Precursor composition and preparation method thereof, and preparation method of inorganic nanocrystals
By using a gel precursor composition, including cationic and anionic precursors and an organic gel medium, the problems of precursor solubility and environmental impact in the synthesis of inorganic nanocrystals are solved, and the stability and reliability of high-quality inorganic nanocrystals are achieved. Repeatable preparation reduces cost and environmental impact.
Patent Information
- Application Number
- CN202111083434.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-16
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-09-16
AI Technical Summary
The existing technology lacks inorganic element precursors that are soluble in hydrocarbon solvents when synthesizing high-quality inorganic nanocrystals, resulting in complex synthesis and high environmental impact, and it is difficult to achieve the stability and repeatability of high-quality nanocrystals at ambient temperatures. preparation.
Using a gel-like precursor composition including cationic and anionic precursors, a stable precursor composition is formed by mixing an organic gel medium such as petroleum jelly with a hydrocarbon solvent for preparing inorganic nanocrystals, and the precursor is expanded selection range and concentration range, and reduce the impact on the environment.
It achieves stable and reproducible preparation of high-quality inorganic nanocrystals at ambient temperature, reduces production costs and environmental impact, and improves the stability and production efficiency of nanocrystals.
Smart Images

Figure CN115818582B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of colloidal nanocrystal preparation, and in particular, to a precursor composition and a preparation method thereof, and a preparation method of inorganic nanocrystals. Background Art
[0002] The synthetic chemistry of colloidal nanocrystals, especially inorganic nanocrystals, has made significant progress in the past 20 years, promoting their applications in displays, solar cells, biopharmaceutical labels, photocatalysis, etc. In general, in order to ensure single crystal structure, high-quality inorganic nanocrystals are synthesized using cationic and anionic precursors in high-boiling hydrocarbon solvents. Dimethylcadmium, as a typical organometallic precursor, was introduced into the synthesis of cadmium sulfide nanocrystals in the early 1990s, achieving quantum confined structural absorption and sharp band-edge photoluminescence. In the early 21st century, people discovered a "green method" to replace precursors of organometallic crystals, such as replacing dimethylcadmium with cadmium oxide dissolved in fatty acids, which expanded the range of high-quality nanocrystals and reduced their production costs. In hydrocarbon solvents, thioureas and thiocarbonates with different organic groups are soluble in diphenyl ether as co-solvents and have been developed as sulfur precursors for the high-yield synthesis of PbS and CdS nanocrystals. The synthesis of III-V semiconductor nanocrystals is still immature, and exploring suitable precursors has long been regarded as a promising solution. Although these and other developments in precursor chemistry have facilitated the synthesis of colloidal nanocrystals, it still has significant shortcomings in terms of many conflicting requirements, such as the need for precursors to contain inorganic elements and to be soluble in hydrocarbon solvents, as well as the need for stability and controllable reactivity at high temperatures. The increasing need for large-scale production of high-quality nanocrystals in industry, at low cost and in an environmentally friendly manner, has brought further challenges to precursor chemistry. Summary of the invention
[0003] The purpose of the present disclosure is to provide a precursor composition and a preparation method thereof, and a preparation method of inorganic nanocrystals.
[0004] The first aspect of the present disclosure provides a precursor composition, which is used to prepare inorganic nanocrystals and is in a gel state. The precursor composition includes a precursor and an organic gel medium for dispersing the precursor, and the precursor is one or more of a cationic precursor and an anionic precursor.
[0005] Further, the organogel medium includes hydrocarbons of different chain lengths.
[0006] Furthermore, the organogel medium is vaseline.
[0007] Furthermore, the precursor composition also includes a hydrocarbon solvent.
[0008] Furthermore, the hydrocarbon solvent is 1-octadecene.
[0009] Furthermore, the volume ratio of the hydrocarbon solvent to the organic gel medium is less than or equal to 4, preferably 4 / 6 to 7 / 3.
[0010] Furthermore, the boiling point of the hydrocarbon solvent is greater than or equal to 150°C.
[0011] Furthermore, the precursor is selected from one or more of the group consisting of metal hydroxides, metal carbonates, metal carboxylates, metal acetylacetonates, Se powder, S powder or thiourea derivatives.
[0012] Furthermore, the precursor composition also includes an organic ligand compound for preparing inorganic nanocrystals.
[0013] Furthermore, the precursor composition also includes fatty acid.
[0014] Furthermore, the melting point of the fatty acid is less than or equal to 30°C.
[0015] The second aspect of the present disclosure provides a method for preparing any one of the above-mentioned precursor compositions, characterized in that a precursor mixture liquid and a molten organic gel medium are mixed and cooled to obtain the precursor composition.
[0016] Furthermore, the precursor and the hydrocarbon solvent are mixed to obtain a precursor mixture liquid, the molten organic gel medium is added to the precursor mixture liquid, and the mixture is cooled to obtain a precursor composition.
[0017] Furthermore, the temperature of the molten organogel medium is 70-80°C.
[0018] Furthermore, the process of mixing the precursor and the hydrocarbon solvent includes mixing the precursor and the hydrocarbon solvent under one or both of ultrasound and stirring to obtain a precursor mixture liquid.
[0019] Furthermore, the process of mixing the precursor and the hydrocarbon solvent further includes heating the precursor mixture liquid, but the temperature of the precursor mixture liquid is less than 100°C.
[0020] Further, the metal oxide and the fatty acid are mixed and reacted to obtain a precursor mixture liquid.
[0021] Furthermore, the volume ratio of the fatty acid to the molten organogel medium is less than or equal to 0.5.
[0022] Furthermore, any one or more of the above precursor compositions are used to prepare inorganic nanocrystals.
[0023] Furthermore, during the preparation of inorganic nanocrystals, the precursor composition is added to the reaction system multiple times.
[0024] Furthermore, the precursor composition includes metal hydroxide, and the surface ligands of the prepared inorganic nanocrystals include hydroxide.
[0025] At present, high-quality inorganic nanocrystals are only synthesized in hydrocarbon solvents, which is complicated to a large extent due to the lack of simple inorganic element precursors that are soluble in solvents at ambient temperature. The application of the technical solution disclosed in the present invention greatly expands the range of potential precursors and their concentration range, simplifies the synthesis system, minimizes the impact on the environment, and improves the stability or repeatability of the inorganic nanocrystal preparation method. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The drawings constituting part of the present application are used to provide a further understanding of the present disclosure. The exemplary embodiments of the present disclosure and their descriptions are used to explain the present disclosure and do not constitute an improper limitation on the present disclosure. In the drawings:
[0027] Figure 1 The UV-visible absorption and fluorescence emission (PL) spectra of the CdSe nanocrystals prepared in Example 1 are shown.
[0028] Figure 2 The transmission electron microscope (TEM) image of the CdSe nanocrystals prepared in Example 1 is shown.
[0029] Figure 3 These are photos of Se gel precursors with different vaseline volume fractions used in Example 2 after being stored for one week.
[0030] Figure 4 The graph shows the evolution of the UV-visible absorption and PL spectrum of CdSe nanocrystals over time as the Se gel precursor is dropped in Example 2.
[0031] Figure 5 The figure above shows that the absorbance of CdSe nanocrystals at 380 nm changes with the reaction time during the reaction process of Example 2. Figure 5 The figure below shows the change of the fluorescence peak position and half-maximum width (FWHM) of CdSe nanocrystals during the reaction process of Example 2 with the change of reaction time, and the error bar shows the deviation range between five repeated reactions.
[0032] Figure 6 The graph shows the changes in various optical properties during the reaction of Example 2 in 5 sets of repeated experiments.
[0033] Figure 7 The UV-visible absorption and PL spectra of the CdS nanocrystals prepared in Example 3 are shown.
[0034] Figure 8 The UV-visible absorption spectrum of the CdS clusters prepared in Example 3 is shown.
[0035] Fig. 9 The UV-visible absorption and PL spectra of ZnSe nanocrystals of different sizes prepared in Example 4 are shown.
[0036] Fig.10 The fluorescence half-width and fluorescence emission peak position change curves of ZnSe nanocrystals of different sizes prepared in Example 4 are shown.
[0037] Fig.11 The PL spectrum of the ZnSe nanocrystals prepared in Example 5 is shown.
[0038] Fig.12 The TEM image of ZnSe nanocrystals prepared in Example 5 is shown.
[0039] Fig.13 The UV-visible absorption spectrum of the product during the reaction of Example 6 is shown.
[0040] Fig.14 The TEM image of the CdSe nanosheets prepared in Example 6 is shown.
[0041] Fig.15 TEM images of the products during the reaction of Examples 7-8 are shown.
[0042] Fig.16 The UV-visible spectra and PL spectra of the CdSe / CdS and CdSe / CdS / ZnS nanocrystals prepared in Examples 7-8 are shown.
[0043] Fig.17 The transient fluorescence spectra of CdSe / CdS and CdSe / CdS / ZnS nanocrystals prepared in Examples 7-8 are shown.
[0044] Fig.18 The UV-visible spectra and PL spectra of the CdSe core used in Example 9 and the obtained CdSe / ZnSe nanocrystals with different single-shell numbers are shown.
[0045] Fig.19 The PL spectra of the CdSe core used in Example 9 and the CdSe / ZnSe nanocrystals having a monolayer ZnSe shell layer are shown under the same excitation intensity.
[0046] Fig. 20 The TEM image of the CdSe / ZnSe nanocrystal with 7 ZnSe shell layers prepared in Example 9 is shown.
[0047] Fig.21 The UV-visible spectrum of the PbS nanocrystals prepared in Example 10 is shown, and the inset is a TEM photograph thereof.
[0048] Fig. 22 The X-ray diffraction (XRD) pattern of the PbS nanocrystalline powder prepared in Example 10 is shown.
[0049] Fig.23 The XRD pattern of the Fe3O4 nanocrystalline powder prepared in Example 12 is shown.
[0050] Fig.24 The TEM image of Fe3O4 nanocrystals prepared in Example 12 is shown.
[0051] Fig.25 The UV-visible spectra and PL spectra of the nanocrystals obtained by adding different P precursors during the reaction process of Example 13 are shown.
[0052] Fig.26 A photograph of a gel-like precursor composition used in each example is shown.
[0053] Fig. 27 The PL spectra of the nanocrystals obtained in Example 14 and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0054] It should be noted that the following detailed description is illustrative and is intended to provide further explanation to the application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the application belongs. If not otherwise defined, all terms (including technical and scientific terms) in the specification may be defined as those skilled in the art generally understand. Unless clearly defined, the terms defined in the common dictionary may not be interpreted ideally or exaggeratedly. In addition, unless explicitly described to the contrary, the word "including (comprising)" will be understood to mean including the stated elements, but does not exclude any other elements.
[0055] According to the first aspect of the present disclosure, a precursor composition is provided. The precursor composition is used to prepare inorganic nanocrystals and is in a gel state. The precursor composition includes a precursor and an organic gel medium in which the precursor is dispersed. The precursor is one or more of a cationic precursor and an anionic precursor.
[0056] For precursors that are insoluble in the organic gel medium or precursors that can be co-melted with the organic gel medium, the uniform dispersion state of the precursor is fixed by the semi-solidified organic gel medium, which brings the following benefits: the use of the organic gel medium greatly expands the selection range of potential precursors and their concentration range. For example, precursors that cannot be uniformly and stably dispersed in conventional dispersants, or cannot be achieved in high concentrations in conventional dispersants (otherwise it is difficult to disperse uniformly), can be uniformly and stably dispersed through the organic gel medium. The uniformly and stably dispersed precursor composition improves the stability or repeatability of the inorganic nanocrystal preparation method. By introducing the organic gel medium, environmentally hazardous organic solvents (such as TOP) can be partially or completely replaced, thereby reducing the impact on the environment. When preparing inorganic nanocrystals, the organic gel medium becomes part of the reaction medium.
[0057] The main reason why the precursor composition is in gel form is the organic gel medium. The organic gel medium is an organic substance or a mixture of organic substances. The organic gel medium is semi-liquid at low or normal temperature, similar to a gel. The organic gel medium is selected according to actual conditions, such as selecting a suitable viscosity so that the precursor can be evenly dispersed therein. In some preferred embodiments, the viscosity range is the same as that of commercial toothpaste.
[0058] The material of the organic gel medium is not limited, and can be selected according to the angle that it does not adversely affect the nanocrystal synthesis reaction. The organic gel medium can include hydrocarbons of different chain lengths, and these hydrocarbons are in a gel state at low temperature or room temperature (room temperature is less than or equal to 40° C.). For example, long-chain docosane is mixed with liquid dodecane in different proportions, and a certain amount of hexadecane is added as appropriate to obtain an organic gel medium.
[0059] In some embodiments, the boiling point of the organogel medium is greater than or equal to 300° C. In other embodiments, the melting point of the organogel medium is greater than or equal to 60° C. If the organogel medium is a mixture, the boiling point or melting point range falls within the aforementioned range.
[0060] In some embodiments, the organogel medium is vaseline. Vaseline is low in cost and can reduce production costs. The structure and chemical properties of vaseline are similar to the most common solvent (1-octadecene, ODE) used to synthesize high-quality colloidal nanocrystals. When preparing inorganic nanocrystals, vaseline simply becomes part of the reaction solvent after melting and does not affect the reaction.
[0061] The precursor and the molten organic gel medium may be co-meltable or inco-meltable. The precursor is evenly dispersed in the above composition. According to the reaction conditions required for preparing inorganic nanocrystals, the precursor may include one or more, such as both anionic precursors and cationic precursors.
[0062] In some embodiments, the inorganic nanocrystals may be metal nanocrystals or non-metal nanocrystals, the metal nanocrystals may be noble metal nanocrystals, and the non-metal nanocrystals may be semiconductor nanocrystals. When the inorganic nanocrystals are semiconductor nanocrystals, in some embodiments, the cationic precursors include but are not limited to zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate, zinc sulfate, zinc hydroxide, iron acetate, iron acetylacetonate, iron iodide, iron bromide, iron chloride, iron fluoride, iron carbonate, iron cyanide, iron nitrate, iron oxide, iron peroxide, iron perchlorate, iron sulfate, iron hydroxide, cadmium acetate, cadmium hydroxide, cadmium acetylacetonate, cadmium iodide, cadmium bromide, cadmium chloride, cadmium fluoride, cadmium carbonate, cadmium nitrate, cadmium oxide, cadmium perchlorate, cadmium phosphide, cadmium sulfate, mercuric acetate, mercuric iodide, Mercuric bromide, mercuric chloride, mercuric fluoride, mercuric cyanide, mercuric nitrate, mercuric oxide, mercuric perchlorate, mercuric sulfate, mercuric carbonate, mercuric hydroxide, lead acetate, lead bromide, lead chloride, lead fluoride, lead oxide, lead perchlorate, lead nitrate, lead sulfate, lead carbonate, lead hydroxide, tin acetate, tin hydroxide, di(acetylacetonate)tin, tin bromide, tin chloride, tin fluoride, tin oxide, tin sulfate, germanium tetrachloride, germanium oxide, germanium ethoxide, gallium acetylacetonate, gallium chloride, gallium fluoride, gallium oxide, gallium nitrate, gallium sulfate, indium acetate, indium hydroxide, indium chloride, indium oxide, indium nitrate, indium sulfate, thallium acetate, thallium acetylacetonate, thallium chloride, thallium oxide, thallium ethoxide, thallium nitrate, thallium sulfate, and thallium carbonate. Depending on the composition of the nanocrystals to be synthesized, they can be used alone or in combination of at least two of the aforementioned compounds. In other embodiments, the cationic precursor used to synthesize perovskite quantum dots can be any known or future developed precursor, including but not limited to cesium acetate, cesium chloride, and lead acetate.
[0063] When the inorganic nanocrystal is a semiconductor nanocrystal, in some embodiments, the anion precursor includes, but is not limited to, a group V element, a compound containing a group V element, a group VI element, or a compound containing a group VI element. Specific examples may include, but are not limited to, sulfur (S), selenium (Se), selenide, tellurium, telluride, phosphorus (P), arsenic (As), arsenide, nitrogen (N) or nitrogen-containing compounds, hexanethiol, octanethiol, decanethiol, dodecanethiol, hexadecanethiol, thiourea derivatives, thiocarbonate derivatives, mercaptopropylsilane, sulfur-trioctylphosphine (S-TOP), sulfur-tributylphosphine (S-TBP), sulfur-triphenylphosphine (S-TPP), sulfur-trioctylamine (S-TOA), bis(trimethylsilyl)sulfide, ammonium sulfide, sodium sulfide, selenium-trioctylphosphine (Se ... P), selenium-tributylphosphine (Se-TBP), selenium-triphenylphosphine (Se-TPP), tellurium-tributylphosphine (Te-TBP), tellurium-triphenylphosphine (Te-TPP), tri(trimethylsilyl)phosphine, tri(dimethylamino)phosphine, triethylphosphine, tributylphosphine, trioctylphosphine, triphenylphosphine, tricyclohexylphosphine, Li—O—C≡P, Na—O—C≡P, K—O—C≡P, Zn—(O—C≡P)2, Ga—(O—C≡P)3, arsenic oxide, arsenic chloride, arsenic sulfate, arsenic bromide, arsenic iodide, nitrogen oxide, nitric acid, and ammonium nitrate. In other embodiments, an anion precursor is used to synthesize perovskite quantum dots, which can be any known or future developed precursor. The choice of precursor depends on the composition of the nanocrystals to be synthesized, and can be used alone or in combination of at least two compounds.
[0064] In some embodiments, the precursor is a solid powder, and the powder is greater than or equal to 100 mesh. 100 mesh means that there are greater than or equal to 100 mesh holes per inch of the sieve, and the powder is the powder that has passed through the aforementioned sieve, so as to be more evenly dispersed in the organic gel medium.
[0065] The volume ratio of the organogel medium in the composition excluding the precursor can be 100%, that is, the remaining liquid can be absent. In some embodiments, the precursor composition also includes a hydrocarbon solvent. The hydrocarbon solvent is a liquid, and the hydrocarbon solvent may include C6-C40 aliphatic hydrocarbons (e.g., alkanes, alkenes or alkynes), such as hexadecane, octadecane, octadecene, squalane, etc.; C6-C30 aromatic hydrocarbons such as phenyldodecane, phenyltetradecane, phenylhexadecane, etc.; C12-C22 aromatic ethers such as phenyl ether, benzyl ether, etc.; and combinations thereof.
[0066] In some preferred embodiments, the hydrocarbon solvent is 1-octadecene (ODE). In some embodiments, the volume ratio of the hydrocarbon solvent (i.e., ODE) to the organic gel medium is less than or equal to 4, preferably 4 / 6 to 7 / 3. The proportion of the organic gel medium affects the viscosity of the composition and also affects the uniform dispersion stability of the precursor. Within the aforementioned range, the viscosity and dispersion stability of the composition are both good. The precursor composition within the aforementioned preferred ratio can be stable for several days or even weeks, which is beneficial to the stability of the raw materials in the production process and is particularly suitable for the reaction of adding the precursor in batches during the synthesis of nanocrystals. If the hydrocarbon solvent is other compounds, the ratio of the hydrocarbon solvent to the organic gel medium is optimized according to the actual selection, so as to synthesize higher quality nanocrystals.
[0067] In some embodiments, the melting point of the hydrocarbon solvent is less than or equal to 25° C. In other embodiments, the boiling point of the hydrocarbon solvent is greater than or equal to 150° C. or greater than or equal to 250° C. to accommodate the reaction of preparing inorganic nanocrystals at high temperature.
[0068] In some preferred embodiments, the precursor is one or more of the group consisting of metal hydroxides, metal carbonates, metal carboxylates, acetylacetonate metal salts, Se powder, S powder or thiourea derivatives. When preparing nanocrystals, when the precursor is a metal hydroxide, the hydroxide anion reacts with H2Se and H2S (typical active precursors converted from elemental selenium and sulfur) to form H2O as a byproduct, which is therefore a better inorganic ligand, while the byproduct of chloride is harmful corrosive HCl. The metal carboxylates can be acetates, stearates, oleates, etc.
[0069] When preparing nanocrystals, precursors such as metal chlorides and fluorides can act as small ligands to promote the growth of face-controlled inorganic nanocrystals by releasing the strain of surface carboxylate ligands.
[0070] In some embodiments, the metal element in the above-mentioned precursor is selected from one or more of cadmium, zinc, magnesium, mercury, aluminum, gallium, indium, and lead.
[0071] In some embodiments, the thiourea derivative includes N,N'-di-n-butylthiourea, N-di-n-butyl, and N'-butylthiourea. Other derivatives can be found in the literature "A tunable library of substituted thiourea precursors to metal sulfide nanocrystals", DOI: 10.1126 / science.aaa2951.
[0072] In some embodiments, the precursor composition also includes an organic ligand compound for preparing inorganic nanocrystals. Examples of organic ligand compounds may include, but are not limited to, methyl mercaptan, ethyl mercaptan, propyl mercaptan, butyl mercaptan, pentyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecanethiol, hexadecyl mercaptan, octadecyl mercaptan, benzyl mercaptan, methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, dodecylamine, hexadecylamine, octadecylamine, dimethylamine, diethylamine, dipropylamine, formic acid, acetic acid, propionic acid, butyric acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecyl acid, oleic acid, benzoic acid, phosphine such as substituted or unsubstituted methyl phosphine (e.g., trimethyl phosphine, methyl diphenyl phosphine, etc.), substituted or unsubstituted ethyl phosphine (e.g., triethyl phosphine, ethyl diphenyl phosphine, etc.) ), substituted or unsubstituted propyl phosphine, substituted or unsubstituted butyl phosphine, substituted or unsubstituted pentyl phosphine, substituted or unsubstituted octyl phosphine (e.g., trioctyl phosphine), etc., phosphine oxide compounds such as substituted or unsubstituted methyl phosphine oxide (e.g., trimethyl phosphine oxide, methyl diphenyl phosphine oxide, etc.), substituted or unsubstituted ethyl phosphine oxide (e.g., triethyl phosphine oxide, ethyl diphenyl phosphine oxide, etc.), substituted or unsubstituted propyl phosphine oxide, substituted or unsubstituted butyl phosphine oxide, substituted or unsubstituted octyl phosphine oxide (e.g., trioctyl phosphine oxide, etc.), diphenyl phosphine compounds, triphenyl phosphine compounds, oxide compounds thereof, etc., and phosphonic acid. The organic ligand compound can be used alone or as a combination of at least two of the aforementioned compounds. Preferably, the organic ligand compound is liquid at room temperature.
[0073] In some embodiments, the precursor composition further comprises fatty acid. For example, Se element, oleic acid and vaseline are mixed to obtain a gel precursor composition.
[0074] In some embodiments, the precursor composition further includes fatty acids, which can be used as ligand raw materials for nanocrystals. In other embodiments, the raw materials of the cationic precursor and fatty acids can react to obtain the cationic precursor, but the fatty acids are excessive, and the precursor composition obtained at this time also includes excess fatty acids.
[0075] In some embodiments, the fatty acid comprises one or more of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid, and benzoic acid.
[0076] In some embodiments, the melting point of the fatty acid is 30°C or less.
[0077] According to a second aspect of the present disclosure, a method for preparing the above-mentioned precursor composition is provided, wherein a precursor mixture liquid and a molten organic gel medium are mixed and cooled to obtain the precursor composition.
[0078] In some embodiments, a precursor and a hydrocarbon solvent are mixed to obtain a precursor mixture liquid, a molten organogel medium is added to the precursor mixture liquid, and the mixture is cooled to obtain a precursor composition.
[0079] In some embodiments, the cooling rate is greater than or equal to 1.5° C. / s to form a gel in which the precursor is evenly dispersed. The faster the cooling rate, the better.
[0080] In some embodiments, the temperature of the molten organogel medium is 70-80°C.
[0081] In some embodiments, the process of mixing the precursor and the hydrocarbon solvent includes mixing the precursor and the hydrocarbon solvent under one or both of ultrasound and stirring to obtain a precursor mixture liquid. Both ultrasound and stirring can accelerate dispersion and improve the dispersibility of the precursor in the mixture. The time required for ultrasound can be determined according to actual conditions. It should be noted that the "precursor mixture liquid" does not require that the precursor is 100% dissolved in the solvent, and can be a suspension.
[0082] In some embodiments, the process of mixing the precursor and the hydrocarbon solvent is performed at room temperature. In some embodiments, the process of mixing the precursor and the hydrocarbon solvent further comprises heating the liquid precursor mixture, but the temperature of the liquid precursor mixture is less than 100° C. to promote the dispersion of the precursor.
[0083] In some embodiments, metal oxide and fatty acid are mixed and reacted to obtain a precursor mixture liquid. The precursor mixture liquid includes metal fatty acid salt.
[0084] The optimization can be performed based on the types of organogel medium and fatty acid actually selected. In some embodiments, the volume ratio of the molten organogel medium to the fatty acid is greater than or equal to 0.5, preferably greater than or equal to 0.9.
[0085] According to the third aspect of the present disclosure, a method for preparing inorganic nanocrystals is provided, and any one or more of the above-mentioned precursor compositions are used to prepare inorganic nanocrystals. The above-mentioned precursor compositions can be used to synthesize high-quality inorganic nanocrystals. For precursors that are insoluble in an organic gel medium or precursors that can be fused with an organic gel medium, the uniform dispersion state of the precursor is fixed by a semi-solidified organic gel medium, thereby bringing the following benefits: the organic gel medium greatly expands the selection range of potential precursors and their concentration range, can improve the convenience of production, and reduce production costs. For example, precursors that cannot be uniformly and stably dispersed in conventional dispersants, or cannot be achieved in high concentrations in conventional dispersants (otherwise it is difficult to disperse uniformly), can be uniformly and stably dispersed through organic gel media. Uniformly and stably dispersed precursors improve the stability or repeatability of the method for preparing inorganic nanocrystals. By introducing an organic gel medium, partially or completely replacing environmentally hazardous organic solvents (such as TOP), the impact on the environment can be reduced.
[0086] In some embodiments, during the preparation of inorganic nanocrystals, the precursor composition is added to the reaction system multiple times. The precursor of the conventional suspension is prone to sedimentation and cannot be evenly dispersed. The amount of the precursor added each time cannot be completely consistent, resulting in a decrease in the controllability of the reaction. The use of the above-mentioned precursor composition can achieve automatic addition without worrying about inconsistent addition amounts, thereby improving production efficiency and nanocrystal quality.
[0087] In some embodiments, the volume ratio of ODE in the precursor composition to the organogel medium is less than or equal to 4, preferably 4 / 6 to 7 / 3, to improve the stability of the uniform dispersion of the precursor composition before use and improve the accuracy of subsequent sampling.
[0088] In some embodiments, the precursor composition includes a metal hydroxide, and the surface ligand of the prepared inorganic nanocrystal includes hydroxide. Nanocrystals with hydroxide as the surface ligand can be prepared using a precursor composition containing a metal hydroxide and vaseline, and the obtained nanocrystals have a higher quantum yield (QY).
[0089] Nanocrystal can be prepared by wet chemical method, and nanocrystal can have other organic ligand compounds on which the surface is coordinated. Ligand compound can be any suitable organic ligand compound known in the art and is not particularly limited. For example, organic ligand compound can comprise formula RCOOH, RNH2, R2NH, R3N, RSH, RH2PO, R2HPO, R3PO, RH2P, R2HP, R3P, ROH, RCOOR', RPO(OH)2 or the compound of R2POOH, wherein R and R' are C1-C24 alkyl, C2-C24 alkenyl or C6-C20 aryl or its combination independently. Organic ligand compound can be coordinated to the surface of nanocrystal as prepared, strengthens the dispersion of nanocrystal in solution, and it can have effect on the luminescence and electrical characteristics of nanocrystal. Examples of the organic ligand compound may include, but are not limited to, methyl mercaptan, ethyl mercaptan, propyl mercaptan, butyl mercaptan, pentyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecanethiol, hexadecyl mercaptan, octadecyl mercaptan, benzyl mercaptan, methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, dodecylamine, hexadecylamine, octadecylamine, dimethylamine, diethylamine, dipropylamine, formic acid, acetic acid, propionic acid, butyric acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecyl acid, oleic acid, benzoic acid, phosphine such as substituted or unsubstituted methyl phosphine (e.g., trimethyl phosphine, methyl diphenyl phosphine, etc.), substituted or unsubstituted ethyl phosphine (e.g., triethyl phosphine, ethyl diphenyl phosphine, etc. ), substituted or unsubstituted propyl phosphine, substituted or unsubstituted butyl phosphine, substituted or unsubstituted pentyl phosphine, substituted or unsubstituted octyl phosphine (e.g., trioctyl phosphine), etc., phosphine oxide compounds such as substituted or unsubstituted methyl phosphine oxide (e.g., trimethyl phosphine oxide, methyl diphenyl phosphine oxide, etc.), substituted or unsubstituted ethyl phosphine oxide (e.g., triethyl phosphine oxide, ethyl diphenyl phosphine oxide, etc.), substituted or unsubstituted propyl phosphine oxide, substituted or unsubstituted butyl phosphine oxide, substituted or unsubstituted octyl phosphine oxide (e.g., trioctyl phosphine oxide, etc.), diphenyl phosphine compounds, triphenyl phosphine compounds, oxide compounds thereof, etc., and phosphonic acid. The organic ligand compound may be used alone or as a combination of at least two of the aforementioned compounds.
[0090] Another aspect of the present disclosure provides a semiconductor nanocrystal, the surface ligands of the semiconductor nanocrystal have more than 15% hydroxide (calculated by the number of all ligands). This semiconductor nanocrystal has a higher quantum yield. The surface ligands of the semiconductor nanocrystal have 15%-20%, 20%-30%, 20%-40%, 20%-50%, 20%-60%, 20%-70%, 20%-80%, 20%-90% or 20%-100% hydroxide ligands. In some embodiments, the semiconductor nanocrystal with hydroxide ligands is cubic. In some embodiments, the nanocrystal with hydroxide ligands is CdSe / CdS or CdSe / CdS / ZnS, and the surface ligands of the semiconductor nanocrystal have 20%±1% hydroxide.
[0091] In some preferred embodiments, the fluorescence half-peak width of the semiconductor nanocrystal is less than or equal to 30 nm, or less than or equal to 25 nm, or less than or equal to 20 nm, or less than or equal to 15 nm, but greater than 10 nm.
[0092] Semiconductor nanocrystals of the present disclosure may include one or more semiconductor materials. The examples of semiconductor materials that may be included in semiconductor nanocrystals (including, for example, semiconductor nanocrystals) include but are not limited to IV group elements, II-VI group compounds, II-V group compounds, III-VI group compounds, III-V group compounds, IV-VI group compounds, I-III-VI group compounds, II-IV-VI group compounds, II-IV-V group compounds, alloys including any of the foregoing, and / or mixtures including any of the foregoing, including ternary and quaternary mixtures or alloys. Non-limiting examples of embodiments include ZnO, ZnS, ZnSe, ZnTe, CdO, CdS, CdSe, CdTe, MgS, MgSe, GaAs, GaN, GaP, GaSe, GaSb, HgO, HgS, HgSe, HgTe, InAs, InN, InP, InSb, AlAs, AlN, AlP, AlSb, TlN, TlP, TlAs, TlSb, PbO, PbS, PbSe, PbTe, Ge, Si, alloys comprising any of the foregoing, and / or mixtures comprising any of the foregoing, including ternary and quaternary mixtures or alloys.
[0093] In certain preferred embodiments, the semiconductor nanocrystal according to the present disclosure may include a core comprising one or more semiconductor materials, and a shell comprising one or more semiconductor materials, wherein the shell is arranged on at least a portion of the core and preferably all outer surfaces. The semiconductor nanocrystal comprising a core and a shell is also referred to as a "core-shell" structure.
[0094] For example, the semiconductor nanocrystal may include a core having the chemical formula MX, wherein M is cadmium, zinc, magnesium, mercury, aluminum, gallium, indium, thallium, or a mixture thereof, and X is oxygen, sulfur, selenium, tellurium, nitrogen, phosphorus, arsenic, antimony, or a mixture thereof. Examples of materials suitable for use as semiconductor nanocrystal cores include, but are not limited to, ZnO, ZnS, ZnSe, ZnTe, CdO, CdS, CdSe, CdTe, MgS, MgSe, GaAs, GaN, GaP, GaSe, GaSb, HgO, HgS, HgSe, HgTe, InAs, InN, InP, InSb, AlAs, AlN, AlP, AlSb, TlN, TlP, TlAs, TlSb, PbO, PbS, PbSe, PbTe, Ge, Si, alloys comprising any of the foregoing, and / or mixtures comprising any of the foregoing, including ternary and quaternary mixtures or alloys.
[0095] The shell can be a semiconductor material having the same or different composition from the core. The shell can include a coating including one or more semiconductor materials on the core surface. The examples of semiconductor materials that can be included in the shell include but are not limited to IV group elements, II-VI group compounds, II-V group compounds, III-VI group compounds, III-V group compounds, IV-VI group compounds, I-III-VI group compounds, II-IV-VI group compounds, II-IV-V group compounds, alloys including any of the foregoing, and / or mixtures including any of the foregoing, including ternary and quaternary mixtures or alloys. Examples include, but are not limited to, ZnO, ZnS, ZnSe, ZnTe, CdO, CdS, CdSe, CdTe, MgS, MgSe, GaAs, GaN, GaP, GaSe, GaSb, HgO, HgS, HgSe, HgTe, InAs, InN, InP, InSb, AlAs, AlN, AlP, AlSb, TlN, TlP, TlAs, TlSb, PbO, PbS, PbSe, PbTe, Ge, Si, alloys comprising any of the foregoing, and / or mixtures comprising any of the foregoing. For example, a ZnS, ZnSe or CdS shell layer (protective layer, overcoating) can be grown on a CdSe or CdTe semiconductor nanocrystal.
[0096] In core-shell semiconductor nanocrystals, the shell may comprise one or more layers. The shell may comprise at least one semiconductor material that is the same as or different from the composition of the core. The shell may have a thickness of about 1 to about 10 monolayers. The shell may also have a thickness greater than 10 monolayers. In certain embodiments, more than one shell may be included on the core. By adjusting the temperature of the reaction mixture during coating and monitoring the absorption spectrum of the core, a shell with high emission quantum efficiency and narrow size distribution may be obtained.
[0097] In certain embodiments, the surrounding "shell" material may have a band gap that is greater than the band gap of the core material. In certain other embodiments, the surrounding shell material may have a band gap that is less than the band gap of the core material.
[0098] In certain preferred embodiments, the core-shell semiconductor nanocrystals have a type I structure.
[0099] Examples of semiconductor nanocrystal core-shell structures include, but are not limited to: red QDs, for example, CdSe / CdZnS (core / shell), CdSe / ZnS / CdZnS (core / shell / shell); green QDs, for example, CdZnSe / CdZnS (core / shell), CdSe / ZnS / CdZnS (core / shell / shell); blue QDs, for example, CdS / CdZnS (core / shell).
[0100] Semiconductor nanocrystals can have a variety of shapes, including but not limited to spheres, rods, disks, flakes, other shapes, and mixtures of particles of various shapes.
[0101] In certain preferred embodiments of the various aspects of the disclosure described herein, the semiconductor nanocrystals are undoped.
[0102] As used herein, "undoped semiconductor nanocrystal" refers to a semiconductor nanocrystal that emits light due to quantum confinement without emission from an activator species.
[0103] In certain preferred embodiments of various aspects of the disclosure described herein, the semiconductor nanocrystal comprises a core comprising a first semiconductor material, and at least a first shell surrounding the core, wherein the first shell comprises a second semiconductor material. In certain such embodiments, the thickness of the first shell is greater than or equal to the thickness of 1 monolayer of the second semiconductor material. In certain such embodiments, the thickness of the first shell can reach the thickness of about 10 monolayers of the second semiconductor material.
[0104] In certain preferred embodiments, the semiconductor nanocrystal may include a second shell surrounding its outer surface. In certain such embodiments, the second shell may include a third semiconductor material.
[0105] Hereinafter, the embodiments are described in more detail with reference to specific examples. However, they are illustrative examples of the present disclosure, and the present disclosure is not limited thereto.
[0106] Chemicals used
[0107] Cadmium acetate dihydrate (Cd(Ac)2·2H2O, 98+%), cadmium oxide (CdO, 99.998%), zinc hydroxide (Zn5(OH)6(CO3)2, ≥58%, based on zinc), selenium powder (Selenium, 200 mesh, 99.999%), 1-octadecene (ODE, 90%), lauric acid (99.5%), oleic acid (HOl, 90%), and oleylamine (≥98%) were purchased from Sigma Aldrich. Zinc acetate dehydrate (Zn(Ac)2·2H2O, >98%), indium acetate (In(Ac)3, 99.99%, based on metal), indium acetylacetonate (In(Acac)3, 98%), lead acetate trihydrate (Pb(Ac)2·3H2O), stearic acid (HSt, >98%), decanoic acid (HCa, 99%), sulfur powder (S, 99.98%), tetramethylammonium hydroxide (98%), N,N'-di-n-butylthiourea (99%), and n-dodecane (99%) were purchased from Alfa Aesar. Cadmium hydroxide (Cd(OH)2, 98.5%) was purchased from Aladdin. Zinc acetylacetonate (Zn(Acac)2, 98%) was purchased from Macklin. (TMS)3P (10% by weight in hexane, >98%) was purchased from Stream Chemicals. All organic solvents were purchased from Sinopharm Chemical Reagents. All chemicals were used directly without further purification.
[0108] Preparation of Cadmium Stearate
[0109] Cadmium acetate dihydrate (10mmol) was dissolved in methanol (20mL) in a 50mL flask. In another flask (500mL), stearic acid (20mmol) and tetramethylammonium hydroxide (20mmol) were dissolved in 100mL methanol by stirring for 20min. Under vigorous stirring, cadmium acetate solution was added dropwise to the solution. White precipitate indicated the formation of cadmium stearate, and after adding cadmium acetate solution, stirring was continued for 20min. The precipitate was separated by filtration and washed three times with methanol. The final precipitate was vacuum dried overnight at room temperature before use.
[0110] Preparation of lead oleate
[0111] Lead acetate trihydrate (10mmol) is dissolved in the methanol (20mL) in the flask. In another flask (500mL), oleic acid (20mmol) and tetramethylammonium hydroxide (20mmol) are dissolved in 100mL methanol by stirring for 20min. Under vigorous stirring, lead acetate solution is added dropwise to the solution. White precipitate shows the formation of lead oleate, and after adding lead acetate solution, stirring is continued for 20min. Filter and separate the precipitation and wash three times with methanol. The final precipitate is vacuum dried overnight at room temperature before use.
[0112] Optical property measurement methods
[0113] UV-Vis spectra were obtained on an Analytik Jena S600 UV-Vis spectrophotometer. PL spectra were recorded on an Edinburgh Instruments FLS920. PL decay kinetics were measured on a time-correlated single photon counting (TCSPC) fluorescence spectrometer (FLS920, Edinburgh Instruments, UK), and the nanocrystals were excited by a 405nm picosecond laser diode at a 2MHz repetition rate. Absolute PL quantum yields (QY) were measured using a calibrated Ocean Optics FOIS-1 integrating sphere and a QE65000 spectrometer. All optical property measurements were performed at room temperature.
[0114] TEM images were taken on a Hitachi 7700 transmission electron microscope at 100 kV, with nanocrystals deposited on ultrathin carbon films on copper grids. XRD measurements were performed on a Rigaku Ultimate IV X-ray diffractometer operating at 40 kV / 30 mA with a Cu Kα line After purification by a standard precipitation process using hexane as solvent and acetone and methanol as precipitants, the nanocrystalline powder samples were placed on a glass substrate.
[0115] Example 1
[0116] Spherical CdSe nanocrystals with an average diameter of 3.3 nm were synthesized using selenium gel precursor (the first exciton absorption peak is located at 550 nm)
[0117] Selenium powder (0.315 g, 4.0 mmol) was dispersed in ODE (6.0 mL) and prepared by ultrasonic treatment for 5 min, and then melted vaseline (4.0 mL) was added to the above suspension to obtain a selenium gel precursor (0.4 M, referred to as selenium gel). In a typical synthesis, CdO (0.0127 g, 0.8 mmol) and stearic acid (0.910 g, 3.2 mmol) were loaded into a 50 mL three-necked flask containing 24.0 mL of ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 280 ° C by a CNC heating mantle to obtain a colorless solution. The temperature was reduced to 250 ° C, and 1 mL of selenium gel was quickly injected into the hot solution. The reaction temperature was maintained at 250 ° C for further growth. After 8 min of growth, a dose of selenium gel (2.0 mL) was loaded into a syringe and added dropwise to the reaction bottle at a rate of 1.0 mL / h by an automatic syringe pump until the first exciton absorption peak of the nanocrystal reached 550 nm. An aliquot (0.05 mL) was taken for ultraviolet visible absorption (UV-Vis) and fluorescence emission (PL) measurements to monitor the reaction. When the desired size was reached, the reaction was stopped by cooling to room temperature in air. Purification was performed using the following method: the reaction mixture (4 mL) was charged into a 20 mL vial, and 4 mL of ethyl acetate was added to the vial. After the vial was rotated and centrifuged at 4000 rpm, the supernatant was removed. The precipitate was dissolved in approximately 3 mL of toluene. Subsequently, 3 mL of methanol was added at room temperature, and the mixture was heated at 85°C for 5 min. After centrifugation at 4000 rpm for 15 s, the supernatant was removed. The sedimentation process was repeated twice. The purified CdSe nanocrystals were dissolved in ODE. The typical fluorescence emission and UV-visible absorption spectra of the obtained CdSe nanocrystals can be found in Figure 1 , TEM images see Figure 2 .
[0118] Example 2
[0119] Vaseline, ODE and Se powder were prepared into selenium gel, in which vaseline accounted for the total volume of liquid (V 凡士林 / (V 凡士林 +V ODE The volume fractions of vaseline were 0%, 10%, 30%, 40%, 50%, 60%, and 70% respectively. Selenium gels with different vaseline volume fractions were placed in small bottles and stored under the same conditions for 1 week. Figure 3 shown.
[0120] Synthesis of CdSe nanocrystals with an average diameter of 6nm using selenium gel and Cd(Ol)2 gel (the first exciton absorption peak is located at 650nm)
[0121] Selenium powder (0.237 g, 3.0 mmol) is suspended in ODE (5 mL) by ultrasonic treatment for 5 min, to which molten vaseline (5.0 mL) is added to form selenium gel. Cd (Ol) 2 gel (Cd (Ol) 2 gel, 0.15 M) is prepared by dissolving CdO powder (0.385 g, 3.0 mmol) in oleic acid (10.0 mL) and molten vaseline (10.0 mL). In a typical synthesis, CdO (0.020 g, 1.6 mmol), stearic acid (1.280 g, 4.5 mmol) and lauric acid (1.322 g, 6.6 mmol) are loaded into a 50 mL three-necked flask, and 10.0 mL ODE is added. After stirring and argon bubbling for 10 min, the mixture was heated to 250 ° C by a CNC heating jacket to obtain a colorless solution, and then an ODE solution (1.0 mL) containing 0.36 μmol of the above-mentioned purified CdSe seeds was injected into the reaction solution. After about 2.5 min, selenium gel (2.0 mL) and Cd (Ol) 2 gel (5.0 mL) were loaded into two syringes, respectively, and added to the reaction bottle at a rate of 0.63 mL / h and 1.26 mL / h respectively by an automatic injection pump. When the desired size is reached, the reaction is stopped by cooling to room temperature in air. The purification process is the same as above.
[0122] The UV-visible absorption and fluorescence emission spectra of CdSe nanocrystals evolve with time as Se gel precursor is added dropwise. Figure 4 During the reaction, the absorbance change of CdSe nanocrystals at 380nm, the fluorescence peak position and the fluorescence half-peak width (FWHM) of CdSe nanocrystals were monitored to obtain Figure 5 , Figure 5 The error bars in the figure give the variation among five replicate experiments. Figure 6 It can be further seen that the reproducibility of the five groups of experiments is very high.
[0123] Example 3
[0124] Synthesis of CdS Nanocrystals Using Gel Precursors
[0125] N,N'-di-n-butylthiourea (0.188 g, 1.0 mmol) was dispersed in ODE (5 mL) by stirring at 80 °C for 5 min, to which was added molten petrolatum (5.0 mL) to form N,N'-di-n-butylthiourea gel precursor (referred to as thiourea gel). S-ODE precursor (S-ODE, 0.1 M) was prepared by dispersing S powder (0.032 g, 1.0 mmol) in ODE (10.0 mL) by ultrasonication for 5 min. Cd(Ol)2-ODE solution (0.1 M) was prepared by dispersing CdO powder (0.128 g, 1.0 mmol) in oleic acid (1.1380 g, 4.0 mmol) at 100 °C for 60 min, to which was added 8.7 mL of ODE.
[0126] In a typical synthesis of CdS nanocrystals, CdO (0.026 g, 0.2 mmol) and stearic acid (0.171 g, 0.6 mmol) were charged into a 50 mL three-necked flask containing 6.0 mL of ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 280 ° C. The temperature was lowered to 250 ° C, and 1 mL of S-ODE was quickly injected into the hot solution. The reaction temperature was maintained at 250 ° C for 5 min for further growth. The temperature was lowered to 150 ° C, and thiourea gel (5.0 mL) and Cd (Ol) 2-ODE (5.0 mL) were loaded into two syringes respectively and added dropwise to the reaction bottle at a rate of 1.0 mL / h by an automatic injection pump. Take an aliquot (about 0.05 mL) for UV-Vis and PL measurements to monitor the reaction. When the desired size is reached, the reaction is stopped by cooling to room temperature in air. After cooling, the reaction mixture (4 mL) is charged into a 20 mL vial. 8 mL of ethyl acetate was added to the vial. After spinning and centrifuging at 4000 rpm, the supernatant was removed. The precipitate was dissolved in about 3 mL of toluene. 3 mL of methanol was added at room temperature, and the mixture was heated at 85 ° C for 50 min under magnetic stirring. After centrifugation at 4000 rpm, the supernatant was removed. The sedimentation process was repeated twice.
[0127] The typical UV-visible absorption and fluorescence emission spectra of CdS nanocrystals obtained are shown in Figure 7 .
[0128] In a typical CdS cluster synthesis, CdO (0.026 g, 0.2 mmol) and stearic acid (0.171 g, 0.6 mmol) were charged into a 25 mL volume three-necked flask with 6.0 mL ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 280 °C. Therefore, the temperature was lowered to 150 °C, and a dose of thiourea gel (5.0 mL) was loaded into a syringe and added dropwise to the reaction bottle at a rate of 1.0 mL / h by an automatic syringe pump. An aliquot (about 0.05 mL) was taken for UV-Vis and PL measurements to monitor the reaction.
[0129] The typical ultra-small size CdS clusters UV-visible absorption spectrum is shown in Figure 8 .
[0130] Example 4
[0131] Synthesis of ZnSe Nanocrystals from Selenium Gel and Zn5(CO3)2(OH)6 Gel
[0132] The selenium gel precursor (selenium gel, 0.4 M) was prepared by ultrasonically dispersing zinc carbonate hydroxide (0.4376 g, 0.8 mmol) in ODE (5 mL) for 5 min, and molten vaseline (5.0 mL) was added thereto to form a Zn5(CO3)2(OH)6 gel precursor (0.08 M, referred to as Zn5(CO3)2(OH)6 gel).
[0133] In a typical synthesis, Zn(St)2 (0.3162 g, 0.5 mmol) was charged into a 25 mL three-necked flask containing 5.0 mL of ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 290 °C. At 290 °C, 0.4 M selenium gel (0.8 mL, as described above) was quickly injected into the reaction bottle. After 8 min of reaction, selenium gel (10.0 mL) and Zn5(CO3)2(OH)6 gel (10.0 mL) were loaded into two syringes respectively and added dropwise at a rate of 2.4 mL / h by an automatic syringe pump. An aliquot (about 0.05 mL) was taken for UV-Vis and PL measurements to monitor the reaction. When the desired size was reached, the reaction was stopped by cooling to room temperature in air. The purification of ZnSe nanocrystals was as follows: an equal volume of acetone was mixed with the reaction mixture and centrifuged. After decantation, the precipitate was dissolved in 4.0 mL of toluene and a small amount of n-octylamine (0.06 mL). Acetonitrile (4.0 mL) was added to the solution to precipitate ZnSe nanocrystals. The precipitate was redissolved in hexane / toluene and reprecipitated 8 times with acetonitrile (hexane: toluene: acetonitrile = 1:1:1, 6 mL in total). The final precipitate of ZnSe nanocrystals was dispersed in 1.0 mL octane for further experiments. This purification process is applicable to another type of ZnSe nanocrystals described in Example 5 below and CdSe / ZnSe core-shell nanocrystals described in Example 9.
[0134] Fig. 9 The UV-visible absorption and fluorescence emission spectra of ZnSe nanocrystals of different sizes prepared in Example 4 are shown; Fig.10 The fluorescence half-width and fluorescence emission peak position change curves of ZnSe nanocrystals of different sizes prepared in Example 4 are shown.
[0135] Example 5
[0136] Synthesis of Ultra-Narrow Blue Luminescent ZnSe Nanocrystals Using Selenium Gel and Zn(Acac)2 Gel Precursors
[0137] Zinc acetylacetonate (0.5272 g, 2 mmol) was dispersed in ODE (5 mL) by ultrasound for 5 min, to which molten vaseline (5.0 mL) was added to form a zinc acetylacetonate gel precursor (0.2 M, referred to as Zn (Acac) 2 gel). In a typical synthesis, ODE (2.0 mL) was loaded into a 25 mL three-necked flask. After stirring and argon bubbling for 10 min, the liquid was heated to 290 ° C. The unpurified ZnSe nanocrystals synthesized above (2.0 mL, PL peak of 440 nm) were injected into the reaction bottle. After holding for 5 min, selenium gel (10.0 mL) and Zn (Acac) 2 gel (10.0 mL) were loaded into two separate syringes and added dropwise to the reaction bottle at a speed of 2.4 mL / h by an automatic injection pump. Take an aliquot (about 0.05 mL) for UV-Vis and PL measurements to monitor the reaction. When the desired size is reached, the reaction is stopped by cooling to room temperature in air. The fluorescence emission spectrum and TEM images of typical ZnSe nanocrystals obtained are shown in Fig.11 and 12 .
[0138] Example 6
[0139] Synthesis of 5.5 monolayer zinc blende CdSe nanosheets using Cd(Ac)2 gel precursor
[0140] Cadmium acetate dihydrate (0.5272 g, 1.5 mmol) was ground into a fine powder and suspended in ODE (6 mL) by stirring for 5 min, to which molten vaseline (4.0 mL) was added to form Cd(Ac)2 gel (0.15 M). In a typical synthesis of sphalerite 5.5-monolayer CdSe nanosheets, CdSt2 (0.020 g, 1.6 mmol) was charged into a 25 mL three-necked flask containing 4.0 mL ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 240 ° C under argon protection, and then selenium gel (1.0 mL) was injected into the flask. When the first exciton absorption peak of the nanocrystals moved to about 490 nm, Cd(Ac)2 gel (1.0 mL) was injected into the flask. Under argon protection, the reaction was maintained at 240 ° C for about 20 min, and then stopped by allowing the reaction mixture to cool in air. Take an aliquot and monitor the reaction by UV-visible absorption spectroscopy. Fig.13 TEM images of the prepared CdSe nanosheets are shown in Fig.14 .
[0141] Example 7
[0142] Synthesis of Hexahedral CdSe / CdS Core-Shell Nanocrystals Using Cd(OH)2 Gel Precursor
[0143] S powder (0.032 g, 1.0 mmol) was dispersed in ODE (9.3 mL) by 5 min ultrasonication, to which oleic acid (H01, 0.424 g, 1.5 mmol) and capric acid (HCa, 0.086 g, 0.5 mmol) were added to form the S precursor. Cadmium hydroxide (0.146 g, 1.0 mmol) was dispersed in ODE (5 mL), and molten vaseline (5.0 mL) was added to ODE to form Cd(OH)2 gel (0.1 M). In a typical synthesis, CdO (0.0128 g, 0.1 mmol), oleic acid (0.127 g, 0.45 mmol) and capric acid (HCa, 0.025 g, 0.15 mmol) were charged into a 25 mL three-necked flask containing 4.0 mL ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 250 ° C by a CNC heating mantle to obtain a colorless solution, and then the ODE solution containing 0.18 μmol of the above CdSe seed nanocrystals was injected into the reaction solution. After holding for 2.0 min, the S-ODE precursor (5.0 mL) and Cd (OH) 2 gel (5.0 mL) were loaded into two separate syringes and added dropwise to the reaction bottle at a rate of 2.0 mL / h by an automatic injection pump. Take an aliquot (about 0.05 mL) for UV-Vis and PL measurements to monitor the reaction. When the desired size is reached, the reaction is stopped by cooling to room temperature in air.
[0144] It is speculated that the ligands of the above-mentioned core-shell nanocrystals are hydroxide and carboxylate. The CdSe / CdS core-shell nanocrystals prepared in Example 7 were tested for the ratio of the number of ligands. The negatively charged (-1 valence) ligands can be replaced by another negatively charged (-1 valence) ligand in a one-to-one ratio, and thus can be replaced by thiolate ligands. Since each carboxylate and thiolate ligand is terminated with a methyl group, the absorbance difference of the methyl group (measured by the liquid phase FTIR method of carbon tetrachloride) gives the ratio of the hydroxide ligands without methyl termination in the original CdSe / CdS core-shell nanocrystals. The test results show that the hydroxide ligands of the CdSe / CdS core-shell nanocrystals are about 20%.
[0145] Example 8
[0146] Synthesis of Hexahedral CdSe / CdS / ZnS Core-Shell Nanocrystals Using Zn5(CO3)2(OH)6 Gel Precursor
[0147] Zn5(CO3)2(OH)6 (0.109 g, 0.2 mmol) was dispersed in ODE (5 mL) and stirred for 5 min, to which molten petrolatum (5.0 mL) was added to form a Zn5(CO3)2(OH)6 gel precursor (0.02 M, Zn5(CO3)2(OH)6 gel). In a typical synthesis, dehydrated zinc acetate (Zn(Ac)2·2H2O, 0.0220 g, 0.1 mmol), oleic acid (0.127 g, 0.45 mmol) and capric acid (HCa, 0.025 g, 0.15 mmol) were charged into a 25 mL three-necked flask with 4.0 mL of ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 250 ° C by a CNC heating jacket to obtain a colorless solution, and then an ODE solution containing about 0.05 μmol of CdSe / CdS core-shell nanocrystals (6 monolayer CdS shells) prepared in Example 7 was injected into the reaction solution. After holding for 2.0 min, S-ODE (5.0 mL) and Zn5 (CO3) 2 (OH) 6 gel (5.0 mL) were loaded into two separate syringes and added dropwise to the reaction bottle at a speed of 2.0 mL / h by an automatic injection pump. Take an aliquot (about 0.05 mL) for UV-Vis and PL measurements to monitor the reaction. When the desired size is reached, the reaction is stopped by cooling to room temperature in air.
[0148] TEM photos of the products during the reaction of Example 7-8 are shown in Fig.15 . Fig.16 The UV-visible spectra and PL spectra of the CdSe / CdS and CdSe / CdS / ZnS nanocrystals obtained in Examples 7-8 are shown. Fig.17 The transient fluorescence spectra of CdSe / CdS and CdSe / CdS / ZnS nanocrystals obtained in Examples 7-8 are shown. After being coated with ZnS, the quantum yield (QY) is increased from 87% to 89%.
[0149] Example 9
[0150] Preparation of CdSe / ZnSe Core-Shell Nanocrystals Using Selenium Gel and Zn(Acac)2 Gel Precursors
[0151] Selenium gel (0.1M, 50% vaseline) and Zn(Acac)2 gel (0.1M, 50% vaseline) were prepared using the above method. In a typical synthesis, Zn(St)2 (0.0316g, 0.05mmol) was loaded into a 25mL three-necked flask containing 4.0mL ODE. After stirring and argon bubbling for 10min, the mixture was heated to 290°C. Then, the ODE solution containing the above 0.18μmolCdSe core nanocrystals was injected into the reaction solution. After holding for 5min, the selenium gel precursor (10.0mL) and Zn(Acac)2 gel (10.0mL) were respectively loaded into two syringes and added dropwise to the reaction bottle at a speed of 2.0mL / h by an automatic injection pump. Take an aliquot (about 0.05mL) for UV-Vis and PL measurements to monitor the reaction. When the desired size is reached, the reaction is stopped by cooling to room temperature in air. CdSe / ZnSe nanocrystals with different single-shell numbers were prepared by calculating the amount of precursor added and controlling the time of precursor addition.
[0152] Fig.18 The UV-visible spectra and fluorescence spectra of the CdSe core used in Example 9 and the obtained CdSe / ZnSe nanocrystals with different single-shell numbers are shown. Fig.18 The "ML" in stands for monolayer, i.e. single shell. Fig.19 The PL spectra of the CdSe core used in Example 9 and the CdSe / ZnSe nanocrystals having a monolayer ZnSe shell layer are shown under the same excitation intensity. Fig. 20 The TEM image of the CdSe / ZnSe nanocrystal with 7 ZnSe shell layers prepared in Example 9 is shown.
[0153] Example 10
[0154] Synthesis of PbS Nanocrystals Using N,N'-Di-n-butylthiourea Gel Precursor
[0155] Thiourea gel (0.1M) was prepared using the above method. In a typical synthesis, lead oleate (Pb(Ol)2, 0.116 g, 0.15 mmol) was charged into a 25 mL three-necked flask containing 4.0 mL of ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 150 ° C, and 1 mL of thiourea gel was quickly injected into the hot solution. The reaction temperature was maintained at 150 ° C to grow PbS nanocrystals. An aliquot (about 0.05 mL) was taken for UV-Vis and PL measurements to monitor the reaction. When the desired size was reached, the reaction was stopped by cooling to room temperature in air. After cooling, the reaction mixture (2.5 mL) was charged into a 10 mL centrifuge tube. 5 mL of ethyl acetate was added to the centrifuge tube. After rotation and centrifugation at 10,000 rpm, the supernatant was removed. The precipitate was dissolved in about 2 mL of toluene. 4 mL of ethyl acetate was added at room temperature. After centrifugation at 10,000 rpm, the supernatant was removed. The sedimentation process was repeated twice.
[0156] Fig.21 The UV-visible spectrum of the PbS nanocrystals of Example 10 is shown, and the inset is a TEM photograph thereof. Fig. 22 The XRD pattern of the PbS nanocrystalline powder of Example 10 is shown.
[0157] Embodiment 11
[0158] Synthesis of PbSe Nanocrystals Using Selenium Gel Precursors
[0159] Selenium gel (0.1 M) was prepared using the above steps. In a typical synthesis, lead oleate (Pb(Ol)2, 0.155 g, 0.2 mmol) was charged into a 25 mL three-necked flask containing 6.0 mL of ODE. After stirring and argon bubbling for 10 min, the mixture was heated to 220 °C and 1 mL of selenium gel was quickly injected into the hot solution. The reaction temperature was maintained at 220 °C to grow PbSe nanocrystals. An aliquot (about 0.05 mL) was taken for UV-Vis and PL measurements to monitor the reaction. When the desired size was reached, the reaction was stopped by cooling to room temperature in air. After cooling, the reaction mixture (5 mL) was charged into a 20 mL vial. 10 mL of acetone was added to the vial. After spinning and centrifuging at 4000 rpm, the supernatant was removed. The precipitate was dissolved in about 4 mL of hexane. 8 mL of acetone was added at room temperature. After centrifugation at 4000 rpm, the supernatant was removed. The sedimentation process was repeated twice.
[0160] Example 12
[0161] Synthesis of Fe3O4 Nanocrystals by Using Fe(Acac)3 Gel
[0162] Ferric acetylacetonate (1.766 g, 5.0 mmol) and oleic acid (H01, 4.237 g, about 4.8 mL) were stirred for 5 min, and molten vaseline (5.2 mL) was added thereto to form Frrric ferric acetylacetonate gel precursor (0.5 M, referred to as Fe(Acac)3 gel). In a typical synthesis, ODE (4.0 mL) was loaded into a 25 mL three-necked flask. After stirring and argon bubbling for 10 min, the mixture was heated to 300 ° C. Fe(Acac)3 gel (5.0 mL) was loaded into a syringe and added dropwise to the reaction bottle at a speed of 2.0 mL / h by an automatic injection pump. After reacting for 30 min, the reaction was stopped by cooling to room temperature in air. After cooling, the reaction mixture (5 mL) was loaded into a 20 mL vial. 10 mL of ethyl acetate was added to the vial. After rotating and centrifuging at 4000 rpm, the supernatant was removed. The precipitate was dissolved in about 4 mL of toluene. 8 mL of acetone was added at room temperature. After centrifugation at 4000 rpm, the supernatant was removed. The precipitation process was repeated twice.
[0163] Fig.23 The XRD pattern of Fe3O4 nanocrystals prepared in Example 12 is shown. Fig.24 The TEM image of Fe3O4 nanocrystals prepared in Example 12 is shown.
[0164] Embodiment 13
[0165] The above method is used to prepare InP nanocrystals with In(Acac)3 gel precursor or In(Ac)3 gel precursor
[0166] In(Acac)3 gel (0.06M) or In(Ac)3 gel (0.06M) was prepared according to the above method. The synthesis of InP nanocrystals includes two consecutive steps, namely, forming small InP nanocrystals by directly injecting a phosphorus precursor into an ODE solution containing dissolved indium fatty acid salts, and continuously growing small InP nanocrystals by secondary injection of anionic precursors and cationic gel precursors. In a typical synthesis, In(Ac)3 (0.125mmol) and 0.375mmol myristic acid (HMy) were heated to 150°C in a 10mL flask and annealed for 30min under an argon flow to remove acetic acid. Trioctylphosphine (0.5mL) and ODE (3.5mL) were added to the solution. After keeping at 150°C for 10min, the mixture was cooled to 100°C. A solution containing 0.05mmol (TMS)3P in ODE (a total of 0.8mL) was quickly injected at 100°C, and the reaction temperature was set to 270°C to grow InP nanocrystals. After 15 min, the growth of InP nanocrystals reached a plateau, and additional (TMS)3P was added to the solution to further grow InP nanocrystals while the temperature was reduced from 270 ° C to 150 ° C. In(Acac)3 gel (0.06 mmol) or In(Ac)3 gel (0.06 mmol) was added to the reaction solution for surface activation, and a secondary indium precursor was added to grow InP nanocrystals. After 30 min at 150 ° C, 0.5 mL of 0.12 mol / L (TMS)3P-ODE solution was added dropwise. When the desired size of InP quantum dots was reached, the heating mantle was removed to cool the reaction mixture to room temperature.
[0167] Fig.25 The UV-visible spectra and PL spectra of the nanocrystals obtained by adding different P precursors during the reaction process of Example 13 are shown.
[0168] See the photo of the gel precursor composition used in each example. Fig.26 Table 1 summarizes the precursors used in various examples.
[0169] Table 1
[0170]
[0171]
[0172] The optical properties of the nanocrystals prepared in various examples are summarized in Table 2. No fluorescence was detected for lead nanocrystals under laboratory conditions. The ferroferric oxide nanocrystals mainly have magnetic properties and no fluorescence.
[0173] Table 2
[0174]
[0175]
[0176] Embodiment 14
[0177] Synthesis of CdSe / CdS Core-Shell Nanocrystals Using Cd(OH)2
[0178] Step 1: Take 0.1mmol CdO in a 25mL three-necked flask, add 0.45mmol oleic acid (OA) and 0.15mmol deca-acid. After the experimental device is set up, pass argon and heat to 150℃. Stir gently (level 1) for a while.
[0179] Step 2: After the solution is clarified, 4 mL of ODE is injected, and the temperature is raised to 250° C. After the temperature stabilizes, CdSe nanocrystals (purified, 0.18 μmmol) with a first exciton absorption peak of 550 nm are quickly injected.
[0180] Step 3: After 1 minute, control the dripping rate to 2 mL / h and simultaneously add 0.1 M Cd(OH)2 gel and S precursor mixture into the flask. The S precursor mixture includes 0.1 MS, 0.15 M OA, 0.05 M decacarbonic acid (CA) and ODE.
[0181] Step 4: Reaction for 150 min. During the reaction, a certain amount of the reaction solution was injected into a quartz watch glass containing 2.3 mL of toluene. The UV-visible absorption spectrum and the fluorescence emission spectrum were measured. When the nanocrystals reached the predetermined size, the heating was stopped immediately.
[0182] Comparative Example 1
[0183] Synthesis of CdSe / CdS Core-Shell Nanocrystals Using Cd(OA)2 and Cd(CA)2
[0184] Steps 1 and 2 are the same as in Example 14.
[0185] Step 3: After 1 minute, the gel Cd precursor composition and 0.1M S-ODE solution were added to the flask at the same time with the dripping rate controlled to 2 mL / h. The gel Cd precursor composition included 0.075M Cd(OA)2, 0.025M Cd(CA)2, 0.15M OA, 0.05M CA and vaseline. The reaction was continued for 170 minutes.
[0186] Step 4: During the reaction, a certain amount of the reaction solution was injected into a quartz watch glass containing 2.3 mL of toluene. The UV-visible absorption spectrum and the fluorescence emission spectrum were measured. When the nanocrystals reached a predetermined size, the heating was stopped immediately.
[0187] From the experimental results of Comparative Example 1 and Example 14 Fig. 27It can be seen that although gelatinous precursor compositions are used, the nanocrystal surface of Example 14 is presumed to have more hydroxide ligands than Comparative Example 1, which confirms that the hydroxide ligands of nanocrystals have a significant positive effect on nanocrystals compared with common carboxylate ligands, and can improve QY. This is also an additional benefit brought by the organic gel medium to expand the range of precursor selection.
[0188] The above description is only a preferred embodiment of the present disclosure and is not intended to limit the present disclosure. For those skilled in the art, the present disclosure may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A precursor composition, characterized in that The precursor composition is used to prepare inorganic nanocrystals and is in a gel state. The precursor composition includes a precursor and an organic gel medium for dispersing the precursor. The precursor is one or more of a cationic precursor and an anionic precursor. The precursor composition also includes a hydrocarbon solvent. The volume ratio of the hydrocarbon solvent to the organic gel medium is less than or equal to 4. The organic gel medium is vaseline. The hydrocarbon solvent is 1-octadecene. The precursor is selected from one or more of the group consisting of metal hydroxides, metal carbonates, metal carboxylates, acetylacetone metal salts, Se powder, S powder or thiourea derivatives.
2. The precursor composition according to claim 1, characterized in that The volume ratio of the hydrocarbon solvent to the organic gel medium is 4 / 6 to 7 / 3.
3. The precursor composition according to claim 1, characterized in that The precursor composition also includes an organic ligand compound for preparing inorganic nanocrystals.
4. The precursor composition according to claim 1, characterized in that The precursor composition also includes a fatty acid.
5. The precursor composition according to claim 4, characterized in that The melting point of the fatty acid is less than or equal to 30°C.
6. A method for preparing the precursor composition according to any one of claims 1 to 5, characterized in that: The precursor mixture liquid and the molten organic gel medium are mixed and cooled to obtain a precursor composition.
7. The preparation method according to claim 6, characterized in that: The precursor and the hydrocarbon solvent are mixed to obtain the precursor mixture liquid, the molten organic gel medium is added to the precursor mixture liquid, and the precursor composition is obtained by cooling.
8. The preparation method according to claim 6, characterized in that: The temperature of the molten organic gel medium is 70-80°C.
9. The preparation method according to claim 7, characterized in that: The process of mixing the precursor and the hydrocarbon solvent includes mixing the precursor and the hydrocarbon solvent under one or both of ultrasonic and stirring conditions to obtain the precursor mixture liquid.
10. The preparation method according to claim 7, characterized in that: The process of mixing the precursor and the hydrocarbon solvent further includes heating the precursor mixture liquid, wherein the temperature of the precursor mixture liquid is less than 100°C.
11. The preparation method according to claim 6, characterized in that: The metal oxide and the fatty acid are mixed and reacted to obtain the precursor mixture liquid.
12. The preparation method according to claim 11, characterized in that: The volume ratio of the fatty acid to the molten organogel medium is less than or equal to 0.
5.
13. A method for preparing inorganic nanocrystals, characterized in that: Inorganic nanocrystals are prepared using any one or more precursor compositions described in claims 1 to 5.
14. The preparation method according to claim 13, characterized in that: During the preparation of inorganic nanocrystals, the precursor composition is added to the reaction system multiple times.
15. The preparation method according to claim 13, characterized in that: The precursor composition includes metal hydroxide, and the surface ligands of the prepared inorganic nanocrystals include hydroxide.