An organic wax composite warm-mix agent based on plasma treatment and its application

By blending the organic wax composite temperature mixer with plasma treated with asphalt, the problem of insufficient low-temperature performance of warm-mixed asphalt composites is solved, the low-temperature toughening performance and high-temperature rutting resistance are improved, the preparation process is simplified, and the waste is realized Plastic recycling and energy conservation.

CN118530603BActive Publication Date: 2024-11-19ANHUI UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410970287.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-19
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing warm-mixed asphalt composites have shortcomings in low-temperature performance, and the preparation process is complicated, making it difficult to meet the improvement of low-temperature performance while ensuring high-temperature performance.

Method used

Using an organic wax composite warm mixer based on plasma treatment, the plasma-treated organic wax, low molecular weight modifier and antioxidant are mixed to prepare a composite warm mixer with viscosity reduction effect and mix it with asphalt. To improve the low-temperature toughening performance of warm-mixed asphalt composites.

Benefits of technology

The low-temperature toughening performance of warm-mixed asphalt composite materials is improved, while reducing the mixing temperature of asphalt, improving the high-temperature rutting resistance and deformation resistance, making up for the poor low-temperature performance and insufficient high-temperature rutting resistance in the existing technology. Defects, and the recycling of waste plastics and energy conservation are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118530603B_ABST
    Figure CN118530603B_ABST
Patent Text Reader

Abstract

The invention discloses an organic wax composite warm mix agent based on plasma treatment and its application, wherein the composite warm mix agent is a mixture of an organic wax treated with plasma, a low molecular weight modifier and an antioxidant. The organic wax composite warm mix agent of the invention can reduce the mixing temperature of asphalt, and has excellent viscosity reduction effect, low temperature plasticity and low temperature ductility, and can increase the resistance to permanent deformation, high elastic recovery and anti-rutting ability of asphalt composite materials, thereby extending their service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer composite materials, and in particular to an organic wax composite warm-mix agent based on plasma treatment and application thereof. Background Art

[0002] Hot mix asphalt (HMA) is widely used in my country's high-grade highways due to its good road performance and mature construction technology. However, it requires high mixing and construction temperatures (usually mixing temperature greater than 160℃, construction temperature greater than 150℃) during use, resulting in a large amount of energy consumption and toxic and harmful gas emissions. In order to reduce energy consumption and harmful gas emissions in road construction, domestic and foreign scholars have developed warm mix asphalt (WMA). WMA improves the workability and compactibility of asphalt mixtures through certain technical measures, so that it can be paved at a lower temperature (usually 100℃~150℃). At present, some wax-based warm mix agents have been used in asphalt composites because they can significantly reduce the high-temperature viscosity of asphalt and improve the adhesion between asphalt and aggregates. However, they will have a significant detrimental effect on the low-temperature performance of asphalt mixtures and are not suitable for use in northern regions. Therefore, in order to enhance the low-temperature performance of warm mix asphalt composites, some low-temperature plasticizers are usually added or the wax-based warm mix agent is plasma treated to change the chemical composition of the warm mix agent.

[0003] Patent CN202211188442.4 "A dispersant for improving the low temperature performance of waxy asphalt, asphalt and preparation method thereof" adds vinyl graphene oxide and 1-butyl-3-methylimidazolium chloride ionic liquid in a mass ratio of 1:1 into a four-necked flask containing initiator 2,2-azobisisobutyronitrile to prepare a vinyl graphene oxide modified ionic liquid nanocomposite as a dispersant. Although this method prepares a low-temperature asphalt dispersant, the method is cumbersome to prepare and is not suitable for large-scale production, and the high-temperature performance of the warm-mix asphalt composite is unknown.

[0004] Patent CN201910549263.0 "A method for improving the low-temperature crack resistance of Russian petroleum asphalt" uses SBS polymer modifiers and asphalt modifiers to modify Russian petroleum asphalt, then adds rubber cracking oil and stirs to obtain Russian modified asphalt. This method significantly improves the low-temperature crack resistance of Russian petroleum asphalt. However, the amount of rubber cracking oil added in this method is very high, the preparation is complicated, and only the low-temperature performance of the asphalt composite material is tested, and the high-temperature performance of the asphalt composite material is not tested.

[0005] The article "Effect of CO2 plasma modified multi-walled carbon nanotubes on the microstructure and properties of asphalt-based carbon materials" (Zhang Zuoqin, Pan Guixiang, Li Jie, et al. Effect of CO2 plasma modified multi-walled carbon nanotubes on the microstructure and properties of asphalt-based carbon materials [J]. Railway Standard Design, 2022, 66(09): 142-147+165.) uses CO2 as a plasma gas to modify the surface of multi-walled carbon nanotubes and graft oxygen-containing functional groups to CNTs, which is beneficial to enhance their dispersibility and bonding with asphalt. In addition, plasma modification only occurs on the surface of carbon nanotubes, which will not damage the nanotube structure and avoid the performance degradation of carbon nanotubes. However, this method only analyzes the compressive strength and resistivity of asphalt composites, and does not test the high and low temperature performance of asphalt composites.

[0006] Therefore, how to ensure that the warm mix agent reduces the viscosity of asphalt composite materials while meeting their required high temperature and low temperature properties, while having a simple preparation process, is of great significance to the promotion of warm mix asphalt technology. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide an organic wax composite warm mix agent based on plasma treatment and its application, aiming to improve the low-temperature toughening performance of warm mix asphalt composite materials.

[0008] In order to achieve the purpose, the present invention adopts the following technical scheme:

[0009] The invention discloses a plasma-treated organic wax composite warm-mix agent, which is characterized in that the organic wax composite warm-mix agent is mixed with plasma-treated organic wax, a low molecular weight modifier and an antioxidant.

[0010] Further, the organic wax includes at least one of plant wax, animal wax, cracking wax, petroleum wax and synthetic wax. Wherein, the preparation method of the cracking wax is: mixing the waste plastic with the catalyst in a twin-screw extruder, and then crushing the extruded product with a crusher to obtain a mixture of the waste plastic and the catalyst; placing the mixture of the waste plastic and the catalyst in a heat treatment furnace, heating and cracking under a nitrogen gas atmosphere to obtain cracking wax. As a preferred embodiment: the waste plastic includes at least one of polyethylene, polypropylene, polystyrene, rubber powder and ethylene-vinyl acetate copolymer. The catalyst is at least one of amorphous aluminosilicate and zeolite molecular sieve. The mass ratio of the catalyst to the waste plastic is 1:5~15. The main engine speed of the twin-screw extruder in the mixing is 300~600 r / min, the barrel temperature is 150~200℃, the feeding frequency is 3~6r / min, and the mixing time is 5~15 min; the heating and cracking temperature in the heat treatment furnace is 350~500℃, and the heating and cracking time is 2~5 h.

[0011] Furthermore, the method for obtaining the organic wax treated by plasma is as follows: placing the organic wax in the treatment chamber of the plasma device, energizing and evacuating, starting the reactive gas after the vacuum is stable, adjusting the RF power, and timing the treatment, and after the treatment is completed, turning off the power supply and the vacuum pump in turn, opening the treatment chamber to take out the sample, obtaining the plasma-treated organic wax, and sealing and storing it. Preferably, the reactive gas comprises one or a combination of oxygen and ammonia. During the treatment, the pressure in the treatment chamber is stabilized at 10 -1 ~10 -5 Pa, the plasma discharge mode is radio frequency discharge, the plasma processing time is 3~7min, and the plasma discharge power is 50~150W.

[0012] Furthermore, the preparation method of the organic wax composite warm-mix agent based on plasma treatment is: adding the plasma-treated organic wax, low molecular weight modifier, and antioxidant to a twin-screw extruder for melt blending in a mass ratio of 70-90:10-30:1, and extruding to obtain the organic wax composite warm-mix agent based on plasma treatment. Preferably, the barrel temperature of the twin-screw extruder is 200-250°C, the main engine speed is 400-700 r / min, the feeding frequency is 5-8 r / min, and the mixing time is 10-20min.

[0013] Further, the low molecular weight modifier is at least one of stearate, metal soap heat stabilizer, stearyl glyceride, silicate, pentaerythritol stearate, ethylene bis stearamide, and the molecular weight of the low molecular weight modifier is 300 to 1000; the antioxidant is at least one of tea polyphenols, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and diphenyl octyl phosphite. Preferably, the stearate is any one of sodium stearate, magnesium stearate, and aluminum stearate.

[0014] The organic wax composite warm mix agent based on plasma treatment prepared by the above method can be directly used in asphalt pavement construction to enhance the low temperature performance of asphalt pavement and increase the scope of warm mix asphalt pavement road construction. The specific method can be: adding the composite warm mix agent to the base asphalt through melt blending and high-speed shearing to obtain a warm mix asphalt composite material, and the mass ratio of the composite warm mix agent to the asphalt is 1-3:100.

[0015] Furthermore, the matrix asphalt is one or any combination of 70#, 90#, SBS modified asphalt and high viscosity asphalt.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0017] 1. The present invention first uses plasma technology to treat organic wax, then mixes the plasma-treated organic wax, low molecular weight modifier and antioxidant to obtain a composite warm mix agent, and finally blends the composite warm mix agent with asphalt to obtain a warm mix asphalt composite material. The organic wax in the composite warm mix agent provided by the present invention has a viscosity-reducing effect on asphalt, and plasma treatment can reduce the crystallinity of the organic wax, increase the surface energy of the organic wax, improve the reaction activity, enhance the ability of the organic wax to absorb light components, improve the bonding of the organic wax and asphalt, reduce the cohesion of the warm mix asphalt, improve the low-temperature plasticity and low-temperature ductility of the asphalt, and improve the low-temperature toughening performance of the warm mix asphalt composite material, which can be used for the laying of asphalt pavements in northern regions. The low molecular weight modifier is inserted between asphalt molecules to enhance the intermolecular force, thereby improving the high-temperature rutting resistance and high-temperature deformation resistance of the asphalt composite material. The composite warm mix agent of the present invention makes up for the defects of the existing warm mix asphalt materials such as poor low-temperature performance and insufficient high-temperature rutting resistance.

[0018] 2. The surface of the organic wax treated with plasma is effectively "etched" to form oxygen anions or nitrogen cations, which can enhance the complexation between the metal cations or anions between the organic wax and low molecular weight modifiers such as stearate, and further improve the interfacial compatibility between the organic wax and the low molecular weight modifiers.

[0019] 3. The organic wax in the composite warm mix agent of the present invention can be obtained by cracking waste plastics, thereby realizing the recycling of waste plastics, reducing energy waste, and helping to reduce white pollution, realizing the concept of energy conservation and environmental protection, and greatly reducing production costs.

[0020] 4. The organic wax composite warm mix agent of the present invention can reduce the mixing temperature of asphalt, and has excellent viscosity reduction effect, low temperature plasticity and low temperature ductility, and can increase the resistance to permanent deformation, high elastic recovery and anti-rutting ability of asphalt composite materials, thereby extending their service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 FTIR graphs of the cracked wax prepared in Example 1 of the present invention after being treated with plasma under different conditions.

[0022] Figure 2 This is the XPS graph of the pyrolysis wax prepared in Example 1 of the present invention after being treated with plasma under different conditions.

[0023] Figure 3 is the phase angle of the warm mix asphalt composite material obtained in Examples 1 to 3 of the present invention and Comparative Example 1.

[0024] Figure 4 It is the high temperature complex shear modulus of the warm mix asphalt composite materials obtained in Examples 1 to 3 of the present invention and Comparative Example 1.

[0025] Figure 5 It is the high temperature rutting factor of the warm mix asphalt composite material obtained in Examples 1 to 3 of the present invention and Comparative Example 1.

[0026] Figure 6 It is the low temperature complex shear modulus of the warm mix asphalt composite materials obtained in Examples 1 to 3 of the present invention and Comparative Example 1.

[0027] Figure 7 It is the low temperature rutting factor of the warm mix asphalt composite material obtained in Examples 1 to 3 of the present invention and Comparative Example 1.

[0028] Figure 8 It is the low temperature complex shear modulus of the warm mix asphalt composite materials obtained in Examples 4 to 6 of the present invention and Comparative Example 1.

[0029] Fig. 9 It is the low temperature rutting factor of the warm mix asphalt composite material obtained in Examples 4 to 6 of the present invention and Comparative Example 1.

[0030] Fig.10 It is the low temperature complex shear modulus of the warm mix asphalt composite material obtained in Example 3 of the present invention and Comparative Examples 2 to 4.

[0031] Fig.11 It is the low temperature rutting factor of the warm mix asphalt composite material obtained in Example 3 of the present invention and Comparative Examples 2 to 4. DETAILED DESCRIPTION

[0032] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.

[0033] Example 1

[0034] This embodiment provides an organic wax composite warm mix agent based on plasma treatment and its application, comprising the following steps:

[0035] 1. Add 5 g of zeolite molecular sieve and 50 g of waste polyethylene into a twin-screw extruder for mixing. The main speed of the extruder is 400 r / min, the barrel temperature is 160°C, the feeding frequency is 4r / min, and the mixing time is 10 min. Then crush the extruded product with a crusher to obtain a mixture of waste polyethylene and catalyst. Add the mixture of waste polyethylene and catalyst into a heat treatment furnace, first pass nitrogen for 30 min, and then heat to 350°C at a heating rate of 5°C / min in a nitrogen atmosphere for 2 h. Wait for the heat treatment furnace to cool to room temperature and take out the obtained cracking wax.

[0036] 2. Place the cracked wax into the treatment chamber of the plasma device, power on and evacuate the chamber to stabilize the pressure at 10-1 After the pressure is within the range of 0.04 Pa, start the oxygen, adjust the RF power to 100 W, and time for 5 min. Then turn off the power supply and vacuum pump in turn, open the treatment chamber and take out the sample to obtain the plasma-treated pyrolysis wax.

[0037] 3. Weigh 10 parts of low molecular weight modifier aluminum stearate, 90 parts of plasma-treated cracked wax and 1 part of tea polyphenols, control the barrel temperature of the twin-screw extruder to 200°C, the main engine speed to 500 r / min, the feeding frequency to 6 r / min, and the mixing time to 15 min. After mixing the three evenly, an organic wax composite warm-mix agent is obtained.

[0038] 4. Weigh 3 parts of organic wax composite warm mix agent and 100 parts of 70# asphalt, raise the temperature to 160℃, wait until the asphalt is completely melted, and use a high-speed shearing machine to shear at a speed of 3000 rpm for 30 min. After shearing, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite material containing an organic wax composite warm mix agent.

[0039] Example 2

[0040] This embodiment provides an organic wax composite warm mix agent based on plasma treatment and its application, comprising the following steps:

[0041] 1. Add 5 g of zeolite molecular sieve and 50 g of waste polyethylene into a twin-screw extruder for mixing. The main speed of the extruder is 400 r / min, the barrel temperature is 160°C, the feeding frequency is 4r / min, and the mixing time is 10 min. Then crush the extruded product with a crusher to obtain a mixture of waste polyethylene and catalyst. Add the mixture of waste polyethylene and catalyst into a heat treatment furnace, first pass nitrogen for 30 min, and then heat to 350°C at a heating rate of 5°C / min in a nitrogen atmosphere for 2 h. Wait for the heat treatment furnace to cool to room temperature and take out the obtained cracking wax.

[0042] 2. Place the cracked wax into the treatment chamber of the plasma device, power on and evacuate the chamber to stabilize the pressure at 10 -1 After the pressure is within the range of 0.04 Pa, start the oxygen, adjust the RF power to 100 W, and time for 5 min. Then turn off the power supply and vacuum pump in turn, open the treatment chamber and take out the sample to obtain the plasma-treated pyrolysis wax.

[0043] 3. Weigh 20 parts of low molecular weight modifier aluminum stearate, 80 parts of plasma-treated cracked wax and 1 part of tea polyphenols, control the barrel temperature of the twin-screw extruder to 200°C, the main engine speed to 500 r / min, the feeding frequency to 6 r / min, and the mixing time to 15 min. After mixing the three evenly, an organic wax composite warm-mix agent is obtained.

[0044] 4. Weigh 3 parts of organic wax composite warm mix agent and 100 parts of 70# asphalt, raise the temperature to 160℃, wait until the asphalt is completely melted, and use a high-speed shearing machine to shear at a speed of 3000 rpm for 30 min. After shearing, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite material containing an organic wax composite warm mix agent.

[0045] Example 3

[0046] This embodiment provides an organic wax composite warm mix agent based on plasma treatment and its application, comprising the following steps:

[0047] 1. Add 5 g of zeolite molecular sieve and 50 g of waste polyethylene into a twin-screw extruder for mixing. The main speed of the extruder is 400 r / min, the barrel temperature is 160°C, the feeding frequency is 4r / min, and the mixing time is 10 min. Then crush the extruded product with a crusher to obtain a mixture of waste polyethylene and catalyst. Add the mixture of waste polyethylene and catalyst into a heat treatment furnace, first pass nitrogen for 30 min, and then heat to 350°C at a heating rate of 5°C / min in a nitrogen atmosphere for 2 h. Wait for the heat treatment furnace to cool to room temperature and take out the obtained cracking wax.

[0048] 2. Place the cracked wax into the treatment chamber of the plasma device, power on and evacuate the chamber to stabilize the pressure at 10 -1 After the pressure is within the range of 0.04 Pa, start the oxygen, adjust the RF power to 100 W, and time for 5 min. Then turn off the power supply and vacuum pump in turn, open the treatment chamber and take out the sample to obtain the plasma-treated pyrolysis wax.

[0049] 3. Weigh 30 parts of low molecular weight modifier aluminum stearate, 70 parts of plasma-treated cracked wax and 1 part of tea polyphenols, control the barrel temperature of the twin-screw extruder to 200°C, the main engine speed to 500 r / min, the feeding frequency to 6 r / min, and the mixing time to 15 min. After mixing the three evenly, an organic wax composite warm-mix agent is obtained.

[0050] 4. Weigh 3 parts of organic wax composite warm mix agent and 100 parts of 70# asphalt, raise the temperature to 160℃, wait until the asphalt is completely melted, and use a high-speed shearing machine to shear at a speed of 3000 rpm for 30 min. After shearing, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite material containing an organic wax composite warm mix agent.

[0051] Example 4

[0052] This embodiment provides an organic wax composite warm mix agent based on plasma treatment and its application, comprising the following steps:

[0053] 1. Add 5 g of zeolite molecular sieve and 50 g of waste polyethylene into a twin-screw extruder for mixing. The main speed of the extruder is 400 r / min, the barrel temperature is 160°C, the feeding frequency is 5r / min, and the mixing time is 10 min. Then crush the extruded product with a crusher to obtain a mixture of waste polyethylene and catalyst. Add the mixture of waste polyethylene and catalyst into a heat treatment furnace, first pass nitrogen for 30 min, and then heat to 350°C at a heating rate of 5°C / min in a nitrogen atmosphere for 2 h. Wait for the heat treatment furnace to cool to room temperature and take out the obtained cracking wax.

[0054] 2. Place the pyrolysis wax and animal wax in the treatment chamber of the plasma device at a mass ratio of 1:1, turn on the power to evacuate the chamber, and stabilize the pressure in the chamber at 10 -1 Pa, start the oxygen, adjust the RF power to 100 W, and time for 5 min. Then turn off the power and vacuum pump in turn, open the treatment chamber and take out the sample to obtain the plasma-treated organic wax.

[0055] 3. Weigh 30 parts of low molecular weight modifier sodium stearate, 70 parts of plasma-treated organic wax and 1 part of tea polyphenols, control the barrel temperature of the twin-screw extruder to 200°C, the main engine speed to 400 r / min, the feeding frequency to 5 r / min, and the mixing time to 10 min. After mixing the three evenly, an organic wax composite warm mix agent is obtained.

[0056] 4. Weigh 3 parts of organic wax composite warm mix agent and 100 parts of 70# asphalt, raise the temperature to 160℃, wait until the asphalt is completely melted, and use a high-speed shearing machine to shear at a speed of 3000 rpm for 30 min. After shearing, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite material containing an organic wax composite warm mix agent.

[0057] Example 5

[0058] This embodiment provides an organic wax composite warm mix agent based on plasma treatment and its application, comprising the following steps:

[0059] 1. Add 5 g of zeolite molecular sieve and 50 g of waste polyethylene into a twin-screw extruder for mixing. The main speed of the extruder is 400 r / min, the barrel temperature is 160°C, the feeding frequency is 4r / min, and the mixing time is 10 min. Then crush the extruded product with a crusher to obtain a mixture of waste polyethylene and catalyst. Add the mixture of waste polyethylene and catalyst into a heat treatment furnace, first pass nitrogen for 30 min, and then heat to 350°C at a heating rate of 5°C / min in a nitrogen atmosphere for 2 h. Wait for the heat treatment furnace to cool to room temperature and take out the obtained cracking wax.

[0060] 2. Place the pyrolysis wax and animal wax in the treatment chamber of the plasma device at a mass ratio of 1:1, turn on the power to evacuate the chamber, and stabilize the pressure in the chamber at 10 -1 After the pressure is within the range of 0.04 Pa, start the oxygen, adjust the RF power to 100 W, and time for 6 min. Then turn off the power supply and vacuum pump in turn, open the treatment chamber and take out the sample to obtain the plasma-treated organic wax.

[0061] 3. Weigh 30 parts of low molecular weight modifier magnesium stearate, 70 parts of plasma-treated organic wax and 1 part of tea polyphenols, control the barrel temperature of the twin-screw extruder to 200°C, the main engine speed to 600 r / min, the feeding frequency to 7 r / min, and the mixing time to 20 min. After mixing the three evenly, an organic wax composite warm-mix agent is obtained.

[0062] 4. Weigh 3 parts of organic wax composite warm mix agent and 100 parts of 70# asphalt, raise the temperature to 160℃, wait until the asphalt is completely melted, and use a high-speed shearing machine to shear at a speed of 3000 rpm for 30 min. After shearing, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite material containing an organic wax composite warm mix agent.

[0063] Example 6

[0064] This embodiment provides an organic wax composite warm mix agent based on plasma treatment and its application, comprising the following steps:

[0065] 1. Add 5 g of zeolite molecular sieve and 50 g of waste polyethylene into a twin-screw extruder for mixing. The main speed of the extruder is 400 r / min, the barrel temperature is 160°C, the feeding frequency is 4r / min, and the mixing time is 10 min. Then crush the extruded product with a crusher to obtain a mixture of waste polyethylene and catalyst. Add the mixture of waste polyethylene and catalyst into a heat treatment furnace, first pass nitrogen for 30 min, and then heat to 350°C at a heating rate of 5°C / min in a nitrogen atmosphere for 2 h. Wait for the heat treatment furnace to cool to room temperature and take out the obtained cracking wax.

[0066] 2. Place the pyrolysis wax and animal wax in the treatment chamber of the plasma device at a mass ratio of 1:1, turn on the power to evacuate the chamber, and stabilize the pressure in the chamber at 10 -1 Pa, start ammonia gas, adjust the RF power to 100 W, and time for 7 min. Then turn off the power supply and vacuum pump in turn, open the treatment chamber and take out the sample to obtain the plasma-treated organic wax.

[0067] 3. Weigh 30 parts of low molecular weight modifier aluminum stearate, 70 parts of plasma-treated organic wax and 1 part of tea polyphenols, control the barrel temperature of the twin-screw extruder to 200°C, the main engine speed to 500 r / min, the feeding frequency to 6 r / min, and the mixing time to 15 min. After mixing the three evenly, an organic wax composite warm-mix agent is obtained.

[0068] 4. Weigh 3 parts of organic wax composite warm mix agent and 100 parts of 70# asphalt, raise the temperature to 160℃, wait until the asphalt is completely melted, and use a high-speed shearing machine to shear at a speed of 3000 rpm for 30 min. After shearing, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite containing a wax-based composite warm mix agent.

[0069] Comparative Example 1

[0070] Weigh 100 parts of 70# asphalt, heat it to 160°C, and then use a high-speed shearing machine to shear at a shear rate of 3000rpm and a shearing time of 30 min. After shearing, pour it into a silicone mold while it is hot to obtain the asphalt material.

[0071] Comparative Example 2

[0072] Weigh 3 parts of the plasma-treated cracking wax prepared in Example 3, weigh 100 parts of 70# asphalt, heat to 160°C, wait until the asphalt is completely melted, and use a high-speed shearing machine for shearing. The shearing speed is 3000 rpm and the shearing time is 30 min. After the shearing is completed, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite material.

[0073] Comparative Example 3

[0074] Weigh 30 parts of low molecular weight modifier aluminum stearate, 70 parts of pyrolysis wax obtained in Example 3 without plasma treatment and 1 part of tea polyphenols, and mix them. Control the barrel temperature of the twin-screw extruder to 200°C, the main engine speed to 500 r / min, the feeding frequency to 6 r / min, and the mixing time to 15 min. After the three are evenly mixed, a composite warm mix agent is obtained.

[0075] Weigh 100 parts of 70# asphalt and 3 parts of composite warm mix agent, heat to 160℃, wait until the asphalt is completely melted, use a high-speed shearing machine to shear, the shearing machine speed is 3000 rpm, and the shearing time is 30 min. After the shearing is completed, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite material.

[0076] Comparative Example 4

[0077] Weigh 3 parts of the unplasma-treated cracked wax prepared in Example 3 and 100 parts of 70# asphalt, heat to 160°C, wait until the asphalt is completely melted, and shear with a high-speed shearing machine at a shearing speed of 3000 rpm and a shearing time of 30 min. After shearing, pour it into a silicone mold while hot to obtain a warm-mix asphalt composite material.

[0078] Figure 1 The FTIR graphs of the pyrolysis wax prepared in Example 1 after plasma treatment for different time periods are shown. From the comparison of the spectra before and after the treatment, it is found that no new characteristic peaks appear in the infrared spectrum of the pyrolysis wax after treatment, which indicates that the plasma treatment of the pyrolysis wax does not cause any changes in the functional groups.

[0079] Figure 2 The XPS graphs of the pyrolysis wax prepared in Example 1 after plasma treatment for different time periods show that a clear oxygen peak can be seen in the XPS graph of the pyrolysis wax after treatment, which indicates that plasma increases the oxygen content of the pyrolysis wax.

[0080] According to the AASHTO T 315-2020 standard, the high temperature performance and low temperature performance of the asphalt composite materials of Examples 1-6 and Comparative Examples 1-4 were tested as follows using the MCR 702 advanced rheometer produced by Anton Paar GmbH of Austria:

[0081] (1) Temperature function phase angle measurement: Based on the temperature sweep test, the temperature function phase angle of warm mix asphalt composite is tested by dynamic shear rheometer (DSR). By applying sinusoidal alternating shear stress, the mechanical response of the sample is measured at different temperatures to evaluate the viscoelastic properties and temperature sensitivity of the warm mix agent.

[0082] (2) Complex shear modulus test: Based on the temperature sweep test, the complex shear modulus test of warm mix asphalt composite is carried out by dynamic shear rheometer (DSR). By applying sinusoidal alternating shear stress, the mechanical response of the sample is measured under different frequency and temperature conditions to evaluate the strain hardening ability and deformation recovery performance of the warm mix agent.

[0083] (3) Rutting test: Based on the temperature sweep test, the warm mix asphalt composite is subjected to a rutting test using a dynamic shear rheometer (DSR). Under a certain load and temperature, the wheels are rolled on the sample, and the rutting depth and rutting width are measured to evaluate the anti-rutting performance of the warm mix.

[0084] Depend on Figure 3 It can be seen that the phase angle of warm mix asphalt composite materials has decreased, and the phase angle is lowest when the mass ratio of plasma treated cracked wax to low molecular weight modifier is the largest, indicating that the viscosity reduction effect is the best at this time. Figure 4 and Figure 5It can be seen that the high-temperature complex shear modulus and high-temperature rutting factor of the warm-mix asphalt composite material using the composite warm-mix agent are greater than those of the comparative example 1, indicating that its high-temperature performance is better than that of the comparative example. The high-temperature complex shear modulus and high-temperature rutting factor are the largest when the mass ratio of the plasma-treated pyrolysis wax to the low molecular weight modifier is the smallest, indicating that the high-temperature performance is the best at this time. Figure 6 and Figure 7 It can be seen that the low-temperature complex shear modulus and low-temperature rutting factor are the largest when the mass ratio of plasma-treated pyrolysis wax to low molecular weight modifier is the largest, indicating that its low-temperature performance is better than that of comparative example 1. In summary, when the mass ratio of plasma-treated organic wax to low molecular weight modifier is 7:3 (Example 3), the warm-mix asphalt composite material of the present invention has the best high and low temperature performance. Figure 8 and Fig. 9 It can be seen that the low-temperature complex shear modulus and low-temperature rutting factor of the samples obtained in Examples 4 to 6 are higher than those in Comparative Example 1, indicating that their low-temperature performance is better than that of Comparative Example 1. It can be seen that the organic wax composite warm mix agent prepared by plasma treatment of pyrolysis wax or plasma treatment of a mixture of pyrolysis wax and animal wax, and then mixing with a low molecular weight modifier and an antioxidant can improve the low-temperature performance of warm-mix asphalt composite materials.

[0085] Depend on Fig.10 and Fig.11 It can be seen that the low-temperature complex shear modulus and low-temperature rutting factor of the warm-mix asphalt composite material using the composite warm-mix agent are greater than those of Comparative Examples 2, 3, and 4, indicating that the composite warm-mix agent made of plasma-treated organic wax and low molecular weight modifier has a better improvement in the low-temperature performance of the warm-mix asphalt composite material.

[0086] Finally, it should be noted that the above is only a preferred embodiment of the present invention and not a limitation on the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An organic wax composite warm mix agent based on plasma treatment, characterized in that: The organic wax composite warm mix agent is formed by mixing plasma-treated cracked wax, a low molecular weight modifier and an antioxidant, wherein the mass ratio of the plasma-treated cracked wax, the low molecular weight modifier and the antioxidant is 70-90:10-30:1; The method for obtaining the plasma-treated cracked wax is as follows: placing the cracked wax in a treatment chamber of a plasma device, evacuating the chamber, starting the reactive gas after the vacuum is stable, adjusting the radio frequency power, and timing the treatment. After the treatment is completed, the sample is taken out to obtain the plasma-treated cracked wax, which is then sealed and stored; the reactive gas is oxygen; during the treatment, the pressure in the treatment chamber is stabilized at 10 -1 ~10 -5 Pa, the plasma discharge mode is radio frequency discharge, the plasma processing time is 3~7 min, and the plasma discharge power is 50~150 W.

2. The organic wax composite warm mix agent based on plasma treatment according to claim 1, characterized in that: The preparation method of the cracking wax comprises: mixing waste plastics and a catalyst in a twin-screw extruder, and then crushing the extruded product with a crusher to obtain a mixture of waste plastics and the catalyst; and heating and cracking the mixture of waste plastics and the catalyst under a nitrogen gas atmosphere to obtain the cracking wax.

3. The organic wax composite warm mix agent based on plasma treatment according to claim 2, characterized in that: The waste plastics include at least one of polyethylene, polypropylene, polystyrene and ethylene-vinyl acetate copolymer; the catalyst is at least one of amorphous aluminosilicate and zeolite molecular sieve.

4. The organic wax composite warm mix agent based on plasma treatment according to claim 2, characterized in that: The mass ratio of the catalyst to the waste plastic is 1:5-15; during the mixing, the main engine speed of the twin-screw extruder is 300-600 r / min, the barrel temperature is 150-200°C, the feeding frequency is 3-6 r / min, and the mixing time is 5-15 min; the heating and cracking temperature is 350-500°C, and the heating and cracking time is 2-5 h.

5. The organic wax composite warm mix agent based on plasma treatment according to claim 1, characterized in that: The preparation method of the plasma-treated organic wax composite warm-mix agent comprises the following steps: adding plasma-treated cracked wax, a low molecular weight modifier and an antioxidant into a twin-screw extruder in a mass ratio of 70-90:10-30:1 for melt blending, and extruding to obtain the plasma-treated organic wax composite warm-mix agent.

6. The organic wax composite warm mix agent based on plasma treatment according to claim 5, characterized in that: The barrel temperature of the twin-screw extruder is 200-250°C, the main engine speed is 400-700 r / min, the feeding frequency is 5-8 r / min, and the mixing time is 10-20 min.

7. The organic wax composite warm mix agent based on plasma treatment according to claim 1 or 5, characterized in that: The low molecular weight modifier is at least one of stearate, metal soap heat stabilizer, stearic acid glyceryl ester, silicate, pentaerythritol stearate, and ethylene bis stearamide, and the molecular weight of the low molecular weight modifier is 300-1000; the antioxidant is at least one of tea polyphenols, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and diphenyl octyl phosphite.

8. Use of the organic wax composite warm mix agent based on plasma treatment as described in any one of claims 1 to 7 in asphalt.

Citation Information

Patent Citations

  • Method for improving low temperature crack resistance of Russian petroleum asphalt

    CN110204912A

  • Dispersing agent for improving low-temperature performance of waxy asphalt and asphalt and preparation method thereof

    CN115368747A

  • Paraffin powder material for 3D printing

    CN108641359A

  • Prefabricated low-temperature-resistant rubber asphalt waterproof coiled material and preparation method thereof

    CN115353817A

  • Composite warm mixing material based on waste polyolefin catalytic cracking product and application of composite warm mixing material