A multi-stage warm forging line
By using a hydraulic press to press and a specific lubricant in the warm forging process, a stable lubricant film is formed, which solves the problem of lubricant failure in the warm forging process, improves the hardness and wear resistance of metal materials, and ensures high-quality forgings Production.
Patent Information
- Application Number
- CN202410484009.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-22
AI Technical Summary
In the warm forging process, existing lubricants fail at high temperatures, resulting in increased friction and oxidation of metal surfaces, affecting the quality and accuracy of forgings.
A multi-stage warm forging line process is used to press the metal material at the temperature forging temperature using a hydraulic press to form ultra-fine and uniform grain tissue, and a lubricant containing sodium borate, tricalcium phosphate and sodium sulfate is used to form stable Lubricating film, reducing friction and adhesion.
It improves the hardness and wear resistance of metal materials, reduces brittleness, and significantly improves the lubricating effect and surface quality.
Smart Images

Figure BDA0004803141280000091 
Figure BDA0004803141280000092 
Figure BDA0004803141280000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of warm forging technology and relates to a multi-section warm forging line. Background Art
[0002] Forging below the recrystallization temperature and above room temperature is usually called warm forging. Parts formed by warm forging technology have good quality, high precision, and save materials. It has been widely used in recent years. The purpose of using warm forging technology is to obtain high-quality precision forgings without the same forming force as cold forging. The application of warm forging technology is also closely related to the forging material, forging size, and complexity of the forging. Compared with hot forging, the surface of warm forged parts will not be strongly oxidized, the surface quality is good, the dimensional tolerance is small, and the working surface of the part can even be directly formed without subsequent machining. Compared with cold forging, although cold forging can obtain higher surface quality and dimensional accuracy, cold forging has stricter requirements on deformed materials and part shapes.
[0003] Lubricant is one of the key technologies in the warm forging process. In this temperature range, cold extrusion is applied to form a phosphate coating on the metal surface first, and then react with sodium stearate to form a metal soap lubricant layer, which decomposes above 200°C and the lubrication effect deteriorates. Zinc phosphate coating also begins to decompose and fail above 300°C. The oxalate coating used in cold extrusion of stainless steel is oxidized to iron oxide and carbon dioxide above 150°C. Therefore, the development of warm forging technology can be said to depend to a certain extent on finding some lubricants that are effective in this temperature range. Summary of the invention
[0004] The present invention relates to a multi-stage warm forging wire, and belongs to the technical field of warm forging process. The present invention discloses the process of the multi-stage warm forging wire as follows: (1) Lubricant is coated on the surface of a block-shaped metal material and heated, and the material is pressed using a hydraulic press. When the thickness of the pressed surface becomes half of the original thickness, the pressing is stopped and the surface is changed to continue pressing. After each surface is pressed twice, forging can be performed; (2) The pressed metal material is placed in a die cavity for forging; (3) The forged metal material is kept warm, and then cooled to remove stress to obtain a metal product. The warm forging process adopted by the present invention uses a hydraulic press to press the metal at a warm forging temperature before forging, so that the metal material grains are refined to form an ultrafine, uniform and non-directional grain structure, and the dislocation density is increased and the hardness is improved. At the same time, the lubricant has the anti-oxidation property, reduces friction, and plays a role in protecting metal materials.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A multi-stage warm forging line, the process of the multi-stage warm forging line comprises the following steps:
[0007] (1) Apply lubricant to the surface of the block-shaped metal material and heat it, and use a hydraulic press to press it. When the thickness of the pressed surface becomes half of the original, stop pressing and continue pressing on the other side. After completing two presses on each side, forging can be carried out;
[0008] (2) The pressed metal material is placed into the die cavity for forging;
[0009] (3) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
[0010] Furthermore, in the step (1), the metal material is carbon steel or alloy steel, and the lubricant accounts for 0.5-0.8% of the mass of the metal material.
[0011] Furthermore, the heating temperature in step (1) is 680-700° C., and the pressure of the hydraulic press is 200-250 MPa.
[0012] Furthermore, the forging temperature in step (2) is 750-900°C.
[0013] Furthermore, in the step (3), the temperature and time of the heat preservation are 700-750° C. and 15-25 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 90-120 min.
[0014] Furthermore, the lubricant is composed of the following raw materials in parts by weight: 20-25 parts of inorganic salt, 60-70 parts of water-based resin, and 10-13 parts of polymer.
[0015] Furthermore, the inorganic salt is composed of sodium borate, tricalcium phosphate and sodium sulfate in a mass ratio of 1:1:1, the water-based resin is one of acrylic resin, styrene-acrylic resin and polyurethane resin, and the polymer is polyamide-imide.
[0016] A process application of a multi-section warm forging wire, wherein the process of the multi-section warm forging wire is applied to the manufacture of bearings and automobile parts.
[0017] Beneficial effects of the present invention:
[0018] 1. Warm forging process Before forging, a hydraulic press is used to press the metal at the temperature of warm forging, so that the metal material grains are refined to form ultra-fine, uniform and non-directional grain structure, and the dislocation density is increased and the hardness is improved. After the forging is completed, the heat is kept for a period of time, and the stress is removed by cooling within the time range, ensuring that the hardness decreases less and preventing the brittleness of the metal product.
[0019] 2. Sodium borate can form a glass-like lubricating film, which helps to reduce the friction coefficient. Tricalcium phosphate can improve the lubrication effect between surfaces and has strong lubrication performance. Sodium sulfate can reduce the adhesion of the surface and further reduce friction. The three complement each other in the lubricant to form a more stable and effective lubricating film, thereby improving the lubrication effect and wear resistance. DETAILED DESCRIPTION
[0020] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.
[0021] Example 1
[0022] A multi-stage warm forging line, the process of the multi-stage warm forging line comprises the following steps:
[0023] (1) Apply lubricant to the surface of the block-shaped metal material and heat it, and use a hydraulic press to press it. When the thickness of the pressed surface becomes half of the original, stop pressing and continue pressing on the other side. After completing two presses on each side, forging can be carried out;
[0024] (2) The pressed metal material is placed into the die cavity for forging;
[0025] (3) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
[0026] In the step (1), the metal material is alloy steel, and the lubricant accounts for 0.5% of the mass of the metal material.
[0027] The heating temperature in step (1) is 680° C. and the pressure of the hydraulic press is 200 MPa.
[0028] The forging temperature in step (2) is 750°C.
[0029] The temperature and time of the heat preservation in the step (3) are 700° C. and 15 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 90 min.
[0030] The lubricant is composed of the following raw materials in parts by weight: 20 parts of inorganic salt, 60 parts of water-based resin, and 10 parts of polymer.
[0031] The inorganic salt is composed of sodium borate, tricalcium phosphate and sodium sulfate in a mass ratio of 1:1:1, the water-based resin is acrylic resin, and the polymer is polyamide-imide.
[0032] A process application of a multi-section warm forging line, wherein the process of the multi-section warm forging line is applied to the manufacture of bearings.
[0033] Example 2
[0034] A multi-stage warm forging line, the process of the multi-stage warm forging line comprises the following steps:
[0035] (1) Apply lubricant to the surface of the block-shaped metal material and heat it, and use a hydraulic press to press it. When the thickness of the pressed surface becomes half of the original, stop pressing and continue pressing on the other side. After completing two presses on each side, forging can be carried out;
[0036] (2) The pressed metal material is placed into the die cavity for forging;
[0037] (3) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
[0038] In the step (1), the metal material is carbon steel, and the lubricant accounts for 0.6% of the mass of the metal material.
[0039] The heating temperature in step (1) is 690° C. and the pressure of the hydraulic press is 220 MPa.
[0040] The forging temperature in step (2) is 800°C.
[0041] The temperature and time of the heat preservation in the step (3) are 720° C. and 20 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 110 min.
[0042] The lubricant is composed of the following raw materials in parts by weight: 22 parts of inorganic salt, 65 parts of water-based resin, and 12 parts of polymer.
[0043] The inorganic salt is composed of sodium borate, tricalcium phosphate and sodium sulfate in a mass ratio of 1:1:1, the water-based resin is styrene-acrylic resin, and the polymer is polyamide-imide.
[0044] A process application of a multi-section warm forging line, wherein the process of the multi-section warm forging line is applied to the manufacture of bearings.
[0045] Example 3
[0046] A multi-stage warm forging line, the process of the multi-stage warm forging line comprises the following steps:
[0047] (1) Apply lubricant to the surface of the block-shaped metal material and heat it, and use a hydraulic press to press it. When the thickness of the pressed surface becomes half of the original, stop pressing and continue pressing on the other side. After completing two presses on each side, forging can be carried out;
[0048] (2) The pressed metal material is placed into the die cavity for forging;
[0049] (3) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
[0050] In the step (1), the metal material is carbon steel, and the lubricant accounts for 0.8% of the mass of the metal material.
[0051] The heating temperature in step (1) is 700° C. and the pressure of the hydraulic press is 250 MPa.
[0052] The forging temperature in step (2) is 900°C.
[0053] The temperature and time of the heat preservation in the step (3) are 750° C. and 25 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 120 min.
[0054] The lubricant is composed of the following raw materials in parts by weight: 25 parts of inorganic salt, 70 parts of water-based resin, and 13 parts of polymer.
[0055] The inorganic salt is composed of sodium borate, tricalcium phosphate and sodium sulfate in a mass ratio of 1:1:1, the water-based resin is polyurethane resin, and the polymer is polyamide-imide.
[0056] A process application of a multi-section warm forging line, wherein the process of the multi-section warm forging line is applied to the manufacture of bearings.
[0057] Comparative Example 1
[0058] On the basis of Example 2, a multi-stage warm forging line, the process of the multi-stage warm forging line comprises the following steps:
[0059] (1) Put the metal material into the die cavity for forging;
[0060] (2) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
[0061] The forging temperature in the step (1) is 800°C.
[0062] The temperature and time of the heat preservation in the step (2) are 720° C. and 20 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 110 min.
[0063] The lubricant is composed of the following raw materials in parts by weight: 22 parts of inorganic salt, 65 parts of water-based resin, and 12 parts of polymer.
[0064] The inorganic salt is composed of sodium borate, tricalcium phosphate and sodium sulfate in a mass ratio of 1:1:1, the water-based resin is styrene-acrylic resin, and the polymer is polyamide-imide.
[0065] A process application of a multi-section warm forging line, wherein the process of the multi-section warm forging line is applied to the manufacture of bearings.
[0066] Comparative Example 2
[0067] On the basis of Example 2, the forged metal material was cooled to room temperature after 60 minutes, and other conditions were consistent with those in the example.
[0068] Comparative Example 3
[0069] On the basis of Example 2, the time for cooling the forged metal material to room temperature is 140 minutes, and other conditions are consistent with the example.
[0070] Comparative Example 4
[0071] On the basis of Example 2, a multi-stage warm forging line, the process of the multi-stage warm forging line comprises the following steps:
[0072] (1) Apply lubricant to the surface of the block-shaped metal material and heat it, and use a hydraulic press to press it. When the thickness of the pressed surface becomes half of the original, stop pressing and continue pressing on the other side. After completing two presses on each side, forging can be carried out;
[0073] (2) The pressed metal material is placed into the die cavity for forging;
[0074] (3) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
[0075] In the step (1), the metal material is carbon steel, and the lubricant accounts for 0.6% of the mass of the metal material.
[0076] The heating temperature in step (1) is 690° C. and the pressure of the hydraulic press is 220 MPa.
[0077] The forging temperature in step (2) is 800°C.
[0078] The temperature and time of the heat preservation in the step (3) are 720° C. and 20 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 110 min.
[0079] The lubricant is composed of the following raw materials in parts by weight: 22 parts of inorganic salt, 65 parts of water-based resin, and 12 parts of polymer.
[0080] The inorganic salt is composed of tricalcium phosphate and sodium sulfate in a mass ratio of 1:1, the water-based resin is styrene-acrylic resin, and the polymer is polyamide-imide.
[0081] A process application of a multi-section warm forging line, wherein the process of the multi-section warm forging line is applied to the manufacture of bearings.
[0082] Comparative Example 5
[0083] On the basis of Example 2, a multi-stage warm forging line, the process of the multi-stage warm forging line comprises the following steps:
[0084] (1) Apply lubricant to the surface of the block-shaped metal material and heat it, and use a hydraulic press to press it. When the thickness of the pressed surface becomes half of the original, stop pressing and continue pressing on the other side. After completing two presses on each side, forging can be carried out;
[0085] (2) The pressed metal material is placed into the die cavity for forging;
[0086] (3) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
[0087] In the step (1), the metal material is carbon steel, and the lubricant accounts for 0.6% of the mass of the metal material.
[0088] The heating temperature in step (1) is 690° C. and the pressure of the hydraulic press is 220 MPa.
[0089] The forging temperature in step (2) is 800°C.
[0090] The temperature and time of the heat preservation in the step (3) are 720° C. and 20 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 110 min.
[0091] The lubricant is composed of the following raw materials in parts by weight: 22 parts of inorganic salt, 65 parts of water-based resin, and 12 parts of polymer.
[0092] The inorganic salt is composed of sodium borate and sodium sulfate in a mass ratio of 1:1, the water-based resin is styrene-acrylic resin, and the polymer is polyamide-imide.
[0093] A process application of a multi-section warm forging line, wherein the process of the multi-section warm forging line is applied to the manufacture of bearings.
[0094] Comparative Example 6
[0095] On the basis of Example 2, a multi-stage warm forging line, the process of the multi-stage warm forging line comprises the following steps:
[0096] (1) Apply lubricant to the surface of the block-shaped metal material and heat it, and use a hydraulic press to press it. When the thickness of the pressed surface becomes half of the original, stop pressing and continue pressing on the other side. After completing two presses on each side, forging can be carried out;
[0097] (2) The pressed metal material is placed into the die cavity for forging;
[0098] (3) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
[0099] In the step (1), the metal material is carbon steel, and the lubricant accounts for 0.6% of the mass of the metal material.
[0100] The heating temperature in step (1) is 690° C. and the pressure of the hydraulic press is 220 MPa.
[0101] The forging temperature in step (2) is 800°C.
[0102] The temperature and time of the heat preservation in the step (3) are 720° C. and 20 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 110 min.
[0103] The lubricant is composed of the following raw materials in parts by weight: 22 parts of inorganic salt, 65 parts of water-based resin, and 12 parts of polymer.
[0104] The inorganic salt is composed of sodium borate and tricalcium phosphate in a mass ratio of 1:1, the water-based resin is styrene-acrylic resin, and the polymer is polyamide-imide.
[0105] A process application of a multi-section warm forging line, wherein the process of the multi-section warm forging line is applied to the manufacture of bearings.
[0106] Performance Testing
[0107] 1. Dislocation density test: The bearings manufactured in Examples 1-3 and Comparative Example 1 were cut in the middle to obtain samples with a size of 12 mm × 12 mm × 6 mm, and the two 12 mm × 12 mm surfaces of the samples were water-grinded using sandpaper from coarse to fine until the two surfaces were parallel and smooth. The samples were tested using an X-ray diffractometer model S8-TIGER, and the test data were imported into the Origin software to obtain the dislocation density;
[0108] Tensile property test: The tensile strength and elongation of the samples of Examples 1-3 and Comparative Examples 2-3 were tested according to the national standard GB / T238.1-2010. In addition, the hardness of the samples was tested using a HVS-1000 Vickers hardness tester.
[0109] 2. Friction and wear test: The bearings manufactured in Examples 1-3 and Comparative Examples 4-6 were cut into 12mm×12mm×4mm specimens respectively, and the two 12mm×12mm surfaces of the specimens were water-grinded using coarse to fine sandpaper until the two surfaces were parallel and smooth. Lubricant was applied to the surface of the specimens and the wear rate was tested on a HSR-2M reciprocating friction and wear tester. The wear rate calculation formula is as follows:
[0110]
[0111] Where m 0 is the mass of the sample before the wear test, m 1 is the mass of the sample after the wear test, ρ is the density of the sample, W is the load of the wear test, and L is the total length of reciprocating wear.
[0112] The above test results are shown in Table 1.
[0113] Table 1 Test results
[0114]
[0115]
[0116] From the data analysis in Table 1, it can be concluded that the dislocation density of Examples 1-3 is greater than that of Comparative Example 1. Since Comparative Example 1 lacks a pressing step, the grains cannot be refined and the hardness is also worse than that of the embodiment. A comprehensive analysis of the hardness, tensile strength and elongation of Examples 1-3 shows that their comprehensive performance is better than that of Comparative Examples 2-3. The cooling time of Comparative Example 2 is less than that of the embodiment, and rapid cooling obtains a greater hardness, but the brittleness increases, i.e., the elongation is the lowest. The cooling time of Comparative Example 3 is greater than that of the embodiment, and its brittleness is the lowest, but the hardness of the metal material is greatly reduced. The wear rate of Examples 1-3 is less than that of Comparative Examples 4-6. Since Comparative Examples 4-6 lack one of the lubricants sodium borate, tricalcium phosphate and sodium sulfate, the complementary effect of the three is weakened, so the wear resistance and lubricity are reduced.
[0117] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A process for multi-stage warm forging line, It is characterized in that The process of the multi-stage warm forging line comprises the following steps: (1) Apply lubricant to the surface of the block-shaped metal material and heat it, and use a hydraulic press to press it. When the thickness of the pressed surface becomes half of the original, stop pressing and continue pressing on the other side. After completing two presses on each side, forging can be carried out; The lubricant accounts for 0.5-0.8% of the mass of the metal material; The lubricant is composed of the following raw materials in parts by weight: 20-25 parts of inorganic salt, 60-70 parts of water-based resin, and 10-13 parts of polymer; The inorganic salt is composed of sodium borate, tricalcium phosphate and sodium sulfate in a mass ratio of 1:1:1, the water-based resin is one of acrylic resin, styrene-acrylic resin and polyurethane resin, and the polymer is polyamide-imide; (2) The pressed metal material is placed into the die cavity for forging; (3) The forged metal material is kept warm and then cooled to remove stress to obtain a metal product.
2. A process for a multi-stage warm forging line according to claim 1, It is characterized in that In the step (1), the metal material is carbon steel or alloy steel.
3. A process for a multi-stage warm forging wire according to claim 1, It is characterized in that The heating temperature in step (1) is 680-700° C., and the pressure of the hydraulic press is 200-250 MPa.
4. A process for a multi-stage warm forging wire according to claim 1, It is characterized in that The forging temperature in step (2) is 750-900°C.
5. A process for a multi-stage warm forging wire according to claim 1, It is characterized in that The temperature and time of the heat preservation in the step (3) are 700-750° C. and 15-25 min respectively, and the cooling refers to cooling to room temperature, and the cooling time to room temperature is 90-120 min.
6. An application of the process of a multi-stage warm forging wire as claimed in any one of claims 1 to 5, It is characterized in that The process of the multi-stage warm forging line is applied to the manufacture of bearings and automobile parts.
Citation Information
Patent Citations
Lubricant composition for metal material plasticity processing, lubricating film and coated metal material provided therewith, and method for manufacturing coated metal material
CN103154216A
Band-shaped lubricating material for dry wiredrawing and process for producing same
CN103649286A
Forging forming method for magnesium alloy rings
CN103736888A
Warming forging precision forming manufacture process for steering bearing ring of motorcycle
CN104139151A