Laser sealing method of glass and titanium alloy by adding copper foam as transition layer

By adding foam copper foam and TiZrNiCu solder at the junction of glass and titanium alloy, a barrier layer is formed to avoid the formation of brittle intermetallic compounds, the problem of defects in the sealing interface between glass and titanium alloy is solved, and the heat resistance of the sealing body is improved and service life.

CN117209169BActive Publication Date: 2024-11-29SUZHOU UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311074425.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-24
Publication Date
2024-11-29
Estimated Expiration
2043-08-24

AI Technical Summary

Technical Problem

The prior art has problems such as poor wetting and high-temperature phase change in the sealing process between glass and titanium alloy, resulting in defects in the sealing interface, poor airtightness, poor insulation resistance, and titanium alloy is prone to oxidation at high temperature, increasing subsequent surfaces. Difficulty in processing.

Method used

Using foam copper as the transition layer, a barrier layer is formed to avoid the formation of brittle intermetallic compounds by adding TiZrNiCu solder and foam copper at the junction of glass and titanium alloy, and laser sealing is achieved.

Benefits of technology

It improves the heat shock resistance and thermal cycling performance of glass and titanium alloy sealing joints, reduces thermal stress and interface pressure, and extends the service life of the sealing joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117209169B_ABST
    Figure CN117209169B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for laser sealing glass and titanium alloy by adding copper foam as a transition layer, and belongs to the technical field of sealing of heterogeneous materials. The present invention uses TiZrNiCu as solder and adds copper foam as an intermediate transition layer to perform laser sealing to obtain a glass-titanium alloy sealing body. During the sealing process of the present invention, copper foam is introduced as a functional gradient material while introducing solder between glass and titanium alloy, which effectively reduces the mismatch caused by the excessive difference in thermal expansion coefficient between glass and titanium alloy, the stress release problem caused by the difference in physical properties and the sensitivity to crack initiation, reduces the thermal stress and interface pressure between them, and improves the allowable limit of thermal shock and thermal cycle resistance of titanium alloy and glass sealing body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealing heterogeneous materials, and in particular to a method for laser sealing glass and titanium alloy by adding foam copper as a transition layer. Background Art

[0002] The sealing of glass and metal is mostly done by sealing with composite rubber strips, or by sealing with butyl rubber and polysulfide rubber. The sealing of glass and metal is achieved by bonding and sealing glass and sealing strips. Alternatively, the metal surface is oxidized to form an oxide film, and then the metal is kept warm for a long time under high temperature conditions in a heat preservation furnace to achieve the sealing of glass and metal. Due to the high temperature and long heat preservation time during sealing, the properties of glass and metal are damaged, and the control of production efficiency and quality is also very inconvenient. Compared with traditional metal materials for sealing, the strength of titanium and titanium alloy materials is similar to that of high-quality steel. It not only has the advantages of low density, light weight, and high specific strength, but also has the advantages of wide working range and corrosion resistance. It is known as the "metal of the 21st century" and is widely used in aerospace, navigation, chemical industry, metallurgy, medical treatment, instrumentation and other fields. However, titanium alloy materials have problems such as poor wettability and high-temperature phase change during the sealing process with glass. Therefore, there are certain defects in the sealing interface between glass and titanium alloy. For example, when disturbed by changes in the external environment, a large number of microcracks will be generated at the defects of the sealing interface, resulting in poor airtightness and poor insulation resistance. At the same time, titanium alloys are very easy to oxidize at high temperatures, and different types of oxide layers are formed at different temperatures, which will increase the difficulty of subsequent surface treatment. Therefore, a convenient and reliable sealing method is still needed to achieve the sealing of glass and titanium alloy.

[0003] At present, to improve the stability of glass and titanium alloy seals under thermal cycle loads, using an intermediate layer to release stress and reduce the formation of brittle intermetallic compounds is an effective solution. Obviously, optimizing the chemical composition of the solder, forming a gradient material, and reducing or preventing the formation of brittle intermetallic compounds is an excellent solution.

[0004] Since copper foam is very easy to form compounds with metallic properties with glass, and copper foam is also very easy to form brittle intermetallic compounds with Fe, Ni and other metals, this makes the commonly used solder form brittle intermetallic compounds in the glass-metal seal. In order to prevent the formation of brittle intermetallic compounds, we add a layer of solder between the copper foam and the metal to form a barrier layer, so that it is difficult or impossible to form brittle intermetallic compounds between the copper foam and the base metal due to the presence of the barrier layer, so that it is possible to further improve the heat cycle load resistance of the glass-metal seal. Since the traditional solder is directly composed of Ag-Cu or Ag-Cu-Ti, this solder is a compound with metallic properties. Its advantage is that it can be combined with glass or ceramics, but it will inevitably form brittle intermetallic compounds with Ti, Al, and Ni in the base metal, so it is urgent to develop a new material system to replace the existing material system. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for laser sealing glass and titanium alloy by adding foam copper as a transition layer. Specifically, it is a method for laser sealing glass and titanium alloy by adding foam copper as a transition layer, which can effectively improve the strength of the sealing joint between glass and titanium alloy.

[0006] The present invention is achieved through the following technical solutions:

[0007] The first object of the present invention is to provide a method for laser sealing glass and titanium alloy by adding copper foam as a transition layer, comprising the following steps:

[0008] S1: Setting the processing trajectory according to the size and shape of the glass and titanium alloy to be sealed;

[0009] S2: evenly spray or place solder on one side of the titanium alloy to be sealed, place foam copper on the solder; and spray or place solder again on the foam copper;

[0010] The solder is TiZrNiCu powder or TiZrNiCu foil, and the TiZrNiCu powder or TiZrNiCu foil comprises the following components in atomic percentage: Ti-5Zr-15Ni-15Cu;

[0011] The foam copper is foam copper powder or foam copper foil;

[0012] S3: placing the glass to be sealed on the titanium alloy with the foam copper and solder, ensuring that the glass to be sealed is in close contact with the titanium alloy to form a body to be sealed;

[0013] S4: Clamping the body to be sealed obtained in step S3, laser irradiating the solder at the interface between the glass and the titanium alloy according to the processing trajectory set in step S1, to obtain a glass-titanium alloy sealing body.

[0014] In one embodiment of the present invention, in step S1, the glass to be sealed and the titanium alloy to be sealed are obtained by the following pretreatment:

[0015] The titanium alloy to be sealed is degreased and deoiled before being oxidized;

[0016] Wash the glass to be sealed with clean water, then cool and air dry.

[0017] In one embodiment of the present invention, in step S1, the titanium alloy is titanium alloy Ti6Al4V.

[0018] In one embodiment of the present invention, in step S1, the glass is high-purity silica glass.

[0019] In one embodiment of the present invention, in step S2, the thickness of the solder is 20 μm-100 μm.

[0020] In one embodiment of the present invention, in step S2, the particle size of the TiZrNiCu powder is 5 μm-50 μm.

[0021] In one embodiment of the present invention, in step S2, when the solder is TiZrNiCu powder, a foam copper foil is placed on the solder;

[0022] When the solder is a TiZrNiCu foil, a foam copper foil is placed on the solder or foam copper powder is sprayed.

[0023] That is, TiZrNiCu and copper foam can be placed as foils at the same time, but cannot be placed as powders at the same time.

[0024] Specifically, the TiZrNiCu powder or TiZrNiCu foil and foam copper foil have metallic luster and do not need to be oxidized.

[0025] In one embodiment of the present invention, in step S2, the thickness of the foam copper foil is 10 μm-30 μm.

[0026] In one embodiment of the present invention, in step S2, the particle size of the foam copper powder is less than 10 μm and the purity is greater than 99.7%.

[0027] In one embodiment of the present invention, in step S4, the wavelength of the laser is 800nm-1100nm.

[0028] In one embodiment of the present invention, in step S4, the parameters of the laser irradiation are: the laser scanning speed is 80 mm·min -1 -160mm·min -1 ; Laser power is 80W-160W; Pulse width is 1.5ms-3.0ms; Frequency is 5Hz-10Hz; Number of scans is 1-3.

[0029] In one embodiment of the present invention, in step S4, laser irradiation is performed in a protective atmosphere; specifically, the protective atmosphere is helium or argon, preferably argon.

[0030] The second object of the present invention is to provide a glass-titanium alloy sealing body made by the laser sealing method. The glass-titanium alloy sealing body comprises glass, titanium alloy, and solder and foam copper for sealing arranged between the edges of the glass and the titanium alloy. The specific structural schematic diagram is as follows Figure 1 shown.

[0031] The solder used in the present invention is composed of TiZrNiCu, and the copper foam is used as a separate solder welding layer, and TiZrNiCu forms a barrier layer between the metal substrate and the copper foam to prevent the formation of brittle intermetallic compounds between the copper foam and the substrate. Therefore, the use of TiZrNiCu as the solder and the copper foam as the transition layer to seal the glass and the titanium alloy proposed in the present invention can further improve the performance of the titanium alloy and glass seal, especially the thermal shock resistance performance.

[0032] The above technical solution of the present invention has the following advantages compared with the prior art:

[0033] In the sealing process of the present invention, solder is introduced between glass and titanium alloy and foam copper is introduced as a functional gradient material at the same time, which effectively reduces the mismatch caused by the large difference in thermal expansion coefficients between glass and titanium alloy and the stress release problem and crack initiation sensitivity caused by the difference in physical properties, reduces the thermal stress and interface pressure between them, and improves the allowable limit of thermal shock and thermal cycle resistance of the titanium alloy and glass seal. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein

[0035] Figure 1 It is a schematic diagram of the material combination of the sealing body of the present invention;

[0036] Explanation of the reference numerals in the specification: 1. titanium alloy steel plate; 2. solder; 3. foamed Ni; 4. glass. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0038] Example 1

[0039] This embodiment provides a method for laser sealing glass and titanium alloy by adding copper foam as a transition layer, and the specific steps are as follows:

[0040] S1: Use a window glass sample of 8mm×20mm×4mm as the glass to be sealed, and a titanium alloy Ti6Al4V steel plate of 10mm×25mm×1.5mm as the titanium alloy Ti6Al4V to be sealed, set the processing trajectory, and prepare the welding fixture;

[0041] S2: Degreasing and deoiling the titanium alloy Ti6Al4V to be sealed and then oxidizing it; washing the glass to be sealed with clean water and then cooling and air-drying it;

[0042] S3: A TiZrNiCu foil with a thickness of about 20 μm is used as solder, placed on one side of the titanium alloy Ti6Al4V to be sealed, and a foam copper powder with a thickness of 11 μm is sprayed on the solder; wherein the TiZrNiCu foil includes the following components in terms of atomic percentage: Ti-5Zr-15Ni-15Cu, and has a metallic luster, and no special treatment is required; the purity of the foam copper powder is greater than 99.7%;

[0043] S4: placing the glass to be sealed on the titanium alloy Ti6Al4V with the foam copper and solder, ensuring that the glass to be sealed is in close contact with the titanium alloy Ti6Al4V to form a body to be sealed; placing a layer of TiZrNiCu foil with a thickness of about 20 μm on the foam copper powder;

[0044] S5; the welding fixture clamps the body to be sealed in step S4 as required, and prepares for laser sealing;

[0045] S6: Use a fiber laser with a wavelength of 1064nm, and set the laser processing parameters of the fiber laser as follows: laser scanning speed 100mm·min -1 , laser power 110W, pulse width 1.5ms, frequency 7Hz, scanning times 1-3;

[0046] The laser follows the processing trajectory set in step S1: the scanning length is 78 mm (X direction) and 18 mm (Y direction), and in an argon atmosphere, at a distance of 2 mm from the solder, the laser is irradiated on the solder at the junction of the glass and the titanium alloy Ti6Al4V, where the solder acts as a "glue" to obtain a glass-titanium alloy Ti6Al4V sealing body;

[0047] S7: Remove the welding fixture and complete the entire laser sealing operation process.

[0048] It is measured through experiments that the shear strength of the glass-titanium alloy Ti6Al4V sealing body obtained by the laser sealing method of this embodiment can reach 30 MPa.

[0049] The thermal fatigue test was conducted with the sealing body without the copper foam layer added as a comparison. The test method was to put the sealing body with and without the copper foam layer into the insulation furnace for insulation at the same time. After insulation for 12 minutes, the sealing body was taken out and placed at room temperature. The fan was used to cool the sealing body for 20 minutes. After the sealing body temperature reached room temperature, the sealing body was placed in the furnace for insulation for 12 minutes. This was repeated. After every 5 times, the sealing body at room temperature was color checked to check whether there were cracks.

[0050] The results show that under the conditions of this embodiment, cracks appeared in the seal without adding the copper foam layer after 5 cycles, and the seal failed. However, cracks did not appear in the seal with the copper foam layer after 5 cycles, and cracks appeared in the 10th cycle. At the same time, the traditional seal without adding solder requires high temperature oxidation of the titanium alloy, and the seal using Ag-Cu as solder fails after more than one cycle.

[0051] Example 2

[0052] This embodiment provides a method for laser sealing glass and titanium alloy by adding copper foam as a transition layer, which is similar to the method in Embodiment 1, except that:

[0053] The thickness of the TiZrNiCu solder used is 32 μm, and the solder is in powder form. A foam copper foil is placed on it. The thickness of the foam copper foil is 15 μm. A Nd-YAG laser with a wavelength of 1000 nm is used. The processing trajectory set by the Nd-YAG laser is a scanning length of 78 mm (X direction) and 18 mm (Y direction), and the laser parameters are set as follows: laser scanning speed 40 mm min -1 , laser power 130W, pulse width 2.5ms, frequency 10Hz, scanning times 1-3, and laser sealing operation on glass and titanium alloy Ti6Al4V was performed at a distance of 1mm from the solder.

[0054] It is measured through experiments that the shear strength of the glass-titanium alloy Ti6Al4V sealing body obtained by the laser sealing method of this embodiment can reach 37 MPa.

[0055] The thermal fatigue test was conducted with the sealing body without the addition of the copper foam layer as a comparison. The results showed that under the conditions of this embodiment, cracks appeared in the sealing body without the addition of the copper foam layer after 10 cycles, and the sealing body failed. However, there was no crack in the sealing body with the addition of the copper foam layer after 15 cycles, and cracks appeared after the 20th cycle. At the same time, the traditional sealing body without the addition of solder requires high-temperature oxidation of the titanium alloy, and the sealing body using Ag-Cu as the solder fails after more than one cycle.

[0056] Example 3

[0057] This embodiment provides a method for laser sealing glass and titanium alloy by adding copper foam as a transition layer, which is similar to the method in Embodiment 1, except that:

[0058] The thickness of the TiZrNiCu solder used is 45μm, and the TiZrNiCu is in the form of a foil, which is covered with a layer of foam copper foil with a thickness of 20μm. A semiconductor laser with a wavelength of 940nm is used, and the processing trajectory set by the semiconductor laser is a scanning length of 78mm (X direction) and 18mm (Y direction), and the laser parameters are set as follows: laser scanning speed 160mm·min -1 , laser power 160W, pulse width 1.8ms, frequency 8Hz, scanning times 1-3, and laser sealing operation on glass and titanium alloy Ti6Al4V was performed at a distance of 3mm from the solder.

[0059] It is measured through experiments that the shear strength of the glass-titanium alloy Ti6Al4V sealing body obtained by the laser sealing method of this embodiment can reach 44 MPa.

[0060] The thermal fatigue test was conducted with the seal without the copper foam layer as a comparison. The results showed that under the conditions of this embodiment, cracks appeared in the seal without the copper foam layer after 20 cycles, and the seal failed. However, there was no crack in the seal with the copper foam layer after 25 cycles, and cracks appeared after the 30th cycle. At the same time, the traditional seal without solder required high-temperature oxidation of the titanium alloy, and the seal using Ag-Cu as solder failed after more than one cycle.

[0061] Example 4

[0062] This embodiment provides a method for laser sealing glass and titanium alloy by adding copper foam as a transition layer, which is similar to the method in Embodiment 1, except that:

[0063] The thickness of the TiZrNiCu component of the solder used is 70 μm, and the TiZrNiCu is in the form of powder, which is covered with a foam copper foil with a thickness of 25 μm. The semiconductor laser with a wavelength of 810 nm is used. The processing trajectory set by the semiconductor laser is a scanning length of 78 mm (X direction) and 18 mm (Y direction), and the laser parameters are set as follows: laser scanning speed 163 mm·min -1 , laser power 161W, pulse width 1.9ms, frequency 9Hz, scanning times 1-3, and laser sealing operation on glass and titanium alloy Ti6Al4V was performed at a distance of 3mm from the solder.

[0064] It is measured through experiments that the shear strength of the glass-titanium alloy Ti6Al4V sealing body obtained by the laser sealing method of this embodiment can reach 46 MPa.

[0065] The thermal fatigue test was conducted with the seal without the copper foam layer as a comparison. The results showed that under the conditions of this embodiment, cracks appeared in the seal without the copper foam layer at 25 cycles and the seal failed. However, cracks did not appear in the seal with the copper foam layer at 30 cycles, and cracks appeared at the 35th cycle. At the same time, the traditional seal without solder required high-temperature oxidation of the titanium alloy, and the seal using Ag-Cu as solder failed after more than one cycle.

[0066] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for laser sealing glass and titanium alloy by adding copper foam as a transition layer, characterized in that: The following steps are included: S1: Setting the processing trajectory according to the size and shape of the glass and titanium alloy to be sealed; S2: evenly spray or place solder on one side of the titanium alloy to be sealed, place foam copper on the solder; and spray or place solder again on the foam copper; The solder is TiZrNiCu powder or TiZrNiCu foil, and the TiZrNiCu powder or TiZrNiCu foil comprises the following components in atomic percentage: Ti-5Zr-15Ni-15Cu; The foam copper is foam copper powder or foam copper foil; S3: placing the glass to be sealed on the titanium alloy with the foam copper and solder, ensuring that the glass to be sealed is in close contact with the titanium alloy to form a body to be sealed; S4: Clamping the body to be sealed obtained in step S3, laser irradiating the solder at the interface between the glass and the titanium alloy according to the processing trajectory set in step S1, to obtain a glass-titanium alloy sealing body; In step S2, when the solder is TiZrNiCu powder, a foam copper foil is placed on the solder; When the solder is a TiZrNiCu foil, a foam copper foil is placed on the solder or foam copper powder is sprayed.

2. The laser sealing method according to claim 1, characterized in that: In step S1, the glass to be sealed and the titanium alloy to be sealed are obtained by the following pretreatment: The titanium alloy to be sealed is degreased and deoiled before being oxidized; Wash the glass to be sealed with clean water, then cool and air dry.

3. The laser sealing method according to claim 1, characterized in that: In step S2, the thickness of the solder is 20 μm-100 μm.

4. The laser sealing method according to claim 1, characterized in that: In step S2, the particle size of the TiZrNiCu powder is 5 μm-50 μm.

5. The laser sealing method according to claim 1, characterized in that: In step S2, the thickness of the foam copper foil is 10 μm-30 μm.

6. The laser sealing method according to claim 1, characterized in that: In step S4, the wavelength of the laser is 800nm-1100nm.

7. The laser sealing method according to claim 1, characterized in that: In step S4, the parameters of the laser irradiation are: the laser scanning speed is 80 mm·min -1 -160 mm min -1 ; Laser power is 80 W-160 W; Pulse width is 1.5ms-3.0 ms; Frequency is 5 Hz-10 Hz; Number of scans is 1-3.

8. The laser sealing method according to claim 1, characterized in that: In step S4, laser irradiation is performed in a protective atmosphere.

9. A glass-titanium alloy seal obtained by the laser sealing method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for realizing laser sealing of glass and stainless steel by adding titanium as transition layer

    CN115213561A