A descaling and bleaching treatment bath and its application
By using alkali metal hydroxide, penetrant, bleach and titanium dioxide in the reboiling bleach treatment bath, combined with photocatalysis and ultrasonic technology, the problem of poor effect of traditional reboiling bleaching technology at low temperatures is solved, and the fabric performance is improved and processing efficiency, achieving energy-saving and environmentally friendly efficient anti-brewing effect.
Patent Information
- Application Number
- CN202310054895.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-02-03
AI Technical Summary
The existing polyester and cotton fabric anti-brewing process is difficult to achieve good results when it is below 80°C, and the traditional process consumes high water and energy, and has serious pollution, which damages the performance of the fabric.
The anti-brew bleaching treatment bath containing alkali metal hydroxide, penetrant, bleach, hydrogen peroxide solution and titanium dioxide is adopted. Through the photocatalytic technology of titanium dioxide and ultrasonic technology, the processing temperature and time are reduced, the processing efficiency is improved, and energy saving is saved.
It significantly improves the desizing rate, whiteness and tensile strength of polyester-cotton fabrics, reduces processing time and energy consumption, and achieves an environmentally friendly and efficient anti-brewing effect.
Smart Images

Figure BDA0004060158380000031 
Figure BDA0004060158380000101 
Figure BDA0004060158380000102
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of descaling, boiling and bleaching treatment of polyester-cotton fabrics, in particular to a descaling, boiling and bleaching treatment bath and application thereof. Background Art
[0002] The sizing agents used for sizing polyester-cotton fabrics are generally natural sizing agents such as starch or synthetic sizing agents such as polyvinyl alcohol or polyacrylic acid, which are difficult to degrade.
[0003] CN115434168A discloses a one-bath two-step exhaust dyeing method for polyester-cotton fabrics using disperse reactive dyes, and relates to the field of one-bath two-step exhaust dyeing for polyester-cotton fabrics. The method comprises the following steps: pre-treatment, dyeing and post-treatment. When performing the descaling and bleaching operation on the polyester-cotton fabric, hydrogen peroxide, caustic soda, an oxygen bleaching stabilizer and a metal complexing agent are added into a dyeing vat at 80-100 DEG C. The caustic soda is used to deform the cotton protein in the polyester-cotton fabric to prevent the polyester-cotton fabric from subsequently turning yellow. The hydrogen peroxide is used to bleach the polyester-cotton fabric to ensure the base color of the polyester-cotton fabric and reduce the color difference of the polyester-cotton fabric after one-bath two-step dyeing. The oxygen bleaching stabilizer is used to stabilize the hydrogen peroxide, inhibit the growth of anaerobic microorganisms and improve the antiseptic effect of the polyester-cotton fabric. The metal complexing agent further stabilizes the hydrogen peroxide by using the strong binding effect between the chelating agent molecules and the metal ions and improves the color fastness of the dye. In addition, in the subsequent dyeing process of step S5, a weak acid penetrant is used to neutralize the caustic soda, improve the dyeing K / S value and enhance the dye depth.
[0004] CN108193477A discloses a short-process pretreatment process for enzyme oxygen descaling and bleaching of cotton fabric, which comprises the following steps: preparing enzyme oxygen descaling and bleaching finishing liquid; the singed cotton fabric is immersed and rolled twice in the enzyme oxygen descaling and bleaching finishing liquid, and the rolling rate is 80%-90%; steaming, 100℃, 45 minutes; washing, 95℃, 2 grids, 85℃, 3 grids, cold water, 2 grids; drying; the enzyme oxygen descaling and bleaching finishing liquid is prepared from 1.5-3kg of pectinase, 0.5-1kg of cellulase, 5-7kg of chelating dispersant, 4-6kg of hydrogen peroxide, 1.5-2kg of hydrogen peroxide stabilizer, 1-2kg of penetrant, and 500kg of tap water. The short-process pretreatment saves water, electricity, steam, and time; reduces the amount of caustic soda and hydrogen peroxide; the process is simple and easy to operate.
[0005] In the existing technology, it is difficult for general chemical descaling and bleaching processes to achieve good results at temperatures below 80°C. Traditional pretreatment of polyester-cotton fabrics uses caustic soda and chemical additives, which has a long process route, high water and energy consumption, and serious pollution. At the same time, the properties of the polyester-cotton fabric itself, such as strength, are also greatly damaged.
[0006] In summary, it is crucial to develop a descaling and bleaching bath and pretreatment process that can overcome the above-mentioned defects. Summary of the invention
[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a desizing bath and an application thereof. When the desizing bath is used in a pretreatment process, the desizing rate, whiteness and tensile strength of the obtained polyester-cotton fabric are significantly higher than those of conventional desizing and desizing treatment. Moreover, this method can not only achieve the effect of a conventional one-bath method over a longer period of time in a shorter period of time, but also significantly reduce the treatment temperature, thereby saving time, improving processing efficiency and saving energy.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a descaling and bleaching treatment bath, comprising the following components: an alkali metal hydroxide, a penetrant, a bleaching agent, a hydrogen peroxide solution, titanium dioxide and a dispersant.
[0010] In the present invention, titanium dioxide is added to the descaling and bleaching treatment bath, and then combined with other components to form a descaling and bleaching treatment bath, which can achieve the effect of a conventional one-bath method for a longer time when used in a pretreatment process, and can significantly reduce the treatment temperature and time, thereby achieving energy conservation and environmental protection, improving processing efficiency, and saving energy. Specifically, titanium dioxide plays multiple roles. First, titanium dioxide photocatalytic technology can be used during the pretreatment process. Second, as a stabilizer in the hydrogen peroxide bleaching process, it can prevent the decomposition of hydrogen peroxide under alkaline conditions, resulting in loss of activity and decreased bleaching effect. Third, it is beneficial to maintain the desizing rate, whiteness, and tensile strength of polyester-cotton fabrics after pretreatment.
[0011] Preferably, the descaling and bleaching treatment bath comprises the following components in terms of mass concentration:
[0012]
[0013] In the present invention, the components of the descaling and bleaching bath are used in combination in a specific ratio to achieve better performance. For example, the mass concentration of titanium dioxide is preferably 1-2 g / L. The reason is that the stability of hydrogen peroxide in the descaling and bleaching bath within this mass concentration range is higher and the bleaching efficiency is higher; if the addition amount is too high, the photosensitization of titanium dioxide will affect the strength of the fiber; if the addition amount is too low, the stability of hydrogen peroxide will be poor, resulting in an insignificant bleaching effect.
[0014] In the present invention, the mass concentration of the alkali metal hydroxide is 4-10 g / L, for example, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, etc.
[0015] The mass concentration of the penetrant is 1-2 g / L, such as 1.2 g / L, 1.4 g / L, 1.6 g / L, 1.8 g / L, etc.
[0016] The mass concentration of the bleaching agent is 2-4 g / L, for example, 2.2 g / L, 2.4 g / L, 2.6 g / L, 2.8 g / L, 3 g / L, 3.2 g / L, 3.4 g / L, 3.6 g / L, 3.8 g / L, etc.
[0017] The mass concentration of the hydrogen peroxide solution is 15-20 g / L, such as 16 g / L, 17 g / L, 18 g / L, 19 g / L, etc.
[0018] The mass concentration of the titanium dioxide is 1-2 g / L, such as 1.2 g / L, 1.4 g / L, 1.6 g / L, 1.8 g / L, etc.
[0019] The mass concentration of the dispersant is 2-4 g / L, for example, 2.2 g / L, 2.4 g / L, 2.6 g / L, 2.8 g / L, 3 g / L, 3.2 g / L, 3.4 g / L, 3.6 g / L, 3.8 g / L, etc.
[0020] Preferably, the alkali metal hydroxide includes sodium hydroxide and / or potassium hydroxide, and more preferably sodium hydroxide.
[0021] Preferably, the osmotic agent comprises a branched chain alkyl glycoside.
[0022] Exemplarily, the penetrant may be selected from JFC2G and isooctyl ether phosphate of Tesco Chemical (Hubei) Co., Ltd., or OEP98 and / or OEP70 of Jinan Quanxing New Materials Co., Ltd., with JFC2G being more preferred.
[0023] Preferably, the bleaching agent comprises an anionic surfactant and / or a nonionic surfactant, and more preferably a combination of an anionic surfactant and a nonionic surfactant.
[0024] In the present invention, the bleaching agent includes any one of M-1011 and NF-1 or a combination of at least two of them.
[0025] Exemplarily, the bleaching agent is selected from the combination of anionic and nonionic surfactants M-1011 produced by Hangzhou Meigao Huayi Chemical Co., Ltd. and / or the combination of anionic and nonionic surfactants NF-1 produced by Shandong Binzhou Pengcheng Additive Co., Ltd., and M-1011 is further preferred.
[0026] In the present invention, the bleaching agent and penetrant used in the descaling and bleaching treatment bath have good alkali resistance and low foaming properties, and are more suitable for the descaling and bleaching process system. The ... contain a variety of surfactants, and have the properties of refining, bleaching and softening. At the same time, the slurry dispersed in the water can have good emulsification and dispersion properties, and the phenomenon of re-staining the fabric will not occur. When used in the pretreatment process, the effect of the conventional one-bath method can be achieved for a longer time, and the treatment temperature and time can be significantly reduced, which plays the role of energy saving and environmental protection, improving processing efficiency, and saving energy.
[0027] Preferably, the mass concentration of the hydrogen peroxide solution is 25%-35%, such as 26%, 28%, 30%, 32%, 34%, etc., and more preferably 30%.
[0028] Preferably, the titanium dioxide comprises anatase titanium dioxide.
[0029] In the present invention, the titanium dioxide is preferably anatase titanium dioxide because, compared with titanium dioxide of other structures, anatase titanium dioxide has higher ultraviolet-induced photosensitivity decolorization and can remove colored substances or slurries.
[0030] Preferably, the dispersant includes sodium dodecyl sulfate (SDS) and / or polyvinyl alcohol (PEG, such as PEG400), and SDS is further preferred.
[0031] Preferably, the method for preparing titanium dioxide comprises the following steps:
[0032] (1) mixing a titanium source and a chelating agent, adjusting the pH, and reacting to obtain a first component;
[0033] mixing the catalyst and the solvent to obtain a second component;
[0034] (2) mixing the first component and the second component, reacting them, and obtaining a titanium dioxide sol;
[0035] (3) Drying and calcining the titanium dioxide sol to obtain the titanium dioxide.
[0036] Preferably, in step (1), the mass ratio of the titanium source to the chelating agent is 1:(6-7), wherein 6-7 can be 6.2, 6.4, 6.6, 6.8, etc.
[0037] Preferably, the mass ratio of the titanium source to the solvent is 1:(60-90), wherein 60-90 can be 65, 70, 75, 80, 85, etc.
[0038] Preferably, based on the total mass of the titanium source, chelating agent, catalyst and solvent as 100%, the mass percentage of the catalyst is 4%-6%, for example 4.2%, 4.4%, 4.6%, 4.8%, 5%, 5.2%, 5.4%, 5.6%, 5.8% and the like.
[0039] Preferably, the titanium source includes any one of tetrabutyl titanate, titanium tetrachloride or titanium sulfate, or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of tetrabutyl titanate and titanium tetrachloride, a combination of titanium tetrachloride and titanium sulfate, a combination of tetrabutyl titanate, titanium tetrachloride and titanium sulfate, etc., and tetrabutyl titanate is further preferred.
[0040] Preferably, the chelating agent comprises acetic acid and / or acetic anhydride, more preferably acetic acid.
[0041] Preferably, the catalyst comprises any one of nitric acid, hydrochloric acid or acetic acid, or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of nitric acid and hydrochloric acid, a combination of hydrochloric acid and acetic acid, a combination of nitric acid, hydrochloric acid and acetic acid, etc., and nitric acid is further preferred.
[0042] Preferably, the solvent comprises any one of ethanol, water, isopropanol or methanol or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of ethanol and water, a combination of isopropanol and methanol, a combination of ethanol, water, isopropanol and methanol, etc., and ethanol is further preferred.
[0043] Preferably, the mixing method includes stirring.
[0044] Preferably, the stirring time is 0.5-1 h, such as 0.6 h, 0.7 h, 0.8 h, 0.9 h, etc.
[0045] Preferably, the pH is adjusted to 2-4, such as 2.5, 3, 3.5, etc.
[0046] Preferably, the reaction temperature is 25-35°C, such as 26°C, 28°C, 30°C, 32°C, 34°C, etc.
[0047] Preferably, in step (2), the first component and the second component are mixed by dropping the second component into the first component and stirring.
[0048] Preferably, after the dropwise addition is completed, stirring is continued for 0.5-1 h, for example, 0.6 h, 0.7 h, 0.8 h, 0.9 h, etc.
[0049] Preferably, in step (3), the drying temperature is 50-70°C, such as 55°C, 60°C, 65°C, etc.
[0050] Preferably, the drying time is 12-36 h, for example, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, 32 h, 34 h, etc.
[0051] Preferably, the calcination temperature is 400-500°C, such as 420°C, 440°C, 460°C, 480°C, etc.
[0052] Preferably, the calcination time is 0.5-1.5 h, such as 0.6 h, 0.8 h, 1 h, 1.2 h, 1.4 h, etc.
[0053] Preferably, the calcination further comprises grinding.
[0054] In a second aspect, the present invention provides a pre-treatment process for descaling and bleaching polyester-cotton fabrics, the pre-treatment process comprising the following steps:
[0055] The polyester-cotton fabric is immersed in the descaling and bleaching bath described in the first aspect, and descaling and bleaching treatment is performed under conditions of less than 70° C. (e.g., 65° C., 60° C., 55° C., 50° C., etc.), ultrasonic vibration and light irradiation, and then washed, dried, and ozone treated to complete the pretreatment process.
[0056] In the present invention, the pretreatment process applies titanium dioxide photocatalytic degradation technology, ultrasonic technology and ozone oxidation technology to the one-bath pretreatment of polyester-cotton fabric by alkali oxygen descaling and bleaching. The process can achieve the effect of the conventional one-bath method for a longer time, and can significantly reduce the treatment temperature and time, thereby achieving the effects of energy saving and environmental protection, improving processing efficiency and saving energy.
[0057] Specifically, ultrasonic technology is used in the pretreatment process described in the present invention. On the one hand, ultrasonic waves can make titanium dioxide powder dissolve better in the descaling and bleaching treatment bath to form a titanium dioxide sol system. On the other hand, during the descaling and bleaching process, the dispersion effect caused by ultrasonic cavitation can separate macromolecules and promote the loosening of the adhesion between the slurry and the fiber; and the emulsification effect caused by ultrasonic waves can convert the removed slurry from a gel state to a sol state, improve the solubility, and make it have a better desizing effect; the cavitation effect of ultrasonic waves can cause dispersion, emulsification, washing and depolymerization, etc., making it easier to remove dirt adhering to the fiber.
[0058] The pre-treatment process of the present invention uses titanium dioxide photocatalytic degradation technology. As is known to all, the sizing materials used in polyester-cotton fabric sizing are generally natural sizing materials such as starch or synthetic sizing materials such as polyvinyl alcohol or polyacrylic acid. These materials are difficult to degrade themselves, and the photocatalytic degradation technology can make the sizing materials or colored components swollen in caustic soda more easily expand and degrade, and be removed mechanically. At the same time, the stabilizing effect of titanium dioxide has a similar function to that of silicon dioxide, and can be used as a stabilizer in the hydrogen peroxide bleaching process to prevent the decomposition of hydrogen peroxide under alkaline conditions, resulting in loss of activity and reduced bleaching effect.
[0059] The ozone technology is used in the pre-treatment process of the present invention. Ozone is also a strong oxidant, which can degrade and remove the slurry on the polyester-cotton fabric. It also has a certain bleaching effect, and the process is ecological and environmentally friendly.
[0060] Preferably, the bath ratio of the polyester-cotton fabric to the descaling and bleaching bath is 1:(10-50), wherein 10-50 can be 15, 20, 25, 30, 35, 40, 45, etc.
[0061] Preferably, the temperature of the system in the water bath during the descaling and bleaching treatment is controlled to be lower than 70°C, for example, 65°C, 60°C, 55°C, 50°C, etc.
[0062] Preferably, the temperature of the water bath is 50-60°C, such as 52°C, 54°C, 56°C, 58°C, etc.
[0063] In the present invention, a good pre-treatment effect can be achieved at a relatively low temperature.
[0064] Preferably, the power of the ultrasonic oscillation is 45-55W, for example, 46W, 48W, 50W, 52W, 54W, etc.
[0065] Preferably, the frequency of the ultrasonic oscillation is 40-50 Hz, for example, 42 Hz, 44 Hz, 46 Hz, 48 Hz, etc.
[0066] Preferably, the light source of the illumination is an ultraviolet radiation lamp.
[0067] Preferably, the descaling and bleaching treatment time is 30-60 min, for example, 35 min, 40 min, 45 min, 50 min, 55 min, etc.
[0068] Preferably, the drum speed of the ozone treatment equipment is 20-24 r / min, such as 21 r / min, 22 r / min, 23 r / min, etc.
[0069] Preferably, the power of the ozone treatment is 60-80W, such as 65W, 70W, 75W, etc.
[0070] Preferably, the ozone treatment time is 20-30 min, such as 22 min, 24 min, 26 min, 28 min, etc.
[0071] Preferably, the ozone treatment further includes washing and drying.
[0072] As a preferred technical solution, the pre-treatment process includes the following steps:
[0073] (1) immersing the polyester-cotton fabric in the descaling and bleaching bath of the first aspect at a bath ratio of 1:(10-50), bathing at 50-60° C., ultrasonically oscillating at 45-55 W and 40-50 Hz, and irradiating with an ultraviolet radiation lamp for 30-60 min of descaling and bleaching treatment, and then washing and drying;
[0074] (2) The dried polyester-cotton fabric is treated with ozone at 20-24 r / min and 60-80 W for 20-30 min to complete the pretreatment process.
[0075] Compared with the prior art, the present invention has the following beneficial effects:
[0076] (1) The desizing rate, whiteness and tensile strength of the polyester-cotton fabric obtained by the desizing and bleaching pretreatment process of the present invention are significantly higher than those of the conventional desizing and desizing treatment. In addition, the method can achieve the effect of the conventional one-bath method in a shorter time while taking a longer time, and can significantly reduce the treatment temperature, thereby saving time, improving processing efficiency and saving energy.
[0077] (2) According to the pretreatment process for desizing, boiling and bleaching of polyester-cotton fabrics described in the present invention, the polyester-cotton fabrics obtained have a desizing rate of more than 92.5%, a whiteness of more than 89.4%, and a tensile strength of more than 513.4N. DETAILED DESCRIPTION
[0078] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0079] In the present invention, the purchase information of some raw materials is as follows:
[0080] Polyester fabric: purchased from Carlofu Textile Co., Ltd.;
[0081] Penetrant: purchased from Tesco Chemical (Hubei) Co., Ltd., brand JFC2G;
[0082] Penetrant: purchased from Jinan Quanxing New Materials Co., Ltd., brand OEP98;
[0083] Penetrant: purchased from Jinan Quanxing New Materials Co., Ltd., brand name OEP-70
[0084] Bleaching agent: purchased from Hangzhou Meigao Huayi Chemical Co., Ltd., brand name M-1011;
[0085] Bleaching agent: purchased from Shandong Binzhou Pengcheng Additives Company, brand NF-1;
[0086] Dispersant: purchased from Shandong Xingqi Chemical Technology Co., Ltd., brand PEG400.
[0087] Example 1
[0088] This embodiment provides a de-boiling and bleaching treatment bath, wherein the de-boiling and bleaching treatment bath comprises the following components in terms of mass concentration:
[0089]
[0090] The preparation method of titanium dioxide comprises the following steps:
[0091] First, add 1g of tetrabutyl titanate and 6g of acetic acid into a beaker, mix them in a constant temperature magnetic stirrer and stir for 0.5h, adjust the pH to 2, and the reaction temperature to 25℃; put 60g of ethanol and 2.68g of nitric acid in a constant pressure funnel, and add them to the tetrabutyl titanate and acetic acid mixed solution at a rate of 1 drop / s and continue stirring. After the ethanol and nitric acid mixed solution in the constant pressure funnel are added, continue stirring for 0.5h to make it fully react, and then nano-titanium dioxide sol can be obtained. After the sol is cooled, nano-titanium dioxide gel is obtained. The gel is placed in a 60℃ drying oven and dried for 24h to obtain nano-titanium dioxide. Finally, the nano-titanium dioxide solid gel is placed in a box-type resistance furnace and calcined at 400℃ for 1h to obtain blocky light yellow nano-titanium dioxide. After grinding, white nano-titanium dioxide powder can be obtained, which is anatase titanium dioxide.
[0092] Example 2
[0093] This embodiment provides a de-boiling and bleaching treatment bath, wherein the de-boiling and bleaching treatment bath comprises the following components in terms of mass concentration:
[0094]
[0095]
[0096] The preparation method of titanium dioxide comprises the following steps:
[0097] First, add 1g of titanium tetrachloride and 7g of acetic anhydride into a beaker, mix and place in a constant temperature magnetic stirrer and stir for 1h, then adjust the pH to 4 and the reaction temperature to 35℃; put 90g of methanol and 5.82g of hydrochloric acid in a constant pressure funnel, add them to the titanium tetrachloride and acetic anhydride mixed solution at a rate of 1 drop / s and continue stirring. After the methanol and hydrochloric acid mixed solution in the constant pressure funnel are added, continue stirring for 1h to allow it to react fully, and then nano-titanium dioxide sol can be obtained. After the sol is cooled, nano-titanium dioxide gel is obtained. The gel is placed in a 60℃ drying oven and dried for 24h to obtain nano-titanium dioxide. Finally, the nano-titanium dioxide solid gel is placed in a box-type resistance furnace and calcined at 500℃ for 1h to obtain blocky light yellow nano-titanium dioxide. After grinding, white nano-titanium dioxide powder can be obtained, which is anatase titanium dioxide.
[0098] Example 3
[0099] This embodiment provides a de-boiling and bleaching treatment bath, wherein the de-boiling and bleaching treatment bath comprises the following components in terms of mass concentration:
[0100]
[0101] The preparation method of titanium dioxide comprises the following steps:
[0102] First, add 1g of titanium sulfate and 6.5g of acetic acid into a beaker, mix and place in a constant temperature magnetic stirrer and stir for 40 minutes, then adjust the pH to 3 and the reaction temperature to 30°C; put 75g of isopropanol and 4.13g of acetic acid in a constant pressure funnel, and drip into the titanium sulfate and acetic acid mixed solution at a rate of 1 drop / s and continue stirring. After the isopropanol and acetic acid mixed solution in the constant pressure funnel are dripped, continue stirring for 40 minutes to make it fully react, and then nano-titanium dioxide sol can be obtained. After the sol is cooled, nano-titanium dioxide gel is obtained. The gel is placed in a 60°C drying oven and dried for 24 hours to obtain nano-titanium dioxide. Finally, the nano-titanium dioxide solid gel is placed in a box-type resistance furnace and calcined at 450°C for 1 hour to obtain blocky light yellow nano-titanium dioxide. After grinding, white nano-titanium dioxide powder can be obtained, which is anatase titanium dioxide.
[0103] Example 4
[0104] This embodiment provides a de-boiling and bleaching treatment bath, wherein the de-boiling and bleaching treatment bath comprises the following components in terms of mass concentration:
[0105]
[0106] The preparation method of titanium dioxide comprises the following steps:
[0107] First, add 1g of tetrabutyl titanate and 6g of acetic acid into a beaker, mix them in a constant temperature magnetic stirrer and stir for 1h, then adjust the pH to 2; the reaction temperature is 30℃; put 60g of ethanol and 2.72g of nitric acid in a constant pressure funnel, and add them to the tetrabutyl titanate and acetic acid mixed solution at a rate of 1 drop / s and continue stirring. After the ethanol and nitric acid mixed solution in the constant pressure funnel are added, continue stirring for 1h to make it fully react, and then nano-titanium dioxide sol can be obtained. After the sol is cooled, nano-titanium dioxide gel is obtained. The gel is placed in a 60℃ drying oven and dried for 24h to obtain nano-titanium dioxide. Finally, the nano-titanium dioxide solid gel is placed in a box-type resistance furnace and calcined at 500℃ for 1h to obtain blocky light yellow nano-titanium dioxide. After grinding, white nano-titanium dioxide powder can be obtained, which is anatase titanium dioxide.
[0108] Embodiment 5-6
[0109] The difference between Examples 5-6 and Example 1 is that the mass concentrations of anatase titanium dioxide are 0.5 g / L (Example 5) and 2.5 g / L (Example 6), respectively, and the rest are the same as Example 1.
[0110] Example 7
[0111] The difference between this embodiment and embodiment 1 is that the anatase titanium dioxide is replaced by rutile titanium dioxide, and the rest is the same as embodiment 1.
[0112] Comparative Example 1
[0113] This comparative example provides a deboiling and bleaching treatment bath, which comprises the following components in terms of mass concentration:
[0114]
[0115] Comparative Example 2
[0116] The difference between this comparative example and Example 1 is that anatase titanium dioxide is not included, and the rest is the same as Example 1.
[0117] Application Example 1
[0118] This application example provides a pre-treatment process for descaling and bleaching polyester-cotton fabrics, the pre-treatment process comprising the following steps:
[0119] The undesized polyester-cotton fabric is placed in the desizing and bleaching treatment bath described in Example 1, with a bath ratio of 1:20. The treatment bath is then placed in a constant temperature water bath with ultrasonic oscillation at 50°C, the ultrasonic switch is turned on, the ultrasonic power / frequency is set to 50W / 45Hz, and the ultraviolet radiation lamp installed above the constant temperature water bath is turned on at the same time. Under this condition, the polyester-cotton fabric is desizing and bleaching for 30 minutes. After the treatment is completed, it is fully washed with cold water and then dried, and then placed in an ozone device, and the ozone device drum speed is set to 20r / min, the power is 60W, and the time is 20min. The polyester-cotton fabric after ozone treatment is washed 3 times with hot water, fully washed with cold water, and then dried, that is, the polyester-cotton fabric desizing and bleaching pre-treatment process is completed.
[0120] Application Example 2
[0121] This application example provides a pre-treatment process for descaling and bleaching polyester-cotton fabrics, the pre-treatment process comprising the following steps:
[0122] The undesized polyester-cotton fabric is placed in the desizing and bleaching treatment bath described in Example 2, with a bath ratio of 1:50. The treatment bath is then placed in a constant temperature water bath with ultrasonic oscillation at 60°C, the ultrasonic switch is turned on, the ultrasonic power / frequency is set to 50W / 45Hz, and the ultraviolet radiation lamp installed above the constant temperature water bath is turned on at the same time. Under this condition, the polyester-cotton fabric is desizing and bleaching for 60 minutes. After the treatment is completed, it is fully washed with cold water and then dried, and then placed in an ozone device, and the ozone device drum speed is set to 24r / min, the power is 80W, and the time is 30min. The polyester-cotton fabric after ozone treatment is washed 3 times with hot water, fully washed with cold water, and then dried, that is, the polyester-cotton fabric desizing and bleaching pre-treatment process is completed.
[0123] Application Example 3
[0124] This application example provides a pre-treatment process for descaling and bleaching polyester-cotton fabrics, the pre-treatment process comprising the following steps:
[0125] The undesized polyester-cotton fabric is placed in the desizing and bleaching treatment bath described in Example 3, with a bath ratio of 1:10. The treatment bath is then placed in a constant temperature water bath with ultrasonic oscillation at 55°C, the ultrasonic switch is turned on, the ultrasonic power / frequency is set to 50W / 45Hz, and the ultraviolet radiation lamp installed above the constant temperature water bath is turned on at the same time. Under this condition, the polyester-cotton fabric is desizing and bleaching for 40 minutes. After the treatment is completed, it is fully washed with cold water and then dried, and then placed in an ozone device, and the ozone device drum speed is set to 22r / min, the power is 70W, and the time is 25min. The polyester-cotton fabric after ozone treatment is washed 3 times with hot water, fully washed with cold water, and then dried, that is, the polyester-cotton fabric desizing and bleaching pre-treatment process is completed.
[0126] Application Example 4
[0127] This application example provides a pre-treatment process for descaling and bleaching polyester-cotton fabrics, the pre-treatment process comprising the following steps:
[0128] The undesized polyester-cotton fabric is placed in the desizing and bleaching treatment bath described in Example 4, with a bath ratio of 1:30. The treatment bath is then placed in a constant temperature water bath with ultrasonic oscillation at 60°C, the ultrasonic switch is turned on, the ultrasonic power / frequency is set to 50W / 45Hz, and the ultraviolet radiation lamp installed above the constant temperature water bath is turned on at the same time. Under this condition, the polyester-cotton fabric is desizing and bleaching for 60 minutes. After the treatment is completed, it is fully washed with cold water and then dried, and then placed in an ozone device, and the ozone device drum speed is set to 24r / min, the power is 80W, and the time is 30min. The polyester-cotton fabric after ozone treatment is washed 3 times with hot water, fully washed with cold water, and then dried, that is, the polyester-cotton fabric desizing and bleaching pre-treatment process is completed.
[0129] Application Example 5-7
[0130] The difference between Application Example 5-7 and Application Example 1 is that the descaling and bleaching bath used in the application example is replaced with the descaling and bleaching bath described in Example 5-7, and the rest is the same as Application Example 1.
[0131] Application Example Comparative Example 1
[0132] This application comparative example provides a pre-treatment process for descaling and bleaching polyester-cotton fabric, and the pre-treatment process comprises the following steps:
[0133] The undesized polyester-cotton fabric was placed in the desizing, boiling and bleaching treatment bath described in Comparative Example 1, with a bath ratio of 1:20. The treatment bath was then placed in a 90°C constant temperature water bath for desizing, boiling and bleaching for 60 minutes. After the treatment, the polyester-cotton fabric was washed three times with hot water, washed thoroughly with cold water and then dried, thus completing the desizing, boiling and bleaching pre-treatment process for the polyester-cotton fabric.
[0134] Application Example Comparative Example 2
[0135] The difference between this comparative example and Application Example 1 is that the descaling and bleaching bath described in Example 1 is replaced by the descaling and bleaching bath described in Comparative Example 2, and the rest is the same as Application Example 1.
[0136] Application Example Comparative Example 3
[0137] This application comparative example provides a pre-treatment process for descaling and bleaching polyester-cotton fabric, and the pre-treatment process comprises the following steps:
[0138] The undesized polyester-cotton fabric was placed in the desizing, boiling and bleaching treatment bath described in Example 1, with a bath ratio of 1:20. The treatment bath was then placed in a constant temperature water bath with ultrasonic oscillation at 60°C, the ultrasonic switch was turned on, the ultrasonic power / frequency was set to 50W / 45Hz, and the ultraviolet radiation lamp installed above the constant temperature water bath was turned on at the same time. Under this condition, the polyester-cotton fabric was desizing, boiling and bleaching for 50 minutes. After the treatment, the polyester-cotton fabric was washed 3 times with hot water, washed thoroughly with cold water and then dried, thus completing the desizing, boiling and bleaching pre-treatment process of the polyester-cotton fabric.
[0139] Application Example Comparative Example 4
[0140] This application comparative example provides a pre-treatment process for descaling and bleaching polyester-cotton fabric, and the pre-treatment process comprises the following steps:
[0141] The undesized polyester-cotton fabric is placed in the desizing and bleaching treatment bath described in Example 1, with a bath ratio of 1:20. The treatment bath is then placed in a 60°C constant temperature water bath, and the ultraviolet radiation lamp installed above the constant temperature water bath is turned on. Under this condition, the polyester-cotton fabric is desizing and bleaching for 50 minutes. After the treatment, it is fully washed with cold water and then dried, and then placed in an ozone device, with the drum speed of the ozone device set at 24r / min, the power at 80W, and the time for 20 minutes. The polyester-cotton fabric after ozone treatment is washed with hot water 3 times, washed with cold water fully, and then dried to complete the desizing and bleaching pre-treatment process of the polyester-cotton fabric.
[0142] Application Example Comparative Example 5
[0143] This application comparative example provides a pre-treatment process for descaling and bleaching polyester-cotton fabric, and the pre-treatment process comprises the following steps:
[0144] The undesized polyester-cotton fabric is placed in the desizing and bleaching treatment bath described in Example 1, with a bath ratio of 1:20. The treatment bath is then placed in a constant temperature water bath with ultrasonic oscillation at 60°C, the ultrasonic switch is turned on, and the ultrasonic power / frequency is set to 50W / 45Hz. Under this condition, the polyester-cotton fabric is desizing and bleaching for 50 minutes. After the treatment, it is fully washed with cold water and then dried. Then it is placed in an ozone device, and the drum speed of the ozone device is set to 24r / min, the power is 80W, and the time is 20min. The polyester-cotton fabric after ozone treatment is washed with hot water 3 times, washed with cold water and then dried to complete the desizing and bleaching pre-treatment process of the polyester-cotton fabric.
[0145] Performance Testing
[0146] The polyester-cotton fabrics after the pre-treatment process of descaling and bleaching of the polyester-cotton fabrics described in Application Examples 1-7 and Comparative Examples 1-5, as well as untreated polyester-cotton fabrics were used as blank comparative examples to conduct the following tests:
[0147] (1) Desizing rate: Take three pieces of polyester-cotton undesized fabric of the same mass and accurately weigh them on an electronic balance, respectively, and record them as W 1 G 1 G 2 , place one of the pieces in an oven at 105-110℃, dry until constant weight (about 2h), quickly take out the fabric and put it in a dryer, cool it to room temperature, and accurately weigh the weight W 2 , calculate the moisture regain A% of the sample according to the following formula:
[0148] A=(W 1 -W 2 ) / W 1 ×100%;
[0149] Desize the other two fabrics according to the process, squeeze out the water and put them into an oven, dry them in an oven at 105-110℃ until they reach constant weight (about 3.5h), quickly take out the fabrics and put them into a dryer, cool them to room temperature, and accurately weigh them. 1 'G 2 ', calculate the fabric desizing rate C% according to the following formula:
[0150] C=[G(1-A)-G'] / G(1-A)×100%.
[0151] (2) Whiteness: Use a whiteness meter to test whiteness. Fold the desized polyester-cotton fabric into four layers and wait for the instrument to be ready for testing. Measure four different points on a piece of fabric and take their average value. The parallel test deviation is less than 0.21%.
[0152] (3) Tensile strength: The desized and dried fabric was tested for tensile strength using an electronic fabric strength tester. The result was the average of two parallel measurements, and the deviation of the parallel tests was less than 4.55%.
[0153] The test results are summarized in Table 1.
[0154] Table 1
[0155] Test subjects Desizing rate / % Whiteness / % Tensile strength / N Application Example 1 96.7 95.2 568.6 Application Example 2 97.8 96.1 602.7 Application Example 3 97.2 95.6 584.3 Application Example 4 97.4 95.7 594.1 Application Example 5 93.1 93.4 573.0 Application Example 6 96.5 95.0 513.4 Application Example 7 92.5 89.4 570.0 Application Comparative Example 1 91.4 85.4 463.5 Application Comparative Example 2 92.3 86.4 572.5 Application Comparative Example 3 92.4 84.8 516.1 Application Comparative Example 4 86.8 87.6 568.3 Application Comparative Example 5 91.4 86.8 601.4 Blank comparison - 69.5 688.2
[0156] Analysis of the data in Table 1 shows that the desizing rate, whiteness and tensile strength of the polyester-cotton fabric obtained by the desizing pretreatment process for desizing, boiling and bleaching of the polyester-cotton fabric of the present invention are above 92.5%, above 89.4%, and above 513.4N; the desizing rate, whiteness and tensile strength of the polyester-cotton fabric obtained by the desizing pretreatment process for desizing, boiling and bleaching of the polyester-cotton fabric of the present invention are significantly higher than those of the conventional desizing and desizing treatment, and the method can not only achieve the effect of the conventional one-bath method in a shorter time, but also significantly reduce the treatment temperature, thereby saving time, improving processing efficiency and saving energy.
[0157] Analysis of application examples 1, 3-5 and application example 1 shows that the performance of application examples 1 and 3-5 is not as good as that of application example 1, which proves that the pre-treatment process for descaling and bleaching of polyester-cotton fabrics described in the present invention has more obvious advantages.
[0158] Analysis of Application Comparative Example 2 and Application Example 1 shows that the performance of Application Comparative Example 2 is not as good as that of Application Example 1, which proves that adding titanium dioxide to the descaling and bleaching bath is more conducive to the pre-treatment process of descaling and bleaching of polyester-cotton fabrics.
[0159] Analysis of Application Examples 5-6 and Application Example 1 shows that the performance of Application Examples 5-6 is not as good as that of Application Example 1, which proves that the mass concentration of titanium dioxide in the descaling and bleaching bath is 1-2g / L, which is more conducive to the pre-treatment process of descaling and bleaching of polyester-cotton fabrics.
[0160] Analysis of Application Example 7 and Application Example 1 shows that the performance of Application Example 7 is not as good as that of Application Example 1, which proves that anatase titanium dioxide is preferably used in the descaling and bleaching bath, which is more conducive to the pretreatment process of descaling and bleaching of polyester-cotton fabrics.
[0161] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A descaling and bleaching bath, characterized in that: The descaling and bleaching treatment bath comprises the following components according to mass concentration: Alkali metal hydroxide 4-10 g / L Penetrant 1-2 g / L Bleach 2-4 g / L Hydrogen peroxide solution 15-20 g / L Titanium dioxide 1-2 g / L Dispersant 2-4 g / L; The titanium dioxide is anatase titanium dioxide.
2. The descaling and bleaching bath according to claim 1, characterized in that: The alkali metal hydroxide includes sodium hydroxide and / or potassium hydroxide.
3. The descaling and bleaching bath according to claim 1, characterized in that: The penetrant includes a branched chain alkyl glycoside.
4. The descaling and bleaching bath according to claim 1, characterized in that: The bleaching agent includes anionic surfactants and / or nonionic surfactants.
5. The descaling and bleaching bath according to claim 1, characterized in that: The mass concentration of the hydrogen peroxide solution is 25%-35%.
6. The descaling and bleaching bath according to claim 1, characterized in that: The dispersant includes sodium dodecyl sulfate and / or polyvinyl alcohol.
7. The descaling and bleaching bath according to claim 1, characterized in that: The preparation method of titanium dioxide comprises the following steps: (1) mixing a titanium source and a chelating agent, adjusting the pH, and reacting to obtain a first component; mixing the catalyst and the solvent to obtain a second component; (2) mixing the first component and the second component, reacting them, and obtaining a titanium dioxide sol; (3) Drying and calcining the titanium dioxide sol to obtain the titanium dioxide.
8. The descaling and bleaching bath according to claim 7, characterized in that: In step (1), the mass ratio of the titanium source to the chelating agent is 1:(6-7).
9. The descaling and bleaching bath according to claim 7, characterized in that: The mass ratio of the titanium source to the solvent is 1:(60-90).
10. The descaling and bleaching bath according to claim 7, characterized in that: Based on the total mass of the titanium source, the chelating agent, the catalyst and the solvent being 100%, the mass percentage of the catalyst is 4%-6%.
11. The descaling and bleaching bath according to claim 7, characterized in that: The titanium source includes any one of tetrabutyl titanate, titanium tetrachloride or titanium sulfate, or a combination of at least two thereof.
12. The descaling and bleaching bath according to claim 7, characterized in that: The chelating agent includes acetic acid and / or acetic anhydride.
13. The descaling and bleaching bath according to claim 7, characterized in that: The catalyst includes any one of nitric acid, hydrochloric acid or acetic acid, or a combination of at least two of them.
14. The descaling and bleaching bath according to claim 7, characterized in that: The solvent includes any one of ethanol, water, isopropanol or methanol, or a combination of at least two of them.
15. The descaling and bleaching bath according to claim 7, characterized in that: The mixing method includes stirring.
16. The descaling and bleaching bath according to claim 15, characterized in that: The stirring time is 0.5-1 h.
17. The descaling and bleaching bath according to claim 7, characterized in that: The pH is adjusted to 2-4.
18. The descaling and bleaching bath according to claim 7, characterized in that: The reaction temperature is 25-35°C.
19. The descaling and bleaching bath according to claim 7, characterized in that: In step (2), the first component and the second component are mixed by dropping the second component into the first component and stirring.
20. The descaling and bleaching bath according to claim 19, characterized in that: After the dropwise addition is completed, stirring is continued for 0.5-1 h.
21. The descaling and bleaching bath according to claim 7, characterized in that: In step (3), the drying temperature is 50-70°C.
22. The descaling and bleaching bath according to claim 7, characterized in that: The drying time is 12-36 h.
23. The descaling and bleaching bath according to claim 7, characterized in that: The calcination temperature is 400-500°C.
24. The descaling and bleaching bath according to claim 7, characterized in that: The calcination time is 0.5-1.5 h.
25. The descaling and bleaching bath according to claim 7, characterized in that: The calcination may further include grinding.
26. A pretreatment process for descaling and bleaching polyester-cotton fabric, characterized in that: The pre-treatment process comprises the following steps: The polyester-cotton fabric is immersed in the descaling and bleaching bath according to any one of claims 1 to 25, and descaling and bleaching treatment is performed under the conditions of less than 70° C., ultrasonic vibration and light irradiation, and then washed, dried and ozone treated to complete the pretreatment process.
27. The pre-treatment process according to claim 26, characterized in that: The bath ratio of the polyester-cotton fabric to the descaling and bleaching bath is 1:(10-50).
28. The pre-treatment process according to claim 26, characterized in that: The descaling and bleaching treatment controls the system temperature in a water bath to be lower than 70°C.
29. The pre-treatment process according to claim 28, characterized in that: The temperature of the water bath is 50-60°C.
30. The pre-treatment process according to claim 26, characterized in that: The power of the ultrasonic oscillation is 45-55 W.
31. The pre-treatment process according to claim 26, characterized in that: The frequency of the ultrasonic oscillation is 40-50 Hz.
32. The pre-treatment process according to claim 26, characterized in that: The light source of the illumination is an ultraviolet radiation lamp.
33. The pre-treatment process according to claim 26, characterized in that: The descaling and bleaching treatment takes 30-60 minutes.
34. The pre-treatment process according to claim 26, characterized in that: The drum speed of the ozone treatment equipment is 20-24 r / min.
35. The pre-treatment process according to claim 26, characterized in that: The power of the ozone treatment is 60-80 W.
36. The pre-treatment process according to claim 26, characterized in that: The ozone treatment time is 20-30 minutes.
37. The pre-treatment process according to claim 26, characterized in that: The ozone treatment also includes washing and drying.
38. The pre-treatment process according to claim 26, characterized in that: The pre-treatment process comprises the following steps: (1) Immerse the polyester-cotton fabric in the descaling and bleaching bath of any one of claims 1 to 25 at a bath ratio of 1:(10-50), place the fabric in a water bath at 50-60°C, and ultrasonically vibrate at 45-55 W and 40-50 Hz, while irradiating it with an ultraviolet radiation lamp, for 30-60 minutes of descaling and bleaching treatment, and then wash and dry the fabric; (2) The dried polyester-cotton fabric is treated with ozone at 20-24 r / min and 60-80 W for 20-30 min to complete the pretreatment process.
Citation Information
Patent Citations
Shortened enzyme-oxygen desizing-scouring-bleaching pretreatment technology of cotton fabric
CN108193477A
Disperse reactive dye one-bath two-step dip dyeing method for polyester-cotton fabric
CN115434168A
Solid phase catalyst, preparation method and uses thereof
CN101367917A
Treatment method of textile
CN101643998A
Method of pre-treatment of desizing, scouring and bleaching in one-bath process for cotton fabric by ultrasonic pre-treatment
CN103774411A