
1. An ablation-resistant structure at the outlet of an expansion section, comprising a tungsten-copper-infiltrated structure, a carbon / carbon back wall, a heat insulation member, and an expansion section inner Lining, characterized in that The thermal insulation member is a step column structure with an axial step hole inside, the outer diameter toward the rear end of the engine is smaller than the outer diameter at the other end, the inner diameter toward the rear end of the engine is smaller than the inner diameter at the other end, the outer wall step surface cooperates with the inner wall step surface at the rear end of the engine metal shell to limit the axial displacement of the thermal insulation member; the carbon / carbon back wall is a columnar structure with an axial step hole inside, coaxially fixedly connected to the large end of the step hole of the thermal insulation member, the rear end of the carbon / carbon back wall cooperates with the inner wall step surface of the thermal insulation member to limit the axial displacement of the carbon / carbon back wall; The tungsten copper infiltrated structure is a step column structure with an axial tapered hole inside, which is coaxially fixed to the thermal insulation and the carbon / carbon back wall, and the step surface of the outer wall cooperates with the step surface of the carbon / carbon back wall to limit the axial displacement of the tungsten copper infiltrated structure; the expansion section lining is a column structure with an axial tapered hole inside, the outer wall is fixed to the metal shell, the inner wall and the inner wall of the tungsten copper infiltrated structure together constitute the inner wall profile of the expansion section outlet, and the rear end cooperates with the thermal insulation and the carbon / carbon back wall to limit the axial displacement of the expansion section lining; the gap between the expansion section lining and the tungsten copper infiltrated structure is butted.
2. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: The tungsten copper infiltration, carbon / carbon back wall, heat insulation component and expansion section lining are all fixed by bonding and finally fixed in the metal shell.
3. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: The carbon / carbon back wall is made of needle-punched carbon-carbon material or punctured carbon-carbon material.
4. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: The axial thickness of the carbon / carbon back wall is not less than 6 mm.
5. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: The coverage length of the tungsten-copper-infiltrated structure is the length of the velocity stagnation influence zone caused when the spoiler completely enters the nozzle outlet plus no less than 5 mm.
6. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: The restraining step between the tungsten copper infiltrated structure and the carbon / carbon back wall has a drop of 3.5 mm and is provided with an R2 arc chamfer.
7. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: At the joint surface between the expansion section liner and the tungsten copper infiltrated structure, the inner diameter of the tungsten copper infiltrated structure is larger than the inner diameter of the expansion section liner, forming an airflow step in the direction facing the incoming flow.
8. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: A gap of not less than 0.3 mm is set between the expansion section lining and the tungsten-copper-infiltrated structure; when the working time exceeds 40 seconds, the gap is not less than 0.5 mm.
9. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: The inner diameter of the expansion section lining is 1.2 mm smaller than the inner diameter of the tungsten copper infiltrated structure.
10. The ablation-resistant structure of the expansion section outlet according to claim 1, characterized in that: The expansion section lining is made of a carbon cloth / high silica cloth / phenolic composite winding material, with an inner layer of carbon cloth / phenolic and an outer layer of high silica cloth / phenolic.