A composite electronic component and its preparation method and application
By using a top-down stacked ferroelectric material and multi-phase ceramic dielectric material combination structure in a multilayer chip ceramic capacitor, the electrostrictive and noise problems are solved, and excellent DC bias and noise reduction effects are achieved. .
Patent Information
- Application Number
- CN202311151012.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-09-06
AI Technical Summary
Existing multilayer chip ceramic capacitors can easily cause electrostriction under high electric fields, produce acoustic noise, affect user experience, and have insufficient performance in terms of DC bias.
A composite electronic component structure stacked from top to bottom is used. The first component is composed of ferroelectric materials, and the second component is composed of complex-phase ceramic dielectric materials, including ferroelectric materials and paraelectric materials. Through the interaction of different dielectric materials, Combination and structural design to optimize DC bias characteristics and noise reduction effect.
It significantly improves the DC bias performance, reduces the amplitude and noise of the circuit board, meets different capacity requirements, and provides a better user experience.
Smart Images

Figure CN117153564B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of electronic components, and specifically relates to a composite electronic component and a preparation method and application thereof. Background Art
[0002] Multilayer ceramic capacitors (MLCC) are electronic components that are small, high capacity, and easy to install, so they are widely used in electronic devices such as liquid crystal displays, plasma display panels, computers, and smart phones. MLCCs are usually composed of multiple alternately stacked dielectric layers, multiple sets of internal electrodes, and external electrodes connected to the internal electrodes. In recent years, MLCCs have gradually developed towards miniaturization and high capacity, with thinner dielectric layers and smaller distances between internal electrodes. Therefore, the corresponding bias electric field will also increase.
[0003] The ceramic dielectric materials used in MLCC are mainly divided into paraelectric materials (also known as Class I) and ferroelectric materials (also known as Class II). Among them, the ceramic dielectric of Class II material is prone to cause capacitance decay as the electric field strength increases, and because the ceramic dielectric of Class II material has an inverse piezoelectric effect, when a changing electric field is applied to the MLCC, electrostriction will occur. At this time, the vibration generated on the MLCC is transmitted to the circuit board through the solder, causing the circuit board to vibrate. When the vibration frequency of the circuit board is within the human hearing range of 20-20000Hz, it can generate uncomfortable noise, resulting in a decrease in the user experience of the final product.
[0004] In view of the problems existing in the use of the above-mentioned electronic components, finding an electronic component that can meet different sample capacity requirements, has low acoustic noise during use, and has good DC bias effect is the current research focus in the field of electronic components. Summary of the invention
[0005] The purpose of the present application is to overcome the deficiencies of the above-mentioned prior art and to provide a composite electronic component and a preparation method and application thereof, wherein the composite electronic component has excellent DC bias characteristics and noise reduction effects.
[0006] To achieve the above purpose, the technical solution adopted by this application is:
[0007] A composite electronic component, characterized in that the composite electronic component includes a first component and a second component stacked in sequence from top to bottom; the first component includes a first dielectric material, a first internal electrode and a first external electrode; the second component includes a second dielectric material and a second external electrode; the first dielectric material includes a ferroelectric material, the second dielectric material includes a complex ceramic dielectric material, and the complex ceramic dielectric material includes a ferroelectric material and a paraelectric material.
[0008] The first component and the second component of the composite electronic element described in the present application use different dielectric materials. Compared with the circuit in the prior art in which both electronic components are composed of ferroelectric materials, the DC bias characteristics are significantly improved. First, since the second dielectric material includes a multiphase ceramic dielectric material, and the multiphase ceramic dielectric material includes a ferroelectric material and a paraelectric material, these two types of materials have different responses under a DC electric field. The ferroelectric material is a tetragonal phase at room temperature, and the Ti in the unit cell is 4+ It deviates from the center position, causing the positive and negative charge centers of the unit cell to not coincide. When no electric field is applied, the directions of the spontaneous polarization of the dipoles in the MLCC are randomly arranged, and the spontaneous polarization intensity is zero. When a certain DC voltage is applied to both ends of the MLCC, the dipoles in the MLCC are oriented and polarized, which will cause the dielectric constant of the MLCC to decrease and the capacitance to decrease. The paraelectric material with the above structure has a small polarization intensity under an external DC electric field. When added to the composite ceramic dielectric material, the dielectric constant attenuation of the MLCC is reduced, so the capacity attenuation is reduced, and it has better DC bias performance.
[0009] Secondly, since the second dielectric material is a composite ceramic mainly composed of ferroelectric materials and paraelectric materials, its dielectric constant is smaller than that of ferroelectric materials. The vibration generated by the second dielectric material under a periodic electric field is smaller than that of the first dielectric material. The vibration of the first dielectric material needs to pass through the second dielectric material to reach the circuit board. As the energy transfer distance increases, the energy lost in the process also increases, and the energy transferred to the circuit board decreases, which can reduce the amplitude of the circuit board and reduce the noise.
[0010] The inventors have discovered that the placement order of the first component and the second component in the composite electronic component must be stacked from top to bottom; this ensures that when the composite electronic component is working, the second component is in contact with the circuit board, and in the process of energy transfer downward, the first component with a large amplitude in the upper layer increases the amplitude of the second component in the lower layer. According to the law of conservation of energy, it can be seen that: a part of the energy of the first dielectric material is divided away by the second dielectric material, so the energy transferred to the circuit board is reduced, the amplitude of the circuit board is reduced, and the noise is reduced; if the second component is on top and the first component is on the bottom, that is, the first component is in contact with the circuit board, then only DC bias resistance can be achieved, and noise reduction cannot be achieved.
[0011] As a preferred embodiment of the composite electronic component of the present application, in the second dielectric material, the ferroelectric material is selected from BaTiO3, BaTi (1-X) Zr X O3 and Ba (1-X) Ca X Zr (1-Y) Ti YO3, wherein 0.9 ≥ X > 0, 1 ≥ Y ≥ 0.1; the paraelectric material is selected from at least one of CaTiO3, CaZrO3, SrZrO3, BaZrO3 and ZrO2; the molar ratio of the ferroelectric material to the paraelectric material is ferroelectric material: paraelectric material = 1: (0.2-10); in the first dielectric material, the ferroelectric material is selected from BaTiO3, BaTi (1-X) Zr X O3 and Ba (1-X) Ca X Zr (1-Y) Ti Y At least one of O3, wherein 0.9≥X>0, 1≥Y≥0.1.
[0012] The inventors have found that the molar ratio of the ferroelectric material to the paraelectric material in the second dielectric material has a great influence on the noise reduction effect and DC bias performance of the composite electronic component prepared therefrom; if the proportion of the ferroelectric material is too large, the Ti 4+ The deviation from the center position causes the positive and negative charge centers of the unit cell to not coincide. Under the action of the periodic electric field, the central Ti 4+ It will make reciprocating motions, driving the lattice to vibrate up and down, causing the electrostrictive phenomenon of MLCC on a macro scale, increasing the energy transferred to the circuit board, causing the circuit board to vibrate too much and emit loud noise, and failing to achieve a good noise reduction effect; at the same time, if the proportion of ferroelectric materials is too large, the polarization intensity under the DC electric field will increase, the capacitance attenuation will increase, and it is easy to cause the deterioration of DC bias performance. If the proportion of paraelectric materials is too large, the dielectric constant of the composite ceramic dielectric material will be too small, making its initial capacity too low and resulting in a low overall capacity of the final composite electronic component, which will make it unsuitable for use in situations with high capacity requirements.
[0013] As a preferred embodiment of the composite electronic component of the present application, in the first component, the first internal electrodes and the first dielectric material layers are alternately stacked and connected, and the first external electrodes are arranged on both sides of the first internal electrodes and the first dielectric material layers.
[0014] As a preferred embodiment of the composite electronic component of the present application, the second component also includes a second internal electrode, which is alternately stacked and connected with the second dielectric material layer, and the second external electrode is arranged on both sides of the second internal electrode and the second dielectric material layer.
[0015] As a preferred embodiment of the composite electronic component described in the present application, the dielectric constant of the first dielectric material is 2000-6000; the dielectric constant of the second dielectric material is 30-1500.
[0016] As a more preferred embodiment of the composite electronic component described in the present application, the dielectric constant of the first dielectric material is 3000-5000; the dielectric constant of the second dielectric material is 100-300; and the dielectric constant ratio of the first dielectric material to the second dielectric material is first dielectric material: second dielectric material = (10-50):1.
[0017] The inventors have found through a large number of experiments that by limiting the dielectric constants of the two dielectric materials to the above range, the effects of reducing product noise and improving DC bias performance can be better achieved.
[0018] As a preferred embodiment of the composite electronic component described in the present application, the ferroelectric material in the first dielectric material includes BaTiO3, the ferroelectric material in the second dielectric material includes BaTiO3, and the paraelectric material includes CaZrO3, SrZrO3 or BaZrO3.
[0019] As a preferred embodiment of the composite electronic component described in the present application, the average particle size of the ferroelectric material in the first dielectric material is 0.3-0.8 μm; the average particle size of the multiphase ceramic dielectric material in the second dielectric material is 0.5-2.5 μm.
[0020] The inventors have found through a large number of experiments that when the particle size of the dielectric material is controlled within the above range, due to the small size of the grains, the degree of lattice deformation is small, the mechanical stress energy is small, the domain wall formation energy is increased, and the crystal growth is inhibited, resulting in the grains being close together, and the difficulty of rearrangement under the action of the electric field increases, so that better DC bias performance can be obtained; if the particle size is larger than the above range, the grain boundaries are reduced, resulting in reduced insulation resistance and reduced reliability of electronic components. If the particle size is smaller than the above range, there is no adverse effect on the performance, but the preparation process is difficult and the cost is high, and it is difficult to make the particle size smaller.
[0021] As a preferred embodiment of the composite electronic component described in the present application, the first and second dielectric materials also include the following elements: element R1, element M1, element M2; the element R1 is selected from at least one of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Y; the element M1 is selected from at least one of Mg, Mn, V, Fe, Co, Cr, Ni and Mo; the element M2 is selected from at least one of Si, B and Li.
[0022] As a more preferred embodiment of the composite electronic component described in the present application, the first dielectric material includes the following elements in molar percentage: element R1 0.05%-1%, element M1 0.1%-10%, element M2 0.1%-10%; the second dielectric material includes the following elements in molar percentage: element R1 0.1%-2%, element M1 0.1%-10%, element M2 0.1%-10%; and the molar ratio of element R1 in the first dielectric material and the second dielectric material is 1:(0.1-2).
[0023] The inventors have found through a large number of experiments that the above elements in the first and second dielectric materials can make the performance of the final composite electronic component more stable when the molar percentage content is within a specific range: if the content of each element in the first dielectric material is less than the above range, the capacitance insulation resistance (IR) value of the material may decrease. For example, if too little M1 element is added, the material's anti-reduction property will be weakened, and Ti will not be easily oxidized during the subsequent sintering process. 4+ Reduced to Ti 3+ , and at the same time, freely movable oxygen vacancies and weakly bound electrons appear, resulting in semiconductivity; if the content of each element is greater than the above range, the temperature stability of the electronic component material may decrease; when the molar percentage content of each element in the second dielectric material is less than the above range, the dielectric properties of the material may deteriorate and the insulation resistance may decrease. For example, if the addition of "amphoteric" rare earth is reduced in R1, it will cause association defects [Ho Ba Ho Ti ] is reduced, the oxygen vacancies under the electric field are restricted and reduced, and the mobility is increased, which leads to a decrease in IR; if the molar percentage of each element in the second dielectric material is greater than the above range, it may lead to an increase in heterogeneous phases, a high sintering temperature, and deterioration in reliability.
[0024] When the molar ratio of the element R1 in the first dielectric material and the second dielectric material is 1:(0.1-2), the various performances of the composite electronic component are more excellent. The content of the element R1 in the first dielectric material is relatively small, resulting in a decrease in the insulation resistance of the material and the occurrence of semiconductivity. The content of the element R1 is relatively large, resulting in a decrease in the temperature stability of the material. The content of the element R1 in the second dielectric material is relatively small, resulting in a deterioration in the dielectric properties of the material and a decrease in the insulation resistance. The content of the element R1 in the second dielectric material is relatively small, resulting in an increase in heterogeneity and a high sintering temperature, and the reliability of the composite electronic component is deteriorated.
[0025] As a preferred embodiment of the composite electronic component described in the present application, the composite electronic component also includes a bracket, which is composed of an upper contact portion, a connecting portion and a lower contact portion, the upper contact portion is in contact with the first external electrode and the second external electrode, the lower contact portion is arranged on the lower side of the second component, and the two ends of the connecting portion are respectively connected to the upper contact portion and the lower contact portion.
[0026] The present invention also provides a method for preparing the composite electronic component, comprising the following steps:
[0027] S1. Mixing the raw materials of the first dielectric material to form slurry A, mixing the raw materials of the second dielectric material to form slurry B, respectively casting slurry A and slurry B into ceramic films, and printing internal electrode slurries on the ceramic films, respectively, or only printing the internal electrode slurry on the ceramic film A, and obtaining the first dielectric material printed sheet and the second dielectric material printed sheet after drying;
[0028] S2, laminating, pressing, and cutting the first dielectric material printed sheet and the second dielectric material printed sheet obtained in step S1 to form a first laminate and a second laminate;
[0029] S3. Debinding, sintering, forming external electrodes, and burning ends are performed on the first and second stacks obtained in step S2, respectively, and then the first component and the second component are obtained respectively. The first component and the second component are bonded to obtain a composite electronic component; or the bonded first component and the second component are welded to a bracket to obtain a composite electronic component.
[0030] As a preferred embodiment of the preparation method of the composite electronic component described in the present application, in the step S3, the specific steps of welding the bonded first component and the second component to the bracket are: assembling the bonded first component and the second component together with the bracket with solder paste, and placing them in a fixing fixture, then placing the fixture in a nitrogen reflow oven at 200-300°C for welding, placing the welded bracket in an organic solvent for ultrasonication for 10-30 minutes, and drying to obtain a composite electronic component.
[0031] Compared with the prior art, the beneficial effects of this application are:
[0032] The first component of the composite electronic component described in the present application includes ferroelectric materials, and the second component includes complex ceramic dielectric materials, and the complex ceramic dielectric materials include ferroelectric materials and paraelectric materials. By using ferroelectric materials and paraelectric materials to cooperate with each other, the composite electronic component can meet different capacity requirements, and the acoustic noise generated is lower and the DC bias effect is better. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a schematic structural diagram of a composite electronic component according to one embodiment of the present application;
[0034] Figure 2 This is a schematic structural diagram of a composite electronic component according to one embodiment of the present application;
[0035] Figure 3 This is a schematic structural diagram of a composite electronic component according to one embodiment of the present application;
[0036] Figure 4 A schematic diagram of the structure of the composite electronic component described in one of the ratios of the present application;
[0037] Figure 5 A schematic diagram of the structure of the composite electronic component described in one of the ratios of the present application;
[0038] (1): first component, (11): first dielectric material layer, (12): first external electrode, (13): first internal electrode, (2): second component, (21): second dielectric material layer, (22): second external electrode, (23): second internal electrode, (3): bracket, (31): upper contact portion, (32): connecting portion, (33): lower contact portion; DETAILED DESCRIPTION
[0039] In order to better illustrate the purpose, technical solutions and advantages of the present application, the present application will be further described below in conjunction with specific embodiments.
[0040] Unless otherwise specified, the reagents, methods and equipment used in this application are conventional reagents, methods and equipment in this technical field.
[0041] Example 1
[0042] As a composite electronic component of an embodiment of the present application, Figure 1 As shown, the composite electronic component comprises a first component (1), a second component (2) and a bracket, and the bracket comprises an upper contact portion (31), a connecting portion (32) and a lower contact portion (33);
[0043] The first component (1) comprises a first dielectric material layer (11), a first internal electrode (13) and a first external electrode (12), wherein the first internal electrode (13) and the first dielectric material layer (11) are alternately stacked and connected, and the first external electrode (12) is arranged on the left and right sides of the first internal electrode (13) and the first dielectric material layer (11), and contacts the upper contact portion (31);
[0044] The second component (2) comprises a second dielectric material layer (21), a second internal electrode (23) and a second external electrode (22), wherein the second internal electrode (23) and the second dielectric material layer (21) are alternately stacked and connected, and the second external electrode (22) is arranged on the left and right sides of the second internal electrode (23) and the second dielectric material layer (21), and is in contact with the upper contact portion (31);
[0045] The lower contact portion (33) is arranged on the lower side of the second component (2), and the two ends of the connecting portion (32) connect the upper contact portion (31) and the lower contact portion (33).
[0046] The formula and parameters of the first dielectric material in the composite electronic component described in this embodiment are shown in Table 1, the formula and parameters of the second dielectric material are shown in Table 2, and the relationship between the dielectric constant ratio, particle size ratio, rare earth element molar ratio and other parameters of the first dielectric material and the second dielectric material is shown in Table 3.
[0047] The method for preparing the composite electronic component of this embodiment comprises the following steps:
[0048] S1. According to the formulas in Table 1 and Table 2, the raw materials of the first dielectric material are mixed to form slurry A, and the raw materials of the second dielectric material are mixed to form slurry B, and slurry A and slurry B are respectively cast into ceramic films, and internal electrode slurries are respectively printed on the ceramic films, and after drying, the first dielectric material printed sheet and the second dielectric material printed sheet are obtained;
[0049] S2, laminating the first dielectric material printed sheet and the second dielectric material printed sheet obtained in step S1 respectively to obtain laminated printed sheets, and cutting them after hydrostatic pressing to form a first laminated body and a second laminated body;
[0050] S3, subjecting the first laminated body and the second laminated body obtained in step S2 to debinding, sintering, forming external electrodes, and sintering ends, respectively, to obtain a first component and a second component;
[0051] S4. Assemble the first component and the second component obtained in step S3 together with the bracket with solder paste, and place them in a fixing fixture. Then place the fixture in a nitrogen reflow oven at 200-300°C for welding. Place the welded bracket in an organic solvent for ultrasonic treatment for 10-30 minutes. After drying, a composite electronic component is obtained.
[0052] Example 2-14
[0053] The difference between Examples 2-14 of the present application and Example 1 is that the formula of the composite electronic component is different, as shown in Tables 1-3; the remaining parameters of Examples 2-14 are consistent with those of Example 1.
[0054] Embodiment 15
[0055] The difference between Example 15 of the present application and Example 1 is that the second component of the composite electronic component does not include the second internal electrode (23). The specific structure is as follows: Figure 2 As shown;
[0056] The formula and parameters of the first dielectric material in the composite electronic component described in this embodiment are shown in Table 1, the formula and parameters of the second dielectric material are shown in Table 2, and the relationship between the dielectric constant ratio, particle size ratio, rare earth element molar ratio and other parameters of the first dielectric material and the second dielectric material is shown in Table 3.
[0057] The preparation method of the composite electronic component described in this embodiment is different from that in Embodiment 1 only in that: in the step S1, after slurry A and slurry B are respectively cast into ceramic films, the internal electrode slurry is only printed on the ceramic film of slurry A, and the internal electrode slurry is not printed on the ceramic film of slurry B, and after drying, a first dielectric material printed sheet and a second dielectric material printed sheet are obtained; the rest are consistent with Embodiment 1.
[0058] Example 16
[0059] The difference between this embodiment and embodiment 1 is that the upper contact portion (31) in the bracket only contacts the second external electrode (22) but not the first external electrode (12). Figure 3 As shown; the formula of the first dielectric material, the formula of the second dielectric material, the dielectric constant ratio of the first dielectric material to the second dielectric material, the particle size ratio, the molar ratio of rare earth elements and other parameters in the composite electronic component described in this embodiment are consistent with those in Example 1.
[0060] Comparative Examples 1-13
[0061] The difference between Comparative Examples 1-13 of the present application and Example 1 is that the formula of the composite electronic component is different, as shown in Tables 1-3; the other parameters of Comparative Examples 1-13 are consistent with those of Example 1.
[0062] Comparative Example 14
[0063] The difference between this comparative example and Example 1 is that the positions of the first component and the second component in the composite electronic component are exchanged, that is, the second component (2) is on the top and the first component (1) is on the bottom, and the first component (1) is in contact with the lower contact portion (33). Figure 4 As shown; the formula of the first dielectric material, the formula of the second dielectric material, the dielectric constant ratio of the first dielectric material to the second dielectric material, the particle size ratio, the molar ratio of rare earth elements and other parameters in the composite electronic component are consistent with those in Example 1.
[0064] Comparative Example 15
[0065] The difference between this comparative example and Example 1 is that the second component of the composite electronic component does not include a second external electrode (22). Figure 5 As shown; the formula of the first dielectric material, the formula of the second dielectric material, the dielectric constant ratio of the first dielectric material to the second dielectric material, the particle size ratio, the molar ratio of rare earth elements and other parameters in the composite electronic component are consistent with those in Example 1.
[0066] Table 1
[0067]
[0068]
[0069]
[0070]
[0071]
[0072] Table 2
[0073]
[0074]
[0075]
[0076]
[0077] Note: The ratios described in the molar content column of the R1 element in Tables 1 and 2 are the molar content ratios of the elements, for example, La:Ce:Ho:Y=1:1:0.2:0.5 represents the molar content ratio of the four elements.
[0078] Table 3
[0079]
[0080]
[0081] Performance Testing
[0082] The composite electronic components prepared in the embodiments and comparative examples were subjected to the following tests:
[0083] 1. Noise test:
[0084] Qualified range: Samples are qualified if their maximum vibration sound pressure is lower than 40dB.
[0085] Test method: The composite electronic component of the present invention is welded on a special circuit board, and the circuit board is placed in a silent box. A power resistor is used as a load, and an AC voltage with a frequency of 20-20000 Hz and a voltage of 10 KV / mm is applied to the electronic component. Then, the maximum sound pressure level of the sound is measured and recorded with a noise meter. The results are shown in Table 4 below.
[0086] 2. Initial capacitance and DC bias characteristics test:
[0087] Qualified range: Samples with a capacity lower than 5μF are considered unqualified; samples with a capacity decay rate exceeding -40% are considered unqualified.
[0088] Test method: Place the composite electronic component in a bias test device, first test the initial capacitance data C0 when the AC voltage is 1.0V and the DC bias is 0, then test the electrostatic capacitance value Cx when a DC bias of 100V is applied, wait for 1 minute after switching the voltage and record the capacitance data; after the sample capacitance test is completed, calculate the capacitance attenuation rate △Cx according to formula (1), and the results are shown in Table 4 below.
[0089]
[0090] 3. Insulation resistance test:
[0091] Qualified range: Insulation resistance below 1GΩ is considered unqualified.
[0092] Test method: A voltage of 4 KV / mm was applied in a resistance tester, and the resistance data of the composite electronic component was recorded. The results are shown in Table 4 below.
[0093] 4. Temperature coefficient of capacitance (TCC) test:
[0094] Qualified range: At -55℃-125℃, the temperature change rate of the capacitor is considered qualified if it is within ±15%.
[0095] Test method: In a high and low temperature rapid cycle box, the electrostatic capacitance of the composite electronic components at different temperatures (25°C, +125°C) is tested, and the temperature change rate of the capacitance at different temperatures and the capacitance at room temperature (+25°C) is calculated, such as △C125°C / C25°C. The results are shown in Table 4 below.
[0096] Table 4
[0097]
[0098]
[0099] According to the data in Table 4, the initial capacity of the composite electronic components prepared in Examples 1-16 of the present application is higher than 5μF, the DC bias capacity change rate does not exceed -40%, and has excellent DC bias characteristics. The maximum vibration sound pressure of the product is lower than 40dB, the noise reduction effect is good, and the insulation resistance is higher than 1GΩ. At -55℃-125℃, the temperature change rate of the capacitor is within ±15%, which can meet different capacity requirements.
[0100] In Comparative Example 1, due to the small dielectric constant of the first dielectric material, the initial capacity of the composite electronic component is low and does not meet the standard; in Comparative Example 2, due to the large dielectric constant of the first dielectric material, the acoustic noise and the DC bias capacity change rate are high; in Comparative Example 3, due to the large dielectric constant of the second dielectric material, the dielectric constant ratio of the first dielectric material to the second dielectric material is too small, and the noise reduction effect and DC bias performance are not ideal; in Comparative Example 4, due to the small molar ratio of the ferroelectric material to the paraelectric material in the second dielectric material, the capacity is low, making the composite electronic component It is not suitable for occasions with high capacity requirements; in Comparative Example 5, due to the excessive molar ratio of ferroelectric material to paraelectric material in the second dielectric material, the dielectric constant of the second dielectric material is high, and the noise reduction performance and DC bias performance are not ideal; in Comparative Examples 6-7, due to the excessive particle size of the first dielectric material or the second dielectric material, the grain boundary is reduced, the insulation resistance is reduced, and the reliability of the electronic component is reduced; in Comparative Examples 8 and Comparative Examples 9, the content of element R1 in the first dielectric material is not within the range provided by the present invention, and the content of element R1 in Comparative Example 8 is relatively small, resulting in a decrease in the insulation resistance of the material and the occurrence of semiconductor The comparative example 9 has a high content of element R1, which leads to unsatisfactory temperature stability of the material; the comparative example 10 has a low content of element R1 in the second dielectric material, which leads to deterioration of the dielectric properties of the material and a decrease in insulation resistance; the comparative example 13 has a high content of element R1 in the second dielectric material, which leads to an increase in heterogeneity and a high sintering temperature, and the reliability of the composite electronic component deteriorates; the comparative examples 11 and 12 do not use the multiphase ceramic dielectric material as the second dielectric material, but only use ferroelectric materials or paraelectric materials, and the final composite electronic component has poor performance, only When ferroelectric materials are used, the acoustic noise and DC bias capacity change rate generated exceed the qualified range; if only paraelectric materials are used, the capacity will be low and the applicable range of the capacitor will be reduced; in Comparative Example 14, since the second component in the composite electronic component is on the top and the first component is on the bottom, that is, the first component is closer to the circuit board, the maximum vibration sound pressure of the final sample is 50dB (A), and the noise reduction effect cannot be achieved; in Comparative Example 15, since the second component does not include a second external electrode, the DC bias capacity change rate of the final composite electronic component exceeds the qualified range and the DC bias performance is poor.
[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A composite electronic component, characterized in that: The composite electronic component comprises a first component and a second component stacked in sequence from top to bottom; the first component comprises a first dielectric material, a first internal electrode and a first external electrode; the second component comprises a second dielectric material and a second external electrode; the first dielectric material comprises a ferroelectric material, the second dielectric material comprises a multiphase ceramic dielectric material, and the multiphase ceramic dielectric material comprises a ferroelectric material and a paraelectric material; In the second dielectric material, the ferroelectric material is selected from BaTiO3, BaTi (1-X) Zr X O3 and Ba (1-X) Ca X Zr (1-Y) Ti Y O3, wherein 0.9 ≥ X > 0, 1 ≥ Y ≥ 0.1; the paraelectric material is selected from at least one of CaTiO3, CaZrO3, SrZrO3 and ZrO2; the molar ratio of the ferroelectric material to the paraelectric material is ferroelectric material: paraelectric material = 1: (0.2-10); in the first dielectric material, the ferroelectric material is selected from BaTiO3, BaTi (1-X) Zr X O3 and Ba (1-X) Ca X Zr (1-Y) Ti Y At least one of O3, wherein 0.9≥X>0, 1≥Y≥0.1; The first and second dielectric materials both further include the following elements: element R1, element M1, and element M2; the element R1 is selected from at least one of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Y; the element M1 is selected from at least one of Mg, Mn, V, Fe, Co, Cr, Ni, and Mo; the element M2 is selected from at least one of Si, B, and Li; the first dielectric material includes the following elements in molar percentage: element R1 0.05%-1%, element M1 0.1%-10%, and element M2 0.1%-10%; the second dielectric material includes the following elements in molar percentage: element R1 0.1%-2%, element M1 0.1%-10%, and element M2 0.1%-10%; and the molar ratio of element R1 in the first dielectric material to the second dielectric material is 1:(0.1-2); The average particle size of the ferroelectric material in the first dielectric material is 0.3-0.8 μm; the average particle size of the multiphase ceramic dielectric material in the second dielectric material is 0.5-2.5 μm; The method for preparing the composite electronic component comprises the following steps: S1. Mixing the raw materials of the first dielectric material to form slurry A, mixing the raw materials of the second dielectric material to form slurry B, casting slurry A and slurry B into ceramic films A and B respectively, and printing internal electrode slurry on ceramic films A and B respectively, or printing internal electrode slurry only on ceramic film A, and obtaining the first dielectric material printed sheet and the second dielectric material printed sheet after drying; S2, laminating, pressing, and cutting the first dielectric material printed sheet and the second dielectric material printed sheet obtained in step S1 to form a first laminate and a second laminate; S3, subjecting the first laminated body and the second laminated body obtained in step S2 to debinding, sintering, forming external electrodes, and burning ends, respectively, and obtaining a first component and a second component after burning the ends, and bonding the first component and the second component to obtain a composite electronic component; or welding the bonded first component and the second component to a bracket to obtain a composite electronic component; The insulation resistance of the composite electronic component is higher than 1 GΩ.
2. The composite electronic component according to claim 1, wherein: In the first component, the first internal electrodes and the first dielectric material are alternately stacked and connected, and the first external electrodes are arranged on both sides of the first internal electrodes and the first dielectric material layer.
3. The composite electronic component according to claim 1, wherein: The second component also includes a second internal electrode, which is alternately stacked and connected with the second dielectric material, and a second external electrode is arranged on both sides of the second internal electrode and the second dielectric material layer.
4. The composite electronic component according to any one of claims 1 to 3, characterized in that: The dielectric constant of the first dielectric material is 2000-6000; the dielectric constant of the second dielectric material is 30-1500.
5. The composite electronic component according to claim 4, wherein: The dielectric constant of the first dielectric material is 3000-5000; the dielectric constant of the second dielectric material is 100-300; and the dielectric constant ratio of the first dielectric material to the second dielectric material is first dielectric material: second dielectric material=(10-50):
1.
6. The composite electronic component according to claim 1, wherein: The composite electronic component also includes a bracket, which consists of an upper contact part, a connecting part and a lower contact part. The upper contact part contacts the first external electrode and the second external electrode, the lower contact part is arranged at the lower side of the second component, and the two ends of the connecting part are respectively connected to the upper contact part and the lower contact part.
7. A method for preparing a composite electronic component according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Mixing the raw materials of the first dielectric material to form slurry A, mixing the raw materials of the second dielectric material to form slurry B, casting slurry A and slurry B into ceramic films A and B respectively, and printing internal electrode slurry on ceramic films A and B respectively, or printing internal electrode slurry only on ceramic film A, and obtaining the first dielectric material printed sheet and the second dielectric material printed sheet after drying; S2, laminating, pressing, and cutting the first dielectric material printed sheet and the second dielectric material printed sheet obtained in step S1 to form a first laminate and a second laminate; S3. Debinding, sintering, forming external electrodes, and burning ends are performed on the first and second stacks obtained in step S2, respectively. After burning ends, the first component and the second component are obtained respectively. The first component and the second component are bonded together to obtain a composite electronic component; or the bonded first component and the second component are welded to a bracket to obtain a composite electronic component.