A method for preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene

By using ZSM-5 molecular sieve catalyst to carry out co-pyrolysis reaction with lignin and low-density polyethylene under anaerobic conditions, and optimizing the temperature and mixing ratio, the problems of waste agricultural film pollution and low quality of pyrolysis oil in agricultural films were solved. Efficient and low-cost preparation of aromatic hydrocarbons was achieved.

CN117247789BActive Publication Date: 2024-10-29SHIHEZI UNIVERSITY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311250295.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-26
Publication Date
2024-10-29
Estimated Expiration
2043-09-26

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively utilize low-density polyethylene and lignin in agricultural films, resulting in a high risk of pollution from waste agricultural films. Moreover, the phenolic substances in pyrolysis oil have high oxygen content and low calorific value, making it difficult to convert into high-quality aromatic hydrocarbons. .

Method used

Under anaerobic conditions, ZSM-5 molecular sieve catalyst is used to carry out co-pyrolysis reaction with lignin and low-density polyethylene. By optimizing the temperature and mixing ratio, the selectivity and conversion rate of aromatic hydrocarbons are improved.

Benefits of technology

It achieves low-cost, pollution-free preparation of aromatic hydrocarbons, significantly increases the content of aromatic hydrocarbons in pyrolysis oil, optimizes raw material conversion rate and selectivity, and solves the problem of resource utilization and pollution of waste agricultural film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117247789B_ABST
    Figure CN117247789B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene. Specifically, the method involves using lignin and low-density polyethylene as raw materials, and carrying out a pyrolysis reaction under the action of a catalyst to prepare aromatic hydrocarbons. In this method, the pyrolysis oil of lignin contains a large amount of phenolic substances, resulting in a high oxygen content and low calorific value. By adding LDPE with a high H / C ratio as a hydrogen source during the pyrolysis process, and mixing it with a ZSM-5 molecular sieve catalyst, the phenolic substances can be converted into aromatic hydrocarbons, thereby improving the quality of the pyrolysis oil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical technology, and particularly relates to a method for preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene. Background Art

[0002] Pyrolysis is an advanced thermochemical technology that obtains valuable products by changing the reaction temperature, heating rate, residence time and catalyst. Biomass pyrolysis refers to the process of placing biomass in an oxygen-poor or even oxygen-free atmosphere, heating it to break the chemical bonds of macromolecular organic matter, and decomposing it to produce coke, pyrolysis oil and non-condensable gases.

[0003] Lignin is a kind of biomass, which is widely present in plants. It is wrapped around the surface of cellulose and hemicellulose as an adhesive material. It is mainly composed of three structures: guaiacyl (G group), syringyl (S group) and p-hydroxyphenyl (H group). A large amount of lignin-containing wastewater is generated in industries such as fermentation and papermaking, and more than 95% of the wastewater is not effectively utilized. Lignin can be converted into biomass oil through pyrolysis technology. Research on efficient oil production from biomass is of great strategic significance to alleviating the fossil fuel crisis.

[0004] Xinjiang is the province with the largest amount of agricultural mulch film usage in China, and the amount of waste agricultural mulch film generated each year is also very large. According to data from the Xinjiang Agriculture and Rural Affairs Department, the area covered by mulch film in the region is more than 36 million mu, and the total amount of mulch film used exceeds 170,000 tons, which are scrapped after one crop. Waste agricultural film is piled up in the fields or at recycling stations, and there is a great risk of pollution if it is not effectively utilized.

[0005] Based on the high H / C characteristics of LDPE (low-density polyethylene) in agricultural film, the present invention proposes a method for preparing aromatic hydrocarbons through catalytic pyrolysis of lignin and low-density polyethylene. LDPE in agricultural film serves as a hydrogen source in the pyrolysis process of lignin, which can improve the quality of pyrolysis oil. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene. After pyrolysis of lignin, the pyrolysis oil contains a large amount of phenolic substances, which has high oxygen content and low calorific value. During the pyrolysis process, LDPE with a high H / C is added as a hydrogen source in the pyrolysis process of lignin, and mixed with a ZSM-5 molecular sieve catalyst for pyrolysis. The phenolic substances can be converted into aromatic hydrocarbons, thereby improving the quality of the pyrolysis oil.

[0007] In order to achieve the above purpose, the technical solution adopted is:

[0008] A method for preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene comprises: taking lignin and low-density polyethylene as raw materials, carrying out catalytic co-pyrolysis reaction under the action of a catalyst to prepare aromatic hydrocarbons.

[0009] Furthermore, the content of lignin in the raw material is 20-80wt%, and the rest is low-density polyethylene.

[0010] Furthermore, the content of lignin in the raw material is 50wt%.

[0011] Furthermore, the fineness of the corncob enzymatic lignin is 60-80 mesh;

[0012] The catalyst is a ZSM-5 molecular sieve catalyst.

[0013] Furthermore, the mass ratio of the raw material to the catalyst is 3-1:1-3.

[0014] Furthermore, the mass ratio of the raw material to the catalyst is 2:1.

[0015] Furthermore, the pyrolysis reaction is carried out under anaerobic conditions.

[0016] Furthermore, the pyrolysis reaction is carried out under an argon atmosphere.

[0017] Furthermore, the pyrolysis reaction is carried out at 400-600°C.

[0018] Furthermore, the pyrolysis reaction is carried out at 500°C.

[0019] Compared with the prior art, the present invention is beneficial in that:

[0020] 1. The technical solution of the present invention utilizes industrial and agricultural wastes, lignin and LDPE, to co-pyrolyze in a fixed bed to prepare aromatic hydrocarbons, which is a clean process with low cost.

[0021] 2. The technical solution of the present invention innovatively adds ZSM-5 molecular sieve catalyst to significantly increase the aromatic hydrocarbon content in pyrolysis oil.

[0022] 3. The technical solution of the present invention obtains a better pyrolysis condition by optimizing the three conditions of temperature, the mixing ratio of lignin and LDPE and the amount of catalyst, thereby improving the raw material conversion rate and aromatic hydrocarbon selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the TG-DTG diagram of lignin;

[0024] Figure 2 The yield of lignin products after pyrolysis at different temperatures;

[0025] Figure 3 The components of pyrolysis oil of lignin pyrolyzed at different temperatures are shown in the figure;

[0026] Figure 4 It is the product yield diagram of pyrolysis of mixtures of lignin and LDPE with different ratios;

[0027] Figure 5 It is the composition diagram of pyrolysis oil of mixture of lignin and LDPE with different proportions;

[0028] Figure 6 This is the product yield diagram of rapid catalytic co-pyrolysis under different catalyst proportions;

[0029] Figure 7 It is the pyrolysis oil composition diagram of rapid catalytic co-pyrolysis under different catalyst proportions;

[0030] Figure 8 It is a simple schematic diagram of the process and device. DETAILED DESCRIPTION

[0031] In order to further illustrate the method of preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene according to the present invention and achieve the intended purpose of the invention, the following is a detailed description of the method of preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene according to the present invention, its specific implementation method, structure, characteristics and efficacy are described in detail in combination with the preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.

[0032] The following is a further detailed description of a method for preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene according to the present invention in conjunction with specific embodiments:

[0033] The technical solution of the present invention is to use corncob enzymatic lignin and LDPE to rapidly catalyze and co-pyrolyze aromatic hydrocarbons, and optimize the effects of temperature, lignin and LDPE mixing ratio and catalyst dosage on the pyrolysis oil yield and the selectivity of aromatic hydrocarbons in the pyrolysis oil through a fixed bed reactor. The technical solution adopted by the present invention is:

[0034] A method for preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene comprises: using corncob enzymatic lignin and low-density polyethylene as raw materials, and carrying out pyrolysis reaction under the action of a catalyst to prepare aromatic hydrocarbons.

[0035] Preferably, the content of lignin in the raw material is 20-80wt%, and the rest is low-density polyethylene.

[0036] Further preferably, the content of lignin in the raw material is 50wt%.

[0037] Preferably, the fineness of the lignin is 60-80 mesh;

[0038] The catalyst is a ZSM-5 molecular sieve catalyst.

[0039] Preferably, the mass ratio of the raw material to the catalyst is 3-1:1-3.

[0040] Further preferably, the mass ratio of the raw material to the catalyst is 2:1.

[0041] Preferably, the pyrolysis reaction is carried out under anaerobic conditions.

[0042] Further preferably, the pyrolysis reaction is carried out under an argon atmosphere.

[0043] Further preferably, the pyrolysis reaction is carried out at 400-600°C.

[0044] Further preferably, the pyrolysis reaction is carried out at 500°C.

[0045] The present invention utilizes lignin, a waste product of fermentation and papermaking industries, to prepare aromatic hydrocarbons, and adds LDPE, a main component of agricultural film, for co-pyrolysis. On the one hand, the waste agricultural film can be utilized as a resource, and on the other hand, LDPE can be used as a hydrogen source for pyrolysis of lignin, which is beneficial to the production of aromatic hydrocarbons.

[0046] In the present invention, the mixed co-pyrolysis of lignin and LDPE is carried out in a fixed bed reactor, which has the characteristics of low cost and no pollution. The addition of ZSM-5 molecular sieve catalyst can greatly increase the yield of aromatic hydrocarbons.

[0047] 1. Implementation

[0048] The lignin used in the examples of the present invention is corncob enzymatic lignin from Shandong Longli Biotechnology Co., Ltd.; ZSM-5 molecular sieve was purchased from Nankai Catalyst Factory.

[0049] Figure 8 The process and device of fixed bed pyrolysis reaction and the schematic diagram are combined Figure 8 The specific operation steps of the embodiment of the present invention are as follows:

[0050] ① Determine the optimal temperature for fixed bed pyrolysis reaction

[0051] Example 1.

[0052] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight;

[0053] (2) Weigh 1.0 g of lignin and place it in a hanging basket, which is fixed on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 400 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw material is pyrolyzed at the target temperature for 10 min.

[0054] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0055] Example 2.

[0056] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight;

[0057] (2) Weigh 1.0 g of lignin and place it in a hanging basket, which is fixed on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 450°C at a heating rate of 10°C / min, and then the hanging basket is placed in the middle of the reactor. The raw material is pyrolyzed at the target temperature for 10 min.

[0058] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0059] Example 3.

[0060] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight;

[0061] (2) Weigh 1.0 g of lignin and place it in a hanging basket, which is fixed on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw material is pyrolyzed at the target temperature for 10 min.

[0062] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0063] Example 4.

[0064] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight;

[0065] (2) Weigh 1.0 g of lignin and place it in a hanging basket, which is fixed on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 550°C at a heating rate of 10°C / min, and then the hanging basket is placed in the middle of the reactor. The raw material is pyrolyzed at the target temperature for 10 min.

[0066] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0067] Example 5.

[0068] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight;

[0069] (2) Weigh 1.0 g of lignin and place it in a hanging basket, which is fixed on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 600 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw material is pyrolyzed at the target temperature for 10 min.

[0070] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0071] ② Determine the optimal mixing ratio of lignin and LDPE for co-pyrolysis

[0072] Example 6.

[0073] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours.

[0074] (2) Weigh 1.0 g of lignin and LDPE, mix them evenly at a mass ratio of 80:20, place them in a hanging basket, and fix them on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw materials are pyrolyzed at the target temperature for 10 min.

[0075] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0076] Example 7.

[0077] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours.

[0078] (2) Weigh 1.0 g of lignin and LDPE, mix them evenly at a mass ratio of 60:40, place them in a hanging basket, and fix them on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw materials are pyrolyzed at the target temperature for 10 min.

[0079] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0080] Example 8.

[0081] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours.

[0082] (2) Weigh 1.0 g of lignin and LDPE, mix them evenly at a mass ratio of 50:50, place them in a hanging basket, and fix them on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw materials are pyrolyzed at the target temperature for 10 min.

[0083] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0084] Example 9.

[0085] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours.

[0086] (2) Weigh 1.0 g of lignin and LDPE, mix them evenly at a mass ratio of 40:60, place them in a hanging basket, and fix them on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw materials are pyrolyzed at the target temperature for 10 min.

[0087] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0088] Example 10.

[0089] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours.

[0090] (2) Weigh 1.0 g of lignin and LDPE, mix them evenly at a mass ratio of 20:80, place them in a hanging basket, and fix them on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw materials are pyrolyzed at the target temperature for 10 min.

[0091] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0092] Example 11.

[0093] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours.

[0094] (2) Weigh 1.0 g of lignin and LDPE, mix them evenly at a mass ratio of 0:100, place them in a hanging basket, and fix them on the top of the reaction tube. Argon (99.999%) is passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace is raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket is placed in the middle of the reactor. The raw materials are pyrolyzed at the target temperature for 10 min.

[0095] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0096] ③Determine the optimal amount of catalyst

[0097] Example 12.

[0098] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours. Lignin and LDPE are evenly mixed in a mass ratio of 50:50 to obtain a raw material mixture.

[0099] (2) The raw material mixture and the catalyst were mixed at a mass ratio of 3:1, and 1.0 g was weighed and placed in a hanging basket, which was fixed on the top of the reaction tube. Argon (99.999%) was passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace was raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket was placed in the middle of the reactor. The raw material was pyrolyzed at the target temperature for 10 min.

[0100] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0101] Example 13.

[0102] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours. Lignin and LDPE are evenly mixed in a mass ratio of 50:50 to obtain a raw material mixture.

[0103] (2) The raw material mixture and the catalyst were mixed at a mass ratio of 2:1, and 1.0 g was weighed and placed in a hanging basket, which was fixed on the top of the reaction tube. Argon (99.999%) was passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace was raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket was placed in the middle of the reactor. The raw material was pyrolyzed at the target temperature for 10 min.

[0104] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0105] Example 14.

[0106] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours. Lignin and LDPE are evenly mixed in a mass ratio of 50:50 to obtain a raw material mixture.

[0107] (2) The raw material mixture and the catalyst were mixed in a mass ratio of 1:1, and 1.0 g was weighed and placed in a hanging basket, which was fixed on the top of the reaction tube. Argon (99.999%) was passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace was raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket was placed in the middle of the reactor. The raw material was pyrolyzed at the target temperature for 10 min.

[0108] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0109] Example 15.

[0110] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours. Lignin and LDPE are evenly mixed in a mass ratio of 50:50 to obtain a raw material mixture.

[0111] (2) The raw material mixture and the catalyst were mixed in a mass ratio of 1:2, and 1.0 g was weighed and placed in a hanging basket, which was fixed on the top of the reaction tube. Argon (99.999%) was passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace was raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket was placed in the middle of the reactor. The raw material was pyrolyzed at the target temperature for 10 min.

[0112] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0113] Example 16.

[0114] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours. Lignin and LDPE are evenly mixed in a mass ratio of 50:50 to obtain a raw material mixture.

[0115] (2) The raw material mixture and the catalyst were mixed in a mass ratio of 1:3, and 1.0 g was weighed and placed in a hanging basket, which was fixed on the top of the reaction tube. Argon (99.999%) was passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace was raised to 500 °C at a heating rate of 10 °C / min, and then the hanging basket was placed in the middle of the reactor. The raw material was pyrolyzed at the target temperature for 10 min.

[0116] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0117] Example 17.

[0118] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours. Lignin and LDPE are evenly mixed in a mass ratio of 20:80 to obtain a raw material mixture.

[0119] (2) The raw material mixture and the catalyst were mixed in a mass ratio of 2:3, and 1.0 g was weighed and placed in a hanging basket, which was fixed on the top of the reaction tube. Argon (99.999%) was passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace was raised to 400 °C at a heating rate of 10 °C / min, and then the hanging basket was placed in the middle of the reactor. The raw material was pyrolyzed at the target temperature for 10 min.

[0120] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0121] Example 18.

[0122] (1) Take an appropriate amount of lignin, crush it, sieve out 60-80 mesh as raw material, and dry it to constant weight; LDPE is dried for 4 hours. Lignin and LDPE are mixed evenly in a mass ratio of 80:20 to obtain a raw material mixture.

[0123] (2) The raw material mixture and the catalyst were mixed in a mass ratio of 3:2, and 1.0 g was weighed and placed in a hanging basket, which was fixed on the top of the reaction tube. Argon (99.999%) was passed into the reaction tube at a rate of 50 mL / min for 20 min to create an inert atmosphere. The temperature of the pyrolysis furnace was raised to 600 °C at a heating rate of 10 °C / min, and then the hanging basket was placed in the middle of the reactor. The raw material was pyrolyzed at the target temperature for 10 min.

[0124] (3) After the pyrolysis is completed, the hanging basket is raised to the top of the reaction tube, the argon flow rate is adjusted to 25 mL / min, the pyrolysis steam is purged by argon to the pyrolysis oil collector, the gas is cooled by a cold trap to obtain pyrolysis oil, and the non-condensable gas is collected by the gas collector.

[0125] 2. Experiment:

[0126] 1. Thermogravimetric characterization of lignin

[0127] The HP-TGA75 thermogravimeter produced by TA Instruments, USA, was used to conduct qualitative and quantitative analysis of lignin. The operation steps were as follows: 10 mg of the sample to be tested was placed in a small crucible, high-purity nitrogen (N2) was used as the protective gas, and the temperature was increased from 30°C to 1000°C at a heating rate of 10°C / min to obtain the weight loss data. Figure 1 shown.

[0128] Depend on Figure 1 It can be seen that the lignin pyrolysis process is mainly divided into three stages. The first stage is 80-150℃, the second stage is 200-320℃, and the third stage is 320-500℃. The process is relatively long, and the maximum mass loss rate is 2.652min -1 At around 350℃, the first stage mainly removes water and some light volatiles, with a mass loss of about 4.453wt.%; the second stage decomposes and generates many volatiles, with a mass loss of about 12.596wt.%; the third stage mass loss is about 28.337wt.%. After 500℃, the weight loss curve tends to be flat until the end of the pyrolysis reaction. Since no catalyst is added, the final solid residue is composed of coke, and the coke yield is 38.58wt.%.

[0129] 2. Effect of temperature on lignin pyrolysis

[0130] The pyrolysis products and pyrolysis oil components obtained at different temperature ranges in Examples 1-5 were analyzed using an Agilent 8890-5977B gas spectrometer; the chromatographic column model was HP-5MS, the column temperature was maintained at 50°C for 5 min, increased to 210°C at a rate of 5°C / min for 0 min, and increased to 270°C at a rate of 10°C / min for 5 min. The components in the pyrolysis oil were determined using the NIST standard mass spectral library.

[0131] The pyrolysis results are as follows Figure 2 and Figure 3 As shown. Figure 2-3It can be seen that the yield of pyrolysis oil shows a trend of first increasing and then decreasing with the increase of temperature, and the yield of pyrolysis oil at 500°C has a maximum value of 39.11wt.%. Compared with other temperatures, the proportion of oxygen-containing substances in pyrolysis oil at 500°C is relatively small, accounting for 1.21%; phenolic substances account for the largest proportion, accounting for 94.71%. Therefore, the pyrolysis temperature of 500°C in the present invention is conducive to improving the yield of pyrolysis oil and the proportion of phenolic substances in pyrolysis oil, making the subsequent catalytic pyrolysis to produce aromatic hydrocarbons favorable.

[0132] 3. Effect of mixing ratio on co-pyrolysis of lignin and LDPE

[0133] Lignin and LDPE in different mixing ratios were co-pyrolyzed according to the method in Examples 6-11.

[0134] Figure 4 The results of the effects of different mixing ratios on the co-pyrolysis products are shown in Figure 2. Figure 4 It can be seen that with the increase of LDPE ratio in the raw material, the yield of pyrolysis oil increases significantly. LDPE can serve as a hydrogen donor for lignin and increase the yield of pyrolysis oil.

[0135] Figure 5 The results of the effects of different mixing ratios on the components of pyrolysis oil are shown in Figure 2. Figure 5 It can be seen that with the addition of LDPE, hydrocarbon substances show a trend of first increasing and then decreasing, while oxygen-containing organic substances such as alcohols, ketones and esters first decrease and then increase. When the mixed mass ratio is 50:50, the content of alcohols, ketones and esters in the pyrolysis oil reaches a minimum value of 11.26%, and the content of hydrocarbon substances reaches a maximum value of 83.74%. Under this ratio, the LDPE has a significant hydrogenation and deoxygenation ability, which makes the subsequent catalytic pyrolysis to produce aromatic hydrocarbons favorable. In the present invention, the mixing ratio of lignin to LDPE is 50:50, which is a better reaction condition.

[0136] 4. Effect of catalyst dosage on rapid catalytic co-pyrolysis of lignin and LDPE

[0137] According to the method in Examples 12-16, the mixture of lignin and LDPE with different catalyst dosages was rapidly catalytically co-pyrolyzed. The results are as follows: Figure 6 and Figure 7 shown.

[0138] Depend on Figure 6-7 It can be seen that the addition of the catalyst significantly increases the amount of aromatic hydrocarbons, and its yield increases first and then decreases with the increase in the amount of catalyst used. When the mass ratio of the raw material to the catalyst is 2:1, the aromatic hydrocarbon content reaches 90.68%, and the pyrolysis oil yield is also relatively high, with a yield of 50.95%, which is better for the production of aromatic hydrocarbons. The mass ratio of the raw material mixture to the catalyst in the present invention is 2:1, which is a better reaction condition.

[0139] The above is only a preferred embodiment of the embodiment of the present invention, and does not impose any form of limitation on the embodiment of the present invention. Any simple modification, equivalent changes and modifications made to the above embodiment based on the technical essence of the embodiment of the present invention are still within the scope of the technical solution of the embodiment of the present invention.

Claims

1. A method for preparing aromatic hydrocarbons by catalytic pyrolysis of lignin and low-density polyethylene, characterized in that: The method is as follows: using a fixed bed pyrolysis catalytic device, taking lignin and low-density polyethylene as raw materials, and carrying out pyrolysis reaction under the action of a catalyst to prepare aromatic hydrocarbons; The content of lignin in the raw material is 20-60wt%, and the rest is low-density polyethylene; The catalyst is a ZSM-5 molecular sieve catalyst; The mass ratio of the raw material to the catalyst is 3-1:1-3.

2. The method according to claim 1, characterized in that The content of lignin in the raw material is 50wt%.

3. The method according to claim 1, characterized in that The fineness of the lignin is 60-80 meshes.

4. The method according to claim 1, characterized in that: The mass ratio of the raw material to the catalyst is 2:

1.

5. The method according to claim 1, characterized in that The pyrolysis reaction is carried out under anaerobic conditions.

6. The method according to claim 5, characterized in that The pyrolysis reaction is carried out under an argon atmosphere.

7. The method according to claim 1, characterized in that The pyrolysis reaction is carried out at 400-600°C.

8. The method according to claim 7, characterized in that The pyrolysis reaction is carried out at 500°C.

Citation Information

Patent Citations

  • Method for synthesizing heteroatomic ZSM-5 molecular sieve and application thereof

    CN103950951A

  • Method for preparing arene-rich fuel oil by co-pyrolysis of lignin and low-density polyethylene