A deposition apparatus for preparing silicon carbide composite cladding using chemical vapor infiltration.

By optimizing the deposition chamber structure and air intake and exhaust methods, the problems of uneven workpiece deposition and insufficient densification during the preparation of silicon carbide composite shells by chemical vapor infiltration were solved, achieving airtightness and dimensional accuracy of full-length silicon carbide composite shells, and producing dense and uniform silicon carbide composite shells.

CN118147606BActive Publication Date: 2026-11-10CHINA NORTH NUCLEAR FUEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211551105.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2026-11-10
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

In the existing chemical vapor infiltration process for preparing silicon carbide composite cladding, uneven deposition on the upper and lower parts of the workpiece and insufficient local densification make it difficult to guarantee the airtightness and dimensional accuracy of full-size silicon carbide composite cladding.

Method used

A deposition apparatus for preparing silicon carbide composite cladding by chemical vapor infiltration was designed. By optimizing the deposition chamber structure, gas inlet method and gas outlet method, including providing a gas inlet channel at the bottom of the deposition chamber and a gas outlet channel at the top, and setting multiple layers of side gas inlets on the outer cylinder wall and uniformly distributed gas outlet channels on the inner cylinder wall, the gas is ensured to be uniformly distributed.

Benefits of technology

The process achieved sufficient densification and uniform deposition of the silicon carbide composite cladding, ensuring the airtightness and dimensional accuracy of the full-length silicon carbide composite cladding. The resulting silicon carbide composite cladding was sufficiently densified and dimensionally uniform.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118147606B_ABST
    Figure CN118147606B_ABST
Patent Text Reader

Abstract

This invention specifically relates to a deposition apparatus for preparing silicon carbide composite cladding using chemical vapor infiltration (CVI), comprising a deposition chamber and a gas guide pipe (14); an inlet channel is provided below the deposition chamber, and an exhaust channel is provided above the deposition chamber, the exhaust channel being connected to the gas guide pipe (14). The deposition apparatus of this invention, by optimizing the deposition chamber structure, the inlet method, and the exhaust method, achieves uniform gas distribution during the preparation of silicon carbide composite cladding using CVI, solving the problems of sufficient densification of the workpiece and uniform deposition during the preparation of silicon carbide composite cladding using CVI, thereby ensuring the airtightness and dimensional accuracy of the full-length silicon carbide composite cladding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicon carbide composite coating preparation technology, and in particular to a deposition apparatus for preparing silicon carbide composite coatings by chemical vapor infiltration. Background Technology

[0002] Currently, almost all commercial water reactor nuclear power plants use zirconium alloy as the cladding material for fuel elements. Years of reactor operation have proven that zirconium alloy cladding is safe and reliable under steady-state conditions. However, with the world's increasing emphasis on reactor safety in recent years, it is necessary to consider reactor safety under accident conditions such as tsunamis. In some nuclear power plant accidents, hydrogen explosions have caused severe damage and released large amounts of radioactive material. The hydrogen released in these explosions was produced by the reaction of zirconium alloy with water at high temperatures during the accident. Furthermore, the performance of zirconium alloy degrades rapidly at high temperatures, thus compromising its safety barrier. Therefore, developing cladding materials with a certain degree of accident containment capability has become a new direction in the international nuclear fuel field.

[0003] Silicon carbide materials possess characteristics such as high temperature resistance, high strength, low neutron absorption cross section, structural stability, and low activity under harsh irradiation conditions, making them promising candidates for applications in the nuclear field and potentially suitable as cladding materials for fourth-generation nuclear reactors. However, pure silicon carbide ceramic materials, due to their inherent brittleness, cannot meet the diverse performance requirements of cladding tubes. Therefore, they need to be prepared into silicon carbide composite materials to achieve pseudo-plasticity. This involves using silicon carbide fibers to create preforms that act as a reinforcing skeleton, and then adding dense silicon carbide between the preforms and on their inner and outer surfaces to act as the matrix. Currently, the main methods for preparing silicon carbide composite cladding include reaction sintering, precursor impregnation pyrolysis, chemical vapor infiltration, and nano-impregnation with transient eutectic phase processes. Due to the high purity, high crystallinity, and superior performance of the prepared silicon carbide matrix, chemical vapor infiltration is considered the mainstream technology for nuclear-grade silicon carbide composite materials.

[0004] Significant progress has been made both domestically and internationally in the preparation of silicon carbide composite cladding using chemical vapor infiltration (CVI). However, most of these studies involve scaled-down samples. Scaled-down samples typically employ a single-cylinder deposition chamber with a multi-hole inlet at the bottom and an outlet at the top. With this inlet method, the concentration of reactant gas at the top gradually decreases as the height increases, making it difficult to achieve the desired deposition effect. The bottom-inlet method can guarantee a deposition height of up to 400-800 mm. Currently, the longest scaled-down sample reported domestically reaches 1500 mm, achieved by using a method of alternating the top and bottom of the deposition chamber for separate deposition. Full-size silicon carbide composite cladding is 3900-4000 mm in length, which this type of deposition chamber cannot meet. Therefore, the preparation of long-size silicon carbide composite cladding is not simply a scaling up of the scaled-down sample preparation process. With increasing length, controlling the uniformity of the gas flow field becomes more difficult, easily leading to uneven deposition between the top and bottom of the workpiece and insufficient local densification, resulting in leakage. Summary of the Invention

[0005] Based on this, the present invention addresses the problems of uneven deposition and insufficient local densification in the preparation of silicon carbide composite shells by chemical vapor infiltration. It provides a deposition apparatus for preparing silicon carbide composite shells by chemical vapor infiltration. This apparatus optimizes the deposition chamber structure, gas inlet method, and gas outlet method to achieve uniform gas distribution during the preparation of silicon carbide composite shells by chemical vapor infiltration, thus solving the problems of sufficient densification and deposition uniformity of the workpiece in the preparation of silicon carbide composite shells by chemical vapor infiltration, and thereby ensuring the airtightness and dimensional accuracy of the full-length silicon carbide composite shell.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A deposition apparatus for preparing silicon carbide composite cladding by chemical vapor infiltration includes a deposition chamber and a gas guide pipe; an air inlet is provided below the deposition chamber, and an exhaust outlet is provided on the deposition chamber, the exhaust outlet being connected to the gas guide pipe.

[0007] Working principle: The silicon carbide composite shell is vertically hung in the deposition chamber. The reaction gas enters the deposition chamber through the air inlet below the deposition chamber. After the reaction, the gas enters the gas guide pipe through the exhaust port on the deposition chamber and is discharged through the gas guide pipe.

[0008] Furthermore, the deposition chamber is composed of a gas distribution plate, an inner cylinder, an outer cylinder, a workpiece hanging cover, and a heat insulation cover; the deposition device also includes a lower air inlet pipe; the inner cylinder, outer cylinder, and air guide pipe are all hollow structures with openings at both the top and bottom; a heat insulation cover is installed at the upper end of the outer cylinder, a base is installed at the lower end of the outer cylinder, and the gas distribution plate, inner cylinder, and workpiece hanging cover are all installed inside the outer cylinder; The lower end of the base is connected to the lower air inlet pipe, the upper end of the base is connected to the air distribution plate, the lower end of the heat preservation cover is connected to the upper end of the workpiece hanging cover, the upper end of the inner cylinder is connected to the lower end of the workpiece hanging cover, and the lower end of the inner cylinder is connected to the upper end of the air distribution plate. The annular space between the outer wall of the inner cylinder, the inner wall of the outer cylinder, the top of the gas distribution plate, and the bottom of the workpiece hanging cover forms a sedimentation chamber; the inner cylinder wall is provided with an exhaust channel, one end of the gas guide pipe passes through the heat insulation cover and the workpiece hanging cover in sequence and is connected to the lower end of the workpiece hanging cover, the other end of the gas guide pipe extends out of the heat insulation cover, and the inside of the inner cylinder is connected to the inside of the gas guide pipe.

[0009] The silicon carbide composite shell is vertically suspended in the deposition chamber through the workpiece hanging cover. The reaction gas enters the deposition chamber through the lower inlet pipe and the gas distribution plate. After the reaction, the gas enters the inner cylinder through the exhaust channel on the inner cylinder wall and is discharged through the gas guide pipe.

[0010] Furthermore, the gas distribution plate has multiple evenly distributed air inlet channels in the annular region between the inner and outer cylinders. These evenly distributed air inlet channels ensure uniform air intake below the deposition chamber.

[0011] Furthermore, the inner cylinder wall is provided with multiple evenly distributed exhaust channels. These multiple evenly distributed exhaust channels ensure the uniform discharge of gases after reaction within the deposition chamber.

[0012] Furthermore, a side air inlet pipe is provided on the outer cylinder wall. The reaction gas enters the deposition chamber through the side air inlet pipe on the outer cylinder wall.

[0013] Furthermore, the outer cylinder wall is provided with multiple layers of side air inlets at equal intervals from bottom to top, and each layer of side air inlets includes multiple circumferentially uniformly arranged side air inlets. The multiple layers of side air inlets at equal intervals and the multiple circumferentially uniformly arranged side air inlets in each layer of side air inlets ensure uniform side air intake in the deposition chamber.

[0014] Preferably, the outer cylinder wall is provided with six layers of side air inlets from bottom to top, namely the first layer of side air inlets, the second layer of side air inlets, the third layer of side air inlets, the fourth layer of side air inlets, the fifth layer of side air inlets and the sixth layer of side air inlets; each layer of side air inlets is spaced 500-700mm apart, and each layer of side air inlets includes three side air inlets evenly arranged in the circumference.

[0015] The present invention also provides a method for preparing silicon carbide composite coatings by chemical vapor infiltration, using the above-mentioned deposition apparatus, comprising the following steps: (1) Suspend the silicon carbide cladding preform in the deposition chamber, then install the deposition device into the furnace and close the furnace cover; (2) Evacuate the furnace to below 10 Pa, heat to the deposition temperature of 1000-1200℃, and then introduce reaction gases into the deposition chamber. The flow rate of trichloromethylsilane is 6 L / min to 12 L / min, the flow rate of argon is 12 L / min to 30 L / min, and the flow rate of hydrogen is 12 L / min to 30 L / min. Adjust the deposition pressure in the deposition chamber to 500-8000 Pa and the vapor deposition time to 60-300 h. (3) After the deposition is completed, stop heating and stop the flow of reaction gas. After cooling to room temperature, open the furnace cover and take out the silicon carbide cladding from the deposition device.

[0016] Preferably, the method for preparing silicon carbide composite shells by chemical vapor infiltration includes the following steps: (1) Suspend the silicon carbide cladding preform in the deposition chamber, then install the deposition device into the furnace and close the furnace cover; (2) The furnace is evacuated to below 10 Pa, heated to the deposition temperature of 1200 °C, and then the reaction gas is introduced into the deposition chamber. The flow rate of trichloromethylsilane is 12 L / min, the flow rate of argon is 30 L / min, the flow rate of hydrogen is 30 L / min, the deposition pressure in the deposition chamber is adjusted to 8000 Pa, and the gas phase deposition time is 300 h. (3) After the deposition is completed, stop heating and stop the flow of reaction gas. After cooling to room temperature, open the furnace cover and take out the silicon carbide cladding from the deposition device.

[0017] Preferably, the method for preparing silicon carbide composite shells by chemical vapor infiltration includes the following steps: (1) Suspend the silicon carbide cladding preform in the deposition chamber, then install the deposition device into the furnace and close the furnace cover; (2) Evacuate the furnace to below 10 Pa, heat to the deposition temperature of 1000℃, and then introduce reaction gases into the deposition chamber. The flow rate of trichloromethylsilane is 6 L / min, the flow rate of argon is 12 L / min, the flow rate of hydrogen is 12 L / min, the deposition pressure in the deposition chamber is adjusted to 500 Pa, and the gas phase deposition time is 60 h. (3) After the deposition is completed, stop heating and stop the flow of reaction gas. After cooling to room temperature, open the furnace cover and take out the silicon carbide cladding from the deposition device.

[0018] Preferably, the method for preparing silicon carbide composite shells by chemical vapor infiltration includes the following steps: (1) Suspend the silicon carbide cladding preform in the deposition chamber, then install the deposition device into the furnace and close the furnace cover; (2) Evacuate the furnace to below 8 Pa, heat to the deposition temperature of 1200℃, and then introduce reaction gases into the deposition chamber. The flow rate of trichloromethylsilane is 8 L / min, the flow rate of argon is 15 L / min, the flow rate of hydrogen is 18 L / min, and the deposition pressure in the deposition chamber is adjusted to 2000 Pa. The gas phase deposition time is 200 h. (3) After the deposition is completed, stop heating and stop the flow of reaction gas. After cooling to room temperature, open the furnace cover and take out the silicon carbide cladding from the deposition device.

[0019] Beneficial technical effects of the present invention: The chemical vapor infiltration (CVI) deposition apparatus for preparing silicon carbide composite cladding of the present invention optimizes the deposition chamber structure, gas inlet method, and gas outlet method, achieving uniform gas distribution during the preparation of silicon carbide composite cladding by CVI. It solves the problems of sufficient densification and deposition uniformity of the workpiece during the preparation of silicon carbide composite cladding by CVI, thereby ensuring the airtightness and dimensional accuracy of the full-length silicon carbide composite cladding. The resulting silicon carbide composite cladding is sufficiently densified and has uniform dimensions. Attached Figure Description

[0020] Figure 1 A schematic diagram of the deposition apparatus for preparing silicon carbide composite cladding by chemical vapor infiltration according to the present invention; Figure 2 This is a schematic diagram of the single-layer side air intake structure of Example 1.

[0021] In the diagram: 1. Lower air inlet pipe; 2. Base; 3. Air distribution plate; 4. Inner cylinder; 5. Outer cylinder; 6. First layer side air inlet pipe; 7. Second layer side air inlet pipe; 8. Third layer side air inlet pipe; 9. Fourth layer side air inlet pipe; 10. Fifth layer side air inlet pipe; 11. Sixth layer side air inlet pipe; 12. Workpiece hanging cover; 13. Insulation cover; 14. Air guide pipe; 15. Workpiece; 16. Exhaust hole; 17. Side air inlet pipe. Detailed Implementation

[0022] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0023] In the description of this invention, it should be understood that the terms "left end", "right end", "above", "below", "outer side", "inner side", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.

[0024] Furthermore, the terms “first,” “second,” “third,” “fourth,” “fifth,” “sixth,” etc., are used for descriptive purposes only and should not be interpreted as indicating or implying relative importance.

[0025] Example 1 A deposition apparatus for preparing silicon carbide composite cladding using chemical vapor infiltration includes a deposition chamber and a gas guide pipe 14. An inlet channel is located below the deposition chamber, and an exhaust channel is located above the deposition chamber, the exhaust channel being connected to the gas guide pipe 14. The silicon carbide composite cladding is vertically suspended within the deposition chamber. Reaction gases enter the deposition chamber through the inlet channel below, and the reacted gases enter the gas guide pipe 14 through the exhaust channel above the deposition chamber and are then discharged through the gas guide pipe 14.

[0026] The deposition chamber comprises a gas distribution plate 3, an inner cylinder 4, an outer cylinder 5, a workpiece hanging cover 12, and a heat insulation cover 13; the deposition device also includes a lower air inlet pipe 1; the inner cylinder 4, the outer cylinder 5, and the air inlet pipe 14 are all hollow structures with openings at both the top and bottom; the heat insulation cover 13 is installed at the upper end of the outer cylinder 5, and a base 2 is installed at the lower end of the outer cylinder 5; the gas distribution plate 3, the inner cylinder 4, and the workpiece hanging cover 12 are all installed inside the outer cylinder 5; the lower end of the base 2 is connected to the lower air inlet pipe 1, the upper end of the base 2 is connected to the gas distribution plate 3, and the lower end of the heat insulation cover 13 is connected to... The upper end of the workpiece hanging cover 12 is connected to the upper end of the inner cylinder 4, which is connected to the lower end of the workpiece hanging cover 12. The lower end of the inner cylinder 4 is connected to the upper end of the gas distribution plate 3. The annular space between the outer wall of the inner cylinder 4, the inner wall of the outer cylinder 5, the upper part of the gas distribution plate 3, and the lower part of the workpiece hanging cover 12 forms a deposition chamber. The inner cylinder 4 has exhaust channels on its wall. One end of the gas guide pipe 14 passes through the insulation cover 13 and the workpiece hanging cover 12 in sequence and is connected to the lower end of the workpiece hanging cover 12. The other end of the gas guide pipe 14 extends out of the insulation cover 13. The interior of the inner cylinder 4 is connected to the interior of the gas guide pipe 14. The silicon carbide composite shell is vertically hung in the deposition chamber through the workpiece hanging cover 12. The reaction gas enters the deposition chamber through the lower air inlet pipe 1 and the gas distribution plate 3. After the reaction, the gas enters the interior of the inner cylinder 4 through the exhaust channels on the wall of the inner cylinder 4 and is discharged through the gas guide pipe 14.

[0027] The gas distribution plate 3 has multiple evenly distributed air inlet channels in the annular area between the inner cylinder 4 and the outer cylinder 5. The multiple evenly distributed air inlet channels ensure uniform air intake below the sedimentation chamber.

[0028] The inner cylinder 4 has multiple evenly distributed venting channels on its wall. These channels ensure the uniform discharge of gases after reaction within the deposition chamber.

[0029] The outer cylinder 5 is equipped with a side air inlet pipe. The reaction gas enters the deposition chamber through the side air inlet pipe on the outer cylinder 5.

[0030] The outer cylinder 5 has six layers of side air inlets spaced from bottom to top, namely the first layer of side air inlets 6, the second layer of side air inlets 7, the third layer of side air inlets 8, the fourth layer of side air inlets 9, the fifth layer of side air inlets 10 and the sixth layer of side air inlets 11; each layer of side air inlets is spaced 500-700mm apart, and each layer of side air inlets includes three side air inlets evenly arranged in the circumference.

[0031] Example 2 The preparation of silicon carbide composite cladding using the chemical vapor infiltration deposition apparatus of Example 1 includes the following steps: (1) Loading the furnace: Fix the silicon carbide shell preform below the workpiece hanging cover 12, place the workpiece hanging cover 12 above the inner cylinder 4 and the outer cylinder 5, at this time the workpiece is vertically suspended between the inner cylinder 4 and the outer cylinder 5, put in the heat insulation cover 13 and the gas guide pipe 14 in sequence, and close the furnace cover. (2) Deposition: After evacuating to below 10 Pa and heating to the deposition temperature of 1000℃, the reaction gas is simultaneously introduced through the lower gas inlet pipe 1 and the side gas inlet pipe. The flow rate of trichloromethylsilane is 6 L / min, the flow rate of argon is 12 L / min, and the flow rate of hydrogen is 12 L / min. The deposition pressure is set to 500 Pa through the pressure regulating valve, and the gas phase deposition time is 60 h. (3) Unloading: After the deposition is completed, stop heating, shut off the gas supply, and after cooling to room temperature, open the furnace cover, take out the gas pipe 14 and the heat preservation cover 13, and take out the workpiece hanging cover 12.

[0032] The prepared silicon carbide composite shell is fully densified and has uniform size. The sample density in different regions along the length direction can reach 2.8 g / cm3, and the leakage rate is better than 2.0×10-10 Pa·cm3·sec-1.

[0033] Example 3 The preparation of silicon carbide composite cladding using the chemical vapor infiltration deposition apparatus of Example 1 includes the following steps: (1) Loading the furnace: Fix the silicon carbide shell preform below the workpiece hanging cover 12, place the workpiece hanging cover 12 above the inner cylinder 4 and the outer cylinder 5, at this time the workpiece is vertically suspended between the inner cylinder 4 and the outer cylinder 5, put in the heat insulation cover 13 and the gas guide pipe 14 in sequence, and close the furnace cover. (2) Deposition: After evacuating to below 10 Pa and heating to the deposition temperature of 1200℃, the reaction gas is simultaneously introduced through the lower gas inlet pipe 1 and the side gas inlet pipe. The flow rate of trichloromethylsilane is 12 L / min, the flow rate of argon is 30 L / min, and the flow rate of hydrogen is 30 L / min. The deposition pressure is set to 8000 Pa through the pressure automatic regulating valve, and the gas phase deposition time is 300 h. (3) Unloading: After the deposition is completed, stop heating, shut off the gas supply, and after cooling to room temperature, open the furnace cover, take out the gas pipe 14 and the heat preservation cover 13, and take out the workpiece hanging cover 12.

[0034] The prepared silicon carbide composite shell is fully densified and has uniform size. The sample density in different regions along the length direction can reach 2.8 g / cm3, and the leakage rate is better than 2.0×10-10 Pa·cm3·sec-1.

[0035] Example 4 The preparation of silicon carbide composite cladding using the chemical vapor infiltration deposition apparatus of Example 1 includes the following steps: (1) Loading the furnace: Fix the silicon carbide shell preform below the workpiece hanging cover 12, place the workpiece hanging cover 12 above the inner cylinder 4 and the outer cylinder 5, at this time the workpiece is vertically suspended between the inner cylinder 4 and the outer cylinder 5, put in the heat insulation cover 13 and the gas guide pipe 14 in sequence, and close the furnace cover. (2) Deposition: After evacuating to below 8 Pa and heating to the deposition temperature of 1200℃, the reaction gas is simultaneously introduced through the lower gas inlet pipe 1 and the side gas inlet pipe. The flow rate of trichloromethylsilane is 8 L / min, the flow rate of argon is 15 L / min, and the flow rate of hydrogen is 18 L / min. The deposition pressure is set to 2000 Pa through the pressure automatic regulating valve, and the gas phase deposition time is 200 h. (3) Unloading: After the deposition is completed, stop heating and stop the flow of reaction gas. After cooling to room temperature, open the furnace cover, take out the gas guide pipe 14 and the heat preservation cover 13, and take out the workpiece hanging cover 12.

[0036] The prepared silicon carbide composite shell is fully densified and has uniform size. The sample density in different regions along the length direction can reach 2.8 g / cm3, and the leakage rate is better than 2.0×10-10 Pa·cm3·sec-1.

[0037] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.

Claims

1. A deposition apparatus for preparing silicon carbide composite coatings using chemical vapor infiltration, characterized in that, It includes a sedimentation chamber and a gas guide pipe (14); the sedimentation chamber is provided with an air inlet channel below and an exhaust channel above, and the exhaust channel is connected to the gas guide pipe (14); The deposition chamber is composed of a gas distribution plate (3), an inner cylinder (4), an outer cylinder (5), a workpiece hanging cover (12), and a heat preservation cover (13). The deposition device also includes a lower air inlet pipe (1). The inner cylinder (4), outer cylinder (5) and air guide pipe (14) are all hollow structures with openings at both the top and bottom. The upper end of the outer cylinder (5) is equipped with a heat insulation cover (13), and the lower end of the outer cylinder (5) is equipped with a base (2). The air distribution plate (3), inner cylinder (4) and workpiece hanging cover (12) are all installed inside the outer cylinder (5). The lower end of the base (2) is connected to the lower air inlet pipe (1), the upper end of the base (2) is connected to the air distribution plate (3), the lower end of the heat preservation cover (13) is connected to the upper end of the workpiece hanging cover (12), the upper end of the inner cylinder (4) is connected to the lower end of the workpiece hanging cover (12), and the lower end of the inner cylinder (4) is connected to the upper end of the air distribution plate (3). The annular space between the outer wall of the inner cylinder (4), the inner wall of the outer cylinder (5), the top of the gas distribution plate (3), and the bottom of the workpiece hanging cover (12) forms a sedimentation chamber; the inner cylinder (4) is provided with an exhaust channel, one end of the air guide pipe (14) passes through the heat insulation cover (13) and the workpiece hanging cover (12) in sequence and is connected to the lower end of the workpiece hanging cover (12), the other end of the air guide pipe (14) extends out of the heat insulation cover (13), and the inside of the inner cylinder (4) is connected to the inside of the air guide pipe (14).

2. The deposition apparatus according to claim 1, characterized in that, The air distribution plate (3) has multiple evenly distributed air inlet channels in the annular area between the inner cylinder (4) and the outer cylinder (5).

3. The deposition apparatus according to claim 1, characterized in that, The inner cylinder (4) has multiple evenly distributed exhaust channels on its wall.

4. The deposition apparatus according to claim 1, characterized in that, The outer cylinder (5) has a side air inlet pipe on its wall.

5. The deposition apparatus according to claim 4, characterized in that, The outer cylinder (5) has multiple layers of side air inlets arranged at equal intervals from bottom to top, and each layer of side air inlets includes multiple side air inlets evenly arranged in the circumferential direction.

6. The deposition apparatus according to claim 5, characterized in that, The outer cylinder (5) has six layers of side air inlets spaced from bottom to top, namely the first layer of side air inlets (6), the second layer of side air inlets (7), the third layer of side air inlets (8), the fourth layer of side air inlets (9), the fifth layer of side air inlets (10) and the sixth layer of side air inlets (11); each layer of side air inlets is spaced 500-700mm apart, and each layer of side air inlets includes three side air inlets evenly arranged in the circumference.

Citation Information

Patent Citations

  • Method for the densification of thin porous substrates by means of vapour phase chemical infiltration and device for loading such substrates

    CN101120116A

  • Interface layer structure of SiCf / SiC composite material fuel cladding and preparation method

    CN113004051A

  • Chemical vapor deposition device for full-size SiC composite cladding tube

    CN113005427A

  • Shims for substrates densified by chemical vapor infiltration

    FR3114107A1