A viscosity-reducing coating dispersant and preparation method thereof
Through the combination of polyether matrix and acid-based monomer and the introduction of modified cellulose, the problem of insufficient flexibility of the coating dispersant is solved, and the excellent viscosity reduction effect and stability of the coating is achieved, and particle settlement is avoided. Improves the overall performance of the paint.
Patent Information
- Application Number
- CN202410180647.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-02-18
AI Technical Summary
The existing coating dispersants have lower molecular flexibility during use, resulting in tackifying raw material particles and reducing the performance of paint/ink. The existing viscosity-reducing dispersants only improve the high shear effect, but improve other performances. Not obvious.
The combination of polyether matrix, acid-based monomer, reducing agent, initiator, chain transfer agent, neutralizing agent and modification additive is used to improve the flexibility of the dispersant and The ionization effect forms an appropriate wrapping layer thickness and potential gradient, enhancing the stability and anti-settlement performance of the paint.
It significantly improves the viscosity reduction effect and stability of the coating molecules, avoids particle aggregation and settlement, significantly reduces interfacial tension, and improves the overall performance of the coating.
Smart Images

Figure BDA0004703727170000141
Abstract
Description
Technical Field
[0001] The invention relates to the field of coating additives, and in particular to a viscosity-reducing coating dispersant and a preparation method thereof. Background Art
[0002] Dispersants are widely used in the chemical industry as a functional additive that can make particles disperse evenly in the medium. Especially in the field of chemical products such as coatings and inks, dispersants are an indispensable raw material. The dispersants used in common aqueous solutions mainly include polymer electrolyte dispersants and polycarboxylic acid and its derivative dispersants. Although these dispersants can meet the dispersion performance requirements of some coatings and ink products, in actual use, the molecular flexibility of the dispersants is low, which can easily increase the viscosity of the raw material particles, thereby reducing the corresponding performance of the coating / ink.
[0003] Existing wetting and dispersing agents use oligomers composed of polycarboxylic acids and polyamines, which cannot form effective steric hindrance due to their low molecular weight and are not suitable for dispersing organic pigments and carbon black. Natural polymer copolymers such as lecithin are amphoteric surfactants that are often used to disperse organic pigments, but they have poor hydrophilicity and stability, which will reduce gloss and coating performance.
[0004] The prior art CN109694445B provides a viscosity reducing dispersant and a paper coating obtained therefrom, wherein the raw materials mainly include ether functional monomers, organic acids and functional additives, and claims that the obtained product has a good viscosity reducing effect, especially a good high shear viscosity reducing effect, is green, environmentally friendly and degradable. However, in actual application, only the high shear effect of the coating is improved, while the enhancement of other properties of the coating is not obvious.
[0005] Therefore, in order to solve the above problems, the present application provides a viscosity-reducing coating dispersant and a preparation method thereof. The prepared viscosity-reducing coating dispersant not only has excellent viscosity-reducing effect, but also can simultaneously improve other properties of coating molecules, and has very excellent market prospects. Summary of the invention
[0006] In order to solve the above problems, the first aspect of the present invention provides a viscosity-reducing coating dispersant, which comprises, by weight, at least 100 to 150 parts of a polyether matrix, 80 to 100 parts of an acid-based monomer, 3 to 8 parts of a reducing agent, 5 to 15 parts of an initiator, 2 to 5 parts of a chain transfer agent, 2 to 5 parts of a neutralizer, and 10 to 30 parts of a modifying additive.
[0007] Furthermore, the polyether matrix includes modified polyether and block polyether.
[0008] Furthermore, the mass ratio of the modified polyether to the block polyether is (3-6):(1-3).
[0009] Furthermore, the mass ratio of the modified polyether to the block polyether is (4-5): (1-1.5).
[0010] Furthermore, the mass ratio of the modified polyether to the block polyether is 4.5:1.2.
[0011] Furthermore, the block polyether is at least one of propylene glycol block polyether, ethylene glycol block polyether, hydroxy polyethylene oxide block copolymer, and carboxyl polyethylene oxide block copolymer.
[0012] Furthermore, the block polyether is propylene glycol block polyether and / or ethylene glycol block polyether.
[0013] Furthermore, the block polyether is propylene glycol block polyether.
[0014] Furthermore, the modified polyether is modified polyethylene glycol monomethyl ether.
[0015] Furthermore, the modified polyether is unsaturated modified polyethylene glycol monomethyl ether.
[0016] Furthermore, the preparation method of the modified polyethylene glycol monomethyl ether comprises the following steps: S1: adding maleic acid and polyethylene glycol monomethyl ether into a reaction container, heating to 60-80° C., and melting and mixing uniformly; S2: adding an inhibitor and a catalyst, stirring uniformly, heating to 90-95° C. under a nitrogen atmosphere, and reacting for 2-4 hours; S3: heating to 140-160° C. for a second time, and reacting at a constant temperature for 3-6 hours to obtain the modified polyethylene glycol monomethyl ether.
[0017] Furthermore, the molar ratio of the polyethylene glycol monomethyl ether to maleic acid is (0.6-1): (0.4-0.6).
[0018] Furthermore, the molar ratio of the polyethylene glycol monomethyl ether to maleic acid is (0.8-1):(0.5-0.6).
[0019] Furthermore, the molar ratio of polyethylene glycol monomethyl ether to maleic acid is 0.9:0.5.
[0020] Furthermore, the catalyst is p-toluenesulfonic acid; the amount of the catalyst is 2-4% of the total mass of polyethylene glycol monomethyl ether and maleic acid.
[0021] Furthermore, the polymerization inhibitor is hydroquinone monomethyl ether; the dosage of the polymerization inhibitor is 0.5-1% of the total mass of polyethylene glycol monomethyl ether and maleic acid.
[0022] Furthermore, the average molecular weight of the polyethylene glycol monomethyl ether is 200-1000.
[0023] Furthermore, the average molecular weight of the polyethylene glycol monomethyl ether is 400-600.
[0024] In the present application, by using the above-mentioned specific polyether composition and acrylic acid compounding, the viscosity reduction effect of the dispersant can be greatly improved, while the stability of the pigment in the coating system can be effectively improved, and the anti-settling and anti-color change performance of the coating can be improved while keeping the particle size basically unchanged. This is mainly because, in the present application, by adding polyether molecules, through the ether bond effect in the long chain, the dispersant provides a suitable coating layer thickness for the coating component particles while obtaining better flexibility, and can also increase the stretching length of the dispersant long chain in the water-based coating system, sufficient long chain stretching and suitable coating thickness can effectively increase the steric hindrance between the coating particles, avoid aggregation, and the thickness change is small and it is not easy to produce particle sedimentation due to excessive inclusion; on the other hand, the sulfonic acid group in the modified cellulose added in the present invention is used to improve the ionization effect in the system, thereby ensuring the independence and specificity between the coating molecules, and it is not easy to deteriorate during long-term storage.
[0025] Furthermore, the acid-based monomer is at least one of acrylic acid, methacrylic acid, itaconic acid and maleic acid.
[0026] Furthermore, the acid-based monomer is any one of acrylic acid, methacrylic acid and itaconic acid.
[0027] Furthermore, the acid-based monomer is acrylic acid.
[0028] Furthermore, the reducing agent is at least one of sodium bisulfite, sodium pyrosulfite, sodium hypophosphite, and sodium formaldehyde sulfoxylate.
[0029] Furthermore, the reducing agent is sodium bisulfite.
[0030] Furthermore, the initiator is at least one of ammonium persulfate, potassium persulfate, benzoyl peroxide, di-tert-butyl peroxide, and azobisisobutyronitrile.
[0031] Furthermore, the initiator is benzoyl peroxide and ammonium persulfate.
[0032] Furthermore, the chain transfer agent is any one of thioglycolic acid, mercaptopropionic acid, and mercaptoethanol.
[0033] Furthermore, the chain transfer agent is mercaptoethanol.
[0034] Furthermore, the neutralizing agent is at least one of sodium hydroxide, potassium hydroxide, ammonia water, potassium carbonate, ethanolamine, diethanolamine, and triethanolamine.
[0035] Furthermore, the neutralizing agent is diethanolamine.
[0036] Furthermore, the modified additive is modified cellulose.
[0037] Furthermore, the preparation method of the modified additive comprises the following steps: S1: acidifying the nanocellulose with hydrochloric acid and washing with water to obtain a nanocellulose mixed liquid; S2: heating the nanocellulose mixed liquid to 60-80° C., adding potassium persulfate, and adding methacrylic acid and tert-butyl acrylamide sulfonic acid and stirring to react for 10-20 hours, extracting after the reaction is completed, and obtaining the nanocellulose by rotary evaporation.
[0038] Furthermore, the mass ratio of the nanocellulose to methacrylic acid and tert-butyl acrylamide sulfonic acid is (5-10): (1-4): (3-5).
[0039] Furthermore, the mass ratio of the nanocellulose to methacrylic acid and tert-butyl acrylamide sulfonic acid is (6-7): (1.5-2): (4-5).
[0040] Furthermore, the mass ratio of the nanocellulose to methacrylic acid and tert-butyl acrylamide sulfonic acid is 6.5:2:4.5.
[0041] In this application, by using the modified nanocellulose as a dispersant raw material, not only can the viscosity reduction effect of the dispersant be further improved, but also the dispersant can effectively improve the effect of improving the stability of the coating. This is mainly because, in this application, by using the modified nanocellulose, not only can a stable long-chain interwoven network be formed on the cellulose surface, thereby enhancing its cross-stretching effect with the dispersant body, but also the compatible binding effect between the components of the dispersant can be effectively improved; on the other hand, the introduced sulfonic acid group can assist the dispersant and the coating particles to produce a large number of charged particles under the alkaline conditions of the dispersant as a whole. The appearance of these particles can form a strong potential gradient, which greatly reduces the probability of collision between coating particles at different potentials under this gradient, and significantly reduces the interfacial tension of the overall coating system.
[0042] The second aspect of the present invention provides a method for preparing the above-mentioned viscosity-reducing coating dispersant, which comprises the following steps: S1: adding the required polyether matrix to a reaction container, heating to 50-60°C and setting aside; S2: uniformly mixing the reducing agent, initiator and chain transfer agent with the acid monomer, and dripping them into the polyether matrix of S1, the dripping reaction time is 2-4 hours, and the temperature is kept warm for 1-1.5 hours after the dripping reaction is completed; S3: adding a neutralizing agent to the product after the reaction is completed to adjust the pH, and then adding a modifying additive and stirring at a speed of 100-200 r / min for 30-60 minutes, and the viscosity-reducing coating dispersant is obtained after being uniformly mixed.
[0043] The present invention has the following beneficial effects:
[0044] 1. The present application provides a viscosity-reducing coating dispersant. The prepared coating dispersant not only has a better viscosity-reducing effect than existing dispersants such as polycarboxylic acid, but can also further improve other properties of coating molecules at the same time, and has a very excellent market prospect.
[0045] 2. The present application provides a viscosity-reducing coating dispersant. By adopting a specific polyether composition and compounding it with acrylic acid, the viscosity-reducing effect of the dispersant can be greatly improved while effectively improving the stability of the pigment in the coating system, and the anti-settling and anti-color change properties of the coating can be improved while keeping the particle size basically unchanged. While obtaining better flexibility, the dispersant provides a suitable coating layer thickness for the coating component particles, and can also increase the stretching length of the dispersant long chain in the water-based coating system. Sufficient long-chain stretching and suitable coating thickness can effectively increase the steric hindrance between the coating particles to avoid aggregation, and the thickness change is small and it is not easy to produce particle sedimentation due to excessive inclusion.
[0046] 3. The present application provides a viscosity-reducing coating dispersant. The modified nanocellulose is used as a dispersant raw material, which can not only further enhance the viscosity-reducing effect of the dispersant, but also effectively enhance the stability-enhancing effect of the dispersant on the coating. A stable long-chain interwoven network is formed on the cellulose surface, thereby enhancing its cross-stretching effect with the main body of the dispersant, and effectively enhancing the compatibility and binding effect between the components of the dispersant. On the other hand, the introduced sulfonic acid group can assist the dispersant and coating particles in generating a large number of charged particles under the alkaline conditions of the dispersant as a whole. The appearance of these particles can form a strong potential gradient, which greatly reduces the probability of collision between coating particles at different potentials under this gradient, and significantly reduces the interfacial tension of the overall coating system.
[0047] 4. The present application provides a viscosity-reducing coating dispersant, which has a simple preparation method and does not involve complex chemical reactions. In addition, the preparation process can effectively improve the sedimentation of materials and products in the equipment, thereby greatly reducing the maintenance cost of the equipment and the labor cost of production. DETAILED DESCRIPTION
[0048] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.
[0049] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.
[0050] Example 1
[0051] Example 1 The first aspect provides a viscosity-reducing coating dispersant, in which the raw materials include at least, by mass: 120 parts of a polyether matrix, 90 parts of an acid-based monomer, 5 parts of a reducing agent, 10 parts of an initiator, 3 parts of a chain transfer agent, 3 parts of a neutralizing agent, and 15 parts of a modifying additive.
[0052] The polyether matrix includes modified polyether and block polyether; the block polyether is propylene glycol block polyether L64, purchased from Jiangsu Haian Petroleum; the mass ratio of modified polyether to block polyether is 4.5:1.2.
[0053] The preparation method of modified polyethylene glycol monomethyl ether comprises the following steps: S1: adding maleic acid and polyethylene glycol monomethyl ether into a reaction container, heating to 70°C, and melting and mixing uniformly; S2: adding an inhibitor and a catalyst, stirring uniformly, heating to 95°C under a nitrogen atmosphere, and reacting for 3 hours; S3: heating to 150°C for a second time, and reacting at a constant temperature for 5 hours to obtain the product.
[0054] Polyethylene glycol monomethyl ether is polyethylene glycol monomethyl ether MPEG-400, which was purchased from Jiangsu Haian Petroleum.
[0055] The catalyst is p-toluenesulfonic acid; the amount of the catalyst is 3.5% of the total mass of polyethylene glycol monomethyl ether and maleic acid.
[0056] The polymerization inhibitor is hydroquinone monomethyl ether; the dosage of the polymerization inhibitor is 0.8% of the total mass of polyethylene glycol monomethyl ether and maleic acid.
[0057] The molar ratio of polyethylene glycol monomethyl ether to maleic acid is 0.9:0.5.
[0058] The acid-based monomer is acrylic acid.
[0059] The reducing agent is sodium bisulfite; the initiator is benzoyl peroxide and ammonium persulfate, and the mass ratio of the two is 1:1; the chain transfer agent is mercaptoethanol; and the neutralizing agent is diethanolamine.
[0060] The modified additive is modified cellulose, and the preparation method of the modified additive includes the following steps, calculated by mass: S1: 6.5 parts of nanocellulose are thoroughly acidified with hydrochloric acid, and then washed with water to obtain a nanocellulose mixed liquid; S2: the nanocellulose mixed liquid is heated to 65°C, 0.005 parts of potassium persulfate are added, and 2 parts of methacrylic acid and 4.5 parts of tert-butyl acrylamide sulfonic acid are added and stirred for 16 hours, and after the reaction is completed, extraction is performed and the product is obtained by rotary evaporation.
[0061] The nanocellulose was 3-10 nm grade nanocellulose sold by Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.
[0062] The second aspect of this embodiment provides a method for preparing the above-mentioned viscosity-reducing coating dispersant, and the preparation method comprises the following steps: S1: adding the required polyether matrix to a reaction container, heating to 55°C, and setting aside; S2: uniformly mixing the reducing agent, initiator, and chain transfer agent with the acid monomer, and dripping them into the polyether matrix of S1, the dripping reaction time is 3.5h, and the temperature is kept warm for 1h after the dripping reaction is completed; S3: adding a neutralizing agent to the product after the reaction is completed to adjust the pH to 8, and then adding a modifying additive and stirring at a speed of 200r / min for 40min, and the viscosity-reducing coating dispersant is obtained after the mixture is uniformly mixed.
[0063] Example 2
[0064] Example 2 The first aspect provides a viscosity-reducing coating dispersant, in which the raw materials include at least, by mass: 130 parts of a polyether matrix, 80 parts of an acid-based monomer, 5 parts of a reducing agent, 10 parts of an initiator, 3 parts of a chain transfer agent, 3 parts of a neutralizer, and 15 parts of a modifying additive.
[0065] The polyether matrix includes modified polyether and block polyether; the block polyether is propylene glycol block polyether L64, purchased from Jiangsu Haian Petroleum; the mass ratio of modified polyether to block polyether is 4.5:1.2.
[0066] The preparation method of modified polyethylene glycol monomethyl ether comprises the following steps: S1: adding maleic acid and polyethylene glycol monomethyl ether into a reaction container, heating to 70°C, and melting and mixing uniformly; S2: adding an inhibitor and a catalyst, stirring uniformly, heating to 95°C under a nitrogen atmosphere, and reacting for 3 hours; S3: heating to 150°C for a second time, and reacting at a constant temperature for 5 hours to obtain the product.
[0067] Polyethylene glycol monomethyl ether is polyethylene glycol monomethyl ether MPEG-400, which was purchased from Jiangsu Haian Petroleum.
[0068] The catalyst is p-toluenesulfonic acid; the amount of the catalyst is 3.5% of the total mass of polyethylene glycol monomethyl ether and maleic acid.
[0069] The polymerization inhibitor is hydroquinone monomethyl ether; the dosage of the polymerization inhibitor is 0.8% of the total mass of polyethylene glycol monomethyl ether and maleic acid.
[0070] The molar ratio of polyethylene glycol monomethyl ether to maleic acid is 0.7:0.5.
[0071] The acid-based monomer is acrylic acid.
[0072] The reducing agent is sodium bisulfite; the initiator is benzoyl peroxide and ammonium persulfate, and the mass ratio of the two is 1:1; the chain transfer agent is mercaptoethanol; and the neutralizing agent is diethanolamine.
[0073] The modified additive is modified cellulose, and the preparation method of the modified additive includes the following steps, calculated by mass: S1: 6.5 parts of nanocellulose are thoroughly acidified with hydrochloric acid, and then washed with water to obtain a nanocellulose mixed liquid; S2: the nanocellulose mixed liquid is heated to 65°C, 0.005 parts of potassium persulfate are added, and 2 parts of methacrylic acid and 4.5 parts of tert-butyl acrylamide sulfonic acid are added and stirred for 16 hours, and after the reaction is completed, extraction is performed and the product is obtained by rotary evaporation.
[0074] The nanocellulose was 3-10 nm grade nanocellulose sold by Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.
[0075] The second aspect of this embodiment provides a method for preparing the above-mentioned viscosity-reducing coating dispersant, and the preparation method comprises the following steps: S1: adding the required polyether matrix to a reaction container, heating to 55°C, and setting aside; S2: uniformly mixing the reducing agent, initiator, and chain transfer agent with the acid monomer, and dripping them into the polyether matrix of S1, the dripping reaction time is 3.5h, and the temperature is kept warm for 1h after the dripping reaction is completed; S3: adding a neutralizing agent to the product after the reaction is completed to adjust the pH to 8, and then adding a modifying additive and stirring at a speed of 200r / min for 40min, and the viscosity-reducing coating dispersant is obtained after the mixture is uniformly mixed.
[0076] Example 3
[0077] Example 3 The first aspect provides a viscosity-reducing coating dispersant, in which the raw materials include at least, by mass: 120 parts of a polyether matrix, 90 parts of an acid-based monomer, 5 parts of a reducing agent, 10 parts of an initiator, 3 parts of a chain transfer agent, 3 parts of a neutralizing agent, and 15 parts of a modifying additive.
[0078] The polyether matrix includes modified polyether and block polyether; the block polyether is propylene glycol block polyether L64, purchased from Jiangsu Haian Petroleum; the mass ratio of modified polyether to block polyether is 4.5:1.2.
[0079] The preparation method of modified polyethylene glycol monomethyl ether comprises the following steps: S1: adding maleic acid and polyethylene glycol monomethyl ether into a reaction container, heating to 70°C, and melting and mixing uniformly; S2: adding an inhibitor and a catalyst, stirring uniformly, heating to 95°C under a nitrogen atmosphere, and reacting for 3 hours; S3: heating to 150°C for a second time, and reacting at a constant temperature for 5 hours to obtain the product.
[0080] Polyethylene glycol monomethyl ether is polyethylene glycol monomethyl ether MPEG-400, which was purchased from Jiangsu Haian Petroleum.
[0081] The catalyst is p-toluenesulfonic acid; the amount of the catalyst is 3.5% of the total mass of polyethylene glycol monomethyl ether and maleic acid.
[0082] The polymerization inhibitor is hydroquinone monomethyl ether; the dosage of the polymerization inhibitor is 0.8% of the total mass of polyethylene glycol monomethyl ether and maleic acid.
[0083] The molar ratio of polyethylene glycol monomethyl ether to maleic acid is 0.9:0.5.
[0084] The acid-based monomer is acrylic acid.
[0085] The reducing agent is sodium bisulfite; the initiator is benzoyl peroxide and ammonium persulfate, and the mass ratio of the two is 1:1; the chain transfer agent is mercaptoethanol; and the neutralizing agent is diethanolamine.
[0086] The modified additive is modified cellulose, and the preparation method of the modified additive includes the following steps, calculated by mass: S1: after 5 parts of nanocellulose are completely acidified with hydrochloric acid, they are washed with water to obtain a nanocellulose mixed liquid; S2: the nanocellulose mixed liquid is heated to 65°C, 0.005 parts of potassium persulfate are added, and 3.5 parts of methacrylic acid and 5 parts of tert-butyl acrylamide sulfonic acid are added and stirred for 16 hours, and after the reaction is completed, extraction is performed and the product is obtained by rotary evaporation.
[0087] The nanocellulose was 3-10 nm grade nanocellulose sold by Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.
[0088] The second aspect of this embodiment provides a method for preparing the above-mentioned viscosity-reducing coating dispersant, and the preparation method comprises the following steps: S1: adding the required polyether matrix to a reaction container, heating to 55°C, and setting aside; S2: uniformly mixing the reducing agent, initiator, and chain transfer agent with the acid monomer, and dripping them into the polyether matrix of S1, the dripping reaction time is 3.5h, and the temperature is kept warm for 1h after the dripping reaction is completed; S3: adding a neutralizing agent to the product after the reaction is completed to adjust the pH to 8, and then adding a modifying additive and stirring at a speed of 200r / min for 40min, and the viscosity-reducing coating dispersant is obtained after the mixture is uniformly mixed.
[0089] Comparative Example 1
[0090] The specific implementation manner of this comparative example is basically the same as that of Example 1, except that: the modified additive is modified cellulose, and the preparation method of the modified additive comprises the following steps, measured in parts by mass: S1: 10 parts of nanocellulose are thoroughly acidified with hydrochloric acid, and then washed with water to obtain a nanocellulose mixed liquid; S2: the nanocellulose mixed liquid is heated to 65° C., 0.005 parts of potassium persulfate are added, and 2 parts of methacrylic acid and 2 parts of tert-butyl acrylamide sulfonic acid are added, stirred and reacted for 16 hours, and after the reaction is completed, extraction is performed, and the obtained product is obtained by rotary evaporation.
[0091] Comparative Example 2
[0092] The specific implementation manner of this comparative example is basically the same as that of Example 1, except that: the modified additive is modified cellulose, and the preparation method of the modified additive comprises the following steps, measured in parts by mass: S1: 6.5 parts of nanocellulose are thoroughly acidified with hydrochloric acid, and then washed with water to obtain a nanocellulose mixed liquid; S2: the nanocellulose mixed liquid is heated to 65° C., 0.005 parts of potassium persulfate are added, and 6 parts of methacrylic acid and 8 parts of tert-butyl acrylamide sulfonic acid are added, stirred and reacted for 16 hours, and after the reaction is completed, extraction is performed, and the obtained product is obtained by rotary evaporation.
[0093] Comparative Example 3
[0094] The specific implementation of this comparative example is basically the same as that of Example 1, except that the mass ratio of the modified polyether to the block polyether is 5:5.
[0095] Comparative Example 4
[0096] The specific implementation of this comparative example is basically the same as that of Example 1, except that the mass ratio of the modified polyether to the block polyether is 8:1.
[0097] Comparative Example 5
[0098] The specific implementation of this comparative example is basically the same as that of Example 1, except that the mass ratio of the modified polyether to the block polyether is 1:8.
[0099] Comparative Example 6
[0100] The specific implementation manner of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified additive comprises the following steps, measured in parts by mass: S1: after 5 parts of cellulose are thoroughly acidified with hydrochloric acid, the mixture is washed with water to obtain a nanocellulose mixed liquid; S2: the nanocellulose mixed liquid is heated to 65°C, 0.005 parts of potassium persulfate are added, and 3.5 parts of methacrylic acid and 5 parts of tert-butyl acrylamide sulfonic acid are added and stirred for 16 hours, and after the reaction is completed, the modified additive is extracted and obtained by rotary evaporation.
[0101] The cellulose was 10-15 μm grade cellulose sold by Wuhan Kemik Biomedical Technology Co., Ltd.
[0102] Performance Evaluation
[0103] The dispersant prepared in the examples and comparative examples was added into water at a content of 20 wt %, and then 40 wt % of phthalocyanine blue pigment was added. After uniform dispersion, zirconium beads were added and ground for a certain period of time to prepare phthalocyanine blue paste, which was used as a test sample.
[0104] Color stability: After the color paste sample was stored at a constant temperature of 60°C and a humidity of 75% for 10 days, the morphology of the color paste was observed and the measured results were recorded in Table 1.
[0105] Hot storage viscosity change: After the color paste is stored at a constant temperature of 60°C and a humidity of 75% for 10 days, the viscosity before and after hot storage is tested by a viscosity tester, and the viscosity change value is calculated. Viscosity change value = viscosity after hot storage - viscosity after hot storage. The average value of 10 measured values is recorded in Table 1.
[0106] Particle size change during hot storage: After the color paste is stored at a constant temperature of 60°C and a humidity of 75% for 10 days, the particle size before and after hot storage is tested by a particle size tester, and the particle size change value is calculated. Particle size change value = particle size after hot storage - particle size after hot storage. The average value of 10 measured values is recorded in Table 1.
[0107] Table 1 Test results of thermal storage particle size change
[0108]
[0109] It can be seen from the examples, comparative examples and the data in Table 1 that the viscosity-reducing coating dispersant prepared in the present application can effectively improve the dispersion effect of the pigment in the aqueous system, and will not excessively affect the particle size of the pigment particles in the system (determined by the wrapping area and thickness), thereby avoiding the sedimentation phenomenon caused by excessively large particles. On the other hand, it can also effectively improve the stability of the pigment particles in the aqueous system, reduce the flocculation and sedimentation phenomenon (determined by the steric hindrance and viscosity between particles), and can also show excellent stability in certain storage tests with only minimal performance changes. However, since comparative examples 1 to 4 do not adopt the specific necessary technical solutions required by the present application, they will show poor performance in the corresponding performance tests due to the reduction of steric hindrance, excessive wrapping thickness and weakening of the potential gradient.
Claims
1. A viscosity-reducing coating dispersant, characterized in that: The raw materials include at least 100-150 parts of polyether matrix, 80-100 parts of acid monomer, 3-8 parts of reducing agent, 5-15 parts of initiator, 2-5 parts of chain transfer agent, 2-5 parts of neutralizing agent, and 10-30 parts of modifying additive in parts by weight. The polyether matrix includes modified polyether and block polyether; The mass ratio of the modified polyether to the block polyether is (3-6): (1-3); The block polyether is at least one of propylene glycol block polyether, ethylene glycol block polyether, hydroxy polyethylene oxide block copolymer, and carboxyl polyethylene oxide block copolymer; The modified polyether is modified polyethylene glycol monomethyl ether; The acid-based monomer is at least one of acrylic acid, methacrylic acid, itaconic acid and maleic acid; The neutralizing agent is at least one of sodium hydroxide, potassium hydroxide, ammonia water, potassium carbonate, ethanolamine, diethanolamine, and triethanolamine; The preparation method of the modified polyethylene glycol monomethyl ether comprises the following steps: S1: adding maleic acid and polyethylene glycol monomethyl ether into a reaction container, heating to 60-80° C., and melting and mixing uniformly; S2: adding an inhibitor and a catalyst, stirring uniformly, heating to 90-95° C. in a nitrogen atmosphere, and reacting for 2-4 hours; S3: heating to 140-160° C. for a second time, and reacting at a constant temperature for 3-6 hours to obtain the modified polyethylene glycol monomethyl ether; The molar ratio of polyethylene glycol monomethyl ether to maleic acid is (0.6-1): (0.4-0.6); The preparation method of the modified additive comprises the following steps: S1: acidifying the nanocellulose with hydrochloric acid, and then washing with water to obtain a nanocellulose mixed liquid; S2: heating the nanocellulose mixed liquid to 60-80° C., adding potassium persulfate, and adding methacrylic acid and tert-butyl acrylamide sulfonic acid, stirring and reacting for 10-20 hours, extracting after the reaction is completed, and obtaining the modified additive by rotary evaporation; The mass ratio of the nanocellulose to methacrylic acid and tert-butyl acrylamide sulfonic acid is (5-10): (1-4): (3-5).
2. The viscosity reducing coating dispersant according to claim 1, characterized in that: The reducing agent is at least one of sodium bisulfite, sodium pyrosulfite, sodium hypophosphite, and sodium formaldehyde sulfoxylate.
3. The viscosity reducing coating dispersant according to claim 1, characterized in that: The initiator is at least one of ammonium persulfate, potassium persulfate, benzoyl peroxide, di-tert-butyl peroxide, and azobisisobutyronitrile.
4. The viscosity-reducing coating dispersant according to claim 1, characterized in that: The chain transfer agent is any one of thioglycolic acid, mercaptopropionic acid and mercaptoethanol.
5. A method for preparing a viscosity-reducing coating dispersant according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: S1: Add the required polyether matrix into a reaction container, heat it to 50-60°C, and set aside; S2: Evenly mix the reducing agent, initiator and chain transfer agent with the acid monomer, and dropwise add them into the polyether matrix of S1. The dropwise reaction time is 2-4 hours. After the dropwise reaction is completed, continue to keep warm for 1-1.5 hours. S3: After the reaction is completed, a neutralizer is added to the product to adjust the pH, and then a modified additive is added and stirred at a speed of 100-200 r / min for 30-60 minutes. After the mixture is uniformly mixed, a viscosity-reducing coating dispersant is obtained.
Citation Information
Patent Citations
A viscosity reducer, its preparation method, and a paper coating
CN109694445B
Viscosity-reducing concrete admixture
CN110218018A
Preparation method of viscosity reduction type coating dispersing agent and viscosity reduction type coating dispersing agent
CN112961288A
Preparation method and application of viscosity-reducing agricultural dispersant
CN115304721A
Aqueous pigment dispersion, its manufacturing method and article using them
JP2008056786A