A method for batch processing of carbon-based electrodes for flow batteries

By pretreatment, low-temperature oxidation, high-temperature activation and graphitization of carbon fibers, the conductivity and catalytic performance of carbon fibers are improved, the problem of insufficient performance of carbon-based electrodes in the prior art is solved, and the flow battery is realized High-efficiency energy conversion and large-scale production.

CN117276560BActive Publication Date: 2024-11-29ZHANGJIAGANG DETAI ENERGY STORAGE EQUIP CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310078839.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-08
Publication Date
2024-11-29
Estimated Expiration
2043-02-08

AI Technical Summary

Technical Problem

At this stage, there is no commercial electrode material for redox flow batteries. The carbon-based electrode performance is insufficient, resulting in low power density and high cost of stacks, making it difficult to achieve mass production and application.

Method used

A method of batch processing of carbon-based electrodes for flow batteries, including pretreatment of carbon felts, low-temperature oxidation, high-temperature activation, graphitization and plasma source etching, etc., to improve the conductivity and catalytic performance of carbon fibers, and prepare A modified carbon-based electrode with high conductivity and catalytic performance is produced.

Benefits of technology

The cycle life and energy conversion efficiency of redox flow batteries are significantly improved, the preparation cost of electrode materials is reduced, and the commercial large-scale production of electrodes is realized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117276560B_ABST
    Figure CN117276560B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for batch processing of carbon-based electrodes for flow batteries, comprising: pre-treating carbon felt; performing low-temperature oxidation in an atmosphere with an oxygen volume content of 5%-30%; adjusting the oxygen content to be lower than 1200ppm in an inert atmosphere, heating to 1000-1500℃, and performing high-temperature activation; adjusting the oxygen content to be lower than 150ppm, heating to 2000-2250℃, and performing graphitization; in a temperature range of 2000-2200℃, introducing an inert gas plasma source to etch the surface of the carbon fiber; heating to 2250℃-2300℃, keeping warm for 1-5min, and naturally cooling to room temperature. The modified carbon-based electrode prepared by the present invention has the advantages of high conductivity, good catalytic performance, and good stability, and improves the cycle life, power density, and energy conversion efficiency of the redox flow battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of liquid flow batteries and relates to a method for batch processing of carbon-based electrodes for liquid flow batteries. Background Art

[0002] Developing sustainable and renewable energy sources such as wind and solar energy is an effective way to solve the energy crisis. However, the intermittent and unstable nature of renewable energy in the process of power output must be effectively balanced by the capabilities of advanced energy storage systems to ensure continuous or on-demand safe and reliable power supply. The power of redox flow batteries is determined by the size and number of units, and the energy density is controlled by the concentration of active substances, the number of electrons transferred by the redox reaction, and the voltage. Due to its advantages such as separation of energy and power, long cycle life, low cost, less maintenance time, high safety, and environmental protection, redox flow batteries are one of the first choices for large-scale energy storage technology. In order to encourage the market to adopt redox flow battery technology, researchers are working hard to maintain high energy efficiency while improving its power density performance. The cost of the power module is mainly determined by the performance of the electrode material, especially the conductivity and catalytic performance. At present, there is no commercial electrode material for redox flow batteries, and the electrodes mainly used are carbon-based materials used for insulation and heat insulation. The performance of such carbon-based materials is not enough, which directly leads to low power density of the battery stack and high cost of power modules, which has become a bottleneck that needs to be broken through. As the output value of redox flow batteries increases rapidly, the demand for electrode materials is bound to increase gradually. The most widely used electrode preparation technology is to modify carbon-based materials (carbon felt, graphite felt, carbon cloth, etc.) to obtain electrodes with high conductivity and electrochemical activity. However, the current electrode preparation technology is immature, the preparation cost is high, and it is difficult to achieve mass production and application, resulting in the lack of commercial redox flow battery electrodes at this stage.

[0003] Up to now, there is still no suitable method to solve the above key problems. It is urgent to develop a method for industrial batch processing of carbon-based electrodes to improve their conductivity and catalytic activity, which will make an important contribution to the large-scale development of redox flow batteries. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a method for batch processing of carbon-based electrodes for liquid flow batteries. The modified carbon-based electrodes prepared have the advantages of high electrical conductivity, good catalytic performance and good stability, which improves the cycle life, power density and energy conversion efficiency of the redox liquid flow battery, and solves the problems existing in the prior art.

[0005] The technical solution adopted by the present invention is a method for batch processing of carbon-based electrodes for liquid flow batteries, comprising the following steps:

[0006] S1, pre-treating the carbon felt;

[0007] S2, in an atmosphere with an oxygen volume content of 5%-30%, heating to 100-400°C, with a heating rate of 4-8°C / min, and keeping warm for 20min-120min, for low-temperature oxidation;

[0008] S3, in an inert atmosphere, adjust the oxygen content to less than 1200ppm (oxygen volume concentration), raise the temperature to 1000-1500℃, at a heating rate of 4-6℃ / min, and keep the temperature for 30min-300min for high temperature activation;

[0009] S4, adjusting the oxygen content to less than 150ppm, heating to 2000-2250°C, heating rate of 3-5°C / min, keeping the temperature for 1min-5min, and graphitizing;

[0010] S5, in a temperature range of 2000-2200°C, an inert gas plasma source is introduced to etch the surface of the carbon fiber, the volume ratio of the plasma source to the ambient gas is 0.02-0.2, the plasma power is 100-1200W, and the etching time is 30-360s;

[0011] S6, heat up to 2250℃-2300℃, keep warm for 1-5min, and naturally cool to room temperature.

[0012] Furthermore, the degree of graphitization of the carbon felt in S1 is less than 30%. Before introducing the inert gas plasma source in S5, a carbon-containing gas plasma source is first introduced to deposit on the surface of the carbon fiber. The volume ratio of the carbon-containing gas plasma source to the ambient gas is 0.3-0.5, the plasma power is 1000-1200w, and the deposition time is 40-60min; wherein, the etching time of the inert gas plasma source is 30-120s.

[0013] Furthermore, in the S1, the graphitization degree of the carbon felt is 30-60%. Before S2, the pretreated carbon felt is etched in an alkaline solution, cleaned to neutrality, and dried; before introducing the inert gas plasma source in S5, a carbon-containing gas plasma source is first introduced to deposit on the surface of the carbon fiber, the volume ratio of the carbon-containing gas plasma source to the ambient gas is 0.3-0.5, the plasma power is 1000-1200w, and the deposition time is 40-60min; wherein, the etching time of the inert gas plasma source is 120-240s.

[0014] Furthermore, in the S1, the graphitization degree of the carbon felt is above 60%. Before S2, the pretreated carbon felt is immersed in an acid solution for oxidation, cleaned to neutrality, and dried; wherein the etching time of the inert gas plasma source is 240-360s.

[0015] Furthermore, the S1 is specifically:

[0016] S11, immersing the carbon felt in excess deionized water for 30-60 minutes and taking it out after it is fully wetted;

[0017] S12, cutting the impregnated carbon felt into electrode sizes, cleaning it with an ethanol solution for 10-15 times, and then soaking it in ultrasound for 15-60 minutes to clean impurities on the surface of the carbon fiber;

[0018] S13, placing the carbon felt after ultrasonic treatment in a blast drying oven, adjusting the temperature to 40-80°C, and drying time to 4-12h.

[0019] Furthermore, in S3, after the temperature reaches 1200°C, the oxygen content needs to be lower than 540 ppm.

[0020] Furthermore, in S4, after the temperature reaches 2200°C, the oxygen content needs to be lower than 60 ppm.

[0021] Furthermore, the alkaline solution is potassium hydroxide or sodium hydroxide solution, the concentration is 2-5 mol / L, and the treatment time is 24-72h.

[0022] Furthermore, the acid solution is sulfuric acid, hydrochloric acid or nitric acid solution, with a concentration of 0.5-3 mol / L and a treatment time of 6-48 hours.

[0023] Furthermore, the carbon-containing gas plasma source is an olefin gas, and the mass content of other elements except C, H, and O is less than 5%; the inert gas plasma source is helium, neon, argon, krypton or xenon.

[0024] The beneficial effects of the present invention are:

[0025] (1) In the specific embodiments of the present invention, for carbon fibers with any degree of graphitization, carbon felt cleaning can be used to wash away impurities, expand the channels between carbon fibers, and increase the contact area between carbon fibers and the electrolyte; for carbon fibers with a degree of graphitization higher than 60%, carbon felt soaking and oxidation can increase the oxygen-containing functional groups on the surface of the carbon fibers and improve the hydrophilicity; for carbon fibers with a degree of graphitization of 30-60%, carbon felt soaking and etching can produce a large number of micropores and mesopores on the surface of the carbon fibers, providing more active sites for redox reactions; these surface treatment methods are conducive to the subsequent regulation of the internal structure of the carbon felt.

[0026] (2) In the specific embodiments of the present invention, for carbon fibers with any degree of graphitization, heat treatment of the carbon felt can transform the amorphous carbon inside the carbon fibers into a graphite structure, increase the order of the carbon structure, and thus improve the conductivity of the carbon fibers; for carbon fibers with a degree of graphitization higher than 60%, inert gas plasma source etching can etch away the wrinkles at the edge of the graphite structure and unstable carbon atoms, effectively increasing the stability of the carbon fiber performance; for carbon fibers with a degree of graphitization of 30-60%, first using an inert gas plasma source etching and then combining it with a carbon-containing gas plasma source deposition can remove unstable carbon atoms, provide more carbon source, and increase the degree of graphitization of the carbon fibers; for carbon fibers with a degree of graphitization of 0-30%, first using a carbon-containing gas plasma source deposition and then combining it with an inert gas plasma source etching can provide more carbon source, thereby increasing the degree of graphitization of the carbon fibers.

[0027] (3) The specific embodiments of the present invention perform surface treatment and structural regulation on the internal carbon fibers of carbon-based materials with different degrees of graphitization. The synergistic effect of the two can significantly enhance the electrochemical properties of carbon fibers, thereby improving their overall application performance in redox flow batteries. The treatment method has low raw material / equipment costs, a simple and convenient process flow, and is easy to scale up for mass production. The samples obtained have the advantages of high electrical conductivity, large specific surface area, good catalytic performance, and good stability, which is conducive to the large-scale production of commercial electrodes for flow batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 It is a process flow chart for batch processing of carbon fibers with different graphitization degrees in an embodiment of the present invention.

[0030] Figure 2 The cyclic voltammetry curves of the batch-processed samples and the original samples of carbon fibers with a graphitization degree of 0-30% in the embodiments of the present invention in an acidic vanadium flow battery system.

[0031] Figure 3 The cyclic voltammetry curves of the batch-processed samples and the original samples of carbon fibers with a graphitization degree of 30-60% in the embodiments of the present invention in an acidic vanadium liquid flow battery system.

[0032] Figure 4The cyclic voltammetry curves of the batch-processed samples and the original samples of carbon fibers with a graphitization degree of more than 60% in the embodiments of the present invention in an acidic vanadium liquid flow battery system.

[0033] Figure 5 This is a comparison chart of the energy efficiency of the batch-processed samples and the original samples of carbon fibers with a graphitization degree of 0-30% in the embodiment of the present invention in an acidic vanadium flow battery system.

[0034] Figure 6 This is a comparison chart of the energy efficiency of the batch-processed samples and the original samples of carbon fibers with a graphitization degree of 30-60% in the embodiment of the present invention in an acidic vanadium flow battery system.

[0035] Figure 7 This is a comparison chart of the energy efficiency of the batch-processed samples and the original samples of carbon fibers with a graphitization degree of more than 60% in the embodiments of the present invention in an acidic vanadium flow battery system.

[0036] Figure 8 It is the XRD spectra of the samples after batch processing and the original samples of carbon fibers with different graphitization degrees in the embodiments of the present invention. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] The design concept of the embodiment of the present invention is: Figure 1 As shown, low-cost carbon-based electrodes are used as raw materials, and the carbon fibers are surface treated and structurally optimized. Through the synergistic effect of the two, a carbon-based electrode for liquid flow batteries with high electrical conductivity, good catalytic performance, large specific surface area and excellent stability is obtained.

[0039] Embodiment 1,

[0040] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0041] S1, immersing the carbon felt with a graphitization degree of less than 30% in excess deionized water for 60 minutes and taking it out after it is fully wetted;

[0042] The impregnated carbon felt was cut into electrode sizes, cleaned with ethanol solution for 15 times, and then immersed in ultrasound for 60 minutes to clean impurities on the surface of the carbon fiber for surface treatment of the carbon felt;

[0043] The carbon felt after ultrasonic treatment was placed in a blast drying oven, the temperature was adjusted to 80°C, and the drying time was 12h;

[0044] S2, placing the sample in the heating chamber of the graphite furnace, closing the valve, adjusting the oxygen volume content to 30% through the high vacuum pump valve, adjusting the graphite furnace heating rate to 4°C / min, heating to 100°C, and keeping the temperature for 120 minutes for low temperature oxidation;

[0045] S3, after the insulation is completed, inert gas (argon) is introduced, the graphite furnace heating rate is adjusted to 4°C / min, the oxygen content is adjusted through the high vacuum pump valve to ensure that the oxygen content is less than 1200ppm (oxygen volume concentration) at 400°C and less than 540ppm at 1200°C, the temperature is raised to 1500°C, and the temperature is kept for 250 minutes for high-temperature activation; the oxygen content is adjusted to prevent the carbon felt from being burned;

[0046] S4, increase the volume flow rate of the inert gas, the volume content of argon is above 99.985%, the oxygen content is reduced to 150ppm, the heating rate of the graphite furnace is adjusted to 3℃ / min, the oxygen content is adjusted by the high vacuum pump valve to ensure that the oxygen content is less than 150ppm at 2000℃ and less than 60ppm at 2200℃, keep warm for 1min, and carry out graphitization;

[0047] S5, at 2200℃, first introduce a carbon-containing gas plasma source (methane) to deposit on the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.3, the plasma power is 1200w, and the deposition time is 60min. Then introduce an inert gas (argon) plasma source to etch the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.02, the plasma power is 100W, and the etching time is 60s;

[0048] S6, heating to 2250°C, keeping the temperature for 5 minutes to ensure that graphitization is fully completed, and naturally cooling to room temperature after the end of the heat preservation to obtain sample 1.

[0049] The carbon-containing gas plasma source is an olefin gas with a purity requirement of more than 95%, including but not limited to methane, ethane, propane, butane, neopentane, ethylene, propylene, butene, acetylene, propyne, butyne, and natural gas of relatively high purity. To ensure sufficient cracking of carbon, high-purity methane is the best choice. The inert gas plasma source is helium, neon, argon, krypton or xenon.

[0050] like Figure 2 and Figure 5As shown, the peak current of sample 1-1 in the acidic vanadium liquid flow battery system measured at room temperature is 300mA and 278mA, while the original carbon felt is only 169mA and 158mA. The potential difference of sample 1-1 is 0.53V, and that of the original carbon felt is 0.83V. The energy efficiency of sample 1-1 is 85.10%, and that of the original carbon felt is 56.44%, indicating that the conductivity and catalytic activity of sample 1-1 are higher than those of the original carbon felt, and it meets the application requirements of liquid flow batteries.

[0051] Embodiment 2,

[0052] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0053] S1, immersing the carbon felt with a graphitization degree of less than 30% in excess deionized water for 30 minutes and taking it out after it is fully wetted;

[0054] The impregnated carbon felt was cut into electrode sizes, cleaned with ethanol solution for 10 times, and then immersed in ultrasound for 15 minutes to clean impurities on the surface of the carbon fiber for surface treatment of the carbon felt;

[0055] The carbon felt after ultrasonic treatment was placed in a blast drying oven, the temperature was adjusted to 40°C, and the drying time was 10 hours;

[0056] S2, placing the sample in the heating chamber of the graphite furnace, closing the valve, adjusting the oxygen volume content to 5% through the high vacuum pump valve, adjusting the graphite furnace heating rate to 8°C / min, heating to 400°C, keeping the temperature for 20 minutes, and performing low-temperature oxidation;

[0057] S3, after the insulation is completed, inert gas (nitrogen) is introduced, the graphite furnace heating rate is adjusted to 6°C / min, the oxygen content is adjusted through the high vacuum pump valve to ensure that the oxygen content is less than 1200ppm at 400°C and less than 540ppm at 1200°C, the temperature is raised to 1300°C, and the temperature is kept for 300min for high temperature activation;

[0058] S4, increase the volume flow rate of the inert gas, the volume content of nitrogen is above 99.985%, the oxygen content is reduced to 150ppm, the heating rate of the graphite furnace is adjusted to 5℃ / min, the oxygen content is adjusted by the high vacuum pump valve to ensure that the oxygen content is less than 150ppm at 2000℃, keep warm for 5min, and carry out graphitization;

[0059] S5, at 2000℃, first introduce a carbon-containing gas plasma source (ethylene) to deposit on the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.5, the plasma power is 1000W, and the deposition time is 50min. Then introduce an inert gas (helium) plasma source to etch the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.2, the plasma power is 1200W, and the etching time is 30s;

[0060] S6, heating to 2300°C, keeping the temperature for 1 min to ensure that graphitization is fully completed, and naturally cooling to room temperature after the end of the heat preservation to obtain sample 1-2.

[0061] At room temperature, the peak current of sample 1-2 in the acidic vanadium liquid flow battery system was measured to be 234mA and 213mA, while the original carbon felt had only 169mA and 158mA. The potential difference of sample 1-2 was 0.75V, while that of the original carbon felt was 0.83V, indicating that the conductivity and catalytic activity of sample 1-2 are higher than those of the original carbon felt, and are suitable for the application requirements of liquid flow batteries.

[0062] Embodiment 3,

[0063] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0064] S1, immersing the carbon felt with a graphitization degree of less than 30% in excess deionized water for 50 minutes and taking it out after it is fully wetted;

[0065] The impregnated carbon felt was cut into electrode sizes, cleaned with ethanol solution for 12 times, and then immersed in ultrasound for 30 minutes to clean impurities on the surface of the carbon fiber for surface treatment of the carbon felt;

[0066] The carbon felt after ultrasonic treatment was placed in a blast drying oven, the temperature was adjusted to 70°C, and the drying time was 4h;

[0067] S2, placing the sample in the heating chamber of the graphite furnace, closing the valve, adjusting the oxygen volume content to 20% through the high vacuum pump valve, adjusting the graphite furnace heating rate to 5°C / min, heating to 300°C, and keeping the temperature for 600 minutes for low temperature oxidation;

[0068] S3, after the insulation is completed, inert gas (helium) is introduced, the graphite furnace heating rate is adjusted to 5°C / min, the oxygen content is adjusted through the high vacuum pump valve to ensure that the oxygen content is less than 1200ppm at 400°C and less than 540ppm at 1000°C, the temperature is raised to 1000°C, and the temperature is maintained for 30 minutes for high-temperature activation;

[0069] S4, increase the volume flow rate of the inert gas, the volume content of helium is above 99.985%, the oxygen content is reduced to 150ppm, the heating rate of the graphite furnace is adjusted to 4℃ / min, the oxygen content is adjusted by the high vacuum pump valve to ensure that the oxygen content is less than 150ppm at 2250℃, keep warm for 3min, and carry out graphitization;

[0070] S5, at 2100℃, first introduce a carbon-containing gas (propyne) plasma source to deposit on the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.4, the plasma power is 1100w, and the deposition time is 40min. Then introduce an inert gas (helium) plasma source to etch the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.1, the plasma power is 500W, and the etching time is 120s;

[0071] S6, heating to 2280°C, keeping the temperature for 3 minutes to ensure that graphitization is fully completed, and then naturally cooling to room temperature after the end of the heat preservation, to obtain sample 1-3.

[0072] The volume content of oxygen in low-temperature oxidation ranges from 5% to 30%. When the oxygen content is too high, the temperature is too high (above 400°C) and the carbon felt will burn. Below 100°C, the surface carbon fibers cannot be oxidized, and high temperatures are required to force the carbon atoms to combine with oxygen in the air to form stable chemical bonds and form oxygen-containing functional groups on the surface.

[0073] The temperature range of graphitization is 2000-2250℃, which makes the carbon fiber fully graphitized. Too high a temperature will increase the cost, and the carbon felt has low toughness at high temperature after graphitization, and is easily broken in the industrial preparation process. Below 2000℃, it is impossible to fully ensure that all structures have been graphitized.

[0074] At room temperature, the peak currents of samples 1-3 in the acidic vanadium liquid flow battery system were measured to be 268mA and 246mA, while the original carbon felt had only 169mA and 158mA. The potential difference of samples 1-3 was 0.68V, while that of the original carbon felt was 0.83V, indicating that the conductivity and catalytic activity of samples 1-3 are higher than those of the original carbon felt, and are suitable for the application requirements of liquid flow batteries.

[0075] Embodiment 4,

[0076] A method for batch processing of carbon-based electrodes for liquid flow batteries, except that the holding time in S3 is 200 minutes, the remaining steps are the same as those in Example 1, and samples 1-4 are prepared.

[0077] The peak currents of samples 1-4 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature were 295 mA and 272 mA, while the peak currents of the original carbon felt were only 169 mA and 158 mA. The potential difference of samples 1-4 was 0.55 V, while that of the original carbon felt was 0.83 V, indicating that the conductivity and catalytic activity of samples 1-4 were higher than those of the original carbon felt, and thus met the application requirements of liquid flow batteries.

[0078] Embodiment 5,

[0079] A method for batch processing of carbon-based electrodes for liquid flow batteries, except that the holding time in S3 is 300 minutes, the remaining steps are the same as those in Example 1, and samples 1-5 are prepared.

[0080] The peak currents of samples 1-5 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature were 294 mA and 271 mA, while the peak currents of the original carbon felt were only 169 mA and 158 mA. The potential difference of samples 1-5 was 0.54 V, while that of the original carbon felt was 0.83 V, indicating that the conductivity and catalytic activity of samples 1-5 were higher than those of the original carbon felt, and thus met the application requirements of liquid flow batteries.

[0081] 0-30% has a low degree of graphitization. Direct acid and alkali treatment will damage the strength of the carbon fiber, so it is directly cleaned. Carbon fibers with a graphitization degree of 0-30% have less initial graphite structure and more disordered structure. During graphitization, there may be insufficient carbon atom content, resulting in inadequate graphitization. It is necessary to first deposit carbon-containing gas to increase additional carbon sources; then use an inert gas plasma source to etch away the carbon defects generated at the edge of the graphite structure (direct inert gas etching may completely destroy the initial disordered structure, resulting in instability between graphite layers, and it is difficult to form a complete interlayer carbon structure in the subsequent graphitization interval).

[0082] The degree of graphitization is low, and it is necessary to keep warm for a long time at a low temperature in a high oxygen environment, so as to fully achieve the purpose of oxidation without burning the carbon material and causing irreversible damage to the strength of the carbon fiber.

[0083] Embodiment 6,

[0084] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0085] S1, immersing the carbon felt with a graphitization degree of 30-60% in excess deionized water for 60 minutes and taking it out after it is fully wetted;

[0086] The impregnated carbon felt was cut into electrode sizes, cleaned with ethanol solution for 15 times, and then immersed in ultrasound for 60 minutes to clean impurities on the carbon fiber surface;

[0087] The cleaned carbon felt was immersed in a 3 mol / L potassium hydroxide solution for 24 h, then taken out and washed with deionized water until neutral, placed in a blast drying oven, adjusted to 80°C, and dried for 12 h for surface treatment of the carbon felt;

[0088] S2, placing the sample in the heating chamber of the graphite furnace, closing the valve, adjusting the oxygen volume content to 15% through the high vacuum pump valve, adjusting the graphite furnace heating rate to 5°C / min, heating to 200°C, and keeping the temperature for 60 minutes for low temperature oxidation;

[0089] S3, after the insulation is completed, inert gas (neon) is introduced, the graphite furnace heating rate is adjusted to 6°C / min, the oxygen content is adjusted through the high vacuum pump valve to ensure that the oxygen content is less than 1200ppm at 400°C and less than 540ppm at 1200°C, the temperature is raised to 1500°C, and the temperature is kept for 180min for high temperature activation;

[0090] S4, increasing the volume flow rate of the inert gas, the volume content of neon is above 99.985%, the oxygen content is reduced to 150ppm, the heating rate of the graphite furnace is adjusted to 5℃ / min, and the oxygen content is adjusted by the high vacuum pump valve to ensure that the oxygen content is less than 150ppm at 2000℃ and less than 60ppm at 2200℃, and graphitization is carried out;

[0091] S5, at 2200℃, first introduce a carbon-containing gas (propane) plasma source to deposit on the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.4, the plasma power is 1100W, and the deposition time is 50min. Then introduce an inert gas plasma source to etch the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.02, the plasma power is 150W, and the etching time is 180s;

[0092] S6, heating to 2250°C, keeping the temperature for 3 minutes to ensure that graphitization is fully completed, and naturally cooling to room temperature after the end of the heat preservation to obtain sample 2-1.

[0093] like Figure 3 and Figure 6 As shown, the peak current of sample 2-1 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 305mA and 282mA, while the original carbon felt has only 191mA and 170mA. The potential difference of sample 2-1 is 0.52V, while that of the original carbon felt is 0.77V. The energy efficiency of sample 2-1 is 85.22%, while that of the original carbon felt is 69.65%, indicating that the conductivity and catalytic activity of sample 2-1 are higher than those of the original carbon felt, and thus meet the application requirements of liquid flow batteries.

[0094] Embodiment 7,

[0095] A method for batch processing of carbon-based electrodes for liquid flow batteries, except that the alkaline washing solution in S1 is 5 mol / L sodium hydroxide and the soaking time is 36 hours; the holding time of high temperature activation in S3 is 120 minutes; the inert gas plasma source etching time in S5 is 120 seconds; the remaining steps are the same as in Example 6, and sample 2-2 is obtained.

[0096] At room temperature, the peak current of sample 2-2 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 303 mA and 280 mA, while the peak current of the original carbon felt was only 191 mA and 170 mA. The potential difference of sample 2-2 was 0.53 V, while that of the original carbon felt was 0.77 V, indicating that the conductivity and catalytic activity of sample 2-2 were higher than those of the original carbon felt, and thus met the application requirements of liquid flow batteries.

[0097] Embodiment 8,

[0098] A method for batch processing of carbon-based electrodes for liquid flow batteries, except that the alkaline washing solution in S1 is 2 mol / L sodium hydroxide and the soaking time is 72 hours; the holding time of high temperature activation in S3 is 240 minutes; the inert gas plasma source etching time in S5 is 240 seconds; the remaining steps are the same as in Example 6, and sample 2-3 is obtained.

[0099] At room temperature, the peak current of sample 2-3 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 300mA and 277mA, while the original carbon felt had only 191mA and 170mA. The potential difference of sample 2-3 was 0.55V, while that of the original carbon felt was 0.77V, indicating that the conductivity and catalytic activity of sample 2-3 were higher than those of the original carbon felt, and thus met the application requirements of liquid flow batteries.

[0100] Inert gas etches carbon defects at the edge of the graphite structure. The etching time of the inert gas plasma source is 120-240s. If the etching time is too long, it will damage the graphite structure itself, resulting in more carbon atoms required for subsequent carbon deposition, which increases the cost. Therefore, it is crucial to adjust the etching time parameters for carbon fibers with different degrees of graphitization.

[0101] The alkaline solution is potassium hydroxide or sodium hydroxide solution, which etches unstable carbon atoms to create micropores and mesopores on the surface of carbon fiber and increase the specific surface area. The concentration of the alkaline solution is 2-5 mol / L, and the treatment time is 24-72h. If the concentration is too high or the treatment time is too long, it will cause irreversible damage to the carbon structure. For carbon fibers with different degrees of graphitization, it is crucial to use alkaline solutions of different types and concentrations to adjust the balance between the two.

[0102] Alkali treatment is used to produce micropores and mesopores on the surface of carbon fiber with a graphitization degree of 30-60%, and at the same time, unstable carbon defects are etched away, which provides favorable conditions for subsequent etching of deposited carbon.

[0103] The initial graphite structure of carbon fibers with a graphitization degree of 30-60% is moderate, indicating that the proportions of graphite structure and disordered carbon structure in the carbon fibers are close. Therefore, an inert gas plasma source can be used to etch away defects at the edge of the graphite structure, and then carbon-containing gas deposition can be used to provide additional carbon source to increase the degree of graphitization.

[0104] Embodiment 9,

[0105] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0106] S1, immersing the carbon felt with a graphitization degree of more than 60% in excess deionized water for 60 minutes and taking it out after it is fully wetted;

[0107] The impregnated carbon felt was cut into electrode sizes, cleaned with ethanol solution for 15 times, and then immersed in ultrasound for 60 minutes to clean impurities on the carbon fiber surface;

[0108] The cleaned carbon felt was immersed in a 2 mol / L sulfuric acid solution for 6 h, then taken out and washed with deionized water until neutral, placed in a blast drying oven, adjusted to 80°C, and dried for 12 h for surface treatment of the carbon felt;

[0109] S2, placing the sample in the heating chamber of the graphite furnace, closing the valve, adjusting the oxygen volume content to 5% through the high vacuum pump valve, adjusting the graphite furnace heating rate to 8°C / min, heating to 300°C, keeping the temperature for 20 minutes, and performing low-temperature oxidation;

[0110] S3, after the insulation is completed, inert gas (argon) is introduced, the graphite furnace heating rate is adjusted to 6°C / min, the oxygen content is adjusted through the high vacuum pump valve to ensure that the oxygen content is less than 1200ppm at 400°C and less than 540ppm at 1200°C, the temperature is raised to 1500°C, and the temperature is kept for 90 minutes for high temperature activation;

[0111] S4, increase the volume flow rate of the ambient gas, the volume content of argon is above 99.985%, the oxygen content is reduced to 150ppm, the heating rate of the graphite furnace is adjusted to 5℃ / min, and the oxygen content is adjusted by the high vacuum pump valve to ensure that the oxygen content is less than 150ppm at 2000℃ and less than 60ppm at 2200℃, and graphitization is carried out;

[0112] S5, at 2200°C, an inert gas plasma source is introduced to etch the carbon fiber surface, the volume ratio of the plasma source to the ambient gas is 0.2, the plasma power is 200 W, and the etching time is 300 s;

[0113] S6, heating to 2250°C, keeping the temperature for 5 minutes to ensure that graphitization is fully completed, and naturally cooling to room temperature after the end of the heat preservation to obtain sample 3-1.

[0114] like Figure 4 and Figure 7 As shown, the peak current of sample 3-1 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 294mA and 271mA, while the original carbon felt has only 212mA and 188mA. The potential difference of sample 3-1 is 0.52V, while that of the original carbon felt is 0.68V. The energy efficiency of sample 3-1 is 86.05%, while that of the original carbon felt is 72.86%, indicating that the conductivity and catalytic activity of sample 3-1 are higher than those of the original carbon felt, and it meets the application requirements of liquid flow batteries.

[0115] Embodiment 11,

[0116] A method for batch processing of carbon-based electrodes for liquid flow batteries, except that the pickling solution in S1 is 0.5 mol / L hydrochloric acid and the immersion time is 48 hours; the temperature of low-temperature oxidation in S2 is 200°C; the etching time of inert gas plasma source in S5 is 240 seconds; the remaining steps are the same as those in Example 9, and sample 3-2 is obtained.

[0117] The peak current of sample 3-2 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 292mA and 269mA, while the original carbon felt has only 212mA and 188mA. The potential difference of sample 3-2 is 0.53V, while that of the original carbon felt is 0.68V, indicating that the conductivity and catalytic activity of sample 3-2 are higher than those of the original carbon felt, and it meets the application requirements of liquid flow batteries.

[0118] Embodiment 12,

[0119] A method for batch processing of carbon-based electrodes for liquid flow batteries, except that the pickling solution in S1 is 3 mol / L nitric acid and the soaking time is 15 hours; the temperature of low-temperature oxidation in S2 is 400°C; the inert gas plasma source etching time in S5 is 360 seconds; the remaining steps are the same as in Example 9, and sample 3-3 is obtained.

[0120] At room temperature, the peak current of sample 3-3 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 291mA and 268mA, while the original carbon felt had only 212mA and 188mA. The potential difference of sample 3-3 was 0.54V, while that of the original carbon felt was 0.68V, indicating that the conductivity and catalytic activity of sample 3-3 were higher than those of the original carbon felt, and thus met the application requirements of liquid flow batteries.

[0121] Embodiment 13,

[0122] A method for batch processing of carbon-based electrodes for liquid flow batteries, except that the holding time for high-temperature activation in S3 is 30 minutes, the remaining steps are the same as those in Example 9, and sample 3-4 is prepared.

[0123] At room temperature, the peak current of sample 3-4 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 291mA and 270mA, while the original carbon felt had only 212mA and 188mA. The potential difference of sample 3-4 was 0.54V, while that of the original carbon felt was 0.68V, indicating that the conductivity and catalytic activity of sample 3-4 were higher than those of the original carbon felt, and thus met the application requirements of liquid flow batteries.

[0124] Embodiment 14,

[0125] A method for batch processing of carbon-based electrodes for liquid flow batteries, except that the holding time for high-temperature activation in S3 is 150 minutes, the remaining steps are the same as those in Example 9, and samples 3-5 are prepared.

[0126] At room temperature, the peak current of sample 3-5 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 288mA and 265mA, while the original carbon felt had only 212mA and 188mA. The potential difference of sample 3-5 was 0.52V, while that of the original carbon felt was 0.68V, indicating that the conductivity and catalytic activity of sample 3-5 were higher than those of the original carbon felt, and thus met the application requirements of liquid flow batteries.

[0127] Acid treatment is used to graft more oxygen-containing functional groups when the graphitization degree is above 60% (below 60% contains more oxygen-containing functional groups). The grafted functional groups will destroy part of the carbon-carbon double bonds, and the carbon-oxygen single bonds can be broken in the subsequent carbonization range to form a complete carbon structure.

[0128] Carbon fibers with a graphitization degree of more than 60% have more initial graphite structures, and the defects at the edge of the graphite structure can be directly etched away using an inert gas plasma source. (If the carbon is deposited, the graphitization degree will be too high, resulting in poor hydrophilicity and reduced performance in the field of flow batteries).

[0129] The degree of graphitization is high, and it is necessary to keep it at a higher temperature for a short time in a low oxygen environment.

[0130] Compared with carbon fibers with a high degree of graphitization, carbon fibers with a low degree of graphitization require longer carbonization and graphitization insulation time and higher temperature in order to achieve sufficient graphitization and ensure the order of the carbon structure.

[0131] Comparative Example 1,

[0132] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0133] Step 1, immersing the carbon felt with a graphitization degree of less than 30% in excess deionized water for 60 minutes, and taking it out after it is fully wetted;

[0134] Step 2, cutting the impregnated carbon felt into electrode sizes, cleaning it with ethanol solution for 15 times, and then soaking it in ultrasound for 60 minutes to clean impurities on the surface of the carbon fiber;

[0135] Step 3, placing the carbon felt after ultrasonic treatment in a blast drying oven, adjusting the temperature to 80° C., and drying time to 12 h, to obtain sample A.

[0136] The peak current of sample A prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 195 mA and 163 mA, the potential difference was 0.74 V, and the energy efficiency was 68.18%. Figure 5 .

[0137] Comparative Example 2,

[0138] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0139] Step 1, immersing the carbon felt with a graphitization degree of 30-60% in excess deionized water for 60 minutes, and taking it out after it is fully wetted;

[0140] Step 2, cutting the impregnated carbon felt into electrode sizes, cleaning it with ethanol solution for 15 times, and then soaking it in ultrasound for 60 minutes to clean impurities on the surface of the carbon fiber;

[0141] Step 3, soak the cleaned carbon felt in a 3 mol / L potassium hydroxide solution for 6 hours, then take it out and wash it with deionized water until it is neutral, place it in a forced air drying oven, adjust the temperature to 80°C, and dry it for 12 hours to obtain sample B.

[0142] The peak current of sample B prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 212 mA and 192 mA, the potential difference was 0.65 V, and the energy efficiency was 79.82%. Figure 6 .

[0143] Comparative Example 3,

[0144] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0145] Step 1, immersing the carbon felt with a graphitization degree of 30-60% in excess deionized water for 60 minutes, and taking it out after it is fully wetted;

[0146] Step 2, cutting the impregnated carbon felt into electrode sizes, cleaning it with ethanol solution for 15 times, and then soaking it in ultrasound for 60 minutes to clean impurities on the surface of the carbon fiber;

[0147] Step 3, soak the cleaned carbon felt in a 3 mol / L sodium hydroxide solution for 6 hours, then take it out and wash it with deionized water until it is neutral, place it in a forced air drying oven, adjust the temperature to 80°C, and dry it for 12 hours to obtain sample C.

[0148] The peak current of sample C prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 210 mA and 191 mA, the potential difference was 0.65 V, and the energy efficiency was 78.21%. Figure 6 .

[0149] The degree of alkali etching is different. Potassium hydroxide is more alkaline (alkali metals are more active) and has stronger etching ability. Alkali etching mainly etches unstable carbon atoms, thereby creating micropores and mesopores on the surface of carbon fibers and increasing the specific surface area. Similarly, if there are too many etching defects, it will also cause irreversible damage to the carbon structure. Therefore, it is very important to use different types and concentrations of alkali solutions for carbon fibers with different degrees of graphitization and adjust the balance between the two.

[0150] Comparative Example 4,

[0151] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0152] Step 1, immersing the carbon felt with a graphitization degree of more than 60% in excess deionized water for 60 minutes, and taking it out after it is fully wetted;

[0153] Step 2, cutting the impregnated carbon felt into electrode sizes, cleaning it with ethanol solution for 15 times, and then soaking it in ultrasound for 60 minutes to clean impurities on the surface of the carbon fiber;

[0154] Step 3, soak the cleaned carbon felt in a 2 mol / L sulfuric acid solution for 6 hours, then take it out and wash it with deionized water until it is neutral, place it in a forced air drying oven, adjust the temperature to 80°C, and dry it for 12 hours to obtain sample D.

[0155] The peak current of sample D prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 230 mA and 217 mA, the potential difference was 0.74 V, and the energy efficiency was 82.02%. Figure 7 .

[0156] Comparative Example 5,

[0157] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0158] Step 1, immersing the carbon felt with a graphitization degree of more than 60% in excess deionized water for 60 minutes, and taking it out after it is fully wetted;

[0159] Step 2, cutting the impregnated carbon felt into electrode sizes, cleaning it with ethanol solution for 15 times, and then soaking it in ultrasound for 60 minutes to clean impurities on the surface of the carbon fiber;

[0160] Step 3, soaking the cleaned carbon felt in a hydrochloric acid solution with a concentration of 2 mol / L for 6 hours, then taking it out and washing it with deionized water until it is neutral, placing it in a forced air drying oven, adjusting the temperature to 80° C., and drying it for 12 hours to obtain sample E;

[0161] The peak current of sample E prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 228 mA and 215 mA, the potential difference was 0.75 V, and the energy efficiency was 80.41%. Figure 7 .

[0162] Comparative Example 6,

[0163] A method for batch processing of carbon-based electrodes for flow batteries comprises the following steps:

[0164] Step 1, immersing the carbon felt with a graphitization degree of more than 60% in excess deionized water for 60 minutes, and taking it out after it is fully wetted;

[0165] Step 2, cutting the impregnated carbon felt into electrode sizes, cleaning it with ethanol solution for 15 times, and then soaking it in ultrasound for 60 minutes to clean impurities on the surface of the carbon fiber;

[0166] Step 3, soaking the cleaned carbon felt in a 2 mol / L nitric acid solution for 6 hours, then taking it out and washing it with deionized water until it is neutral, placing it in a forced air drying oven, adjusting the temperature to 80° C., and drying it for 12 hours to obtain sample F;

[0167] The peak current of sample F prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 226 mA and 216 mA, the potential difference was 0.74 V, and the energy efficiency was 78.94%. Figure 7 .

[0168] The types of acids in Comparative Examples 4, 5, and 6 are different, and the degrees of oxidation are different. Acid oxidation mainly grafts carbon-oxygen single bonds (which has a positive effect within a certain range), but if the degree of oxidation is too low, a certain number of carbon-oxygen double bonds will be grafted, which will have a negative effect and reduce some performance; and if the degree of oxidation is too high, it will lead to too many oxygen-containing functional groups on the surface, and the conductivity will be significantly reduced.

[0169] Comparative Example 7,

[0170] A method for batch processing of carbon-based electrodes for flow batteries, in step 7, first introducing an inert gas plasma source to etch the surface of the carbon fiber in the temperature range of 2000-2200°C, the volume ratio of the plasma source to the ambient gas is 0.02-0.2, the plasma power is 100W, and the etching time is 60s. Then, a carbon-containing gas plasma source is introduced to deposit on the surface of the carbon fiber, the volume ratio of the plasma source to the ambient gas is 0.3-0.5, the plasma power is 1200w, and the deposition time is 60min; the remaining steps are the same as in Example 1; and sample G is obtained.

[0171] The peak current of sample G prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 238 mA and 216 mA, the potential difference was 0.63 V, and the energy efficiency was 78.85%. Figure 5 .

[0172] Comparative Example 8,

[0173] A method for batch processing of carbon-based electrodes for flow batteries, in step 7, first introducing an inert gas plasma source in the temperature range of 2000-2200°C to etch the surface of the carbon fiber, the volume ratio of the plasma source to the ambient gas is 0.02-0.2, the plasma power is 150W, and the etching time is 180s. Then, a carbon-containing gas plasma source is introduced to deposit on the surface of the carbon fiber, the volume ratio of the plasma source to the ambient gas is 0.3-0.5, the plasma power is 1100w, and the deposition time is 50min; the remaining steps are the same as in Example 6; and sample H is obtained.

[0174] The peak current of the sample H prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 180 mA and 179 mA, the potential difference was 0.71 V, and the energy efficiency was 73.30%. Figure 6 .

[0175] Comparative Example 9,

[0176] In step S1, the graphitization degree of the carbon felt is less than 30%. Before step S2, the pretreated carbon felt is etched in an alkaline solution (3 mol / L potassium hydroxide) for 24 h, cleaned to neutrality, and dried; the remaining steps are the same as in Example 1; and sample I is obtained.

[0177] The peak current of sample I prepared in this comparative example in the acidic vanadium liquid flow battery system measured at room temperature was 18 mA and 14 mA, and the potential difference was 0.84 V.

[0178] Comparative Example 10,

[0179] In step S1, the graphitization degree of the carbon felt is 30%-60%. Before step S2, the pretreated carbon felt is immersed in an acid solution (2 mol / L sulfuric acid solution) for oxidation for 6 h, washed to neutrality, and dried; the remaining steps are the same as those in Example 6; and sample J is obtained.

[0180] The peak current of sample J prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 183 mA and 159 mA, and the potential difference was 0.79 V.

[0181] Comparative Example 11,

[0182] In step S1, the graphitization degree of the carbon felt is above 60%. Before step S2, the pretreated carbon felt is etched in an alkaline solution (3 mol / L potassium hydroxide) for 24 h, cleaned to neutrality, and dried; the remaining steps are the same as in Example 9; and sample K is obtained.

[0183] The peak current of sample K prepared in this comparative example in the acidic vanadium liquid flow battery system measured at room temperature was 206 mA and 186 mA, and the potential difference was 0.73 V.

[0184] Comparative Example 12,

[0185] In step S1, the graphitization degree of the carbon felt is more than 60%; in step S5, at 2200°C, a carbon-containing gas plasma source (methane) is first introduced to deposit on the surface of the carbon fiber, the volume ratio of the plasma source to the ambient gas is 0.3, the plasma power is 1200W, and the deposition time is 60min. Subsequently, an inert gas (argon) plasma source is introduced to etch the surface of the carbon fiber, the volume ratio of the plasma source to the ambient gas is 0.2, the plasma power is 200W, and the etching time is 300s; the remaining steps are the same as in Example 9; and sample L is obtained.

[0186] The peak current of sample L prepared in this comparative example in the acidic vanadium liquid flow battery system was measured at room temperature to be 120 mA and 84 mA, and the potential difference was 0.79 V.

[0187] Some existing technologies only use temperature and holding time to adjust the carbon structure of carbon fiber. The order of the carbon structure is largely determined by the raw materials of the carbon fiber (most of the raw materials on the market use polypropylene-based fibers or viscose-based fibers). This means that when the carbon structure of the raw materials themselves is quite different, there will be a large error in adjusting the performance of the carbon fiber only by temperature and holding time, and it is difficult to mass-produce carbon fiber products with high performance requirements. The embodiment of the present invention uses acid-base treatment as pretreatment to provide a basis for subsequent carbonization and graphitization. According to the performance characteristics required by the electrode materials for liquid flow batteries, the carbon fibers on the market are divided into three different types according to the degree of graphitization, and different pretreatment methods are used for different types to adjust the temperature range and holding time of oxidation, carbonization, and graphitization, and according to the specific structure of different raw materials combined with the performance requirements of liquid flow battery electrodes, carbon deposition and etching are performed on the surface of the carbon fiber to achieve a suitable degree of graphitization. After testing, it can meet the application requirements of the liquid flow battery field, and the process is easy to control and easy to achieve large-scale batch production.

[0188] The embodiment of the present invention controls the deposition time and the etching time. The carbon-containing plasma source deposition is to add more carbon atoms so that the intrinsic carbon defects inside the carbon fiber are supplemented. During the deposition process, linear defects will inevitably be generated at the junction of the graphite structure. Plasma etching can etch the unstable defects.

[0189] In the embodiment, the power of the carbon-containing gas plasma source and the deposition time are key parameters. If the parameters are beyond the range, the performance will decrease. If the degree of graphitization is too high, the hydrophilicity will deteriorate and the balance between hydrophilicity and conductivity cannot be ensured.

[0190] In the embodiment, the inert gas plasma source power and the etching time are key parameters. If they are out of range, the performance will be degraded. If the defect level is too high, the conductivity will be poor and the balance between hydrophilicity and conductivity cannot be guaranteed.

[0191] In addition to carbon felt, the carbon-based electrode raw material of the present invention can directly use pre-oxidized felt as a raw material. The purpose of the present invention is to prepare an electrode material suitable for a liquid flow battery. The final effect mainly depends on the process. The original felt only needs to ensure good hydrophilicity and a density within a suitable range. Pre-oxidized felt is the raw material of carbon felt. All carbon fibers are obtained by carbonizing or graphitizing pre-oxidized fibers. However, the commercial carbon felt and graphite felt processing processes on the current market cannot fully meet the requirements of liquid flow battery electrode materials. There is a gap in the market for liquid flow battery-specific electrode materials.

[0192] In the embodiment of the present invention, a plasma source is introduced to deposit and etch the surface of the carbon felt in the temperature range of 2200-2200°C. Only through a single heating process, the graphitization degree of the carbon felt can be significantly improved while ensuring the stable bonding of the carbon bonds. This is a further optimization and improvement in the technical combination of the two. The calcination of the embodiment of the present invention does not introduce other elements. Only the carbon structure inside the carbon felt changes. The balance between deposition and etching can obtain a stable and conductive sp2 structure, such as Figure 8 As shown, all samples diffract obvious (002) crystal planes and (100) crystal planes, and the (002) crystal plane corresponds to the sp2 structure of graphite. It can be seen that in the original sample, as the degree of graphitization increases, the (002) crystal plane is enhanced, and in all samples after treatment, the (002) crystal plane is significantly enhanced, indicating that the order of the carbon structure is improved during the treatment process, the degree of graphitization of the sample is increased, and the electrochemical properties of the carbon fiber itself are enhanced. There is no doping of other elements or compounding between materials, the cost is low, the process flow is convenient, and it is easy to achieve mass production. The improvements of different processes of the present invention enable the carbon felt electrode samples to have different electrochemical properties, significantly improve the catalytic activity of the carbon felt surface for redox, and are widely applicable to many liquid flow battery systems. In the specific embodiment of the present invention, only the all-vanadium redox liquid flow battery is selected as an example, and all other redox liquid flow battery system electrodes prepared by this method belong to the protection scope of the present invention. Utilizing the synergistic effect of the preparation method of the present invention, the carbon fiber inside the original carbon felt is surface treated and the structure is optimized, which greatly improves the conductivity and catalytic activity of the electrode. The method for batch processing of carbon-based electrodes for liquid flow batteries of the present invention is simple and easy to operate, environmentally friendly, has low raw material cost, is easy to be industrialized on a large scale, and can be widely used in various liquid flow battery commercialization fields.

[0193] The embodiments of the present invention greatly improve the activation ability of carbon atoms inside the fiber, improve the controllability of performance, and facilitate the application of electrodes in different liquid flow battery systems rather than a single system. No manual control is required during the entire heating process, and the cost increase caused by the temperature increase is limited, but the gas environment requirements are higher, so it should be carried out in a large-scale continuous graphite furnace that meets safety standards to avoid burning of carbon felt materials. In addition, the surface treatment and low-temperature oxidation of carbon felt in the embodiments of the present invention can remove most impurities, improve the adaptability of carbon felt to high temperatures, and be suitable for industrial production.

[0194] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for batch processing of carbon-based electrodes for liquid flow batteries, characterized in that: The following steps are involved: S1, pre-treating the carbon felt; S2, in an atmosphere with an oxygen volume content of 5%-30%, heating to 100-400°C, with a heating rate of 4-8°C / min, and keeping warm for 20min-120min, for low-temperature oxidation; S3, in an inert atmosphere, adjust the oxygen content to less than 1200ppm, raise the temperature to 1000-1500℃, at a heating rate of 4-6℃ / min, and keep the temperature for 30min-300min to perform high temperature activation; S4, adjusting the oxygen content to less than 150ppm, heating to 2000-2250°C, heating rate of 3-5°C / min, keeping the temperature for 1min-5min, and graphitizing; S5, in a temperature range of 2000-2200°C, an inert gas plasma source is introduced to etch the surface of the carbon fiber, the volume ratio of the plasma source to the ambient gas is 0.02-0.2, the plasma power is 100-1200W, and the etching time is 30-360s; S6, heating to 2250℃-2300℃, keeping warm for 1-5min, and naturally cooling to room temperature; The graphitization degree of the carbon felt in S1 is less than 30%. Before the inert gas plasma source is introduced in S5, a carbon-containing gas plasma source is first introduced to deposit on the surface of the carbon fiber. The volume ratio of the carbon-containing gas plasma source to the ambient gas is 0.3-0.5, the plasma power is 1000-1200w, and the deposition time is 40-60min; wherein the etching time of the inert gas plasma source is 30-120s; Or the graphitization degree of the carbon felt in S1 is 30-60%, and before S2, the pretreated carbon felt is etched in an alkaline solution, cleaned to neutrality, and dried; before introducing the inert gas plasma source in S5, a carbon-containing gas plasma source is first introduced to deposit on the surface of the carbon fiber, the volume ratio of the carbon-containing gas plasma source to the ambient gas is 0.3-0.5, the plasma power is 1000-1200w, and the deposition time is 40-60min; wherein, the etching time of the inert gas plasma source is 120-240s; Alternatively, the graphitization degree of the carbon felt in S1 is above 60%. Before S2, the pretreated carbon felt is immersed in an acid solution for oxidation, cleaned to neutrality, and dried; wherein the etching time of the inert gas plasma source is 240-360s.

2. A method for batch processing of carbon-based electrodes for liquid flow batteries according to claim 1, characterized in that: The S1 is specifically: S11, immersing the carbon felt in excess deionized water for 30-60 minutes and taking it out after it is fully wetted; S12, cutting the impregnated carbon felt into electrode sizes, cleaning it with an ethanol solution for 10-15 times, and then soaking it in ultrasound for 15-60 minutes to clean impurities on the surface of the carbon fiber; S13, placing the carbon felt after ultrasonic treatment in a blast drying oven, adjusting the temperature to 40-80°C, and drying time to 4-12h.

3. A method for batch processing of carbon-based electrodes for liquid flow batteries according to claim 1, characterized in that: In S3, after the temperature reaches 1200°C, the oxygen content must be lower than 540 ppm.

4. A method for batch processing of carbon-based electrodes for liquid flow batteries according to claim 1, characterized in that: In the above-mentioned S4, after the temperature reaches 2200°C, the oxygen content needs to be lower than 60ppm.

5. The method for batch processing of carbon-based electrodes for liquid flow batteries according to claim 1, characterized in that: The alkaline solution is potassium hydroxide or sodium hydroxide solution, the concentration is 2-5 mol / L, and the treatment time is 24-72h.

6. A method for batch processing of carbon-based electrodes for liquid flow batteries according to claim 1, characterized in that: The acid solution is sulfuric acid, hydrochloric acid or nitric acid solution, with a concentration of 0.5-3 mol / L and a treatment time of 6-48 hours.

7. A method for batch processing of carbon-based electrodes for liquid flow batteries according to claim 1, characterized in that: The carbon-containing gas plasma source is an olefin gas, and the mass content of other elements except C, H, and O is less than 5%; the inert gas plasma source is helium, neon, argon, krypton or xenon.

Citation Information

Patent Citations

  • Surface modification method for raising activity of electrode material of vanadium cell

    CN102723502A

  • Method for preparing high-performance asphalt-based carbon fiber through rapid pre-oxidation

    CN114790592A