Al-Si series die-casting aluminum alloy, preparation method thereof, and heat dissipation structure
Through the preparation method of Al-Si die-cast aluminum alloy, combined with the reasonable proportioning and treatment of Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb, the mechanical properties and thermal conductivity of aluminum alloys in the prior art were solved. The difficult problem to take into account has achieved high-efficiency molding and excellent performance aluminum alloy materials.
Patent Information
- Application Number
- CN202410168157.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-02-05
AI Technical Summary
While the existing die-cast aluminum alloys improve yield strength, tensile strength and molding properties, it is difficult to meet the requirements of heat dissipation parts for thermal conductivity, making it difficult to optimize mechanical properties and thermal conductivity at the same time.
Using a preparation method of Al-Si-based die-cast aluminum alloy, Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb are added after heating the pure aluminum, and refining, slag removal, die-casting and aging are carried out. The composition content and ratio are controlled to form an alloy with excellent mechanical properties and thermal conductivity.
The thermal conductivity, mechanical properties and molding properties of Al-Si die-cast aluminum alloy are achieved, ensuring that the alloy has excellent thermal conductivity and mechanical properties on the basis of efficient molding, and is suitable for structural parts made of various processes.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to an Al-Si series die-casting aluminum alloy, a preparation method of the Al-Si series die-casting aluminum alloy, and a heat dissipation structure. Background Art
[0002] For die-cast aluminum alloys, it is usually necessary to sacrifice thermal conductivity to improve yield strength, tensile strength, formability, and elongation. This results in the heat sink being difficult to meet the heat dissipation performance requirements of the heat sink when the existing die-cast aluminum alloy is used to make the heat sink.
[0003] Therefore, there is an urgent need to develop a die-cast aluminum alloy with excellent thermal conductivity, mechanical properties, and forming properties. Summary of the invention
[0004] In view of the above-mentioned defects of the prior art, the present invention provides a method for preparing an Al-Si series die-casting aluminum alloy, aiming to obtain an Al-Si series die-casting aluminum alloy having excellent thermal conductivity, mechanical properties, and forming properties.
[0005] The present invention provides a method for preparing an Al-Si series die-casting aluminum alloy, comprising the following steps:
[0006] The pure aluminum is subjected to a first heating treatment to obtain pure aluminum liquid;
[0007] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb to the pure aluminum liquid, performing a second heating treatment, and obtaining an alloy liquid;
[0008] Refining and slagging the alloy liquid, and testing its composition and content; and
[0009] After the composition and content are qualified, the alloy liquid after the refining treatment and the slag removal treatment is subjected to die casting treatment and aging treatment to obtain an Al-Si die-casting aluminum alloy, wherein the Al-Si die-casting aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.0005-0.05% Cu by mass, 0.0005-0.06% Mg by mass, 0.005-0.04% Sr by mass, 0.0001-0.005% Zn by mass, 0.0001-0.001% Ni by mass, and 0.001-0.2% Sb by mass.
[0010] Further, the aging treatment temperature is 250° C. to 350° C., and the time is 0.05 h to 20 h; or
[0011] The aging treatment includes a primary low-temperature aging treatment, a secondary low-temperature aging treatment, and a tertiary high-temperature aging treatment, wherein the temperature of the primary low-temperature aging treatment is -100°C to -200°C, and the time is 1h to 15h; the temperature of the secondary low-temperature aging treatment is 0°C to 70°C, and the time is 1h to 24h; the temperature of the tertiary high-temperature aging treatment is 250°C to 350°C, and the time is 0.05h to 20h.
[0012] Furthermore, at least one of the following conditions is met:
[0013] The mass ratio of Si to Fe is 5-20:1;
[0014] The mass ratio of Si to Sr is 200-1500:1;
[0015] The mass ratio of Mg to Sb is 0.002-5:1;
[0016] The mass ratio of Mg, Cu, and Zn is 0.05-10:0.05-10:1;
[0017] The sum of the mass percentages of Cu, Mg, Zn, and Sb shall not exceed 0.22%;
[0018] The sum of the mass percentages of Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb shall not exceed 9%;
[0019] When the Al-Si series die-casting aluminum alloy contains Mn, Ti, Cr and V, the mass percentage content of Mn is 0.0001-0.0005%, the mass percentage content of Ti is 0.0001-0.0005%, the mass percentage content of Cr is 0.0001-0.0005%, the mass percentage content of V is 0.0001-0.0005%, and the sum of the mass percentage contents of Mn, Ti, Cr and V is not more than 0.002%;
[0020] The mass percentage content of a single impurity in the Al-Si series die-casting aluminum alloy is less than 0.009%, and the sum of the mass percentage content of the impurities is less than 0.05%.
[0021] Furthermore, the preparation method of the Al-Si based die-casting aluminum alloy also includes the step of adding at least one of In, Nb, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, and RE to the pure aluminum liquid.
[0022] Furthermore, at least one of the following conditions is met:
[0023] When the Al-Si die-casting aluminum alloy further contains 0-0.009% by mass of In, the mass ratio of Cu to In is 0.05-20:1;
[0024] When the Al-Si die-casting aluminum alloy further contains 0-0.005% by mass of Nb, the mass ratio of Ni to Nb is 0.025-10:1;
[0025] When the Al-Si die-casting aluminum alloy further contains Bi with a mass percentage content of 0-0.006%, the mass ratio of Mg to Bi is 1-400:1;
[0026] When the Al-Si die-casting aluminum alloy further contains Ge with a mass percentage content of 0-0.005%, the mass ratio of Si to Ge is 1000-2000:1;
[0027] When the Al-Si die-casting aluminum alloy further contains 0-0.005% by mass of Mo, the mass ratio of Si to Mo is 1500-2000:1;
[0028] When the Al-Si die-casting aluminum alloy further contains 0-0.005% Ag by mass, the mass ratio of Mg to Ag is 1-500:1, and the mass ratio of Cu to Ag is 1-400:1;
[0029] When the Al-Si die-casting aluminum alloy further contains 0-0.1% by mass of Sn and 0-0.005% by mass of Te, the mass ratio of Mg to Sn is 0.1-10:1, and the mass ratio of Te to Sn is 0.01-1:1;
[0030] When the Al-Si die-casting aluminum alloy further contains 0-0.01% Be by mass and 0-0.1% Co by mass, the mass ratio of Be, Co, and Fe is 0.001-0.03:0.004-0.25:1, and the mass ratio of Fe to Co is 1-250:1;
[0031] When the Al-Si die-casting aluminum alloy further contains 0-0.02% by mass of RE and 0-0.01% by mass of Cd, the mass ratio of RE, Sr, and Fe is 0.002-0.1:0.02-0.08:1, the mass ratio of RE to Cd is 0.1-25:1, and RE is at least one of La, Ce, Pr, Nd, Er, Sm, Y, and Gd.
[0032] The present invention also provides an Al-Si die-casting aluminum alloy obtained by the preparation method of the Al-Si die-casting aluminum alloy, wherein the Al-Si die-casting aluminum alloy contains aluminum, and also contains Si with a mass percentage content of 5-8%, Fe with a mass percentage content of 0.4-0.8%, Cu with a mass percentage content of 0.0005-0.05%, Mg with a mass percentage content of 0.0005-0.06%, Sr with a mass percentage content of 0.005-0.04%, Zn with a mass percentage content of 0.0001-0.005%, Ni with a mass percentage content of 0.0001-0.001%, and Sb with a mass percentage content of 0.001-0.2%.
[0033] Furthermore, the Al-Si die-casting aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.03% Sr by mass, 0.0001-0.001% Zn by mass, 0.0002-0.0008% Ni by mass, and 0.005-0.05% Sb by mass.
[0034] Furthermore, the Al-Si die-casting aluminum alloy also contains 0.0001-0.0003% by mass of Mn, 0.0001-0.0003% by mass of Ti, 0.0001-0.0003% by mass of Cr, and 0.0001-0.0003% by mass of V.
[0035] Furthermore, the Al-Si die-casting aluminum alloy also contains 0.0001-0.009% by mass of In, 0.0001-0.005% by mass of Nb, 0.0001-0.006% by mass of Bi, 0.0001-0.005% by mass of Ge, 0.0001-0.005% by mass of Mo, and 0. 0.0001-0.005% Ag, 0.0001-0.1% Sn, 0.0001-0.005% Te, 0.0001-0.01% Be, 0.001-0.1% Co, 0.001-0.01% Cd, and 0.001-0.02% RE.
[0036] The present invention also provides a heat dissipation structure, at least part of which is made of the Al-Si series die-casting aluminum alloy prepared by the preparation method of the Al-Si series die-casting aluminum alloy or the Al-Si series die-casting aluminum alloy.
[0037] In the technical solution of the present invention, the Al-Si die-cast aluminum alloy prepared by the preparation method of the Al-Si die-cast aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.0005-0.05% Cu by mass, 0.0005-0.06% Mg by mass, 0.005-0.04% Sr by mass, 0.0001-0.005% Zn by mass, 0.0001-0.001% Ni by mass, and 0.001-0.2% Sb by mass. Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb within the above content range interact with each other as a whole, and on the basis of ensuring that the Al-Si die-cast aluminum alloy has better formability, it also has excellent mechanical properties and thermal conductivity. The details are as follows:
[0038] (1) When the mass percentage content of Si is 5-8%, on the one hand, Si can improve the fluidity and density of the aluminum alloy, thereby improving the forming performance and mechanical properties of the aluminum alloy. On the other hand, Si can react with other elements as much as possible to form a second phase to avoid the adverse effect of Si dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Si can react with Al, Fe, Cu, Mg, Mn, etc. to form Mg2Si, AlFeSi, AlMnSi, AlFeSiCu, AlFeMgSi, AlFeMnSi and other second phases;
[0039] (2) When the mass percentage content of Fe is 0.4-0.8%, on the one hand, Fe can reduce the tendency of aluminum alloy castings to stick to the mold and improve the mechanical properties and thermal conductivity of the aluminum alloy. On the other hand, Fe can react with other elements as much as possible to form a second phase to avoid the adverse effect of Fe dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Fe can react with Al, Si, Mg, Cu, Mn, Ni, etc. to form Al3Fe, AlFeSi, AlFeMgSi, AlFeSiCu, AlFeSiNi, AlFeMgSiNi, AlFeMnSi, FeNiAl9 and other second phases;
[0040] (3) When the mass percentage of Cu is 0.0005-0.05%, on the one hand, Cu can improve the mechanical properties, thermal conductivity, and fatigue resistance of aluminum alloys. On the other hand, Cu can react with other elements to form a second phase as much as possible to avoid the adverse effect of Cu dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Cu can react with Al, Fe, Si, Mg, Zn, etc. to form second phases such as CuAl2, AlFeSiCu, Al2CuZn, (CuMg)Al2, etc. In addition, Cu can also promote the precipitation of second phases such as Mg2Si, Mg3Sb2, MgZn2, Mg2SiZn, (CuMg)Al2, AlFeMgSi, AlFeMgSiNi, etc., increase their volume fraction and dispersion, and reduce the solid solubility of the above elements in the aluminum matrix;
[0041] (4) When the mass percentage content of Mg is 0.0005-0.06%, on the one hand, Mg can improve the mechanical properties and thermal conductivity of the aluminum alloy, and on the other hand, Mg can react with other elements to form a second phase as much as possible to avoid the adverse effect of Mg dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Mg can react with Al, Fe, Si, Cu, Zn, Ni, Sb, etc. to form second phases such as Mg2Si, Mg3Sb2, Mg2Zn, Mg2SiZn, (CuMg)Al2, AlFeMgSi, AlFeMgSiNi, etc. In addition, Mg can also promote the precipitation of second phases such as CuAl2, AlFeSiCu, Al2CuZn, (CuMg)Al2, etc., increase their volume fraction and dispersion, and reduce the solid solubility of the above elements in the aluminum matrix;
[0042] (5) When the mass percentage of Sr is 0.005-0.04%, on the one hand, Sr can be modified through the heterogeneous nucleation theory or twin valley mechanism to refine the second phase such as eutectic silicon, improve the thermal conductivity and mechanical properties of the aluminum alloy, and also transform the β-AlFeSi phase in the ingot into the Chinese character α-AlFeSi phase to improve the mechanical properties of the aluminum alloy. On the other hand, Sr can preferentially combine with Fe, Cu, Mn, Cr, Si and other elements to form dispersion strengthening to avoid the adverse effect of Sr dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. In addition, Sr can also promote the precipitation of CuAl2, Mg2Si, Mg3Sb2 and other phases to reduce the solid solubility of these alloy elements in the aluminum matrix;
[0043] (6) When the mass percentage content of Zn is 0.0001-0.005%, on the one hand, Zn can improve the mechanical properties of aluminum alloys, and on the other hand, Zn can react with other elements to form a second phase as much as possible to avoid the adverse effect of Zn dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Zn can react with Al, Mg, Cu and Si to form second phases such as MgZn2, Mg2SiZn, Al2CuZn, etc. In addition, Zn can eliminate elemental Si to reduce the adverse effect of elemental Si on the performance of aluminum alloys. Zn can also promote the precipitation of phases such as Mg2Si, Al2Cu, Mg3Sb2, etc., to improve mechanical properties and thermal conductivity;
[0044] (7) When the mass percentage content of Ni is 0.0001-0.001%, on the one hand, Ni can be used to improve the mechanical properties and thermal conductivity of the aluminum alloy, and on the other hand, Ni can be made to react with other elements to form a second phase as much as possible to avoid the adverse effect of Ni dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Ni can react with Al, Fe, Mg, Si, etc. to form Al3Ni, AlFeSiNi, AlFeMgSiNi, FeNiAl9 and other second phases, which promote the precipitation of elements such as Cu, Mg, Zn, Si, Fe and other elements dissolved in the alloy; Ni can also refine the grains, promote the precipitation of strengthening phases such as CuAl2, (CuMg)Al2, Mg3Sb2, increase the volume fraction and dispersion of the precipitated phase, and reduce the solid solubility of the alloy elements in the aluminum matrix. In addition, Ni and Cu, Mg can promote each other's precipitation to improve the thermal conductivity and mechanical properties of the aluminum alloy;
[0045] (8) When the mass percentage of Sb is 0.0001-0.2%, on the one hand, Sb is added to act as a modifier in the aluminum alloy, which effectively reduces the size of the eutectic silicon layer, greatly reduces the possibility of splitting the matrix, and improves the mechanical properties of the alloy. At the same time, antimony has little effect on the electrical conductivity of the alloy. On the other hand, Sb can react with other elements such as Mg as much as possible to generate the second phase Mg3Sb2, so as to avoid the adverse effects of Sb, Mg and other elements dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy, and significantly improve the mechanical properties of the alloy. In addition, the addition of Sb can also increase the mutual precipitation of elements such as Cu, Zn, Ni, etc. that have a large solid solubility in the alloy matrix, further improving the mechanical properties and electrical conductivity of the alloy.
[0046] Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb in the above content range interact with each other as a whole, which can remove the content of transition elements Ti, Mn, Cr, and V in the aluminum matrix that have a great influence on thermal conductivity, and refine the grains, reduce the solid solubility of alloy elements in the aluminum matrix, and increase the volume fraction of the precipitated phase, so as to reduce the adverse effects of alloy elements on the thermal conductivity of the aluminum alloy and improve the comprehensive properties of the aluminum alloy (including mechanical properties, thermal conductivity, and forming properties, etc.). At the same time, under the further effect of aging treatment, the solid solubility of each element in the aluminum matrix is further reduced, which can eliminate the adverse effects of alloy elements on the thermal conductivity of the aluminum alloy as much as possible, and the second phase (such as Al3Fe, Mg2Si, Mg3Sb2, Al2Cu, AlFeSiNi, AlMnSi phase, etc.) can also be refined in the aluminum matrix and at the grain boundary or in the grain boundary, which greatly improves the mechanical properties and thermal conductivity of the aluminum alloy.
[0047] Specifically, since transition elements such as Mn, Cr, Ti, and V have a great influence on the thermal conductivity and mechanical properties of aluminum alloys, their content needs to be strictly controlled; when the amount of elements such as Cu, Mg, Zn, and Sb added is large, the thermal conductivity and mechanical properties of aluminum alloys will also be reduced, and their content also needs to be controlled; but when the mass percentage content of at least one of Si, Fe, Cu, Mg, Sr, Zn, Ni, Sb, Mn, Cr, Ti, and V is low, the elements with a low mass percentage content are not easy to precipitate, and will exist in the aluminum matrix in the form of solid solution, thereby reducing the thermal conductivity and mechanical properties of the aluminum alloy, and the refinement and modification effect of the aluminum alloy will also deteriorate, causing the single substance Si at the grain boundary of the aluminum alloy to exist in the form of coarse flakes and strips, seriously splitting the aluminum matrix, and further reducing the thermal conductivity and mechanical properties of the aluminum alloy. In the technical solution of the present invention, as described in the above items (1) to (8), Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb within the above content range interact with each other as a whole, which can refine the grains (such as the modification effect of Sr and the grain refining effect of Ni), reduce the solid solubility of each other in the aluminum matrix (such as the elements can react with each other to form a second phase), and increase the volume fraction of the precipitated phase (such as Cu, Mg, Sr, Zn, and Ni can promote the precipitation of the second phase), so as to improve the mechanical properties and thermal conductivity of the aluminum alloy; even if the mass percentage content of one or some elements is low, during the aging treatment process, all or almost all of the elements can be precipitated, avoiding adverse effects on the thermal conductivity of the aluminum alloy. DETAILED DESCRIPTION
[0048] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] The present invention also provides a method for preparing an Al-Si series die-casting aluminum alloy, comprising the following steps:
[0050] The pure aluminum is heated at a temperature of 720-780°C to obtain pure aluminum liquid;
[0051] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb to the pure aluminum liquid, and keeping the temperature at 700-750° C. for 10-30 minutes to obtain an alloy liquid;
[0052] After refining, degassing, and slagging the alloy liquid, the composition and content are tested; and
[0053] After the composition and content are qualified, the alloy liquid is subjected to die casting and aging treatment to obtain an Al-Si die casting aluminum alloy. The Al-Si die casting aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.0005-0.05% Cu by mass, 0.0005-0.06% Mg by mass, 0.005-0.04% Sr by mass, 0.0001-0.005% Zn by mass, 0.0001-0.001% Ni by mass, and 0.001-0.2% Sb by mass.
[0054] The pure aluminum may be industrial pure aluminum or high purity aluminum. Industrial pure aluminum is generally aluminum with a purity of 99.0-99.9%. The purity of high purity aluminum is generally greater than 99.8%. High purity aluminum can be further divided into sub-ultra-high purity aluminum (purity of 99.5-99.95%), ultra-high purity aluminum (purity of 99.996-99.999%) and extremely high purity aluminum (purity of more than 99.999%). Pure aluminum may generally contain impurities such as Mn, Ti, Cr, or V. Of course, it is not excluded that pure aluminum contains only aluminum and no impurities. The mass percentage content of a single impurity in the Al-Si die-casting aluminum alloy is less than 0.009%, preferably less than 0.0005%, and the sum of the mass percentage content of impurities is less than 0.01%, preferably less than 0.001%. It can be understood that when pure aluminum is used as an aluminum source, the impurities introduced into the alloy liquid can be minimized. When the Al-Si based die-casting aluminum alloy contains Mn, Ti, Cr and V, the mass percentage content of Mn may be 0.0001-0.0005%, the mass percentage content of Ti may be 0.0001-0.0005%, the mass percentage content of Cr may be 0.0001-0.0005%, the mass percentage content of V may be 0.0001-0.0005%, and the sum of the mass percentage contents of Mn, Ti, Cr and V is not more than 0.002%, preferably not more than 0.001%, and further preferably not more than 0.0005%.
[0055] At least one of Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb may be added in the form of an alloy or a single substance.
[0056] The sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb is not more than 9%, preferably not more than 8.5%, and more preferably not more than 8%. In this way, while ensuring the excellent thermal conductivity and mechanical properties of the aluminum alloy, it is avoided that too many elements are added to form a solid solution in the aluminum matrix. In one embodiment, the sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb is 5.5-9%, preferably 6-8%, and more preferably 6-7%, and specifically can be 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, or 9%.
[0057] The mass percentage content of Si can be 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, 7.6%, 7.7%, 7.8%, 7.9%, or 8%.
[0058] The mass percentage content of Fe can be 0.4%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49%, 0.5%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.5 9%, 0.6%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.7%, 0.71%, 0.72%, 0.73%, 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, or 0.8%.
[0059] The mass percentage content of Cu can be 0.0005%, 0.0006%, 0.0007%, 0.00058%, 0.0009%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, 0.02%, 0.021%, 0.022%, 0.023%, 0.024%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.030%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.040%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, 0.050%, 0.051%, 0.052%, 0.053%, 0.054%, 0.055%, 0.0 0.022%, 0.023%, 0.024%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.03%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.04%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, or 0.05%.
[0060] The mass percentage content of Mg can be 0.0005%, 0.0006%, 0.0007%, 0.0008%, 0.0009%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, 0.02%, 0.021%, 0.022%, 0.023%, 0.024%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.030%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.040%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, 0.050%, 0.051%, 0.052%, 0.053%, 0.054%, 0.055%, 0.056%, 0.057%, 0.058%, 0.059%, 0.060%, 0.061%, 0.062%, 0.063%, 0.064%, 0.065%, 0.066%, 0 0.027%, 0.028%, 0.029%, 0.03%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.04%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, 0.05%, 0.051%, 0.052%, 0.053%, 0.054%, 0.055%, 0.056%, 0.057%, 0.058%, 0.059%, or 0.06%.
[0061] The mass percentage content of Sr can be 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, 0.02%, 0.021%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.040%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, 0.050%, 0.051%, 0.052%, 0.053%, 0.054%, 0.055%, 0.056%, 0.057%, 0.058%, 0.059%, 0.060%, 0.061%, 0.062%, 0.063%, 0.064%, 0.065%, 0.066%, 0.067%, 0.068%, 0.069%, 0.070%, 0.071%, 0.072%, 0.073%, 0.074%, 0.075%, 0 .022%, 0.023%, 0.024%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.03%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, or 0.04%.
[0062] The mass percentage content of Zn may be 0.0001%, 0.0002%, 0.0003%, 0.0004%, 0.0005%, 0.0006%, 0.0007%, 0.0008%, 0.0009%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005%.
[0063] The mass percentage content of Ni may be 0.0001%, 0.0002%, 0.0003%, 0.0004%, 0.0005%, 0.0006%, 0.0007%, 0.0008%, 0.0009%, or 0.001%.
[0064] The mass percentage content of Sb may be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, or 0.2%.
[0065] The mass ratio of Si to Fe is 5-20:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Si to Fe is preferably 10-20:1, and more preferably the mass ratio of Si to Fe is 15-20:1, specifically 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, or 20:1.
[0066] The mass ratio of Si to Sr is 200-1500:1. Within the range of this mass ratio, as the mass ratio decreases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Si to Sr is preferably 500-1000:1, more preferably 700-800:1, and specifically can be 200:1, 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 550:1, 600:1, 650:1, 700:1, 750:1, 800:1, 850:1, 900:1, 950:1, 1000:1, 1100:1, 1200:1, 1300:1, 1400:1, or 1500:1.
[0067] The mass ratio of Mg to Sb is 0.002-5:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Mg to Sb is preferably 0.01-3:1, more preferably 0.1-1:1, and more preferably 0.1-0.5:1. Specifically, it can be 0.002:1, 0.003:1, 0.004:1, 0.005:1, 0.006:1, 0.007:1, 0.008:1, 0.009:1, 0.01:1, 0.02:1, 0.03:1, 0 .04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, or 5:1.
[0068] The mass ratio of Mg, Cu, and Zn is 0.05-10:0.05-10:1. Within the range of this mass ratio, as the mass ratio decreases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Mg, Cu, and Zn is preferably 0.1-5:0.1-5:1, and more preferably 1-2:1-2:1. Specifically, it can be 0.05:0.05:1, 0.05:0.1:1, 0.05:0.5:1, 0.05:1:1, 0.05:5:1, 0.05:10:1, 0.1:0.05:1, 0.1:0.1:1, 0.1:0.5:1, 0.1:1:1, 0.1:5:1, 0.1:10:1, 0.5:0.05:1, 0. 5:0.1:1, 0.5:0.5:1, 0.5:1:1, 0.5:5:1, 0.5:10:1, 1:0.05:1, 1:0.1:1, 1:0.5:1, 1:1:1, 1:5:1, 1:10:1, 5:0.05:1, 5:0.1:1, 5:0.5:1, 5:1:1, 5:5:1, 5:10:1, 10:0.05:1, 10:0.1:1, 10:0.5:1, 10:1:1, 10:5:1, or 10:10:1.
[0069] The sum of the mass percentage contents of Cu, Mg, Zn, and Sb is not greater than 0.2%, preferably 0.15%, and more preferably not greater than 0.12%. In one embodiment, the sum of the mass percentage contents of Cu, Mg, Zn, and Sb is 0.0021-0.3%, preferably 0.005-0.2%, and more preferably 0.05-0.15%, and specifically may be 0.0021%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.015%, 0.02%, 0.025%, 0.03%, 0.035%, 0.04%, 0.045%, 0.05%, 0.055%, 0.06%, 0.065%, 0.07%, 0.075%, 0.08%, 0.085%, 0.09%, 0.095%, 0.1%, 0.15%, or 0.2%.
[0070] The sum of the mass percentages of Cu, Mg, and Zn is no more than 0.115%, preferably 0.1%, and more preferably no more than 0.05%. In one embodiment, the sum of the mass percentages of Cu, Mg, Zn, and Sb is 0.0011-0.115%, preferably 0.005-0.1%, more preferably 0.01-0.1%, and even more preferably 0.05-0.1%.
[0071] The preparation method of the Al-Si series die-casting aluminum alloy also includes the step of adding at least one of In, Nb, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, and RE to the pure aluminum liquid. At least one of In, Nb, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, and RE can be added in the form of an alloy or a single substance.
[0072] The mass percentage content of In can be 0-0.009%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, or 0.009%. On the one hand, In can improve the mechanical properties of aluminum alloys, and on the other hand, In can react with other elements as much as possible to form a second phase to avoid the adverse effect of Si dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, In can react with Al and Cu to form second phases such as AlIn and CuIn. In addition, In can also refine the grains to improve the elongation of the aluminum alloy.
[0073] The mass ratio of Cu to In is 0.05-20:1. Within this mass ratio range, as the mass ratio increases, the mechanical properties of the aluminum alloy gradually increase. The mass ratio of Cu to In is preferably 0.1-15:1, more preferably 1-10:1, and still more preferably 5-10:1, and specifically may be 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, or 20:1.
[0074] The mass percentage content of Nb is 0-0.005%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005%. On the one hand, Nb can improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Nb can react with other elements to form a second phase as much as possible to avoid the adverse effect of Nb dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Nb can react with Ti and Al to form TiAl-Nb phase. In addition, Nb can also refine the grains to improve the elongation of the aluminum alloy.
[0075] The mass ratio of Ni to Nb is 0.025-10:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Ni to Nb is preferably 0.05-5:1, more preferably 0.1-1:1, specifically 0.025:1, 0.026:1, 0.027:1, 0.028:1, 0.029:1, 0.03:1, 0.05:1, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0. : 1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1, or 10:1.
[0076] The sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, Nb and Sb is 5.5-9%, preferably 6-8%, more preferably 6-7%, and specifically may be 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, or 9%.
[0077] The mass percentage content of Bi can be 0-0.006%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, or 0.006%. On the one hand, Bi can improve the mechanical properties of aluminum alloys, and on the other hand, Bi can react with other elements as much as possible to form a second phase to avoid the adverse effect of Bi dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Bi can react with Mg and Cd to form second phases such as Mg3Bi2 and Mg3(BiCd)2.
[0078] The mass ratio of Mg to Bi is 1-400:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties of the aluminum alloy gradually increase. The mass ratio of Mg to Bi is preferably 50-400:1, more preferably 100-300:1, and more preferably 150-200:1, and specifically can be 1:1, 5:1, 10:1, 50:1, 100:1, 150:1, 200:1, 250:1, 300:1, 350:1, or 400:1.
[0079] The mass percentage content of Ge is 0-0.005%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005%. On the one hand, Ge can improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Ge can react with other elements as much as possible to form a second phase to avoid the adverse effect of Ge dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Ge can react with Al and Si to form second phases such as Al9Ge7, Al6Ge5, Al5Ge2, Al3Ge4, SiGe, etc. In addition, Ge can promote the precipitation of second phases such as Mg2Si and CuAl2, refine the precipitation phase, and reduce the solubility of the above elements in the aluminum matrix. Ge can also replace part of Si atoms in the metastable precipitation phase. The Si-Ge phase precipitated at the initial stage of aging provides a nucleation site for the θ phase, increasing the density of the θ phase, to further improve the mechanical properties and thermal conductivity of the aluminum alloy.
[0080] The mass ratio of Si to Ge is 1000-2000:1. Within the range of this mass ratio, as the mass ratio decreases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Si to Ge is preferably 1000-1500:1, more preferably 1300-1500:1, and specifically can be 1000:1, 1100:1, 1200:1, 1300:1, 1400:1, 1500:1, 1600:1, 1700:1, 1800:1, 1900:1, 2000:1.
[0081] The mass percentage content of Mo is 0-0.005%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005%. On the one hand, Mo can improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Mo can react with other elements as much as possible to form a second phase to avoid the adverse effect of Ge dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Mo can react with Al, Si, Fe, etc. to form AlMo, AlSiMo, AlSiFeMo and other second phases, which are dispersed in the aluminum matrix grain boundaries. In addition, Mo can also refine the grains, improve the morphology of Fe-containing intermetallic compounds, and further improve the mechanical properties of aluminum alloys.
[0082] The mass ratio of Si to Mo is 1500-2000:1. Within the mass ratio range, as the mass ratio decreases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Si to Mo is preferably 1500-1800:1, more preferably 1500-1600:1, specifically 1500:1, 1600:1, 1700:1, 1800:1, 1900:1, or 2000:1.
[0083] The mass percentage content of Ag can be 0-0.005%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005%. Ag can promote the precipitation of the second phase (such as Al2Cu, Mg2Si, Mg2Sb, Mg3Sn2, and Mg3Bi2), refine the precipitation phase and increase the density of the precipitation phase, and enhance the precipitation strengthening effect of the aluminum alloy, thereby improving the mechanical properties and thermal conductivity of the aluminum alloy.
[0084] The mass ratio of Mg to Ag is 1-500:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Mg to Ag is preferably 50-400:1, more preferably 100-300:1, and more preferably 200-300:1. Specifically, it can be 1:1, 5:1, 10:1, 50:1, 100:1, 150:1, 200:1, 250:1, 300:1, 350:1, 400:1, 450:1, or 500:1.
[0085] The mass ratio of Cu to Ag is 1-400:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Cu to Ag is preferably 50-300:1, more preferably 100-200:1, and specifically can be 1:1, 5:1, 10:1, 50:1, 100:1, 150:1, 200:1, 250:1, 300:1, 350:1, or 400:1.
[0086] The mass percentage content of Sn can be 0-0.1%, specifically 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.015%, 0.02%, 0.025%, 0.03%, 0.035%, 0.04%, 0.045%, 0.05%, 0.055%, 0.06%, 0.065%, 0.07%, 0.075%, 0.08%, 0.085%, 0.09%, 0.095%, or 0.1%.
[0087] The mass percentage content of Te can be 0-0.005%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005%. Te can improve the mechanical properties and thermal conductivity of aluminum alloys. Te can narrow the solidification temperature range of aluminum alloys, form fine petal-shaped rather than dendritic primary crystals, reduce or eliminate micro-shrinkage, and thus improve the mechanical properties and thermal conductivity of aluminum alloys. Sn can improve the thermal conductivity of aluminum alloys, and can also react with other elements as much as possible to generate a second phase to avoid the adverse effect of Ge dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Sn can react with Al to generate a variety of high-temperature strengthening phases such as Al9Sn7, Al6Sn5, Al5Sn2, and Al3Sn4.
[0088] The mass ratio of Mg to Sn is 0.1-10:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Mg to Sn is preferably 0.5-8:1, more preferably 1-8:1, and more preferably 5-8:1, and specifically can be 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, or 10:1.
[0089] The mass ratio of Te to Sn is 0.01-1:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Te to Sn is preferably 0.05-1:1, more preferably 0.1-8:1, and more preferably 1-5:1, and specifically can be 0.01:1, 0.02:1, 0.04:1, 0.06:1, 0.08:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, or 1:1.
[0090] The mass percentage content of Be may be 0-0.01%, specifically 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, or 0.01%. Be can transform the eutectic Si phase from a lamellar phase into a fine phase to refine the Si phase, thereby reducing or eliminating the adverse effects of Si on aluminum alloys, and can transform the plate-like β intermediate phase into a relatively harmless Chinese character-shaped Be-Fe (Al8Fe2SiBe) phase to reduce or eliminate the adverse effects of Fe on the performance of aluminum alloys. Secondly, it can reduce the formation of Mg-containing Fe-rich phases, thereby increasing the Mg content participating in the aging process; Be can also combine with vacancies to prevent the migration and disappearance of vacancies. The addition of Be significantly increases the nucleation rate of the metastable phase, improves the strengthening effect of aging, and reduces the solid solubility of the above elements in the aluminum matrix; Ni and Be are complexed, which greatly promotes the precipitation of the second phase and reduces the solid solubility of alloy elements in the matrix.
[0091] The mass percentage content of Co can be 0-0.1%, specifically 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, or 0.1%. On the one hand, Co can refine the grains to improve the thermal conductivity and mechanical properties of the aluminum alloy. On the other hand, it can react with other elements to form a second phase as much as possible to avoid the adverse effect of Be dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Co can react with Al, Fe, Si, etc. to form Al 15 (Fe, Co)3Si2, Al3(Fe, Co) and other second phases. In addition, Co has a refining effect on the Al3Fe phase, transforming the coarse needle-shaped and flake-shaped β-Al3Fe phase into small flower-shaped and fine strip-shaped α-Al 15 (Fe,Co)3Si2 phase can also promote the α-Al 15 The precipitation of (Fe, Co)3Si2 phase further improves the mechanical properties and thermal conductivity of aluminum alloy. The composite addition of Ni and Co can effectively modify Fe and transform free Fe into the second phase. The composite addition of Co, Ni and Be can quickly reduce the solid solubility of each other in the alloy and increase the volume fraction of the second phase to improve the mechanical properties and thermal conductivity of aluminum alloy.
[0092] The mass ratio of Be, Co, and Fe is 0.001-0.03:0.004-0.25:1. Within this mass ratio range, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Be, Co, and Fe is preferably 0.005-0.02:0.005-0.2:1, more preferably 0.01-0.015:0.01-0.05:1, specifically 0.001:0.004:1, 0.001:0.01:1, 0.001:0.05:1, 0.001:0.1:1, 0.001:0.2:1, 0.001:0.25:1, 0.005:0.004:1, 0.005:0.01:1, 0.005:0.05:1, 0.005:0.1:1, 0.005:0.2:1, 0.005:0 .25:1, 0.01:0.004:1, 0.01:0.01:1, 0.01:0.05:1, 0.01:0.1:1, 0.01:0.2:1, 0.01:0.25:1, 0.02:0.004:1, 0.02:0.01:1, 0.02:0.05:1, 0.02:0.1:1, 0.02:0.2:1, 0.02:0.25:1, 0.03:0.004:1, 0.03:0.01:1, 0.03:0.05:1, 0.03:0.1:1, 0.03:0.2:1, or 0.03:0.25:1.
[0093] The mass ratio of Co, Ni, and Be is 0.1-10:0.001-1:1. Within this mass ratio range, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Co, Ni, and Be is preferably 0.5-5:0.01-1:1, more preferably 1-5:0.05-0.5:1, and still more preferably 1-3:0.1-0.3:1. Specifically, it can be 0.1:0.001:1, 0.1:0.005:1, 0.1:0.01:1, 0.1:0.05:1, 0.1:0.1:1, 0.1:0.5:1, 0.1:1:1, 0.5:0.001:1, 0.5:0.005:1, 0.5:0.01:1, 0.5:0.05:1, 0.5:0.1:1, 0.5:0.5:1, 0.5:1:1, 1:0.001:1, 1:0.005:1, 1:0.01:1, 1:0.05:1, 1:0.1:1, 1:0.5:1, 1:1:1, 5:0.001:1, 5:0.005:1, 5:0.01:1, 5:0.05:1, 5:0.1:1, 5:0.5:1, 5:1:1, 10:0.001:1, 10:0.005:1, 10:0.01:1, 10:0.05:1, 10:0.1:1, 10:0.5:1, or 10:1:1.
[0094] The mass ratio of Fe to Co is 1-250:1. Within this mass ratio range, as the mass ratio increases, the thermal conductivity of the aluminum alloy gradually increases. The mass ratio of Fe to Co is preferably 10-80:1, more preferably 30-50:1, and specifically can be 1:1, 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1, 55:1, 60:1, 65:1, 70:1, 75:1, 80:1, 85:1, 90:1, 95:1, 100:1, 110:1, 120:1, 130:1, 140:1, 150:1, 160:1, 170:1, 180:1, 190:1, 200:1, 210:1, 220:1, 230:1, 240:1, or 250:1.
[0095] The mass percentage content of RE is 0-0.02%, specifically 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, or 0.02%. RE is at least one of La, Ce, Pr, Nd, Er, Sm, Y, and Gd. RE can refine the alloy structure to improve the mechanical properties of aluminum alloy, and can also form a rare earth active film on the surface of the Fe-containing phase or combine with Al, Fe, Ti and other atoms to form rare earth compounds to effectively reduce the solid solution of harmful elements in the aluminum matrix. RE can also transform the long strip β-Fe phase into the spherical α-Fe phase and modify the elemental Si. RE can also promote the precipitation of dispersed phases such as CuAl2 and (CuMg)Al2, further improving the mechanical properties of aluminum alloys. RE can also refine grains, second phases and precipitated phases (for example, it can refine Al3RE, Al3Fe, Mg2Si phases, etc.), further improving the mechanical properties and thermal conductivity of aluminum alloys.
[0096] The mass percentage content of Cd is 0-0.01%, specifically 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, or 0.01%. Cd can refine α-Al, and can also form strengthening phases such as REAl2Cd3, Al3Cd, Al2Cd3, (CuCd)Al2, Mg2(SiCdREFe), Mg3(BiCd)2 with Al, RE, Cu, Mg, Si, Fe, Bi to reduce the solid solubility of each other in the aluminum matrix and increase the volume fraction of the precipitated phase. In addition, Cd will form a large number of Cd-vacancy clusters in the aging stage, promote and accelerate the precipitation of CuAl2 phase, and reduce the solid solubility of the above elements in the aluminum matrix.
[0097] The sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, Mo, In, Nb, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, RE, and Sb is 5.7-9.1%, preferably 6-9%, more preferably 6.5-7%, and specifically may be 5.7%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, or 9.1%.
[0098] The mass ratio of RE, Sr, and Fe is 0.002-0.1:0.02-0.08:1. Within the range of this mass ratio, as the mass ratio increases, the thermal conductivity and mechanical properties of the aluminum alloy gradually increase. The mass ratio of RE, Sr, and Fe is preferably 0.005-0.05:0.04-0.06:1, and more preferably 0.01-0.03:0.05-0.06:1, and specifically 0.002:0.02:1, 0.002:0.04:1, 0.002:0.06:1, 0.002:0.08:1, 0.005:0.02:1, 0.005:0.04:1, 0.005:0.0 6:1, 0.005:0.08:1, 0.01:0.02:1, 0.01:0.04:1, 0.01:0.06:1, 0.01:0.08:1, 0.05:0.02:1, 0.05:0.04:1, 0.05:0.06:1, 0.05:0.08:1, 0.1:0.02:1, 0.1:0.04:1, 0.1:0.06:1, or 0.1:0.08:1.
[0099] The mass ratio of RE to Cd is 0.1-25:1. Within the range of this mass ratio, as the mass ratio increases, the thermal conductivity and mechanical properties of the aluminum alloy gradually increase. The mass ratio of RE to Cd is preferably 1-20:1, more preferably 5-20:1, and more preferably 10-15:1, and specifically can be 0.1:1, 0.5:1, 1:1, 5:1, 10:1, 15:1, 20:1, or 25:1.
[0100] In one embodiment, the aging treatment is performed at a temperature of 250 to 350° C. and for a time of 0.05 to 20 hours. The temperature of the aging treatment may be 250°C, 255°C, 260°C, 265°C, 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, or 350°C; the time of the aging treatment may be 0.05h, 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, or 20h. During the aging treatment, the size of the precipitated phase gradually changes to a smaller size, and all or almost all of the alloying elements dissolved in the alloy are precipitated, increasing the pinning effect on dislocations and greatly improving the thermal conductivity and mechanical properties of the aluminum alloy.
[0101] In another embodiment, the aging treatment may also be referred to as a multi-stage aging treatment, including a primary low-temperature aging treatment, a secondary low-temperature aging treatment, and a tertiary high-temperature aging treatment. The temperature of the primary low-temperature aging treatment is -100°C to -200°C, and the time is 1h to 15h; the temperature of the secondary low-temperature aging treatment is 0°C to 70°C, and the time is 1h to 24h; the temperature of the tertiary high-temperature aging treatment is 250°C to 350°C, and the time is 0.05h to 20h. The temperature of the primary low-temperature aging treatment may be -200°C, -190°C, -180°C, -170°C, -160°C, -150°C, -140°C, -130°C, -120°C, -110°C, or -100°C. The time of the primary low-temperature aging treatment may be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, or 15h. The temperature of the secondary low-temperature aging treatment may be 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, or 70°C. The time of the secondary low-temperature aging treatment may be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, or 24h. The temperature of the three-stage high temperature aging treatment may be 250°C, 255°C, 260°C, 265°C, 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, or 350°C. The time of the three-stage high temperature aging treatment may be 0.05h, 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, or 20h.
[0102] During the first-level low-temperature aging treatment, deep cryogenic treatment can inhibit the segregation of atoms such as Mg, Cu, Ni and Si, and at the same time make the alloy produce a greater degree of supercooling, significantly increase the range of the GP zone, facilitate the subsequent high-temperature process nucleation rate to increase, and the alloy elements can be more fully precipitated. Aluminum alloys also undergo volume and lattice contraction during low-temperature processes, the supersaturation of alloy elements increases, solute atoms will precipitate in the alloy, and the content of alloy elements participating in aging will be increased. In addition, the reduction in the solubility of solute atoms will cause solute atoms to segregate at dislocations, significantly improving the formation of GP zones. During the second-level low-temperature aging treatment, the atomic segregation under the action of internal stress and dislocation will be uniformly diffused and dispersed in the aluminum matrix and grain boundaries. During the three-level high-temperature aging treatment, the GP zone gradually transforms into a precipitation phase with a smaller size but a larger volume fraction, and all or nearly all of the alloy elements dissolved in the alloy are precipitated, increasing the pinning effect on dislocations, greatly improving the thermal conductivity and mechanical properties of aluminum alloys.
[0103] The alloy liquid is subjected to die casting at a temperature of 660-700°C, wherein the die casting speed of the die casting machine is 0.23-2.5 m / s. It can be understood that the die casting process of the present invention is a common die casting process, and vacuum die casting can also be used to die cast the alloy liquid. The strength (such as yield strength and tensile strength) and elongation of the aluminum alloy after vacuum die casting will be higher than the strength (such as yield strength and tensile strength) and elongation of the aluminum alloy after common die casting.
[0104] The temperature of the refining treatment is 690-750°C and the time is 10-20 minutes. The refining agent of the refining treatment may include the following raw materials in parts by weight: 60-70 parts of KF, 50-60 parts of NaCl, 40-60 parts of LiCl, 20-25 parts of cryolite, 10-25 parts of AIF3, 10-15 parts of CaF2, 5-10 parts of light calcium carbonate, 15-20 parts of graphite powder, 10-20 parts of talc, 20-30 parts of MgCl2, and 10-30 parts of rare earth acid salt. The rare earth acid salt may be one of the chlorides, fluorides, and nitric acid compounds of light rare earths, or a combination thereof. The rare earth acid salt may be one of the chlorides, fluorides, and nitric acid compounds of heavy rare earths, or a combination thereof. The mass ratio of the refining agent to the alloy liquid is 0.0013-0.0018:1.
[0105] It is understandable that when the content of each component in the alloy liquid after degassing and slag removal treatment meets the standard, subsequent treatments such as die casting are carried out. Among them, the aluminum alloy that meets the standard contains Si with a mass percentage content of 5-8%, Fe with a mass percentage content of 0.4-0.8%, Cu with a mass percentage content of 0.0005-0.05%, Mg with a mass percentage content of 0.0005-0.06%, Sr with a mass percentage content of 0.005-0.04%, Zn with a mass percentage content of 0.0001-0.005%, Ni with a mass percentage content of 0.0001-0.001%, Sb with a mass percentage content of 0.001-0.2%, and Al. The aluminum alloy that meets the standard may also contain inevitable impurities. When the composition and content are unqualified, the corresponding elements can be added for adjustment until the composition and content are qualified.
[0106] In one embodiment, the Al-Si die-casting aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.03% Sr by mass, 0.0001-0.001% Zn by mass, 0.0002-0.0008% Ni by mass, and 0.005-0.05% Sb by mass.
[0107] In another embodiment, the Al-Si die-casting aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.009% Cu by mass, 0.003-0.009% Mg by mass, 0.02-0.04% Sr by mass, 0.001-0.005% Zn by mass, 0.0002-0.0005% Ni by mass, and 0.005-0.03% Sb by mass.
[0108] In another embodiment, the Al-Si die-casting aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.03% Sr by mass, 0.0001-0.001% Zn by mass, 0.0002-0.0008% Ni by mass, 0.005-0.03% Sb by mass, 0.0001-0.009% In by mass, 0.0001-0.00 5% Nb, 0.0001-0.006% Bi, 0.0001-0.005% Ge, 0.0001-0.005% Mo, 0.0001-0.005% Ag, 0.0001-0.1% Sn, 0.0001-0.005% Te, 0.0001-0.01% Be, 0.001-0.1% Co, 0.001-0.01% Cd, and 0.001-0.02% RE.
[0109] In another embodiment, the Al-Si die-casting aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.0005-0.05% Cu by mass, 0.0005-0.06% Mg by mass, 0.005-0.04% Sr by mass, 0.0001-0.005% Zn by mass, 0.0001-0.001% Ni by mass, 0.001-0.001% Sb by mass, 0.0001-0.0005% Mn by mass, 0.0001-0.0005% Ti by mass, 0.0001-0.0005% Cr by mass, and 0.0001-0.0005% V by mass.
[0110] In another embodiment, the Al-Si die-casting aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.0005-0.05% Cu by mass, 0.0005-0.06% Mg by mass, 0.005-0.04% Sr by mass, 0.0001-0.005% Zn by mass, 0.0001-0.001% Ni by mass, 0.001-0.001% Sb by mass, 0.0001-0.0005% Mn by mass, 0.0001-0.0005% Ti by mass, 0.0001-0.0005% Cr ... 0.005% V, 0.0001-0.009% In, 0.0001-0.005% Nb, 0.0001-0.006% Bi, 0.0001-0.005% Ge, 0.0001-0.005% Mo, 0.0001-0.005% Ag, 0.0001-0.005% Sn, 0.0001-0.005% Te, 0.0001-0.005% Be, 0.001-0.1% Co, 0.001-0.008% Cd, and 0.001-0.02% RE.
[0111] In the technical solution of the present invention, the Al-Si die-cast aluminum alloy prepared by the preparation method of the Al-Si die-cast aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.0005-0.05% Cu by mass, 0.0005-0.06% Mg by mass, 0.005-0.04% Sr by mass, 0.0001-0.005% Zn by mass, 0.0001-0.001% Ni by mass, and 0.001-0.2% Sb by mass. Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb within the above content range interact with each other as a whole, and on the basis of ensuring that the Al-Si die-cast aluminum alloy has better formability, it also has excellent mechanical properties and thermal conductivity. The details are as follows:
[0112] (1) When the mass percentage content of Si is 5-8%, on the one hand, Si can improve the fluidity and density of the aluminum alloy, thereby improving the forming performance and mechanical properties of the aluminum alloy. On the other hand, Si can react with other elements as much as possible to form a second phase to avoid the adverse effect of Si dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Si can react with Al, Fe, Cu, Mg, Mn, etc. to form Mg2Si, AlFeSi, AlMnSi, AlFeSiCu, AlFeMgSi, AlFeMnSi and other second phases;
[0113] (2) When the mass percentage content of Fe is 0.4-0.8%, on the one hand, Fe can reduce the tendency of aluminum alloy castings to stick to the mold and improve the mechanical properties and thermal conductivity of the aluminum alloy. On the other hand, Fe can react with other elements as much as possible to form a second phase to avoid the adverse effect of Fe dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Fe can react with Al, Si, Mg, Cu, Mn, Ni, etc. to form Al3Fe, AlFeSi, AlFeMgSi, AlFeSiCu, AlFeSiNi, AlFeMgSiNi, AlFeMnSi, FeNiAl9 and other second phases;
[0114] (3) When the mass percentage of Cu is 0.0005-0.05%, on the one hand, Cu can improve the mechanical properties, thermal conductivity, and fatigue resistance of aluminum alloys. On the other hand, Cu can react with other elements to form a second phase as much as possible to avoid the adverse effect of Cu dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Cu can react with Al, Fe, Si, Mg, Zn, etc. to form second phases such as CuAl2, AlFeSiCu, Al2CuZn, (CuMg)Al2, etc. In addition, Cu can also promote the precipitation of second phases such as Mg2Si, Mg3Sb2, MgZn2, Mg2SiZn, (CuMg)Al2, AlFeMgSi, AlFeMgSiNi, etc., increase their volume fraction and dispersion, and reduce the solid solubility of the above elements in the aluminum matrix;
[0115] (4) When the mass percentage content of Mg is 0.0005-0.06%, on the one hand, Mg can improve the mechanical properties and thermal conductivity of the aluminum alloy, and on the other hand, Mg can react with other elements to form a second phase as much as possible to avoid the adverse effect of Mg dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Mg can react with Al, Fe, Si, Cu, Zn, Ni, Sb, etc. to form second phases such as Mg2Si, Mg3Sb2, Mg2Zn, Mg2SiZn, (CuMg)Al2, AlFeMgSi, AlFeMgSiNi, etc. In addition, Mg can also promote the precipitation of second phases such as CuAl2, AlFeSiCu, Al2CuZn, (CuMg)Al2, etc., increase their volume fraction and dispersion, and reduce the solid solubility of the above elements in the aluminum matrix;
[0116] (5) When the mass percentage of Sr is 0.005-0.04%, on the one hand, Sr can be modified through the heterogeneous nucleation theory or twin valley mechanism to refine the second phase such as eutectic silicon, improve the thermal conductivity and mechanical properties of the aluminum alloy, and also transform the β-AlFeSi phase in the ingot into the Chinese character α-AlFeSi phase to improve the mechanical properties of the aluminum alloy. On the other hand, Sr can preferentially combine with Fe, Cu, Mn, Cr, Si and other elements to form dispersion strengthening to avoid the adverse effect of Sr dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. In addition, Sr can also promote the precipitation of CuAl2, Mg2Si, Mg3Sb2 and other phases to reduce the solid solubility of these alloy elements in the aluminum matrix;
[0117] (6) When the mass percentage content of Zn is 0.0001-0.005%, on the one hand, Zn can improve the mechanical properties of aluminum alloys, and on the other hand, Zn can react with other elements to form a second phase as much as possible to avoid the adverse effect of Zn dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Zn can react with Al, Mg, Cu and Si to form second phases such as MgZn2, Mg2SiZn, Al2CuZn, etc. In addition, Zn can eliminate elemental Si to reduce the adverse effect of elemental Si on the performance of aluminum alloys. Zn can also promote the precipitation of phases such as Mg2Si, Al2Cu, Mg3Sb2, etc., to improve mechanical properties and thermal conductivity;
[0118] (7) When the mass percentage content of Ni is 0.0001-0.001%, on the one hand, Ni can be used to improve the mechanical properties and thermal conductivity of the aluminum alloy, and on the other hand, Ni can be made to react with other elements to form a second phase as much as possible to avoid the adverse effect of Ni dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Ni can react with Al, Fe, Mg, Si, etc. to form Al3Ni, AlFeSiNi, AlFeMgSiNi, FeNiAl9 and other second phases, which promote the precipitation of elements such as Cu, Mg, Zn, Si, Fe and other elements dissolved in the alloy; Ni can also refine the grains, promote the precipitation of strengthening phases such as CuAl2, (CuMg)Al2, Mg3Sb2, increase the volume fraction and dispersion of the precipitated phase, and reduce the solid solubility of the alloy elements in the aluminum matrix. In addition, Ni and Cu, Mg can promote each other's precipitation to improve the thermal conductivity and mechanical properties of the aluminum alloy;
[0119] (8) When the mass percentage of Sb is 0.0001-0.2%, on the one hand, Sb is added to act as a modifier in the aluminum alloy, which effectively reduces the size of the eutectic silicon layer, greatly reduces the possibility of splitting the matrix, and improves the mechanical properties of the alloy. At the same time, antimony has little effect on the electrical conductivity of the alloy. On the other hand, Sb can react with other elements such as Mg as much as possible to generate the second phase Mg3Sb2, so as to avoid the adverse effects of Sb, Mg and other elements dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy, and significantly improve the mechanical properties of the alloy. In addition, the addition of Sb can also increase the mutual precipitation of elements such as Cu, Zn, Ni, etc. that have a large solid solubility in the alloy matrix, further improving the mechanical properties and electrical conductivity of the alloy.
[0120] Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb in the above content range interact with each other as a whole, which can remove the content of transition elements Ti, Mn, Cr, and V in the aluminum matrix that have a great influence on thermal conductivity, and refine the grains, reduce the solid solubility of alloy elements in the aluminum matrix, and increase the volume fraction of the precipitated phase, so as to reduce the adverse effects of alloy elements on the thermal conductivity of the aluminum alloy and improve the comprehensive properties of the aluminum alloy (including mechanical properties, thermal conductivity, and forming properties, etc.). At the same time, under the further effect of aging treatment, the solid solubility of each element in the aluminum matrix is further reduced, which can eliminate the adverse effects of alloy elements on the thermal conductivity of the aluminum alloy as much as possible, and the second phase (such as Al3Fe, Mg2Si, Mg3Sb2, Al2Cu, AlFeSiNi, AlMnSi phase, etc.) can also be refined in the aluminum matrix and at the grain boundary or in the grain boundary, which greatly improves the mechanical properties and thermal conductivity of the aluminum alloy.
[0121] Specifically, since transition elements such as Mn, Cr, Ti, and V have a great influence on the thermal conductivity and mechanical properties of aluminum alloys, their content needs to be strictly controlled; when the amount of elements such as Cu, Mg, Zn, and Sb added is large, the thermal conductivity and mechanical properties of aluminum alloys will also be reduced, and their content also needs to be controlled; but when the mass percentage content of at least one of Si, Fe, Cu, Mg, Sr, Zn, Ni, Sb, Mn, Cr, Ti, and V is low, the elements with a low mass percentage content are not easy to precipitate, and will exist in the aluminum matrix in the form of solid solution, thereby reducing the thermal conductivity and mechanical properties of the aluminum alloy, and the refinement and modification effect of the aluminum alloy will also deteriorate, causing the single substance Si at the grain boundary of the aluminum alloy to exist in the form of coarse flakes and strips, seriously splitting the aluminum matrix, and further reducing the thermal conductivity and mechanical properties of the aluminum alloy. In the technical solution of the present invention, as described in the above items (1) to (8), Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb within the above content range interact with each other as a whole, which can refine the grains (such as the modification effect of Sr and the grain refining effect of Ni), reduce the solid solubility of each other in the aluminum matrix (such as the elements can react with each other to form a second phase), and increase the volume fraction of the precipitated phase (such as Cu, Mg, Sr, Zn, and Ni can promote the precipitation of the second phase), so as to improve the mechanical properties and thermal conductivity of the aluminum alloy; even if the mass percentage content of one or some elements is low, during the aging treatment process, all or almost all of the elements can be precipitated, avoiding adverse effects on the thermal conductivity of the aluminum alloy.
[0122] It is understandable that, since the addition of alloying elements will reduce the thermal conductivity of aluminum alloys, the addition amount of at least one element among Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb of the present invention may be less than the addition amount of the element in the prior art, wherein the addition amount of all elements among Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb of the present invention may be less than the addition amount of the elements in the prior art. Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb within the above content range interact and influence each other as a whole, on the one hand, it can avoid the addition of too many elements to reduce the thermal conductivity of aluminum alloys, on the other hand, at least one of Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb can still improve the comprehensive properties of aluminum alloys (including mechanical properties and thermal conductivity, etc.) when the addition amount is small.
[0123] The present invention also provides an Al-Si die-cast aluminum alloy obtained by the method for preparing the Al-Si die-cast aluminum alloy. Since the Al-Si die-cast aluminum alloy is obtained by the method for preparing the Al-Si die-cast aluminum alloy, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0124] The present invention also provides a heat dissipation structure. At least part of the heat dissipation structure is made of the Al-Si die-cast aluminum alloy or the Al-Si die-cast aluminum alloy prepared by the preparation method of the Al-Si die-cast aluminum alloy. The heat dissipation structure has excellent thermal conductivity and mechanical properties. The Al-Si die-cast aluminum alloy has excellent elongation, so that the Al-Si die-cast aluminum alloy can be suitable for a variety of processes to make different structural parts.
[0125] The heat dissipation structure can be a filter housing of a communication base station, a heat dissipation substrate of a communication base station, a cabinet shell of a communication base station, a three-electric structural component housing of a car, a car shell, a heat sink of a computer device, a middle plate of a mobile phone, a mobile phone shell, a heat sink of an LED lamp, thin parts of 5G products, etc.
[0126] Since the heat dissipation structure adopts all the technical solutions of all the embodiments of the above-mentioned Al-Si series die-cast aluminum alloy, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.
[0127] Embodiment 1
[0128] Pure aluminum is heated at 780°C to obtain pure aluminum liquid;
[0129] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb to the pure aluminum liquid, and keeping the temperature at 750° C. for 10 minutes to obtain an alloy liquid;
[0130] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si die-casting aluminum alloy of Example 1. In the aging treatment, the temperature of the first-level low-temperature aging treatment is -200°C and the time is 1h; the temperature of the second-level low-temperature aging treatment is 0°C and the time is 24h; the temperature of the third-level high-temperature aging treatment is 350°C and the time is 0.1h. The alloy liquid is subjected to die casting treatment at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5m / s. The Al-Si die-casting aluminum alloy contains 5% Si by mass, 0.8% Fe by mass, 0.0005% Cu by mass, 0.0005% Mg by mass, 0.005% Sr by mass, 0.0001% Zn by mass, 0.0001% Ni by mass, and 0.001% Sb by mass.
[0131] Comparative Example 1
[0132] Pure aluminum is heated at 780°C to obtain pure aluminum liquid;
[0133] Adding Si, Fe, Cu, Mg, Sr, Zn, and Ni to the pure aluminum liquid, and keeping the temperature at 750° C. for 10 minutes to obtain an alloy liquid;
[0134] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si die casting aluminum alloy of comparative example 1. In the aging treatment, the temperature of the first low temperature aging treatment is -200°C and the time is 1h; the temperature of the second low temperature aging treatment is 0°C and the time is 24h; the temperature of the third high temperature aging treatment is 350°C and the time is 0.1h. The alloy liquid is die-casted at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5m / s. The Al-Si die casting aluminum alloy contains 5% Si by mass, 0.8% Fe by mass, 0.0005% Cu by mass, 0.0005% Mg by mass, 0.005% Sr by mass, 0.0001% Zn by mass, and 0.0001% Ni by mass.
[0135] Comparative Example 2
[0136] Pure aluminum is heated at 780°C to obtain pure aluminum liquid;
[0137] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb to the pure aluminum liquid, and keeping the temperature at 750° C. for 10 minutes to obtain an alloy liquid;
[0138] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si die-casting aluminum alloy of embodiment 1. In the aging treatment, the temperature is 200°C and the time is 5h. The alloy liquid is subjected to die casting treatment at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5m / s. The Al-Si die-casting aluminum alloy contains 5% Si by mass, 0.8% Fe by mass, 0.0005% Cu by mass, 0.0005% Mg by mass, 0.005% Sr by mass, 0.0001% Zn by mass, 0.0001% Ni by mass, and 0.001% Sb by mass.
[0139] Embodiment 2
[0140] The pure aluminum is heated at a temperature of 720° C. to obtain pure aluminum liquid, wherein the pure aluminum liquid contains Mn, Cr, Ti, and V;
[0141] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb to the pure aluminum liquid, and keeping the temperature at 700° C. for 30 minutes to obtain an alloy liquid;
[0142] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si series die casting aluminum alloy of Example 2. In the aging treatment, the temperature is 300° C. and the time is 8 hours. The alloy liquid is subjected to die casting treatment at a temperature of 665° C., wherein the die casting speed of the die casting machine is 1 m / s. The Al-Si die-casting aluminum alloy contains 5% Si by mass, 0.4% Fe by mass, 0.0005% Cu by mass, 0.0005% Mg by mass, 0.005% Sr by mass, 0.0001% Zn by mass, 0.0001% Ni by mass, 0.001% Sb by mass, 0.0002% Mn by mass, 0.0003% Ti by mass, 0.0003% Cr by mass, and 0.0002% V by mass.
[0143] Embodiment 3
[0144] The pure aluminum is heated at a temperature of 740° C. to obtain pure aluminum liquid, wherein the pure aluminum liquid contains Mn, Cr, Ti, and V;
[0145] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and Sb to the pure aluminum liquid, and keeping the temperature at 730° C. for 20 minutes to obtain an alloy liquid;
[0146] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si series die casting aluminum alloy of Example 3. In the aging treatment, the temperature of the first-level low-temperature aging treatment is -150°C and the time is 3h; the temperature of the second-level low-temperature aging treatment is 70°C and the time is 1h; the temperature of the third-level high-temperature aging treatment is 310°C and the time is 2h. The alloy liquid is die-casted at a temperature of 680°C, wherein the die-casting speed of the die-casting machine is 1.5m / s. The Al-Si die-casting aluminum alloy contains 8% Si by mass, 0.4% Fe by mass, 0.005% Cu by mass, 0.005% Mg by mass, 0.02% Sr by mass, 0.005% Zn by mass, 0.001% Ni by mass, 0.04% Sb by mass, 0.0001% Mn by mass, 0.0001% Ti by mass, 0.0001% Cr by mass, and 0.0001% V by mass.
[0147] Embodiment 4
[0148] The pure aluminum is heated at a temperature of 725° C. to obtain pure aluminum liquid, wherein the pure aluminum liquid contains Mn, Cr, Ti, and V;
[0149] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, In, Nb, Bi, Ge, and Sb to the pure aluminum liquid, and keeping the temperature at 730° C. for 20 minutes to obtain an alloy liquid;
[0150] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si die-casting aluminum alloy of Example 4. In the aging treatment, the temperature of the first-level low-temperature aging treatment is -120°C and the time is 5h; the temperature of the second-level low-temperature aging treatment is 40°C and the time is 10h; the temperature of the third-level high-temperature aging treatment is 330°C and the time is 4h. The alloy liquid is die-casted at a temperature of 670°C, wherein the die-casting speed of the die-casting machine is 1.2m / s. The Al-Si die-casting aluminum alloy contains 6% Si by mass, 0.5% Fe by mass, 0.005% Cu by mass, 0.005% Mg by mass, 0.01% Sr by mass, 0.01% Zn by mass, 0.0001% Ni by mass, 0.2% Sb by mass, 0.0002% Mn by mass, 0.0001% Ti by mass, 0.0003% Cr by mass, 0.0001% V by mass, 0.004% In by mass, 0.003% Nb by mass, 0.001% Bi by mass, and 0.003% Ge by mass.
[0151] Embodiment 5
[0152] The pure aluminum is heated at a temperature of 735° C. to obtain pure aluminum liquid, wherein the pure aluminum liquid contains Mn, Cr, Ti, and V;
[0153] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, Ag, Sn, Te, Mo, and Sb to the pure aluminum liquid, and keeping the temperature at 740° C. for 20 minutes to obtain an alloy liquid;
[0154] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si die casting aluminum alloy of Example 4. In the aging treatment, the temperature of the first low temperature aging treatment is -140°C and the time is 6 hours; the temperature of the second low temperature aging treatment is 50°C and the time is 11 hours; the temperature of the third high temperature aging treatment is 300°C and the time is 5 hours. The alloy liquid is subjected to die casting treatment at a temperature of 665°C, wherein the die casting speed of the die casting machine is 1 m / s. The Al-Si die-casting aluminum alloy contains 6% Si by mass, 0.5% Fe by mass, 0.005% Cu by mass, 0.005% Mg by mass, 0.01% Sr by mass, 0.01% Zn by mass, 0.0001% Ni by mass, 0.2% Sb by mass, 0.0002% Mn by mass, 0.0001% Ti by mass, 0.0003% Cr by mass, 0.0001% V by mass, 0.002% Ag by mass, 0.05% Sn by mass, 0.005% Te by mass, and 0.004% Mo by mass.
[0155] Embodiment 6
[0156] The pure aluminum is heated at a temperature of 740° C. to obtain pure aluminum liquid, wherein the pure aluminum liquid contains Mn, Cr, Ti, and V;
[0157] Add Si, Fe, Cu, Mg, Sr, Zn, Ni, Be, Co, Cd, RE, and Sb to the pure aluminum liquid, and keep the temperature at 710° C. for 25 minutes to obtain an alloy liquid;
[0158] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si die casting aluminum alloy of Example 4. In the aging treatment, the temperature of the first low temperature aging treatment is -140°C and the time is 6 hours; the temperature of the second low temperature aging treatment is 50°C and the time is 11 hours; the temperature of the third high temperature aging treatment is 300°C and the time is 5 hours. The alloy liquid is subjected to die casting treatment at a temperature of 665°C, wherein the die casting speed of the die casting machine is 1 m / s. The Al-Si die-casting aluminum alloy contains 6% Si by mass, 0.5% Fe by mass, 0.005% Cu by mass, 0.005% Mg by mass, 0.01% Sr by mass, 0.01% Zn by mass, 0.0001% Ni by mass, 0.2% Sb by mass, 0.0002% Mn by mass, 0.0001% Ti by mass, 0.0003% Cr by mass, 0.0001% V by mass, 0.002% Be by mass, 0.01% Co by mass, 0.001% Cd by mass, and 0.003% RE by mass.
[0159] Table 1 Performance test results of Examples 1 to 6 and Comparative Examples 1 to 2
[0160] Group Yield strength(MPa) Elongation(%) Thermal conductivity (w / mk) Embodiment 1 125 18.6 215 Embodiment 2 127 18.8 213 Embodiment 3 130 18.9 219 Embodiment 4 132 18.2 220 Embodiment 5 131 18.3 216 Embodiment 6 135 17.8 212 Comparative Example 1 106 14.1 188 Comparative Example 2 108 14.3 190
[0161] According to Table 1, the yield strength, elongation, and electrical conductivity of the Al-Si die-casting aluminum alloys of Examples 1 to 6 are better than those of the Al-Si die-casting aluminum alloys of Comparative Examples 1 to 2. Moreover, the Al-Si die-casting aluminum alloys of Examples 1 to 6 can simultaneously meet the following requirements: thermal conductivity greater than 210, yield strength greater than 120 MPa, and elongation greater than 17%, and have great market application prospects.
[0162] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or direct / indirect application in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing an Al-Si die-casting aluminum alloy, comprising the following steps: The pure aluminum is subjected to a first heating treatment to obtain pure aluminum liquid; Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, Nb and Sb to the pure aluminum liquid, performing a second heating treatment, and obtaining an alloy liquid; Refining and slagging the alloy liquid, and testing its composition and content; and After the composition and content are qualified, the alloy liquid after the refining treatment and the slag removal treatment is subjected to die casting treatment and aging treatment to obtain an Al-Si series die-casting aluminum alloy, wherein the Al-Si series die-casting aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.0005-0.05% Cu by mass, 0.0005-0.0009% Mg by mass, 0.005-0.04% Sr by mass, 0.0001-0.005% Zn by mass, 0.0001-0.001% Ni by mass, 0.001-0.001% Sb by mass, 0.0001-0.005% Nb by mass, 0.0001-0.005% Mn by mass, and 0.0001-0.005% Mn by mass. The present invention relates to a method for preparing the steel structure of the present invention, wherein the steel structure comprises a Cr content of 0.0001-0.0005% by mass, a Ti content of 0.0001-0.0005% by mass and a V content of 0.0001-0.0005% by mass, wherein Mn, Cr, Ti and V are impurities, and the sum of the mass percentage contents of Mn, Ti, Cr and V is not more than 0.002%, and the sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, Nb and Sb is 6-7%, and the aging treatment comprises a primary low-temperature aging treatment, a secondary low-temperature aging treatment and a tertiary high-temperature aging treatment, wherein the temperature of the primary low-temperature aging treatment is -100°C to -200°C, and the time is 1h to 15h; the temperature of the secondary low-temperature aging treatment is 0°C to 70°C, and the time is 1h to 24h; the temperature of the tertiary high-temperature aging treatment is 250°C to 350°C, and the time is 0.05h to 20h.
2. The method for preparing an Al-Si based die-casting aluminum alloy according to claim 1, characterized in that: The preparation method of the Al-Si based die-casting aluminum alloy also includes the step of adding at least one of In, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, and RE to the pure aluminum liquid.
3. An Al-Si based die-casting aluminum alloy prepared by the method for preparing an Al-Si based die-casting aluminum alloy according to any one of claims 1 to 2, containing aluminum, characterized in that: The Al-Si die-casting aluminum alloy further contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.0005-0.05% Cu by mass, 0.0005-0.0009% Mg by mass, 0.005-0.04% Sr by mass, 0.0001-0.005% Zn by mass, 0.0001-0.001% Ni by mass, 0.001-0.001% Sb by mass, and 0. 0.0001-0.005% Nb, 0.0001-0.0005% Mn, 0.0001-0.0005% Cr, 0.0001-0.0005% Ti and 0.0001-0.0005% V, wherein Mn, Cr, Ti and V are impurities, and the sum of the mass percentage contents of Mn, Ti, Cr and V is not more than 0.002%, and the sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, Nb and Sb is 6-7%.
4. The Al-Si based die casting aluminum alloy according to claim 3, characterized in that: In the Al-Si series die-casting aluminum alloy, the mass percentage content of Mn is 0.0001-0.0003%, the mass percentage content of Ti is 0.0001-0.0003%, the mass percentage content of Cr is 0.0001-0.0003%, and the mass percentage content of V is 0.0001-0.0003%.
5. The Al-Si based die casting aluminum alloy according to claim 3, characterized in that: The Al-Si die-casting aluminum alloy also contains 0.0001-0.009% In by mass, 0.0001-0.006% Bi by mass, 0.0001-0.005% Ge by mass, 0.0001-0.005% Mo by mass, 0.0001-0.005% Ag by mass, 0.0001-0.005% Sn by mass, 0.0001-0.1% Te by mass, 0.0001-0.005% Be by mass, 0.001-0.01% Co by mass, 0.001-0.01% Cd by mass and 0.001-0.02% RE by mass.
6. A heat dissipation structure, characterized in that: At least part of the heat dissipation structure is made of the Al-Si die-cast aluminum alloy prepared by the preparation method of the Al-Si die-cast aluminum alloy described in any one of claims 1-2 or the Al-Si die-cast aluminum alloy described in any one of claims 3-5.
Citation Information
Patent Citations
Aluminum alloy and application thereof
CN112159916A
Al-Si heat-treatment-free aluminum alloy as well as preparation method and application thereof
CN116987936A
Aluminum alloys with grain refiners, and methods of making and using same
CN117144196A