A method for preparing vanadium-doped layered selenide and single crystal thereof

Through the high-temperature firing of vanadium-doped layered selenide and the dual-temperature gas phase transport and growth method, the problems of insufficient electromagnetic performance and small single crystal size of titanium-doped Cr2Se3 materials were solved, and large-size VxCr2-xSe3 single crystals were obtained, suitable for High-performance spintronic devices and microelectromechanical systems.

CN118653214BActive Publication Date: 2024-11-01JIHUA LAB
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411123865.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

In the prior art, the electromagnetic transport performance of the titanium-doped Cr2Se3 material is insufficient, and it is difficult to obtain large-sized single crystals, and there are problems such as composition uncertainty and long growth time.

Method used

The preparation method of vanadium-doped layered selenide is adopted, and the gas phase transport and growth of vanadium powder, chromium powder, selenium powder and iodine are used as raw materials to control the raw material ratio and temperature gradient to obtain the diamond formula Phase VxCr2-xSe3 (0

Benefits of technology

It has achieved the preparation of VxCr2-xSe3 single crystal with large size (up to 1 cm) and has excellent electromagnetic transport performance. It is suitable for spintronic devices and microelectromechanical systems, and has shortened growth time and low energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118653214B_ABST
    Figure CN118653214B_ABST
Patent Text Reader

Abstract

The invention discloses a vanadium-doped layered selenide and a preparation method of a single crystal thereof, and relates to the technical field of crystal material preparation. The chemical formula of the selenide is V x Cr 2‑x Se3, where 0<x≤0.25, the selenide is a rhombohedral phase ( R ‑3) Crystal structure. The electromagnetic transport properties of the material are related to the vanadium content and can be used in spin electronics, hard disk drives, micro-electromechanical systems and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of crystal material preparation, and in particular to a vanadium-doped layered selenide and a preparation method of a single crystal thereof. Background Art

[0002] There are many types of layered transition metal chalcogenides and they exhibit many novel physical properties. They have good application prospects in field effect transistors, optoelectronic devices, photodetectors, photoelectrocatalysis and batteries.

[0003] Compared with other material systems, the structure of Cr-containing chalcogenides has a "sandwich" configuration, with Cr vacancies between layers, and Cr vacancies can form different crystal structures according to a certain arrangement order, showing different physical properties. Among them, rhombohedral phase Cr2Se3 (space group: R -3) is a NiAs type lattice structure with Cr vacancies, which is a CrSe layer and a Cr-poor 1 / 3 Se layers are stacked alternately in a two-dimensional layered structure, where Cr vacancies are located in the Cr 1 / 3 The Se layer is orderly distributed. The study found that a slight change in the Cr content in the Cr2Se3 structure will cause changes in the electromagnetic properties of the material, which provides a direction for exploring the mutual coupling between magnetism and electrical transport of such materials, as well as the regulation of the physical properties of such materials by element doping, and also makes such materials have better prospects for application in the fields of spin electronics, hard disk drives, and micro-electromechanical systems.

[0004] Finding doping elements that can regulate Cr2Se3 materials in a wide synthesis range and growing large-sized, high-quality corresponding single crystals is of great significance for studying the intrinsic properties of such materials and further promoting the application of such materials in related technical fields. At present, there are few studies on doping Cr2Se3 single crystals to change their electromagnetic transport properties. Among them, the literature (ACSAppl. Mater. Interfaces 2021, 13, 49, 58949–58955.) reported that Ti:Cr2Se3 single crystals doped with 1.5% atomic content of Ti were obtained by chemical vapor transport, and their electromagnetic properties were studied. It was found that the incorporation of Ti transformed Cr2Se3 into a semiconductor and reduced its residual resistivity (ρ 300 K / ρ 2 K). However, the document does not specify the synthetic composition range of the material, and the composition of the prepared Ti:Cr2Se3 single crystal deviates from the raw material ratio. Moreover, there are problems such as high iodine concentration, long growth time and small crystal size in the preparation process. It can be seen that it is necessary to seek doping elements that can effectively regulate the performance of materials, clarify their synthesis range and shorten the growth cycle to obtain single-phase and large-sized single crystal materials with precise stoichiometric ratios, so as to provide corresponding materials for the performance regulation and function development of such materials, and provide technical references for the controllable growth of Cr-Se compounds.

[0005] It can be seen that the existing technology still needs to be improved and enhanced. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for preparing vanadium-doped layered selenide and single crystals thereof, aiming to solve the defects of the prior art that titanium-doped Cr2Se3 has insufficient electromagnetic transport performance and it is difficult to obtain large-sized single crystals.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A vanadium-doped layered selenide, wherein the chemical formula of the selenide is V x Cr 2-x Se3, where 0<x≤0.25.

[0009] The vanadium-doped layered selenide has a crystal structure of a rhombohedral phase ( R -3).

[0010] A method for preparing a vanadium-doped layered selenide single crystal, wherein the method uses vanadium powder, chromium powder, and selenium powder as raw materials, uses iodine as a transport agent, and obtains the vanadium-doped layered selenide single crystal as described above by high-temperature sintering and transport growth in dual temperature zones.

[0011] The preparation method of the vanadium-doped layered selenide single crystal comprises the following steps: taking vanadium powder, chromium powder, selenium powder and iodine particles, mixing them evenly, sealing them in a quartz tube, and making the vacuum degree in the quartz tube ≤1 Pa, placing the end of the quartz tube with the material in the high temperature zone of a dual-temperature furnace, and placing the end without the material in the low temperature zone of the dual-temperature furnace; raising the temperature so that the temperature of the low temperature zone end is 875±25°C and the temperature of the high temperature zone end is 975±25°C, keeping the temperature at this temperature gradient for 5 to 10 days, cooling to room temperature, and obtaining the vanadium-doped layered selenide single crystal after cleaning and drying.

[0012] In the method for preparing the vanadium-doped layered selenide single crystal, the molar ratio of the vanadium powder, the chromium powder and the selenium powder is x:(2-x):3, and 0<x≤0.25.

[0013] In the method for preparing the vanadium-doped layered selenide single crystal, the amount of iodine particles added is such that the iodine concentration in the quartz tube is 10 mg / mL.

[0014] In the method for preparing the vanadium-doped layered selenide single crystal, the purity of the vanadium powder, chromium powder, selenium powder and iodine particles is ≥99.99%.

[0015] Beneficial effect: The present invention provides a method for preparing a vanadium-doped layered selenide and a single crystal thereof, wherein the vanadium-doped layered selenide has a chemical formula of V x Cr 2-x Se3 single crystal (0<x≤0.25) has good electromagnetic transport performance and can be used as materials for spin electronic devices, hard disk drives, and micro-electromechanical systems. The preparation method of the vanadium-doped layered selenide is to use vanadium powder, chromium powder, and selenium powder as raw materials, and iodine as a transport agent, and to obtain a chemical formula of V by high temperature sintering. x Cr 2-x Single crystal of Se3 (0<x≤0.25). The single crystal prepared by this method has a size of up to 1 cm, which is a single crystal with ultra-large particles. Therefore, it can provide materials for the physical property research of such materials and the production of functional devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 V in Example 1 0.25 Cr 1.75 Optical photograph of Se3 single crystal.

[0017] Figure 2 V in Example 1 0.25 Cr 1.75 X-ray diffraction analysis pattern of Se3 single crystal.

[0018] Figure 3 V in Example 1 0.25 Cr 1.75 X-ray diffraction analysis spectrum of Se3 powder.

[0019] Figure 4 V in Example 1 0.25 Cr 1.75 Surface morphology of Se3 single crystal.

[0020] Figure 5 V in Example 1 0.25 Cr 1.75 Energy spectrum of Se3 single crystal.

[0021] Figure 6 V in Example 2 0.125 Cr 1.875 X-ray diffraction analysis pattern of Se3 single crystal.

[0022] Figure 7 V in Comparative Example 2 0.25 Cr 1.75 X-ray diffraction analysis pattern of Se3 single crystal.

[0023] Figure 8 V in Example 1 0.25 Cr 1.75 Normalized resistivity curve of Se3 sample versus temperature (the resistivity of the sample at 300 K is the standard).

[0024] Fig. 9 V of Example 2 0.125 Cr 1.875 Normalized resistivity curve of Se3 sample versus temperature (the resistivity of the sample at 300K is the standard).

[0025] Fig.10 This is the X-ray diffraction analysis spectrum of the powder prepared in Comparative Example 1. DETAILED DESCRIPTION

[0026] The present invention provides a method for preparing a vanadium-doped layered selenide and a single crystal thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the following examples. It should be understood that the specific examples described herein are only used to explain the present invention and are not intended to limit the present invention.

[0027] In a first aspect, the present invention provides a vanadium-doped layered selenide, the chemical formula of which is V x Cr 2-x Se3, where 0<x≤0.25, the crystal structure of the selenide is rhombohedral phase ( R -3), with a layered structure, the selenide achieves successful doping of element V without changing the rhombohedral phase Cr2Se3 crystal structure. And by adjusting the doping amount of V, V x Cr 2-x Se3 materials exhibit different conductive properties (among which, at low temperatures (below 50 K) a change from conductor to semiconductor occurs), and have good prospects for application in spin electronics devices, hard disk drives, micro-electromechanical systems, and other fields.

[0028] The second aspect of the present invention also provides a method for preparing a vanadium-doped layered selenide single crystal, wherein the method uses high-purity vanadium powder, chromium powder, and selenium powder as raw materials, and uses iodine as a transport agent, and grows through high-temperature dual-temperature zone gas phase transport to obtain a single crystal with a chemical formula of V x Cr 2-x Single crystal of Se3 (where 0<x≤0.25).

[0029] In the preparation method, chemical vapor transport is used for preparation, which has the characteristics of simple steps and easy implementation. In addition, during the preparation process, the materials can be accurately fed according to the element stoichiometric ratio of the target product molecular formula to obtain single crystals with accurate stoichiometric ratios. The size of the obtained single crystals is up to 1 cm, which can be used for studying V x Cr 2-x The properties and applications of materials such as Se3 are provided.

[0030] To obtain V for a specific molecular formula x Cr 2-x Se3 single crystal, the raw material ratio and firing temperature need to be well controlled. In this regard, in a preferred embodiment, the method includes the steps of: taking vanadium powder, chromium powder, and selenium powder in a molar ratio of x: (2-x): 3, wherein 0 < x ≤ 0.25, and adding iodine particles at a concentration of 10 mg / mL based on the volume of the quartz tube, mixing the vanadium powder, chromium powder, selenium powder, and iodine particles evenly, sealing them in a quartz tube, and making the vacuum degree in the quartz tube ≤ 1 Pa, placing the end of the quartz tube with material in the high temperature zone of a dual temperature furnace, and placing the end without material in the low temperature zone of the dual temperature furnace; heating the dual temperature furnace, and controlling the heating rate at 2 to 3 °C / min, so that the temperature at the low temperature zone end is 875 ± 25 °C, and the temperature at the high temperature zone end is 975 ± 25 °C, keeping the temperature at this temperature gradient for 5 to 10 days, cooling to room temperature, washing by alcohol immersion, and drying to obtain vanadium-doped layered selenide crystals.

[0031] Through this preparation method, V with a size larger than 1 cm can be obtained. x Cr 2-x Se3 single crystal (0<x≤0.25), due to its large size and layered structure, can be peeled off to obtain a single layer or several layers of thin layer materials, which is convenient for studying its properties, or using the special properties of thin layer materials to expand its application and provide materials for its research and application.

[0032] In the above preparation method, the raw material ratio and sintering temperature are the key factors to obtain large-sized V x Cr 2-x The key factors of Se3 single crystal are that the raw material ratio is too high or too low, or the temperature in the low temperature zone and the high temperature zone is too high or too low, it is difficult to obtain the corresponding single crystal. Therefore, in the preparation process, the raw material ratio needs to be controlled within the range of x: (2-x): 3 (where 0<x≤0.25), and the sintering temperature is such that the temperature in the low temperature zone is 875±25 ℃, the temperature in the high temperature zone is 975±25 ℃, and the temperature difference between the high and low temperature zones is about 100 ℃, preferably 100 ℃. Under such conditions, large-sized single crystals can be obtained with short preparation time and low energy consumption.

[0033] In addition, the purity of the raw materials will also affect the formation of single crystals, so the purity of vanadium powder, chromium powder, selenium powder and iodine particles must be ≥99.99%.

[0034] Furthermore, the concentration of iodine particles added must be controlled to avoid long preparation time and increased cleaning difficulty due to excessive iodine concentration. The optimal iodine concentration is 10 mg / mL, which has better transport properties, enables single crystals to grow faster, shortens growth time, and reduces furnace energy consumption, while making subsequent alcohol immersion and cleaning easier.

[0035] To further illustrate the method for preparing a vanadium-doped layered selenide single crystal provided by the present invention, the following examples are provided. Example 1

[0036] A V x Cr 2-x The preparation method of Se3 (x=0.25) single crystal comprises the following steps: taking vanadium powder, chromium powder and selenium powder in a molar ratio of 0.25:1.75:3, adding iodine particles at a concentration of 10 mg / mL based on the volume of a quartz tube, mixing the vanadium powder, chromium powder, selenium powder and iodine particles evenly, sealing them in a quartz tube, and the vacuum degree in the quartz tube is ≤1 Pa, placing the end of the quartz tube with the material in the high temperature zone of a double temperature furnace, and placing the end without the material in the low temperature zone of the double temperature furnace; heating, the heating time is 380 min, making the temperature of the low temperature zone 875±25°C, and the temperature of the high temperature zone 975±25°C, keeping the temperature at the temperature gradient for 5 days, cooling to room temperature, washing by alcohol immersion, and drying to obtain the following Figure 1 A vanadium-doped layered selenide crystal is shown.

[0037] The morphology, structure and chemical composition of the material obtained in Example 1 were analyzed and characterized by optical microscopy, X-ray diffractometer and scanning electron microscopy. The results are as follows: Figure 1-5 As shown, Figure 1 This is an optical photograph of the single crystal prepared in Example 1. The size of the single crystal is as long as 1 cm, which is a single crystal with ultra-large particles. It is found from observation that the single crystal is a crystal with a layered structure. Figure 2 This is the X-ray diffraction analysis spectrum of the material obtained in Example 1, Figure 3 This is the X-ray diffraction analysis spectrum of the material obtained in Example 1 after being ground into powder, Figure 4 This is the surface morphology of the material obtained in Example 1. Figure 5 is the energy spectrum of the material obtained in Example 1, Figure 2-5 It can be determined that the material obtained under this condition is a single crystal, and its chemical composition is V 0.25 Cr 1.75 Se3, the crystal structure is rhombohedral phase ( R -3). Example 2

[0038] A V x Cr 2-x The preparation method of Se3 (x=0.125) comprises the following steps: taking vanadium powder, chromium powder and selenium powder in a molar ratio of 0.125:1.875:3, adding iodine particles at a concentration of 10 mg / mL based on the volume of a quartz tube, mixing the vanadium powder, chromium powder, selenium powder and iodine particles evenly, sealing them in a quartz tube, and the vacuum degree in the quartz tube is ≤1 Pa, placing one end of the quartz tube with the material in the high temperature zone of a double-temperature furnace, and placing the other end without the material in the low temperature zone of the double-temperature furnace; heating for 380 min, making the temperature of the low temperature zone 875±25°C, and the temperature of the high temperature zone 975±25°C, keeping the temperature at the temperature gradient for 5 days, cooling to room temperature, and obtaining vanadium-doped layered selenide crystals after washing and drying.

[0039] The morphology, structure and chemical composition of the obtained material were analyzed and characterized by optical microscopy, X-ray diffractometer and scanning electron microscopy, and it was determined that the material obtained under this condition was a single crystal ( Figure 6 is the X-ray diffraction analysis spectrum of the obtained material), its chemical composition is V 0.125 Cr 1.875 Se3, the crystal structure is rhombohedral phase ( R -3).

[0040] Comparative Example 1

[0041] A vanadium-doped selenide, the preparation method of which is substantially the same as the method of Example 1, except that the molar ratio of vanadium powder, chromium powder and selenium powder is 0.3:1.7:3.

[0042] The material obtained in Comparative Example 1 was subjected to powder X-ray diffraction analysis, and its spectrum is as follows: Fig.10 As shown by Fig.10 It can be seen that the material R -3 and I 2 / m The two phases coexist. Fig.10 The diffraction peaks marked by arrows belong to I 2 / m It can be seen from the diffraction peaks of the phase that single crystals cannot be obtained using this raw material ratio.

[0043] Comparative Example 2

[0044] A vanadium-doped selenide, the preparation method of which is substantially the same as the method of Example 1, the difference being that the temperature of the low temperature zone is 925±25°C, and the temperature of the high temperature zone is 975±25°C.

[0045] The morphology, structure and chemical composition of the material obtained in Comparative Example 2 were analyzed and characterized by optical microscopy, X-ray diffractometer and scanning electron microscopy. The X-ray diffraction analysis spectrum is as follows: Figure 7 As shown by Figure 7 It can be seen that the material obtained under this condition is a single crystal, and its chemical composition is V 0.25 Cr 1.75 Se3, the crystal structure is rhombohedral phase ( R -3). However, by comparing with Example 1, it is found that the size of the single crystal obtained in Comparative Example 2 is smaller, which shows that when the temperature difference between the high temperature zone and the low temperature zone is small, it will affect the size of the single crystal.

[0046] Comparative Example 3

[0047] A vanadium-doped selenide, the preparation method of which is substantially the same as the method of Example 1, except that the temperature of the low temperature zone is 400±25°C, and the temperature of the high temperature zone is 500±25°C.

[0048] However, since the temperatures of the low temperature zone and the high temperature zone in Comparative Example 3 are relatively low, gas phase transport is not easy to occur, so that no single crystal is generated in the low temperature zone under the experimental conditions.

[0049] It should be noted that in Examples 1-2 and Comparative Examples 1-3, the purity of the vanadium powder, chromium powder, selenium powder and iodine particles is 99.99%.

[0050] In addition, the V obtained in Example 1 0.25 Cr 1.75 Se3 material and V obtained in Example 2 0.125 Cr 1.875 The resistivity of Se3 material was tested as a sample, with the resistivity of the sample at 300 K as the reference standard. The test results are shown in Figure 8 and Fig. 9 As shown. Figure 8 It can be seen that V 0.25 Cr 1.75 Se3 exhibits metallic conductivity in the test temperature range. Fig. 9 It can be seen that V 0.125 Cr 1.875 When the measurement temperature of Se3 is above about 50 K, the resistivity increases with the increase of temperature, indicating that the sample exhibits metallic conductivity; when it is below 50 K, its resistivity decreases slightly with the increase of temperature, showing semiconductor conductivity. It can be seen that the change of V doping amount can achieve effective regulation of the electromagnetic transport properties of the material.

[0051] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and inventive concept of the present invention, and all these changes or substitutions should fall within the protection scope of the claims attached to the present invention.

Claims

1. A vanadium-doped layered selenide single crystal, characterized in that: The chemical formula of the selenide single crystal is V x Cr 2- x Se3, wherein 0<x≤0.25; the crystal structure of the selenide single crystal is a rhombohedral phase R -3.

2. A method for preparing a vanadium-doped layered selenide single crystal, characterized in that: The method uses vanadium powder, chromium powder and selenium powder as raw materials, uses iodine as a transport agent, and obtains the single crystal of vanadium-doped layered selenide as claimed in claim 1 through high-temperature sintering and transport growth in double temperature zones.

3. The method for preparing a vanadium-doped layered selenide single crystal according to claim 2, characterized in that: The method comprises the steps of taking vanadium powder, chromium powder, selenium powder and iodine particles, mixing them evenly, sealing them in a quartz tube, making the vacuum degree in the quartz tube ≤1Pa, placing one end of the quartz tube with materials in a high temperature zone of a dual-temperature furnace, and placing the other end without materials in a low temperature zone of the dual-temperature furnace; heating the tube so that the temperature of the low temperature zone end is 875±25°C and the temperature of the high temperature zone end is 975±25°C, keeping the temperature at the temperature gradient for 5 to 10 days, cooling to room temperature, and obtaining a vanadium-doped layered selenide single crystal after cleaning and drying.

4. The method for preparing a vanadium-doped layered selenide single crystal according to claim 3, characterized in that: The molar ratio of the vanadium powder, the chromium powder and the selenium powder is x:(2-x):3, and 0<x≤0.

25.

5. The method for preparing a vanadium-doped layered selenide single crystal according to claim 3, characterized in that: The amount of iodine particles added was such that the iodine concentration in the quartz tube was 10 mg / mL.

6. The method for preparing a vanadium-doped layered selenide single crystal according to claim 2, characterized in that: The purity of the vanadium powder, chromium powder, selenium powder and iodine particles is ≥99.99%.

Citation Information