A method for efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue
By adjusting the aluminum-silicon molar ratio through alkaline calcination and NaAl(OH)4 solution, germanium and aluminum-silicon components in germanium chlorination distillation residue are separated under alkaline conditions. This solves the problems of low separation efficiency and high acid consumption in existing technologies, and achieves efficient and low-cost germanium recovery.
Patent Information
- Application Number
- CN202311509793.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-14
AI Technical Summary
Existing methods for recovering germanium from germanium chloride distillation residues suffer from problems such as low separation efficiency of aluminum and silicon components, high acid consumption, and precipitation and adsorption of germanium ions by silicon components, resulting in low germanium recovery rates.
The germanium chloride distillation residue is decomposed by alkaline roasting to form soluble sodium germanate. Then, under alkaline conditions, the molar ratio of aluminum and silicon is adjusted using NaAl(OH)4 solution to form zeolite compound precipitates, thereby achieving the separation of aluminum and silicon components from germanium.
The method achieves efficient separation of germanium and aluminum-silicon components in an alkaline system, reducing acid usage, simplifying the process, lowering costs, and improving germanium recovery rate.
Smart Images

Figure CN117551878B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste comprehensive recycling technology, and in particular to a method for efficient separation of aluminum-silicon components and germanium from germanium chloride distillation residue. Background Technology
[0002] Germanium is an important strategic rare metal and a key raw material for manufacturing semiconductors, infrared optical instruments, optical fibers, and other materials. It has been increasingly widely used in fields such as electronics, aerospace, and fiber optic communications. Many countries have included it in their lists of critical metals to ensure the secure supply of germanium and its materials from the perspective of national development strategies.
[0003] Germanium is extremely dispersed in nature, almost non-existent as an independent mineral, mainly existing as an associated form in sulfide ores such as lead, zinc, and copper, and in lignite. Germanium-containing zinc dust and germanium-containing coal dust generated during lignite combustion are the main raw materials for the germanium extraction industry, and chlorination distillation is currently the primary process for germanium extraction. Some of the germanium in the form of GeO2 and germanium-silicon solid solutions in germanium-containing coal dust is difficult to dissolve during chlorination distillation and enters the chlorination distillation residue. How to recover germanium from the chlorination distillation residue is key to improving the efficient utilization of germanium resources. The recovery of germanium from the residue first requires solving the dissolution problem of germanium-silicon solid solutions and tetragonal GeO2. CN102181649A discloses a process that uses NaOH heating for pretreatment and decomposition, followed by distillation extraction of germanium using hydrochloric acid; CN109777961A discloses a process that uses sodium carbonate for mixed roasting, which decomposes sodium carbonate into sodium silicate and sodium germanate, and then extracts germanium using water leaching-acid leaching; existing processes also typically involve mixing distillation residue with NaOH for alkaline roasting, dissolving aluminum, silicon, and germanium simultaneously in the solution through water leaching, adjusting the pH of the solution from strongly alkaline to acidic, and then recovering germanium by tannin precipitation.
[0004] In summary, most methods for recovering germanium from chlorination distillation residues employ alkaline decomposition to convert germanium into germanate for further recovery. The challenge lies in the efficient separation of aluminum-silicon components from germanium components in the leachate. Existing methods mostly involve adjusting the alkaline solution to acidic conditions to precipitate germanate, but this approach suffers from high acid consumption and the co-precipitation / adsorption of germanium ions by silicon components in the form of silicic acid, which negatively impacts germanium recovery. Summary of the Invention
[0005] Based on the above analysis, the present invention aims to provide a method for efficient separation of aluminum-silicon components and germanium from germanium chloride distillation residue, in order to solve one of the problems of existing methods, such as the precipitation of germanate after adjusting the alkaline solution with acid, the large amount of acid consumption, and the co-precipitation / adsorption of germanium ions by silicon components in the form of silicic acid, resulting in a high content of aluminum-silicon components in the recovered germanium solution.
[0006] In a first aspect, the present invention provides a method for the efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0007] (1) Mix the germanium chloride distillation residue with NaOH or Na2CO3 and calcine to obtain the calcined product;
[0008] (2) The roasted product is leached in water to obtain an extract;
[0009] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0010] (4) Add NaAl(OH)4 solution to the germanium-containing leachate until the molar concentration ratio of aluminum to silicon is 0.5 to 4:1, and heat to react to obtain the product;
[0011] (5) The product is filtered and separated to obtain a germanium solution with low aluminum-silicon component concentration.
[0012] Furthermore, in step (1), the mass fraction of germanium in the germanium chloride distillation residue is 0.1-0.6%.
[0013] Furthermore, in step (1), the mass ratio of germanium chloride distillation residue to NaOH or Na2CO3 is 1:1.5 to 4.5.
[0014] Furthermore, in step (1), the roasting temperature is 400-900℃ and the roasting time is 0.5-5h.
[0015] Furthermore, in step (2), the leaching process also includes controlling the pH value of the leaching system to always be greater than 13.0.
[0016] Furthermore, in step (2), the leaching temperature is 40-100℃, the leaching liquid-solid ratio is 5-25:1, and the leaching time is 30-120 min.
[0017] Furthermore, in step (4), the concentration of the NaAl(OH)4 solution is 0.5–1.5 mol / L.
[0018] Furthermore, in step (4), the heating temperature is 80–180°C and the reaction time is 60–240 min.
[0019] Furthermore, the germanium chlorination distillation residue is the germanium-containing leaching residue produced by the chlorination distillation process of germanium-containing lignite dust.
[0020] Secondly, the present invention provides a germanium solution with a low aluminum-silicon component concentration obtained by the method.
[0021] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0022] (1) The method of the present invention decomposes the insoluble germanium in the germanium chloride distillation residue by alkaline roasting and converts it into soluble sodium germanate. The molar ratio of aluminum and silicon in the germanium-containing leachate is adjusted by NaAl(OH)4 solution and the reaction is carried out under heating so that the sodium aluminum silicon component in the solution forms zeolite-like compound precipitate, thereby achieving the separation of aluminum silicon component from germanium in the leachate under alkaline conditions.
[0023] (2) In the existing process, silicon components are formed by adding acid to form silica gel. A large amount of acid needs to be added to make the alkaline solution acidic. In addition, the formed silica gel is difficult to filter and will adsorb germanium, resulting in the loss of germanium. The method of the present invention can separate germanium from aluminum-silicon components in an alkaline system, avoiding the use of a large amount of acid. The process is short, clean, and low in cost, and the germanium recovery rate is significantly improved.
[0024] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0025] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0026] Figure 1 The XRD pattern of the zeolite prepared in Example 1 of this invention;
[0027] Figure 2 This is a SEM image of the zeolite prepared in Example 1 of the present invention. Detailed Implementation
[0028] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0029] A specific embodiment of the present invention discloses a method for efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0030] (1) Mix the germanium chloride distillation residue with NaOH or Na2CO3 and calcine to obtain the calcined product;
[0031] (2) The roasted product is leached in water to obtain an extract;
[0032] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0033] (4) Add NaAl(OH)4 solution to the germanium-containing leachate until the molar concentration ratio of aluminum to silicon is 0.5 to 4:1, and heat to react to obtain the product;
[0034] (5) The product is filtered and separated to obtain a germanium solution with low aluminum-silicon component concentration.
[0035] Compared with existing technologies, the existing process involves adding acid to form silica gel from silicon components, which requires a large amount of acid to make the alkaline solution acidic. In addition, the formed silica gel is difficult to filter and will adsorb germanium, resulting in germanium loss. The method of the present invention achieves the separation of germanium and aluminum-silicon components in an alkaline system, avoiding the use of large amounts of acid. The process is short, clean, and low in cost, and the germanium recovery rate is significantly improved.
[0036] Furthermore, the method of the present invention decomposes the insoluble germanium in the germanium chloride distillation residue by alkaline roasting and converts it into soluble sodium germanate. The molar ratio of aluminum and silicon in the germanium-containing leachate is adjusted by using NaAl(OH)4 solution, and the reaction is carried out under heating so that the sodium aluminum silicon components in the solution form zeolite-like compound precipitates, thereby achieving the separation of aluminum silicon components from germanium in the leachate under alkaline conditions.
[0037] In one specific embodiment, in step (1), the mass fraction of germanium in the germanium chloride distillation residue is 0.1-0.6%.
[0038] It should be noted that the germanium chlorination distillation residue mentioned in this invention refers to the germanium-containing leaching residue produced by the chlorination distillation process of germanium-containing lignite dust, obtained using existing processes.
[0039] In one specific embodiment, in step (1), the mass ratio of germanium chloride distillation residue to NaOH or Na2CO3 is 1:1.5 to 4.5. For example, the mass ratios are 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, and 1:4.5.
[0040] It should be noted that if the mass ratio of germanium chloride distillation residue to NaOH or Na2CO3 is too low, the aluminum and silicon components in the sample will not react completely; if it is too high, it will easily lead to corrosion of the reaction vessel.
[0041] In one specific implementation, in step (1), the calcination temperature is 400-900°C and the calcination time is 0.5-5h.
[0042] For example, the roasting temperatures are 400℃, 450℃, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃, 800℃, 850℃, and 900℃; and the roasting times are 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, and 5h.
[0043] It should be noted that if the calcination temperature or time is too low, it will affect the degree of reaction, while if it is too high, it will place too high demands on the reactor and affect the reaction process.
[0044] In one specific implementation, step (2) further includes controlling the pH value of the leaching system to always be greater than 13.0 during the leaching process.
[0045] It should be noted that the pH value is always greater than 13.0 when using NaOH solution. If the pH value is less than 13.0, the proportion of aluminum and silicon components in the leaching system will increase. The preferred concentration range of NaOH solution is 1.0 to 3.0 mol / L.
[0046] In one specific embodiment, in step (2), the leaching temperature is 40-100°C, the leaching liquid-solid ratio is 5-25:1, and the leaching time is 30-120 min.
[0047] For example, the leaching temperatures are 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, 80℃, 85℃, 90℃, 95℃, and 100℃; the leaching liquid-solid ratios are 5:1, 10:1, 15:1, 20:1, and 25:1; and the leaching times are 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, and 120min.
[0048] It should be noted that, according to thermodynamic analysis of the solution composition, excessively high leaching temperatures lead to an increase in amorphous sodium aluminosilicate during the water leaching process, while excessively low temperatures are not conducive to the reaction. Similarly, excessively long leaching times will also increase the amount of amorphous sodium aluminosilicate during the water leaching process.
[0049] In one specific embodiment, the calcined product in step (2) is ground and then leached in water for reaction.
[0050] In one specific embodiment, in step (4), the solvent in the NaAl(OH)4 solution is water, and the concentration of NaAl(OH)4 is 0.5 to 1.5 mol / L.
[0051] In one specific embodiment, in step (4), the heating temperature is 80-180°C and the reaction time is 60-240 min.
[0052] For example, the heating temperatures are 80℃, 90℃, 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, 160℃, 170℃, and 180℃; and the reaction times are 60min, 70min, 80min, 90min, 100min, 110min, 120min, 130min, 140min, 150min, 160min, 170min, 180min, 190min, 200min, 210min, 220min, 230min, and 240min.
[0053] It should be noted that the temperature range is determined based on thermodynamic calculations. Heating the temperature too high will increase the equilibrium concentration of Si in the solution, while heating the temperature too low will not facilitate a rapid reaction. The time range is determined experimentally. If the time is too short, the reaction will not proceed completely.
[0054] In another specific embodiment of the present invention, a germanium solution with a low aluminum-silicon component concentration obtained by the method is disclosed.
[0055] It should be noted that the final germanium recovery rate using the method of the present invention is 68-86%, and the aluminum concentration in the germanium solution with low aluminum-silicon component concentration is 0.087-0.124 g / L, the silicon concentration is 0.641-1.086 g / L, and the germanium concentration is 0.0176-0.0211 g / L.
[0056] The technical solution of the present invention will be further explained below with reference to specific embodiments. In the following embodiments, the germanium chloride distillation residue mainly contains phases such as CaSO4·2(H2O), SiO2, and Al2O3, with mass fractions of aluminum, silicon, and germanium of 3.59%, 28.66%, and 0.17%, respectively.
[0057] Example 1
[0058] This embodiment provides a method for the efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0059] (1) After mixing the germanium chloride distillation residue with NaOH, grind it into a homogeneous phase, and calcine it in air at a temperature of 400℃ for 60 min with a heating rate of 10℃ / min to obtain the calcined product, wherein the mass of NaOH is 1.5 times the mass of the germanium chloride distillation residue;
[0060] (2) The roasted product was ground in a three-head ball mill for 10 min, and then leached with deionized water at a leaching temperature of 40°C and a leaching time of 30 min. The leaching liquid-solid ratio was 25:1. At the same time, the pH of the leaching system was controlled to be greater than 13.0 by adding 3.0 mol / L NaOH solution to obtain the leached material.
[0061] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0062] (4) Add a 1.5 mol / L NaAl(OH)4 solution to the germanium-containing leachate until the molar ratio of aluminum to silicon is 0.5:1, and react at 100°C for 240 min to obtain the product;
[0063] (5) The product is subjected to liquid-solid separation. The solid is zeolite and the liquid is a germanium solution with low aluminum-silicon component concentration.
[0064] The solid in step (5) was subjected to XRD and SEM tests, and the results are as follows: Figure 1 and 2 As shown. Among them, Figure 1 This indicates that the precipitate is a zeolite-phase sodium aluminosilicate compound. Figure 2 This indicates that the precipitate has good crystallinity, uniform particle size, and a smooth surface morphology.
[0065] Example 2
[0066] This embodiment provides a method for the efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0067] (1) After mixing the germanium chloride distillation residue with NaOH, grind it into a homogeneous phase and calcine it in air at a temperature of 700℃ for 180 min with a heating rate of 10℃ / min to obtain the calcined product, wherein the mass of NaOH is 3 times the mass of the germanium chloride distillation residue.
[0068] (2) The calcined product was ground in a three-head ball mill for 10 min, and then leached with deionized water at a leaching temperature of 60°C and a leaching time of 60 min. The leaching liquid-solid ratio was 20:1. At the same time, the pH of the leaching system was controlled to be greater than 13.0 by adding 3.0 mol / L NaOH solution to obtain the leached material.
[0069] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0070] (4) Add a 1.5 mol / L NaAl(OH)4 solution to the germanium-containing leachate until the molar ratio of aluminum to silicon is 1:1, and react at 160°C for 240 min to obtain the product;
[0071] (5) The product is subjected to liquid-solid separation. The solid is zeolite and the liquid is a germanium solution with low aluminum-silicon component concentration.
[0072] The solid in step (5) of this embodiment was subjected to XRD and SEM tests, and the results were basically the same as those in Example 1. Due to space limitations, they will not be listed one by one.
[0073] Example 3
[0074] This embodiment provides a method for the efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0075] (1) The germanium chloride distillation residue was mixed with NaOH and ground until a homogeneous phase was formed. The mixture was then calcined in air at 900°C for 120 min at a heating rate of 10°C / min to obtain the calcined product. The mass of NaOH was 4.5 times that of the germanium chloride distillation residue.
[0076] (2) The roasted product was ground in a three-head ball mill for 10 min, and then leached with deionized water at a leaching temperature of 40°C and a leaching time of 90 min. The leaching liquid-solid ratio was 10:1. At the same time, the pH of the leaching system was controlled to be greater than 13.0 by adding 3.0 mol / L NaOH solution to obtain the leached material.
[0077] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0078] (4) Add a 1.5 mol / L NaAl(OH)4 solution to the germanium-containing leachate until the molar ratio of aluminum to silicon is 2:1, and react at 140°C for 240 min to obtain the product;
[0079] (5) The product is subjected to liquid-solid separation. The solid is zeolite and the liquid is a germanium solution with low aluminum-silicon component concentration.
[0080] The solid in step (5) of this embodiment was subjected to XRD and SEM tests, and the results were basically the same as those in Example 1. Due to space limitations, they will not be listed one by one.
[0081] Example 4
[0082] This embodiment provides a method for the efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0083] (1) After mixing the germanium chloride distillation residue with NaOH, grind it into a homogeneous phase and calcine it in air at a temperature of 600℃ for 240 min with a heating rate of 10℃ / min to obtain the calcined product, wherein the mass of NaOH is 3 times the mass of the germanium chloride distillation residue.
[0084] (2) The roasted product was ground in a three-head ball mill for 10 min, and then leached with deionized water at a leaching temperature of 40°C and a leaching time of 120 min. The leaching liquid-solid ratio was 5:1. At the same time, the pH of the leaching system was controlled to be greater than 13.0 by adding 2.5 mol / L NaOH solution to obtain the leached material.
[0085] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0086] (4) Add a 1.0 mol / L NaAl(OH)4 solution to the germanium-containing leachate until the molar ratio of aluminum to silicon is 3.0:1, and react at 180°C for 120 min to obtain the product;
[0087] (5) The product is subjected to liquid-solid separation. The solid is zeolite and the liquid is a germanium solution with low aluminum-silicon component concentration.
[0088] The solid in step (5) of this embodiment was subjected to XRD and SEM tests, and the results were basically the same as those in Example 1. Due to space limitations, they will not be listed one by one.
[0089] Example 5
[0090] This embodiment provides a method for the efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0091] (1) After mixing the germanium chloride distillation residue with NaOH, grind it into a homogeneous phase, and calcine it in air at a temperature of 600℃ for 300 min with a heating rate of 10℃ / min to obtain the calcined product, wherein the mass of NaOH is 3 times the mass of the germanium chloride distillation residue.
[0092] (2) The calcined product was ground in a three-head ball mill for 10 min, and then leached with deionized water at a leaching temperature of 90°C and a leaching time of 30 min. The leaching liquid-solid ratio was 25:1. At the same time, the pH of the leaching system was controlled to be greater than 13.0 by adding 2.0 mol / L NaOH solution to obtain the leached material.
[0093] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0094] (4) Add a 1.5 mol / L NaAl(OH)4 solution to the germanium-containing leachate until the molar ratio of aluminum to silicon is 3.0:1, and react at 120°C for 180 min to obtain the product;
[0095] (5) The product is subjected to liquid-solid separation. The solid is zeolite and the liquid is a germanium solution with low aluminum-silicon component concentration.
[0096] The solid in step (5) of this embodiment was subjected to XRD and SEM tests, and the results were basically the same as those in Example 1. Due to space limitations, they will not be listed one by one.
[0097] Example 6
[0098] This embodiment provides a method for the efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0099] (1) After mixing the germanium chloride distillation residue with NaOH, grind it into a homogeneous phase, and calcine it in air at a temperature of 400℃ for 60 min with a heating rate of 10℃ / min to obtain the calcined product, wherein the mass of NaOH is 1.5 times the mass of the germanium chloride distillation residue;
[0100] (2) The calcined product was ground in a three-head ball mill for 10 min, and then leached with deionized water at a leaching temperature of 40°C and a leaching time of 90 min. The leaching liquid-solid ratio was 5:1. At the same time, the pH of the leaching system was controlled to be greater than 13.0 by adding 2.0 mol / L NaOH solution to obtain the leached material.
[0101] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0102] (4) Add a 1.0 mol / L NaAl(OH)4 solution to the germanium-containing leachate until the molar ratio of aluminum to silicon is 4:1, and react at 80°C for 60 min to obtain the product;
[0103] (5) The product is subjected to liquid-solid separation. The solid is zeolite and the liquid is a germanium solution with low aluminum-silicon component concentration.
[0104] The solid in step (5) of this embodiment was subjected to XRD and SEM tests, and the results were basically the same as those in Example 1. Due to space limitations, they will not be listed one by one.
[0105] Example 7
[0106] This embodiment provides a method for the efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue, comprising the following steps:
[0107] (1) After mixing the germanium chloride distillation residue with NaOH, grind it into a homogeneous phase, and calcine it in air at a temperature of 600℃ for 90 min with a heating rate of 10℃ / min to obtain the calcined product, wherein the mass of NaOH is 3 times the mass of the germanium chloride distillation residue.
[0108] (2) The roasted product was ground in a three-head ball mill for 10 min, and then leached with deionized water at a leaching temperature of 50°C and a leaching time of 30 min. The leaching liquid-solid ratio was 15:1. At the same time, the pH of the leaching system was controlled to be greater than 13.0 by adding 1.5 mol / L NaOH solution to obtain the leached material.
[0109] (3) The leaching material is filtered and separated to obtain a germanium-containing leaching solution;
[0110] (4) Add 1.5 mL of 4.0 mol / L NaAl(OH)4 solution to the germanium-containing leachate until the molar ratio of aluminum to silicon is 3.5:1, and react at 140 °C for 120 min to obtain the product;
[0111] (5) The product is subjected to liquid-solid separation. The solid is zeolite and the liquid is a germanium solution with low aluminum-silicon component concentration.
[0112] The solid in step (5) of this embodiment was subjected to XRD and SEM tests, and the results were basically the same as those in Example 1. Due to space limitations, they will not be listed one by one.
[0113] Comparative Example 1
[0114] This comparative example describes a method for efficient separation of aluminum and silicon components from germanium in germanium chloride distillation residue. The method is the same as in Example 1, except that in step (4), a NaAl(OH)4 solution with a concentration of 1.5 mol / L is added to the germanium-containing leachate until the molar concentration ratio of aluminum to silicon is 5:1.
[0115] Comparative Example 2
[0116] This comparative example describes a method for efficient separation of aluminum and silicon components from germanium in germanium chloride distillation residue. The method is the same as in Example 1, except that in step (4), a NaAl(OH)4 solution with a concentration of 1.5 mol / L is added to the germanium-containing leachate until the molar concentration ratio of aluminum to silicon is 1.7:10.6.
[0117] Comparative Example 3
[0118] The method for efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue in this comparative example is the same as that in Example 1, except that the reaction temperature in step (4) is 75°C.
[0119] Comparative Example 4
[0120] The method for efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue in this comparative example is the same as that in Example 1, except that the reaction temperature in step (4) is 185°C.
[0121] Comparative Example 5
[0122] This comparative example describes a method for efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue. The method is the same as in Example 1, except that step (4) is omitted, and the germanium-containing leachate from step (3) is directly filtered and separated to obtain a solution.
[0123] Experimental Example 1
[0124] The leaching rates of aluminum, silicon, and germanium in the leaching material of step (2) in Examples 1-7 and Comparative Examples 1-4 were tested using ICP-OES. The precipitation conversion rates of aluminum, silicon, and germanium in step (4), the concentrations of aluminum, silicon, and germanium in the germanium solution with low aluminum and silicon component concentration in step (5), and the final germanium recovery rate in the whole process were also tested. In the method of Comparative Example 5, the leaching rates of aluminum, silicon, and germanium in the leaching material of step (2) and the concentrations of aluminum, silicon, and germanium in the final solution were also tested. The results are shown in Table 1.
[0125]
[0126] As can be seen from the table above, the molar concentrations of aluminum and silicon and the reaction temperature in step (4) need to be within the range specified in this invention in order to achieve efficient separation of the aluminum-silicon component from germanium. Without adding NaAl(OH)4 solution in step (4), efficient separation of the aluminum-silicon component from germanium cannot be achieved.
[0127] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for efficiently separating aluminum-silicon components from germanium in germanium chloride distillation residue, characterized in that, Includes the following steps: (1) The germanium chloride distillation residue was mixed with Na2CO3 and calcined to obtain the calcined product; The germanium chloride distillation residue contains CaSO4•2(H2O), SiO2, and Al2O3 phases, with aluminum, silicon, and germanium elemental mass fractions of 3.59%, 28.66%, and 0.17%, respectively. (2) The roasted product is leached in water to obtain a leaching material; wherein, the leaching process also includes controlling the pH value of the leaching system to always be greater than 13.0; (3) The leaching material is filtered and separated to obtain a germanium-containing leachate; (4) Add NaAl(OH)4 solution to the germanium-containing leachate until the molar concentration ratio of aluminum to silicon is 0.5~4:1, heat to react, and obtain the product; The concentration of the NaAl(OH)4 solution is 0.5~1.5 mol / L, and the heating temperature is 80~180℃. The NaAl(OH)4 solution is used to adjust the molar ratio of aluminum and silicon in the germanium-containing leachate. The reaction is carried out under heating, causing the sodium aluminum silicon components in the solution to form zeolite-like compound precipitates, thereby achieving the separation of aluminum silicon components from germanium in the leachate under alkaline conditions. (5) The product is filtered and separated to obtain a germanium solution with a low aluminum-silicon component concentration; In germanium solutions with low aluminum and silicon concentrations, the aluminum concentration is 0.087–0.124 g / L, the silicon concentration is 0.641–1.086 g / L, and the germanium concentration is 0.0176–0.0211 g / L, with a germanium recovery rate of 68–86%.
2. The method for efficient separation of aluminum-silicon components and germanium from germanium chloride distillation residue according to claim 1, characterized in that, In step (1), the mass fraction of germanium in the germanium chloride distillation residue is 0.1~0.6%.
3. The method for efficient separation of aluminum-silicon components and germanium from germanium chloride distillation residue according to claim 1, characterized in that, In step (1), the mass ratio of germanium chloride distillation residue to NaOH or Na2CO3 is 1:1.5~4.
5.
4. A method for efficient separation of aluminum-silicon components and germanium from germanium chloride distillation residue according to any one of claims 1-3, characterized in that, In step (1), the roasting temperature is 400~900℃ and the roasting time is 0.5~5h.
5. The method for efficient separation of aluminum-silicon components and germanium from germanium chloride distillation residue according to claim 1, characterized in that, In step (2), the leaching temperature is 40~100℃, the leaching liquid-solid ratio is 5~25:1, and the leaching time is 30~120min.
6. The method for efficient separation of aluminum-silicon components and germanium from germanium chloride distillation residue according to claim 1, characterized in that, In step (4), the concentration of the NaAl(OH)4 solution is 1.0~1.5 mol / L.
7. The method for efficient separation of aluminum-silicon components and germanium from germanium chloride distillation residue according to claim 1, characterized in that, In step (4), the heating temperature is 90~170℃ and the reaction time is 60~240min.
8. A method for efficient separation of aluminum-silicon components from germanium in germanium chloride distillation residue according to any one of claims 1-7, characterized in that, Germanium chlorination distillation residue is germanium-containing leaching residue produced by chlorination distillation of germanium-containing lignite dust.
Citation Information
Patent Citations
Method for recovering germanium from germanium extraction residues
CN102181649A
Method for leaching out germanium from germanium chlorination distilled calcium slag
CN109777961A
Resource comprehensive utilization method of germanium extraction residues
CN115477501A