A quaternized polyarylethernitrile anion exchange membrane and its preparation method and application

By introducing benzimidazole into the polyarylene ether nitrile anion exchange membrane and modifying the main chain structure, the degradation problem of polyarylene ether membranes under alkaline conditions was solved, and a quaternized polyarylene ether nitrile membrane with high alkalinity and high ion conductivity was achieved, which is suitable for fuel cell materials.

CN117844020BActive Publication Date: 2024-11-29UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410042904.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-11
Publication Date
2024-11-29
Estimated Expiration
2044-01-11

AI Technical Summary

Technical Problem

Existing polyarylether anion exchange membranes are prone to aryl ether cleavage under alkaline conditions, leading to main chain degradation. Furthermore, the synthesis process is complex and requires noble metal catalysts, which limits their practical application.

Method used

A quaternized polyarylene ether nitrile anion exchange membrane with a backbone free of electron-withdrawing linkers and a para-quaternary ammonium group structure of etheroxy groups was developed. The base stability was improved by introducing benzimidazole, and the polymer backbone was modified by Leuckart and Menshutkin reaction to form a hydrogen bond network to enhance mechanical properties.

Benefits of technology

It improves the alkaline stability and ionic conductivity of the membrane, reduces the swelling rate, and has excellent mechanical properties, making it suitable for fuel cell-related materials and devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117844020B_ABST
    Figure CN117844020B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of special functional polymer materials, and specifically relates to a quaternized polyarylether nitrile anion exchange membrane and a preparation method and application thereof. In order to solve the problem of poor alkali resistance of the main chain of polyarylether anion exchange membranes, the present invention discloses and prepares a high alkali-resistant anion exchange membrane whose main chain does not contain electron-withdrawing groups and has an etheroxy para-quaternary ammonium group structure, eliminating key triggering factors such as electron-withdrawing linking groups and etheroxy ortho-cationic groups that cause aromatic ether cracking. This strategy does not require precious metal catalysts, and the subsequent quaternization process is simple. In addition, the present invention introduces benzimidazole into the quaternized polyarylether nitrile anion exchange membrane, and on the basis of retaining the aromatic structure of the main chain polyarylether nitrile, it is converted into an amine group through a novel Leuckart reaction and a carbonyl reaction of the main chain, which is simple to operate and eliminates key triggering factors such as electron-withdrawing linking groups and etheroxy ortho-cationic groups that cause aromatic ether cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of special functional polymer materials, and specifically relates to a quaternary ammonium polyarylethernitrile anion exchange membrane and a preparation method and application thereof. Background Art

[0002] Fuel cell technology is considered one of the most promising candidate technologies to address the impending energy crisis. Compared with proton exchange membrane fuel cells (PEMFCs), anion exchange membrane fuel cells (AEMFCs) operate under alkaline conditions, so they exhibit faster oxygen reduction kinetics and can use non-precious metal catalysts. As one of the key components, anion exchange membrane (AEM) has high hydroxide conductivity, excellent mechanical stability and alkaline stability, which will greatly affect the performance and life of AMFCs.

[0003] Polyarylethers, such as polyaryletherketones, polyarylethersulfones, partially fluorinated polyarylethers, and polyarylethernitriles, are the most widely used aromatic polymers in AEMs, with good mechanical and thermal stability. They can be synthesized by nucleophilic aromatic substitution (SNAr). In addition, functionalization by conventional synthetic routes of chloromethylation / bromination quaternization usually introduces cations adjacent to the arylether bond (ortho position of the C=O bond). However, these arylether-containing AEMs may undergo arylether cleavage under alkaline conditions, resulting in main chain degradation. Therefore, the introduction of polyelectrolytes without arylethers has been shown to be an effective method to prevent polymer main chain degradation. However, they usually result in brittle membranes without flexible arylether bonds in the polymer main chain, and require special monomers, noble metal catalysts, and complex synthesis processes, which limits their practical applications. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a quaternized poly(arylether nitrile) anion exchange membrane and its preparation method and application in view of the problems existing in the prior art. Among them, the quaternized poly(arylether nitrile) anion exchange membrane modified by benzimidazole includes a skeleton without electron-withdrawing linking groups and a para-quaternary ammonium group structure of the ether oxygen group, which can effectively enhance the electron cloud density and steric hindrance of the arylether carbon and the benzyl carbon, inhibit the attack of OH- on them, increase the reaction activation energy of the arylether cracking and the degradation of the quaternary ammonium group, and improve the ion conductivity. The remaining C-NH 2 There is a strong hydrogen bond between the groups, and the formed hydrogen bond network can effectively improve the mechanical properties of the membrane.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] Considering that electron-withdrawing linkages and adjacent cationic groups can enhance the electrophilicity of the aromatic carbon atom linked to the ether, promoting and accelerating the OH −Therefore, the present invention grafts the polymer backbone of the pendant ortho-type cation with a flexible spacer to reduce the aryl ether cleavage caused by the adjacent cationic group and improve the alkaline stability.

[0007] In addition, benzimidazole has excellent chemical stability due to the resonance effect. The present invention introduces benzimidazole into the quaternized poly(arylethernitrile) anion exchange membrane to further improve the alkali stability.

[0008] The second object of the present invention is to provide a method for preparing the quaternized poly(arylene ether nitrile) anion exchange membrane as described above.

[0009] A method for preparing a quaternized polyarylethernitrile anion exchange membrane comprises the following steps: firstly preparing tetramethyl polyaryletherketonenitrile, then subjecting the tetramethyl polyaryletherketonenitrile to bromomethylation with a brominating agent, then converting the electron-withdrawing carbonyl group in the main chain of the bromomethylated polyaryletherketonenitrile into an electron-donating amine group through a Leuckart reaction, then subjecting the amine group to one-step quaternization through a Menshutkin reaction, and finally introducing benzimidazole into the quaternized polyarylethernitrile anion exchange membrane to obtain the quaternized polyarylethernitrile anion exchange membrane.

[0010] It is worth noting that the anion exchange membrane as a core component of the alkaline membrane fuel cell is required to have good chemical stability. Benzimidazole has excellent chemical stability due to the resonance effect. The present invention introduces benzimidazole into the quaternized polyarylethernitrile anion exchange membrane. On the basis of retaining the aromatic structure of the main chain polyarylethernitrile, it is converted into an amine group through a novel Leuckart reaction and a carbonyl reaction of the main chain. The operation is simple, and at the same time, the key triggering factors such as the electron-withdrawing linking group and the etheroxy ortho-position cationic group that cause the cleavage of the aromatic ether are eliminated. Therefore, the structure designed by the present invention that does not contain an electron-withdrawing linking group skeleton and an etheroxy para-position quaternary ammonium group can effectively enhance the electron cloud density and steric hindrance of the aromatic ether carbon and benzyl carbon, inhibit the attack of OH- on it, increase the reaction activation energy of aromatic ether cleavage and quaternary ammonium group degradation, and improve the ion conductivity. The remaining C-NH 2 There is a strong hydrogen bond between the groups, and the formed hydrogen bond network can effectively improve the mechanical properties of the membrane.

[0011] Furthermore, the preparation method comprises the following steps:

[0012] (1) Preparation of tetramethyl poly(aryletherketonenitrile): Use solvent A to dissolve appropriate amounts of 3,3',5,5'-tetramethyl-4,4'-biphenol, 4,4'-difluorobenzophenone, 2,6-difluorobenzonitrile and anhydrous potassium carbonate in sequence, introduce nitrogen to remove air in the reaction system, and add a certain amount of solvent B in the water separator; heat the system to 140°C, and dehydrate for 3 h to remove the water generated during the reaction; after releasing the water in the water separator, increase the system temperature to 170°C, and the viscosity of the liquid in the system continues to increase. After about 10 h, the viscosity of the system no longer changes. Pour the polymer solution into deionized water to precipitate an off-white fibrous polymer. The precipitate is crushed, washed with deionized water and ethanol for several times, and placed in a 100°C vacuum oven for drying for later use. The collected polymer tetramethyl poly(aryletherketonenitrile) is named TMPAEK;

[0013] (2) Synthesis of bromomethylated poly(aryletherketonenitrile): Tetramethyl poly(aryletherketonenitrile) was dissolved in solvent C. After the polymer was completely dissolved, a brominating agent with a concentration of 0.57 w / v% and an initiator with a concentration of 0.078 w / v% were added. Under the protection of nitrogen atmosphere, the system was heated to reflux temperature and maintained for 12 h. After the reaction was completed, the polymer was discharged into precipitating agent A to precipitate a slightly yellow flocculent polymer. The polymer was broken and washed several times with precipitating agent A, and dried in a vacuum oven at 80°C for later use. The collected polymer, bromomethylated poly(aryletherketonenitrile), was named BrPEKN.

[0014] (3) Synthesis of polyaryletheramine by BrPEKN modified by Leuckart reaction: BrPEKN was dissolved in solvent D and heated to 160°C. 4.5 mL of formic acid was added dropwise to the mixture and stirred continuously for 24 h. After cooling to room temperature, the product was precipitated with precipitating agent B and washed several times. 50 mL of precipitating agent B was added to the reaction product. Then, 100 mL of 15 wt% HCl solution was added dropwise and the mixture was stirred at 80°C for 96 h. After cooling to room temperature, the product was precipitated and washed with 0.53 mol KOH solution and deionized water until pH = 7. Finally, the product was vacuum dried at 60°C overnight.

[0015] (4) Menshutkin quaternization reaction: the polyaryletheramine obtained in step (3) is dissolved in solvent E to obtain a solution with a concentration of 11 wt%, and then a certain proportion of methyl iodide is added to the solution, and the reaction is carried out at 40°C for a period of time, and then an equimolar equivalent of sodium bicarbonate is added, and the reaction is continued at 40°C for 24 hours, and the product is precipitated with a precipitation agent C and washed with deionized water several times, and then the product is vacuum dried at 60°C overnight;

[0016] (5) Preparation of benzimidazole functionalized quaternized poly(arylether nitrile) anion exchange membrane: benzimidazole is added in an amount of 1-3 times the amount of quaternized poly(arylether amine), and the reaction is carried out at a temperature of 80°C for 24 hours. After the reaction is completed, the membrane is precipitated with a precipitating agent D, and repeatedly washed in the agent for 3 times, placed in a vacuum oven at 60°C for drying overnight, taken out and dissolved in a solvent again, and a solution of a certain concentration is prepared, namely, a casting solution. The casting solution is placed on a glass plate by a solution casting method, dried, and the membrane is peeled off from the plate, placed under alkaline conditions for 48 hours, ion exchange is carried out, and deionized water is washed until neutral to obtain the quaternized poly(arylether nitrile) anion exchange membrane.

[0017] Furthermore, the solvent A in step (1) is a mixed solution of dimethyl sulfoxide and toluene in a volume ratio of 3:1, and the solvent B is toluene;

[0018] According to the mass / volume ratio, the concentration of 3,3',5,5'-tetramethyl-4,4'-biphenol is 1.21~1.25 w / v%, the concentration of 4,4'-difluorobenzophenone is 1.09~1.125 w / v%, the concentration of 2,6-difluorobenzonitrile is 18 w / v%, and the concentration of anhydrous potassium carbonate is 0.69~0.75 w / v%.

[0019] Furthermore, the solvent C in step (2) is chloroform, the concentration of tetramethyl poly(aryletherketonenitrile) is 0.84-0.90 w / v %, the bromination reagent is N-bromosuccinimide, and the initiator is benzoyl peroxide.

[0020] Furthermore, in the step (3), the solvent D is N,N-dimethylformamide and N,N-dimethylacetamide in a volume ratio of 3:1, the concentration of the bromomethylated poly(aryletherketonenitrile) is 0.4 w / v%, and the precipitation agent B is ethanol.

[0021] Furthermore, in step (4), the solvent E is dimethyl sulfoxide and the precipitating agent C is ethyl acetate.

[0022] Furthermore, the precipitation agent D in step (5) is N,N-dimethylformamide.

[0023] The third object of the present invention is to provide an application of the quaternized poly(arylene ether nitrile) anion exchange membrane as described above.

[0024] The invention discloses an application of a quaternized polyarylethernitrile anion exchange membrane in the preparation of fuel cell related materials and related devices.

[0025] It is worth noting that the benzimidazole-modified quaternary ammonium poly(arylether nitrile) functionalized anion exchange membrane disclosed in the present invention has high proton conductivity, excellent mechanical properties and suppressed swelling rate, and therefore has excellent application prospects in the preparation of fuel cell related materials and related devices.

[0026] Compared with the prior art, in order to solve the problem of poor alkali resistance of the main chain of polyarylether anion exchange membranes, the present invention discloses and prepares a highly alkali-resistant anion exchange membrane whose main chain does not contain electron-withdrawing groups and has a para-quaternary ammonium group structure of etheroxy groups, eliminating key triggering factors such as electron-withdrawing linking groups and etheroxy ortho-cationic groups that cause aromatic ether cracking. This strategy does not require precious metal catalysts, and the subsequent quaternization process is simple.

[0027] Considering that the anion exchange membrane as the core component of the alkaline membrane fuel cell is required to have good chemical stability. Benzimidazole has excellent chemical stability due to the resonance effect. The present invention introduces benzimidazole into the quaternized polyarylethernitrile anion exchange membrane, and on the basis of retaining the aromatic structure of the main chain polyarylethernitrile, it is converted into an amine group through a novel Leuckart reaction and a carbonyl reaction of the main chain. The operation is simple, and at the same time, the key triggering factors such as the electron-withdrawing linking group and the etheroxy ortho-position cationic group that cause the cleavage of the aromatic ether are eliminated. Therefore, the structure designed by the present invention that does not contain an electron-withdrawing linking group skeleton and an etheroxy para-position quaternary ammonium group can effectively enhance the electron cloud density and steric hindrance of the aromatic ether carbon and benzyl carbon, inhibit the attack of OH- on it, increase the reaction activation energy of aromatic ether cleavage and quaternary ammonium group degradation, and improve the ion conductivity. The remaining C-NH 2 There is a strong hydrogen bond between the groups, and the formed hydrogen bond network can effectively improve the mechanical properties of the membrane.

[0028] Therefore, the benzimidazole-modified quaternized poly(arylether nitrile) functionalized anion exchange membrane disclosed in the present invention has high proton conductivity, excellent mechanical properties and suppressed swelling rate, and has excellent application prospects in the preparation of fuel cell related materials and related devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without creative work.

[0030] Figure 1 Graph showing the coulombic efficiency of different anion exchange membranes of the present invention.

[0031] Figure 2Graph showing the energy efficiency of different anion exchange membranes of the present invention. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.

[0034] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.

[0035] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.

[0036] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.

[0037] The invention provides a quaternized polyarylether nitrile anion exchange membrane and a preparation method thereof. The main preparation steps include: preparing a tetramethyl polyarylether ketone nitrile polymer PAEKN; preparing a bromomethylated polyarylether ketone nitrile polymer BrPEKN; and, through a Leuckart reaction, converting the electron-withdrawing carbonyl group in the main chain of the bromomethylated polyarylether ketone nitrile into an electron-donating group amine group, and then quaternizing the amine group in one step through a Menshutkin reaction. Finally, benzimidazole is introduced into the quaternized polyarylether nitrile anion exchange membrane to obtain a quaternized polyarylether nitrile anion exchange membrane.

[0038] In order to better understand the present invention, the present invention is further specifically described through the following examples, but it should not be understood as limiting the present invention. Some non-essential improvements and adjustments made by technicians in this field according to the above invention content are also considered to fall within the protection scope of the present invention. Example 1

[0039] (1) Preparation of tetramethyl poly(aryletherketonenitrile): 3,3',5,5'-tetramethyl-4,4'-biphenyldiphenol (w / v concentration of 1.21%), 4,4'-difluorobenzophenone (w / v concentration of 1.09%~1.125%), 2,6-difluorobenzonitrile (w / v concentration of 18%), and anhydrous potassium carbonate (w / v concentration of 0.69%) were dissolved in a mixed solvent of 60 mL of dimethyl sulfoxide and 20 mL of toluene. Nitrogen was introduced to remove the air in the reaction system, and a certain amount of toluene solution was added to the water separator. The system temperature was heated to 140°C, and the dehydration reaction was carried out for 3 h to remove the water generated during the reaction. After the water in the water separator was released, the system temperature was raised to 170°C. The viscosity of the liquid in the system continued to increase. After about 10 h, the viscosity of the system no longer changed. The polymer solution was poured into deionized water to precipitate an off-white fibrous polymer. The precipitate was crushed, washed with deionized water and ethanol and refluxed several times, and dried in a vacuum oven at 100°C for later use. The collected polymer was named TMPAEK.

[0040] (2) Synthesis of bromomethylated poly(aryletherketonenitrile): Tetramethyl poly(aryletherketonenitrile) was dissolved in chloroform (0.84% ​​w / v solution). After the polymer was completely dissolved, 0.57% w / v bromination reagent N-bromosuccinimide and 0.078% w / v initiator benzoyl peroxide were added. Under nitrogen atmosphere, the system was heated to reflux temperature and maintained for 12 h. After the reaction was completed, the polymer was discharged into acetone to precipitate a slightly yellow flocculent polymer. The polymer was broken up and washed with acetone several times, dried in a vacuum oven at 80°C and set aside. The collected polymer was named BrPEKN.

[0041] (3) Synthesis of polyaryletheramines by Leuckart reaction-modified BrPEKN: The above reaction product was dissolved in a mixed solvent of 20 mL of N,N-dimethylformamide and 5 mL of N,N-dimethylacetamide to a w / v concentration of 0.4%, and heated to 160°C. Next, 4.5 mL of formic acid was added dropwise to the above mixture, and then stirred continuously for 24 h. After cooling to room temperature, the product was precipitated with ethanol and washed several times. 50 mL of ethanol was added to the reaction product. Next, 100 mL of HCl solution (15 wt%) was added dropwise, and the mixture was stirred at 80°C for 96 h. After cooling to room temperature, the product was precipitated and washed with KOH solution (0.53 mol) and deionized water until pH = 7. Finally, the product was vacuum dried at 60°C overnight.

[0042] (4) Menshutkin quaternization reaction: The dried poly(aryletheramine) was dissolved in dimethyl sulfoxide to obtain a solution with a concentration of 11 wt%, and then a certain proportion of methyl iodide was added to the solution. The reaction was carried out at 40°C for a period of time, and then an equimolar amount of sodium bicarbonate was added and the reaction was continued at 40°C for 24 h. After precipitation with ethyl acetate and washing with deionized water several times, the product was vacuum dried at 60°C overnight.

[0043] (5) Preparation of benzimidazole functionalized quaternized poly(arylether nitrile) anion exchange membrane: benzimidazole was added in an amount of 1-3 times the amount of quaternized poly(arylether amine), and the reaction was carried out at a temperature of 80°C for 24 h. After the reaction was completed, it was precipitated with N,N-dimethylformamide and repeatedly washed in the reagent for 3 times. It was placed in a vacuum oven at 60°C for drying overnight. It was taken out and dissolved in a solvent again to prepare a solution of a certain concentration, which was the casting solution. The casting solution was placed on a glass plate by solution casting, dried, and the membrane was peeled off from the plate and placed under alkaline conditions for 48 h for ion exchange. It was washed with deionized water until neutral to obtain a high alkaline stability benzimidazole quaternized poly(arylether nitrile) anion exchange membrane M1.

[0044] The ion exchange capacity of the obtained quaternary ammonium poly(arylether nitrile) anion exchange membrane M1 is 2.55 mol·g -1 , the swelling degree is 6.5%. Assembled into a battery, at 100 mA·cm -2 The coulombic efficiency of the lower battery is 94.8%, the energy efficiency is 83.5%, and the voltage efficiency is 86.4%. Example 2

[0045] (1) Preparation of tetramethyl poly(aryletherketonenitrile): 3,3',5,5'-tetramethyl-4,4'-biphenyldiphenol (w / v concentration of 1.22% solution), 4,4'-difluorobenzophenone (w / v concentration of 1.09875% solution), 2,6-difluorobenzonitrile (w / v concentration of 18%), and anhydrous potassium carbonate (w / v concentration of 0.705%) were dissolved in a mixed solvent of 60 mL of dimethyl sulfoxide and 20 mL of toluene. Nitrogen was introduced to remove the air in the reaction system, and a certain amount of toluene solution was added to the water separator. The system temperature was heated to 140°C, and the dehydration reaction was carried out for 3 h to remove the water generated during the reaction. After the water in the water separator was released, the system temperature was raised to 170°C. The viscosity of the liquid in the system continued to increase. After about 10 h, the viscosity of the system no longer changed. The polymer solution was poured into deionized water to precipitate an off-white fibrous polymer. The precipitate was crushed, washed with deionized water and ethanol and refluxed several times, and dried in a vacuum oven at 100°C for later use. The collected polymer was named TMPAEK.

[0046] (2) Synthesis of bromomethylated poly(aryletherketonenitrile): Tetramethyl poly(aryletherketonenitrile) was dissolved in chloroform (0.85% w / v solution). After the polymer was completely dissolved, 0.57% w / v bromination reagent N-bromosuccinimide and 0.078% w / v initiator benzoyl peroxide were added. Under nitrogen atmosphere, the system was heated to reflux temperature and maintained for 12 h. After the reaction was completed, the polymer was discharged into acetone to precipitate a slightly yellow flocculent polymer. The polymer was broken up and washed with acetone several times, dried in a vacuum oven at 80°C and set aside. The collected polymer was named BrPEKN.

[0047] (3) Synthesis of polyaryletheramines by BrPEKN modified by Leuckart reaction: The above reaction product was dissolved in a mixed solvent of 20 mL of N,N-dimethylformamide and 5 mL of N,N-dimethylacetamide to a w / v concentration of 0.4% and heated to 160°C. Next, 4.5 mL of formic acid was added dropwise to the above mixture, and then stirred continuously for 24 h. After cooling to room temperature, the product was precipitated with ethanol and washed several times. 50 mL of ethanol was added to the reaction product. Next, 100 mL of HCl solution (15 wt%) was added dropwise, and the mixture was stirred at 80°C for 96 h. After cooling to room temperature, the product was precipitated and washed with KOH solution (0.53 mol) and deionized water until pH = 7. Finally, the product was vacuum dried at 60°C overnight.

[0048] (4) Menshutkin quaternization reaction: The dried poly(aryletheramine) was dissolved in dimethyl sulfoxide to obtain a solution with a concentration of 11 wt%, and then a certain proportion of methyl iodide was added to the solution. The reaction was carried out at 40°C for a period of time, and then an equimolar amount of sodium bicarbonate was added and the reaction was continued at 40°C for 24 h. After precipitation with ethyl acetate and washing with deionized water several times, the product was vacuum dried at 60°C overnight.

[0049] (5) Preparation of benzimidazole functionalized quaternized poly(arylether nitrile) anion exchange membrane: benzimidazole was added in an amount of 1-3 times the amount of quaternized poly(arylether amine), and the reaction was carried out at a temperature of 80°C for 24 h. After the reaction was completed, it was precipitated with N,N-dimethylformamide and repeatedly washed in the reagent for 3 times. It was placed in a vacuum oven at 60°C and dried overnight. It was taken out and dissolved in a solvent again to prepare a solution of a certain concentration, which was the casting solution. The casting solution was placed on a glass plate by solution casting, dried, and the membrane was peeled off from the plate and placed under alkaline conditions for 48 h for ion exchange. It was washed with deionized water until neutral to obtain a high alkaline stability benzimidazole quaternized poly(arylether nitrile) anion exchange membrane M2.

[0050] The ion exchange capacity of the obtained quaternary ammonium poly(arylether nitrile) anion exchange membrane M2 is 2.65 mol·g -1 , the swelling degree is 10.5%. Assembled into a battery, at 100 mA·cm -2 The coulombic efficiency of the lower battery is 96.5%, the energy efficiency is 84.2%, and the voltage efficiency is 86.8%. Example 3

[0051] (1) Preparation of tetramethyl poly(aryletherketonenitrile): 3,3',5,5'-tetramethyl-4,4'-biphenyldiphenol (w / v concentration of 1.23% solution), 4,4'-difluorobenzophenone (w / v concentration of 1.1075% solution), 2,6-difluorobenzonitrile (w / v concentration of 18%), and anhydrous potassium carbonate (w / v concentration of 0.72%) were dissolved in a mixed solvent of 60 mL of dimethyl sulfoxide and 20 mL of toluene. Nitrogen was introduced to remove the air in the reaction system, and a certain amount of toluene solution was added to the water separator. The system temperature was heated to 140°C, and the dehydration reaction was carried out for 3 h to remove the water generated during the reaction. After the water in the water separator was released, the system temperature was raised to 170°C. The viscosity of the liquid in the system continued to increase. After about 10 h, the viscosity of the system no longer changed. The polymer solution was poured into deionized water to precipitate an off-white fibrous polymer. The precipitate was crushed, washed with deionized water and ethanol and refluxed several times, and dried in a vacuum oven at 100°C for later use. The collected polymer was named TMPAEK.

[0052] (2) Synthesis of bromomethylated poly(aryletherketonenitrile): Dissolve tetramethyl poly(aryletherketonenitrile) (0.87% w / v solution) in chloroform. After the polymer is completely dissolved, add 0.57% w / v bromination reagent N-bromosuccinimide and 0.078% w / v initiator benzoyl peroxide. Under nitrogen atmosphere, heat the system to reflux temperature and maintain for 12 h. After the reaction is completed, discharge the polymer into acetone to precipitate a slightly yellow flocculent polymer. Crush the polymer and wash it with acetone several times. Dry it in a vacuum oven at 80°C for later use. The collected polymer is named BrPEKN.

[0053] (3) Synthesis of polyaryletheramines by BrPEKN modified by Leuckart reaction: The above reaction product was dissolved in a mixed solvent of 20 mL of N,N-dimethylformamide and 5 mL of N,N-dimethylacetamide to a w / v concentration of 0.4% and heated to 160°C. Next, 4.5 mL of formic acid was added dropwise to the above mixture, and then stirred continuously for 24 h. After cooling to room temperature, the product was precipitated with ethanol and washed several times. 50 mL of ethanol was added to the reaction product. Next, 100 mL of HCl solution (15 wt%) was added dropwise, and the mixture was stirred at 80°C for 96 h. After cooling to room temperature, the product was precipitated and washed with KOH solution (0.53 mol) and deionized water until pH = 7. Finally, the product was vacuum dried at 60°C overnight.

[0054] (4) Menshutkin quaternization reaction: The dried poly(aryletheramine) was dissolved in dimethyl sulfoxide to obtain a solution with a concentration of 11 wt%, and then a certain proportion of iodomethane was added to the solution. The reaction was carried out at 40 °C for a period of time, and then an equimolar amount of sodium bicarbonate was added and the reaction was continued at 40 °C for 24 h. After precipitation with ethyl acetate and washing with deionized water several times, the product was vacuum dried at 60 °C overnight.

[0055] (5) Preparation of benzimidazole functionalized quaternized poly(arylether nitrile) anion exchange membrane: Add benzimidazole, the amount of benzimidazole added is 1-3 times the amount of quaternized poly(arylether amine), react at a reaction temperature of 80°C for 24 h, after the reaction is completed, precipitate with N,N-dimethylformamide, and repeatedly wash in the reagent 3 times, place in a vacuum oven at 60°C to dry overnight, take out and dissolve in a solvent again, and prepare a solution of a certain concentration, which is the casting solution. The casting solution is placed on a glass plate by solution casting method, dried, and the membrane is peeled off from the plate, placed under alkaline conditions for 48 hours, ion exchange is carried out, and deionized water is washed to neutrality to obtain a high alkaline stability benzimidazole quaternized poly(arylether nitrile) anion exchange membrane M3.

[0056] The ion exchange capacity of the obtained quaternary ammonium poly(arylether nitrile) anion exchange membrane M3 is 2.85 mol·g -1 , the swelling degree is 11.3%. Assembled into a battery, at 100 mA·cm -2 The coulombic efficiency of the lower battery is 97.1%, the energy efficiency is 85.4%, and the voltage efficiency is 87.5%. Example 4

[0057] (1) Preparation of tetramethyl poly(aryletherketonenitrile): 3,3',5,5'-tetramethyl-4,4'-biphenyldiphenol (w / v concentration of 1.24% solution), 4,4'-difluorobenzophenone (w / v concentration of 1.11625% solution), 2,6-difluorobenzonitrile (w / v concentration of 18% solution), and anhydrous potassium carbonate (w / v concentration of 0.735% solution) were dissolved in a mixed solvent of 60 mL of dimethyl sulfoxide and 20 mL of toluene. Nitrogen was introduced to remove the air in the reaction system, and a certain amount of toluene solution was added to the water separator. The system temperature was heated to 140°C, and the dehydration reaction was carried out for 3 h to remove the water generated during the reaction. After the water in the water separator was released, the system temperature was raised to 170°C. The viscosity of the liquid in the system continued to increase. After about 10 h, the viscosity of the system no longer changed. The polymer solution was poured into deionized water to precipitate an off-white fibrous polymer. The precipitate was crushed, washed with deionized water and ethanol and refluxed several times, and dried in a vacuum oven at 100°C for later use. The collected polymer was named TMPAEK.

[0058] (2) Synthesis of bromomethylated poly(aryletherketonenitrile): Tetramethyl poly(aryletherketonenitrile) (w / v concentration of 0.885%) was dissolved in chloroform. After the polymer was completely dissolved, 0.57% w / v concentration of bromination reagent N-bromosuccinimide and 0.078% w / v concentration of initiator benzoyl peroxide were added. Under the protection of nitrogen atmosphere, the system was heated to reflux temperature and maintained for 12 h. After the reaction was completed, the polymer was discharged into acetone to precipitate a slightly yellow flocculent polymer. The polymer was broken and washed with acetone several times, dried in a vacuum oven at 80°C and set aside. The collected polymer was named BrPEKN.

[0059] (3) Synthesis of polyaryletheramines by modified BrPEKN by Leuckart reaction: The above reaction product was dissolved in a mixed solvent of 20 mL of N,N-dimethylformamide and 5 mL of N,N-dimethylacetamide to a w / v concentration of 0.4% and heated to 160°C. Next, 4.5 mL of formic acid was added dropwise to the above mixture, and then stirred continuously for 24 h. After cooling to room temperature, the product was precipitated with ethanol and washed several times. 50 mL of ethanol was added to the reaction product. Next, 100 mL of HCl solution (15 wt%) was added dropwise, and the mixture was stirred at 80°C for 96 h. After cooling to room temperature, the product was precipitated and washed with KOH solution (0.53 mol) and deionized water until pH = 7. Finally, the product was vacuum dried at 60°C overnight.

[0060] (4) Menshutkin quaternization reaction: The dried poly(aryletheramine) was dissolved in dimethyl sulfoxide to obtain a solution with a concentration of 11 wt%, and then a certain proportion of iodomethane was added to the solution. The reaction was carried out at 40 °C for a period of time, and then an equimolar amount of sodium bicarbonate was added and the reaction was continued at 40 °C for 24 h. After precipitation with ethyl acetate and washing with deionized water several times, the product was vacuum dried at 60 °C overnight.

[0061] (5) Preparation of benzimidazole functionalized quaternized poly(arylether nitrile) anion exchange membrane: benzimidazole was added in an amount of 1-3 times the amount of quaternized poly(arylether amine) and the reaction was carried out at a temperature of 80°C for 24 h. After the reaction was completed, it was precipitated with N,N-dimethylformamide and repeatedly washed in the reagent for 3 times. It was placed in a vacuum oven at 60°C and dried overnight. It was taken out and dissolved in a solvent again to prepare a solution of a certain concentration, which was the casting solution. The casting solution was placed on a glass plate by solution casting, dried, and the membrane was peeled off from the plate and placed under alkaline conditions for 48 h for ion exchange. It was washed with deionized water until neutral to obtain a high alkaline stability benzimidazole quaternized poly(arylether nitrile) anion exchange membrane M4.

[0062] The ion exchange capacity of the obtained quaternary ammonium poly(arylether nitrile) anion exchange membrane M4 was 2.81 mol·g -1 , the swelling degree is 9.5%. Assembled into a battery, at 100 mA·cm -2 The coulombic efficiency of the lower battery is 96.3%, the energy efficiency is 83.5%, and the voltage efficiency is 85.6%. Example 5

[0063] (1) Preparation of tetramethyl poly(aryletherketonenitrile): 3,3',5,5'-tetramethyl-4,4'-biphenyldiphenol (w / v concentration of 1.25% solution), 4,4'-difluorobenzophenone (w / v concentration of 1.125% solution), 2,6-difluorobenzonitrile (w / v concentration of 18%), and anhydrous potassium carbonate (w / v concentration of 0.75%) were dissolved in a mixed solvent of 60 mL of dimethyl sulfoxide and 20 mL of toluene. Nitrogen was introduced to remove the air in the reaction system, and a certain amount of toluene solution was added to the water separator. The system temperature was heated to 140°C, and the dehydration reaction was carried out for 3 h to remove the water generated during the reaction. After the water in the water separator was released, the system temperature was raised to 170°C. The viscosity of the liquid in the system continued to increase. After about 10 h, the viscosity of the system no longer changed. The polymer solution was poured into deionized water to precipitate an off-white fibrous polymer. The precipitate was crushed, washed with deionized water and ethanol and refluxed several times, and dried in a vacuum oven at 100°C for later use. The collected polymer was named TMPAEK.

[0064] (2) Synthesis of bromomethylated poly(aryletherketonenitrile): Dissolve tetramethyl poly(aryletherketonenitrile) (0.9% w / v solution) in chloroform. After the polymer is completely dissolved, add 0.57% w / v bromination reagent N-bromosuccinimide and 0.078% w / v initiator benzoyl peroxide. Under nitrogen atmosphere, heat the system to reflux temperature and maintain for 12 h. After the reaction is completed, discharge the polymer into acetone to precipitate a slightly yellow flocculent polymer. Crush the polymer and wash it with acetone several times. Dry it in a vacuum oven at 80°C for later use. The collected polymer is named BrPEKN.

[0065] (3) Synthesis of polyaryletheramines by modified BrPEKN by Leuckart reaction: The above reaction product was dissolved in a mixed solvent of 20 mL of N,N-dimethylformamide and 5 mL of N,N-dimethylacetamide to a w / v concentration of 0.4% and heated to 160°C. Next, 4.5 mL of formic acid was added dropwise to the above mixture, and then stirred continuously for 24 h. After cooling to room temperature, the product was precipitated with ethanol and washed several times. 50 mL of ethanol was added to the reaction product. Next, 100 mL of HCl solution (15 wt%) was added dropwise, and the mixture was stirred at 80°C for 96 h. After cooling to room temperature, the product was precipitated and washed with KOH solution (0.53 mol) and deionized water until pH = 7. Finally, the product was vacuum dried at 60°C overnight.

[0066] (4) Menshutkin quaternization reaction: The dried poly(aryletheramine) was dissolved in dimethyl sulfoxide to obtain a solution with a concentration of 11 wt%, and then a certain proportion of iodomethane was added to the solution. The reaction was carried out at 40 °C for a period of time, and then an equimolar amount of sodium bicarbonate was added and the reaction was continued at 40 °C for 24 h. After precipitation with ethyl acetate and washing with deionized water several times, the product was vacuum dried at 60 °C overnight.

[0067] (5) Preparation of benzimidazole functionalized quaternized poly(arylether nitrile) anion exchange membrane: benzimidazole was added in an amount of 1-3 times the amount of quaternized poly(arylether amine) and the reaction was carried out at a temperature of 80°C for 24 h. After the reaction was completed, the membrane was precipitated with N,N-dimethylformamide and repeatedly washed in the reagent for 3 times. The membrane was placed in a vacuum oven at 60°C and dried overnight. The membrane was taken out and dissolved in a solvent again to prepare a solution of a certain concentration, which was the casting solution. The casting solution was placed on a glass plate by solution casting and dried. The membrane was peeled off from the plate and placed under alkaline conditions for 48 h for ion exchange. The membrane was washed with deionized water until neutral to obtain a high alkaline stability benzimidazole quaternized poly(arylether nitrile) anion exchange membrane M5.

[0068] The ion exchange capacity of the obtained quaternary ammonium poly(arylether nitrile) anion exchange membrane M5 was 2.81 mol·g -1 , the swelling degree is 9.8%. Assembled into a battery, at 100 mA·cm -2 The coulombic efficiency of the lower battery is 96.5%, the energy efficiency is 83.9%, and the voltage efficiency is 85.4%.

[0069] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the application performance of the quaternized poly(arylether nitrile) anion exchange membrane disclosed in the present invention is further illustrated by the following comparative examples, but it should not be construed as a limitation of the present invention. Other determination experiments or comparative examples made by those skilled in the art based on the above-mentioned invention content and the application based on the above-mentioned properties are also considered to fall within the protection scope of the present invention.

[0070] Comparative Example 1

[0071] The cell was assembled with commercially available anion exchange membrane Nafion 212 and the current was 100 mA·cm -2 The following compares the coulombic efficiency and energy efficiency of the battery ( Figure 1 , Figure 2 ). It can be seen that compared with Examples 1-5, the commercial anion exchange membrane Nafion 212 is significantly lower than the quaternized poly(arylene ether nitrile) anion exchange membrane disclosed in the present invention.

[0072] Therefore, the benzimidazole-modified quaternized poly(arylether nitrile) functionalized anion exchange membrane disclosed in the present invention has high proton conductivity, excellent mechanical properties and suppressed swelling rate, and has excellent application prospects in the preparation of fuel cell related materials and related devices.

[0073] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a quaternized poly(arylene ether nitrile) anion exchange membrane, characterized in that: First, tetramethyl poly(aryletherketonenitrile) is prepared, and then the tetramethyl poly(aryletherketonenitrile) is subjected to bromomethylation reaction with N-bromosuccinimide, and then the electron-withdrawing carbonyl group in the main chain of the bromomethylated poly(aryletherketonenitrile) is converted into an electron-donating group amine group through Leuckart reaction, and then the amine group is quaternized in one step through Menshutkin reaction, and finally benzimidazole is introduced into the quaternized poly(aryletherketonenitrile) anion exchange membrane to obtain the quaternized poly(aryletherketonenitrile) anion exchange membrane; the specific steps include: (1) Preparation of tetramethyl poly(aryletherketonenitrile): Solvent A is used to dissolve appropriate amounts of 3,3',5,5'-tetramethyl-4,4'-biphenol, 4,4'-difluorobenzophenone, 2,6-difluorobenzonitrile and anhydrous potassium carbonate in sequence, nitrogen is introduced to remove the air in the reaction system, and a certain amount of solvent B is added to the water separator; the system temperature is heated to 140°C, and a dehydration reaction is carried out for 3 hours to remove the water generated during the reaction; after the water in the water separator is released, the system temperature is increased to 170°C, and the viscosity of the liquid in the system continues to increase. After 10 hours, the viscosity of the system no longer changes. The polymer solution is poured into deionized water to precipitate an off-white fibrous polymer. The precipitate is crushed, washed with deionized water and ethanol for several times, and then placed in a 100°C vacuum oven for drying for later use. The collected polymer tetramethyl poly(aryletherketonenitrile) is named TMPAEK; (2) Synthesis of bromomethylated poly(aryletherketonenitrile): Tetramethyl poly(aryletherketonenitrile) was dissolved in solvent C. After the polymer was completely dissolved, 0.57 w / v% N-bromosuccinimide and 0.078 w / v% initiator were added. Under nitrogen atmosphere, the system was heated to reflux temperature and maintained for 12 h. After the reaction was completed, the polymer was discharged into precipitating agent A to precipitate a slightly yellow flocculent polymer. The polymer was broken and washed several times with precipitating agent A, and dried in a vacuum oven at 80°C for later use. The collected polymer, bromomethylated poly(aryletherketonenitrile), was named BrPEKN. (3) Synthesis of polyaryletheramine by BrPEKN modified by Leuckart reaction: BrPEKN was dissolved in solvent D and heated to 160°C, 4.5 mL of formic acid was added dropwise to the mixture, and the mixture was stirred for 24 h. After cooling to room temperature, the product was precipitated with precipitating agent B and washed several times. 50 mL of precipitating agent B was added to the reaction product, and then 100 mL of 15 wt% HCl solution was added dropwise, and the mixture was stirred at 80°C for 96 h. After cooling to room temperature, the product was precipitated and washed with 0.53 mol KOH solution and deionized water until pH = 7. Finally, the product was vacuum dried at 60°C overnight. The solvent D was N,N-dimethylformamide and N,N-dimethylacetamide in a volume ratio of 3:

1. (4) Menshutkin quaternization reaction: the polyaryletheramine obtained in step (3) is dissolved in solvent E to obtain a solution with a concentration of 11 wt%, and then a certain proportion of methyl iodide is added to the solution, and the reaction is carried out at 40°C for a period of time, and then an equimolar equivalent of sodium bicarbonate is added, and the reaction is continued at 40°C for 24 hours, and the product is precipitated with a precipitation agent C and washed with deionized water several times, and then the product is vacuum dried at 60°C overnight; (5) Preparation of benzimidazole functionalized quaternized poly(arylether nitrile) anion exchange membrane: adding benzimidazole in an amount of 1-3 times the amount of quaternized poly(arylether amine), reacting at a temperature of 80°C for 24 h, and after the reaction, precipitating with a precipitating agent D, and repeatedly washing in the agent for 3 times, placing in a vacuum oven at 60°C for drying overnight, taking out and dissolving in a solvent again, and preparing a solution of a certain concentration, namely, a casting solution, placing the casting solution on a glass plate by a solution casting method, drying, peeling the membrane from the plate, placing it under alkaline conditions for 48 h, performing ion exchange, and washing with deionized water until neutral, thereby obtaining the quaternized poly(arylether nitrile) anion exchange membrane.

2. The preparation method according to claim 1, characterized in that: The solvent A in step (1) is a mixed solution of dimethyl sulfoxide and toluene in a volume ratio of 3:1, and the solvent B is toluene; According to the mass / volume ratio, the concentration of 3,3',5,5'-tetramethyl-4,4'-biphenol is 1.21~1.25 w / v%, the concentration of 4,4'-difluorobenzophenone is 1.09~1.125 w / v%, the concentration of 2,6-difluorobenzonitrile is 18 w / v%, and the concentration of anhydrous potassium carbonate is 0.69~0.75 w / v%.

3. The preparation method according to claim 1, characterized in that: The solvent C in step (2) is chloroform, the concentration of tetramethyl poly(aryletherketonenitrile) is 0.84-0.90 w / v %, and the initiator is benzoyl peroxide.

4. The preparation method according to claim 1, characterized in that: The concentration of the brominated poly(aryletherketonenitrile) in step (3) is 0.4 w / v%, and the precipitation agent B is ethanol.

5. The preparation method according to claim 1, characterized in that: In the step (4), the solvent E is dimethyl sulfoxide, and the precipitation agent C is ethyl acetate.

6. The preparation method according to claim 1, characterized in that: The precipitation agent D in the step (5) is N,N-dimethylformamide.