An integral slow-release iron-carbon catalytic material and its preparation method and application
Through the integrated sustained release iron-carbon catalytic material, the use of foam iron or foam nickel framework and porous structure silica and activated carbon composite materials, the separation and recovery of transition metal catalysts and complex acid-base regulation in the prior art are solved. The problem has achieved efficient degradation and stability improvement of petroleum hydrocarbon pollutants.
Patent Information
- Application Number
- CN202111277541.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-30
AI Technical Summary
Transition metal catalysts in existing advanced oxidation catalysts have difficulty in separation and recovery of metal ions, complex acid-base regulation and secondary pollution risks. In addition, iron-carbon reactions require acid-base regulation and iron sludge precipitation, making it difficult to achieve large-scale industrial applications.
The integrated sustained-release iron-carbon catalytic material is used, and the foam iron or foam nickel is used as the framework. Silicon dioxide and carbon and inorganic resistant oxide are distributed in the pores to form a porous structure, which weakens the null microelectrolytic reaction between iron and carbon. Combined with activated carbon composites to improve catalytic efficiency and stability.
It has achieved efficient degradation of petroleum hydrocarbon pollutants, reduced iron sludge generation, expanded the scope of pH application, improved the stability and application value of the catalyst, and avoided the problems of groove flow and dead zone caused by voids.
Smart Images

Figure CN116060006B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic materials, and in particular relates to a catalytic oxidation catalytic material and a preparation method thereof. Background Art
[0002] Advanced oxidation techniques (AOPs) can utilize highly active and strongly oxidizing free radical species generated by the activation of oxidants such as persulfate, percarbonate, hydrogen peroxide, and ozone to efficiently oxidize and degrade organic pollutants. They have the advantages of fast reaction rate, strong oxidation ability, almost no selectivity for organic matter, and high mineralization rate. They have received more and more widespread attention, especially in the field of organic pollutant wastewater treatment and have developed rapidly.
[0003] At present, commonly used advanced oxidation catalysts generally use transition metals as active components. The mass transfer rate of homogeneous transition metal ion catalytic oxidation systems is high, the probability of contact between catalysts and oxidants is large, and the catalytic reaction efficiency is high. However, there is a problem of difficulty in separating and recovering metal ions, especially transition metals such as Cu, Co, Ni, and Mn, which have strict limits in sewage discharge standards and are prone to secondary pollution. The reaction requires frequent adjustment of acidity and alkalinity, and precipitation is easily generated under alkaline conditions to reduce activity. Therefore, it is of great significance to develop heterogeneous catalysts based on transition metals.
[0004] Iron and iron-containing compounds are low-cost, environmentally friendly and other advantages as active components of catalysts, and are often used as activation materials for advanced oxidation reactions. Commonly used iron filings, zero-valent iron, and the latest research hotspots such as nano-zero-valent iron, nano-Fe3O4, and porous Fe2O3 particles can slowly release Fe in advanced oxidation reactions. 2+ , thereby controlling the activation speed of the oxidant and ensuring that the system continuously and efficiently degrades pollutants. The above materials have achieved good results in laboratory research, but they are difficult to apply on a large scale in industry due to their complex preparation methods.
[0005] The iron-carbon reaction uses the principle of electrochemical corrosion of metals to treat wastewater. The potential difference between the iron element and the carbon element can form a primary battery, generate electron flow, and electrolyze pollutants in the water. This reaction mainly uses the combined effects of iron's reducibility, iron's electrochemical properties, and iron ion flocculation and adsorption to purify wastewater. However, it needs to react under aeration and acidic conditions to achieve better treatment effects. Therefore, the pH value of the wastewater needs to be adjusted to 3-4 before the reaction, and the pH value after the reaction is about 5.7. In order to further remove Fe in the wastewater, 2+ and Fe 3+ , alkali needs to be added to adjust the pH value of the effluent to a weak alkaline state. The reaction has problems such as acid-base adjustment, iron sludge precipitation and hardening. The iron-carbon advanced oxidation reaction has broadened the application scope of the iron-carbon reaction.
[0006] CN109999811A discloses the preparation of a biomass iron-carbon composite material and its use in catalytic activation of sodium persulfate to degrade bisphenol A. Cherry pit powder and anhydrous FeCl3 are mixed evenly, calcined at high temperature under an inert atmosphere, and FeCl3 is used to decompose bisphenol A. 3+ The oxidative property of cherry pit powder can be utilized to activate the cherry pit powder, which is itself reduced to iron nanoparticles and loaded onto cherry pit powder biomass activated carbon. The material can be used to catalyze the activation of sodium persulfate to produce active free radicals to degrade the endocrine disruptor bisphenol A.
[0007] CN110429309A discloses a method for preparing a membraneless formic acid fuel cell based on an integral carbonaceous self-breathing cathode, comprising the following steps: 1. cathode preparation: step A, algae slurry preparation: dissolving protein core chlorella algae powder in an ethanol solution, stirring fully on a magnetic stirrer to prepare a paste-like algae slurry; step B, foamed iron-nickel loaded algae slurry: completely immersing the cut foamed iron-nickel into the prepared paste-like algae slurry, ultrasonically oscillating in an ultrasonic oscillator until the inside of the foamed iron-nickel is filled with algae slurry, and after drying, using a hot press to hot-press the foamed iron-nickel filled with algae slurry; step C, cathode carbonization, step D, cathode surface hydrophobic treatment; 2. anode preparation: electroplating a palladium catalyst layer on the surface of a graphite rod by a repeated deposition and impregnation method; 3. anode activation: immersing the anode in a sulfuric acid solution and activating it by cyclic voltammetry; 4. battery assembly. Summary of the invention
[0008] In view of the deficiencies in the prior art, the main purpose of the present invention is to provide a catalytic oxidation catalytic material and a preparation method and application thereof, and in particular to provide an integral slow-release iron-carbon catalytic material and a preparation method and application thereof. The catalytic material has the characteristics of stable structure and high catalytic degradation ability for petroleum hydrocarbon pollutants.
[0009] The first aspect of the present invention provides an integral slow-release iron-carbon catalytic material, which includes an iron source, silica, carbon and an inorganic refractory oxide. The catalytic material is based on the iron source, silica is coated on the surface of the iron source, and the carbon and the inorganic refractory oxide are distributed in the pores of the iron source and / or on its surface.
[0010] Furthermore, in the above-mentioned integral slow-release iron-carbon catalytic material, the iron source is foamed iron and / or foamed iron-nickel, wherein the porosity of the foamed iron is 50 to 98%, preferably 70 to 95%.
[0011] Furthermore, in the above-mentioned integral slow-release iron-carbon catalytic material, the pore distribution of the catalytic material has the following characteristics: the pore diameter of the first-level channel is less than 4nm, and the most probable pore diameter is 2.4nm; the pore diameter of the second-level channel is 4-9nm, and the most probable pore diameter is 7.3nm; the pore diameter of the third-level channel is greater than 9nm, preferably 9-20nm, and the most probable pore diameter is 13.3nm.
[0012] Furthermore, in the above-mentioned integral slow-release iron-carbon catalytic material, the ratio of the peak intensity (peak height) represented by the Y-axis coordinates corresponding to the most probable pore diameters of the primary pores, the second pores and the third pores is 10:3~15:4~20.
[0013] Furthermore, in the above-mentioned integral slow-release iron-carbon catalytic material, based on the weight of the catalytic material, the iron source content is 20wt%~50wt%, preferably 25wt%~40wt%; the silica content is 0.5wt%~6.0wt%, preferably 1.0wt%~4.0wt%; the carbon content is 10wt%~50wt%, preferably 20wt%~40wt%; the inorganic refractory oxide content is 15wt%~60wt%, preferably 20wt%~50wt%.
[0014] Furthermore, in the above-mentioned integral slow-release iron-carbon catalytic material, the thickness of the catalytic material is 1 to 10 mm.
[0015] Furthermore, in the above-mentioned monolithic slow-release iron-carbon catalytic material, the specific surface area of the catalytic material is 50 to 800 m 2 / g.
[0016] Furthermore, in the above-mentioned integral slow-release iron-carbon catalytic material, the inorganic refractory oxide can be one or more of alumina, molecular sieve, and clay; further, the molecular sieve can be selected from one or more of ZSM-5 molecular sieve, A-type molecular sieve, Y-type molecular sieve, and β molecular sieve; the clay can be silica-alumina clay with a particle size of 300 to 2000 mesh, the sum of the mass of SiO2 and Al2O3 in the component accounts for more than 80% of the total mass of silica-alumina clay, and the specific surface area is 5 to 500 m 2 / g.
[0017] The second aspect of the present invention provides a method for preparing a monolithic slow-release iron-carbon catalytic material, the preparation method comprising the following contents:
[0018] (1) Under contact conditions, the silicon-containing compound and the organic solvent are uniformly mixed to obtain material A;
[0019] (2) Under contact conditions, material A, iron source, formaldehyde, and additives are mixed and reacted, and material B is obtained after the reaction is completed and heat treated;
[0020] (3) Under contact conditions, the carbon precursor, the inorganic refractory oxide and the binder are uniformly mixed, and then further formed, heat treated and calcined with material B to obtain a catalytic material.
[0021] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the silicon-containing compound in step (1) is one or more of silica sol, water glass, sodium silicate, and silicic acid, preferably silica sol; and more preferably, the silica sol is an acidic silica sol with a pH between 2 and 5 and a mass fraction of 10 to 40%.
[0022] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the organic solvent in step (1) is an alcohol compound and / or an ether compound, wherein the alcohol compound can be selected from linear and / or branched alcohol compounds, preferably linear alcohol compounds.
[0023] Furthermore, in the preparation method of the above-mentioned monolithic slow-release iron-carbon catalytic material, the straight-chain alcohol compound can be selected from one or more of methanol, ethanol, n-propanol, n-butanol and n-pentanol, preferably ethanol. The branched alcohol compound can be selected from one or more of isopropanol, isobutanol and isopentanol. The ether compound can be specifically selected from one or more of diethyl ether, tetrahydrofuran and 1,4-dioxane, preferably tetrahydrofuran.
[0024] Furthermore, in the preparation method of the above-mentioned monolithic slow-release iron-carbon catalytic material, a silicon-containing auxiliary agent can be further introduced when mixing the silicon-containing compound with the organic solvent in step (1), and the silicon-containing auxiliary agent is an organic silicone ester and / or an organic siloxane, which can be specifically selected from one or more of tetraethyl silicate, methyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, trimethylchlorosilane, and octyltrimethoxysilane; preferably tetraethyl silicate. The mass of silicon dioxide in the silicon-containing auxiliary agent accounts for 10 to 40% of the total mass of silicon dioxide.
[0025] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the iron source in step (2) is foamed iron and / or foamed iron-nickel, preferably foamed iron; further, the porosity of the foamed iron is generally 50-98%, preferably 70-95%.
[0026] Furthermore, in the preparation method of the above-mentioned monolithic slow-release iron-carbon catalytic material, the iron source in step (2) is usually purified before use, and the iron source is added to an acidic solution for soaking during the purification process. The acidic solution can be one or more of hydrochloric acid, nitric acid, and sulfuric acid, preferably nitric acid; the mass fraction of the acidic solution is 3-30%. The mass ratio of the acidic solution to the iron source can generally be 10-40:1.
[0027] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the heat treatment temperature in step (2) is 50-100°C, preferably 55-75°C, and it is further preferred to carry out the heat treatment under vacuum conditions, specifically, a vacuum drying oven can be used. The choice of heat treatment equipment can be selected by those skilled in the art according to actual needs.
[0028] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the auxiliary agent in step (2) is at least one of phenol, cresol, xylenol, resorcinol, and urea, and the molar ratio of phenol, cresol, xylenol, resorcinol or urea to formaldehyde is 0.5 to 0.9:1.
[0029] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the reaction in step (2) is carried out under acidic conditions, and specifically, the pH value of the system can be adjusted to no more than 7 by an acidic substance, and the preferred pH value is 1.0 to 3.0; the acidic substance can be at least one of hydrochloric acid, carbonic acid, oxalic acid, and citric acid, and preferably hydrochloric acid is used for adjustment.
[0030] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the carbon precursor in step (3) can be one or more selected from biomass charcoal, petroleum-based charcoal, coal-based charcoal, etc., and the carbon content in the carbon precursor is higher than 60wt%, specifically; it can be one or more of activated carbon, fruit shell powder, wood powder, coconut shell powder, coal powder, coal tar, asphalt, organic polymer (the organic polymer can be one or more of polyethylene, polystyrene, polyvinyl chloride, polyacrylic acid, polyacrylonitrile, polymethyl methacrylate, polylactic acid, polycarbonate, phenolic resin, urea-formaldehyde resin), cellulose.
[0031] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the inorganic refractory oxide in step (3) can be one or more of alumina, molecular sieve, and clay; further, the molecular sieve can be one or more of ZSM-5 molecular sieve, A-type molecular sieve, Y-type molecular sieve, and β molecular sieve; the clay can be silica-alumina clay with a particle size of 300 to 2000 mesh, the sum of the mass of SiO2 and Al2O3 in the component accounts for more than 80% of the total mass of the silica-alumina clay, and the specific surface area is 5 to 500 m 2 / g.
[0032] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the binder in step (3) is one or more of water, an inorganic binder and an organic binder, the inorganic binder can be selected from one or more of silica sol, aluminum sol, aluminum dihydrogen phosphate, and water glass, and the organic binder can be selected from one or more of hydroxymethyl cellulose, carboxymethyl cellulose, carboxyethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol, and polyethylene glycol.
[0033] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the specific molding process described in step (3) is generally to first introduce the material obtained by evenly mixing the carbon precursor, the inorganic refractory oxide and the binder into the gaps of the material B, preferably by pressing, and specifically by a template extrusion molding method.
[0034] Furthermore, in the method for preparing the above-mentioned integral slow-release iron-carbon catalytic material, the heat treatment temperature in step (3) is 50 to 100°C, preferably 55 to 75°C.
[0035] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the calcination in step (3) is carried out under oxygen-free conditions, such as in an inert atmosphere such as nitrogen, helium, neon, argon, etc., and the calcination temperature is 500-900°C, preferably 600-700°C; the calcination time is 1-8h, preferably 2-4h.
[0036] The third aspect of the present invention provides an integral slow-release iron-carbon catalytic material obtained by the above-mentioned preparation method.
[0037] The fourth aspect of the present invention provides an application of the above-mentioned integral slow-release iron-carbon catalytic material in the treatment of organic wastewater. The specific process is that in the presence of the above-mentioned integral slow-release iron-carbon catalytic material, the organic wastewater contacts and reacts with an oxidant to obtain purified water after the reaction.
[0038] Furthermore, in the application of the above-mentioned integral slow-release iron-carbon catalytic material in the treatment of organic wastewater, the oxidant is one or more of ozone, hydrogen peroxide, sodium persulfate, and sodium percarbonate.
[0039] Furthermore, in the application of the above-mentioned integral slow-release iron-carbon catalytic material in the treatment of organic wastewater, the organic wastewater is wastewater containing petroleum hydrocarbons, wherein the petroleum hydrocarbons contained therein are mainly C4-C40 hydrocarbons, and the hydrocarbons are generally one or more of alkanes, olefins, benzene series, halogenated hydrocarbons, etc.
[0040] Compared with the prior art, the monolithic slow-release iron-carbon catalytic material and its preparation method and application described in the present invention have the following advantages:
[0041] The present invention provides a slow-release iron-carbon catalytic material with foamed iron and / or foamed iron-nickel as a skeleton, wherein the iron source is impregnated in a silica-containing sol, and silicon dioxide is pre-mixed and cross-linked to form a hydrophobic silicon dioxide porous structure to wrap the foamed iron and / or foamed iron-nickel active center therein, and iron and carbon undergo micro-electrolysis reaction through the pores, which significantly weakens the ineffective micro-electrolysis reaction of iron and carbon, so that iron slowly participates in the reaction and is not easy to produce iron mud. A small amount of carbonizable precursor auxiliary agent is introduced in an in-situ generated manner, which can firmly bond the foamed iron skeleton and silicon dioxide, which not only enhances the bonding ability of the two, but also protects the reduction performance of the foamed iron during high-temperature roasting. The catalyst is used in combination with an oxidant in an advanced oxidation manner, has a wider pH application range, and has a wider application value.
[0042] In the slow-release iron-carbon catalytic material with foamed iron and / or foamed iron-nickel as the skeleton provided by the present invention, the activated carbon composite material is filled in the skeleton of foamed iron and / or foamed iron to form a monolithic catalytic material, and the activated carbon composite material is in uniform contact with the iron surface, so that the micro-electrolysis reaction that occurs is also relatively uniform, and when the wastewater containing pollutants passes through the catalytic material, the problems such as channel flow and dead zone caused by the gap are avoided. Moreover, the activated carbon composite material has a strong adsorption capacity for organic pollutant components, and the pollutant molecules can be adsorbed to the surface of the catalytic material, so that the probability of contact between the active components and the pollutant molecules is increased, the local concentration is increased, and the initial reaction rate is promoted to increase, which is conducive to the catalytic oxidation reaction. The content of activated carbon in the activated carbon composite material is controlled at a reasonable ratio, and the ineffective reaction of iron-carbon micro-electrolysis is also significantly reduced. The activated carbon composite material has a porous structure, and can also adsorb the iron ions produced by the iron-carbon reaction, form catalytic active centers in situ, and continuously maintain good catalytic oxidation activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is the pore size distribution diagram of the catalytic material A1 prepared in Example 1 of the present invention.
[0044] Figure 2 This is an electron microscope photograph (100 microns) of the catalytic material A2 prepared in Example 2 of the present invention.
[0045] Figure 3 This is an electron microscope photograph (1 mm) of the catalytic material A2 prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0046] The preparation method of the present invention is further described below in conjunction with specific examples, but the scope of the present invention is not limited to the scope of these examples.
[0047] The specific surface area and average pore size involved in the embodiments of the present invention and the comparative examples are measured by a nitrogen physical adsorption instrument. The ratio of the most probable pore size corresponding to the Y-axis value on the pore size distribution curve is recorded as the peak intensity ratio. The iron ion analysis method is microwave digestion / inductively coupled plasma mass spectrometry. The silica content involved in the present invention is the mass of silica combined with the iron source when added, excluding the mass of silica introduced in the inorganic refractory oxide and the binder.
[0048] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned in this specification are based on weight and pressure is gauge pressure.
[0049] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0050] In this document, for the convenience of description, spatial relative terms such as "below", "below", "down", "above", "above", "upper", etc. may be used to describe the relationship between one element or feature and another element or feature in the accompanying drawings. It should be understood that the spatial relative terms are intended to include different directions of objects in use or operation in addition to the directions drawn in the drawings. For example, if the object in the figure is turned over, the elements described as being "below" or "below" other elements or features will be oriented "above" the elements or features. Therefore, the exemplary term "below" can include both below and above directions. Objects may also have other orientations (rotated 90 degrees or other orientations) and the spatial relative terms used in this document should be interpreted accordingly.
[0051] In this document, the terms "first", "second", etc. are used to distinguish two different elements or parts, and are not used to limit a specific position or relative relationship. In other words, in some embodiments, the terms "first", "second", etc. can also be interchangeable.
[0052]
[0043] All numerical values for parameters (eg, amounts or conditions) herein are to be understood as being modified in all instances by the term "about", whether or not "about" actually appears before the numerical value.
[0053] In the context of this specification, any two or more embodiments of the present invention may be arbitrarily combined, and the technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.
[0054] Example 1
[0055] Catalytic material A1
[0056] Weigh 50g of 30% silica sol, 10.4g of tetraethyl silicate, and 15g of ethanol, add water to 100mL, and stir evenly to obtain material A. Immerse 20g of foamed iron washed with 5wt% nitric acid into material A, and add 1.6g of formaldehyde and 10.4g of phenol at the same time. Adjust the pH value to 2.5 with hydrochloric acid, stir the reaction in a 50℃ water bath for 20min, and let it stand for 12h. Take out the foamed iron and dry it in a vacuum at 70℃ for 4h to obtain material B. Mix activated carbon, alumina, and water glass in a mass ratio of 2:1:0.3, add water to adjust to viscosity, and then press it with a flat plate to introduce it into the gap of material B. After forming, dry it at 70℃ for 7h, and then calcine it at 600℃ for 3h under anaerobic conditions. Take it out after cooling to obtain catalytic material A1. The specific surface area of the catalytic material is 441m 2 / g, the peak intensity ratios at 2.4nm, 7.3nm and 13.3nm are 10.0:6.6:6.8.
[0057] Example 2
[0058] Catalytic material A2
[0059] Weigh 24.5g of sodium silicate, 7.4g of methyltriethoxysilane, 30ml of ethanol and 70mL of distilled water and mix to obtain material A. Weigh 26g of foamed iron, add it to material A, stir evenly, add 5.7g of urea, add 2.3g of formaldehyde dropwise, adjust the pH to 2.8 with citric acid, continue stirring for 30min and let stand for 10h, generate resin material in situ, attach it to the surface of the foamed iron pores together with silicon dioxide, then put it into a rotary evaporator and dry it in a vacuum at 75°C to obtain material B. Mix activated carbon, silica-alumina clay and hydroxypropyl methylcellulose in a mass ratio of 1.0:2.0:0.2, add water to adjust to viscosity, then use a tablet press to press and introduce it into the gap of material B, dry it at 75°C for 6h after molding, then calcine it at 650°C for 3h under anaerobic conditions, take it out after cooling, and obtain catalytic material A2. The specific surface area of the catalytic material is 203m 2 / g, the peak intensity ratios at 2.4nm, 7.3nm and 13.3nm are 10.0:7.6:12.1.
[0060] Example 3
[0061] Catalytic material A3
[0062] Weigh 25g of 40% silica sol, 7.3g of tetraethyl silicate, 20mL of tetrahydrofuran and 60mL of distilled water, mix, stir evenly, add 9.8g of resorcinol, and adjust the pH to 1.8 with hydrochloric acid. Weigh 35g of foamed iron, add it to the above sol, soak for 1h, add 2.2g of formaldehyde, continue stirring for 30min, let stand for 10h, then take out, dry the material at 65℃ to obtain material B. Mix activated carbon, silica-alumina clay, and dihydrogen aluminum phosphate in a mass ratio of 2.8:2.5:0.5, add water to adjust to viscosity, then press with a flat plate to introduce it into the gap of material B, dry at 60℃ for 10h after molding, then calcine at 700℃ for 4h under anaerobic conditions, take out after cooling, and obtain catalytic material A3. The specific surface area of the catalytic material is 383m 2 / g, the peak intensity ratios at 2.4nm, 7.3nm and 13.3nm are 10.0:6.8:7.0.
[0063] Example 4
[0064] Catalytic material A4
[0065] Weigh 17.5g of silicic acid, 9g of trimethylchlorosilane, 50ml of ethanol and 50mL of deionized water to mix to obtain material A. After stirring evenly, add 18g of foamed iron nickel to material A, then add 2.2g of formaldehyde and 7.8g of phenol and continue stirring for 30min, then stand for 24h, and evaporate the excess water at 75℃ to obtain material B. Mix the fruit shell powder, silica-alumina clay and aluminum dihydrogen phosphate in a mass ratio of 1.8:1.0:0.3, add water to adjust to viscosity, and then press it into the gap of material B with a tablet press. After forming, dry it at 90℃ for 6h, then roast it at 620℃ for 4h under anaerobic conditions, and take it out after cooling to obtain catalytic material A4. The specific surface area of the catalytic material is 197m 2 / g, the peak intensity ratios at 2.4nm, 7.3nm and 13.3nm are 10.0:6.7:9.2.
[0066] Example 5
[0067] Catalytic material A5
[0068] Weigh 60g of 20% acidic silica sol, 8.6g of tetraethyl silicate, 50mL of ether and 20mL of deionized water and mix them evenly to obtain material A. Then add 8.1g of urea, stir and add 20g of foamed iron nickel to the above material A, drop 2.9g of formaldehyde and continue stirring for 30min, then let stand for 24h, and evaporate the excess water at 68℃ to obtain material B. Mix activated carbon and silica-alumina clay in a mass ratio of 2.0:1.2, add water to adjust to viscosity, and then press with a flat plate to introduce it into the gap of material B. After molding, dry at 72℃ for 6h, then calcine at 660℃ for 4h under anaerobic conditions, take out after cooling, and obtain catalytic material A5. The specific surface area of the catalytic material is 387m 2 / g, the peak intensity ratios at 2.4nm, 7.3nm and 13.3nm are 10.0:3.2:7.2.
[0069] Example 6
[0070] Weigh 60g of 30% acidic silica sol and 40mL of deionized water and mix them evenly to obtain material A. Then add 8.4g of xylenol, stir and add 32g of foamed iron to the above material A, add 1.6g of formaldehyde and continue stirring for 30min, then let stand for 24h, and evaporate the excess water at 75℃ to obtain material B. Mix activated carbon, 5A molecular sieve and hydroxypropyl methylcellulose in a mass ratio of 2.5:3.0:0.1, add water to adjust to viscosity, and then press with a flat plate to introduce it into the gap of material B. After forming, dry it at 55℃ for 12h, then calcine it at 660℃ for 4h under anaerobic conditions, and take it out after cooling to obtain catalytic material A6. The specific surface area of the catalytic material is 276m 2 / g, the peak intensity ratios at 2.4nm, 7.3nm and 13.3nm are 10.0:8.1:10.6.
[0071] Example 7
[0072] Weigh 37.5 g of acidic silica sol with a mass concentration of 40% and 50 mL of deionized water and mix them evenly to obtain material A. Then add 7.7 g of urea, stir, add 28 g of foamed iron to the above material A, add 3.3 g of formaldehyde and continue stirring for 15 minutes, then let it stand for 20 hours, and evaporate the excess water at 70°C to obtain material B. Mix activated carbon, ZSM-5 molecular sieve and carboxymethyl cellulose in a mass ratio of 1.0:1.8:0.1, add water to adjust to viscosity, and then press with a flat plate to introduce it into the gap of material B. After molding, dry it at 75°C for 5 hours, then calcine it at 680°C for 3 hours under anaerobic conditions, and take it out after cooling to obtain catalytic material A7. The specific surface area of the catalytic material is 293m 2 / g, the peak intensity ratios at 2.4nm, 7.3nm and 13.3nm are 10.0:5.2:11.8.
[0073] Example 8
[0074] The catalytic material A1 was cut into a circle and 5 layers were stacked and loaded into a cylindrical reaction tube. Gasoline simulated petroleum hydrocarbon wastewater with a COD of about 100 mg / L was introduced from the bottom. Under the condition of a sodium persulfate dosage of 200 mg / L, the COD removal rate after stable operation can reach 90.6%, and the iron ion concentration in the effluent is 61 mg / L.
[0075] Example 9
[0076] The catalytic material A2 was cut into a circle, 5 layers were stacked and loaded into a cylindrical reaction tube, and diesel simulated petroleum hydrocarbon wastewater with a COD of 100 mg / L was introduced. Under the condition of a sodium persulfate dosage of 300 mg / L, the COD removal rate after stable operation can reach 87.5%, and the iron ion concentration in the effluent is 73 mg / L.
[0077] Example 10
[0078] The catalytic material A3 was cut into a circle, 10 layers were stacked and loaded into a cylindrical reaction tube, and gasoline-simulated petroleum hydrocarbon wastewater with a COD of 300 mg / L was introduced. Under the condition of a sodium persulfate dosage of 250 mg / L, the COD removal rate after stable operation can reach 84.3%, and the iron ion concentration in the effluent is 86 mg / L.
[0079] Embodiment 11
[0080] The catalytic material A4 was cut into long strips and used in a box reactor. A catalyst plate was fixed every 3 mm, and a total of 5 plates were fixed. Gasoline-simulated petroleum hydrocarbon wastewater with a COD of 120 mg / L was slowly passed through the catalytic material, and sodium persulfate was added to the raw water at a dosage of 200 mg / L. After stable operation, the COD removal rate can reach 86.2%, and the iron ion concentration in the effluent is 77 mg / L.
[0081] Example 12
[0082] The catalytic material A5 was cut into long strips and used in a box reactor. A catalyst plate was fixed every 3 mm, and a total of 5 plates were fixed. Gasoline-simulated petroleum hydrocarbon wastewater with a COD of 120 mg / L was slowly passed through the catalytic material, and sodium persulfate was added to the raw water at a dosage of 200 mg / L. After stable operation, the COD removal rate can reach 88.9%, and the iron ion concentration in the effluent is 71 mg / L.
[0083] Example 13
[0084] The catalytic material A6 was cut into a circle, 5 layers were stacked and loaded into a cylindrical reaction tube, and diesel simulated petroleum hydrocarbon wastewater with a COD of 180 mg / L was introduced. Under the condition of a sodium persulfate dosage of 250 mg / L, the COD removal rate after stable operation can reach 89.2%, and the iron ion concentration in the effluent is 81 mg / L.
[0085] Embodiment 14
[0086] The catalytic material A7 was cut into a circle, 10 layers were stacked and loaded into a cylindrical reaction tube, and gasoline-simulated petroleum hydrocarbon wastewater with a COD of 200 mg / L was introduced. Under the condition of a sodium persulfate dosage of 250 mg / L, the COD removal rate after stable operation can reach 90.3%, and the iron ion concentration in the effluent is 87 mg / L.
[0087] Comparative Example 1
[0088] 32g and 16g of iron filings and activated carbon were weighed respectively, mixed and loaded in a cylindrical reaction tube, and the conventional iron-carbon reaction was used for continuous reaction to treat gasoline simulated petroleum hydrocarbon wastewater with a COD of 150 mg / L. There was obvious yellow precipitation in the effluent, and the contact between the iron filings and the activated carbon quickly hardened. The iron ion concentration was 5813 mg / L, and the COD removal rate was 94.1% after the iron ions were precipitated.
[0089] Comparative Example 2
[0090] Weigh 25g and 50g of foamed iron and activated carbon respectively, mix and load them in a cylindrical reaction tube, and continuously react and treat diesel simulated petroleum hydrocarbon wastewater with COD of 100mg / L under the action of 200mg / L of sodium persulfate. The contact between foamed iron and activated carbon quickly hardens. The iron ion concentration in the effluent is 5336 mg / L, and the COD removal rate is 86.1% after the iron ions are precipitated.
[0091] Comparative Example 3
[0092] Weigh 25g, 30g and 20g of foamed iron, activated carbon and inert porcelain balls respectively, mix and load them in a cylindrical reaction tube, add 200mg / L of sodium persulfate, and treat diesel simulated petroleum hydrocarbon wastewater with COD of 200mg / L. The reaction runs continuously, and the contact between foamed iron and activated carbon quickly hardens. The iron ion concentration in the effluent is 4687 mg / L, and the COD removal rate is 82.5% after the iron ions are precipitated.
[0093] Comparative Example 4
[0094] Weigh 25g of foamed iron, mix activated carbon, silica-alumina clay and 30% silica sol in a mass ratio of 45:47:8, add water to adjust to viscosity, and then press with a flat plate to introduce it into the gaps of the foamed iron. After molding, dry it at 80°C for 5h, and then calcine it at 600°C for 3h under anaerobic conditions. After cooling, take it out to obtain a catalytic material.
[0095] The catalytic material was cut into a circle, 5 layers were stacked and loaded into a cylindrical reaction tube, and gasoline-simulated petroleum hydrocarbon wastewater with a COD of 150 mg / L was introduced. Under the condition of a sodium persulfate dosage of 200 mg / L, the COD removal rate after stable operation can reach 80.5%, and the iron ion concentration in the effluent is 2393 mg / L.
Claims
1. An integral slow-release iron-carbon catalytic material, the catalytic material comprising an iron source, silicon dioxide, carbon and an inorganic refractory oxide, the catalytic material having an iron source as a substrate, silicon dioxide coated on the surface of the iron source, carbon and the inorganic refractory oxide distributed in the pores of the iron source and / or on its surface; the iron source is foamed iron and / or foamed iron-nickel; The method for preparing the monolithic slow-release iron-carbon catalytic material comprises the following contents: (1) Under contact conditions, a silicon-containing compound and an organic solvent are uniformly mixed to obtain material A; a silicon-containing auxiliary agent is introduced when the silicon-containing compound and the organic solvent are mixed, and the silicon-containing auxiliary agent is an organic silicone ester and / or an organic siloxane; (2) under contact conditions, material A, an iron source, formaldehyde, and an auxiliary agent are mixed and reacted, and after the reaction is completed and heat treated, material B is obtained; the auxiliary agent is at least one of phenol, cresol, xylenol, resorcinol, and urea; (3) Under contact conditions, the carbon precursor, the inorganic refractory oxide and the binder are uniformly mixed, and then further formed, heat treated and calcined with material B to obtain a catalytic material.
2. The monolithic slow-release iron-carbon catalytic material according to claim 1, wherein: The porosity of foamed iron is 50-98%.
3. The monolithic slow-release iron-carbon catalytic material according to claim 1, wherein: The porosity of foamed iron is 70-95%.
4. The monolithic slow-release iron-carbon catalytic material according to claim 1, wherein: In the integral slow-release iron-carbon catalytic material, the pore distribution of the catalytic material has the following characteristics: the pore diameter of the first-level channel is less than 4nm, and the most probable pore diameter is 2.4nm; the pore diameter of the second-level channel is 4-9nm, and the most probable pore diameter is 7.3nm; the pore diameter of the third-level channel is 9-20nm, and the most probable pore diameter is 13.3nm.
5. The monolithic slow-release iron-carbon catalytic material according to claim 4, wherein: The peak intensity ratios represented by the Y-axis coordinates of the most probable apertures of the first-order pores, the second-order pores and the third-order pores are 10:3 to 15:4 to 20.
6. The monolithic slow-release iron-carbon catalytic material according to claim 1, wherein: Based on the weight of the catalytic material, the iron source content is 20wt% to 50wt%, the silicon dioxide content is 0.5wt% to 6.0wt%, the carbon content is 10wt% to 50wt%, and the inorganic refractory oxide content is 15wt% to 60wt%.
7. The monolithic slow-release iron-carbon catalytic material according to claim 1 or 6, wherein: Based on the weight of the catalytic material, the iron source content is 25wt% to 40wt%; the silicon dioxide content is 1.0wt% to 4.0wt%; the carbon content is 20wt% to 40wt%; and the inorganic refractory oxide content is 20wt% to 50wt%.
8. The monolithic slow-release iron-carbon catalytic material according to claim 1, wherein: The thickness of the catalytic material is 1 to 10 mm.
9. The monolithic slow-release iron-carbon catalytic material according to claim 1, wherein: The specific surface area of the catalytic material is 50 to 800 m 2 / g.
10. The monolithic slow-release iron-carbon catalytic material according to claim 1, wherein: The inorganic refractory oxide is one or more of alumina, molecular sieve, and clay; the molecular sieve is one or more of ZSM-5 molecular sieve, A-type molecular sieve, Y-type molecular sieve, and β molecular sieve; the clay is silica-alumina clay, with a particle size of 300 to 2000 mesh, the sum of the mass of SiO2 and Al2O3 in the components accounts for more than 80% of the total mass of silica-alumina clay, and the specific surface area is 5 to 500m 2 / g.
11. A method for preparing a monolithic slow-release iron-carbon catalytic material, the method comprising the following contents: (1) Under contact conditions, a silicon-containing compound and an organic solvent are uniformly mixed to obtain material A; a silicon-containing auxiliary agent is introduced when the silicon-containing compound and the organic solvent are mixed, and the silicon-containing auxiliary agent is an organic silicone ester and / or an organic siloxane; (2) under contact conditions, material A, an iron source, formaldehyde, and an auxiliary agent are mixed and reacted, and after the reaction is completed and heat treated, material B is obtained; the iron source is foamed iron and / or foamed iron-nickel; the auxiliary agent is at least one of phenol, cresol, xylenol, resorcinol, and urea; (3) Under contact conditions, the carbon precursor, the inorganic refractory oxide and the binder are uniformly mixed, and then further formed, heat treated and calcined with material B to obtain a catalytic material.
12. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: The silicon-containing compound in step (1) is one or more of silica sol, water glass, sodium silicate and silicic acid.
13. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11 or 12, wherein: The silicon-containing compound in step (1) is silica sol, which is an acidic silica sol with a pH value between 2 and 5 and a mass fraction between 10 and 40%.
14. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: In step (1), the organic solvent is an alcohol compound and / or an ether compound, wherein the alcohol compound is selected from linear and / or branched alcohol compounds.
15. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 14, wherein: The straight-chain alcohol compound is selected from one or more of methanol, ethanol, n-propanol, n-butanol and n-pentanol; the branched alcohol compound is selected from one or more of isopropanol, isobutanol and isopentanol; the ether compound is selected from one or more of diethyl ether, tetrahydrofuran and 1,4-dioxane.
16. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 14 or 15, wherein: The straight-chain alcohol compound is selected from ethanol; the ether compound is selected from tetrahydrofuran.
17. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: The silicon-containing auxiliary agent is selected from one or more of tetraethyl silicate, methyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, trimethylchlorosilane, and octyltrimethoxysilane.
18. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11 or 17, wherein: The silicon-containing additive is tetraethyl silicate.
19. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: In step (2), the iron source is foamed iron, and the porosity of the foamed iron is 50-98%.
20. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 19, wherein: The porosity of foamed iron is 70-95%.
21. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: The heat treatment temperature in step (2) is 50-100°C.
22. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11 or 21, wherein: In step (2), the heat treatment temperature is 55-75° C. and the heat treatment is carried out under vacuum conditions.
23. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: In step (2), the molar ratio of the auxiliary agent to formaldehyde is 0.5-0.9:
1.
24. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: The reaction in step (2) is carried out under acidic conditions, and the pH value of the system is adjusted to no more than 7 by using an acidic substance; the acidic substance is at least one of hydrochloric acid, carbonic acid, oxalic acid, and citric acid.
25. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11 or 24, wherein: The reaction in step (2) is carried out under acidic conditions, and the pH value of the system is adjusted to 1.0-3.0 by an acidic substance; the acidic substance is hydrochloric acid.
26. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: In step (3), the carbon precursor is selected from one or more of biomass carbon, petroleum-based carbon, and coal-based carbon, and the carbon content of the carbon precursor is higher than 60wt%.
27. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11 or 26, wherein: In step (3), the carbon precursor is one or more of activated carbon, fruit shell powder, wood powder, coconut shell powder, coal powder, coal tar, asphalt, organic polymer, and cellulose.
28. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: The inorganic refractory oxide in step (3) is one or more of alumina, molecular sieve, and clay.
29. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: In step (3), the binder is one or more of water, an inorganic binder and an organic binder, wherein the inorganic binder is selected from one or more of silica sol, alumina sol, aluminum dihydrogen phosphate and water glass, and the organic binder is selected from one or more of hydroxymethyl cellulose, carboxymethyl cellulose, carboxyethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol and polyethylene glycol.
30. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: The heat treatment temperature in step (3) is 50-100°C.
31. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: The heat treatment temperature in step (3) is 55-75°C.
32. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: In step (3), the calcination is carried out under oxygen-free conditions at a temperature of 500 to 900°C.
33. The method for preparing the monolithic slow-release iron-carbon catalytic material according to claim 11, wherein: In step (3), the calcination is carried out under oxygen-free conditions at a temperature of 600-700°C.
34. Use of the integral slow-release iron-carbon catalytic material described in any one of claims 1 to 10 or the integral slow-release iron-carbon catalytic material obtained by the preparation method described in any one of claims 11 to 33 in the treatment of organic wastewater, wherein the application process is that in the presence of the integral slow-release iron-carbon catalytic material, the organic wastewater contacts and reacts with an oxidant to obtain purified water after the reaction.
35. Use of the monolithic slow-release iron-carbon catalytic material in organic wastewater treatment according to claim 34, wherein: The oxidant is one or more of ozone, hydrogen peroxide, sodium persulfate and sodium percarbonate.
36. Use of the monolithic slow-release iron-carbon catalytic material according to claim 34 in treating organic wastewater, wherein: Organic wastewater refers to wastewater containing petroleum hydrocarbons.