A kind of high and low temperature resistant silicone grease and preparation method thereof

By adding components such as polytetrafluoroethylene and nano-titanium nitride to silicone oil, and mixing and grinding them at high temperatures, high and low temperature resistant silicone grease lubricating oil is prepared, which solves the problem of lubricant's lack of stability and waterproofing in high and low temperature environments. problems, achieving wider applicability and self-healing effect.

CN116082842BActive Publication Date: 2024-10-29DONGGUAN CITY ODSI LUBRICANT TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211685339.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-10-29
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

It is difficult for existing lubricants to maintain stability and waterproof and moisture-proof properties in high and low temperature environments, and traditional additives cannot achieve self-healing and zero wear of materials.

Method used

Silicone oil is used as the base oil, combined with polytetrafluoroethylene, nano-titanium nitride, antioxidants, extruded anti-wear additives, anti-corrosion additives and anti-rust additives, and added with nano-montmorillonite, nano-graphite powder and vegetable wax, through high temperature Mix and grind to prepare silicone lubricant that is resistant to high and low temperatures.

Benefits of technology

It achieves the stable performance of silicone grease lubricating oil in the temperature range of -30 to 230°C, improves its waterproof, anti-corrosion and lubrication properties, enhances self-healing capabilities, and is suitable for a wide range of environments and high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004020644670000111
    Figure BDA0004020644670000111
  • Figure BDA0004020644670000121
    Figure BDA0004020644670000121
Patent Text Reader

Abstract

The present application proposes a high and low temperature resistant silicone grease and a preparation method thereof, and relates to the field of lubricating oil technology. A high and low temperature resistant silicone grease, divided by weight, includes the following raw materials: 70-80 parts of silicone oil, 10-20 parts of polytetrafluoroethylene, 2-5 parts of nano titanium nitride, 0.2-1 parts of antioxidant, 0.5-2 parts of extreme pressure anti-wear additives, 0.2-1 parts of anti-corrosion additives and 0.1-0.5 parts of rust-proof additives. The silicone grease lubricant prepared in the present application has good pumpability, extreme pressure and wear resistance, lubricity, waterproof and moisture-proof properties, and stability in high and low temperature environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lubricating oils, and in particular to a high and low temperature resistant silicone grease and a preparation method thereof. Background Art

[0002] Since humans entered the industrial society, various mechanical equipment has emerged. The various parts of mechanical equipment are in relative motion all the time. Friction and wear are common phenomena in the friction process. According to statistics, more than one-third of the world's disposable energy loss comes from friction. Therefore, reducing the economic losses caused by friction and wear is of great significance. Lubrication is an effective technology to reduce friction, reduce or avoid wear. At present, most lubricants are improved by adding a variety of lubricating additives, while traditional additives achieve good tribological properties through physical adsorption and chemical reactions, and cannot achieve zero wear of materials or repair damage to materials. Lubricating additives largely determine the performance of lubricants. The development and research of new self-repairing lubricating additives to blend lubricating oils, thereby reducing friction and wear, is of development significance to the national economy.

[0003] Lubricating oil generally consists of two parts: base oil and additives. Base oil is the main component of lubricating oil and determines the basic properties of lubricating oil. Currently, the widely used base oils include mineral oil, vegetable oil and synthetic oil. Among them, mineral oil has a long history of use and is currently used in the largest amount. The biggest advantage of vegetable oil is that it is biodegradable and beneficial to environmental protection. The history of synthetic oil is relatively short. Because of its advantages of good stability and long lubrication life, it has been the research direction of scholars in recent years. Therefore, it is of great significance to develop synthetic oil-based grease with excellent performance in all aspects. Summary of the invention

[0004] The purpose of the present application is to provide a high and low temperature resistant silicone grease, which has good pumpability, extreme pressure resistance and wear resistance, lubricity, waterproofness and moisture resistance, and stability in high and low temperature environments.

[0005] Another object of the present application is to provide a method for preparing high and low temperature resistant silicone grease, which is simple and convenient.

[0006] The present application solves the technical problem by adopting the following technical solution.

[0007] On the one hand, an embodiment of the present application provides a high and low temperature resistant silicone grease, which includes the following raw materials by weight: 70-80 parts of silicone oil, 10-20 parts of polytetrafluoroethylene, 2-5 parts of nano-titanium nitride, 0.2-1 parts of antioxidant, 0.5-2 parts of extreme pressure and anti-wear additives, 0.2-1 parts of anti-corrosion additives and 0.1-0.5 parts of anti-rust additives.

[0008] On the other hand, the present invention provides a method for preparing a high and low temperature resistant silicone grease, comprising the following steps:

[0009] Put silicone oil and polytetrafluoroethylene in a reaction kettle, heat and mix them evenly, then add other raw materials and stir them evenly to obtain a fat-forming mixture;

[0010] The grease mixture is ground to obtain the silicone grease.

[0011] Compared with the prior art, the embodiments of the present application have at least the following advantages or beneficial effects:

[0012] 1. This application uses silicone oil as the base oil, which has the advantage of good stability. It is matched with polytetrafluoroethylene as a thickener. Both have excellent high and low temperature resistance and water resistance, which can make the entire silicone grease lubricant have high and low temperature resistance and water resistance. It has stable performance in the temperature range of -30 to 230°C and is suitable for a wider range of environments.

[0013] 2. The present application further adds titanium nitride, antioxidants, extrusion anti-wear additives, anti-corrosion additives and anti-rust additives on the basis of silicone oil and thickener, wherein titanium nitride still has stable lubrication and wear resistance at high temperatures, thereby increasing the operating temperature range of silicone grease lubricants, wherein the extrusion anti-wear additives, anti-corrosion additives and anti-rust additives can respectively increase the waterproof, corrosion-resistant and wear-resistant properties of silicone grease lubricants.

[0014] 3. Nano-montmorillonite, nano-graphite powder and plant wax are also added in the preferred mode of the present application. On the one hand, montmorillonite plays a role in increasing the viscosity and dispersibility of each raw material in the lubricating oil, and the graphite powder forms a graphite lubricating film under high temperature friction, which improves its lubricity and wear resistance; on the other hand, montmorillonite, graphite powder and titanium nitride are all nanomaterials, and the solid nanoparticles in the grease prepared therefrom can not only improve the thermal conductivity of the grease, but also improve the surface finish of the workpiece due to the ball bearing-like effect of the nanoparticles, fill the damaged parts of the metal material, reduce the surface roughness of the metal material, and then reduce the cutting force during cutting, and improve the lubrication effect. In addition, the plant wax itself has excellent anti-friction and anti-wear properties, and with the excellent heat transfer and dispersion stability of the nanoparticles, it can prevent blockage at the friction interface and improve its self-repairing ability.

[0015] In summary, the silicone grease lubricant prepared in the present application has good pumpability, extreme pressure resistance and wear resistance, lubricity, water and moisture resistance, and stability in high and low temperature environments. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0017] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to specific embodiments.

[0018] A high and low temperature resistant silicone grease comprises the following raw materials by weight: 70-80 parts of silicone oil, 10-20 parts of polytetrafluoroethylene, 2-5 parts of nano titanium nitride, 0.2-1 parts of antioxidant, 0.5-2 parts of extreme pressure anti-wear additive, 0.2-1 parts of anti-corrosion additive and 0.1-0.5 parts of anti-rust additive.

[0019] This application uses silicone oil as the base oil, which has the advantage of good stability. It is matched with polytetrafluoroethylene as a thickener. Both have excellent high and low temperature resistance and water resistance, which can make the entire silicone grease lubricant have high and low temperature resistance and water resistance. It has stable performance in the temperature range of -30 to 230°C and is suitable for a wider range of environments.

[0020] The present application further adds titanium nitride, antioxidants, extrusion anti-wear additives, anti-corrosion additives and anti-rust additives on the basis of silicone oil and thickener, wherein titanium nitride still has stable lubrication and wear resistance at high temperatures, thereby improving the operating temperature range of silicone grease lubricants, wherein the extrusion anti-wear additives, anti-corrosion additives and anti-rust additives can respectively improve the waterproofness, corrosion resistance and wear resistance of silicone grease lubricants.

[0021] In some embodiments of the present application, the silicone grease further comprises the following raw materials in parts by weight: 0.5-2 parts of nano-montmorillonite, 1-3 parts of nano-graphite powder and 5-10 parts of plant wax.

[0022] The present application also adds nano-montmorillonite, nano-graphite powder and plant wax, wherein the plant wax is carnauba wax, sugarcane wax or laurel wax. On the one hand, montmorillonite plays a role in increasing the viscosity and dispersibility of each raw material in the lubricating oil, and the graphite powder forms a graphite lubricating film under high temperature friction, improving its lubricity and wear resistance; on the other hand, montmorillonite, graphite powder and titanium nitride are all nanomaterials, and the solid nanoparticles in the grease prepared therefrom can not only improve the thermal conductivity of the grease, but also improve the surface finish of the workpiece due to the ball bearing-like effect of the nanoparticles, fill the damaged parts of the metal material, reduce the surface roughness of the metal material, and then reduce the cutting force during cutting, and improve the lubrication effect. In addition, the plant wax itself has excellent anti-friction and anti-wear properties, and with the excellent heat transfer and dispersion stability of the nanoparticles, it can prevent blockage at the friction interface and improve its self-repairing ability.

[0023] In some embodiments of the present application, the above-mentioned silicone grease is composed of the following raw materials in parts by weight: 76 parts of silicone oil, 13 parts of polytetrafluoroethylene, 3 parts of nano-titanium nitride, 0.5 parts of antioxidant, 1 part of extreme pressure anti-wear additive, 0.5 parts of anti-corrosion additive, 0.3 parts of anti-rust additive, 1 part of nano-montmorillonite, 2 parts of nano-graphite powder and 6 parts of vegetable wax.

[0024] In some embodiments of the present application, the antioxidant is octylbutyldiphenylamine.

[0025] In some embodiments of the present application, the extreme pressure anti-wear additive is sodium primary / secondary alkyl sulfonate.

[0026] In some embodiments of the present application, the anti-corrosion additive is octylbutyl diphenylamine.

[0027] In some embodiments of the present application, the anti-rust additive is barium dinonylnaphthalenesulfonate.

[0028] A method for preparing high and low temperature resistant silicone grease comprises the following steps:

[0029] Put silicone oil and polytetrafluoroethylene in a reaction kettle, heat and mix them evenly, then add other raw materials and stir them evenly to obtain a fat-forming mixture;

[0030] The grease mixture is ground to obtain the silicone grease.

[0031] In some embodiments of the present application, the temperature after the heating is 75-85° C., and the stirring time is 1-3 h.

[0032] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0033] Example 1

[0034] A high and low temperature resistant silicone grease is prepared by the following method:

[0035] Preparation: Weigh 75kg of silicone oil, 15kg of polytetrafluoroethylene, 3kg of nano-titanium nitride, 0.5kg of antioxidant (octylbutyldiphenylamine), 1kg of extreme pressure anti-wear additive (sodium primary / secondary alkyl sulfonate), 0.5kg of anti-corrosion additive (octylbutyldiphenylamine) and 0.2kg of anti-rust additive (barium dinonylnaphthalenesulfonate).

[0036] Mixing: First add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 75°C, and add nano titanium nitride, octylbutyldiphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyldiphenylamine and barium dinonylnaphthalenesulfonate, and continue stirring for 2 hours to form fat.

[0037] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0038] Example 2

[0039] A high and low temperature resistant silicone grease is prepared by the following method:

[0040] Preparation: Weigh 80kg of silicone oil, 18kg of polytetrafluoroethylene, 4kg of nano-titanium nitride, 0.8kg of antioxidant (octylbutyldiphenylamine), 1.5kg of extreme pressure anti-wear additive (sodium primary / secondary alkyl sulfonate), 0.2kg of anti-corrosion additive (octylbutyldiphenylamine) and 0.5kg of anti-rust additive (barium dinonylnaphthalenesulfonate).

[0041] Mixing: First add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 80°C, and add nano titanium nitride, octylbutyldiphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyldiphenylamine and barium dinonylnaphthalenesulfonate, and continue stirring for 2.5 hours to form fat.

[0042] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0043] Example 3

[0044] A high and low temperature resistant silicone grease is prepared by the following method:

[0045] Preparation: Weigh 70kg of silicone oil, 12kg of polytetrafluoroethylene, 2kg of nano-titanium nitride, 0.2kg of antioxidant (octylbutyldiphenylamine), 0.5kg of extreme pressure anti-wear additive (sodium primary / secondary alkyl sulfonate), 1kg of anti-corrosion additive (octylbutyldiphenylamine) and 0.2kg of anti-rust additive (barium dinonylnaphthalenesulfonate).

[0046] Mixing: First add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 74°C, and add nano titanium nitride, octylbutyldiphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyldiphenylamine and barium dinonylnaphthalenesulfonate, and continue stirring for 1.5 hours to form fat.

[0047] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0048] Example 4

[0049] A high and low temperature resistant silicone grease is prepared by the following method:

[0050] Preparation: Weigh 70kg of silicone oil, 10kg of polytetrafluoroethylene, 5kg of nano titanium nitride, 1kg of antioxidant (octylbutyl diphenylamine), 2kg of extreme pressure anti-wear additive (sodium primary / secondary alkyl sulfonate), 0.2kg of anti-corrosion additive (octylbutyl diphenylamine) and 0.1kg of anti-rust additive (barium dinonylnaphthalene sulfonate).

[0051] Mixing: First add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 80°C, and add nano titanium nitride, octylbutyldiphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyldiphenylamine and barium dinonylnaphthalenesulfonate, and continue stirring for 1 hour to form fat.

[0052] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0053] Example 5

[0054] A high and low temperature resistant silicone grease is prepared by the following method:

[0055] Preparation: Weigh 78kg of silicone oil, 12kg of polytetrafluoroethylene, 2kg of nano-titanium nitride, 1.2kg of nano-montmorillonite, 2kg of nano-graphite powder, 8kg of vegetable wax, 0.8kg of antioxidant (octylbutyldiphenylamine), 1.8kg of extreme pressure and anti-wear additive (sodium primary / secondary alkyl sulfonate), 0.6kg of anti-corrosion additive (octylbutyldiphenylamine) and 0.2kg of anti-rust additive (barium dinonylnaphthalenesulfonate).

[0056] Mixing: first add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 80°C, and add nano titanium nitride, nano montmorillonite, nano graphite powder, vegetable wax, octylbutyl diphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyl diphenylamine and barium dinonylnaphthalene sulfonate, and continue stirring for 2 hours to form fat.

[0057] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0058] Example 6

[0059] A high and low temperature resistant silicone grease is prepared by the following method:

[0060] Preparation: Weigh 76kg of silicone oil, 13kg of polytetrafluoroethylene, 3kg of nano-titanium nitride, 1kg of nano-montmorillonite, 2kg of nano-graphite powder, 6kg of vegetable wax, 0.5kg of antioxidant (octylbutyldiphenylamine), 1kg of extreme pressure and anti-wear additive (sodium primary / secondary alkyl sulfonate), 0.5kg of anti-corrosion additive (octylbutyldiphenylamine) and 0.3kg of anti-rust additive (barium dinonylnaphthalenesulfonate).

[0061] Mixing: first add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 70°C, and add nano titanium nitride, nano montmorillonite, nano graphite powder, vegetable wax, octylbutyl diphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyl diphenylamine and barium dinonylnaphthalene sulfonate, and continue stirring for 2 hours to form fat.

[0062] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0063] Example 7

[0064] A high and low temperature resistant silicone grease is prepared by the following method:

[0065] Preparation: Weigh 72kg of silicone oil, 20kg of polytetrafluoroethylene, 2kg of nano-titanium nitride, 2kg of nano-montmorillonite, 3kg of nano-graphite powder, 5kg of vegetable wax, 0.2kg of antioxidant (octylbutyldiphenylamine), 2kg of extreme pressure and anti-wear additive (sodium primary / secondary alkyl sulfonate), 1kg of anti-corrosion additive (octylbutyldiphenylamine) and 0.1kg of anti-rust additive (barium dinonylnaphthalenesulfonate).

[0066] Mixing: First add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 72°C, and add nano titanium nitride, nano montmorillonite, nano graphite powder, vegetable wax, octylbutyl diphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyl diphenylamine and barium dinonylnaphthalene sulfonate, and continue stirring for 3 hours to form fat.

[0067] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0068] Example 8

[0069] A high and low temperature resistant silicone grease is prepared by the following method:

[0070] Preparation: Weigh 70kg of silicone oil, 10kg of polytetrafluoroethylene, 3kg of nano-titanium nitride, 0.5kg of nano-montmorillonite, 1.5kg of nano-graphite powder, 10kg of vegetable wax, 0.3kg of antioxidant (octylbutyldiphenylamine), 2kg of extreme pressure and anti-wear additive (sodium primary / secondary alkyl sulfonate), 0.5kg of anti-corrosion additive (octylbutyldiphenylamine) and 0.5kg of anti-rust additive (barium dinonylnaphthalenesulfonate).

[0071] Mixing: First add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 75°C, and add nano titanium nitride, nano montmorillonite, nano graphite powder, vegetable wax, octylbutyl diphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyl diphenylamine and barium dinonylnaphthalene sulfonate, and continue stirring for 3 hours to form fat.

[0072] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0073] Example 9

[0074] A high and low temperature resistant silicone grease is prepared by the following method:

[0075] Preparation: Weigh 76kg of silicone oil, 10kg of polytetrafluoroethylene, 2kg of nano-titanium nitride, 0.8kg of nano-montmorillonite, 2.5kg of nano-graphite powder, 10kg of vegetable wax, 0.3kg of antioxidant (octylbutyldiphenylamine), 1.2kg of extreme pressure and anti-wear additive (sodium primary / secondary alkyl sulfonate), 0.5kg of anti-corrosion additive (octylbutyldiphenylamine) and 0.2kg of anti-rust additive (barium dinonylnaphthalenesulfonate).

[0076] Mixing: first add silicone oil and polytetrafluoroethylene into the reactor, stir while heating, start keeping warm when the temperature reaches 80°C, and add nano titanium nitride, nano montmorillonite, nano graphite powder, vegetable wax, octylbutyl diphenylamine, primary / secondary alkyl sodium sulfonate, octylbutyl diphenylamine and barium dinonylnaphthalene sulfonate, and continue stirring for 2 hours to form fat.

[0077] Grinding: The greased mixture is transferred to a three-roll grinder for grinding to obtain the silicone grease lubricating oil of this embodiment.

[0078] Experimental example

[0079] The silicone grease prepared in Example 1 and Examples 5-7 of the present application was tested for appearance, cone penetration, dropping point, four-ball sintering load, Timken, corrosion, evaporation and steel mesh oil separation, and the results are shown in Table 1.

[0080] Table 1

[0081]

[0082]

[0083] It can be seen from Table 1 that the various properties of the high temperature resistant anti-seizure grease prepared in the examples of the present application meet the relevant regulations, and it has good viscosity, water and moisture resistance, corrosion resistance and lubrication performance.

[0084] In summary, the high and low temperature resistant silicone grease and its preparation method according to the embodiment of the present application have the following advantages:

[0085] 1. This application uses silicone oil as the base oil, which has the advantage of good stability. It is matched with polytetrafluoroethylene as a thickener. Both have excellent high and low temperature resistance and water resistance, which can make the entire silicone grease lubricant have high and low temperature resistance and water resistance. It has stable performance in the temperature range of -30 to 230°C and is suitable for a wider range of environments.

[0086] 2. The present application further adds titanium nitride, antioxidants, extrusion anti-wear additives, anti-corrosion additives and anti-rust additives on the basis of silicone oil and thickener, wherein titanium nitride still has stable lubrication and wear resistance at high temperatures, thereby increasing the operating temperature range of silicone grease lubricants, wherein the extrusion anti-wear additives, anti-corrosion additives and anti-rust additives can respectively increase the waterproof, corrosion-resistant and wear-resistant properties of silicone grease lubricants.

[0087] 3. Nano-montmorillonite, nano-graphite powder and plant wax are also added in the preferred mode of the present application. On the one hand, montmorillonite plays a role in increasing the viscosity and dispersibility of each raw material in the lubricating oil, and the graphite powder forms a graphite lubricating film under high temperature friction, which improves its lubricity and wear resistance; on the other hand, montmorillonite, graphite powder and titanium nitride are all nanomaterials, and the solid nanoparticles in the grease prepared therefrom can not only improve the thermal conductivity of the grease, but also improve the surface finish of the workpiece due to the ball bearing-like effect of the nanoparticles, fill the damaged parts of the metal material, reduce the surface roughness of the metal material, and then reduce the cutting force during cutting, and improve the lubrication effect. In addition, the plant wax itself has excellent anti-friction and anti-wear properties, and with the excellent heat transfer and dispersion stability of the nanoparticles, it can prevent blockage at the friction interface and improve its self-repairing ability.

[0088] In summary, the silicone grease lubricant prepared in the present application has good pumpability, extreme pressure resistance and wear resistance, lubricity, water and moisture resistance, and stability in high and low temperature environments.

[0089] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present application.

Claims

1. A high and low temperature resistant silicone grease, characterized in that: The invention is composed of the following raw materials by weight: 70-80 parts of silicone oil, 10-20 parts of polytetrafluoroethylene, 2-5 parts of nano titanium nitride, 0.2-1 parts of antioxidant, 0.5-2 parts of extreme pressure anti-wear additive, 0.2-1 parts of anti-corrosion additive, 0.1-0.5 parts of anti-rust additive, 0.5-2 parts of nano montmorillonite, 1-3 parts of nano graphite powder and 5-10 parts of vegetable wax.

2. The high and low temperature resistant silicone grease according to claim 1, characterized in that: The invention is composed of the following raw materials in parts by weight: 76 parts of silicone oil, 13 parts of polytetrafluoroethylene, 3 parts of nano titanium nitride, 0.5 parts of antioxidant, 1 part of extreme pressure anti-wear additive, 0.5 parts of anti-corrosion additive, 0.3 parts of anti-rust additive, 1 part of nano montmorillonite, 2 parts of nano graphite powder and 6 parts of vegetable wax.

3. A high and low temperature resistant silicone grease according to claim 1 or 2, characterized in that: The antioxidant is octylbutyldiphenylamine.

4. A high and low temperature resistant silicone grease according to claim 1 or 2, characterized in that: The extreme pressure anti-wear additive is sodium primary / secondary alkyl sulfonate.

5. The high and low temperature resistant silicone grease according to claim 1 or 2, characterized in that: The anti-corrosion additive is octylbutyl diphenylamine.

6. A high and low temperature resistant silicone grease according to claim 1 or 2, characterized in that: The anti-rust additive is barium dinonylnaphthalenesulfonate.

7. A method for preparing high and low temperature resistant silicone grease according to any one of claims 1 to 6, characterized in that: The following steps are involved: Put silicone oil and polytetrafluoroethylene in a reaction kettle, heat and mix them evenly, then add other raw materials and stir them evenly to obtain a fat-forming mixture; The grease mixture is ground to obtain the silicone grease.

8. The method for preparing a high and low temperature resistant silicone grease according to claim 7, characterized in that: The temperature after heating is 75-85° C., and the stirring time is 1-3 hours.

Citation Information

Patent Citations

  • Heat-resistant grease

    CN103265998A

  • Heat conducting silicone grease composition

    CN104119685A

  • Lubricant grease composition and preparation method of same

    CN105907446A

  • Use of calcium complex lubricating greases and calcium sulfonate complex lubricating greases for the lubrication of wire ropes

    CN110234745A