Layered oxide material and preparation method thereof, positive electrode material and positive electrode sheet and lithium ion battery

By adjusting the molar ratio and doping elements of lithium elements and other metal elements, maintaining the layered structure of nickel-cobalt-manganate, the problems of material uniformity and cycle life in the existing technology are solved, and the performance of lithium-ion batteries is improved and Stability is enhanced.

CN115974177BActive Publication Date: 2024-11-12PINNACLE MATERIAL TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211725051.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-11-12
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

The existing layered oxide materials form an uneven hybrid crystal phase structure during the preparation process, resulting in the inability to guarantee material uniformity, the capacity cannot be effectively exerted, and the cycle life of lithium-ion batteries is attenuated.

Method used

By adjusting the molar ratio of lithium elements and other metal elements to (1.0-1.8): 1, doping an appropriate amount of transition metals and doping elements, keeping the layered structure of nickel-cobalt-manganate unchanged, and a specific preparation method is used to improve the Material uniformity and battery performance.

Benefits of technology

It improves the first effect and specific capacity of lithium-ion batteries, extends the cycle life of the battery, and avoids the generation of Li2MnO3 crystal phase, improving the stability of the material and battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115974177B_ABST
    Figure CN115974177B_ABST
Patent Text Reader

Abstract

The invention discloses a layered oxide material and a preparation method thereof, a positive electrode material and a positive electrode sheet and a lithium ion battery. The chemical formula of the layered oxide material is: Li 1+x M y A (1‑y) O2, wherein M is a transition metal cation, A is a doping element, 0<x<0.8, 0.9<y<1.0, and the layered oxide material can be prepared by a liquid phase lithium addition method or a solid phase lithium addition method. The layered oxide material of the present invention controls the molar ratio of lithium element and other metal elements by doping metal elements while keeping the structure of the original material unchanged. The layered oxide material prepared by the present invention is used in lithium ion batteries, which improves the first efficiency and specific capacity of the battery and can be applied to high cut-off voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a layered oxide material and a preparation method thereof, a positive electrode material and a positive electrode sheet, and a lithium-ion battery. Background Art

[0002] In 1990, Sony successfully commercialized layered LiCoO2 as a positive electrode material for lithium-ion batteries. Later, layered lithium nickel oxide, lithium manganese oxide, lithium iron phosphate, and lithium nickel cobalt manganese oxide (ternary materials) became common materials for lithium-ion batteries.

[0003] At present, the conventional layered oxide material LiNi in the industry x Co y Mn 1-x-y O2 is divided into NCM111, NCM523, NCM622, NCM811 and other models according to the different ratios of transition metal ions Co / Ni / Mn elements, in which the molar ratio of Li ions to transition metal ions is between 0.9 and 1.05. Its specific capacity at 4.2V0.2C is generally 140-190mAh / g. The lithium storage capacity of the material limits the capacity of the material.

[0004] The industry increases the lithium ion content to obtain higher energy density, but as the lithium storage capacity of the material increases, the layered structure will be destroyed, that is, the lithium-rich manganese phase / ternary layered phase is formed: Li2MnO3*LiNi x Co y Mn 1-x-y O2, 0<x<1, 0<y<1, the material forms an uneven hybrid crystal phase structure, resulting in a decrease in the battery cycle life.

[0005] Chinese patent CN201711308893.6 provides a method for preparing a high-capacity lithium-rich ternary positive electrode material, wherein lithium salt, manganese salt, cobalt salt and nickel salt are weighed respectively, mixed according to the general formula zLi2MnO3·(1-z)LiMO2 in a metering ratio, deionized water is added, and the mixed salt solution is stirred and dissolved; then a chelating agent is dissolved in deionized water to form a chelating agent solution, which is slowly added dropwise to the mixed salt solution by back titration, stirred until the mixture is uniformly mixed, an alkaline solution is added to adjust the end point pH value of the solution, and the mixed solution system is transferred to a water bath condition for continuous stirring; when the mixed solution is in a sol state, it is transferred to the feed port of a spray dryer for spray drying to obtain a lithium-rich ternary positive electrode material, which is placed in a muffle furnace for sintering according to a certain sintering curve to obtain a high-capacity lithium-rich ternary positive electrode material, wherein 0<z<1, M=Mn x Ni y Co (1-x-y) , 0<x<1, 0<y≤0.6.

[0006] Chinese patent CN201910179492.8 provides a preparation method of aluminum-coated lithium-rich ternary positive electrode material, 1) dissolving soluble nickel salt, cobalt salt and manganese salt according to a certain stoichiometric ratio, adding an excess of sodium hydroxide solution, stirring and reacting, filtering, repeatedly washing the filtrate with deionized water until the filtrate is completely neutral, and vacuum drying the filtrate to obtain a precursor A; 2) weighing lithium salt according to the stoichiometric ratio, mixing it with the precursor A and then ball milling to obtain a lithium-rich material B; 3) adding soluble aluminum salt and the lithium-rich material B to the alcohol solution and the deionized water alcohol-water mixed solution according to the stoichiometric ratio, then adjusting the solution pH to 8-14 with ammonia water, stirring, filtering after the reaction is complete, and drying the filtrate to obtain a composite material C; 4) keeping the composite material C at a temperature of 500-700°C for 8-12h, and after the insulation is completed, passing the obtained material through a sieve to obtain an aluminum-coated lithium-rich ternary positive electrode material.

[0007] In the method mentioned in the above patent application, the material chemical formula is zLi2MnO3·(1-z)Li X The essence of MO2 is to improve the capacity by preparing the lithium-rich manganese material Li2MnO3, but the lithium-rich manganese material Li2MnO3 will affect the crystal phase composition of the material, the uniformity of the material cannot be guaranteed, and its capacity cannot be effectively exerted.

[0008] Chinese patent CN201410176821.0 provides a method for preparing a lithium-rich ternary composite lithium-ion battery positive electrode material, comprising: (1) dissolving an organic precipitant in an organic solvent by stirring in a constant temperature water bath to obtain a solution 1; (2) ultrasonically dissolving soluble cobalt salt, nickel salt, manganese salt and lithium salt in deionized water to obtain a solution 2; (3) uniformly adding the solution 2 obtained in step (2) to the solution 1 obtained in step (1), reacting for 2-4 hours and then drying to obtain a solid powder, calcining in a high temperature tubular furnace system, and cooling to room temperature with the furnace to obtain a lithium-rich ternary composite lithium-ion battery positive electrode material.

[0009] In the method mentioned in the above patent application, the material chemical formula is Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2, because the materials prepared by the above method use a large amount of organic solvents and adopt an organic co-precipitation method, the organic solvents have a negative impact on the environment, the process route has a large environmental pressure, and is not conducive to the concept of sustainable development.

[0010] In view of the above-mentioned defects of current layered oxide materials, it is indeed necessary to provide a technical solution to the above-mentioned problems. Summary of the invention

[0011] The purpose of the present invention is to solve the problem that the existing ternary positive electrode materials form an uneven hybrid crystal phase structure during the preparation process, the material uniformity cannot be guaranteed, the capacity cannot be effectively exerted, and the battery cycle life is reduced. The present invention provides a layered oxide material, which does not change the layered structure of lithium nickel cobalt manganese oxide, and increases the molar ratio of Li element and other metal elements to (1.0-1.8):1, so as to solve the problem that the existing positive electrode materials have poor battery cycle stability and cannot effectively exert capacity due to the presence of the hybrid crystal phase structure.

[0012] In order to achieve the above object, the present invention adopts the following technical solutions:

[0013] The present invention provides a layered oxide material, the chemical formula of which is: Li 1+x M y A (1-y) O2, wherein M is a transition metal cation, A is a doping element, 0<x<0.8, 0.9<y<1.0.

[0014] The XRD spectrum of the layered oxide material has the following characteristic peaks: characteristic peak A: 18°~19°, characteristic peak B: 35°~36°, characteristic peak C: 36°~36.5°, characteristic peak D: 36.5°~37°, characteristic peak E: 44°~46°, characteristic peak F: 64°~64.5°, characteristic peak G: 65°~65.5°.

[0015] Preferably, the transition metal cation is at least one of Ni, Co and Mn elements.

[0016] Preferably, the doping element is at least one of Mg, Al, Fe, Ti, Sb, V, Y, Ce, Nb, and Zr.

[0017] Preferably, the weight percentage of the Li element in the layered oxide material is 7.8-12.8%.

[0018] Preferably, the transition metal cations account for 45-60% by weight of the layered oxide material.

[0019] Preferably, the median particle size D50 of the layered oxide is 3-16 μm, and the specific surface area is 0.2-15 m 2 / g.

[0020] The present invention also provides a method for preparing the above-mentioned layered oxide material, comprising the following steps:

[0021] (1) Raw material preparation: lithium salt, transition metal element salt, and doping element salt are prepared into a mixed solution with a metal ion concentration of 0.5 to 4 mol / L according to the metal molar ratio of 1+x:y:1-y; a precipitant is prepared into a solution with a concentration of 0.5 to 6 mol / L; a pH adjuster is prepared into a solution C with a concentration of 1 to 6 mol / L; a polymer surfactant is prepared into a solution with a concentration of 0.1 to 10 g / L;

[0022] (2) Feeding reaction: Add a polymer surfactant to a reaction kettle containing deionized water, stir at a stirring speed of 500 to 1500 rpm for 20 to 80 min, and then use a metering pump to simultaneously add a transition metal soluble salt solution and a precipitant solution at a feed flow rate of 2 to 50 ml / min;

[0023] (3) Aging and washing of the slurry: After the addition of the material in step (2) is completed, a pH adjusting agent solution is added at a feed flow rate of 5 to 50 ml / min using a metering pump to adjust the pH value to 7 to 11. After aging for 5 to 15 hours, the slurry is discharged into a centrifuge for washing and filtration;

[0024] (4) Drying: Drying the filtered product obtained in step (3) to obtain a layered oxide precursor;

[0025] (5) Sintering: The layered oxide precursor obtained in step (4) is placed in a muffle furnace, heated to 400-900° C. at a heating rate of 1-6° C. / min, and sintered for 2-20 h under protective atmosphere conditions. After natural cooling, the layered oxide material is obtained.

[0026] Preferably, in step (1), the transition metal element salt and the doping element salt are at least one of chloride, sulfate and nitrate.

[0027] Preferably, in step (1), the lithium salt is at least one of lithium chloride, lithium sulfate, lithium nitrate, lithium carbonate, lithium acetate and lithium oxalate.

[0028] Preferably, in step (1), the transition metal element salt is at least one of metal salts containing Ni, Co, and Mn elements.

[0029] Preferably, in step (1), the doping element salt is at least one of metal salts containing Mg, Al, Fe, Ti, Sb, V, Y, Ce, Nb, and Zr elements.

[0030] Preferably, in step (1), in the molar ratio of the metal amount 1+x:y:1-y, 0 <x<0.8,0.9<y<1.0。

[0031] Preferably, in step (1), the precipitant is at least one of ammonium fluoride, sodium hydroxide, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, sodium monohydrogen phosphate, sodium dihydrogen phosphate, sodium phosphate, ammonia water, sodium carbonate, sodium bicarbonate, and ammonium bicarbonate.

[0032] Preferably, in step (1), the pH adjuster is at least one of sodium hydroxide, potassium hydroxide, aqueous ammonia, sodium carbonate and sodium bicarbonate, more preferably aqueous ammonia.

[0033] Preferably, in step (1), the polymer surfactant is at least one of polyacrylamide and polyacryl alcohol.

[0034] Preferably, in step (2), the volume of deionized water is 1 to 10 L, more preferably 3 L.

[0035] Preferably, in step (2), the stirring speed is 800 to 1200 rpm, and the stirring time is 40 to 60 min.

[0036] Preferably, in step (2) and step (3), the feed flow rate is 10 to 25 ml / min, more preferably 10 ml / min.

[0037] Preferably, in step (3), the pH value is 8 to 9, and the aging time is 5 to 10 hours.

[0038] Preferably, in step (4), the drying temperature is 60 to 120° C., and the drying time is 2 to 6 hours.

[0039] Preferably, in step (5), the heating rate is 2-5°C / min, more preferably 3°C / min.

[0040] Preferably, in step (5), the heating temperature is 500-950°C, more preferably 550-900°C.

[0041] Preferably, in step (5), the sintering time is 4-15 hours, more preferably 5-10 hours.

[0042] The present invention also provides a method for preparing the above-mentioned layered oxide material, comprising the following steps:

[0043] (1) Preparation: Weigh the lithium source, commercially available nickel cobalt manganese hydroxide, and doping element salt in a metal molar ratio of 1+x:y:1-y;

[0044] (2) Mixing: Disperse and mix the weighed lithium source, commercially available nickel, cobalt and manganese hydroxide, and doping element compounds under the action of water, and perform solvent desorption at 110 to 160° C. for 2 to 6 hours;

[0045] (3) Sintering: The mixed materials are placed in a muffle furnace, heated to 400-900° C. at a heating rate of 1-6° C. / min, and sintered for 2-20 h under protective atmosphere conditions. After natural cooling, the layered oxide material is obtained.

[0046] Preferably, in step (1), the lithium source is at least one of lithium chloride, lithium sulfate, lithium nitrate, lithium carbonate, lithium acetate and lithium oxalate.

[0047] Preferably, in step (1), in the molar ratio of the metal amount 1+x:y:1-y, 0 <x<0.8,0.9<y<1.0。

[0048] Preferably, in step (1), the doping element compound is at least one of oxides, oxalates, carbonates, acetates and chlorides.

[0049] Preferably, in step (2), the desorption temperature is 110-160° C., and the desorption time is 2-6 hours.

[0050] Preferably, in step (3), the heating rate is 2-5°C / min, more preferably 3°C / min.

[0051] Preferably, in step (3), the heating temperature is 500-950°C, more preferably 550-900°C.

[0052] Preferably, in step (3), the sintering time is 4-15 hours, more preferably 5-10 hours.

[0053] The present invention also provides a positive electrode material, which comprises a positive electrode active material, a positive electrode binder and a positive electrode conductor, and the positive electrode active material is a layered oxide material obtained by the above preparation method.

[0054] The present invention also provides a positive electrode sheet, comprising a positive current collector and a positive electrode material coated on the positive current collector, wherein the positive electrode material is the positive electrode material mentioned above.

[0055] The present invention also provides a lithium-ion battery, comprising a shell, a battery cell located inside the shell, a cover plate sealing the shell, and an electrolyte located inside the shell and between the battery cells. The battery cell comprises positive and negative electrode sheets and a separator located between the positive and negative electrode sheets. The positive electrode sheet is the above-mentioned positive electrode sheet.

[0056] Preferably, the discharge curve of the lithium-ion battery has two redox peaks in the range of 3.6-4.2V.

[0057] Preferably, the charging cut-off voltage of the lithium-ion battery is 4.0-5.0V.

[0058] Compared with the prior art, the present invention has at least the following beneficial effects:

[0059] 1) The layered oxide material can reduce the structural changes caused by the change of the oxidation potential of the manganese element by element doping. On the premise that the XRD keeps the layered structure of lithium nickel cobalt manganese oxide unchanged, the Li:M molar ratio is increased to (1.0-1.8):1.

[0060] 2) The layered oxide material, based on a lithium content of ≥10%, increases the specific capacity of commercially available nickel cobalt manganese oxide by ≥10% under the same cut-off voltage conditions.

[0061] 3) The first efficiency of the lithium-ion battery made using the layered oxide material of the present invention is increased from 85-89% to 92-95%.

[0062] 4) The present invention can effectively avoid the generation of Li2MnO3 crystal phase as the Li content increases during the preparation of layered oxide materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 The XRD diagrams of the layered oxides prepared in Example 1, Comparative Example 1 and Comparative Example 2 are shown.

[0064] Figure 2 4.2V / 0.1CDQ / DV curves of the layered oxides prepared in Example 1, Comparative Example 1 and Comparative Example 2.

[0065] Figure 3 4.5 / 0.1C charge-discharge curves of the layered oxides prepared in Example 1 and Comparative Example 1.

[0066] Figure 4 This is the particle size distribution diagram of the layered oxide prepared in Example 1. DETAILED DESCRIPTION

[0067] In order to make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0068] According to a first aspect of the present invention, the present invention provides a layered oxide material, the chemical formula of the layered oxide material is: Li 1+x M y A (1-y) O2, wherein M is a transition metal cation, A is a doping element, 0<x<0.8, 0.9<y<1.0.

[0069] In one embodiment of the present invention, the XRD spectrum of the layered oxide material has the following characteristic peaks: characteristic peak A: 18°~19°, characteristic peak B: 35°~36°, characteristic peak C: 36°~36.5°, characteristic peak D: 36.5°~37°, characteristic peak E: 44°~46°, characteristic peak F: 64°~64.5°, characteristic peak G: 65°~65.5°.

[0070] In one embodiment of the present invention, the transition metal cation is at least one of Ni, Co, and Mn elements.

[0071] In one embodiment of the present invention, the doping element is at least one of Mg, Al, Fe, Ti, Sb, V, Y, Ce, Nb, and Zr.

[0072] In one embodiment of the present invention, the weight percentage of Li element in the layered oxide material is 7.8-12.8%, for example, 7.8%, 8.8%, 9.8%, 10.8%, 11.8%, or 12.8%.

[0073] In one embodiment of the present invention, the transition metal cation accounts for 45-60% by weight of the layered oxide material, for example, 45%, 50%, 55%, or 60%.

[0074] In one embodiment of the present invention, the median particle size D50 of the layered oxide is 3 to 16 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, and the specific surface area is 0.2-15 m 2 / g, for example, it can be 0.2m 2 / g, 0.8m 2 / g, 1.2m 2 / g, 2m 2 / g, 3m 2 / g, 4m 2 / g, 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g, 10m 2 / g, 11m 2 / g, 12m 2 / g, 13m 2 / g, 14m 2 / g, 15m 2 / g. The particle size of the material is controlled within the above range because if the particle size is too small, the specific surface area will increase, resulting in more side reactions and affecting the cycle performance of the battery. If the particle size is too large, the material will pierce the current collector when it is made into an electrode, causing a short circuit in the battery and a fire and explosion.

[0075] The specific surface area of ​​the material is controlled within the above range because if the specific surface area is too low, it is not conducive to the contact between the material and the electrolyte, and the capacity, cycle and other performances will deteriorate after the battery is made. If the specific surface area is too high, the contact area between the material and the electrolyte is too large, and more side reactions occur between the material and the electrolyte, and the cycle performance of the battery will deteriorate.

[0076] According to a second aspect of the present invention, the present invention also provides a method for preparing the above-mentioned layered oxide material, comprising the following steps:

[0077] (1) Raw material preparation: lithium salt, transition metal element salt, and doping element salt are prepared into a mixed solution with a metal ion concentration of 0.5 to 4 mol / L according to the metal molar ratio of 1+x:y:1-y; a precipitant is prepared into a solution with a concentration of 0.5 to 6 mol / L; a pH adjuster is prepared into a solution C with a concentration of 1 to 6 mol / L; a polymer surfactant is prepared into a solution with a concentration of 0.1 to 10 g / L;

[0078] (2) Feeding reaction: Add a polymer surfactant to a reaction kettle containing deionized water, stir at a stirring speed of 500 to 1500 rpm for 20 to 80 min, and then use a metering pump to simultaneously add a transition metal soluble salt solution and a precipitant solution at a feed flow rate of 2 to 50 ml / min;

[0079] (3) Aging and washing of the slurry: After the addition of the material in step (2) is completed, a pH adjusting agent solution is added at a feed flow rate of 5 to 50 ml / min using a metering pump to adjust the pH value to 7 to 11. After aging for 5 to 15 hours, the slurry is discharged into a centrifuge for washing and filtration;

[0080] (4) Drying: Drying the filtered product obtained in step (3) to obtain a layered oxide precursor;

[0081] (5) Sintering: The layered oxide precursor obtained in step (4) is placed in a muffle furnace, heated to 400-900° C. at a heating rate of 1-6° C. / min, and sintered for 2-20 h under protective atmosphere conditions. After natural cooling, the layered oxide material is obtained.

[0082] In addition, each solution in step (1) is controlled within this range because if it is below this range, the efficiency is too low. If it exceeds this range, the precipitation rate in the slurry system will become faster, and it will even become a colloid, adsorbing and entraining a large amount of impurities, making it difficult to filter the final product during washing, resulting in poor washing effect and the appearance of amorphous large agglomerates. If it is higher, it will even exceed the solubility limit and cannot be dissolved.

[0083] In one embodiment of the present invention, in step (1), the transition metal element salt and the doping element salt are at least one of chloride, sulfate and nitrate.

[0084] In one embodiment of the present invention, in step (1), the lithium salt is at least one of lithium chloride, lithium sulfate, lithium nitrate, lithium carbonate, lithium acetate, and lithium oxalate.

[0085] In one embodiment of the present invention, in step (1), the transition metal element salt is at least one of metal salts containing Ni, Co, and Mn elements.

[0086] In one embodiment of the present invention, in step (1), the doping element salt is at least one of metal salts containing Mg, Al, Fe, Ti, Sb, V, Y, Ce, Nb, and Zr elements.

[0087] In one embodiment of the present invention, in step (1), in the metal molar ratio 1+x:y:1-y, 0 <x<0.8,0.9<y<1.0。

[0088] In one embodiment of the present invention, in step (1), the precipitant is at least one of ammonium fluoride, sodium hydroxide, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, sodium monohydrogen phosphate, sodium dihydrogen phosphate, sodium phosphate, ammonia water, sodium carbonate, sodium bicarbonate, and ammonium bicarbonate.

[0089] In one embodiment of the present invention, in step (1), the pH adjuster is at least one of sodium hydroxide, potassium hydroxide, ammonia water, sodium carbonate, and sodium bicarbonate, more preferably ammonia water.

[0090] In one embodiment of the present invention, in step (1), the polymer surfactant is at least one of polyacrylamide and polyacryl alcohol.

[0091] In one embodiment of the present invention, in step (2), the volume of deionized water is 1-10 L, more preferably 3 L, for example, 1 L, 2 L, 3 L, 4 L, 5 L, 6 L, 7 L, 8 L, 9 L, or 10 L.

[0092] In one embodiment of the present invention, in step (2), the stirring speed is 800-1200 rpm, for example, 800 rpm, 850 rpm, 900 rpm, 950 rpm, 1000 rpm, 1100 rpm, 1200 rpm, and the stirring time is 40-60 min, for example, 40 min, 45 min, 50 min, 55 min, 60 min. 40 min,.

[0093] In one embodiment of the present invention, in step (2) and step (3), the feed flow rate is 10-25 ml / min, more preferably 10 ml / min, for example, 10 ml / min, 12 ml / min, 15 ml / min, 18 ml / min, 20 ml / min, 22 ml / min, 25 ml / min.

[0094] In one embodiment of the present invention, in step (3), the pH value is 8-9, and the aging time is 5-10 hours, for example, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, or 10 hours.

[0095] In one embodiment of the present invention, in step (4), the drying temperature is 60-120°C, for example, it can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, and the drying time is 2-6h, for example, it can be 2h, 3h, 4h, 5h, 6h.

[0096] In one embodiment of the present invention, in step (5), the heating rate is 2-5°C / min, more preferably 3°C / min.

[0097] In one embodiment of the present invention, in step (5), the heating temperature is 500-950°C, more preferably 550-900°C, for example, it can be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C.

[0098] In one embodiment of the present invention, in step (5), the sintering time is 4-15 h, more preferably 5-10 h, for example, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h.

[0099] According to a third aspect of the present invention, the present invention also provides a method for preparing the above-mentioned layered oxide material, comprising the following steps:

[0100] (1) Preparation: Weigh the lithium source, commercially available nickel cobalt manganese hydroxide, and doping element salt in a metal molar ratio of 1+x:y:1-y;

[0101] (2) Mixing: Disperse and mix the weighed lithium source, commercially available nickel, cobalt and manganese hydroxide, and doping element compounds under the action of water, and perform solvent desorption at 110 to 160° C. for 2 to 6 hours;

[0102] (3) Sintering: The mixed materials are placed in a muffle furnace, heated to 400-900°C at a heating rate of 1-6°C / min, and sintered for 2-20 hours under protective atmosphere conditions. After natural cooling, the layered oxide material is obtained.

[0103] In one embodiment of the present invention, in step (1), the lithium source is at least one of lithium chloride, lithium sulfate, lithium nitrate, lithium carbonate, lithium acetate, and lithium oxalate.

[0104] In one embodiment of the present invention, in step (1), in the metal molar ratio 1+x:y:1-y, 0 <x<0.8,0.9<y<1.0。

[0105] In one embodiment of the present invention, in step (1), the doping element compound is at least one of oxides, oxalates, carbonates, acetates, and chlorides.

[0106] In one embodiment of the present invention, in step (2), the desorption temperature is 110-160°C, for example, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, and the desorption time is 2-6h, for example, 2h, 3h, 4h, 5h, 6h.

[0107] In one embodiment of the present invention, in step (3), the heating rate is 2-5°C / min, more preferably 3°C / min, for example, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min.

[0108] In one embodiment of the present invention, in step (3), the heating temperature is 500-950°C, more preferably 550-900°C, for example, it can be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C.

[0109] In one embodiment of the present invention, in step (3), the sintering time is 4-15 h, more preferably 5-10 h, for example, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h.

[0110] According to a fourth aspect of the present invention, the present invention further provides a positive electrode material, which includes a positive electrode active material, a positive electrode binder and a positive electrode conductor, and the positive electrode active material is a layered oxide material obtained by the above preparation method.

[0111] Among them, the positive electrode binder and the positive electrode conductor can be selected from various binders used in lithium ion batteries known to those skilled in the art, for example, it can be at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyacrylate and water-based polyurethane, and the positive electrode conductor can be at least one of carbon nanotubes, conductive carbon black, conductive graphite, carbon fiber, and graphene.

[0112] According to a fifth aspect of the present invention, the present invention further provides a positive electrode sheet, comprising a positive current collector and a positive electrode material coated on the positive current collector, wherein the positive electrode material is the positive electrode material mentioned above.

[0113] According to the sixth aspect of the present invention, the present invention also provides a lithium-ion battery, comprising a shell, a battery cell located inside the shell, a cover plate sealing the shell, and an electrolyte located inside the shell and between the battery cells, the battery cell comprising positive and negative electrode sheets and a separator located between the positive and negative electrode sheets, and the positive electrode sheet is the above-mentioned positive electrode sheet.

[0114] In one embodiment of the present invention, the Dq / Dv curve of the lithium-ion battery discharge has two redox peaks in the range of 3.6-4.2V.

[0115] In one embodiment of the present invention, the charging cut-off voltage of the lithium-ion battery is 4.0-5.0V.

[0116] Among them, the preparation method of the positive / negative electrode sheet of the lithium ion battery is well known to those skilled in the art, for example, the positive / negative electrode active material, the positive / negative electrode conductive agent and the positive / negative electrode binder are dissolved in a solvent in a certain proportion and mixed into a positive / negative electrode slurry, and then the slurry is coated on a wide conductive substrate, and then dried, rolled and cut to obtain the positive / negative electrode sheet. The conditions of drying and rolling are well known to those skilled in the art, for example, the temperature for drying the negative electrode sheet is generally 60-120°C, preferably 80-110°C, and the drying time is 0.5-5 hours.

[0117] The cell structure of the battery provided by the present invention is a commonly used cell structure in the art. Generally speaking, the cell can be prepared by winding or stacking positive electrode sheets, separators and negative electrode sheets. The winding or stacking methods are well known to those skilled in the art.

[0118] The separator of the battery of the present invention has electrical insulation performance and liquid retention performance. The separator can be selected from various separators used in lithium ion secondary batteries known to those skilled in the art, such as polyolefin microporous membranes, polyethylene felts, glass fiber felts or ultrafine glass fiber paper.

[0119] The negative electrode of the lithium ion battery of the present invention can be a negative electrode conventionally used in the art; for example, the negative electrode includes a current collector and a negative electrode material coated and / or filled on the current collector, and the negative electrode material includes a negative electrode active material and a negative electrode binder; the negative electrode active material is not particularly limited, and conventional negative electrode active materials that can be embedded and released lithium in the art can be used, such as natural graphite, artificial graphite, petroleum coke, organic cracked carbon, mesophase carbon microspheres, carbon fiber, tin alloy, silicon alloy one or more, preferably artificial graphite. The negative electrode material can also include a negative electrode conductive agent, which is not particularly limited and can be a conventional negative electrode conductive agent in the art, such as ketjen carbon black, acetylene black, furnace black, carbon fiber VGCF, conductive carbon black and conductive graphite one or more; based on the weight of the negative electrode material, the content of the negative electrode conductive agent is 1-15wt%, preferably 2-10wt%. The type and content of the negative electrode binder are well known to those skilled in the art, for example, it can be selected from one or more of fluorine-containing resins and polyolefin compounds such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and styrene-butadiene rubber (SBR); generally speaking, depending on the type of binder used, the content of the negative electrode binder is 0.01-8wt%, preferably 0.02-5wt%, based on the weight of the negative electrode material; preferably, the negative electrode binder is a mixture of cellulose-based polymer and rubber latex, such as a mixture of cellulose-based polymer and styrene-butadiene rubber (SBR). The amount of cellulose-based polymer and styrene-butadiene rubber is well known to those skilled in the art; the negative electrode collector can be a conventional negative electrode collector in a lithium-ion battery, such as stamped metal, metal foil, mesh metal, and foam metal.

[0120] The electrolyte of the battery of the present invention is a non-aqueous electrolyte. The non-aqueous electrolyte is a solution of an electrolyte lithium salt in a non-aqueous solvent, and conventional non-aqueous electrolytes known to those skilled in the art can be used. For example, the electrolyte lithium salt can be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium hexafluorosilicate (LiSiF6), lithium tetraphenylborate (LiB(C6H5)4), lithium chloride (LiCl), lithium bromide (LiBr), lithium chloroaluminate (LiAlCl4), and lithium fluorocarbon sulfonate (LiC(SO2CF3)3), LiCH3SO3, and LiN(SO2CF3)2. The non-aqueous solvent can be selected from a mixed solution of chain acid esters and cyclic acid esters, wherein the chain acid ester can be one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), dipropyl carbonate (DPC) and other chain organic esters containing fluorine, sulfur or unsaturated bonds. The cyclic acid ester can be one or more of ethylene carbonate (EC), propylene carbonate (PC), vinylene carbonate (VC), γ-butyrolactone (γ-BL), sultone and other cyclic organic esters containing fluorine, sulfur or unsaturated bonds. In the non-aqueous electrolyte, the concentration of the electrolyte lithium salt is generally 0.1-2 mol / L, preferably 0.8-1.2 mol / L.

[0121] The preparation method of the battery of the present invention is well known to those skilled in the art. Generally speaking, the preparation method of the battery includes placing a battery cell in a battery case, adding an electrolyte, and then sealing the case to obtain a battery. The sealing method and the amount of electrolyte used are well known to those skilled in the art.

[0122] In order to make the technical solutions and advantages of the present invention more clear, the present invention is further described below through specific embodiments.

[0123] Comparative Example 1

[0124] Commercially available lithium nickel cobalt manganese oxide LiNi 0.5 Co 0.2 Mn 0.3 O2 is used as the positive electrode active material and is denoted as A1.

[0125] Preparation of the battery: The positive electrode active material A1, acetylene black and PVDF are dissolved in N-methylpyrrolidone in a weight ratio of 100:4:5, stirred evenly and coated on aluminum foil, baked at a temperature of 100°C, rolled to a certain thickness using a tablet press, and rolled into a positive electrode sheet; graphite, acetylene black and PVDF are dissolved in N-methylpyrrolidone in a weight ratio of 100:3:6, stirred evenly and coated on copper foil, baked at a temperature of 100°C, rolled to a certain thickness using a tablet press, and rolled into a negative electrode sheet; the above positive and negative electrode sheets and a 16μm thick polypropylene separator are wound into a square lithium-ion battery cell, placed in a battery shell and welded, and then injected with 1.0mol / L LiPF6 / (EC+EMC+DMC) (wherein the mass ratio of EC, EMC and DMC is 1:1:1) electrolyte, sealed, and made into a lithium battery A2.

[0126] Comparative Example 2

[0127] Commercially available lithium nickel cobalt manganese oxide LiNi 0.5 Co 0.2 Mn 0.3 O2 and lithium carbonate were mixed in a mass ratio of 100:7.7 and placed in a muffle furnace (Sigma ML-6000). The temperature was raised to 800 °C within 3 hours and kept at this temperature for 5 hours under a protective atmosphere. After natural cooling, the mixture was subjected to air flow pulverization to obtain a lithium-rich lithium manganese oxide / nickel cobalt lithium manganese oxide positive electrode material, zLi2MnO3·(1-z)LiNi 0.5 Co 0.2 Mn 0.3 O2, recorded as B1.

[0128] Preparation of the battery: The positive electrode active material A1, acetylene black and PVDF are dissolved in N-methylpyrrolidone in a weight ratio of 100:4:5, stirred evenly and coated on aluminum foil, baked at a temperature of 105°C, rolled to a certain thickness using a tablet press, and rolled into a positive electrode sheet; graphite, acetylene black and PVDF are dissolved in N-methylpyrrolidone in a weight ratio of 100:3:6, stirred evenly and coated on copper foil, baked at a temperature of 105°C, rolled to a certain thickness using a tablet press, and rolled into a negative electrode sheet; the above positive and negative electrode sheets and a 16μm thick polypropylene separator are wound into a square lithium-ion battery cell, which is placed in a battery shell and welded, and then 1.0mol / L LiPF6 / (EC+EMC+DMC) (wherein the mass ratio of EC, EMC and DMC is 1:1:1) electrolyte is injected, sealed, and a lithium battery B2 is made.

[0129] Example 1

[0130] Weigh 84.8g of LiCl, 248.6g of NiSO4·6H2O, 146.2g of CoSO4·7H2O, 310.4g of MnSO4·H2O, and 135.2g of Al2(SO4)3·18H2O, dissolve them in 2000g of deionized water at about 50°C, and dilute to 3L to obtain liquid A; weigh 487.6g of Na2CO3 and 46.1g of NH4H2PO4, dissolve them in 2000g of deionized water at about 50°C, and dilute to 3L to obtain liquid B; prepare 2L of 10mol / L ammonia solution, that is, weigh 700g of 25% ammonia solution, and dilute to 2L to obtain liquid C; weigh 6g of high molecular surfactant propylene glycol according to 0.1% of the total volume of liquids A and B, and dissolve it in 3L of deionized water to obtain liquid D. Liquid D was added into the reactor and stirred at a stirring speed of 800 rpm for 40 min; Liquid A and Liquid B were added simultaneously at a feeding speed of 10 ml / min using a peristaltic pump, and the feeding was continued for 3.5 h. After the feeding was completed, a 5 mol / L ammonia solution was added at 20 ml / min using a peristaltic pump, and the pH value was adjusted to a specified value of 8, and the stirring speed was kept unchanged at 800 rpm. After aging for 7 h, the slurry was centrifugally filtered using a centrifuge (model YLT-1200) to obtain a filter cake; the filter cake was placed in an electric hot air dryer (model 101-0ABS) and dried at a constant temperature of 80°C for 3 h, and then taken out to obtain a layered oxide precursor, and the layered oxide precursor was mixed with 14.8 g of lithium carbonate, and after mixing, it was placed in a muffle furnace (Sigma ML-6000), heated to 800°C within 3 hours, and kept warm for 5 hours in an air atmosphere, and then naturally cooled and air flow crushed to obtain Li 1.2 Ni 0.5 Co 0.15 Mn 0.3 Al 0.05 O 2.0 Lithium-rich layered nickel cobalt manganese oxide material, denoted as C1.

[0131] Preparation of the battery: The positive electrode active material C1, acetylene black and PVDF are dissolved in N-methylpyrrolidone in a weight ratio of 100:4:5, stirred evenly and coated on aluminum foil, baked at a temperature of 100°C, rolled to a certain thickness using a tablet press, and rolled into a positive electrode sheet; graphite, acetylene black and PVDF are dissolved in N-methylpyrrolidone in a weight ratio of 100:3:6, stirred evenly and coated on copper foil, baked at a temperature of 100°C, rolled to a certain thickness using a tablet press, and rolled into a negative electrode sheet; the above positive and negative electrode sheets and a 16μm thick polypropylene separator are wound into a square lithium-ion battery cell, placed in a battery shell and welded, and then injected with 1.0mol / L LiPF6 / (EC+EMC+DMC) (wherein the mass ratio of EC, EMC and DMC is 1:1:1) electrolyte, sealed, and made into a lithium battery C2.

[0132] Example 2

[0133] Lithium carbonate, commercially available nickel cobalt manganese hydroxide LiNi 0.5 Co 0.2 Mn 0.3 O2 and aluminum sulfate were weighed in a metal molar ratio of 1.2:0.95:0.05, dispersed and mixed under the action of water, desorbed by solvent at 130°C for 4 hours, placed in a muffle furnace, heated to 600°C at a heating rate of 5°C / min, and sintered for 12 hours under protective atmosphere conditions. After natural cooling, the layered oxide material, i.e., Li 1.2 Ni 0.5 Co 0.15 Mn 0.3 Al 0.05 O 2.0 Lithium-rich layered nickel cobalt manganese oxide material, denoted as D1.

[0134] Preparation of the battery: The positive electrode active material D1, acetylene black and PVDF are dissolved in N-methylpyrrolidone at a weight ratio of 100:4:5, stirred evenly and coated on aluminum foil, baked at a temperature of 105°C, rolled to a certain thickness using a tablet press, and rolled into a positive electrode sheet; graphite, acetylene black and PVDF are dissolved in N-methylpyrrolidone at a weight ratio of 100:3:6, stirred evenly and coated on copper foil, baked at a temperature of 105°C, rolled to a certain thickness using a tablet press, and rolled into a negative electrode sheet; the above positive and negative electrode sheets and a 16μm thick polypropylene separator are wound into a square lithium-ion battery cell, which is placed in a battery shell and welded, and then 1.0mol / L LiPF6 / (EC+EMC+DMC) (wherein the mass ratio of EC, EMC and DMC is 1:1:1) electrolyte is injected, sealed, and a lithium battery D2 is made.

[0135] The particle size and XRD analysis were performed on the layered oxides prepared in the examples and comparative examples.

[0136] (1) Particle size analysis

[0137] The particle size was measured using a laser particle size detector (model Mastersizer 3000E); the test conditions were: water as the dispersant, wet injection, refractive index of 2.0, absorbance of 0.1, and the obtained particle size was the volume-integrated particle size statistical result, such as Figure 4 shown.

[0138] (2) XRD analysis

[0139] The crystal phase structure of the layered oxide materials obtained in Example 1, Comparative Example 1 and Comparative Example 2 was detected by an X-ray diffractometer (Ultima IV model); the detection conditions were: target material: Cu target, angle range: 10-50°, scanning time: 23 min, voltage: 10 kV, current: 5 mA, and the detection results were as follows: Figure 1 shown.

[0140] Characteristic peaks of layered oxide materials in Example 1: characteristic peak A: 18°~19°, characteristic peak B: 35°~36°, characteristic peak C: 36°~36.5°, characteristic peak D: 36.5°~37°, characteristic peak E: 44°~46°, characteristic peak F: 64°~64.5°, characteristic peak G: 65°~65.5°.

[0141] Among them, after the layered oxide material is made into a battery, its discharge Dq / Dv curve has two redox peaks in the same position in the range of 3.6-4.2V as that of a battery made of commercially available nickel cobalt manganese oxide lithium material.

[0142] Comparative Example 2 is a material obtained by directly adding 20% ​​molar ratio of Li to commercially available lithium nickel cobalt manganese oxide. The diffraction peak of the crystal structure of Li2MnO3 can be detected. That is, the material is not a pure phase layered structure, but a two-phase structure: zLi2MnO3·(1-z)LiNi 0.5 Co 0.2 Mn 0.3 O2.

[0143] Comparative Example 1 uses commercially available lithium nickel cobalt manganese oxide without any treatment, and from the XRD spectrum, it is a layered structure.

[0144] Example 1 is a layered oxide material (lithium-rich ternary material) Li prepared by the present invention 1.2 Ni 0.5 Co 0.15 Mn 0.3 Al 0.05 O2, from the XRD spectrum, has a layered structure and no impurity diffraction peaks.

[0145] (3) Specific surface area analysis

[0146] The specific surface area of ​​the layered oxide materials obtained in Example 1, Comparative Example 1 and Comparative Example 2 was measured using a specific surface area meter (JW-BK300, Precision Gaobo). Reference standard: GB / T13390; adsorbent: high-purity N2; sample amount: about 3.0-3.5 g (accurate to 0.0001); heating temperature: 100°C; heating time: 1 h; the test results are shown in Table 1.

[0147] (4)ICP element analysis

[0148] Detection equipment: Agilent 5110VDV ICP-OES; sample pretreatment; sample amount: about 0.25g±0.05 (accurate to 0.0001); 5ml ultrapure water + 1ml concentrated HNO3 (GR); digestion at 120℃ for 30min; the test results are shown in Table 1.

[0149] (5) Half-cell electrical performance analysis

[0150] The electrical properties of the layered oxides obtained in Example 1 and Comparative Example 1 were analyzed (2.85-4.5V0.1C). The results are as follows: Figure 2 shown.

[0151] Table 1

[0152]

[0153]

[0154] As can be seen from Table 1, by using the layered oxide material described in the present invention, while keeping the structure of the original material unchanged, by doping metal elements and controlling the molar ratio of lithium element and other metal elements, the layered oxide material prepared by the present invention is used in lithium-ion batteries, which improves the first efficiency and specific capacity of the battery and can be applied to high cut-off voltage.

[0155] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A layered oxide material, characterized in that: The chemical formula of the layered oxide material is: Li 1+x M y A (1-y) O2, wherein M is a transition metal cation, A is a doping element, 0<x<0.8, 0.9<y<1.0; the XRD spectrum of the layered oxide material has the following characteristic peaks: characteristic peak A: 18°~19°, characteristic peak B: 35°~36°, characteristic peak C: 36°~36.5°, characteristic peak D: 36.5°~37°, characteristic peak E: 44°~46°, characteristic peak F: 64°~64.5°, characteristic peak G: 65°~65.5°; the transition metal cation is at least one of Ni, Co, and Mn elements; the doping element is at least one of Mg, Al, Fe, Ti, Sb, V, Y, Ce, Nb, and Zr elements.

2. A layered oxide material according to claim 1, characterized in that: The weight percentage of the Li element in the layered oxide material is 7.8-12.8%.

3. A layered oxide material according to claim 1, characterized in that: The transition metal cation accounts for 45-60% of the layered oxide material by weight.

4. A layered oxide material according to claim 1, characterized in that: The median particle size D50 of the layered oxide is 3 to 16 μm, and the specific surface area is 0.2 to 15 m 2 / g.

5. A method for preparing a layered oxide material according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Raw material preparation: lithium salt, transition metal element salt, and doping element salt are prepared into a mixed solution with a metal ion concentration of 0.5 to 4 mol / L according to the metal molar ratio of 1+x:y:1-y; the precipitant is prepared into a solution with a concentration of 0.5 to 6 mol / L; the pH adjuster is prepared into a solution C with a concentration of 1 to 6 mol / L; the polymer surfactant is prepared into a solution with a concentration of 0.1 to 10 g / L; (2) Feeding reaction: Add a polymer surfactant to a reaction kettle containing deionized water, stir at a stirring speed of 500 to 1500 rpm for 20 to 80 min, and then use a metering pump to simultaneously add a transition metal soluble salt solution and a precipitant solution at a feed flow rate of 2 to 50 ml / min; (3) Aging and washing of the slurry: After the addition of the material in step (2) is completed, a pH adjusting agent solution is added at a feed flow rate of 5 to 50 ml / min using a metering pump to adjust the pH value to 7 to 11. After aging for 5 to 15 hours, the slurry is discharged into a centrifuge for washing and filtration; (4) Drying: Drying the filtered product obtained in step (3) to obtain a layered oxide precursor; (5) Sintering: The layered oxide precursor obtained in step (4) is placed in a muffle furnace, heated to 400-900° C. at a heating rate of 1-6° C. / min, and sintered for 2-20 h under protective atmosphere conditions. After natural cooling, the layered oxide material is obtained.

6. The method for preparing a layered oxide material according to claim 5, characterized in that: In step (1), the transition metal element salt and the doping element salt are at least one of chloride, sulfate, and nitrate; and the lithium salt is at least one of lithium chloride, lithium sulfate, lithium nitrate, lithium carbonate, lithium acetate, and lithium oxalate.

7. A positive electrode material, characterized in that: The positive electrode material comprises a positive electrode active material, a positive electrode binder and a positive electrode conductor, and the positive electrode active material is the layered oxide material according to any one of claims 1 to 4.

8. A positive electrode sheet, characterized in that: It comprises a positive current collector and a positive electrode material coated on the positive current collector, wherein the positive electrode material is the positive electrode material described in claim 7.

9. A lithium ion battery, characterized in that: The invention comprises the positive electrode sheet as claimed in claim 8.

10. A lithium ion battery according to claim 9, characterized in that: The discharge curve of the lithium-ion battery has two redox peaks in the range of 3.6-4.2V.

11. A lithium ion battery according to claim 10, characterized in that: The charging cut-off voltage of the lithium-ion battery is 4.0-5.0V.

Citation Information

Patent Citations

  • Preparation method of cathode material of lithium-rich ternary compound lithium ion battery

    CN103956477A

  • Preparation method of high-capacity lithium-rich ternary positive electrode material

    CN108063226A

  • Aluminum-coated lithium-rich ternary positive electrode material and preparation method thereof

    CN109755547A

  • Preparation method of submicron level LiniO.5MnO.5O2 cathode material

    CN101834291A

  • Zirconium-doped lithium-rich cathode material of lithium ion battery and preparation method of zirconium-doped lithium-rich cathode material

    CN105098158A