Self-healing aramid fiber laminated paper and preparation method thereof
By setting a repair layer of epoxy resin composite nanocellulose microcapsules on aramid insulating paper, the material can self-heal after damage, solving the problem of easy damage of traditional insulating materials and improving the reliability and service life of insulating materials. .
Patent Information
- Application Number
- CN202411165322.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Traditional insulation materials are prone to minor damage during long-term use, resulting in a decrease in mechanical and insulation properties, making it difficult to balance the reliability and service life of electrical equipment.
Self-healing aramid laminated paper is used. By setting an epoxy resin composite nanocellulose microcapsule repair layer on the surface of the aramid insulating paper core layer, the microcapsules are used to release epoxy resin and nanocellulose when damaged to fill the damaged area. and cures, restoring the material's insulating properties and mechanical strength.
Significantly improves the reliability and safety of dielectric materials, extends the service life of electrical equipment, and reduces the need for maintenance and replacement.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, in particular to a self-healing aramid laminated paper and a preparation method thereof. Background Art
[0002] Insulating materials play a vital role in power systems, electronic equipment, and various high-performance motors. These application scenarios place extremely high demands on insulating materials, requiring not only excellent electrical insulation performance, mechanical strength, and heat resistance, but also long-term stability and reliability. Although traditional insulating materials perform well in some aspects, it is difficult to meet all requirements, especially in the long-term use process, they are prone to minor damage, which will gradually accumulate and eventually lead to a decrease in mechanical and insulation performance, and even failure. Therefore, the development of an insulating material with self-healing function has become the key to improving the reliability of electrical equipment and extending its service life. Summary of the invention
[0003] In view of this, the technical problem to be solved by the present invention is to provide a self-healing aramid laminated paper and a preparation method thereof. The self-healing aramid laminated paper provided by the present invention can self-heal and repair after damage, so that the mechanical strength and insulation performance are restored, which significantly improves the reliability and safety of the dielectric material, reduces the performance degradation caused by material aging or minor damage, helps to extend the service life of electrical equipment, and reduces the need for maintenance and replacement.
[0004] The present invention provides a self-healing aramid laminated paper, comprising: an aramid insulation paper core layer and an epoxy resin composite nano-cellulose microcapsule repair layer arranged on the surface of the aramid insulation paper core layer; the epoxy resin composite nano-cellulose microcapsule repair layer is prepared from raw materials including a nano-cellulose complex, epoxy resin and a temperature-sensitive polymer.
[0005] In the self-healing aramid laminated paper provided by the present invention, the epoxy resin composite nano-cellulose microcapsule repair layer is arranged on the surface of the aramid insulation paper core layer. Specifically, the epoxy resin composite nano-cellulose microcapsule repair layer is arranged on the upper surface and the lower surface of the aramid insulation paper core layer. The thickness of the epoxy resin composite nano-cellulose microcapsule repair layer of the present invention is 10~15 μm. The self-healing aramid laminated paper provided by the present invention is provided with an epoxy resin composite nano-cellulose microcapsule repair layer. When microcracks or minor damages appear on the material, the microcapsules at the corresponding positions will rupture, releasing epoxy resin / nanocellulose to fill the damaged area, and solidify under certain conditions to restore the insulation performance and mechanical strength of the material.
[0006] In the self-healing aramid laminated paper provided by the present invention, the epoxy resin composite nano-cellulose microcapsule repair layer is prepared from raw materials including a nano-cellulose composite, an epoxy resin and a temperature-sensitive polymer. Specifically, the nanocellulose composite of the present invention is prepared from raw materials including nanocellulose and polyurethane in a mass ratio of 1:(0.6-0.8); the nanocellulose is selected from at least one of carbon nanocellulose, cellulose nanocrystals (CNC) or bacterial cellulose (BC); the temperature-sensitive polymer is selected from at least one of poly(N-isopropylacrylamide), poly(N-ethylacrylamide), poly(N,N-diethylacrylamide) or poly(N,N-dimethylacrylamide); the modified epoxy resin is prepared from raw materials including unmodified epoxy resin, toughness modifier, tertiary amine compound, curing agent and accelerator, and the mass ratio of the unmodified epoxy resin, toughness modifier and tertiary amine compound is (15-20):(3-5.5):(0.8-1.6); the mass ratio of the total mass of the unmodified epoxy resin, toughness modifier and tertiary amine compound to the curing agent and the accelerator is (85-100):(70-80):(1.2-1.8). In certain embodiments of the present invention, the toughness modifier is selected from at least one of carboxyl-terminated polyester elastomers, polyurethane elastomers, carboxyl-terminated polyurethanes or acrylate elastomers; the tertiary amine compound is selected from at least one of triethylamine, trimethylamine or N,N-dimethylaniline; the curing agent is selected from at least one of methylhexahydrophthalic anhydride, adipic dianhydride, methyltetrahydrophthalic anhydride or vinyltriethoxysilane; the accelerator is selected from at least one of 2,4,6-tris(dimethylaminomethyl)phenol (Q-DMP 30), N,N-dimethylaminomethylphenol (DMP-10), N,N-dimethylbenzylamine (BDMA) or triethylenetetramine (TETA).
[0007] In the self-healing aramid laminated paper provided by the present invention, the aramid insulation paper core layer is made of aramid fibers and boron nitride nanotubes; the filling concentration of the boron nitride nanotubes in the aramid insulation paper core layer is 5 wt%~15 wt%. In certain embodiments of the present invention, the thickness of the aramid insulation paper core layer is 25 μm~35 μm, preferably 30 μm. The aramid insulation paper core layer of the present invention is a composite of aramid fibers and boron nitride nanotubes, and has excellent insulation properties, mechanical properties and temperature resistance, and to a certain extent resists the negative effects caused by minor damage to the surface material.
[0008] The present invention also provides a method for preparing the self-healing aramid laminated paper described in any of the above technical solutions, comprising the following steps: coating the surface of the aramid insulation paper core layer with an epoxy resin composite nanocellulose microcapsule dispersion, and hot pressing to obtain the self-healing aramid laminated paper.
[0009] The aramid insulation paper core layer of the present invention is made of aramid fibers and boron nitride nanotubes. Specifically, after the aramid fibers are sheared, the obtained material is subjected to ultrasonic treatment for 2.5 h to 3.5 h, and then the obtained material is mixed with the boron nitride nanotubes and ultrasonic treatment is continued for 1.5 h to 2.5 h, and then pulping and papermaking are performed to obtain the aramid insulation paper core layer. The shearing and ultrasonic treatment of the aramid fibers of the present invention can improve the dispersion and uniformity of the fibers. The beating time of the present invention is 35 min to 45 min, and the beating speed is 2500 rpm to 3500 rpm. After beating, the present invention also includes screening to remove large particles and remove bubbles. Before the aramid fibers are sheared, the present invention also includes pre-treating the aramid fibers, specifically, washing the aramid fibers with organic solvents, water and alkaline solutions to remove surface impurities and grease and improve the hydrophilicity of the fibers.
[0010] The epoxy resin composite nanocellulose microcapsule dispersion of the present invention is prepared from epoxy resin composite nanocellulose microcapsules and epoxy resin-based adhesive. Specifically, the present invention mixes epoxy resin composite nanocellulose microcapsules and epoxy resin-based adhesive, stirs for 1 h to 2 h, and then performs vacuum degassing to eliminate air bubbles introduced during the mixing process to obtain the epoxy resin composite nanocellulose microcapsule dispersion. The epoxy resin-based adhesive of the present invention is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin or epoxy novolac resin. The mass proportion of the epoxy resin composite nanocellulose microcapsules in the dispersion of the present invention is 5 wt% to 20 wt%.
[0011] In the dispersion of the present invention, the epoxy resin composite nanocellulose microcapsules are prepared from a nanocellulose composite solution, an epoxy resin emulsion and a temperature-sensitive polymer solution. Specifically, the present invention mixes the nanocellulose composite solution and the epoxy resin emulsion to obtain a microcapsule suspension having a preliminary shell, and then adds the temperature-sensitive polymer solution to the microcapsule suspension to obtain the epoxy resin composite nanocellulose microcapsule precursor liquid, and solidifies, washes and dries the obtained precursor liquid to obtain the epoxy resin composite nanocellulose microcapsules. More specifically, the solidification is: adjusting the pH of the obtained precursor liquid to 2-3, and then heating at 55-65°C for 1.5-2.5 h, and heating to 115-125°C for 3.5-4.5 h to obtain the epoxy resin composite nanocellulose microcapsules.
[0012] In the process of preparing the epoxy resin composite nanocellulose microcapsule of the present invention, the temperature sensitive polymer in the temperature sensitive polymer solution is the same as above, and no further description is given; the nanocellulose composite solution is prepared from a nanocellulose solution and a polyurethane solution, and the concentration of the nanocellulose solution is 15 wt%~25 wt%. Specifically, the nanocellulose composite solution is prepared by the following method: dispersing nanocellulose in water, heating and stirring at 55°C~65°C for 35 min~45 min to obtain a nanocellulose solution; mixing a polyurethane solution and the nanocellulose solution, heating and stirring at 55°C~65°C for 25 min~35 min to obtain a nanocellulose composite solution. The nanocellulose and polyurethane of the present invention are the same as above, and no further description is given.
[0013] In the process of preparing the epoxy resin composite nanocellulose microcapsules of the present invention, the epoxy resin emulsion is a modified epoxy resin emulsion, which is obtained by mixing unmodified epoxy resin, toughness modifier, tertiary amine compound, curing agent, accelerator and surfactant solution. Specifically, the modified epoxy resin emulsion of the present invention is prepared by the following method: adding toughness modifier solution and tertiary amine compound to unmodified epoxy resin solution, and then stirring the obtained material liquid at 65℃~75℃ for 55 min~65 min, and then adding curing agent and accelerator thereto, stirring for 0.5 h~1.5 h, and then mixing the obtained material with surfactant solution, heating at 75℃~85℃ for 6 h~10 h, and obtaining the modified epoxy resin emulsion. The surfactant in the surfactant solution of the present invention is selected from at least one of hexadecyltrimethylammonium bromide, sodium dodecyl sulfate or polyethylene glycol octylphenyl ether, and the surfactant concentration in the surfactant solution is 1.5wt%~4wt%. In the present invention, the total volume of the material obtained by mixing the unmodified epoxy resin, the toughness modifier, the tertiary amine compound, the curing agent and the accelerator accounts for 15% to 30% of the total volume of the modified epoxy resin emulsion. The toughness modifier, the tertiary amine compound, the curing agent and the accelerator of the present invention are the same as those described above and will not be described in detail.
[0014] The present invention coats the surface of the aramid insulation paper core layer with an epoxy resin composite nanocellulose microcapsule dispersion, and hot presses to obtain a self-healing aramid laminated paper. Specifically, after the aramid insulation paper core layer is laid flat, the present invention coats the upper and lower surfaces of the aramid insulation paper core layer with an epoxy resin composite nanocellulose microcapsule dispersion, and then hot presses the obtained material, and vacuum dries to obtain a self-healing aramid laminated paper. The hot pressing temperature of the present invention is 100°C to 140°C; the hot pressing time is 15 min to 25 min; the hot pressing pressure is 130 MPa to 170 MPa. The coating time of the present invention is 4 h to 8 h. The aramid insulation paper core layer of the present invention and the epoxy resin composite nanocellulose microcapsules in the dispersion are the same as those described above, and will not be repeated. The self-healing aramid laminated paper finally obtained by the present invention is also the same as those described above, and will not be repeated.
[0015] The present invention provides a self-healing aramid laminated paper and a preparation method thereof. Based on the need to improve the self-healing ability of insulating materials, the present invention utilizes microcapsule technology to prepare epoxy resin / nanocellulose microcapsules, and evenly sprays them on the upper and lower surfaces of aramid insulating paper to obtain aramid laminated insulating paper. When microcracks or slight damage appear in the material, the microcapsules at the corresponding positions will rupture, releasing epoxy resin / nanocellulose to fill the damaged area, and solidify under certain conditions to restore the insulating properties and mechanical strength of the material. This self-healing mechanism greatly improves the reliability and safety of insulating materials and extends the service life of the materials. The prepared epoxy resin / nanocellulose microcapsule self-healing aramid laminated paper not only meets the needs of the power and electronics industries for high-performance insulating materials, but also provides a new solution for improving the reliability and safety of equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a scanning electron microscope image of the epoxy resin / nanocellulose microcapsule obtained in Example 1 of the present invention;
[0017] Figure 2 This is a scanning electron microscope image of the aramid fiber before pretreatment used in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0018] The present invention discloses a self-healing aramid laminated paper and a method for preparing the same. A person skilled in the art can refer to the contents of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to a person skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0019] The present invention will be further described below in conjunction with embodiments:
[0020] Example 1
[0021] The preparation of the epoxy resin / nanocellulose microcapsule self-healing aramid laminated paper of the present invention comprises the following steps S1, S2 and S3:
[0022] S1. Preparation of epoxy resin / nanocellulose microcapsules, comprising the following steps:
[0023] S11, Epoxy resin pretreatment
[0024] First, epoxy resin was weighed and placed in a 45°C constant temperature water bath for heating for 15 min, and then acetone was added and stirred with a magnetic stirrer for 30 min to obtain epoxy resin 1. Secondly, carboxyl-terminated polyester elastomer (toughness modifier) was weighed, acetone was added for mixing, and a 35°C constant temperature magnetic stirrer was used for stirring for 30 min to obtain a modifier mixed solution. Subsequently, the carboxyl-terminated polyester elastomer mixed solution was slowly added to the epoxy mixed solution 1, and a 55°C constant temperature magnetic stirrer was used for high-speed stirring. After stirring for 30 min, triethylamine (tertiary amine compound) was added and continued to stir for 1 h to obtain epoxy resin 2. Finally, epoxy resin 2 was placed in a 70°C constant temperature oil bath and stirred for 60 min. After completely removing acetone, it was degassed under vacuum to obtain bubble-free epoxy resin 3. Among them, the mass ratio of epoxy resin, carboxyl-terminated polyester elastomer and tertiary amine compound was 15:3:0.8.
[0025] S12, mixing of epoxy resin and curing agent
[0026] The epoxy resin 3, methyl hexahydrophthalic anhydride (curing agent) and Q-DMP 30 (accelerator) were weighed and mixed, and stirred at room temperature for 1 h to obtain epoxy resin 4. The mass ratio of epoxy resin 3, curing agent and accelerator was 85:70:1.2.
[0027] S13. Preparation of nanocellulose aqueous solution
[0028] Nanocellulose CNF was weighed and dispersed in deionized water, heated and stirred in a constant temperature water bath at 60 °C for 40 min to prepare a solution with a concentration of 15 wt% and marked as CNF aqueous solution.
[0029] S14. Preparation of nanocomposite solution
[0030] Add the polyurethane solution to the CNF aqueous solution, heat and stir in a 60°C constant temperature water bath for 30 min, and stir thoroughly to form a uniform nanocomposite solution, wherein the mass ratio of CNF to polyurethane is 1:0.6.
[0031] S15, Emulsification of microcapsule core materials
[0032] Weigh hexadecyltrimethylammonium bromide (surfactant) and disperse it in deionized water, stir at 80°C for 15 minutes to obtain a surfactant aqueous solution; slowly drop the above epoxy resin 4 into the hexadecyltrimethylammonium bromide solution, stir with a magnetic stirrer during the dropwise addition, then perform ultrasonic treatment for 30 minutes, heat to 80°C, react for 6 hours to form a stable epoxy resin emulsion, which is marked as epoxy resin 5. Among them, epoxy resin 4 accounts for 15% of the total volume.
[0033] S16. Formation of microcapsule shell
[0034] The above-mentioned nanocomposite solution was slowly added to the epoxy resin 5, and stirred continuously at a constant temperature of 60°C for 2 h to obtain a microcapsule suspension with a preliminary shell, which was marked as microcapsule suspension 1; then the poly (N-isopropylacrylamide) solution (temperature-sensitive polymer solution) was slowly added to the microcapsule suspension 1 to obtain epoxy resin / nanocellulose microcapsules.
[0035] S17, microcapsule curing process
[0036] The pH value of the epoxy resin / nanocellulose microcapsule suspension was first adjusted to 2.3 by hydrochloric acid (acid regulator) and maintained at 60 °C for 2 h to promote uniform curing, and then the temperature was increased to 120 °C and maintained for 4 h to complete the curing process.
[0037] S18, post-processing of microcapsules
[0038] The cured epoxy resin microcapsules were repeatedly washed with deionized water, centrifuged to remove impurities and excess surfactants in the solution, and then freeze-dried for 36 h to prepare epoxy resin / nanocellulose microcapsules for use. Figure 1 As shown, Figure 1 This is a scanning electron microscope image of the epoxy resin / nanocellulose microcapsule obtained in Example 1 of the present invention.
[0039] S2. Preparation of aramid insulation paper
[0040] S21, Aramid fiber pretreatment
[0041] The aramid fiber was cut into small pieces of about 0.5 cm in length, soaked in acetone for ultrasonic treatment for 36 h, washed repeatedly with deionized water, then added to an alkaline environment, stirred for 2 h, washed repeatedly with deionized water again, and vacuum dried at 45 °C for 24 h to remove surface impurities and grease and improve the hydrophilicity of the fiber. Figure 2 As shown, Figure 2 This is a scanning electron microscope image of the aramid fiber before pretreatment used in a specific embodiment of the present invention.
[0042] S22. Preparation of aramid pulp
[0043] The treated aramid fibers were weighed and sheared at high speed to break them into fine microfibers, and then dispersed in deionized water and ultrasonically treated for 3 h to improve fiber dispersion and uniformity. The ultrasonically treated aramid fibers were compounded with boron nitride nanotubes (BNNTs), ultrasonically treated again for 2 h, and placed in a pulping machine. After the pulping was completed, large particles were first removed by screening, and then ultrasonically treated to remove bubbles to obtain bubble-free uniform aramid pulp, which was marked as AF / BNNT. Among them, the BNNT filling concentration was 5 wt%, the pulping time was 40 min, and the pulping speed was 3000 rpm.
[0044] S23. Preparation of aramid insulation paper
[0045] The bubble-free and uniform aramid pulp treated as above was fed into a papermaking machine to prepare AF / BNNT aramid insulation paper having a thickness of 30 μm.
[0046] S3. Preparation of self-healing aramid laminated paper using epoxy resin / nanocellulose microcapsules
[0047] S31. Preparation of epoxy resin / nanocellulose microcapsule dispersion
[0048] The epoxy resin / nanocellulose microcapsules were slowly added to the epoxy resin-based adhesive on a constant temperature magnetic stirrer at 45°C and stirred for 1 h. After stirring, vacuum degassing was performed to remove air bubbles introduced during the mixing process. The amount of epoxy resin / nanocellulose microcapsules added accounted for 10% of the total weight.
[0049] S32, Preparation of Aramid Laminated Rough Paper
[0050] The AF / BNNT aramid insulation paper was laid flat, and the epoxy resin / nanocellulose microcapsule dispersion was evenly sprayed on the upper and lower surfaces of the aramid insulation paper using a sprayer to obtain aramid laminated insulation paper rough paper; then the aramid laminated paper was obtained by high-temperature hot pressing and vacuum drying at 45°C for 48 hours. The spraying time was 4 hours, the spraying thickness was 10 μm, the hot pressing temperature was 120°C, the hot pressing time was 20 minutes, and the pressure was 150 MPa.
[0051] Example 2
[0052] Compared with Example 1, the difference is that in step S11, the mass ratio of the epoxy resin, the carboxyl-terminated polyester elastomer and the tertiary amine compound is 15:5.5:1.6.
[0053] Example 3
[0054] Compared with Example 1, the difference is that in step S12, the mass ratio of the epoxy resin 3, the curing agent and the accelerator is 85:80:1.8.
[0055] Example 4
[0056] Compared with Example 1, the difference is that the concentration of the CNF aqueous solution in step S13 is 20 wt%.
[0057] Example 5
[0058] Compared with Example 1, the difference is that the concentration of the CNF aqueous solution in step S13 is 25 wt%.
[0059] Example 6
[0060] Compared with Example 1, the difference is that in step S14, the mass ratio of CNF to polyurethane is 1:0.8.
[0061] Example 7
[0062] Compared with Example 1, the difference is that in step S15, the epoxy resin 4 accounts for 20% of the total volume.
[0063] Example 8
[0064] Compared with Example 1, the difference is that in step S15, the epoxy resin 4 accounts for 30% of the total volume.
[0065] Example 9
[0066] Compared with Example 1, the difference is that the BNNT filling concentration in step S22 is 10 wt%.
[0067] Example 10
[0068] Compared with Example 1, the difference is that the BNNT filling concentration in step S22 is 15 wt%.
[0069] Embodiment 11
[0070] Compared with Example 1, the difference is that the amount of epoxy resin / nanocellulose microcapsules added in step S31 accounts for 20% of the total weight.
[0071] Example 12
[0072] Compared with Example 1, the difference is that the spraying time in step S32 is 8 h and the spraying thickness is 15 μm.
[0073] Comparative Example 1
[0074] Compared with Example 1, the difference is that the aramid fibers in step S21 are directly fed into the papermaking machine after pulping, without compounding with BNNT, and without spraying epoxy resin / nanocellulose microcapsule dispersion on the upper and lower surfaces, and aramid insulating paper is made after high-temperature hot pressing.
[0075] Comparative Example 2
[0076] Compared with Example 1, the difference is that the aramid pulp in step S22 is directly fed into the papermaking machine without spraying the upper and lower surfaces with epoxy resin / nanocellulose microcapsule dispersion, and the AF / BNNT aramid insulation paper is made after high temperature hot pressing. Among them, the ratios between the substances are the same, and the BNNT filling concentration is 5 wt%.
[0077] Comparative Example 3
[0078] Compared with Example 1, the difference is that the core aramid insulation paper is not compounded with BNNT. The proportions of the substances are the same.
[0079] Comparative Example 4
[0080] The other preparation steps of this comparative example are the same as those of Example 1, except that: no epoxy resin / nanocellulose microcapsules are prepared, and in the preparation of the aramid laminated paper rough paper in step S32, the upper layer material of the sprayed aramid laminated paper is epoxy resin 5, and the lower layer material of the sprayed aramid laminated paper is a nanocomposite solution, and the spraying thickness and the ratio between the materials are the same.
[0081] In order to evaluate the performance and self-healing ability of a self-healing aramid laminated paper using epoxy resin / nanocellulose microcapsules, the present invention uses a precise control method to make fine cuts or holes on the insulating paper in the above embodiments and comparative examples to simulate actual damage, and sets the ambient temperature after damage to 120°C to promote the self-healing of epoxy resin / nanocellulose microcapsules, and tests its performance before damage, after damage, and after self-healing (self-healing for 24 hours at 45°C). The mechanical properties test results are shown in Table 1, and the breakdown characteristics test results are shown in Table 2.
[0082] Table 1
[0083]
[0084] Table 2
[0085]
[0086] It can be seen from Table 1 and Table 2 that the epoxy resin / nanocellulose microcapsule self-healing aramid laminated paper and its preparation method provided by the present invention can effectively restore the mechanical strength and insulation performance of the insulating paper after minor damage, significantly improve the reliability and safety of the dielectric material, reduce the performance degradation caused by material aging or minor damage, help to extend the service life of electrical equipment, and reduce the need for maintenance and replacement.
[0087] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A self-healing aramid laminated paper, characterized in that: include: An aramid insulation paper core layer and an epoxy resin composite nanocellulose microcapsule repair layer arranged on the surface of the aramid insulation paper core layer; The epoxy resin composite nano-cellulose microcapsule repairing layer is prepared from raw materials including a nano-cellulose composite, an epoxy resin and a temperature-sensitive polymer.
2. The self-healing aramid laminated paper according to claim 1, characterized in that: The nanocellulose composite is prepared from raw materials including nanocellulose and polyurethane; The epoxy resin is a modified epoxy resin, which is prepared from raw materials including unmodified epoxy resin, toughness modifier, tertiary amine compound, curing agent and accelerator.
3. The self-healing aramid laminated paper according to claim 2, characterized in that: The mass ratio of the nanocellulose to the polyurethane is 1:(0.6-0.8); The mass ratio of the unmodified epoxy resin, toughness modifier and tertiary amine compound is (15-20): (3-5.5): (0.8-1.6); The mass ratio of the total mass of the unmodified epoxy resin, the toughness modifier and the tertiary amine compound to the mass ratio of the curing agent and the accelerator is (85-100): (70-80): (1.2-1.8).
4. The self-healing aramid laminated paper according to claim 2, characterized in that: The nanocellulose is selected from at least one of carbon nanocellulose, cellulose nanocrystals or bacterial cellulose; The temperature sensitive polymer is selected from at least one of poly(N-isopropylacrylamide), poly(N-ethylacrylamide), poly(N,N-diethylacrylamide) or poly(N,N-dimethylacrylamide); The toughness modifier is selected from at least one of a carboxyl-terminated polyester elastomer, a polyurethane elastomer, a carboxyl-terminated polyurethane or an acrylate elastomer; The tertiary amine compound is selected from at least one of triethylamine, trimethylamine and N,N-dimethylaniline; The curing agent is selected from at least one of methylhexahydrophthalic anhydride, adipic anhydride, methyltetrahydrophthalic anhydride or vinyltriethoxysilane; The accelerator is selected from at least one of Q-DMP 30, N,N-dimethylaminomethylphenol (DMP-10), N,N-dimethylbenzylamine (BDMA) or triethylenetetramine (TETA).
5. The self-healing aramid laminated paper according to claim 1, characterized in that: The aramid insulation paper core layer is made of aramid fibers and boron nitride nanotubes; The filling concentration of the boron nitride nanotubes in the aramid insulation paper core layer is 5 wt% to 15 wt%.
6. The self-healing aramid laminated paper according to claim 1, characterized in that: The thickness of the epoxy resin composite nanocellulose microcapsule repair layer is 10 μm to 15 μm.
7. The method for preparing the self-healing aramid laminated paper according to any one of claims 1 to 6, characterized in that: The following steps are involved: The epoxy resin composite nano-cellulose microcapsule dispersion is coated on the surface of the aramid insulation paper core layer, and hot pressing is performed to obtain a self-healing aramid laminated paper.
8. The preparation method according to claim 7, characterized in that: The mass proportion of the epoxy resin composite nanocellulose microcapsules in the dispersion is 5 wt% to 20 wt%.
9. The preparation method according to claim 7, characterized in that: The epoxy resin composite nanocellulose microcapsules are prepared by the following method: The nanocellulose composite solution, epoxy resin emulsion and temperature-sensitive polymer solution were mixed and the pH was adjusted to 2-3, and then heated at 55-65°C for 1.5 h-2.5 h, and then heated to 115-125°C and continued to heat for 3.5 h-4.5 h to obtain epoxy resin composite nanocellulose microcapsules.
10. The preparation method according to claim 7, characterized in that: The temperature of the hot pressing is 100°C to 140°C; The hot pressing pressure is 130 MPa to 170 MPa; The hot pressing time is 15 min to 25 min.
Citation Information
Patent Citations
Nanocellulose and epoxy resin composite material with excellent electrical properties and preparation method of nanocellulose and epoxy resin composite material
CN112980140A
Epoxy resin composite insulating material with mechanical damage targeted self-healing performance
CN114874587A
Preparation method of modified polyurethane microcapsule and dispersion method of modified polyurethane microcapsule in composite epoxy resin
CN118122233A
Nanocomposite microcapsules for self-healing of composite articles
US20170100902A1
Process for self-repair of insulation material
US7285306B1
Cited By
Cellulose insulation paper damage repairing method based on mechanical enhanced microcapsule
CN119372961A
Preparation method of self-repairing cellulose insulation paper doped with ultraviolet light triggered microcapsules
CN119372962A
Preparation method of self-repairing cellulose insulating paper doped with ultraviolet light triggered microcapsules
CN119372962B
Preparation method of bi-component microcapsule self-repairing insulation paper based on epoxy resin and polymercaptan
CN119711253A
Preparation method of two-component microcapsule self-repairing insulating paper based on epoxy resin and polythiol
CN119711253B