A high-performance mildew-proof and antibacterial matte beauty edge adhesive and preparation method thereof

By preparing processed hollow silica and nano-titanium dioxide as matte agents and anti-mildew and antibacterial agents, combined with ingredients such as α,ω-dihydroxypolydimethylsiloxane, we solve the problem of adding matte agents to beauty edge glue. And the problem of performance degradation after anti-fungal and anti-bacterial agents has been achieved, a high-performance beauty edge glue has been realized.

CN118530691BActive Publication Date: 2024-10-29SHANDONG WOSAI NEW MATERIALS TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411017146.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-29
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

After adding matte agents and anti-mildew and anti-bacterial agents to the existing beauty edge-tightening adhesives, the extrusion and storage resistance are deteriorated, the adhesion and weather resistance are reduced, and the anti-mold and anti-bacterial properties are insufficient.

Method used

By preparing hollow silica and nano-titanium dioxide, they are subjected to amination, carboxylation, esterification, silanization, chelation and other treatments respectively to form an efficient matte agent and anti-mildew and anti-bacterial agent, and combine α, ω in the mixture. -Ingredients such as dihydroxypolydimethylsiloxane can improve the gloss, anti-fungal and antibacterial properties and mechanical properties of the beauty edge glue.

Benefits of technology

It achieves low gloss, excellent mildew and antibacterial properties, extrudability, storage resistance, adhesion and weather resistance, ensuring the high performance of the beauty edge tape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a high-performance anti-mildew and antibacterial matte beauty edge glue and preparation method thereof, belongs to the technical field of beauty edge glue, and the preparation method is composed of the following steps: prepare matte agent, prepare anti-mildew and antibacterial agent, and mix; the method of the mixing is, α, ω-dihydroxy polydimethylsiloxane, matte agent are added to a kneader for dehydration, then cooled to room temperature, and base material is obtained; base material, dimethicone, anti-mildew and antibacterial agent, methyl tributanoximosilane, phenyl tributanoximosilane, 3-aminopropyl triethoxysilane, dibutyl tin dilaurate are added to a high-speed mixer for high-speed stirring, and high-performance anti-mildew and antibacterial matte beauty edge glue is obtained. The matte beauty edge glue prepared by the present invention has low gloss, has excellent anti-mildew and antibacterial property, extrudability, storage resistance, heat resistance, and also has excellent bonding force, tear strength, tensile strength, elongation, weather resistance, and moisture resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of beauty edge finishing adhesives, and in particular to a high-performance mildew-proof and antibacterial matte beauty edge finishing adhesive and a preparation method thereof. Background Art

[0002] Beauty edge glue, also known as "beauty glue", "edge sealing glue" and "glass glue", is a new type of home edge material. Beauty edge glue is a material that bonds and seals various glasses with other substrates. It is mainly divided into silicone glue and polyurethane glue. Among them, silicone glue has strong adhesion, high strength, high elongation, and excellent weather resistance, moisture resistance, and odor resistance. In addition, it has a wide range of applicability and can achieve bonding between most building materials products, so it has great application value.

[0003] The main component of silicone glue is polydimethylsiloxane, which is composed of silicon atoms and oxygen atoms arranged alternately, and silicon atoms and oxygen atoms form silicon-oxygen bonds. Polydimethylsiloxane has both the stability and high temperature resistance of inorganic silicon compounds and the high elasticity and flexibility of organic silicon compounds. In addition to polydimethylsiloxane, auxiliary ingredients such as curing agents and catalysts are also added to silicone glue. According to the classification of small molecules released during the curing process, silicone glue is mainly divided into deacetated silicone glue, dealcoholized silicone glue, deaminated silicone glue, and deacrylic silicone glue; according to the appearance classification, silicone glue is mainly divided into matte silicone glue and glossy silicone glue.

[0004] With the development of the beauty edge glue industry, people have higher and higher requirements for the appearance of beauty edge glue. Since matte silicone glue has low gloss, natural color, strong concealment and good decorative effect, people's demand for matte silicone glue is increasing. Matting agent is added in the preparation process of matte silicone glue. Currently, commonly used matting agents include silicon dioxide, calcium carbonate, aluminum hydroxide, etc. Matting agent forms an uneven surface on the surface of the cured beauty edge glue, increases the scattering of light, and reduces the reflection of light, thereby achieving a matte effect.

[0005] However, when adding the matte agent to the silicone adhesive to prepare the matte silicone adhesive, it was found that the addition of the matte agent would affect the extrusion properties of the silicone adhesive. In addition, it would also cause the storage resistance of the silicone adhesive to deteriorate, which is manifested by the easy occurrence of precipitation at the bottom during long-term storage.

[0006] In addition, since silicone glue itself does not have antifungal and antibacterial properties, in the preparation of silicone glue, in order to improve the antifungal and antibacterial properties of silicone glue, it is necessary to add antifungal and antibacterial agents. Currently, commonly used antifungal and antibacterial agents include organic antifungal and antibacterial agents and inorganic antifungal and antibacterial agents. Among them, organic antifungal and antibacterial agents include quaternary ammonium salt antifungal and antibacterial agents, biguanide antifungal and antibacterial agents, organic metal antifungal and antibacterial agents, pyridine antifungal and antibacterial agents, isothiazolinone antifungal and antibacterial agents, etc., and inorganic antifungal and antibacterial agents include metal inorganic salts, nano titanium dioxide, nano zinc oxide, nano silver, etc. Among them, organic antifungal and antibacterial agents have the advantages of broad-spectrum sterilization and fast sterilization speed, but poor heat resistance, and inorganic antifungal and antibacterial agents have the advantages of good heat resistance and broad-spectrum sterilization. Therefore, the most commonly used antifungal and antibacterial agents in silicone glue are inorganic antifungal and antibacterial agents.

[0007] However, the following problems were found after adding inorganic antifungal and antibacterial agents to matte silicone adhesive: First, the antifungal and antibacterial properties of inorganic antifungal and antibacterial agents are lower than those of organic antifungal and antibacterial agents; second, since both inorganic antifungal and antibacterial agents and matting agents are inorganic powders, excessive addition of inorganic powders will further lead to the deterioration of the extrusion and storage resistance of the silicone adhesive; third, the simultaneous addition of inorganic antifungal and antibacterial agents and matting agents will also lead to the deterioration of the adhesion, tear strength, tensile strength and elongation of the silicone adhesive; fourth, the simultaneous addition of inorganic antifungal and antibacterial agents and matting agents will also affect the distribution of silicon-oxygen bonds in the silicone adhesive, thereby affecting the weather resistance and moisture resistance of the silicone adhesive. Summary of the invention

[0008] In view of the shortcomings of the prior art, the present invention provides a high-performance anti-mildew and antibacterial matte beauty edge finishing glue and a preparation method thereof. The prepared matte beauty edge finishing glue has low gloss, excellent anti-mildew and antibacterial properties, extrudability, storage resistance, heat resistance, as well as excellent adhesion, tear strength, tensile strength, elongation, weather resistance, and moisture resistance.

[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing a high-performance mildew-proof and antibacterial matte beauty edge adhesive, comprising the following steps: preparing a matte agent, preparing a mildew-proof and antibacterial agent, and mixing;

[0011] The preparation of the matte agent comprises the following steps: preparing hollow silica, amination, carboxylation, and esterification;

[0012] The method for preparing hollow silica comprises the following steps: adding nano calcium carbonate, hexadecyl trimethyl ammonium bromide and anhydrous ethanol into a reaction kettle, adjusting the stirring speed to 300-500 rpm, stirring at room temperature for 1-1.5 hours, adding ammonia water, stirring for 20-30 minutes, adjusting the temperature of the reaction kettle to 50-55° C., adding tetraethyl orthosilicate, stirring for 75-80 hours, transferring the reaction kettle into a centrifuge, adjusting the centrifugal speed of the centrifuge to 9000-10000 rpm, and centrifuging for 10-12 minutes. , take the precipitate, add the precipitate and the hydrochloric acid aqueous solution into the reactor, adjust the stirring speed of the reactor to 300-500 rpm, stir at room temperature for 20-30 minutes, transfer to a centrifuge, adjust the centrifugal speed of the centrifuge to 11000-12000 rpm, centrifuge for 10-12 minutes, take the precipitate, wash the precipitate with deionized water for 3-4 times, transfer to an oven, adjust the drying temperature of the oven to 120-130°C, dry for 8-10 hours, and obtain hollow silica;

[0013] In the preparation of hollow silica, the mass volume ratio of nano calcium carbonate, hexadecyltrimethylammonium bromide, anhydrous ethanol, ammonia water, ethyl orthosilicate, and hydrochloric acid aqueous solution is 9-10g:4-4.5g:550-600mL:55-60mL:23-25mL:300-320mL;

[0014] The concentration of the ammonia water is 25wt%;

[0015] The concentration of the hydrochloric acid aqueous solution is 5wt%;

[0016] The amination method comprises the following steps: adding hollow silica, anhydrous ethanol and deionized water into a reaction kettle, adjusting the temperature of the reaction kettle to 40-45° C., adjusting the stirring speed to 200-400 rpm, stirring for 10-20 min, adding 3-aminopropyltriethoxysilane, continuing stirring for 4-4.5 h, transferring to a centrifuge, adjusting the centrifugal speed of the centrifuge to 11000-12000 rpm, centrifuging for 10-12 min, taking a precipitate, washing the precipitate with deionized water for 3-4 times, transferring to an oven, adjusting the drying temperature of the oven to 70-80° C., and drying for 12-14 h to obtain the amination hollow silica;

[0017] In the amination, the mass volume ratio of hollow silica, anhydrous ethanol, deionized water, and 3-aminopropyltriethoxysilane is 25-26 g: 400-450 mL: 40-60 mL: 30-35 mL;

[0018] The carboxylation method comprises the following steps: adding aminated hollow silica, N,N-dimethylformamide and succinic anhydride into a reaction kettle, adjusting the temperature of the reaction kettle to 40-45° C., adjusting the stirring speed to 200-400 rpm, stirring for 16-18 hours, transferring the reaction kettle into a centrifuge, adjusting the centrifugal speed of the centrifuge to 11000-12000 rpm, centrifuging for 10-12 minutes, taking a precipitate, washing the precipitate with deionized water for 3-4 times, transferring the reaction kettle into an oven, adjusting the drying temperature of the oven to 70-80° C., drying for 12-14 hours, and obtaining carboxylated hollow silica;

[0019] In the carboxylation, the mass volume ratio of the aminated hollow silica, N,N-dimethylformamide, and succinic anhydride is 25-26 g:700-800 mL:20-23 g;

[0020] The esterification method comprises the following steps: adding carboxylated hollow silica, terminal hydroxyl silicone oil and xylene into a reaction kettle, adjusting the temperature of the reaction kettle to 65-80° C., adjusting the stirring speed to 300-400 rpm, stirring for 5-6 hours, transferring the reaction kettle into a centrifuge, adjusting the centrifugal speed of the centrifuge to 12000-13000 rpm, centrifuging for 15-18 minutes, taking a precipitate, washing the precipitate with xylene for 3-4 times, transferring the reaction kettle into an oven, adjusting the drying temperature of the oven to 70-80° C., drying for 20-24 hours, and obtaining a matte agent;

[0021] In the esterification, the mass volume ratio of carboxylated hollow silica, terminal hydroxyl silicone oil and xylene is 28-30 g:130-150 mL:300-400 mL;

[0022] The viscosity of the hydroxy-terminated silicone oil at 25° C. is 60 mpa·s;

[0023] The method for preparing the mildew and antibacterial agent comprises the following steps: silanization, chelation, and coating;

[0024] The silanization method comprises the following steps: adding nano titanium dioxide, anhydrous ethanol and deionized water into a reaction kettle, adjusting the temperature of the reaction kettle to 40-45° C., adjusting the stirring speed to 200-400 rpm, stirring for 10-20 min, adding 3-aminopropyltriethoxysilane, continuing stirring for 3-3.5 h, transferring to a centrifuge, adjusting the centrifugal speed of the centrifuge to 8000-9000 rpm, centrifuging for 10-12 min, taking a precipitate, washing the precipitate with deionized water for 3-4 times, transferring to an oven, adjusting the drying temperature of the oven to 70-80° C., drying for 9-10 h, and obtaining silanized titanium dioxide;

[0025] In the silanization, the mass volume ratio of nano titanium dioxide, anhydrous ethanol, deionized water, and 3-aminopropyltriethoxysilane is 50-55g:700-750mL:70-90mL:25-35mL;

[0026] The particle size of the nano titanium dioxide is 50 nm;

[0027] The chelation method comprises the following steps: adding silanized titanium dioxide, silver nitrate, polyvinyl pyrrolidone and deionized water into a reaction kettle, adjusting the stirring speed of the reaction kettle to 100-200 rpm, stirring at room temperature for 40-60 minutes, transferring the reaction kettle into a centrifuge, adjusting the centrifugal speed of the centrifuge to 8000-9000 rpm, centrifuging for 10-12 minutes, taking a precipitate, washing the precipitate with deionized water for 3-4 times, transferring the reaction kettle into an oven, adjusting the drying temperature of the oven to 70-80° C., and drying for 10-12 hours to obtain chelated silver titanium dioxide;

[0028] In the chelation, the mass volume ratio of silanized titanium dioxide, silver nitrate, polyvinyl pyrrolidone and deionized water is 50-55g:20-21g:30-35g:3500-4000mL;

[0029] The coating method comprises the following steps: adding chelated silver titanium dioxide and anhydrous ethanol to a reaction kettle, adjusting the stirring speed of the reaction kettle to 200-400 rpm, stirring at room temperature for 40-60 minutes, dripping an ethanol solution of tannic acid, continuing to stir for 5-6 hours after the dripping is completed, transferring the mixture into a centrifuge, adjusting the centrifugal speed of the centrifuge to 8000-9000 rpm, centrifuging for 10-12 minutes, taking a precipitate, washing the precipitate with deionized water for 3-4 times, transferring the mixture into an oven, adjusting the drying temperature of the oven to 60-70° C., and drying for 5-6 hours to obtain an antifungal and antibacterial agent;

[0030] In the coating, the mass volume ratio of the chelated silver titanium dioxide, anhydrous ethanol, and tannic acid ethanol solution is 55-58g:550-600mL:400-450mL;

[0031] The concentration of the tannic acid ethanol solution is 1wt%;

[0032] The dropping speed of the ethanol solution of tannic acid is 5-6 mL / min;

[0033] The mixing method comprises the following steps: adding α,ω-dihydroxy polydimethylsiloxane and a matte agent into a kneader, adjusting the dehydration temperature of the kneader to 120-125° C., dehydrating for 170-190 min, and then cooling to room temperature to obtain a base material; adding the base material, dimethyl silicone oil, an anti-mildew and antibacterial agent, methyl tributylidene oxime silane, phenyl tributylidene oxime silane, 3-aminopropyl triethoxysilane, and dibutyltin dilaurate into a high-speed stirrer, adjusting the vacuum degree of the high-speed stirrer to 0.08-0.085 MPa, adjusting the high-speed stirring speed to 350-450 rpm, and stirring at high speed for 100-120 min to obtain a high-performance anti-mildew and antibacterial matte beauty edge adhesive;

[0034] In the mixture, the mass ratio of α,ω-dihydroxy polydimethylsiloxane, matting agent, dimethyl silicone oil, mildew and antibacterial agent, methyl tributylidene oxime silane, phenyl tributylidene oxime silane, 3-aminopropyl triethoxysilane and dibutyltin dilaurate is 500-520:70-100:45-50:17-20:20-22:26-30:7-10:1-1.1;

[0035] The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 35000 mPa·s;

[0036] The viscosity of the dimethyl silicone oil at 25° C. is 350 mPa·s.

[0037] A high-performance mildew-proof and antibacterial matte beauty edge finishing adhesive obtained by the above-mentioned preparation method.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) The preparation method of the high-performance mildew-proof and antibacterial matte beauty edge glue of the present invention comprises adding a matte agent and a mildew-proof and antibacterial agent into the mixed material; when preparing the matte agent, hollow silica is first prepared, and then the hollow silica is aminated with 3-aminopropyltriethoxysilane to introduce amino groups on the surface of the hollow silica, and then carboxylation is performed, and carboxyl groups are introduced by reacting succinic anhydride with the amino groups on the surface of the hollow silica, and finally esterification is performed, and terminal hydroxyl silicone oil is reacted with the carboxyl groups on the surface of the hollow silica to graft terminal hydroxyl silicone oil on the surface of the hollow silica, and the hollow silica is Silicon oxide can reduce the glossiness of the beauty edge glue while reducing the weight of the matte agent, avoiding the precipitation of hollow silica during long-term storage. The terminal hydroxy silicone oil can promote the dispersion of hollow silica in the beauty edge glue, thereby improving the extrusion of the beauty edge glue; it can also improve the bonding force between hollow silica and the beauty edge glue, and the cross-linking density of the beauty edge glue after curing, thereby improving the 100% fixed elongation adhesion, cold drawing and hot pressing ±50% adhesion, tear strength, tensile strength, elongation at break, storage resistance, weather resistance, Moisture resistance: When preparing the mildew and antibacterial agent, firstly, 3-aminopropyltriethoxysilane is used to silanize the nano titanium dioxide, and amino groups are introduced on the surface of the nano titanium dioxide. Then, silver nitrate and polyvinyl pyrrolidone are added. The silver ions in the silver nitrate can be chelated with the amino groups, and polyvinyl pyrrolidone can promote dispersion, thereby chelating a layer of silver ions on the surface of the nano titanium dioxide. Finally, tannic acid is added. Tannic acid is adsorbed on the outer surface of the nano titanium dioxide through intermolecular forces, and can also play a role in further chelating and fixing the silver ions, thereby avoiding the silver ions. The presence of tannic acid, on the one hand, can improve the mildew and antibacterial properties of the beauty edge glue; on the other hand, it can promote the rapid dispersion of nano titanium dioxide, avoiding the influence of agglomeration and precipitation on the 100% fixed elongation adhesion, cold drawing and hot pressing ±50% adhesion, tear strength, tensile strength, elongation at break, and storage resistance of the beauty edge glue; on the third hand, after tannic acid chelates silver ions and bonds with the amino groups on the surface of titanium dioxide through intermolecular forces, the heat resistance, weather resistance, and moisture resistance are increased, thereby improving the heat resistance, weather resistance, and moisture resistance of the beauty edge glue;

[0040] (2) The high-performance anti-mildew and antibacterial matte beauty edge glue of the present invention has a low glossiness, and the glossiness at 60° is 5.7-6.3 GU;

[0041] (3) The high-performance anti-mildew and anti-bacterial matte beauty edge adhesive of the present invention has excellent anti-mildew and anti-bacterial properties, and the anti-mildew grade is 0;

[0042] (4) The high-performance mildew-proof and antibacterial matte beauty edge adhesive of the present invention has excellent extrusion properties, and the extrusion properties are 250-280 mL / min;

[0043] (5) The high-performance mildew-proof and antibacterial matte beauty edge adhesive of the present invention has excellent bonding strength, with 100% fixed elongation bonding without damage, and cold drawing and hot pressing ±50% bonding without damage;

[0044] (6) The high-performance mildew-proof and antibacterial matte beauty edge adhesive of the present invention has excellent tear strength, tensile strength and elongation. The tear strength is 18.1-19.5N / mm, the tensile strength is 4.1-4.7MPa, and the elongation at break is 615-624%;

[0045] (7) The high-performance mildew-proof and antibacterial matte beauty edge adhesive of the present invention has excellent storage resistance. After being sealed and stored at room temperature for 90 days, there is no precipitation at the bottom;

[0046] (8) The high-performance anti-mildew and antibacterial matte beauty edge adhesive of the present invention has excellent heat resistance. After being placed in an environment of 80°C for 30 days and then restored to room temperature, the anti-mildew grade is 0;

[0047] (9) The high-performance mildew-proof and antibacterial matte beauty edge adhesive of the present invention has excellent weather resistance. After continuous irradiation in a xenon lamp aging box, the power of the xenon lamp in the xenon lamp aging box is 1800W, and the distance between the sample holder and the xenon lamp is 250mm, after continuous irradiation for 30 days, the tear strength is 17.0-18.1N / mm, the tensile strength is 3.7-4.4MPa, and the elongation at break is 575-587%;

[0048] (10) The high-performance mildew-proof and antibacterial matte beauty edge adhesive of the present invention has excellent moisture resistance, and the water vapor permeability is 7.0-8.1g / (m 2 ·24h). DETAILED DESCRIPTION

[0049] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0050] Example 1

[0051] A method for preparing a high-performance mildew-proof and antibacterial matte beauty edge adhesive, specifically comprising:

[0052] 1. Prepare matte agent:

[0053] (1) Preparation of hollow silica: 9 g of nano calcium carbonate, 4 g of hexadecyltrimethylammonium bromide, and 550 mL of anhydrous ethanol were added to a reactor, the stirring speed was adjusted to 300 rpm, and the mixture was stirred at room temperature for 1 h. 55 mL of 25 wt% ammonia water was added and stirred for 20 min. The temperature of the reactor was adjusted to 50°C, 23 mL of ethyl orthosilicate was added and stirred for 75 h. The mixture was transferred to a centrifuge and the centrifugal speed of the centrifuge was adjusted to 9000 rpm. The mixture was centrifuged for 10 min. The precipitate was taken. The precipitate and 300 mL of 5 wt% aqueous hydrochloric acid solution were added to the reactor, the stirring speed of the reactor was adjusted to 300 rpm, and the mixture was stirred at room temperature for 20 min. The mixture was transferred to a centrifuge and the centrifugal speed of the centrifuge was adjusted to 11000 rpm. The mixture was centrifuged for 10 min. The precipitate was taken and washed with deionized water for 3 times. The mixture was transferred to an oven and the drying temperature of the oven was adjusted to 120°C. The mixture was dried for 8 h to obtain hollow silica.

[0054] (2) Amination: 25 g of hollow silica, 400 mL of anhydrous ethanol and 40 mL of deionized water were added to a reactor, the temperature of the reactor was adjusted to 40°C, the stirring speed was adjusted to 200 rpm, and the stirring was continued for 10 min. 30 mL of 3-aminopropyltriethoxysilane was added, and the stirring was continued for 4 h. The mixture was transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 11000 rpm. The mixture was centrifuged for 10 min. The precipitate was taken and washed with deionized water for 3 times. The mixture was transferred to an oven, and the drying temperature of the oven was adjusted to 70°C. The mixture was dried for 12 h to obtain aminated hollow silica.

[0055] (3) Carboxylation: 25 g of amino hollow silica, 700 mL of N,N-dimethylformamide, and 20 g of succinic anhydride were added to a reactor, the temperature of the reactor was adjusted to 40°C, the stirring speed was adjusted to 200 rpm, and the stirring was performed for 16 h. The reactor was transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 11000 rpm, and the centrifugation was performed for 10 min. The precipitate was taken and washed with deionized water for 3 times. The precipitate was transferred to an oven, the drying temperature of the oven was adjusted to 70°C, and the mixture was dried for 12 h to obtain carboxylated hollow silica.

[0056] (4) Esterification: 28 g of carboxylated hollow silica, 130 mL of terminal hydroxyl silicone oil, and 300 mL of xylene were added to a reactor, the temperature of the reactor was adjusted to 65°C, the stirring speed was adjusted to 300 rpm, stirring was performed for 5 h, the reactor was transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 12000 rpm, centrifuged for 15 min, the precipitate was taken, the precipitate was washed 3 times with xylene, the reactor was transferred to an oven, the drying temperature of the oven was adjusted to 70°C, and the reactor was dried for 20 h to obtain a matte agent;

[0057] The viscosity of the hydroxy-terminated silicone oil at 25° C. is 60 mpa·s;

[0058] 2. Preparation of mildew and antibacterial agent:

[0059] (1) Silanization: Add 50 g of nano titanium dioxide, 700 mL of anhydrous ethanol, and 70 mL of deionized water into a reactor, adjust the temperature of the reactor to 40°C, adjust the stirring speed to 200 rpm, stir for 10 min, add 25 mL of 3-aminopropyltriethoxysilane, continue stirring for 3 h, transfer to a centrifuge, adjust the centrifugal speed of the centrifuge to 8000 rpm, centrifuge for 10 min, take the precipitate, wash the precipitate with deionized water 3 times, transfer to an oven, adjust the drying temperature of the oven to 70°C, and dry for 9 h to obtain silanized titanium dioxide;

[0060] The particle size of the nano titanium dioxide is 50 nm;

[0061] (2) Chelation: 50 g of silanized titanium dioxide, 20 g of silver nitrate, 30 g of polyvinyl pyrrolidone, and 3500 mL of deionized water were added to a reactor, the stirring speed of the reactor was adjusted to 100 rpm, and the mixture was stirred at room temperature for 40 min. The mixture was transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 8000 rpm. The mixture was centrifuged for 10 min. The precipitate was taken and washed with deionized water for 3 times. The precipitate was transferred to an oven, and the drying temperature of the oven was adjusted to 70°C. The mixture was dried for 10 h to obtain chelated silver titanium dioxide.

[0062] (3) Coating: Add 55g of chelated silver titanium dioxide and 550mL of anhydrous ethanol into a reactor, adjust the stirring speed of the reactor to 200rpm, stir at room temperature for 40min, dropwise add 400mL of 1wt% tannic acid ethanol solution, control the dropping speed to 5mL / min, continue stirring for 5h after the dropping is completed, transfer to a centrifuge, adjust the centrifugal speed of the centrifuge to 8000rpm, centrifuge for 10min, take the precipitate, wash the precipitate with deionized water for 3 times, transfer to an oven, adjust the drying temperature of the oven to 60°C, dry for 5h, and obtain an antifungal and antibacterial agent;

[0063] 3. Mixing: Add 500g α,ω-dihydroxypolydimethylsiloxane and 70g matting agent into a kneader, adjust the dehydration temperature of the kneader to 120°C, dehydrate for 170min, and then cool to room temperature to obtain a base material; add the base material, 45g dimethyl silicone oil, 17g mildew and antibacterial agent, 20g methyl tributylidene oxime silane, 26g phenyl tributylidene oxime silane, 7g 3-aminopropyl triethoxysilane, and 1g dibutyltin dilaurate into a high-speed stirrer, adjust the vacuum degree of the high-speed stirrer to 0.08MPa, adjust the high-speed stirring speed to 350rpm, and stir at high speed for 100min to obtain a high-performance mildew and antibacterial matte beauty edge glue;

[0064] The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 35000 mPa·s;

[0065] The viscosity of the dimethyl silicone oil at 25° C. is 350 mPa·s.

[0066] This embodiment also provides a high-performance mildew-proof and antibacterial matte beauty edge finishing adhesive obtained by the aforementioned preparation method.

[0067] Example 2

[0068] A method for preparing a high-performance mildew-proof and antibacterial matte beauty edge adhesive, specifically comprising:

[0069] 1. Prepare matte agent:

[0070] (1) Preparation of hollow silica: 9.5 g of nano calcium carbonate, 4.2 g of hexadecyltrimethylammonium bromide, and 580 mL of anhydrous ethanol were added to a reactor, the stirring speed was adjusted to 400 rpm, and the mixture was stirred at room temperature for 1 h. 58 mL of 25 wt% ammonia water was added and stirred for 25 min. The temperature of the reactor was adjusted to 52 °C, 24 mL of tetraethyl orthosilicate was added and stirred for 78 h. The mixture was transferred to a centrifuge and the centrifugal speed of the centrifuge was adjusted to 9500 rpm. The mixture was centrifuged for 11 min. The precipitate was taken. The precipitate and 310 mL of 5 wt% aqueous hydrochloric acid solution were added to the reactor, the stirring speed of the reactor was adjusted to 400 rpm, and the mixture was stirred at room temperature for 25 min. The mixture was transferred to a centrifuge and the centrifugal speed of the centrifuge was adjusted to 11000 rpm. The mixture was centrifuged for 11 min. The precipitate was taken and washed with deionized water for 3 times. The mixture was transferred to an oven and the drying temperature of the oven was adjusted to 125 °C. The mixture was dried for 9 h to obtain hollow silica.

[0071] (2) Amination: 25.5 g of hollow silica, 420 mL of anhydrous ethanol and 50 mL of deionized water were added to a reactor, the temperature of the reactor was adjusted to 42 ° C, the stirring speed was adjusted to 300 rpm, and the stirring was continued for 15 min. 32 mL of 3-aminopropyltriethoxysilane was added, and the stirring was continued for 4 h. The mixture was transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 11000 rpm. The mixture was centrifuged for 11 min. The precipitate was taken and washed with deionized water for 3 times. The precipitate was transferred to an oven, and the drying temperature of the oven was adjusted to 75 ° C. The mixture was dried for 13 h to obtain aminated hollow silica.

[0072] (3) Carboxylation: 25.5 g of amino hollow silica, 750 mL of N,N-dimethylformamide, and 22 g of succinic anhydride were added to a reactor, the temperature of the reactor was adjusted to 42 ° C, the stirring speed was adjusted to 300 rpm, and the stirring was performed for 17 h. The reactor was transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 11000 rpm, and the centrifugation was performed for 11 min. The precipitate was taken and washed with deionized water for 3 times. The precipitate was transferred to an oven, the drying temperature of the oven was adjusted to 75 ° C, and the mixture was dried for 13 h to obtain carboxylated hollow silica.

[0073] (4) Esterification: 29 g of carboxylated hollow silica, 140 mL of terminal hydroxyl silicone oil, and 350 mL of xylene were added to a reactor, the temperature of the reactor was adjusted to 70°C, the stirring speed was adjusted to 350 rpm, stirring was performed for 5.5 h, the reactor was transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 12000 rpm, centrifuged for 16 min, the precipitate was taken, the precipitate was washed 3 times with xylene, the reactor was transferred to an oven, the drying temperature of the oven was adjusted to 75°C, and the reactor was dried for 22 h to obtain a matte agent;

[0074] The viscosity of the hydroxy-terminated silicone oil at 25° C. is 60 mpa·s;

[0075] 2. Preparation of mildew and antibacterial agent:

[0076] (1) Silanization: Add 52 g of nano titanium dioxide, 720 mL of anhydrous ethanol, and 80 mL of deionized water into a reactor, adjust the temperature of the reactor to 42 ° C, adjust the stirring speed to 300 rpm, stir for 15 min, add 30 mL of 3-aminopropyltriethoxysilane, continue stirring for 3 h, transfer to a centrifuge, adjust the centrifugal speed of the centrifuge to 8500 rpm, centrifuge for 11 min, take the precipitate, wash the precipitate with deionized water 3 times, transfer to an oven, adjust the drying temperature of the oven to 75 ° C, and dry for 9.5 h to obtain silanized titanium dioxide;

[0077] The particle size of the nano titanium dioxide is 50 nm;

[0078] (2) Chelation: 52 g of silanized titanium dioxide, 20.5 g of silver nitrate, 32 g of polyvinyl pyrrolidone, and 3800 mL of deionized water were added to a reactor, the stirring speed of the reactor was adjusted to 150 rpm, stirred at room temperature for 50 min, transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 8500 rpm, centrifuged for 11 min, the precipitate was taken, the precipitate was washed 3 times with deionized water, transferred to an oven, the drying temperature of the oven was adjusted to 75°C, and dried for 11 h to obtain chelated silver titanium dioxide;

[0079] (3) Coating: 56 g of chelated silver titanium dioxide and 580 mL of anhydrous ethanol were added to a reactor, the stirring speed of the reactor was adjusted to 300 rpm, and the mixture was stirred at room temperature for 50 min. 420 mL of an ethanol solution of tannic acid with a concentration of 1 wt% was added dropwise, and the dropping speed was controlled to 5 mL / min. After the addition was completed, the mixture was stirred for 5.5 h, and the mixture was transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 8500 rpm. The mixture was centrifuged for 11 min, and the precipitate was taken. The precipitate was washed three times with deionized water, and the mixture was transferred to an oven. The drying temperature of the oven was adjusted to 65°C, and the mixture was dried for 5.5 h to obtain an antifungal and antibacterial agent.

[0080] 3. Mixing: Add 510g α,ω-dihydroxypolydimethylsiloxane and 80g matting agent into a kneader, adjust the dehydration temperature of the kneader to 120°C, dehydrate for 180min, and then cool to room temperature to obtain a base material; add the base material, 48g dimethyl silicone oil, 18g mildew and antibacterial agent, 21g methyl tributylidene oxime silane, 28g phenyl tributylidene oxime silane, 9g 3-aminopropyl triethoxysilane, and 1g dibutyltin dilaurate into a high-speed stirrer, adjust the vacuum degree of the high-speed stirrer to 0.08MPa, adjust the high-speed stirring speed to 400rpm, and stir at high speed for 110min to obtain a high-performance mildew and antibacterial matte beauty edge glue;

[0081] The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 35000 mPa·s;

[0082] The viscosity of the dimethyl silicone oil at 25° C. is 350 mPa·s.

[0083] This embodiment also provides a high-performance mildew-proof and antibacterial matte beauty edge finishing adhesive obtained by the aforementioned preparation method.

[0084] Example 3

[0085] A method for preparing a high-performance mildew-proof and antibacterial matte beauty edge adhesive, specifically comprising:

[0086] 1. Prepare matte agent:

[0087] (1) Preparation of hollow silica: 10 g of nano calcium carbonate, 4.5 g of hexadecyltrimethylammonium bromide, and 600 mL of anhydrous ethanol were added to a reactor, the stirring speed was adjusted to 500 rpm, and the mixture was stirred at room temperature for 1.5 h. 60 mL of 25 wt% ammonia water was added and stirred for 30 min. The temperature of the reactor was adjusted to 55 ° C. 25 mL of tetraethyl orthosilicate was added and stirred for 80 h. The mixture was transferred to a centrifuge and the centrifugal speed of the centrifuge was adjusted to 10,000 rpm. The mixture was centrifuged for 12 min. The precipitate was taken. The precipitate and 320 mL of 5 wt% hydrochloric acid aqueous solution were added to the reactor, the stirring speed of the reactor was adjusted to 500 rpm, and the mixture was stirred at room temperature for 30 min. The mixture was transferred to a centrifuge and the centrifugal speed of the centrifuge was adjusted to 12,000 rpm. The mixture was centrifuged for 12 min. The precipitate was taken and washed with deionized water for 4 times. The mixture was transferred to an oven and the drying temperature of the oven was adjusted to 130 ° C. The mixture was dried for 10 h to obtain hollow silica.

[0088] (2) Amination: 26 g of hollow silica, 450 mL of anhydrous ethanol and 60 mL of deionized water were added to a reactor, the temperature of the reactor was adjusted to 45 ° C, the stirring speed was adjusted to 400 rpm, and the stirring was continued for 20 min. 35 mL of 3-aminopropyltriethoxysilane was added, and the stirring was continued for 4.5 h. The mixture was transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 12000 rpm. The mixture was centrifuged for 12 min. The precipitate was taken and washed with deionized water for 4 times. The precipitate was transferred to an oven, and the drying temperature of the oven was adjusted to 80 ° C. The mixture was dried for 14 h to obtain aminated hollow silica.

[0089] (3) Carboxylation: 26 g of amino hollow silica, 800 mL of N,N-dimethylformamide, and 23 g of succinic anhydride were added to a reactor, the temperature of the reactor was adjusted to 45°C, the stirring speed was adjusted to 400 rpm, and the stirring was performed for 18 h. The reactor was transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 12000 rpm, and the centrifugation was performed for 12 min. The precipitate was taken and washed with deionized water for 4 times. The precipitate was transferred to an oven, the drying temperature of the oven was adjusted to 80°C, and the mixture was dried for 14 h to obtain carboxylated hollow silica.

[0090] (4) Esterification: 30 g of carboxylated hollow silica, 150 mL of terminal hydroxyl silicone oil, and 400 mL of xylene were added to a reactor, the temperature of the reactor was adjusted to 80°C, the stirring speed was adjusted to 400 rpm, stirring was performed for 6 hours, the reactor was transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 13000 rpm, centrifuged for 18 minutes, the precipitate was taken, the precipitate was washed 4 times with xylene, the reactor was transferred to an oven, the drying temperature of the oven was adjusted to 80°C, and the reactor was dried for 24 hours to obtain a matte agent;

[0091] The viscosity of the hydroxy-terminated silicone oil at 25° C. is 60 mpa·s;

[0092] 2. Preparation of mildew and antibacterial agent:

[0093] (1) Silanization: Add 55 g of nano titanium dioxide, 750 mL of anhydrous ethanol, and 90 mL of deionized water into a reactor, adjust the temperature of the reactor to 45 ° C, adjust the stirring speed to 400 rpm, stir for 20 min, add 35 mL of 3-aminopropyltriethoxysilane, continue stirring for 3.5 h, transfer to a centrifuge, adjust the centrifugal speed of the centrifuge to 9000 rpm, centrifuge for 12 min, take the precipitate, wash the precipitate with deionized water 4 times, transfer to an oven, adjust the drying temperature of the oven to 80 ° C, and dry for 10 h to obtain silanized titanium dioxide;

[0094] The particle size of the nano titanium dioxide is 50 nm;

[0095] (2) Chelation: 55 g of silanized titanium dioxide, 21 g of silver nitrate, 35 g of polyvinyl pyrrolidone, and 4000 mL of deionized water were added to a reactor, the stirring speed of the reactor was adjusted to 200 rpm, and the mixture was stirred at room temperature for 60 min. The mixture was transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 9000 rpm. The mixture was centrifuged for 12 min. The precipitate was taken and washed with deionized water for 4 times. The precipitate was transferred to an oven, and the drying temperature of the oven was adjusted to 80° C. The mixture was dried for 12 h to obtain chelated silver titanium dioxide.

[0096] (3) Coating: 58 g of chelated silver titanium dioxide and 600 mL of anhydrous ethanol were added to a reactor, the stirring speed of the reactor was adjusted to 400 rpm, and the mixture was stirred at room temperature for 60 min. 450 mL of an ethanol solution of tannic acid with a concentration of 1 wt% was added dropwise, and the dropping speed was controlled to 6 mL / min. After the addition was completed, the mixture was stirred for 6 h, and the mixture was transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 9000 rpm. The mixture was centrifuged for 12 min, and the precipitate was taken. The precipitate was washed 4 times with deionized water, and the mixture was transferred to an oven. The drying temperature of the oven was adjusted to 70°C, and the mixture was dried for 6 h to obtain an antifungal and antibacterial agent.

[0097] 3. Mixing: Add 520g α,ω-dihydroxypolydimethylsiloxane and 100g matting agent into a kneader, adjust the dehydration temperature of the kneader to 125°C, dehydrate for 190min, and then cool to room temperature to obtain a base material; add the base material, 50g dimethyl silicone oil, 20g mildew and antibacterial agent, 22g methyl tributylidene oxime silane, 30g phenyl tributylidene oxime silane, 10g 3-aminopropyl triethoxysilane, and 1.1g dibutyltin dilaurate into a high-speed stirrer, adjust the vacuum degree of the high-speed stirrer to 0.085MPa, adjust the high-speed stirring speed to 450rpm, and stir at high speed for 120min to obtain a high-performance mildew and antibacterial matte beauty edge glue;

[0098] The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 35000 mPa·s;

[0099] The viscosity of the dimethyl silicone oil at 25° C. is 350 mPa·s.

[0100] This embodiment also provides a high-performance mildew-proof and antibacterial matte beauty edge finishing adhesive obtained by the aforementioned preparation method.

[0101] Comparative Example 1

[0102] This comparative example is based on the preparation method of Example 2, omitting the first step of preparing the matting agent, and using an equal amount of silicon dioxide with a particle size of 2 μm to replace the matting agent in the mixing step;

[0103] The remaining operations are the same as those in Example 2.

[0104] This comparative example also provides a high-performance mildew-proof and antibacterial matte beauty edge adhesive prepared by the aforementioned preparation method.

[0105] Comparative Example 2

[0106] This comparative example is based on the preparation method of Example 2, omitting the second step of preparing the mildew and antibacterial agent, and using 8.6g of nano titanium dioxide with a particle size of 50nm, 3.4g of silver nitrate, 5.2g of polyvinyl pyrrolidone, and 0.8g of tannic acid instead of adding the mildew and antibacterial agent in the mixing step;

[0107] The remaining operations are the same as those in Example 2.

[0108] This comparative example also provides a high-performance mildew-proof and antibacterial matte beauty edge adhesive prepared by the aforementioned preparation method.

[0109] Test Example 1

[0110] The glossiness, mildew resistance, extrusion, 100% fixed stretch adhesion, cold drawing and hot pressing ±50% adhesion, tear strength, tensile strength, and elongation at break of the beauty edge adhesives of Examples 1-3 and Comparative Examples 1-2 were tested, and the test results are as follows:

[0111]

[0112] Test Example 2

[0113] The beauty edge trimming adhesives of Examples 1-3 and Comparative Examples 1-2 were sealed and stored at room temperature for 90 days, and then the bottom was observed to see if there was precipitation. The observation results were as follows:

[0114]

[0115] Test Example 3

[0116] After the beauty edge glues of Examples 1-3 and Comparative Examples 1-2 were made into test samples, the test samples were placed in an environment of 80° C. for 30 days, and then returned to room temperature, and the mildew resistance level was tested. The test results are as follows:

[0117]

[0118] Test Example 4

[0119] After the beauty edge glues of Examples 1-3 and Comparative Examples 1-2 were made into test samples, the test samples were continuously irradiated in a xenon lamp aging box. The power of the xenon lamp in the xenon lamp aging box was 1800W, and the distance between the sample holder and the xenon lamp was 250mm. After continuous irradiation for 30 days, the tear strength, tensile strength and elongation at break of the test samples were tested. The test results are as follows:

[0120]

[0121] Test Example 5

[0122] After the beauty edge trimming adhesives of Examples 1-3 and Comparative Examples 1-2 were made into test samples, the water vapor transmission rates of the test samples were tested, and the test results were as follows:

[0123]

[0124] It can be seen from the test results of Test Examples 1-5 that by adding a matte agent to the beauty edge glue, the glossiness of the beauty edge glue can be reduced, and the extrusion property, 100% fixed stretch adhesion, cold drawing and hot pressing ±50% adhesion, tear strength, tensile strength, elongation at break, storage resistance, weather resistance, and moisture resistance of the beauty edge glue can be improved;

[0125] By adding anti-mildew and antibacterial agents to the beauty edge glue, the 100% fixed elongation adhesion, cold drawing and hot pressing ±50% adhesion, tear strength, tensile strength, elongation at break, storage resistance, heat resistance, weather resistance and moisture resistance of the beauty edge glue can be improved.

[0126] Unless otherwise specified, all percentages used in the present invention are by mass.

[0127] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-performance mildew-proof and antibacterial matte beauty edge adhesive, characterized in that: The method comprises the following steps: preparing a matting agent, preparing an antifungal and antibacterial agent, and mixing materials; The preparation of the matte agent comprises the following steps: preparing hollow silica, amination, carboxylation, and esterification; The method for preparing hollow silica comprises: mixing nano calcium carbonate, hexadecyltrimethylammonium bromide and anhydrous ethanol, stirring at room temperature, adding ammonia water, stirring, adding tetraethyl orthosilicate at 50-55° C., stirring, centrifuging, taking a precipitate, mixing the precipitate with a hydrochloric acid aqueous solution, stirring at room temperature, centrifuging, taking a precipitate, washing and drying the precipitate to obtain hollow silica; The amination method comprises mixing hollow silica, anhydrous ethanol and deionized water, stirring at 40-45° C., adding 3-aminopropyltriethoxysilane, continuing stirring, centrifuging, taking a precipitate, washing and drying the precipitate to obtain the amination hollow silica; The carboxylation method comprises mixing aminated hollow silica, N,N-dimethylformamide and succinic anhydride, stirring at 40-45° C., centrifuging, taking a precipitate, washing and drying the precipitate to obtain carboxylated hollow silica; The esterification method comprises mixing carboxylated hollow silica, terminal hydroxyl silicone oil and xylene, stirring at 65-80° C., centrifuging, taking a precipitate, washing and drying the precipitate to obtain a matte agent; The method for preparing the mildew and antibacterial agent comprises the following steps: silanization, chelation, and coating; The silanization method comprises mixing nano titanium dioxide, anhydrous ethanol and deionized water, stirring at 40-45° C., adding 3-aminopropyltriethoxysilane, continuing stirring, centrifuging, taking a precipitate, washing and drying the precipitate to obtain silanized titanium dioxide; The chelation method comprises mixing silanized titanium dioxide, silver nitrate, polyvinyl pyrrolidone and deionized water, stirring at room temperature for 40-60 minutes, centrifuging, taking a precipitate, washing and drying the precipitate to obtain chelated silver titanium dioxide; The coating method comprises mixing chelated silver titanium dioxide and anhydrous ethanol, stirring at room temperature, dropping tannic acid ethanol solution, continuing stirring after the dropping, centrifuging, taking precipitates, washing and drying the precipitates, and obtaining the mildew and antibacterial agent; The mixing method comprises the following steps: adding α,ω-dihydroxy polydimethylsiloxane and a matte agent into a kneader for dehydration, and then cooling to room temperature to obtain a base material; adding the base material, dimethyl silicone oil, an anti-mildew and antibacterial agent, methyl tributylidene oxime silane, phenyl tributylidene oxime silane, 3-aminopropyl triethoxysilane, and dibutyltin dilaurate into a high-speed stirrer for high-speed stirring to obtain a high-performance anti-mildew and antibacterial matte beauty edge adhesive; In the mixture, the mass ratio of α,ω-dihydroxypolydimethylsiloxane, matting agent, dimethyl silicone oil, mildew and antibacterial agent, methyltributylacetonatoximosilane, phenyltributylacetonatoximosilane, 3-aminopropyltriethoxysilane and dibutyltin dilaurate is 500-520:70-100:45-50:17-20:20-22:26-30:7-10:1-1.

1.

2. The method for preparing the high-performance mildew-proof and antibacterial matte beauty edge adhesive according to claim 1, characterized in that: In the preparation of hollow silica, the mass volume ratio of nano calcium carbonate, hexadecyltrimethylammonium bromide, anhydrous ethanol, ammonia water, ethyl orthosilicate, and hydrochloric acid aqueous solution is 9-10g:4-4.5g:550-600mL:55-60mL:23-25mL:300-320mL; The concentration of the ammonia water is 25wt%; The concentration of the hydrochloric acid aqueous solution is 5wt%.

3. The method for preparing the high-performance mildew-proof and antibacterial matte beauty edge adhesive according to claim 1, characterized in that: In the amination, the mass volume ratio of hollow silica, anhydrous ethanol, deionized water and 3-aminopropyltriethoxysilane is 25-26 g: 400-450 mL: 40-60 mL: 30-35 mL.

4. The method for preparing the high-performance mildew-proof and antibacterial matte beauty edge adhesive according to claim 1, characterized in that: In the carboxylation, the mass volume ratio of the aminated hollow silica, N,N-dimethylformamide and succinic anhydride is 25-26 g:700-800 mL:20-23 g.

5. The method for preparing the high-performance mildew-proof and antibacterial matte beauty edge adhesive according to claim 1, characterized in that: In the esterification, the mass volume ratio of carboxylated hollow silica, terminal hydroxyl silicone oil and xylene is 28-30 g:130-150 mL:300-400 mL.

6. The method for preparing the high-performance mildew-proof and antibacterial matte beauty edge adhesive according to claim 1, characterized in that: In the silanization, the mass volume ratio of nano titanium dioxide, anhydrous ethanol, deionized water and 3-aminopropyltriethoxysilane is 50-55g:700-750mL:70-90mL:25-35mL.

7. The method for preparing the high-performance mildew-proof and antibacterial matte beauty edge adhesive according to claim 1, characterized in that: In the chelation, the mass volume ratio of silanized titanium dioxide, silver nitrate, polyvinyl pyrrolidone and deionized water is 50-55g:20-21g:30-35g:3500-4000mL.

8. The method for preparing the high-performance mildew-proof and antibacterial matte beauty edge adhesive according to claim 1, characterized in that: In the coating, the mass volume ratio of the chelated silver titanium dioxide, anhydrous ethanol, and tannic acid ethanol solution is 55-58g:550-600mL:400-450mL; The concentration of the tannic acid ethanol solution is 1wt%; The dropping speed of the tannic acid ethanol solution is 5-6 mL / min.

9. The method for preparing the high-performance mildew-proof and antibacterial matte beauty edge adhesive according to claim 1, characterized in that: In the mixing, the temperature of the dehydration kneader is 120-125°C, and the dehydration time is 170-190min; The vacuum degree of the high-speed stirrer in the high-speed stirring is 0.08-0.085 MPa, the high-speed stirring speed is 350-450 rpm, and the high-speed stirring time is 100-120 min.

10. A high-performance mildew-proof and antibacterial matte beauty edge adhesive obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Matt sealant as well as preparation method and application thereof

    CN115785890A

  • Preparation method of environment-friendly super-strong mildewproof matte degreasing type beautifying and edging sealant

    CN117659936A

Cited By

  • Beautifying, edge-shrinking and anti-mildew glue and preparation method thereof

    CN121108900A