A kind of iron-modified biochar gel composite material and its preparation method and application

By filling the iron-modified biochar prepared from rice husk into the graphene gel network, the shortcomings of biochar in adsorption of Sb(III) were solved, the adsorption amount and stability were significantly improved, and Sb(III in wastewater were achieved ) efficient repair.

CN118059814BActive Publication Date: 2024-11-22FOSHAN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410097891.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2024-11-22
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

The existing biochar has problems such as insufficient surface charge, few active sites and instability in adsorbing heavy metal oxides. It is especially poor adsorption effect on Sb(III) and is difficult to effectively repair in a water environment.

Method used

Iron-modified biochar is prepared through rice husks and filled it into the porous three-dimensional network of graphene gel. The flexible coating of graphene and the characteristics of iron-modified biochar gel are used to construct iron-modified biochar gel composite using the flexible coating of graphene and the characteristics of iron-modified biochar. material, increasing adsorption sites and stability.

Benefits of technology

The maximum adsorption amount to Sb(III) is significantly improved, reaching 10 times that of the original biochar, and maintaining good adsorption capacity within the initial pH range of 2-9, significantly improving the repair performance of Sb(III) in wastewater and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118059814B_ABST
    Figure CN118059814B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of adsorption materials, and specifically discloses an iron-modified biochar gel composite material, a preparation method and an application thereof. After preparing biochar from agricultural waste - rice husk and modifying it, the iron-modified biochar is filled into the porous three-dimensional network of graphene gel. By utilizing the advantages of flexible coating of graphene and combining with iron-modified biochar, an iron-modified biochar gel composite material with better Sb(III) remediation performance and long-term stability is constructed. The doping of a small amount of graphene oxide can effectively improve the adsorption performance of the iron-modified biochar gel composite material for Sb(III). Compared with the original biochar, the maximum adsorption capacity of the iron-modified biochar gel composite material for Sb(III) is increased by 10 times. Moreover, the iron-modified biochar gel composite material of the present invention has good adsorption capacity for Sb(III) within the range of 2 < pH < 9 of the initial pH of the sewage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adsorption materials, in particular to an iron-modified biochar gel composite material and a preparation method and application thereof. Background Art

[0002] Although previous studies have shown that biochar has a certain effect in the remediation of Sb(III) pollution, the original biochar has defects such as negative charge on the surface, few active sites, and low specific surface area, which limits its adsorption of heavy metal cations and oxygen-containing anions. The loading of heavy metal oxides can provide more adsorption active sites for biochar and change its surface charge, so heavy metal oxides are potential substances for improving the adsorption performance of original biochar. However, the limited loading capacity of biochar for iron active substances, and its unique magnetic properties make it easy to agglomerate and unstable in water environments, resulting in its remediation performance still needs to be further improved.

[0003] Chinese patent application number CN202110483480.1 discloses a biochar composite material loaded with nano-magnesium oxide and its preparation method and application, by soaking the biochar material in a nano-magnesium hydroxide impregnation solution prepared by mixing ammonia water and magnesium chloride solution, and then forming a biochar composite material loaded with nano-magnesium oxide after high temperature decomposition. The nano-magnesium oxide particles of the prepared biochar composite material loaded with nano-magnesium oxide are evenly distributed, and have a good adsorption effect on heavy metals such as Pb (II), Cd (II), Cr (VI) and Sb (III), and have a good potential for repairing heavy metal pollution in water bodies. The preparation process is simple and easy, the preparation cost is low, and the waste agricultural and forestry biomass is fully utilized. The ammonia water and magnesium chloride in the modification process will not cause secondary pollution to the environment, which is conducive to reducing the environmental pollution and carbon emissions of the waste biomass. It can be used in the remediation of heavy metal pollution to efficiently remove lead, cadmium, antimony and chromium in aqueous solution.

[0004] In fact, the above-mentioned biochar composite material loaded with nano-magnesium oxide has a good adsorption effect on Pb(II), Cd(II), and Cr(VI), but the adsorption effect on Sb(III) does not reach an ideal effect. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an iron-modified biochar gel composite material and a preparation method and application thereof.

[0006] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0007] One of the purposes of the present invention is to provide a method for preparing an iron-modified biochar gel composite material, comprising the following steps:

[0008] S1. Preparation of rice husk biochar using rice husk;

[0009] S2, take 20.0g rice husk biochar and disperse it in 200mL water, add 500mL of a mixed solution of ferric chloride and ferric sulfate, then add NaOH solution to adjust the pH to 10, and continue stirring at 80°C for 1h; after solid-liquid separation, collect the precipitate and rinse it with deionized water for 3-5 times, and finally dry it at 60°C to obtain iron-modified biochar;

[0010] S3. Take 0.2g of graphene oxide and disperse it in 100mL of deionized water, then add 0.40g of reducing agent, 0.8g of iron-modified biochar and 0.12g of Fe3O4 nanoparticles in sequence, and homogenize and disperse for 30min; finally, heat it in a 92℃ oven for 2h to separate the solid and liquid, collect the precipitate and rinse it with deionized water 3 times, then freeze-dry it for 48h, take it out, grind it and pass it through a 100-mesh sieve to obtain the iron-modified biochar gel, which is stored in a clean and sealed container.

[0011] Furthermore, the step S1 specifically comprises: pyrolyzing the rice husk in a tubular muffle furnace at 500° C. for 1 hour under N2 conditions, passing through a 10-mesh sieve, and obtaining rice husk biochar.

[0012] Preferably, the mixed solution of ferric chloride and ferric sulfate is a mixed solution in which 20.0 g of FeCl3·6H2O and 11.1 g of FeSO4·7H2O are dissolved.

[0013] Preferably, the reducing agent is sodium ascorbate.

[0014] Preferably, the concentration of the NaOH solution is 4M.

[0015] The second object of the present invention is to provide an iron-modified biochar gel composite material prepared by the above method.

[0016] The third object of the present invention is to provide an iron-modified biochar gel composite material for use as an adsorbent for adsorbing Sb(III) in wastewater.

[0017] Compared with the prior art, the present invention prepares biochar from agricultural waste - rice husk and then modifies it. Then, the iron - modified biochar is filled into the porous three - dimensional network of graphene gel. Utilizing the advantage of flexible coating of graphene and combining with iron - modified biochar, an iron - modified biochar gel composite material with better Sb(III) remediation performance and long - term stability is constructed. The doping of a small amount of graphene oxide can effectively improve the adsorption performance of the iron - modified biochar gel composite material for Sb(III). Compared with the original biochar, the maximum adsorption capacity of the iron - modified biochar gel composite material for Sb(III) is increased by 10 times. Moreover, the iron - modified biochar gel composite material of the present invention has good adsorption capacity for Sb(III) in the range of 2 < pH < 9 of the initial pH of the sewage. Brief Description of the Drawings

[0018] Figure 1 Schematic diagram for the preparation of the iron - modified biochar gel composite material FeBCG prepared by the present invention.

[0019] Figure 2 Scanning electron microscope (SEM) image of the iron - modified biochar gel composite material FeBCG prepared by the present invention.

[0020] Figure 3 Scanning electron microscope (SEM) image of the iron - modified biochar gel composite material FeBCG after adsorbing Sb(III).

[0021] Figure 4 Energy - dispersive X - ray fluorescence (EDS) spectra of the iron - modified biochar gel composite material FeBCG before and after adsorbing Sb(III).

[0022] Figure 5 Adsorption isotherms of 2BC and FeBCG for adsorbing Sb(III).

[0023] Figure 6 Pseudo - first - order, pseudo - second - order kinetics, Elovich model fitting (A) and intraparticle diffusion model fitting results (B) of BC and FeBCG for adsorbing Sb(III).

[0024] Figure 7 Effect of the initial pH of the solution on the adsorption of Sb(III) by FeBCG biochar.

[0025] Figure 8 Effect of co - existing ions on the adsorption of Sb(III) by FeBCG.

[0026] Fig. 9 Morphology of the iron - modified biochar gel (FeBCG) prepared in Example 1. Detailed Description of the Invention

[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the invention.

[0028] Unless otherwise specified, the raw materials, reagents and equipment used in the following examples were commercially available.

[0029] Example 1

[0030] Reference Figure 1 This embodiment exemplarily provides a preparation process of an iron-modified biochar gel composite material, and the specific steps are as follows:

[0031] 1) Preparation of rice husk biochar (BC)

[0032] In this example, rice husk, an agricultural waste, was used as the biochar raw material. The rice husk was pyrolyzed in a tubular muffle furnace at 500° C. under N2 conditions for 1 hour and passed through a 10-mesh sieve to obtain rice husk biochar (BC).

[0033] 2) Preparation of iron-modified biochar (FeBC)

[0034] Iron-modified biochar (FeBC) was prepared by chemical precipitation method, specifically: 20.0g BC was dispersed in 200mL water and placed in a high-speed disperser (IKAT18 digital ULTRA-TURRAX, Germany) for 30min; 500mL of a mixed solution containing 20.0g FeCl3·6H2O and 11.1g FeSO4·7H2O was added; then 4M NaOH solution was added dropwise to adjust the pH to 10, and stirring was continued at 80°C for 1h; the precipitate was collected after centrifugation and rinsed with deionized water for 3-5 times, and finally dried at 60°C to obtain iron-modified biochar (FeBC).

[0035] 3) Preparation of iron-modified biochar gel (FeBCG)

[0036] 0.2 g of graphene oxide was added to 100 mL of deionized water and dispersed in a high-speed disperser (IKAT18 digital ULTRA-TURRAX, Germany) for 30 min; then 0.40 g of sodium ascorbate, 0.8 g of iron-modified biochar and 0.12 g of Fe3O4 nanoparticles were added to the homogeneous dispersion in sequence, and the mixture was homogenized and dispersed in a high-speed disperser (IKAT18 digital ULTRA-TURRAX, Germany) for 30 min; the mixture was heated in an oven at 92 °C for 2 h and then centrifuged to collect the precipitate and rinsed with deionized water three times; the mixture was then freeze-dried for 48 h, taken out, ground and sieved through a 100-mesh sieve to obtain iron-modified biochar gel (FeBCG); the mixture was stored in a clean and sealed container.

[0037] Material characterization

[0038] The morphology of the prepared iron-modified biochar gel (FeBCG) is as follows: Fig. 9 The surface morphology and element distribution of FeBCG were visualized and detected using a scanning electron microscope (SEM, Hitachi, Regulus 8100, Japan). The results are shown in Figure 2. The SEM image describes the surface morphology of FeBCG. Figure 2 It can be seen that the surface morphology of FeBCG is rough and has a rich porous structure, which provides a suitable location for the adsorption of Sb(III). In addition, typical graphene oxide wrinkles were observed on the surface of FeBCG, indicating that physical cross-linking between graphene oxide and FeBC occurred during the gelation process; after the FeBCG image was magnified, iron oxide particles were found to be deposited on the surface and pores of biochar.

[0039] Example 2

[0040] The FeBCG prepared in the above example can be used as an adsorbent to adsorb Sb(III) in sewage. In order to verify its adsorption effect, the following tests were performed:

[0041] 1. Batch test

[0042] In a 50 mL polyethylene centrifuge tube, 0.03 (± 0.0002) g of adsorbent FeBCG was added to 20 mL of Sb solution in the centrifuge tube, which was then loaded into a thermostatic shaker (150 rpm, 25°C) for cyclotron shaking. Samples for the adsorption kinetics test were collected at specific time intervals from 0 to 8 hours.

[0043] 2. Adsorption isotherm experiment

[0044] In addition, at 5-50 mg L -1 Adsorption isotherm experiments were conducted in the range of initial concentrations of 2.5 wt % and 1.5 wt % respectively. Blank experiments were performed without adsorbent under otherwise identical conditions.

[0045] 3. Test of influencing factors

[0046] In order to explore the effect of pH on the adsorption system, the initial antimony solution was adjusted to pH = 2.0-11.0 in advance, and the adsorbent FeBCG was added in an amount of 1.2 g L -1 Regarding the effect of coexisting anions and organic acid radicals on the adsorption capacity of the adsorbent, chlorine (Cl - ), nitrate (NO3 - ), sulfate (SO4 2- ), phosphate (HPO4 2- ) and citrate (CA -). The concentrations of coexisting ions were 0.1 M and 0.2 M, respectively. After the adsorption reaction was terminated, the sample was filtered through a filter membrane (pore size 0.22 μm), and the remaining Sb(Ⅲ) concentration in the aqueous solution was measured using an inductively coupled plasma spectrometer ICP-OES. The samples used for the test were stored in a refrigerator at 4°C.

[0047] Wherein: the adsorption efficiency (formula (1)) and the Sb(III) equilibrium adsorption capacity per unit adsorbent (formula (2)) are calculated by the following equations:

[0048]

[0049]

[0050] Where C0 and C e (mg L -1 ) represent the initial and equilibrium concentrations of Sb(Ⅲ), V(L) is the volume of the solution, and W(g) is the mass of the adsorbent.

[0051] The pseudo-first-order kinetics (Equation (3)), pseudo-second-order kinetics model (Equation (4)) and intra-particle diffusion model (Equation (5)) were used to analyze the adsorption kinetics characteristics. The model equations are as follows:

[0052] ln(Q e -Q t )=lnQ e -k1 (3)

[0053]

[0054] Q t =K i t 1 / 2 +C i (5)

[0055] Where Q e (mg g -1 ) and Q t (mg g -1 ) represent the adsorption amount of Sb(Ⅲ) at equilibrium and at time t, respectively (mgg -1 ); k1(min -1 ) and k2(g mg -1 min -1 ) are the equilibrium rate constants of the pseudo-first-order and pseudo-second-order models, respectively; K i (mg g - 1 min -0.5 ) is the adsorption rate constant of the intraparticle diffusion model; C i (mg g -1 ) is a constant that characterizes the thickness of the boundary layer.

[0056] The adsorption isotherm data were fitted by Langmuir (Equation (7)), Freundlich (Equation (8)), Temkin (Equation (9)) and Sips (Equation (10)) models, and the model equations were as follows:

[0057]

[0058]

[0059] Q e =Bln(AC e ) (9)

[0060]

[0061] Where Q e (mg g -1 ) represents the equilibrium adsorption amount of Sb(III); Q m (mg g -1 ) is the theoretical maximum adsorption capacity; C e (mg L -1 ) is the residual concentration in the solution at adsorption equilibrium; K L (L g -1 ) and K F (mg g -1 (L mg -1 ) 1 / n represent the Langmuir constant and the Freundlich constant respectively; n represents the binding energy constant; N represents the equilibrium adsorption amount (mg g -1 ); B(J mol -1 ) is a constant related to the heat of adsorption and is defined as B = RT / b, T is the absolute temperature (K), R is the gas constant (8.314 J mol -1 K -1 ); A is the Temkin isotherm constant (L g -1 ). s (Lmg -1 ) is the Sips constant; m is a dimensionless constant.

[0062] The above experimental results are as follows:

[0063] Adsorption isotherms can be used to analyze the interaction between adsorbent FeBCG and Sb(Ⅲ) and the characteristics of the adsorption layer. The results show that the adsorption capacity of Sb(Ⅲ) on BC and FeBCG gradually increases with the increase of the initial concentration of Sb(Ⅲ). The Langmuir model, Freundlich model, Temkin model and Sips model were used to fit these adsorption isotherm data to further evaluate the adsorption capacity and adsorption mechanism of BC and FeBCG for Sb(Ⅲ). The curves after fitting the four models are shown in Figure 2. Figure 5 The relevant isotherm parameters are listed in Table 1. The maximum adsorption capacities of BC and FeBCG for Sb(Ⅲ) are estimated to be 2.455 and 25.216 mg g, respectively, based on the Langmuir model. -1 Compared with the original carbon, the maximum adsorption capacity of Sb(Ⅲ) by FeBCG was increased by 10 times. 2 ) found that Sips ≥ Langmuir> Freundlich> Temkin.

[0064] Table 1

[0065]

[0066] Kinetics describes the relationship between mass transfer of adsorbate and time, and can be used to estimate the adsorption rate of the adsorbent. The kinetic data of Sb(Ⅲ) adsorption by BC and FeBCG were fitted by pseudo-first-order, pseudo-second-order kinetic models and intraparticle diffusion models. The fitting results and parameters are shown in Figure 6 and Table 2. The Sb(Ⅲ) adsorption capacity of BC and FeBCG increased rapidly within 10 min and reached 70% and 77% of the maximum adsorption capacity, respectively. This is because the adsorbent surface is rich in free active sites that can effectively adsorb Sb(III). After 120 min, the adsorbent basically reached adsorption equilibrium, but overall FeBCG had a faster and better adsorption performance for Sb(Ⅲ). This is because it has a larger specific surface area, rich mesoporous structure and sufficient adsorption sites compared to BC. By comparing the nonlinear correlation coefficient of pseudo-first-order kinetics and the adsorption amount, it was found that the pseudo-second-order kinetic model is more consistent with the actual adsorption process of Sb(Ⅲ) on BC and FeBCG (R 2 =0.977-0.987), and the Q of FeBCG to Sb(III) calculated by this model t Value and Experimental Q t The values ​​are basically consistent, indicating that Sb(Ⅲ) is adsorbed onto BC and FeBCG through chemical action.

[0067] The intraparticle diffusion model simulates the entire adsorption process to explore the kinetic mechanism between BC and FeBCG and Sb(Ⅲ) and the reasons that control the adsorption rate.

[0068] Table 2

[0069]

[0070] The scanning electron microscope (SEM) image of FeBCG after adsorbing Sb(III) is as Figure 3 shown, and the energy-dispersive X-ray fluorescence (EDS) spectra of FeBCG before and after adsorbing Sb(III) are as Figure 4 shown. Figure 3 , Figure 4 It clearly presents the significant correlation among the distributions of O, Fe, and Sb on the surface of the FeBCG sample after adsorbing Sb(III) (FeBCG-Sb), indicating that the presence of oxygen-containing functional groups and Fe elements has an important impact on the adsorption process of Sb(III).

[0071] Example 3

[0072] In addition to the characteristics of the adsorbent and heavy metal pollutants, the changes in pH and background ionic strength in the solution are also considered key factors determining adsorption. The dependence of the adsorption effect on pH is related to the existence form of Sb(III) in the solution and the ionization state of the functional groups on the adsorbent surface, thereby affecting the availability of binding sites. As Figure 7 , the adsorption effect of FeBCG on Sb(III) reaches the best at pH = 2, and its adsorption capacity begins to decline slowly as the pH increases, but it changes relatively stably in the wide range of pH = 4 - 9. This is because the existence forms of Sb(III) in aqueous solution vary greatly under different pH conditions. (1) When pH < 2, Sb(III) mainly exists as positively charged Sb(OH)2 + ; (2) in the relatively wide range of 2 < pH < 10, it mainly exists in the form of electrically neutral Sb(OH)3, and the remaining part exists as Sb(OH)2 + ; (3) when pH > 10, it mainly exists in the form of negatively charged H2SbO3 - and Sb(OH)4 - .

[0073] In the actual water environment treatment, coexisting anions in the water body may affect the removal effect of Sb(III) through competition, changing the adsorbent potential, steric hindrance, etc. Previous studies have shown that inner-sphere complexes are less susceptible to changes in ionic strength than outer-sphere complexes. Therefore, studying the influence of the changes in coexisting ions and their strength is of great significance for exploring the adsorption mechanism and water environment restoration. In this example, Cl - , SO4 2- , HPO4 2- , CA -Four common anions in natural waters were selected to evaluate their effects on the adsorption performance of FeBCG at high concentrations, as Figure 8 . The results showed that different coexisting ions had varying degrees of hindrance to the adsorption of the target pollutant Sb(III) by FeBCG. As the concentration of interfering ions increased further, the adsorption capacity of FeBCG was more limited.

[0074] In summary, in the present invention, biochar was prepared from agricultural waste - rice husk and then modified, and the iron - modified biochar was filled into the porous three - dimensional network of graphene hydrogel. Utilizing the advantages of flexible graphene coating and combining with iron - modified biochar, an iron - modified biochar hydrogel composite with better Sb(III) remediation performance and long - term stability was constructed. The doping of iron active substances and a small amount of graphene oxide can effectively improve the adsorption performance of the iron - modified biochar hydrogel composite for Sb(III). Compared with the original biochar, the maximum adsorption capacity of the iron - modified biochar hydrogel composite for Sb(III) is increased by 10 times; moreover, the iron - modified biochar hydrogel composite of the present invention has good adsorption capacity for Sb(III) in the range of 2 < pH < 9 of the initial pH of the sewage.

[0075] The technical solution of the present invention is not limited to the limitations of the above - mentioned specific embodiments. Any technical deformation made according to the technical solution of the present invention falls within the protection scope of the present invention.

Claims

1. A method for preparing an iron-modified biochar gel composite material, characterized in that: The following steps are involved: S1, pyrolyzing rice husk in a tubular muffle furnace at 500°C under N2 conditions for 1 hour, passing through a 10-mesh sieve to obtain rice husk biochar; S2, take 20.0 g of rice husk biochar and disperse it in 200 mL of water, add 500 mL of a mixed solution of ferric chloride and ferric sulfate, then add NaOH solution to adjust the pH to 10, and continue stirring at 80 ° C for 1 h; after solid-liquid separation, collect the precipitate and rinse it with deionized water for 3-5 times, and finally dry it at 60 ° C to obtain iron-modified biochar; S3. Take 0.2 g of graphene oxide and disperse it in 100 mL of deionized water. Then add 0.40 g of reducing agent sodium ascorbate, 0.8 g of iron-modified biochar and 0.12 g of Fe3O4 nanoparticles in sequence and homogenize and disperse for 30 min. Finally, heat it in a 92°C oven for 2 h to separate the solid and liquid. Collect the precipitate and rinse it with deionized water for 3 times. Then freeze-dry it for 48 h. Take it out, grind it and pass it through a 100-mesh sieve to obtain the iron-modified biochar gel, which is stored in a clean and sealed container.

2. The method for preparing the iron-modified biochar gel composite material according to claim 1, characterized in that: The mixed solution of ferric chloride and ferric sulfate is a mixed solution in which 20.0 g of FeCl3·6H2O and 11.1 g of FeSO4·7H2O are dissolved.

3. The method for preparing the iron-modified biochar gel composite material according to claim 1, characterized in that: The concentration of the NaOH solution is 4M.

4. An iron-modified biochar gel composite material prepared by the method according to any one of claims 1 to 3.

5. Use of the iron-modified biochar gel composite material as claimed in claim 4 as an adsorbent for adsorbing trivalent Sb in sewage.